Composite substrate

By introducing a high Si concentration region in the intermediate SiO2 layer within composite substrates, the bonding strength between functional and support substrates is enhanced, addressing the issue of peeling and achieving robust substrate integration.

WO2024225277A1PCT designated stage expired Publication Date: 2024-10-31NGK INSULATORS LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015944
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The bonding strength between functional and support substrates in composite substrates is insufficient, leading to potential peeling issues during subsequent processes, despite the use of intermediate SiO2 layers for bonding.

Method used

Incorporating a high Si concentration region in the intermediate SiO2 layer between the functional and support substrates, with Si content exceeding 33 atomic%, to enhance bonding through increased covalent bonds at the interface, formed using methods like sputtering or chemical vapor deposition.

Benefits of technology

This approach significantly improves the bonding strength, as demonstrated by joint strength evaluations, with Si content within the range of 35 to 40 atomic% providing optimal results, preventing peeling and ensuring robust substrate integration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015944_31102024_PF_FP_ABST
    Figure JP2024015944_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A composite substrate includes: a functional substrate which has a predetermined function; a support substrate which supports the functional substrate; and an intermediate layer which is composed of SiO2 and is provided between the support substrate and the functional substrate. The functional substrate and the support substrate are joined to one another by means of the intermediate layer. The intermediate layer includes: SiO2 regions which are respectively provided on the functional substrate side and the support substrate side and are composed of SiO2; and a high-Si-concentration region which is provided so as to be sandwiched between the SiO2 regions and has a Si content larger than that of the SiO2 regions.
Need to check novelty before this filing date? Find Prior Art

Description

Composite PCB

[0001] The present invention relates to a composite substrate.

[0002] Conventionally, composite substrates formed by bonding multiple layers of substrates have been widely used as materials for various devices such as semiconductor elements. For example, a composite substrate that realizes a high-performance semiconductor element with excellent response speed and power consumption is made by bonding a support substrate and a Si substrate to a SiO 2 SOI (Silicon On Insulator) substrates are known, in which the substrate is bonded via a layer. Furthermore, to realize piezoelectric devices such as SAW (Surface Acoustic Wave) filters, LN (LiNbO 3 ) and LT (LiTaO 3 Composite substrates using piezoelectric material substrates such as .

[0003] For example, Patent Document 1 discloses a method for manufacturing a composite substrate in which an LN or LT single crystal wafer and a silicon wafer with an oxide film are bonded together after performing an activation treatment on the bonding surfaces of both wafers.

[0004] Japanese Patent Application Publication No. 2016-225537

[0005] One method for producing such a composite substrate is to combine a functional substrate having a predetermined function, such as a Si substrate or a piezoelectric material substrate, with a supporting substrate, and a SiO 2 In this case, the functional substrate and the support substrate are directly bonded via an intermediate layer of SiO 2 A composite substrate can be formed by forming a layer on each side, and then directly bonding the bonding surfaces of the functional substrate and the support substrate after surface activation treatment. This improves the bonding strength compared to bonding the functional substrate and the support substrate without an intermediate layer.

[0006] However, even with the above method, SiO 2 The bonding strength between layers is insufficient, and the functional substrate may peel off in a later process, so there is room for improvement.

[0007] The present invention has been made in view of the above, and a main object of the present invention is to improve the bonding strength in a composite substrate in which a functional substrate and a support substrate are bonded via an intermediate layer.

[0008] The composite substrate according to the present invention comprises a functional substrate having a predetermined function, a support substrate supporting the functional substrate, and a SiO 2 and an intermediate layer provided between the support substrate and the functional substrate, the functional substrate and the support substrate being bonded to each other via the intermediate layer, the intermediate layer being provided on the functional substrate side and the support substrate side, respectively, and 2 SiO 2 region, and the SiO 2 The SiO 2 and a high Si concentration region having a higher Si content than the low Si concentration region.

[0009] According to the present invention, it is possible to improve the bonding strength in a composite substrate in which a functional substrate and a support substrate are bonded via an intermediate layer.

[0010] Fig. 1 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to one embodiment of the present invention. Fig. 2 is a view showing an example of a manufacturing process for a composite substrate according to one embodiment of the present invention. Fig. 3 is a view showing an example of a manufacturing process for a composite substrate according to one embodiment of the present invention. Fig. 4 is a view showing an example of a manufacturing process for a composite substrate according to one embodiment of the present invention. Fig. 5 is a schematic cross-sectional view showing a schematic configuration of a composite according to a comparative example. Fig. 6 is a graph summarizing the relationship between Si content and bonding strength. Fig. 7 is a graph showing the change in Si content near the bonding interface.

[0011] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the drawings may show the width, thickness, shape, etc. of each part more schematically than in the embodiments, but these are merely examples and do not limit the interpretation of the present invention.

[0012] 1 is a schematic cross-sectional view showing the overall configuration of a composite substrate according to one embodiment of the present invention. The composite substrate 100 in this embodiment has a structure in which a functional substrate 10 having a predetermined function is bonded to a support substrate 30 via an intermediate layer 20.

[0013] The functional substrate 10 has functions for realizing various devices, and is made of materials according to the functions. For example, the composite substrate 100 used for a SAW filter or an optical waveguide is made of LN (LiNbO 3 : lithium niobate) and LT (LiTaO 3 The functional substrate 10 can be formed using a piezoelectric material such as silicon dioxide (SiO2) or lithium tantalate (lithium tantalate). In the composite substrate 100 used as an SOI substrate, the functional substrate 10 is formed using a silicon substrate, which is a semiconductor. In addition to this, various materials can be used as the functional substrate 10 depending on the application of the composite substrate 100.

[0014] In the following, an example in which the functional substrate 10 is made of an LT material will be described, but the same applies to cases in which other materials are used.

[0015] The intermediate layer 20 is provided on the support substrate 30 and is disposed between the functional substrate 10 and the support substrate 30. The material of the intermediate layer 20 is SiO 2 The intermediate layer 20 is provided on the functional substrate 10 side and the support substrate 30 side, and is made of SiO 2 SiO 2 Regions 21A, 21B (first SiO 2 Region 21A and second SiO 2 Between the regions 21B), the Si content is SiO 2 The regions 21A and 21B are configured by sandwiching a high-Si concentration region 22, which is larger than the regions 21A and 21B. 2 If the Si content is higher than in regions 21A and 21B, the bonding strength is improved. That is, by providing a region in intermediate layer 20 that has a higher Si content (e.g., 33 atomic % or more) than other portions, the strength when functional substrate 10 and support substrate 30 are bonded via intermediate layer 20 is improved compared to when this region is not provided. The inventors speculate as follows about the effect of improving the bonding strength.

[0016] When the composite substrate 100 is produced, SiO 2 The composition of the surface regions of the regions 21A and 21B is made to have a higher Si content than the other regions, thereby forming Si-rich regions 22 in these surface regions. The functional substrate 10 and the support substrate 30 are then bonded together using the Si-rich regions 22 as the bonding interface. In this way, in addition to the Si-O-Si covalent bond formed by the conventional bonding method according to the following reaction formula (1), a further SiO 2 It is believed that the covalent bond of the formula (I) can also be formed at the bonding interface. As a result, compared to the conventional bonding method in which the Si-rich region 22 is not provided, the final number of covalent bonds at the bonding interface can be increased, improving the bonding strength and suppressing peeling of the functional substrate 10. Si-OH (support substrate 30 side) + Si-OH (functional substrate 10 side) → Si-O-Si + H 2 O...(1) Si (support substrate 30 side, functional substrate 10 side) +2H 2 O →SiO 2 +2H 2 ... (2)

[0017] The Si content in the Si-rich region 22 before bonding is preferably 35 to 45 atomic %, more preferably 35 to 40 atomic %. A Si content of 40 atomic % or less is more preferable because the Si—O—Si covalent bonds according to the above reaction formula (1) are sufficiently present and voids are suppressed.

[0018] The intermediate layer 20 can be formed by any suitable method, such as sputtering, vacuum deposition, physical vapor deposition such as ion beam assisted deposition (IAD), chemical vapor deposition, or atomic layer deposition (ALD). The intermediate layer 20 can be formed at a temperature of, for example, room temperature (25° C.) to 300° C.

[0019] The support substrate 30 supports the functional substrate 10. Any appropriate substrate can be used as the support substrate 30. The support substrate 30 may be made of a single crystal or a polycrystalline material. It may also be made of a metal. The functional substrate 10 and the support substrate 30 are bonded to each other via an intermediate layer 20.

[0020] The material constituting the support substrate 30 is preferably silicon, sialon, sapphire, cordierite, mullite, glass, quartz, crystal, alumina, SUS, iron-nickel alloy (42 alloy), MgF 2 , CaF 2 and brass. The support substrate 30 may have any suitable thickness.

[0021] The silicon may be single crystal silicon, polycrystalline silicon, or high-resistivity silicon.

[0022] Typically, the sialon is a ceramic obtained by sintering a mixture of silicon nitride and alumina, and for example, Si 6 -wAlwOwN 8 Sialon has a composition represented by -w. Specifically, sialon has a composition in which alumina is mixed into silicon nitride, and w in the formula represents the mixing ratio of alumina. w is preferably 0.5 or more and 4.0 or less.

[0023] Typically, the sapphire is Al 2 O 3 The alumina is a single crystal having a composition of Al 2 O 3 The alumina is preferably a translucent alumina.

[0024] Typically, the cordierite is 2MgO.2Al 2 O 3 5SiO 2 The mullite is a ceramic having a composition of 3Al 2 O 3 2SiO 2 ~2Al 2 O 3 SiO 2It is a ceramic having a composition in the range of

[0025] Although not shown, the composite substrate 100 may further include any layer. The type, function, number, combination, arrangement, etc. of such layers may be appropriately set depending on the purpose.

[0026] The composite substrate 100 can be manufactured in any suitable shape. In one embodiment, the composite substrate 100 can be manufactured in the form of a so-called wafer. The size of the composite substrate 100 can be appropriately set depending on the purpose, for example, with a wafer (substrate) diameter of 50 mm to 200 mm.

[0027] 2 to 4 are diagrams showing an example of a manufacturing process for a composite substrate according to an embodiment of the present invention.

[0028] 2A shows a preparation step in the manufacturing process of the composite substrate 100. In this step, a support substrate 30 is prepared. For example, a high-resistivity Si substrate (resistivity of 2 kΩ·cm or more) having a thickness of 0.23 mm is used as the support substrate 30.

[0029] 2B shows a first film-forming step for the support substrate 30 in the manufacturing process of the composite substrate 100. In this step, a SiO.sub.2 film, for example, is formed to a predetermined thickness on the surface of the support substrate 30 prepared in the preparation step of FIG. 2 By forming an amorphous film of the second SiO 2 Region 21B is formed.

[0030] 2C shows a second film formation step for the support substrate 30 in the manufacturing process of the composite substrate 100. In this step, the second SiO 2 On the region 21B, a second SiO 2 SiO having a higher Si content than region 21B 2 By depositing the amorphous material, the second high Si concentration region 22B for constituting the high Si concentration region 22 in the intermediate layer 20 is formed.

[0031] 2(d) shows a step of planarizing the bonding surface in the manufacturing process of the composite substrate 100. In this step, the surface of the second Si high concentration region 22B formed on the support substrate 30 in the step of FIG. 2(c) is polished to planarize the bonding surface of the support substrate 30 (second Si high concentration region 22B).

[0032] 3(e) shows the activation step in the manufacturing process of the composite substrate 100. In this step, first, an LT substrate 10A made of an LT material with a predetermined thickness and a mirror-polished surface is prepared, and then, by carrying out the film-forming and planarizing steps similar to those shown in FIGS. 2(b), (c), and (d), a first SiO 2 film is formed on the LT substrate 10A. 2 The region 21A and the first Si-rich region 22A are formed, and their surfaces are planarized. Next, N is applied to the surface of the second Si-rich region 22B on the support substrate 30 and the surface of the first Si-rich region 22A on the LT substrate 10A, which have been planarized in the planarization step of FIG. 2 The surfaces are activated by irradiating them with plasma.

[0033] 3(f) shows the bonding step in the manufacturing process of the composite substrate 100. In this step, the surface of the second Si-rich region 22B on the support substrate 30 side, which has been activated in the activation step of FIG. 3(e), is directly bonded to the surface of the first Si-rich region 22A on the LT substrate 10A side, thereby forming a bonded body of the support substrate 30 and the LT substrate 10A with these surfaces serving as bonding surfaces.

[0034] 4(g) shows a bonded body of the support substrate 30 and the LT substrate 10A. By the bonding process of FIG. 4(g), the first Si high concentration region 22A and the second Si high concentration region 22B are bonded and integrated, and the first SiO 2 Region 21A and second SiO 2 An intermediate layer 20 is formed in which the Si-rich region 22 is sandwiched between the regions 21B. As a result, the support substrate 30 and the LT substrate 10A are bonded to each other via the intermediate layer 20, forming a bonded body of the support substrate 30 and the LT substrate 10A as shown in FIG.

[0035] 4(h) shows the annealing step in the manufacturing process of the composite substrate 100. In this step, the bonded assembly of the support substrate 30 and the LT substrate 10A formed in the bonding step of FIG. 4(g) is heated to a predetermined temperature. This forms covalent bonds via OH groups inside the intermediate layer 20, improving the bonding strength of the bonded assembly.

[0036] Fig. 4(i) shows the thinning step in the manufacturing process of the composite substrate 100. In this step, the LT substrate 10A is polished to a predetermined thickness to thin the bonded body after the annealing treatment step shown in Fig. 4(h), thereby forming the functional substrate 10 made of the LT material. For example, the LT substrate 10A can be polished to thin the substrate using grinding, CMP (Chemical Mechanical Polishing), surface planarization using a gas cluster ion beam, or the like.

[0037] Through the above steps, the composite substrate 100 having the structure shown in FIG. 1 is manufactured.

[0038] Examples for verifying the structure of the composite substrate according to the present invention will be specifically described below. Unless otherwise specified, the following procedures were carried out at room temperature.

[0039] Example 1 A bonded body was fabricated according to the manufacturing process described with reference to Figures 2 to 4. Specifically, an LT substrate 10A having a thickness of 0.25 mm and a support substrate 30 made of a high-resistivity Si substrate having a thickness of 0.23 mm were used. Then, SiO 2 The amorphous bodies of the first SiO 2 Region 21A and second SiO 2 The region 21B is formed, and a SiO layer having a high Si content is formed on the region 21B. 2 The amorphous body of the above was deposited to a thickness of 0.11 μm to form the first Si-rich region 22A and the second Si-rich region 22B. These deposition processes were carried out using a reactive sputtering device. 2During deposition of regions 21A and 21B, the oxygen radical discharge power was set to 3 kW and the oxygen flow rate was set to 120 sccm. During deposition of first Si-rich region 22A and second Si-rich region 22B, the oxygen radical discharge power was kept at 3 kW, and the oxygen flow rate was changed from 120 sccm to 60 sccm to change (increase) the Si content. The target power and Ar gas flow rate were kept constant throughout the deposition process. The surfaces of the respective regions were then polished by CMP to a depth of approximately 0.1 μm each to achieve planarization.

[0040] Next, the surface of the first Si-rich region 22A on the LT substrate 10A and the surface of the second Si-rich region 22B on the support substrate 30 are subjected to N 2 After irradiating each with plasma to activate them, the surfaces of these were placed together and pressed together under room temperature conditions to directly bond them together. As a result, the first Si-rich region 22A and the second Si-rich region 22B were integrated to form the Si-rich region 22, and the first SiO 2 Region 21A and second SiO 2 An intermediate layer 20 was formed in which a high-Si concentration region 22 was sandwiched between the regions 21B, and a bonded body was obtained in which the support substrate 30 and the LT substrate 10A were bonded to each other via the intermediate layer 20.

[0041] Next, the resulting bonded body was placed in a high-temperature furnace, heated from room temperature to 130° C., held there for about 4 hours, and then returned to room temperature, thereby carrying out an annealing treatment.

[0042] Next, the LT substrate 10A of the bonded body after the annealing treatment was ground and polished to thin the LT substrate 10A to 1 μm, thereby forming the functional substrate 10, thereby obtaining the composite substrate 100 having the structure shown in FIG. 1. In the composite substrate 100 of Example 1, no peeling of the LT substrate 10A occurred during the thinning process. Furthermore, when the bonding strength was evaluated by the crack opening method, it was found to be 2.5 J / m 2 and had sufficient bonding strength.

[0043] Furthermore, composite substrate 100 of Example 1 was cut, and composition analysis was performed by EDX on a cross section including the bonding interface between first Si-rich region 22A and second Si-rich region 22B formed in intermediate layer 20 to measure the Si content in Si-rich region 22. As a result, the Si content in Si-rich region 22 was found to be 37 atomic %.

[0044] Example 2 In Example 2, the oxygen radical discharge output in the film formation process of the first Si-rich region 22A and the second Si-rich region 22B was set to SiO 2 The oxygen flow rate was changed from the time of forming regions 21A and 21B. Specifically, during the formation of first Si-rich region 22A and second Si-rich region 22B, the oxygen flow rate was kept at 120 sccm, and the oxygen radical discharge output was changed from 3 kW to 1.5 kW, thereby changing (increasing) the Si content. The other conditions were the same as in Example 1, and the other steps were also performed under the same conditions as in Example 1, to obtain composite substrate 100 having the structure shown in FIG. 1 .

[0045] In the composite substrate 100 of Example 2, similar to Example 1, no peeling of the LT substrate 10A occurred during the thinning process. In addition, when the bonding strength was evaluated by the crack opening method, it was found to be 2.7 J / m 2 and had sufficient bonding strength.

[0046] Furthermore, composite substrate 100 of Example 2 was cut, and composition analysis was performed by EDX on a cross section including the bonding interface between first Si-rich region 22A and second Si-rich region 22B formed in intermediate layer 20 to measure the Si content in Si-rich region 22. As a result, the Si content in Si-rich region 22 was found to be 40 atomic %.

[0047] Example 3 In Example 3, both the oxygen radical discharge output and the oxygen flow rate in the film formation process of the first Si high concentration region 22A and the second Si high concentration region 22B were set to SiO 2The conditions were changed from the time of forming regions 21A and 21B. Specifically, when forming first Si-rich region 22A and second Si-rich region 22B, the oxygen flow rate was changed from 120 sccm to 60 sccm, and the oxygen radical discharge output was changed from 3 kW to 1.5 kW, thereby changing (increasing) the Si content. The other conditions were the same as in Example 1, and the other steps were also performed under the same conditions as in Example 1, to obtain composite substrate 100 having the structure shown in FIG.

[0048] In the composite substrate 100 of Example 3, similarly to Example 1, no peeling of the LT substrate 10A occurred during the thinning process. In addition, when the bonding strength was evaluated by the crack opening method, it was found to be 2.8 J / m 2 and had sufficient bonding strength.

[0049] Furthermore, composite substrate 100 of Example 3 was cut, and composition analysis was performed by EDX on a cross section including the bonding interface between first Si-rich region 22A and second Si-rich region 22B formed in intermediate layer 20 to measure the Si content in Si-rich region 22. As a result, the Si content in Si-rich region 22 was found to be 45 atomic %.

[0050] Comparative Example 1 In Comparative Example 1, the process of forming the first Si-rich region 22A and the second Si-rich region 22B and the process of thinning the LT substrate 10A were omitted, and the other processes were performed under the same conditions as in Example 1, thereby obtaining a composite 100A having the structure shown in Fig. 5(a). In this composite 100A, the support substrate 30 and the LT substrate 10A are bonded to each other via an intermediate layer 20A, and the Si-rich region 22 as shown in Fig. 1 is not formed inside the intermediate layer 20A.

[0051] The composite 100A of Comparative Example 1 was evaluated for bonding strength by the crack opening method, and found to have a bonding strength of 1.8 J / m 2 The extent was insufficient.

[0052] Comparative Example 2 In Comparative Example 2, instead of the first Si high concentration region 22A and the second Si high concentration region 22B, a silicon dioxide film having a Si content of SiO 2The low-Si concentration region, which is lower than the regions 21A and 21B, is formed by a first SiO 2 film formed on the LT substrate 10A side. 2 The second SiO film formed on the region 21A and on the support substrate 30 side 2 Specifically, SiO 2 When forming the regions 21A and 21B, the oxygen radical discharge output was set to 3 kW and the oxygen flow rate to 120 sccm, as in Example 1. On the other hand, when forming the low-Si concentration region, the oxygen radical discharge output was kept at 3 kW, and the oxygen flow rate was changed from 120 sccm to 200 sccm, thereby changing (decreasing) the Si content. In addition, the thinning process for thinning the LT substrate 10A was omitted, and the other processes were performed under the same conditions as in Example 1, thereby obtaining a composite 100B having the structure shown in FIG. 5(b). In this composite 100B, the support substrate 30 and the LT substrate 10A are bonded to each other via an intermediate layer 20B, and the intermediate layer 20B is made of a first SiO 2 Region 21A and second SiO 2 Between the regions 21B, the content of Si is 2 The regions 21A and 21B are configured with a low Si concentration region 23 sandwiched therebetween, the low Si concentration region 23 being smaller than the regions 21A and 21B. The low Si concentration region 23 is formed by joining the low Si concentration regions together.

[0053] The composite 100B of Comparative Example 2 was evaluated for bonding strength by the crack opening method, and found to have a bonding strength of 1.5 J / m 2 The extent was insufficient.

[0054] Furthermore, composite 100B of Comparative Example 2 was cut, and a composition analysis was performed by EDX on a cross section including the bonding interface between the low-Si-concentration regions formed in intermediate layer 20B to measure the Si content in low-Si-concentration region 23. As a result, the Si content in low-Si-concentration region 23 was found to be 30 atomic %.

[0055] 6 is a graph summarizing the relationship between the Si content of the high-Si concentration region 22 or the low-Si concentration region 23 and the bonding strength in each composite substrate 100 of Examples 1 to 3 and the composites 100A and 100B of Comparative Examples 1 and 2. In FIG. 6, point 101 represents Example 1, point 102 represents Example 2, point 103 represents Example 3, point 104 represents Comparative Example 1, and point 105 represents Comparative Example 2. Note that in Comparative Example 1, as described above, neither the high-Si concentration region 22 nor the low-Si concentration region 23 was formed in the intermediate layer 20, and therefore the Si content was calculated using SiO 2 The atomic % was set to 33 atomic %, which corresponds to the value of

[0056] From the graph in FIG. 2 SiO 2 It can be seen that if a Si-rich region 22 having a higher Si content than regions 21A and 21B (a Si content greater than 33 atomic%) is formed in the intermediate layer 20, the bonding strength is improved compared to when the Si-rich region 22 is not formed or when the Si-lower concentration region 23 is formed. However, as in Example 3, when the Si content increases to about 45 atomic%, a lack of O atoms can cause a decrease in the Si-O-Si covalent bonds at the bonding interface, which can lead to the generation of voids. Therefore, it is more preferable that the Si content be in the range of 35 to 40 atomic%. In other words, in the composite substrate 100 produced in each step of Figures 2 to 4, by setting the conditions of the second film formation step described above so that a Si-rich region 22 having a higher Si content than other portions is formed inside the intermediate layer 20, a composite substrate 100 with improved bonding strength can be realized.

[0057] 7 is a graph showing the change in the Si content near the bonding interface in composite substrate 100 of Example 1. As can be seen from FIG. 7, a high-Si-concentration region 22 is formed in intermediate layer 20 with a thickness of about 20 nm across the bonding interface.

[0058] According to the embodiment of the present invention described above, the following advantageous effects are achieved.

[0059] (1) The composite substrate 100 includes a functional substrate 10 having a predetermined function, a support substrate 30 supporting the functional substrate 10, and a SiO 2The functional substrate 10 and the support substrate 30 are bonded to each other via the intermediate layer 20, and the intermediate layer 20 is provided on the functional substrate 10 side and the support substrate 30 side, respectively, and is made of SiO 2 SiO 2 Regions 21A and 21B and SiO 2 It is sandwiched between the regions 21A and 21B, and is made of SiO 2 The functional substrate 10 and the supporting substrate 30 are bonded together via the intermediate layer 20, and the bonding strength of the composite substrate 100 is improved.

[0060] (2) The Si-rich region 22 preferably has a Si content of more than 33 atomic %, and more preferably has a Si content in the range of 35 to 40 atomic %. This ensures the formation of the Si-rich region 22, which contributes to improving the bonding strength.

[0061] (3) The functional substrate 10 is made of LN (LiNbO 3 ) or LT(LiTaO 3 The functional substrate 10 may be a piezoelectric material substrate made of a silicon (Si) material. The functional substrate 10 may also be a semiconductor substrate made of a silicon (Si) material. In this way, substrates having various functions can be used as the functional substrate 10 depending on the application of the composite substrate 100.

[0062] The present invention is not limited to the above-described embodiment, and can be implemented using any components without departing from the spirit of the present invention.

[0063] The above-described embodiments and modifications are merely examples, and the present invention is not limited to these details as long as the features of the invention are not impaired. Furthermore, although various embodiments and modifications have been described above, the present invention is not limited to these details. Other aspects that can be considered within the scope of the technical idea of ​​the present invention are also included within the scope of the present invention.

[0064] 10: Functional substrate 10A: LT substrate 20: Intermediate layer 21A: First SiO 2Field 21B: 2nd SiO 2 Area 22: Si high concentration area 30: Support substrate 100: Composite substrate

Claims

1. A functional substrate having a predetermined function; a support substrate supporting the functional substrate; and a SiO 2 and an intermediate layer provided between the support substrate and the functional substrate, the functional substrate and the support substrate being bonded to each other via the intermediate layer, the intermediate layer being provided on the functional substrate side and the support substrate side, and the intermediate layer being made of SiO 2 SiO 2 region, and the SiO 2 The SiO 2 and a Si-rich region having a higher Si content than the Si-rich region.

2. A composite substrate according to claim 1, wherein the high Si concentration region has a Si content of more than 33 atomic %.

3. A composite substrate according to claim 2, wherein the high Si concentration region has a Si content within the range of 35 to 40 atomic %.

4. A composite substrate according to claim 1, wherein the functional substrate is a piezoelectric material substrate.

5. The composite substrate according to claim 4, wherein the piezoelectric material substrate is LiNbO 3 or LiTaO 3 A composite substrate made of materials.

6. A composite substrate according to claim 1, wherein the functional substrate is a semiconductor substrate made of a Si material.

Citation Information

Patent Citations

  • Semiconductor device and manufacturing method thereof

    JP2008288232A

  • Method for performing direct bonding between two structures

    JP2017118113A

  • Bonding method

    WO2017163722A1