Coated fertilizer, method for producing coated fertilizer, and composition for coating fertilizer

The use of a fatty acid salt with 20 or more carbon atoms and a wax in the coating composition addresses lamination defects in coated fertilizers, achieving a high non-defective product rate and controlled elution, thus enhancing the quality and yield of the coated fertilizer.

WO2024225299A1PCT designated stage expired Publication Date: 2024-10-31CENT GLASS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016020
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-16
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional coated fertilizers face issues with lamination defects due to the formation of agglomerates and blocking particles when using stearate-based coatings, which restricts the design freedom and yield of the coating process.

Method used

A coated fertilizer is developed using a coating composition containing a salt of a fatty acid with 20 or more carbon atoms and a wax, specifically a salt of a fatty acid with 31 or more carbon atoms, which suppresses lamination defects and improves the non-defective product rate.

Benefits of technology

The solution effectively reduces lamination defects, enhances the non-defective product rate to 50% or more, and improves the initial elution control, while maintaining low moisture permeability, thereby improving the overall quality and yield of the coated fertilizer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016020_31102024_PF_FP_ABST
    Figure JP2024016020_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A coated fertilizer comprising a water-soluble granular fertilizer and a coating film covering the water-soluble granular fertilizer, wherein the coating film contains a salt of a fatty acid having 20 or more carbon atoms and a wax.
Need to check novelty before this filing date? Find Prior Art

Description

Coated fertilizer, method for producing coated fertilizer, and composition for coating fertilizer

[0001] The present disclosure relates to a coated fertilizer, a method for producing the coated fertilizer, and a composition for coating a fertilizer.

[0002] Conventionally, there has been a demand for more labor-saving and efficient fertilizers and their use methods, due to the environmental impact of the runoff of active ingredients in water-soluble fertilizers and the need for labor-saving measures due to the aging of agricultural workers. Against this background, various granular fertilizers with adjustable release times have been proposed and put into practical use. One example of an adjustable release time granular fertilizer is a coated fertilizer. A coated fertilizer is a fertilizer in which the release time of the active ingredients inside is adjusted by coating the surface of the water-soluble fertilizer with a film made of a laminate of organic or inorganic coating materials. Various types of coating materials have been investigated to control the release time of the active ingredients. Patent Document 1 describes a coated granular fertilizer having a coating formed from a coating material containing resin and high-purity talc. Patent Document 2 describes a coated fertilizer coated with a sulfur modifier composed of sulfur and an alicyclic unsaturated hydrocarbon compound. Non-Patent Document 1 describes a coated fertilizer in which a water-soluble fertilizer is coated, in order, with a layer of calcium stearic acid and a layer of paraffin wax.

[0003] Japanese Patent Application Publication No. 2019-156681 Japanese Patent Application Publication No. 2007-084414

[0004] Ebtisam K. Heikal, Salah A. Khalil “Coating Potassium Nitrate and Urea Fertilizers by some Organic and Inorganic Materials to Improve their Dissolution and Releasing Characteristics”, AMSE JOURNALS -2015-Series: Modelling C; Vol. 76;N°1; pp 33-45

[0005] However, when attempting to coat a water-soluble fertilizer with stearates, it was found that adding wax or stearic acid to the surface of the formed stearate coating caused the rolling particles to form agglomerates that could not be broken down without the application of additional external force, tending to cause lamination defects. The occurrence of such lamination defects makes it difficult to laminate the coating material, limiting the freedom of coating design. The present disclosure aims to provide a coated fertilizer in which lamination defects are suppressed.

[0006] The coated fertilizer of the present disclosure can solve the above problems by employing a coating containing a salt of a fatty acid having 20 or more carbon atoms and a wax. More specifically, the above problems can be solved by the following configuration.

[0007] <1> A coated fertilizer comprising a water-soluble granular fertilizer and a coating covering the water-soluble granular fertilizer, wherein the coating contains a salt of a fatty acid having 20 or more carbon atoms and a wax. <2> The coated fertilizer according to <1>, wherein the salt of the fatty acid contains a salt of a fatty acid having 31 or more carbon atoms. <3> The coated fertilizer according to <1> or <2>, wherein the salt of the fatty acid contains at least one of a salt of a dimer acid and a salt of a trimer acid. <4> The coated fertilizer according to any one of <1> to <3>, wherein the salt of the fatty acid contains a salt of a fatty acid having at least one of a branched structure and a cyclic structure. <5> The coated fertilizer according to any one of <1> to <4>, wherein the wax contains at least one of a petroleum-based wax and a vegetable wax. <6> The coated fertilizer according to any one of <1> to <5>, wherein the coating is composed of at least one layer, at least one of which contains the salt of the fatty acid and the wax. <7> The coated fertilizer according to any one of <1> to <6>, wherein the coating is composed of at least one layer, and the layer closest to the water-soluble granular fertilizer contains the salt of the fatty acid and the wax. <8> The coated fertilizer according to any one of <1> to <7>, wherein the coating is composed of at least four layers, and at least four layers contain the salt of the fatty acid and the wax. <9> The fertilizer moisture permeability of the coating at 40°C is 52 g / (m 2<10> The coated fertilizer according to any one of <1> to <9>, wherein the coating does not contain a resin. <11> A method for producing a coated fertilizer comprising a water-soluble granular fertilizer and a coating covering the water-soluble granular fertilizer, wherein a coating containing a salt of a fatty acid having 20 or more carbon atoms and a wax is formed on the water-soluble granular fertilizer. <12> A method for producing a coated fertilizer according to <11>, wherein the coating has at least one layer containing the salt of the fatty acid and the wax, and wherein the following steps 1 to 3 are carried out in this order. <13> A method for producing a coated fertilizer according to <12>, wherein, after step 3, steps 2 and 3 are each performed one or more times. <14> A method for producing a coated fertilizer according to <12> or <13>, wherein step 2 includes step 2a of supplying the fatty acid and the wax to the surface of the water-soluble granular fertilizer. <15> A method for producing a coated fertilizer according to any one of <12> to <14>, wherein four or more cycles are performed, each cycle consisting of performing steps 2 and 3 in this order once. <16> A method for producing a coated fertilizer according to any one of <12> to <15>, wherein the fatty acid comprises a fatty acid having 31 or more carbon atoms. <17> A method for producing a coated fertilizer according to any one of <12> to <16>, wherein the fatty acid comprises at least one of a dimer acid and a trimer acid. <18> A composition for coating a fertilizer, comprising a salt of a fatty acid having 20 or more carbon atoms and a wax. <19> The composition for coating a fertilizer according to <18>, wherein the salt of the fatty acid comprises a salt of a fatty acid having 31 or more carbon atoms. <20> The composition for coating a fertilizer according to <18> or <19>, wherein the salt of the fatty acid comprises at least one of a salt of a dimer acid and a salt of a trimer acid. <21> A compound fertilizer comprising the coated fertilizer according to any one of <1> to <10> and another fertilizer.<22> The compound fertilizer according to <21>, wherein the other fertilizer is at least one selected from the group consisting of highly chemical fertilizers, nitrogenous fertilizers, phosphate fertilizers, potassium fertilizers, organic fertilizers, silicate fertilizers, and magnesium fertilizers.

[0008] According to the present disclosure, a coated fertilizer in which stacking defects are suppressed can be provided.

[0009] FIG. 1 is a schematic diagram showing a cross section of an example of a coated fertilizer.

[0010] The present disclosure will be described in detail below, but the following description of the constituent elements is an example of an embodiment of the present disclosure and is not limited to these specific details. Various modifications can be made within the scope of the gist of the disclosure. In this specification, the term "to" is used to mean that the numerical values ​​before and after it are included as the lower and upper limits. In addition, in this specification, the period from the start of the dissolution test until three days have passed may be referred to as "initial". The dissolution rate three days after the start of the dissolution test may be referred to as "initial dissolution".

[0011] (Layer) In this specification, the term "layer" refers to a state in which raw materials supplied for coating have hardened or solidified to cover particles to be coated (water-soluble granular fertilizer or coated water-soluble granular fertilizer). A state in which further raw materials are supplied on top of the layer and hardened or solidified may also be referred to as a "layer". Furthermore, a layer may or may not have boundaries between layers. When the terms "first layer", "second layer", etc. are used in this specification, for example, the first layer refers to a layer obtained by hardening or solidifying a coating material derived from the raw materials supplied the first time, and the layer may or may not have boundaries, and the component ratio and distribution of the components constituting the layer may be uniform or non-uniform.

[0012] (Lamination Defects) In this specification, the formation of the aforementioned agglomerates or the occurrence of a large amount of blocking particles is considered a lamination defect. Agglomerates are clumps of a size that can be seen with the naked eye, and the occurrence of agglomerates tends to make it difficult for the coated particles to maintain a fluid or rolling state. Furthermore, agglomerates can often be broken down into individual particles by the application of external force. Blocking refers to the phenomenon in which a small number of particles are integrated together while maintaining a fluid or rolling state, and blocked particles refer to particles in which blocking has occurred. Particles integrated by blocking are solidified by strong forces, and therefore often cannot be broken down as easily as the above-mentioned agglomerates even when an external force is applied. If there are only a small number of blocking particles, they are difficult to detect during production because they are in a fluid or rolling state together with particles that are not blocked. However, due to their poor fluidity, if there are a large number of blocking particles, those left on the surface of the fluid or rolling particle group can be easily visually confirmed. Therefore, if blocking particles are visually confirmed during production, they are considered a lamination defect. Furthermore, if the blocking defect rate described below exceeds 20%, a lamination defect may also be detected.

[0013] [1. Coated Fertilizer] The coated fertilizer disclosed herein includes a water-soluble granular fertilizer and a coating covering the water-soluble granular fertilizer, the coating containing a salt of a fatty acid having 20 or more carbon atoms and a wax. The inventors conducted studies using a salt of a fatty acid having 18 or fewer carbon atoms and found that a layer containing a salt of a fatty acid having 18 or fewer carbon atoms is easily dissolved in the coating material of the next layer (e.g., a fatty acid or wax having 18 or fewer carbon atoms) or easily absorbs and swells by the coating material. It is presumed that the layer containing the fatty acid salt is likely to form the above-mentioned clumps by dissolving or swelling in the coating material of the next layer. Furthermore, it has been newly discovered that even if the above-mentioned clumps are eliminated, the greater the number of carbon atoms in the fatty acid salt, the more likely the aforementioned blocking is to occur. Blocking occurs during hardening or solidification of the coating material, and once it occurs, it is difficult to disintegrate. Blocked particles cannot be used in a spreader and are ultimately removed. In other words, if blocking is likely to occur, the yield decreases with increasing layer thickness. Further investigations have revealed that the above-mentioned blocking can be suppressed by using wax as a coating material. Furthermore, the coated fertilizer of the present disclosure can achieve a yield rate of 50% or more, as described below. The yield rate is an index showing the proportion of defects contained in the coating, and the higher the yield rate, the easier it tends to suppress initial elution. Therefore, the yield rate is preferably 50% or more, and more preferably 70% or more.

[0014] <Water-soluble granular fertilizer> The coated fertilizer of the present disclosure includes a water-soluble granular fertilizer. The water-soluble granular fertilizer is used as a fertilizer component. The water-soluble granular fertilizer is not particularly limited as long as it is water-soluble. Examples of water-soluble granular fertilizers include urea, ammonium chloride, ammonium sulfate, ammonium nitrate, potassium chloride, potassium nitrate, sodium nitrate, potassium ammonium phosphate, ammonium ammonium phosphate, and calcium ammonium phosphate, with urea being preferred. The water-soluble granular fertilizer may be a fertilizer using one type selected from the above, or a compound fertilizer using two or more types. Furthermore, the water-soluble granular fertilizer may contain water-soluble or insoluble impurities, etc., as long as the impurities do not significantly affect the properties of the fertilizer.

[0015] The size and shape of the water-soluble granular fertilizer are not particularly limited, and those of commonly used sizes can be used. For example, for convenience in spreading on farms using existing machinery, etc., the fertilizer is preferably solid particles (e.g., spherical, approximately spherical, rod-like, needle-like, rectangular, flat, irregular, etc.), and the particle diameter as determined by sieving is preferably 1.0 mm to 5.0 mm, more preferably 2.0 mm to 4.0 mm.

[0016] The water-soluble granular fertilizer may be commercially available or may be produced by a known method such as extrusion granulation or compression granulation.

[0017] <Coating> The coating in the coated fertilizer of the present disclosure refers to the entire film covering the water-soluble granular fertilizer. The film on the water-soluble granular fertilizer may be in contact with the surface of the water-soluble granular fertilizer, or any film or layer may be interposed between the water-soluble granular fertilizer and the film. The surface of the coating may also have any particles. Note that, in this specification, particles that adhere to the surface of the coating after coating formation are not considered to be part of the coating. In the coated fertilizer of the present disclosure, the coating is composed of at least one layer, preferably at least two layers, and more preferably at least four layers. The upper limit of the number of layers constituting the coating is not particularly limited, but may be, for example, 100 or less, or 50 or less. In the present disclosure, when there are two or more layers covering the water-soluble granular fertilizer, the entire film consisting of a laminate of two or more layers is referred to as the "coating." When there are two or more layers constituting the coating, the layers may have different compositions, or all may have the same composition. Note that the "composition" refers to the components contained in the layer and their content.

[0018] The coating contains a salt of a fatty acid having 20 or more carbon atoms and a wax. Fatty acids having 20 or more carbon atoms are also referred to as "specific fatty acids," and salts of fatty acids having 20 or more carbon atoms are also referred to as "salts of specific fatty acids." Furthermore, among all the fatty acid salts contained in the coating, salts of fatty acids other than the salts of specific fatty acids may be contained to the extent that the various performance properties of the coating are not significantly impaired. However, it is desirable that the main component of the fatty acid salt contained in the coating is the salt of the specific fatty acid. The "main component" refers to the component that is most abundant among the fatty acid salts. For example, if the total mass of the fatty acid salts contained in the coating is 100 mass%, the main component may have a content of 60 mass% or more. Preferably, the main component may have a content of 75 mass% or more, more preferably a content of 80 mass% or more, even more preferably a content of 85 mass% or more, and particularly preferably a content of 90 mass% or more. The upper limit of the main component content is not particularly limited, but may be, for example, 100 mass% or less, preferably 98 mass% or less. Furthermore, when there are two or more types of salts of specific fatty acids, the total value may be used as the "content of salts of specific fatty acids."

[0019] When the coating has two or more layers, the salt of the specific fatty acid and the wax may be contained in the same layer or in separate layers (i.e., one layer may contain the salt of the specific fatty acid but not the wax, and another layer may contain the wax but not the salt of the specific fatty acid). From the viewpoints of improving the yield rate of coated fertilizers, reducing the blocking defect rate, improving initial dissolution, and improving the moisture permeability of the fertilizer at 40°C, it is preferable that the coating be composed of at least one layer, at least one of which contains the salt of the specific fatty acid and the wax. It is more preferable that the coating be composed of at least four layers, at least four of which contain the salt of the specific fatty acid and the wax. It is preferable that the coating be composed of at least one layer, and that the layer closest to the water-soluble granular fertilizer (the layer in contact with the surface of the water-soluble granular fertilizer) contain the salt of the specific fatty acid and the wax.

[0020] FIG. 1 is a schematic diagram showing a cross section of an example of a coated fertilizer according to the present disclosure. The coated fertilizer 1 in FIG. 1 includes a water-soluble granular fertilizer F and a coating L covering the water-soluble granular fertilizer F. The coating L is composed of four layers, namely, a first layer L1, a second layer L2, a third layer L3, and a fourth layer L4, in order from the side closest to the water-soluble granular fertilizer F. At least one of the first layer L1, the second layer L2, the third layer L3, and the fourth layer L4 contains a salt of a specific fatty acid, and at least one of the layers contains a wax. It is preferable that at least one of the first layer L1, the second layer L2, the third layer L3, and the fourth layer L4 contains a salt of a specific fatty acid and a wax. It is more preferable that the first layer L1 contains a salt of a specific fatty acid and a wax. It is particularly preferable that the first layer L1, the second layer L2, the third layer L3, and the fourth layer L4 contain a salt of a specific fatty acid and a wax. 1, the boundaries between the layers L1 to L4 are clearly shown, but the boundaries may be unclear. The thicknesses of the layers may be the same or different.

[0021] The thickness of the coating can be changed appropriately according to the desired elution pattern, and may be, for example, 10 μm to 250 μm, 30 μm to 200 μm, or 50 μm to 150 μm. The total thickness of the coating is the thickness of the coating. There are no particular limitations on the thickness of each layer constituting the coating, and the thickness can be changed appropriately depending on the thickness of the coating. However, a thickness of 5 μm to 30 μm is preferable from the viewpoint of ease of coating.

[0022] The total mass of the coating is preferably 1.0 to 30% by mass, more preferably 2.0 to 25% by mass, and even more preferably 3.0 to 20% by mass, relative to the total mass of the coated fertilizer. The ratio of the total mass of the coating to the total mass of the coated fertilizer is also called the coating rate. Coating rate (%) = (total mass of the coating / total mass of the coated fertilizer) x 100

[0023] The fertilizer moisture permeability of the coating at 40°C is 52 g / (m 224h) or less. The fertilizer moisture permeability indicates the sum of the ease of permeation of water through the coating and the ease of permeation of urea dissolved in water (urea water) through the coating. When the salt of a specific fatty acid in the coating is the same, the smaller the value of the fertilizer moisture permeability, the higher the rate of non-defective products and the easier it is to suppress initial elution. Also, more preferably, it is 50g / (m 2 24h) or less, and more preferably 20g / (m 2 ・24h) or less, 10g / (m 2 ・24h) or less may also be used.

[0024] <Other Optional Components> The coated fertilizer of the present disclosure may have an optional material on the surface of the coating for the purposes of preventing scratches, floating in water, caking, etc. Examples include talc, silica, diatomaceous earth, etc. These optional materials adhere to the coating by being applied to the surface of the coated fertilizer. Furthermore, as described below, they may be mixed into the coating as one component of the coating material. Furthermore, the coated fertilizer of the present disclosure may contain unreacted raw materials (e.g., fatty acids such as specific fatty acids, metal hydroxides, etc.) and reaction by-products, etc., that were produced during coating formation, as described below, in the coating.

[0025] The components contained in the coating will be described below.

[0026] (Salt of specific fatty acid) The salt of specific fatty acid is a salt of a fatty acid having 20 or more carbon atoms. It preferably contains a salt of a fatty acid having 21 or more carbon atoms, and more preferably contains a salt of a fatty acid having 31 or more carbon atoms. It is even more preferable that the main component of the salt of fatty acid contained in the coating is a salt of a fatty acid having 31 or more carbon atoms. There is no particular limitation on the upper limit of the number of carbon atoms in the salt of specific fatty acid, but it may be, for example, 100 or less.

[0027] The salt of the specific fatty acid may be a salt of a monobasic acid, a salt of a dibasic acid, or a salt of a tribasic acid, but preferably contains at least one of a salt of a dibasic acid and a salt of a tribasic acid. The salt of the specific fatty acid contained in the coating may be one type or two or more types. The salt of the specific fatty acid preferably contains at least one of a salt of a dimer acid and a salt of a trimer acid. More preferably, the total amount of the salt of the specific fatty acid contained in the coating may be at least 60% by mass of the salt of the dimer acid or the salt of the trimer acid. Even more preferably, the salt of at least the dimer acid may be at least 60% by mass, and even more preferably, the salt of at least the dimer acid may be at least 70% by mass. The upper limit of the content of the salt of the dimer acid is not particularly limited, but may be, for example, 100% by mass or less, 90% by mass or less, or 85% by mass or less.

[0028] The salt of the specific fatty acid preferably includes a salt of a fatty acid having at least one of a branched structure and a cyclic structure. The specific fatty acid having the above structure is suitable because it tends to be compatible with the wax and to easily retain the wax inside the fatty acid salt of the coating. Furthermore, it is more preferable that the main component of the fatty acid salt contained in the coating is a salt of a fatty acid having at least one of a branched structure and a cyclic structure. The branched structure refers to a structure in which at least one hydrogen atom in the hydrocarbon chain of the fatty acid is replaced with carbon, and the cyclic structure refers to a hydrocarbon ring.

[0029] The salt of the specific fatty acid may be a salt of a saturated fatty acid or a salt of an unsaturated fatty acid. The salt of the specific fatty acid is preferably a salt of an aliphatic carboxylic acid having 20 or more carbon atoms. The salt of the specific fatty acid is preferably a salt of a vegetable fatty acid having 20 or more carbon atoms. Specific examples of the specific fatty acid in the salt of the specific fatty acid will be described later.

[0030] The salt of the specific fatty acid is preferably a metal salt of the specific fatty acid, and more preferably at least one of an alkali metal salt of the specific fatty acid and an alkaline earth metal salt of the specific fatty acid. For example, at least one selected from the group consisting of a sodium salt of the specific fatty acid, a potassium salt of the specific fatty acid, a lithium salt of the specific fatty acid, a calcium salt of the specific fatty acid, and a magnesium salt of the specific fatty acid is even more preferable. Since the specific fatty acid salt tends to be difficult to coat even when supplied to a water-soluble granular fertilizer, a salt obtained by the production method described below is used. Specifically, a coating of the specific fatty acid salt can be obtained by reacting the specific fatty acid with a metal hydroxide on the water-soluble granular fertilizer. From the viewpoint of ease of reaction with the specific fatty acid to form a salt of the specific fatty acid, calcium hydroxide is preferably used as the metal hydroxide. That is, the specific fatty acid salt is particularly preferably a calcium salt of the specific fatty acid.

[0031] The content of the salt of the specific fatty acid is not particularly limited as long as the desired coating is obtained, and is, for example, preferably 1 to 99% by mass, more preferably 5 to 95% by mass, and even more preferably 10 to 90% by mass, relative to the total mass of the coating.

[0032] (Wax) The wax is not particularly limited. The wax is preferably one that becomes liquid at the coating temperature, and more preferably one having a melting point of 45 to 100°C. Examples of the wax include petroleum wax such as paraffin wax, vegetable wax such as carnauba wax, polymer wax such as polyethylene wax, hydrogenated oil such as palm hydrogenated oil and beef tallow hydrogenated oil, and synthetic ester wax.

[0033] The wax preferably contains at least one of a petroleum wax and a vegetable wax. Furthermore, when the mass of all waxes contained in the coating is taken as 100, the total content of the petroleum wax and the vegetable wax is more preferably 80 mass% or more, and it is even more preferable that all waxes contained in the coating are at least one of a petroleum wax and a vegetable wax.

[0034] The wax content is not particularly limited as long as it is contained in an amount that can suppress lamination defects, and is, for example, preferably 1 to 40 mass %, more preferably 2.5 to 30 mass %, and even more preferably 5 to 20 mass %, relative to the total mass of the coating.

[0035] (Other Components) In addition to the salt of the specific fatty acid and the wax, the coating may contain other components within the coating. Examples of other components include resin, surfactant, talc, diatomaceous earth, silica, sulfur powder, etc. When these are optional components within the coating, they can be incorporated into the coating as the coating material cures or solidifies by supplying the above components before the coating material supplied into the coating device hardens or solidifies. The content of the other components may be 0 to 20% by mass, or 0 to 10% by mass, relative to the total mass of the coating.

[0036] The coating may or may not contain a resin (for example, polyethylene, polyester, acrylic resin, polyurethane, etc.), but from the viewpoint of reducing the burden on the environment, it is preferable that the coating does not contain a resin.

[0037] [2. Compound Fertilizer] The coated fertilizer of the present disclosure may be mixed with other fertilizers to form a compound fertilizer. Examples of the other fertilizers include, but are not limited to, highly chemical fertilizers such as NK and NPK compounds, nitrogenous fertilizers such as ammonium chloride, ammonium sulfate, and urea, phosphate fertilizers such as monoammonium phosphate and diammonium phosphate, potassium fertilizers such as potassium chloride and potassium silicate, organic fertilizers such as fish meal, meat and bone meal, vegetable oil cake and powder thereof, silicate fertilizers such as silica gel, and magnesium fertilizers such as magnesium ammonium phosphate.

[0038] [3. Manufacturing method of coated fertilizer] Hereinafter, a manufacturing method of the coated fertilizer of the present disclosure will be described. The manufacturing method of the coated fertilizer of the present disclosure is a manufacturing method of a coated fertilizer including a water-soluble granular fertilizer and a coating covering the water-soluble granular fertilizer, and is a manufacturing method of a coated fertilizer in which a coating containing a salt of a fatty acid having 20 or more carbon atoms and a wax is formed on the water-soluble granular fertilizer. The water-soluble granular fertilizer, the salt of a fatty acid having 20 or more carbon atoms (salt of a specific fatty acid), and the wax are as described above.

[0039] Examples of methods for producing coated fertilizers include the following methods 1 and 2. From the viewpoints of improving the yield rate of coated fertilizers, improving the blocking defect rate, improving initial dissolution, improving the moisture permeability of the fertilizer at 40°C, and shortening the production time, it is preferable to include the following method 1. Method 1 is particularly suitable because it can improve blocking defects that are more likely to occur as the number of carbon atoms in the specific fatty acid increases.

[0040] <Method 1> A method for producing a coated fertilizer, in which the coating has at least one layer containing a salt of a specific fatty acid and a wax, and the following steps 1 to 3 are carried out in this order: Step 1: A step of bringing the water-soluble granular fertilizer into a fluidized or tumbling state in a coating device; Step 2: A step of supplying the specific fatty acid and the wax into the coating device; and Step 3: A step of supplying a metal hydroxide into the coating device, reacting the specific fatty acid with the metal hydroxide to generate a salt of the specific fatty acid, and forming a layer containing the salt of the specific fatty acid and the wax.

[0041] <Method 2> A method for producing a coated fertilizer, in which the coating has at least one layer A containing a salt of a specific fatty acid and one layer B containing a wax, and the method comprises carrying out the following steps 1, a, and b in this order: Step 1: A step of bringing the water-soluble granular fertilizer into a fluidized or tumbling state in a coating device; Step a: A step of supplying a specific fatty acid and a metal hydroxide into the coating device, reacting the specific fatty acid with the metal hydroxide to generate a salt of the specific fatty acid, and forming layer A; Step b: A step of supplying a wax and a metal hydroxide into the coating device, solidifying the wax, and forming layer B on the surface of layer A.

[0042] First, method 1 will be described.

[0043] (Step 1) Step 1 will now be described. In step 1, the water-soluble granular fertilizer is brought into a fluidized or tumbling state within a coating device. By bringing the water-soluble granular fertilizer into a fluidized or tumbling state, the uniformity of the coating film thickness is improved. The coating device is not particularly limited, but a device such as a rotating drum can be suitably used. Furthermore, in step 1, the temperature within the device may be maintained at approximately the coating temperature in advance, and the water-soluble granular fertilizer may be heated before step 2. The coating temperature may be determined based on the melting points of the specific fatty acid, wax, and water-soluble granular fertilizer used, and is not particularly limited, but is, for example, 20 to 150°C, preferably 40 to 100°C. The coating temperature is the temperature at which steps 2 and 3 are performed. Furthermore, the humidity within the device may be adjusted so as not to interfere with steps 2 and 3, which will be described later.

[0044] (Step 2) Step 2 will be described. In Step 2, the specific fatty acid and the wax are supplied into a coating device. In Step 2, the specific fatty acid and the wax are supplied onto the water-soluble granular fertilizer in a fluidized or tumbling state. When supplied into the coating device in Step 2, the specific fatty acid and the wax are preferably in liquid form. When Step 2 is performed, the water-soluble granular fertilizer is preferably maintained in a tumbling or fluidized state. Furthermore, when Step 2 is performed, it is preferable to heat the device in order to maintain the coating temperature, as in Step 1. The method for supplying the specific fatty acid and the wax is not particularly limited, and examples include, but are not limited to, a spraying method and a dropping method. Furthermore, the water-soluble granular fertilizer may contain any component (e.g., water, a solvent, various additives, etc.) as long as it can maintain the solid state of the water-soluble granular fertilizer and does not impair the compatibility between the specific fatty acid and the wax or the reactivity between the specific fatty acid and the metal hydroxide, which will be described later.

[0045] The specific fatty acid and the wax may be supplied independently, or may be supplied after some or all of the components have been mixed together in advance. When supplied independently, they may be supplied simultaneously, sequentially, or at different timings, with some of them being supplied simultaneously.

[0046] It is preferable that step 2 includes step 2a of supplying the specific fatty acid and wax to the surface of the water-soluble granular fertilizer. Step 2a and step 3 described below form a layer that is closest to the water-soluble granular fertilizer and contains the salt of the specific fatty acid and the wax. For example, when the coated fertilizer 1 in Fig. 1 is produced by method 1 including step 2a, the first layer L1 becomes a layer containing the salt of the specific fatty acid and the wax.

[0047] (Specific Fatty Acid) The specific fatty acid may be a fatty acid having 20 or more carbon atoms that can form the salt of the specific fatty acid described above and is liquid at the coating temperature. It is preferable to include a fatty acid having 21 or more carbon atoms, and more preferably a fatty acid having 31 or more carbon atoms. The upper limit of the number of carbon atoms in the specific fatty acid is not particularly limited, but may be, for example, 100 or less. The specific fatty acid may be a monobasic acid, a dibasic acid, or a tribasic acid, but preferably includes at least one of a dibasic acid and a tribasic acid. It is preferable to include at least one of a dimer acid and a trimer acid. It is preferable to include a fatty acid having at least one of a branched structure and a cyclic structure. The specific fatty acid may be a saturated fatty acid or an unsaturated fatty acid. It is preferable to include an aliphatic carboxylic acid having 20 or more carbon atoms. It is preferable to include a vegetable fatty acid having 20 or more carbon atoms.

[0048] As the specific fatty acid, known saturated fatty acids or conjugated fatty acids having 20 or more carbon atoms can be suitably used. Commercially available products may be used, or the specific fatty acids may be synthesized by known methods. Specific examples of commercially available products of the specific fatty acids include SB-20, IPU-22, and IPS-22 (all manufactured by Okamura Oil Mills), Cyclocarboxypropyloleic acid (manufactured by ALFA Chemistry), Tsunodym 205, and Tsunodym 346 (both manufactured by Tsuno Oleochemicals), and the like. In addition, examples of vegetable fatty acids include those obtained by modifying oleic acid, linoleic acid, linolenic acid, erucic acid, dehydrated condensed castor oil fatty acid, etc. so that the number of carbon atoms is 20 or more, or by dimerization or trimerization.

[0049] (Step 3) Step 3 will now be described. In Step 3, a metal hydroxide is supplied into a coating apparatus, and the specific fatty acid and the metal hydroxide are reacted to generate a salt of the specific fatty acid, thereby forming a layer containing the salt of the specific fatty acid and wax. When supplied into the coating apparatus in Step 3, the metal hydroxide is preferably in powder form. Furthermore, if the metal hydroxide is in powder form, it is preferable that the water content and particle shape be adjusted to a degree that does not impair the reactivity between the specific fatty acid and the metal hydroxide. For example, in the coating apparatus prior to the reaction of the specific fatty acid with the metal hydroxide, the water content may be 50% by mass or less, more preferably 0.1 to 30% by mass, of the total mass of the specific fatty acid, wax, and metal hydroxide used in Step 3, taken as 100. When Step 3 is performed, it is desirable that the water-soluble granular fertilizer be maintained in a rolling or fluidized state. Furthermore, when Step 3 is performed, as in Step 1, it is preferable that the apparatus be heated to maintain the coating temperature. The method for supplying the metal hydroxide is not particularly limited. For example, when the metal hydroxide is a liquid, the spraying method or the dropping method can be used, as in step 2. When the metal hydroxide is a solid, the method can include, but is not limited to, a method of mechanically supplying the metal hydroxide while dispersing it (mechanical method) or a method of supplying the metal hydroxide together with a gas (airflow method). The metal hydroxide can be supplied all at once, or can be supplied successively over a predetermined time period. Alternatively, the metal hydroxide can be supplied in portions at predetermined time intervals.

[0050] (Metal Hydroxide) The metal hydroxide preferably contains at least one hydroxide of an alkali metal and an alkaline earth metal, and more preferably contains at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, and magnesium hydroxide. Furthermore, as mentioned above, calcium hydroxide is more preferably used because of its favorable reaction with the specific fatty acid. The mass ratio of the metal hydroxide used in step 3 to the specific fatty acid used in step 2 (mass of metal hydroxide / mass of specific fatty acid) is preferably 10 / 1 to 0.5 / 1, and more preferably 5 / 1 to 1 / 1.

[0051] After step 3, it is preferable to further perform step 2 and step 3 one or more times each. It is preferable to perform four or more cycles, with step 2 and step 3 being performed once in this order as one cycle. For example, when the coated fertilizer 1 of FIG. 1 is produced by method 1, which performs four cycles, with step 2 and step 3 being performed once in this order as one cycle, the first layer L1, the second layer L2, the third layer L3, and the fourth layer L4 all contain a salt of a specific fatty acid and a wax. Furthermore, even in method 1, at least one of step a and step b of method 2 may be performed one or more times after step 1, as long as it does not significantly affect various properties such as the blocking defect rate and the non-defective product rate.

[0052] Next, we will explain Method 2. Step 1 is the same as Step 1 of Method 1 described above.

[0053] (Step a) The above-mentioned step a will be explained. In step a, a specific fatty acid and a metal hydroxide are supplied into a coating device, and the specific fatty acid and the metal hydroxide are reacted to generate a salt of the specific fatty acid, thereby forming layer A. Layer A is one of the layers constituting the coating film. By step a, layer A containing a salt of the specific fatty acid is formed on the water-soluble granular fertilizer in a fluidized or tumbling state. When supplied into the coating device in step a, the specific fatty acid is preferably in a liquid state. When performing step a, it is preferable that the water-soluble granular fertilizer be maintained in a tumbling or fluidized state. Furthermore, when performing step a, it is preferable that the inside of the device be heated to maintain the coating temperature, as in step 1. The method of supplying the specific fatty acid and the method of supplying the metal hydroxide may be the same as in steps 2 and 3 described above. Furthermore, when the metal hydroxide is a powder, it is preferable that the moisture content and particle shape be adjusted to an extent that does not impair the reactivity between the specific fatty acid and the metal hydroxide. For example, in the coating device prior to the reaction between the specific fatty acid and the metal hydroxide, when the total mass of the specific fatty acid and the metal hydroxide used in step a is taken as 100, the water content may be 60% by mass or less, more preferably in the range of 0.2 to 40% by mass. Furthermore, the specific fatty acid and the metal hydroxide may be supplied independently. When supplied independently, they may be supplied simultaneously, sequentially, or with staggered supply start times, so that they may be supplied partially simultaneously. Furthermore, from the viewpoint of ease of coating, it is preferable to start supplying the metal hydroxide at least after the supply of the specific fatty acid has begun. The specific fatty acid and the metal hydroxide are as described above.

[0054] (Step b) The above step b will be explained. In step b, wax and metal hydroxide are supplied into a coating device, the wax is solidified, and layer B is formed on the surface of layer A. When supplied into the coating device in step b, the wax is preferably in a liquid state. When performing step b, the water-soluble granular fertilizer is preferably maintained in a rolling or fluidized state. Furthermore, when performing step b, it is preferable to heat the inside of the device to maintain the coating temperature, as in step 1. The method of supplying the wax may be the same as in step 3 described above. The method of supplying the metal hydroxide may be the same as in step a described above. The wax and the metal hydroxide may be supplied independently. When supplied independently, the timing of supply may be simultaneous, or they may be supplied sequentially, or they may be supplied partially simultaneously by staggering the timing of supply start. Furthermore, from the viewpoint of ease of coating, it is preferable to start supplying the metal hydroxide at least after the start of supplying the wax. The wax and the metal hydroxide are as described above.

[0055] After step b, it is preferable to further perform step a and step b at least once each. It is preferable to perform four or more cycles, with step a and step b being performed once in this order as one cycle. For example, when the coated fertilizer 1 of FIG. 1 is produced by method 2, which performs two cycles, with step a and step b being performed once in this order as one cycle, the first layer L1 and the third layer L3 become layers containing a salt of a specific fatty acid (layer A), and the second layer L2 and the fourth layer L4 become layers containing a wax (layer B). Furthermore, in method 2, after step 1, at least one of step 2 and step 3 of method 1 may be performed once or more.

[0056] After the above-mentioned methods 1 and 2, the rolling or fluidizing state may be further maintained to dry the coating surface or promote the reaction of the unreacted specific fatty acid. At this time, the heating inside the coating apparatus may be stopped and the temperature may be lowered to the desired temperature.

[0057] 4. Fertilizer Coating Composition The fertilizer coating composition of the present disclosure will be described below. The fertilizer coating composition of the present disclosure contains a salt of a fatty acid having 20 or more carbon atoms and a wax. The salt of the fatty acid having 20 or more carbon atoms (the salt of the specific fatty acid) and the wax are as described above. A preferred form of the fertilizer coating composition is a coating that covers the fertilizer, and a coating that covers the surface of a water-soluble granular fertilizer is particularly preferred.

[0058] 5. Measurement and Evaluation Methods The measurement and evaluation methods for each evaluation item for the coated fertilizer are shown below. The same methods were used for the non-defective rate and initial dissolution of the coated fertilizer in a mixed fertilizer prepared by mixing the coated fertilizer with other fertilizers.

[0059] (Blocking Defect Rate) Approximately 15 g of particles are randomly taken from the produced coated fertilizer, and the total mass is measured. Next, blocking particles are removed from the taken particles, and the total mass of the blocking particles is measured. From the obtained value, the ratio (mass%) of the total mass of the blocking particles to the total mass is calculated, and this is taken as the blocking defect rate.

[0060] (Quality Rate) Approximately 10 g of particles were randomly taken from the produced coated fertilizer, and the total mass was measured. Next, the taken particles were placed in 150 ml of ion-exchanged water, and ultrasonic vibrations were applied for 5 minutes using an ultrasonic cleaner. Undissolved coated fertilizer was then selected, dried at 60°C for 2 hours or more, and then its mass was measured. From the obtained value, the ratio (mass%) of the total mass of the undissolved coated fertilizer to the total mass was calculated, and this was taken as the quality rate.

[0061] (Dissolution Rate) In this specification, the dissolution rate of the fertilizer component of a water-soluble granular fertilizer is determined by measuring the mass of the fertilizer component dissolved after a predetermined number of days in the following dissolution test, and calculating the ratio to the mass of the fertilizer component before the start of the dissolution test. First, 12.5 g of the reduced coated fertilizer is taken and placed in 250 ml of ion-exchanged water, and stored in a thermostatic chamber at 25°C. Next, after a predetermined number of days has passed, the coated fertilizer is removed, and the amount of the fertilizer component dissolved in the water is quantified, and the dissolution rate is calculated. When the fertilizer component is urea, the quantification is performed using a total nitrogen analyzer.

[0062] (Fertilizer moisture permeability) Approximately 10 g of particles are randomly taken from the urea-coated fertilizer, and the total mass is measured. Next, the taken-out particles are left to stand in a constant temperature and humidity chamber at 40°C and a relative humidity of 90% RH. After 24 hours, the coated fertilizer is taken out and the total mass is measured. The fertilizer moisture permeability is calculated from the obtained value and the surface area of ​​the coated fertilizer.

[0063] (Hardness) The hardness of the coated fertilizer of the present disclosure is not particularly limited, and may be, for example, 1 to 10 kgf or 3 to 8 kgf.

[0064] (Angle of Repose) The angle of repose of the coated fertilizer of the present disclosure is not particularly limited, and may be, for example, 20 to 40° or 30 to 40°.

[0065] (Bulk Density) The loose bulk density of the coated fertilizer of the present disclosure is not particularly limited, and is, for example, 0.1 to 2 g / cm 3 and 0.5 to 1.5 g / cm 3 The bulk density of the coated fertilizer of the present disclosure is not particularly limited, and may be, for example, 0.1 to 2 g / cm 3 and 0.5 to 1.5 g / cm 3 may be.

[0066] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples.

[0067] [Materials Used] Materials used in preparing the coated fertilizers of the Examples and Comparative Examples will be described.

[0068] <Water-soluble granular fertilizer> Urea with a particle size of 2.0 mm to 4.0 mm was used.

[0069] <Specific Fatty Acid 1> Cyclocarboxylic propyloleic acid (containing the largest amount of linoleic acid acrylic acid adduct (dimeric acid having a ring structure (21 carbon atoms))) manufactured by ALFA chemistry was used.

[0070] <Specific Fatty Acid 2> Tsunodyme 205 (having a branched structure and containing the largest amount of dimer acid (36 carbon atoms) of unsaturated fatty acid) manufactured by Tsuno Oleochemicals was used.

[0071] <Specific Fatty Acid 3> Tsunodim 346 (having a branched structure and containing the largest amount of unsaturated fatty acid trimer acid (54 carbon atoms)) manufactured by Tsuno Oleochemicals was used.

[0072] <C18 Fatty Acid> TFA-45 (containing the largest amount of linear unsaturated fatty acid monomers (18 carbon atoms)) manufactured by Tsuno Oleochemicals was used.

[0073] <C10 Fatty Acid> Sebacic acid (a dicarboxylic acid having 10 carbon atoms) was used.

[0074] <Wax> Paraffin wax (melting point: 50°C) manufactured by Nippon Seiro was used.

[0075] <Metal hydroxide> Fine particle slaked lime M-300 manufactured by Inoue Mitsuyoshi Shoten was used.

[0076] Example 1 In Example 1, a coated fertilizer was produced by the aforementioned method 1, as described in detail below. Water-soluble granular fertilizer (250 g) was loaded into a drum-type tumbling coating device with a diameter of 300 mm, and while the device was being tumbling at 25 rpm (rotations per minute), the temperature inside the coating device was maintained at 70°C using a hot air generator (Step 1). Next, while maintaining the tumbling state, a liquid mixture of specific fatty acid 1 (0.67 g) and wax (0.33 g) was prepared and dripped into the device through the supply port (Step 2a). Next, while maintaining the tumbling state, after 3 minutes, metal hydroxide (2.40 g) was supplied into the device, and the tumbling state was maintained for 3 minutes (Step 3). By Step 3, the metal hydroxide and the specific fatty acid reacted to form a solidified layer on the surface of the water-soluble granular fertilizer. The following constituted one cycle, and 13 cycles were repeated. (1 cycle) While maintaining the rolling state, a mixture of specific fatty acid 1 (0.67 g) and wax (0.33 g) was dropped into the device through the supply port (step 2), and after 3 minutes, metal hydroxide (2.40 g) was supplied into the device and the rolling state was maintained for 3 minutes (step 3). Next, after rolling for 6 minutes, the device was gradually cooled to room temperature (approximately 25°C) to obtain a coated fertilizer.

[0077] Example 2 In Example 2, a coated fertilizer was produced by the above-described Method 2, as described in detail below. Water-soluble granular fertilizer (250 g) was charged into a drum-type tumbling coating device with a diameter of 300 mm, and while the device was being tumbling at 25 rpm (rotations per minute), the temperature inside the coating device was maintained at 70°C using a hot air generator (Step 1). Next, while maintaining the tumbling state, specific fatty acid 1 (0.67 g) and metal hydroxide (2.29 g) were prepared, and specific fatty acid 1 was added dropwise into the device through a supply port. After tumbling for 3 minutes, the metal hydroxide was added through a separate supply port, and the tumbling state was maintained for 3 minutes to obtain Layer A (Step a). Next, while maintaining the rolling state, wax (0.33 g) was dropped into the device and rolled for 3 minutes, after which metal hydroxide (0.11 g) was fed into the device through a separate feed port and the rolling state was maintained for 3 minutes to obtain Layer B (Step b). Next, the following constitutes one cycle, and 13 cycles were repeated. (1 cycle) While maintaining the rolling state, specific fatty acid 1 (0.67 g) was dropped into the device through the feed port and rolled for 3 minutes, after which metal hydroxide (2.29 g) was added into the device through a separate feed port and the rolling state was maintained for 3 minutes to form Layer A (Step a), wax (0.33 g) was dropped into the device and rolled for 3 minutes, after which metal hydroxide (0.11 g) was fed into the device through a separate feed port and the rolling state was maintained for 3 minutes to obtain Layer B (Step b). Next, after rolling for 6 minutes, the device was slowly cooled to room temperature (approximately 25°C) to obtain a coated fertilizer.

[0078] [Example 3] A coated fertilizer was obtained in the same manner as in Example 1, except that specific fatty acid 2 was used as the specific fatty acid. Furthermore, the hardness, angle of repose, and bulk density of the coated fertilizer of Example 3 were measured.

[0079] (Hardness) The hardness of 10 coated fertilizer grains was measured using a Kiya hardness tester, and the average value was calculated. The results are shown in Table 1 below.

[0080]

[0081] (Angle of Repose) The angle of repose of the coated fertilizer was measured three times in accordance with "JIS R 9301-2-2:1999 Alumina powder - Part 2: Measurement of physical properties - 2: Angle of repose" and the average value was calculated. The results are shown in Table 2 below.

[0082]

[0083] (Bulk Density) The bulk density of the coated fertilizer was measured three times in accordance with "JIS R 1628:1997 Method for measuring bulk density of fine ceramic powders," and the average value was calculated. The results are shown in Table 3 below.

[0084]

[0085] Example 4 A coated fertilizer was obtained in the same manner as in Example 2, except that specific fatty acid 2 was used as the specific fatty acid.

[0086] Example 5 A coated fertilizer was obtained in the same manner as in Example 1, except that specific fatty acid 3 was used as the specific fatty acid.

[0087] Comparative Example 1 In Comparative Example 1, a coated fertilizer was produced by the method described in detail below. Although a fatty acid having 20 or more carbon atoms was not used in Comparative Example 1, the terms "method 1," "step 2a," "step 2," and "step 3" were used for convenience in Comparative Example 1. The same applies to Comparative Example 2, which will be described later. A water-soluble granular fertilizer (250 g) was charged into a drum-type tumbling coating device with a diameter of 300 mm, and while rolling at 25 rpm (rotations per minute), the temperature of the particles was maintained at 70°C using a hot air generator (step 1). Next, while maintaining the rolling state, a mixture of C18 fatty acid (0.67 g) and wax (0.33 g) was prepared and dropped into the device through the supply port (step 2a). Next, while maintaining the rolling state, after 3 minutes, a metal hydroxide (2.40 g) was supplied into the device, and the rolling state was maintained for 3 minutes (step 3). In step 3, the metal hydroxide and the C18 fatty acid reacted to form a solidified layer on the surface of the water-soluble granular fertilizer. Next, the following constituted one cycle, and 13 cycles were repeated. (1 cycle) While maintaining the tumbling state, a mixture of C18 fatty acid (0.67 g) and wax (0.33 g) was dripped into the device through the supply port (step 2). After 3 minutes, metal hydroxide (2.40 g) was supplied into the device, and the tumbling state was maintained for 3 minutes (step 3). Since agglomerates formed after step 2, the tumbling device was stopped each time they were formed, manually crushed, and the tumbling state was resumed, and step 3 was performed. Next, after tumbling for 6 minutes, the mixture was slowly cooled to room temperature (approximately 25°C), and a coated fertilizer was obtained.

[0088] Comparative Example 2: Water-soluble granular fertilizer (250 g) was placed in a drum-type tumbling coating device with a diameter of 300 mm, and while rolling at 25 rpm (rotations per minute), the temperature of the particles was maintained at 70°C using a hot air generator (Step 1). Next, while maintaining the rolling state, C10 fatty acid (0.67 g) and wax (0.33 g) were mixed, but they were not compatible. Therefore, they were prepared separately and dropped into the device from separate supply ports (Step 2a). However, after dropping, the C10 fatty acid immediately crystallized in the device, and it was determined that coating was impossible, so the coating was stopped. Therefore, no coated fertilizer was obtained.

[0089] [Comparative Example 3] Water-soluble granular fertilizer (250 g) was placed in a drum-type rolling coating device with a diameter of 300 mm, and while rolling at 25 rpm (rotations per minute), the temperature of the particles was maintained at 70 ° C. using a hot air generator. Next, while maintaining the rolling state, specific fatty acid 2 (1.0 g) and metal hydroxide (2.40 g) were prepared, and specific fatty acid 2 was dropped into the device through a supply port. After rolling for 3 minutes, the metal hydroxide was added through another supply port, and the rolling state was maintained for 3 minutes to obtain a layer. Next, the above-mentioned layer-obtaining process was repeated 6 times to form a layer. Blocking particles consisting of approximately 2 to 5 particles integrated together were visually confirmed among the rolling particles, so the rolling state was stopped, and the coating was stopped. The blocking defect rate of the obtained particles was measured and found to be greater than 20%.

[0090] [Various measurements and evaluations]

[0091] (Lumps) Lumps were evaluated according to the following criteria. ◯: The coated fertilizer did not form lumps, the rolling state could be maintained, and no crushing treatment was required. ×: The coated fertilizer formed lumps, it was difficult to maintain the rolling state, and crushing treatment was required.

[0092] (Blocking Defect Rate) Approximately 15 g of particles were randomly taken from the produced coated fertilizer, and the total mass was measured. Next, blocking particles were removed from the taken particles, and the total mass of the blocking particles was measured. From the obtained value, the ratio (mass%) of the total mass of the blocking particles to the total mass was calculated, and this was taken as the blocking defect rate.

[0093] (Quality Rate) Approximately 10 g of particles were randomly taken from the produced coated fertilizer, and the total mass was measured. Next, the taken particles were placed in 150 ml of ion-exchanged water, and ultrasonic vibrations were applied for 5 minutes using an ultrasonic cleaner. Thereafter, undissolved coated fertilizer was selected, dried at 60°C for 2 hours or more, and then its mass was measured. From the obtained value, the ratio (mass%) of the total mass of the undissolved coated fertilizer to the total mass was calculated, and this was taken as the quality rate.

[0094] (Initial Dissolution) 12.5 g of the reduced coated fertilizer was taken and placed in 250 ml of ion-exchanged water, and stored in a thermostatic chamber at 25°C. Next, after 3 days had passed, the coated fertilizer was removed, and the amount of fertilizer components dissolved in the water was quantified, and the dissolution rate was calculated. The quantification was carried out using a total nitrogen analyzer. Evaluation was based on the following criteria: ◎: Dissolution rate from the start of dissolution to 3 days was less than 10%. ○: Dissolution rate from the start of dissolution to 3 days was 10% or more but less than 40%. △: Dissolution rate from the start of dissolution to 3 days was 40% or more but less than 70%. ×: Dissolution rate from the start of dissolution to 3 days was 70% or more.

[0095] (80% Dissolution) 12.5 g of the reduced coated fertilizer was taken and placed in 250 ml of ion-exchanged water and stored in a thermostatic chamber at 25°C. Next, the amount of fertilizer active ingredients dissolved in the water was quantified every specified number of days, and the dissolution rate was calculated. This was continued until the dissolution rate reached 80% or more, and the number of days required for the dissolution rate to reach 80% was calculated from a plot of the dissolution rate against the number of days elapsed. The above quantification was performed using a total nitrogen analyzer.

[0096] (Fertilizer moisture permeability) Approximately 10 g of particles were randomly taken out from the produced coated fertilizer, and the total mass was measured. Next, the taken-out particles were left to stand in a constant temperature and humidity chamber at 40°C and 90% RH. After 24 hours, the coated fertilizer was taken out, and the total mass was measured. The fertilizer moisture permeability was calculated from the obtained value and the surface area of ​​the coated fertilizer. The surface area was calculated assuming that the coated fertilizer was a sphere with a diameter of 3 mm.

[0097] The results are shown in Table 4 below. In the table, "ND" indicates that the measurement was not performed.

[0098]

[0099] In none of the examples were lumps observed during the manufacturing process, and the blocking defect rate of the resulting coated fertilizers was 10% or less, indicating that stacking faults did not occur. Furthermore, the yield rate of the coated fertilizers was 52% or higher. On the other hand, in Comparative Example 1, which contained the highest amount of fatty acid salt with 18 carbon atoms as the fatty acid salt, lumps occurred each time the next layer of coating material was added. Furthermore, when sebacic acid with 10 carbon atoms was used as the fatty acid, it was incompatible with the wax, and the fatty acid crystallized immediately after addition, so the coating itself was abandoned. Furthermore, in Comparative Example 3, in which no wax was used, a large number of blocking particles were observed when the seventh layer was formed, indicating the occurrence of stacking faults. From the above, the coated fertilizers of the present disclosure can suppress stacking faults. Furthermore, since it is easy to increase the number of layers and the coverage rate, further improvements in the yield rate, fertilizer moisture permeability, and initial dissolution can be expected.

[0100] Furthermore, it was found that Examples 3 to 5, which contained a salt of a fatty acid having 31 or more carbon atoms in the coating, had a non-defective product rate of 72% or more, and were able to suppress initial elution to ◎ (less than 10%), ◯ (10% or more and less than 40%), or ◯ (40% or more and less than 70%). Furthermore, Examples 3 and 5 obtained using Method 1 achieved initial elution of ◎ or ◯. It was also found that it took more than 70 days for the elution rate to reach 80% in Examples 3 and 5.

[0101] In addition, Examples 1, 3, and 5 obtained by Method 1 have a fertilizer moisture permeability of 49 g / (m 2 -24h) or less. When Example 2 (the specific fatty acid used as the raw material is the same as in Example 1) and Example 4 (the specific fatty acid used as the raw material is the same as in Example 3) obtained by Method 2 were compared with Examples 1 and 3 obtained by Method 1, it was found that when the specific fatty acid used as the raw material was the same, the coated fertilizers obtained by Method 1 in both cases had a lower blocking defect rate, a higher yield rate, a lower fertilizer moisture permeability, and a lower initial leaching. Furthermore, the time required for film formation using Method 1 in Examples 1, 3, and 5 was approximately 90 minutes, while the time required for film formation using Method 2 in Examples 2 and 4 was approximately 174 minutes, demonstrating that Method 1 can shorten the film formation time.

[0102] [Preparation of Blended Fertilizer] A blended fertilizer was prepared by mixing the coated fertilizer of Example 3 / other fertilizers at a mass ratio of 3 / 7 using a two-axis roller at 100 rpm for 10 minutes. Specific examples of the other fertilizers used were "Granular Composite No. 888" (Central Chemical Co., Ltd.), "Kumiai Nitrogen Potassium Chemical C-26" (Central Chemical Co., Ltd.), "Magnesium Chloride Phosphate Ammonium 532" (Central Chemical Co., Ltd.), and Magnesium Phosphate Ammonium (Central Chemical Co., Ltd.). Observation of the prepared blended fertilizer revealed that the coated fertilizer and other fertilizers were thoroughly mixed. The coated fertilizer was removed from the prepared blended fertilizer, and the yield rate and initial dissolution were measured and evaluated using the methods described above. The results are shown in Table 5 below.

[0103]

[0104] The results shown in Table 5 reveal that the coated fertilizer of Example 3 had a high yield and could suppress the initial elution to ⊚ (less than 10%) even when mixed with other fertilizers of various hardness to prepare a compound fertilizer.

[0105] According to the present disclosure, a coated fertilizer in which stacking defects are suppressed can be provided.

[0106] Although the present disclosure has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present disclosure. This application is based on Japanese patent applications filed on April 28, 2023 (Patent Application No. 2023-74671) and June 16, 2023 (Patent Application No. 2023-99249), the contents of which are incorporated herein by reference.

Claims

1. A coated fertilizer comprising a water-soluble granular fertilizer and a coating covering the water-soluble granular fertilizer, the coating containing a salt of a fatty acid having 20 or more carbon atoms and a wax.

2. The coated fertilizer according to claim 1, wherein the salt of a fatty acid includes a salt of a fatty acid having 31 or more carbon atoms.

3. The coated fertilizer according to claim 1 or 2, wherein the salt of the fatty acid includes at least one of a salt of a dimer acid and a salt of a trimer acid.

4. The coated fertilizer according to claim 1 or 2, wherein the salt of a fatty acid includes a salt of a fatty acid having at least one of a branched structure and a cyclic structure.

5. The coated fertilizer according to claim 1 or 2, wherein the wax comprises at least one of a petroleum-based wax and a vegetable-based wax.

6. The coated fertilizer according to claim 1 or 2, wherein the coating is composed of at least one layer, and has at least one layer containing the salt of the fatty acid and the wax.

7. The coated fertilizer according to claim 1 or 2, wherein the coating is composed of at least one layer, and the layer closest to the water-soluble granular fertilizer contains the salt of the fatty acid and the wax.

8. The coated fertilizer according to claim 1 or 2, wherein the coating is composed of at least four layers, and at least four layers contain the salt of the fatty acid and the wax.

9. The fertilizer moisture permeability of the coating at 40°C is 52 g / (m 2 The coated fertilizer according to claim 1 or 2, wherein the drying time is 24 h or less.

10. The coated fertilizer according to claim 1 or 2, wherein the coating does not contain a resin.

11. A method for producing a coated fertilizer comprising a water-soluble granular fertilizer and a coating covering the water-soluble granular fertilizer, the method comprising forming a coating containing a salt of a fatty acid having 20 or more carbon atoms and a wax on the water-soluble granular fertilizer.

12. The method for producing a coated fertilizer according to claim 11, wherein the coating has at least one layer containing the salt of the fatty acid and the wax, and the following steps 1 to 3 are carried out in this order: Step 1: A step of bringing the water-soluble granular fertilizer into a fluidized or rolling state in a coating device, Step 2: A step of supplying a fatty acid having 20 or more carbon atoms and a wax into the coating device, and Step 3: A step of supplying a metal hydroxide into the coating device, reacting the fatty acid with the metal hydroxide to generate a salt of a fatty acid having 20 or more carbon atoms, and forming a layer containing the salt of the fatty acid and the wax.

13. The method for producing a coated fertilizer according to claim 12, wherein after step 3, steps 2 and 3 are each carried out one or more times.

14. The method for producing a coated fertilizer according to claim 12 or 13, wherein step 2 includes step 2a of supplying the fatty acid and the wax to the surface of the water-soluble granular fertilizer.

15. The method for producing a coated fertilizer according to claim 12 or 13, wherein step 2 and step 3 are performed once in this order as one cycle, and the method comprises performing four or more cycles.

16. The method for producing a coated fertilizer according to claim 12 or 13, wherein the fatty acid includes a fatty acid having 31 or more carbon atoms.

17. The method for producing a coated fertilizer according to claim 12 or 13, wherein the fatty acid includes at least one of a dimer acid and a trimer acid.

18. A composition for coating a fertilizer, comprising a salt of a fatty acid having 20 or more carbon atoms and a wax.

19. The fertilizer coating composition of claim 18, wherein the salt of a fatty acid comprises a salt of a fatty acid having 31 or more carbon atoms.

20. The fertilizer coating composition of claim 18 or 19, wherein the salt of a fatty acid comprises at least one of a salt of a dimer acid and a salt of a trimer acid.

21. A compound fertilizer comprising the coated fertilizer according to claim 1 or 2 and another fertilizer.

22. The compound fertilizer according to claim 21, wherein the other fertilizer is at least one selected from the group consisting of highly chemical fertilizers, nitrogenous fertilizers, phosphorus fertilizers, potassium fertilizers, organic fertilizers, silicate fertilizers and magnesium fertilizers.

Citation Information

Patent Citations

  • Game machine

    JP2023074671A

  • Wire discharge machining device and wire discharge machining method

    JP2023099249A

  • Polyurethane coated controlled-release fertilizer and preparation method thereof

    CN111423281A

  • Sulfur coated fertilizer having improved coating film strength and method of manufacturing the same

    JP2007084414A

  • Coated granular material

    JP2009242195A