Light-emitting semiconductor element and method for manufacturing same

By implementing a compositionally graded layer with decreasing bandgap energy and varying n-type impurity concentrations in semiconductor light emitting devices, the issue of increased operating voltage is addressed, resulting in improved performance and reduced optical loss.

WO2024225306A1PCT designated stage expired Publication Date: 2024-10-31NICHIA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016038
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Semiconductor light emitting devices with nitride semiconductors face increased operating voltage due to electron movement inhibition at the interface between the n-side cladding and waveguide layers when Al composition is altered, leading to conductivity issues and increased voltage requirements.

Method used

Incorporating a compositionally graded layer with a decreasing bandgap energy and a second semiconductor layer with varying n-type impurity concentrations, including a high concentration region, to reduce band barriers and operating voltage, while minimizing optical loss.

Benefits of technology

The solution effectively reduces operating voltage and optical loss by smoothing the band barrier at the hetero interface and optimizing n-type impurity distribution, enhancing the semiconductor light emitting device's performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016038_31102024_PF_FP_ABST
    Figure JP2024016038_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A light-emitting semiconductor element (100) includes a nitride-semiconductor stack (10) comprising: a first semiconductor layer (21) that contains an n-type impurity; a composition gradient layer (23) that contains an n-type impurity and is formed on the first semiconductor layer (21) and that has a band gap energy which decreases as the distance from the first semiconductor layer (21) increases; and a second semiconductor layer (22) that contains an n-type impurity and is formed on the composition gradient layer (23) and that has a lower band gap energy than the first semiconductor layer (21). At least some of the composition gradient layer (23) contains the n-type impurity in a first concentration, at least some of the second semiconductor layer (22) contains the n-type impurity in a second concentration, and the composition gradient layer (23) and / or the second semiconductor layer (22) includes a high-concentration region (233) in which the n-type impurity is contained in a third concentration, higher than the first concentration and the second concentration. Such a configuration makes it possible to provide a light-emitting semiconductor element (100) having an operating voltage that can be reduced effectively, and to provide a method for manufacturing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor light emitting device and method for manufacturing the same

[0001] The present invention relates to a semiconductor light-emitting element and a method for manufacturing the same.

[0002] Semiconductor light-emitting devices containing nitride semiconductors that emit light ranging from ultraviolet to green are used in a wide variety of applications, such as light sources for optical discs. Known examples of such semiconductor light-emitting devices include an n-side cladding layer, an n-side waveguide layer, an active layer, a p-side waveguide layer, and a p-side cladding layer, arranged in this order on a substrate (see, for example, Patent Document 1). Furthermore, the Al composition may be varied between the n-side cladding layer and the n-side waveguide layer, for example, to control conductivity.

[0003] Japanese Patent Application Laid-Open No. 2021-111785

[0004] However, if the Al composition in the n-side cladding layer and the n-side waveguide layer is changed, the movement of electrons at the interface between the n-side cladding layer and the n-side waveguide layer may be hindered, resulting in an increase in the operating voltage.

[0005] The semiconductor light-emitting element of the present disclosure comprises a nitride semiconductor stack having: a first semiconductor layer containing an n-type impurity; a compositionally graded layer containing the n-type impurity and formed on the first semiconductor layer, the bandgap energy of which decreases with increasing distance from the first semiconductor layer; and a second semiconductor layer containing the n-type impurity and formed on the compositionally graded layer, the second semiconductor layer having a smaller bandgap energy than the first semiconductor layer, wherein at least a portion of the compositionally graded layer contains the n-type impurity at a first concentration, and at least a portion of the second semiconductor layer contains the n-type impurity at a second concentration, and at least one of the compositionally graded layer and the second semiconductor layer includes a high-concentration region containing the n-type impurity at a third concentration higher than the first concentration and the second concentration. The method for manufacturing a semiconductor light-emitting element according to the present disclosure includes, in this order: forming a first semiconductor layer containing an n-type impurity; forming a compositionally graded layer containing an n-type impurity and having a band gap energy that decreases with increasing distance from the first semiconductor layer; and forming a second semiconductor layer containing an n-type impurity and having a band gap energy smaller than that of the first semiconductor layer; in the step of forming the compositionally graded layer, the n-type impurity is doped at least in part to the compositionally graded layer at a first concentration; in the step of forming the second semiconductor layer, the n-type impurity is doped at least in part to the second semiconductor layer at a second concentration; and in at least one of the steps of forming the compositionally graded layer and forming the second semiconductor layer, the n-type impurity is doped in at least one of the compositionally graded layer and the second semiconductor layer at a third concentration that is higher than the first concentration and the second concentration.

[0006] According to the embodiments of the present disclosure, it is possible to provide a semiconductor light emitting device that can effectively reduce the operating voltage and a method for manufacturing the same.

[0007] 1 is a schematic cross-sectional view showing the structure of a portion of a semiconductor light-emitting device according to an embodiment of the present invention. FIG. 2 is a schematic cross-sectional view showing the structure of a portion of a nitride semiconductor stack in the semiconductor light-emitting device of FIG. 1. FIG. 3 is a schematic cross-sectional view showing another structure of a portion of the nitride semiconductor stack in the semiconductor light-emitting device of FIG. 1. FIG. 4 is a schematic cross-sectional view showing a semiconductor light-emitting device according to an embodiment. FIG. 5 is a graph showing the current density-voltage (J-V) characteristics of a semiconductor light-emitting device in an example and a semiconductor light-emitting device in a comparative example. FIG. 6 is a graph showing the results of a simulation of a band diagram of the conduction band in an example of a semiconductor light-emitting device. FIG. 7 is a schematic diagram showing an example of changes in the molar ratio of Al to the sum of Al and Ga and the Si concentration for each layer in a portion of a semiconductor light-emitting device according to an embodiment. "Al" represents the molar ratio of Al to the sum of Al and Ga, and "Si" represents the Si concentration.

[0008] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the embodiments shown below are merely examples for embodying the technical concept of the present invention and are not intended to limit the present invention. The size and positional relationship of components shown in each drawing may be exaggerated for clarity. An end view showing only the cut surface may be used as a cross-sectional view. In principle, the same names and symbols indicate components that are the same or of the same quality, and redundant explanations will be omitted as appropriate. In this specification, with respect to a semiconductor light-emitting device, the direction from the first semiconductor layer to the second semiconductor layer or the direction from the n-side semiconductor layer to the p-side semiconductor layer is referred to as "up" or "upper," and the opposite direction is referred to as "down" or "downward."

[0009] 1 , the semiconductor light-emitting element of the present disclosure includes a nitride semiconductor stack 10 including a first semiconductor layer 21 containing n-type impurities, a compositionally graded layer 23 containing n-type impurities and formed on the first semiconductor layer 21, the bandgap energy of which decreases with increasing distance from the first semiconductor layer 21, and a second semiconductor layer 22 containing n-type impurities and formed on the compositionally graded layer 23, the bandgap energy of which is smaller than that of the first semiconductor layer 21. At least a portion of the compositionally graded layer 23 contains n-type impurities at a first concentration. At least a portion of the second semiconductor layer 22 contains n-type impurities at a second concentration. At least one of the compositionally graded layer 23 and the second semiconductor layer 22 includes a high-concentration region 233 containing n-type impurities at a third concentration higher than the first and second concentrations. That is, only the second semiconductor layer 22 may include the high concentration region 233, only the composition gradient layer 23 may include the high concentration region 233, or both the composition gradient layer 23 and the second semiconductor layer 22 may include the high concentration region 233.

[0010] If the compositionally graded layer 23 is not provided between the first semiconductor layer 21 and the second semiconductor layer 22, a band barrier may occur at the heterointerface between the first semiconductor layer 21 and the second semiconductor layer 22, resulting in an increase in operating voltage. On the other hand, by providing the compositionally graded layer 23 between the first semiconductor layer 21 and the second semiconductor layer 22, the band barrier occurring at the heterointerface can be reduced, thereby reducing the operating voltage. Furthermore, by providing a region containing a high concentration of n-type impurities between the compositionally graded layer 23 and the second semiconductor layer 22, the operating voltage can be reduced. Furthermore, by providing a region containing a high concentration of n-type impurities, the n-type impurity concentration in the second semiconductor layer 22 can be relatively reduced, thereby reducing optical loss due to n-type impurities.

[0011] 1, the nitride semiconductor stack 10 further includes an active layer 3 and a p-side semiconductor layer 4 in this order on the n-side semiconductor layer 2 including the first semiconductor layer 21, the compositionally graded layer 23, and the second semiconductor layer 22. The types and materials of the n-side semiconductor layer 2, the active layer 3, and the p-side semiconductor layer 4 are not particularly limited, and may be, for example, a III-V group compound semiconductor, In X Al Y Ga 1-X-Y Examples of suitable nitride semiconductor materials include nitride semiconductor materials such as InN (0≦X, 0≦Y, X+Y≦1). Specifically, InN, AlN, GaN, InGaN, AlGaN, InGaAlN, and the like can be used. The thickness and structure of each layer can be those known in the art. Furthermore, as shown in FIG. 3, the semiconductor light-emitting device 100 including the nitride semiconductor stack 10 is preferably formed on a substrate 1. The substrate 1 may be any material that allows epitaxial growth of a semiconductor layer. Examples of materials that can be used for such a substrate include nitride semiconductor substrates made of GaN or sapphire. The substrate 1 may be, for example, a substrate having a C-plane (0001) as its principal surface. The principal surface of the substrate 1 may have an off-angle of, for example, within ±5 degrees. Using a substrate having a C-plane as its principal surface offers the advantage of excellent mass productivity.

[0012] (n-Side Semiconductor Layer 2) The n-side semiconductor layer 2 can have a multilayer structure having a first semiconductor layer 21, a compositionally graded layer 23, and a second semiconductor layer 22 in this order. In the n-side semiconductor layer 2, for example, the first semiconductor layer 21 can be an n-side cladding layer, and the second semiconductor layer 22 can be an n-side optical guide layer. The n-side semiconductor layer 2 contains n-type impurities such as Si and Ge. The concentration of the n-type impurities in the n-side semiconductor layer 2 is 1×10 16 cm -3 1x10 or more 21 cm -3 It can be set appropriately within the following range: 1 × 10 17 cm -3 1x10 or more 20 cm -3 It is preferable to set the concentration of n-type impurities within the following range: 17 cm -3By setting the concentration of the n-type impurity at 1×10 or more, the n-side semiconductor layer 2 can obtain good electrical conductivity. 20 cm -3 By setting the content below, it is possible to prevent light loss due to excessive n-type impurities. However, some of the layers constituting the n-side semiconductor layer 2 may not contain n-type impurities.

[0013] (First Semiconductor Layer 21) The first semiconductor layer 21 is preferably composed of, for example, an AlGaN layer, a GaN layer, an InGaN layer, and / or an InGaAlN layer. Among these, the first semiconductor layer 21 is preferably composed of an AlGaN layer. This configuration reduces the refractive index of the first semiconductor layer 21 and increases the reflectance of light from the compositionally graded layer 23 (described later). When the first semiconductor layer 21 includes a semiconductor layer containing Al, the molar ratio of Al to the total of Al and Ga can be 0.005 or more and 0.2 or less, and preferably 0.01 or more and 0.1 or less. By setting the molar ratio of Al to the total of Al and Ga to 0.01 or more, the refractive index of the first semiconductor layer 21 can be reduced and the reflectance of light from the compositionally graded layer 23 (described later). Furthermore, by setting the molar ratio of Al to the total of Al and Ga to 0.1 or less, the occurrence of cracks during crystal growth of the first semiconductor layer 21 can be suppressed. The first semiconductor layer 21 contains an n-type impurity. The n-type impurity may include, for example, Si. The concentration of the n-type impurity in the first semiconductor layer 21 is referred to as a fourth concentration, and the concentration is 1×10 18 cm -3 1x10 or more 19 cm -3 The following are listed: 2 x 10 18 cm -3 9x10 or more 18 cm -3 Preferably, it is 2 x 10 18 cm -3 By setting the ratio to the above, the first semiconductor layer 21 can obtain good electrical conductivity. 18 cm -3 By setting the thickness to the value below, optical loss due to n-type impurities can be reduced. The thickness of the first semiconductor layer 21 can be set appropriately, and may be, for example, 1000 nm or more and 10000 nm or less.

[0014] (Compositional Graded Layer 23) The compositional graded layer 23 contains n-type impurities and is disposed on the first semiconductor layer 21. The compositional graded layer 23 is composed of, for example, an AlGaN layer, a GaN layer, an InGaN layer, and / or an InGaAlN layer. In particular, when the first semiconductor layer 21 is composed of an AlGaN layer and the second semiconductor layer 22 (described later) is composed of a GaN layer, the compositional graded layer 23 is preferably composed of an AlGaN layer and / or a GaN layer. With this configuration, the band barrier from the first semiconductor layer 21 to the second semiconductor layer 22 can be reduced, and the operating voltage can be reduced. The band gap energy of the compositional graded layer 23 decreases with increasing distance from the first semiconductor layer 21. When the composition gradient layer 23 includes a semiconductor layer containing Al, the molar ratio of Al to the sum of Al and Ga can be, for example, in the range of 0.005 to 0.2. Within this range, the molar ratio of Al to the sum of Al and Ga decreases with increasing distance from the first semiconductor layer 21. For example, when the composition gradient layer 23 is formed of an AlGaN layer, the Al composition decreases with increasing distance from the first semiconductor layer 21. For example, the molar ratio of Al to the sum of Al and Ga can be decreased from a first molar ratio in the range of 0.005 to 0.2 to a second molar ratio in the range of 0 to 0.18 and smaller than the first molar ratio. Furthermore, for example, the molar ratio of Al to the sum of Al and Ga can be changed from a third molar ratio in the range of 0.06 to 0.1 to a fourth molar ratio in the range of 0 to 0.02. In this case, the decrease may be a stepwise monotonic decrease or a linear decrease. In this way, by changing the molar ratio of Al to the total of Al and Ga in the compositionally graded layer 23, the band barrier occurring at the heterointerface can be reduced, and the operating voltage can be reduced.

[0015] As long as the composition gradient layer 23 contains n-type impurities, the concentration of the n-type impurities may be the same or different throughout the entire region of the composition gradient layer 23. At least a portion of the composition gradient layer 23 contains the n-type impurities at a predetermined concentration, which is referred to as a first concentration. The first concentration is 1×10 18 cm -3 1x10 or more 19 cm -3 The following are listed: 2 x 1018 cm -3 9 x 10 or more 18 cm -3 Preferably, it is 2 x 10 18 cm -3 By setting the composition gradient layer 23 at 9×10 or more, good electrical conductivity can be obtained. 18 cm -3 By setting the concentration of n-type impurities at or below 1 / 2, it is possible to reduce optical loss due to n-type impurities. The first concentration may be different from the fourth concentration, for example, the first concentration may be smaller or larger than the fourth concentration. Furthermore, the first concentration may be the same as the fourth concentration.

[0016] A region containing n-type impurities at a third concentration that is relatively higher than the first concentration and the second concentration described below is referred to as a high concentration region 233. The third concentration is, for example, 1×10 18 cm -3 1x10 or more 20 cm -3 The third concentration may be 1×10 or less. 19 cm -3 1x10 or more 20 cm -3 By setting the third concentration in this range, the operating voltage can be reduced more effectively. 18 cm -3 1x10 or more 20 cm -3or less. By setting this concentration, the effect of reducing the operating voltage is significant. In particular, the third concentration is preferably greater than the first concentration, the second concentration, and the fourth concentration. By setting the third concentration to a high value, the Fermi level in the high-concentration region 233 shifts toward the conduction band, thereby reducing the operating voltage. Furthermore, even when the concentrations other than the third concentration are set to low values, setting the third concentration to a high value can lower the operating voltage. Therefore, the concentration of n-type impurities in regions containing n-type impurities at concentrations other than the third concentration can be reduced, thereby reducing optical loss due to the n-type impurities. The thickness of the high-concentration region 233 can be 0.1 nm to 10 nm, and preferably 0.1 nm to 5 nm. Setting the thickness of the high-concentration region 233 to 0.1 nm or more can further reduce the operating voltage. Furthermore, by setting the thickness of the high-concentration region 233 to 10 nm or less, the region where n-type impurities are present at a high concentration can be reduced, thereby reducing optical loss due to the n-type impurities. Furthermore, by setting the thickness of the high concentration region 233 to 5 nm or less, the effect of reducing optical loss becomes more pronounced.

[0017] The compositionally graded layer 23 may include a high-concentration region 233. The inclusion of the high-concentration region 233 in the compositionally graded layer 23 allows for a reduction in operating voltage. When the compositionally graded layer 23 includes an n-type impurity at a first concentration and includes the high-concentration region 233, the high-concentration region 233 is preferably a layered region. That is, within a predetermined plane of the compositionally graded layer 23, the n-type impurity concentration at any point is either the first concentration or the third concentration. The "predetermined plane" refers to a plane that grows simultaneously in the semiconductor layer. In other words, the "predetermined plane" refers to a plane parallel to the interface between the first semiconductor layer 21 and the compositionally graded layer 23. By including the high-concentration region 233 as a layered region, the n-type impurity concentration can be increased at all points within the predetermined plane, thereby reducing the operating voltage at all points within the predetermined plane. When the compositionally graded layer 23 includes a high-concentration region 233, the high-concentration region 233 may be disposed at an end of the compositionally graded layer 23, or the high-concentration region 233 may be disposed in at least a portion of the region of the compositionally graded layer 23 excluding the end. Disposing the high-concentration region 233 in at least a portion of the region of the compositionally graded layer 23 excluding the end refers to a state in which both the top and bottom of the high-concentration region 233 are the compositionally graded layer 23. The thicknesses of the compositionally graded layer 23 and the high-concentration region 233 can be appropriately set depending on the thicknesses of the n-side semiconductor layer 2, the active layer 3, the p-side semiconductor layer 4, etc. The thickness of the compositionally graded layer 23, regardless of whether or not the high-concentration region 233 is present, can be 5 nm or more and 50 nm or less. Furthermore, the thickness of the high-concentration region 233 is thinner than the thickness of the compositionally graded layer 23. This configuration can suppress optical loss due to the high-concentration region 233 while achieving the effect of reducing band spikes.

[0018] When the compositionally graded layer 23 does not include the high-concentration region 233, the second semiconductor layer 22 described below includes the high-concentration region 233. When the compositionally graded layer 23 includes the high-concentration region 233, the second semiconductor layer 22 may also include the high-concentration region 233. In this case, the effect of reducing the operating voltage can be obtained in both the compositionally graded layer 23 and the second semiconductor layer 22. Furthermore, when the compositionally graded layer 23 includes the high-concentration region 233, the second semiconductor layer 22 does not need to include the high-concentration region 233. In this case, optical loss in the second semiconductor layer 22 can be reduced. All of the portions of the compositionally graded layer 23 other than the high-concentration region 233 may have the same concentration. When the compositionally graded layer 23 does not include the high-concentration region 233, the entire compositionally graded layer 23 may contain n-type impurities at a first concentration. When the compositionally graded layer 23 includes the high-concentration region 233, the entire compositionally graded layer 23 except for the high-concentration region 233 may contain n-type impurities at a first concentration. Furthermore, at least a portion of the compositionally graded layer 23 may contain n-type impurities at a concentration different from both the first concentration and the third concentration. When the compositionally graded layer 23 includes a high-concentration region 233, it is preferable that the concentration of n-type impurities be lower in a region adjacent to the high-concentration region 233 and closer to the second semiconductor layer 22 than the high-concentration region 233 than in a region adjacent to the high-concentration region 233 and closer to the first semiconductor layer 21 than the high-concentration region 233. This configuration reduces the n-type impurity concentration in the region closer to the second semiconductor layer 22, which has a higher optical density than the first semiconductor layer 21, and more effectively reduces optical loss. It is preferable that the high-concentration region 233 does not exist between the first semiconductor layer 21 and the compositionally graded layer 23. This structure reduces optical loss between the first semiconductor layer 21 and the compositionally graded layer 23. It is preferable that the high-concentration region 233 does not exist throughout the compositionally graded layer 23. For example, the high concentration region 233 may be provided only in a part of the composition gradient layer 23, or the high concentration region 233 may not be provided in the composition gradient layer 23. With this structure, the optical loss caused by providing the high concentration region 233 can be reduced.

[0019] (Second Semiconductor Layer 22) The second semiconductor layer 22 contains n-type impurities and is formed on the compositionally graded layer 23. The second semiconductor layer 22 is preferably made of, for example, an AlGaN layer, a GaN layer, an InGaN layer, and / or an InGaAlN layer, and is preferably made of a GaN layer. This configuration reduces the refractive index of the second semiconductor layer 22, allowing light to be efficiently trapped inside the second semiconductor layer 22. The second semiconductor layer 22 has a smaller bandgap energy than the first semiconductor layer 21. For example, if the second semiconductor layer 22 includes a semiconductor layer containing Al, the molar ratio of Al to the sum of Al and Ga is smaller than the molar ratio of Al to the sum of Al and Ga in the first semiconductor layer 21. If the first semiconductor layer 21 is formed of, for example, an AlGaN layer, the molar ratio of Al to the sum of Al and Ga in the second semiconductor layer 22 is smaller than that in the first semiconductor layer 21 or is zero. Specifically, the molar ratio of Al to the total of Al and Ga is 0 or more and 0.05 or less. The concentration of the n-type impurity in at least a part of the second semiconductor layer 22 is referred to as the second concentration. The second concentration is preferably lower than the fourth concentration. The second concentration is also preferably lower than the first concentration. Furthermore, the second concentration is preferably lower than the third concentration. Specifically, the second concentration is 1×10 17 cm -3 1x10 or more 18 cm -3 The following are listed: 2 x 10 17 cm -3 9 x 10 or more 17 cm -3 The following is preferable: By setting the second concentration to a low value, optical loss due to n-type impurities can be reduced.

[0020] The second semiconductor layer 22 may include the previously described high-concentration region 233. Including the high-concentration region 233 in the second semiconductor layer 22 can reduce the operating voltage. When the second semiconductor layer 22 contains n-type impurities at the second concentration and includes the high-concentration region 233, the high-concentration region 233 is preferably a layered region. That is, within a predetermined plane of the second semiconductor layer 22, the n-type impurity concentration at any point is either the second concentration or the third concentration. The "predetermined plane" refers to a plane that grows simultaneously in the semiconductor layer. In other words, the "predetermined plane" refers to a plane parallel to the interface between the compositionally graded layer 23 and the second semiconductor layer 22. By including the high-concentration region 233 as a layered region, the n-type impurity concentration can be increased at all points within the predetermined plane, thereby reducing the operating voltage at all points within the predetermined plane. When the second semiconductor layer 22 includes a high-concentration region 233, the high-concentration region 233 may be disposed at an end of the second semiconductor layer 22, or the high-concentration region 233 may be disposed in at least a portion of the region of the second semiconductor layer 22 excluding the end. Disposing the high-concentration region 233 in at least a portion of the region of the second semiconductor layer 22 excluding the end refers to a state in which both the top and bottom of the high-concentration region 233 are the second semiconductor layer 22. The thicknesses of the second semiconductor layer 22 and the high-concentration region 233 can be appropriately set depending on the thicknesses of the n-side semiconductor layer 2, the active layer 3, the p-side semiconductor layer 4, etc. The thickness of the second semiconductor layer 22 may be 5 nm or more and 50 nm or less, regardless of whether the high-concentration region 233 is present. Note that when the high-concentration region 233 is not included in the second semiconductor layer 22, the high-concentration region 233 is included in the compositionally graded layer 23. The entire portion of the second semiconductor layer 22 that is not the high-concentration region 233 may have the same concentration. That is, when the second semiconductor layer 22 does not include the high-concentration region 233, the entire second semiconductor layer 22 may contain the n-type impurity at the second concentration. When the second semiconductor layer 22 includes the high-concentration region 233, the entire second semiconductor layer 22 excluding the high-concentration region 233 may contain the n-type impurity at the second concentration. Note that at least a portion of the composition gradient layer 23 may contain the n-type impurity at a concentration different from both the second concentration and the third concentration.

[0021] (Other Layers) As described above, the n-side semiconductor layer 2 may further include another semiconductor layer, as long as it includes the first semiconductor layer 21, the compositionally graded layer 23, and the second semiconductor layer 22 in this order. For example, a stacked structure including, from the substrate 1 side, an underlayer, a crack prevention layer, a first n-side cladding layer, a first n-side compositionally graded layer (i.e., the compositionally graded layer 23), an intermediate layer (i.e., the high-concentration region 233), a first n-side light guide layer (i.e., the second semiconductor layer 22), a second n-side compositionally graded layer, and a hole blocking layer may be used. The hole blocking layer may include a first hole blocking layer and a second hole blocking layer. Note that n-type impurities may be added from the underlayer to the first n-side light guide layer. The underlayer may be, for example, an n-type AlGaN layer. The crack prevention layer may be, for example, an InGaN layer, the band gap energy of which is greater than that of the well layer in the active layer 3 described below. Providing the crack prevention layer reduces the probability of cracks occurring. The first n-side cladding layer may be, for example, a layer doped with n-type impurities and having a bandgap energy larger than that of the underlayer and the crack prevention layer. The first n-side cladding layer may be, for example, an AlGaN layer. The first n-side cladding layer may have the largest bandgap energy in the n-side semiconductor layer 2. The first n-side compositionally graded layer may be, for example, an AlGaN layer whose Al composition decreases with increasing distance from the first n-side cladding layer. At the end of the first n-side compositionally graded layer on the intermediate layer side, the composition of the first n-side compositionally graded layer may be considered to be GaN. The intermediate layer has a lattice constant equivalent to that of the first n-side optical guiding layer and may be, for example, a GaN layer. The intermediate layer is preferably provided with a thickness thinner than that of the first n-side compositionally graded layer and the first n-side optical guiding layer.

[0022] The first n-side optical guiding layer preferably has a smaller bandgap energy and a lower n-type impurity concentration than the first n-side cladding layer. The first n-side optical guiding layer may be, for example, a GaN layer. The second n-side optical guiding layer may be, for example, an undoped InGaN layer. The second n-side compositionally graded layer may be a layer whose composition is graded so that the bandgap energy decreases toward the active layer 3. When a compositionally graded layer is provided as the second n-side compositionally graded layer, it is preferable that the layer have a composition that changes so that the refractive index increases toward the active layer 3. This allows the n-side compositionally graded layer to continuously form a barrier for the optical waveguide, thereby enhancing light confinement in the active layer 3. When a compositionally graded layer whose lattice constant increases toward the active layer 3 is provided in the n-side semiconductor layer 2, it is preferable to add n-type impurities to the compositionally graded layer. In other words, a compositionally graded layer can be composed of multiple sublayers whose compositions vary slightly. For this reason, in a layer with a graded composition, it is difficult to avoid the generation of fixed charges even if the rate of composition change is reduced. Adding n-type impurities can shield fixed charges, thereby reducing the degree of voltage increase caused by the generation of fixed charges. It is preferable that at least a portion of the hole blocking layer contains n-type impurities. This allows for more efficient blocking of holes. When the hole blocking layer has a first hole blocking layer and a second hole blocking layer, for example, the first hole blocking layer can be a GaN layer and the second hole blocking layer can be an InGaN layer.

[0023] (Active Layer 3) The active layer 3 can have a multilayer structure composed of nitride semiconductor layers such as GaN and InGaN. The active layer 3 has a single quantum well structure or a multiple quantum well structure. A multiple quantum well structure is easier to obtain gain than a single quantum well structure. When the active layer 3 has a multiple quantum well structure, it has multiple well layers and intermediate barrier layers sandwiched between the well layers. For example, the active layer 3 includes, in order from the n-side semiconductor layer 2 side, a well layer, an intermediate barrier layer, and a well layer. An n-side barrier layer may be provided between the well layer closest to the n-side semiconductor layer 2 and the n-side semiconductor layer 2. The n-side barrier layer may function as part of a hole blocking layer. The n-side barrier layer may be omitted, and the hole blocking layer and the n-side optical guide layer may function as the n-side barrier layer. Similarly, a p-side barrier layer may be provided between the well layer closest to the p-side semiconductor layer 4 and the p-side semiconductor layer 4. If this p-side barrier layer is not provided or is thin, a part of the p-side semiconductor layer 4 may function as the p-side barrier layer. When a p-side barrier layer is provided in the active layer 3, the thickness of the p-side barrier layer is, for example, 5 nm or less. As described above, the addition of p-type impurities increases the optical absorption loss, so it is preferable to form the active layer 3 without adding p-type impurities. Each layer of the active layer 3 can be, for example, an undoped layer. When the oscillation wavelength of the semiconductor light-emitting device is set to 530 nm or more, In x Ga 1-x The In composition ratio x of the N well layer may be slightly increased or decreased depending on the layer structure other than the active layer 3, and may be, for example, 0.25 or more. The upper limit of the In composition ratio x of the well layer is, for example, 0.50 or less.

[0024] (P-Side Semiconductor Layer 4) The p-side semiconductor layer 4 may have a convex ridge 4a on its surface. The p-side semiconductor layer 4 may have a multilayer structure made of nitride semiconductors such as GaN, InGaN, or AlGaN. The p-side semiconductor layer 4 may include a p-side cladding layer, a p-side optical guide layer, and other layers. The p-side semiconductor layer 4 includes one or more p-type semiconductor layers. Examples of p-type semiconductor layers include layers made of nitride semiconductors containing p-type impurities such as Mg. However, a layer with a low p-type impurity concentration, such that p-type impurities are not detected by analysis such as SIMS, may be disposed on the active layer 3 side. The layer with a low p-type impurity concentration may have a thickness of, for example, 400 nm to 660 nm. Furthermore, the layer with a low p-type impurity concentration preferably has a layer with a smaller band gap energy than the layer containing p-type impurities above it.

[0025] The p-side semiconductor layer 4 may include, from the active layer 3 side, an undoped p-side compositionally graded layer, an undoped p-side intermediate layer, a p-side electron barrier layer containing p-type impurities, and / or a p-type semiconductor layer containing p-type impurities. The p-side compositionally graded layer can function, for example, as a p-side optical guide layer. The thickness of the p-side compositionally graded layer is preferably 200 nm or more and 350 nm or less. When the p-side semiconductor layer 4 has a ridge 4a, it is preferable that the lower end of the ridge 4a is not located in the p-side compositionally graded layer. The p-side electron barrier layer can be, for example, an AlGaN layer. When the p-side electron barrier layer is AlGaN, its Al composition can be 0.08 or more and 0.3 or less. The thickness of the p-side electron barrier layer can be, for example, 5 nm or more and 100 nm or less. The p-type semiconductor layer containing p-type impurities has a thickness of, for example, 1×10 18 / cm 3 1x10 or more 22 / cm 3The p-type impurity concentration can be set as follows. The p-type semiconductor layer having p-type impurities can function as a p-side cladding layer and / or a p-side contact layer. The p-type semiconductor layer can be, for example, an AlGaN layer or a GaN layer. The thickness of the p-side semiconductor layer 4 can be, for example, 5 nm or more and 300 nm or less. However, the p-side semiconductor layer 4 does not need to include all of the above-mentioned layers, and it is sufficient to include one or more layers. For these p-side semiconductor layers 4, for example, the semiconductor layers described in JP 2020-115539 A can be used.

[0026] As shown in FIG. 3 , a semiconductor light-emitting device 100 including the nitride semiconductor stack 10 described above includes a substrate 1 and, above the substrate, an n-side semiconductor layer 2, an active layer 3, and a p-side semiconductor layer 4. The semiconductor light-emitting device 100 may be, for example, an edge-emitting laser element having a light-emitting end face and a light-reflecting end face intersecting with the main surfaces of the semiconductor layers, such as the active layer 3. A ridge 4a is provided on the upper side of the p-side semiconductor layer 4. The ridge 4a has a mesa structure. The top view shape of the ridge 4a is elongated in the direction connecting the light-emitting end face and the light-reflecting end face, e.g., a rectangle with its short side parallel to the light-reflecting end face and its long side perpendicular to the light-reflecting end face. The portion of the active layer 3 directly below the ridge 4a and its vicinity constitutes an optical waveguide region. An insulating film 5 may be provided on the side surface of the ridge 4a and on the surface of the p-side semiconductor layer 4 that is continuous from the side surface of the ridge 4a. The substrate 1 is, for example, made of an n-type semiconductor, and an n-electrode 8 is provided on its underside. A p-electrode 6 is provided in contact with the upper surface of the ridge 4a, and a p-side pad electrode 7 is further provided thereon. Such a semiconductor light emitting element 100 can have a structure that emits laser light in a long wavelength region. The semiconductor light emitting element 100 can emit laser light in the blue wavelength band and the green wavelength band, for example, laser light with a wavelength of 420 nm or more.

[0027] The insulating film 5 can be formed of a single layer or a multilayer of oxides or nitrides of, for example, Si, Al, Zr, Ti, Nb, Ta, etc. The n-electrode 8 is provided, for example, over almost the entire lower surface of the n-type substrate 1. The p-electrode 6 is provided on the upper surface of the ridge 4a. If the width of the p-electrode 6 is narrow, a p-side pad electrode 7 wider than the p-electrode 6 may be provided on the p-electrode 6, and a wire or the like may be connected to the p-side pad electrode 7. Examples of materials for each electrode include a single layer or a multilayer of a metal or alloy such as Ni, Rh, Cr, Au, W, Pt, Ti, or Al, or a conductive oxide containing at least one selected from Zn, In, and Sn. Examples of conductive oxides include indium tin oxide (ITO), indium zinc oxide (IZO), and gallium-doped zinc oxide (GZO). The thickness of the electrode is, for example, 0.1 μm or more and 2 μm or less. The p-electrode 6 is preferably a transparent conductive film having a refractive index smaller than that of the active layer 3. This allows it to function as a cladding layer. The p-electrode 6 may be, for example, a p-electrode 6 made of ITO.

[0028] [Method for Manufacturing a Semiconductor Light-Emitting Device] A method for manufacturing a semiconductor light-emitting device includes, for example, first forming a first semiconductor layer 21 containing n-type impurities (S1). Next, forming a compositionally graded layer 23 containing n-type impurities and having a bandgap energy that decreases with increasing distance from the first semiconductor layer 21 (S2). Next, forming a second semiconductor layer 22 containing n-type impurities and having a bandgap energy smaller than that of the first semiconductor layer 21 (S3). The first semiconductor layer 21, compositionally graded layer 23, and second semiconductor layer 22 are preferably formed on a substrate 1. The semiconductor layer may be formed using any method known in the art, such as an MOCVD method or a sputtering method. The semiconductor layer can be formed using an MOCVD apparatus. The n-type impurity can be doped into the semiconductor layer by introducing a gas containing an element to be used as the n-type impurity during the formation of the semiconductor layer. In this case, the n-type impurity concentration can be adjusted by increasing or decreasing the concentration or supply amount of the gas containing the element to be used as the n-type impurity. Furthermore, when forming a semiconductor layer, the band gap energy of the semiconductor layer to be formed can be adjusted by adjusting the composition of a plurality of gases containing semiconductor raw materials.

[0029] In one embodiment, for example, when forming the compositionally graded layer 23, the concentration or supply amount of at least one gas among multiple gases containing semiconductor raw materials is adjusted to grade the composition of the semiconductor layer. Furthermore, the compositionally graded layer 23 is formed so as to contain n-type impurities at a first concentration by adjusting the concentration or supply amount of a gas containing an element to be an n-type impurity. Thereafter, when forming the second semiconductor layer 22, the multiple gases containing the semiconductor raw materials are set to predetermined concentrations and supply amounts to form the second semiconductor layer 22 having a predetermined composition. Furthermore, for example, at the initial stage of forming the second semiconductor layer 22, the gas containing the element to be an n-type impurity is set to a predetermined concentration or supply amount to form a high-concentration region 233 containing n-type impurities at a third concentration. Subsequently, the gas containing the element to be an n-type impurity may be set to a predetermined concentration or supply amount to contain n-type impurities at a second concentration. By performing these steps, the high-concentration region 233 in the second semiconductor layer 22 containing n-type impurities at a third concentration higher than the first and second concentrations can be formed.

[0030] In another embodiment, for example, when forming the compositionally graded layer 23, the concentration or supply amount of at least one gas among multiple gases containing semiconductor raw materials is adjusted to grade the composition of the semiconductor layer. At this time, a gas containing an element to be an n-type impurity is adjusted to a predetermined concentration or supply amount to form a portion of the compositionally graded layer 23 so as to contain the n-type impurity at a first concentration. Subsequently, a gas containing an element to be an n-type impurity is adjusted to a predetermined concentration or supply amount to form a high-concentration region 233 containing the n-type impurity at a third concentration as part of the compositionally graded layer 23. Next, a gas containing an element to be an n-type impurity may be adjusted to a predetermined concentration or supply amount to form a portion of the compositionally graded layer 23 so as to contain the n-type impurity at a first concentration. The compositionally graded layer 23 may then be formed in a stacked state such that the compositionally graded layer 23 is located above and below the high-concentration region 233. Subsequently, when forming the second semiconductor layer 22, multiple gases containing semiconductor raw materials are adjusted to predetermined concentrations and supply amounts to form the second semiconductor layer 22 having a predetermined composition. In this case, by adjusting the gas containing the element to be used as the n-type impurity to a predetermined concentration or supply amount, the second semiconductor layer 22 containing the n-type impurity at a second concentration can be formed on the composition gradient layer 23 on the high concentration region 233.

[0031] After forming the second semiconductor layer 22 in S3, the active layer 3, p-side semiconductor layer 4, insulating film 5, p-electrode 6, p-side pad electrode 7, n-electrode 8, etc. are sequentially formed by known methods to manufacture a semiconductor light-emitting device.

[0032] Example 1 A nitride semiconductor stack consisting of an n-side semiconductor layer 2, an active layer 3, and a p-side semiconductor layer 4 was formed on an n-type GaN substrate (substrate 1) with the (0001) plane as the upper surface as follows: First, in an MOCVD apparatus, a layer of 4×10 Si was deposited on the n-type GaN substrate (substrate 1) as the n-side semiconductor layer 2. 18 cm -3 The Al film of 1.5 μm thickness was doped to have a concentration of 0.016 Ga 0.984 N layer (underlayer) and Si 1×10 19 cm -3 A 150 nm thick In film was doped to a concentration of 0.04 Ga0.96 N layer (crack prevention layer) and Si 7 × 10 18 cm -3 The Al film was doped to a thickness of 900 nm to a concentration of 0.08 Ga 0.92 N layer (first n-side cladding layer) and Si 7×10 18 cm -3 and a 19-nm-thick first n-side compositionally graded layer doped with Si to a concentration of 7×10 19 cm -3 and a 1 nm thick GaN layer (intermediate layer) doped with Si to a concentration of 5×10 17 cm -3 and a 350 nm thick GaN layer (first n-side optical guide layer) doped with Si to a concentration of 1×10 18 cm -3 and a 200 nm thick composition gradient layer (second n-side composition gradient layer) doped with Si to a concentration of 7×10 19 cm -3 The second n-side compositionally graded layer was grown in this order, with GaN as the starting point and In as the terminal point. 0.05 Ga 0.95 The N composition was formed so that the In composition was substantially monotonically decreased in 120 steps so that the composition gradient was nearly linear.

[0033] Of the above layers, the fourth concentration is 7×10 18 cm -3 The first n-side cladding layer containing Si at a concentration of 7×10 corresponds to the first semiconductor layer 21. 18 cm -3 The first n-side compositionally graded layer containing Si at a concentration of 7×10 corresponds to the compositionally graded layer 23, and the third concentration is 7×10 19 cm -3 The intermediate layer containing Si at a concentration of 5×10 corresponds to the high concentration region 233, and the second concentration is 5×10 17 cm -3 The first n-side optical guide layer containing Si at a concentration of 1000 nm corresponds to the second semiconductor layer 22. 0.07 Ga 0.83 N layer and undoped In 0.20 Ga 0.80An active layer 3 including an N layer and an undoped GaN layer in this order was grown. Subsequently, as a p-side semiconductor layer 4, an undoped composition gradient layer having a thickness of 200 nm, an undoped GaN layer having a thickness of 120 nm, and an undoped Al layer having a thickness of 130 nm were grown. 0.04 Ga 0.96 N layer and Mg 2 × 10 19 cm -3 A 10 nm thick Al film was added to give a concentration of 0.25 Ga 0.75 N layer and Mg 8 × 10 18 cm -3 The Al film of 100 nm thickness was doped to have a concentration of 0.04 Ga 0.96 N layer and Mg 1 × 10 20 cm -3 The p-side composition gradient layer was grown in this order, with the starting point of growth being In. 0.05 Ga 0.95 The growth was terminated with GaN, and the In composition was substantially monotonically decreased in 120 steps so that the composition gradient was nearly linear. The resulting nitride semiconductor stack was then removed from the MOCVD apparatus, and a ridge 4a, an insulating film 5, a p-electrode 6, a p-side pad electrode 7, and an n-electrode 8 were formed. The depth of the ridge 4a was approximately 280 nm. The p-electrode 6 was an ITO film with a thickness of 200 nm. Reflective films were then formed on the light-emitting end facet and the light-reflecting end facet, respectively, and the stack was singulated to obtain semiconductor laser elements as semiconductor light-emitting elements 100. The peak wavelength of the laser light emitted by the resulting semiconductor light-emitting elements 100 was approximately 455 nm.

[0034] Of the above-mentioned layers, the first semiconductor layer 21, the compositionally graded layer 23, the high-concentration region 233, and the second semiconductor layer 22 have varying molar ratios of Al to the sum of Al and Ga and Si concentrations, as shown in FIG. 7 . That is, the molar ratio of Al to the sum of Al and Ga is constant in the first semiconductor layer 21, but decreases in the compositionally graded layer 23 with increasing distance from the first semiconductor layer 21. The molar ratio of Al to the sum of Al and Ga is constant in the high-concentration region 233 and the second semiconductor layer 22. Meanwhile, the Si concentration is constant at a first concentration in the compositionally graded layer 23 and a third concentration higher than the first concentration in the high-concentration region 233. The Si concentration in the second semiconductor layer 22 is constant at a second concentration lower than the first and third concentrations. The Si concentration in the first semiconductor layer 21 is constant at a fourth concentration, which is the same as the first concentration. Note that the values ​​in FIG. 7 merely qualitatively illustrate the magnitude relationships and are not quantitatively accurate. Furthermore, the molar ratio of Al to the total of Al and Ga and the Si concentration in each layer are not limited to the example shown in FIG. 7, and various modifications can be made as long as the problems of the present application can be solved.

[0035] Comparative Example 1 As Comparative Example 1, a semiconductor light-emitting device was fabricated having the same structure as in Example 1, except that the composition gradient layer 23 and the intermediate layer thereon were not formed in the n-side semiconductor layer 2. The peak wavelength of light emitted from the semiconductor light-emitting device of Comparative Example 1 was approximately 455 nm.

[0036] (Experimental Result 1) Simulation results of the J-V characteristics and band spikes of the semiconductor light-emitting devices of Example 1 and Comparative Example 1 are shown in FIGS. 4, 5, and 6, respectively. In Comparative Example 1, polarization charges accumulate at the heterointerface, causing band spikes as shown in the simulation results of FIG. 6. These band spikes act as barriers that hinder the flow of electrons, resulting in a higher operating voltage as shown by the solid line in FIG. 4. On the other hand, in the semiconductor light-emitting device of Example 1, a reduction in band spikes was confirmed as shown in the simulation results of FIG. 5. As a result, it is possible to lower the operating voltage as shown by the dashed line in FIG. 4.

[0037] The present application includes the following disclosures: (1) A semiconductor light-emitting device comprising: a nitride semiconductor stack including: a first semiconductor layer containing an n-type impurity; a compositionally graded layer containing the n-type impurity and formed on the first semiconductor layer, the compositionally graded layer having a bandgap energy that decreases with increasing distance from the first semiconductor layer; and a second semiconductor layer containing the n-type impurity and formed on the compositionally graded layer, the second semiconductor layer having a bandgap energy smaller than that of the first semiconductor layer, wherein at least a portion of the compositionally graded layer contains the n-type impurity at a first concentration, and at least a portion of the second semiconductor layer contains the n-type impurity at a second concentration, and at least one of the compositionally graded layer and the second semiconductor layer includes a high-concentration region containing the n-type impurity at a third concentration higher than the first concentration and the second concentration. (2) The semiconductor light-emitting device according to (1), wherein the first semiconductor layer contains the n-type impurity at a fourth concentration, and the second concentration is lower than the fourth concentration. (3) The semiconductor light-emitting device according to (1) or (2), wherein the second concentration is lower than the first concentration. (4) The first semiconductor layer is 1×10 18 cm -3 1x10 or more 19 cm -3 the first concentration is 1×10 18 cm -3 1x10 or more 19 cm -3 the second concentration is 1×10 or less 17 cm -3 1x10 or more 18 cm -3 (5) The semiconductor light-emitting device according to any one of (1) to (3), wherein the composition gradient layer has a thickness of 5 nm to 50 nm. (6) The third concentration is 1×10 18 cm -3 1x10 or more 20 cm -3The semiconductor light-emitting device according to any one of (1) to (5), which is: (7) The semiconductor light-emitting device according to any one of (1) to (6), wherein the high-concentration region is a layer region having a thickness of 0.1 nm to 10 nm, (8) The semiconductor light-emitting device according to any one of (1) to (7), wherein the n-type impurity is Si. (9) A method for manufacturing a semiconductor light-emitting element, comprising the steps of: forming a first semiconductor layer containing an n-type impurity; forming a compositionally graded layer containing the n-type impurity and having a band gap energy that decreases with increasing distance from the first semiconductor layer; and forming a second semiconductor layer containing the n-type impurity and having a band gap energy smaller than that of the first semiconductor layer, wherein in the step of forming the compositionally graded layer, the n-type impurity is doped into at least a portion of the compositionally graded layer at a first concentration; and in the step of forming the second semiconductor layer, the n-type impurity is doped into at least a portion of the second semiconductor layer at a second concentration; and in at least one of the steps of forming the compositionally graded layer and forming the second semiconductor layer, the n-type impurity is doped into at least one of the compositionally graded layer and the second semiconductor layer at a third concentration higher than the first and second concentrations. (10) The method for manufacturing a semiconductor light-emitting element according to (9), wherein the step of forming the first semiconductor layer comprises the step of doping at least a portion of the first semiconductor layer with the n-type impurity at a fourth concentration, and the second concentration is lower than the fourth concentration. (11) The method for manufacturing a semiconductor light-emitting element according to (9) or (10), wherein the second concentration is lower than the first concentration. (12) The method for manufacturing a semiconductor light-emitting element according to any one of (9) to (11), wherein the second concentration is lower than the third concentration. (13) The third concentration is 1×10 18 cm -3 1x10 or more 20 cm -3 A method for manufacturing a semiconductor light-emitting element according to any one of (9) to (12) below.

[0038] REFERENCE SIGNS LIST 1 substrate 2 n-side semiconductor layer 21 first semiconductor layer 22 second semiconductor layer 23 compositionally graded layer 233 high concentration region 3 active layer 4 p-side semiconductor layer 4a ridge 5 insulating film 6 p-electrode 7 p-side pad electrode 8 n-electrode 10 stacked body 100 semiconductor light emitting element

Claims

1. A semiconductor light-emitting device comprising: a nitride semiconductor stack having: a first semiconductor layer containing an n-type impurity; a compositionally graded layer containing the n-type impurity, formed on the first semiconductor layer, and having a band gap energy that decreases with increasing distance from the first semiconductor layer; and a second semiconductor layer containing the n-type impurity, formed on the compositionally graded layer, and having a smaller band gap energy than the first semiconductor layer, wherein at least a portion of the compositionally graded layer contains the n-type impurity at a first concentration, and at least a portion of the second semiconductor layer contains the n-type impurity at a second concentration, and at least one of the compositionally graded layer and the second semiconductor layer includes a high-concentration region containing the n-type impurity at a third concentration higher than the first concentration and the second concentration.

2. The semiconductor light-emitting element according to claim 1, wherein the first semiconductor layer contains the n-type impurity at a fourth concentration, and the second concentration is lower than the fourth concentration.

3. A semiconductor light-emitting element according to claim 1 or 2, wherein the second concentration is lower than the first concentration.

4. The first semiconductor layer is 1×10 18 cm -3 Above 1 x 10 19 cm -3 The n-type impurity is contained at a concentration of 1×10 18 cm -3 Above 1 x 10 19 cm -3 the second concentration is 1×10 17 cm -3 Above 1 x 10 18 cm -3 The semiconductor light emitting device according to any one of claims 1 to 3, wherein:

5. The semiconductor light-emitting device according to any one of claims 1 to 4, wherein the composition gradient layer has a thickness of 5 nm or more and 50 nm or less.

6. The third concentration is 1×10 18 cm -3 Above 1 x 10 20 cm -3 The semiconductor light-emitting device according to any one of claims 1 to 5, wherein:

7. A semiconductor light-emitting device according to any one of claims 1 to 6, wherein the high concentration region is a layer region having a thickness of 0.1 nm or more and 10 nm or less.

8. A semiconductor light-emitting device according to any one of claims 1 to 7, wherein the n-type impurity is Si.

9. A method for manufacturing a semiconductor light-emitting element, comprising the steps of: forming a first semiconductor layer containing an n-type impurity; forming a compositionally graded layer containing the n-type impurity and having a band gap energy decreasing with increasing distance from the first semiconductor layer; and forming a second semiconductor layer containing the n-type impurity and having a band gap energy smaller than that of the first semiconductor layer, wherein in the step of forming the compositionally graded layer, the n-type impurity is doped at least a portion of the compositionally graded layer at a first concentration; and in the step of forming the second semiconductor layer, the n-type impurity is doped at least a portion of the second semiconductor layer at a second concentration; and in at least one of the steps of forming the compositionally graded layer and forming the second semiconductor layer, the n-type impurity is doped at least one of the compositionally graded layer and the second semiconductor layer at a third concentration higher than the first concentration and the second concentration.

10. A method for manufacturing a semiconductor light-emitting element as described in claim 9, wherein the step of forming the first semiconductor layer includes a step of adding the n-type impurity at a fourth concentration to at least a portion of the first semiconductor layer, and the second concentration is lower than the fourth concentration.

11. A method for manufacturing a semiconductor light-emitting element according to claim 9 or 10, wherein the second concentration is lower than the first concentration.

12. A method for manufacturing a semiconductor light-emitting element according to any one of claims 9 to 11, wherein the second concentration is lower than the third concentration.

13. The third concentration is 1×10 18 cm -3 Above 1 x 10 20 cm -3 The method for producing a semiconductor light-emitting device according to any one of claims 9 to 12, wherein:

Citation Information

Patent Citations

  • Ultraviolet light emission element

    JP2022041740A

  • Laser diode

    JP2022150772A

  • Violet semiconductor light emitting element

    JP2022179037A

  • Polarization field assisted heterostructure design for efficient deep ultra-violet light emitting diodes

    US20190148593A1

  • Vertical-type ultraviolet light-emitting diode

    WO2017150280A1