Projection welded joint and method for manufacturing same
The controlled composition and welding process for projection welded joints address the brittleness and delayed fracture issues in high-strength steel plates by softening the joint surface and reducing residual stress, enhancing peel strength and fracture resistance.
Patent Information
- Application Number
- PCT/JP2024/016151
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
High-strength steel plates used in projection welding tend to form brittle joints, leading to decreased peel strength and increased susceptibility to delayed fracture, particularly due to high carbon content and the effects of rust preventive oils and plating layers incorporating hydrogen into the weld.
A projection welded joint with a specific composition of the steel plate (0.05-0.50% C, 0.1-2.0% Si, 1.5-4.0% Mn, etc.) and a nut, where the minimum hardness of region c is controlled to be less than or equal to 0.85 times the base metal hardness, and a manufacturing method involving controlled current values and energization times during projection welding to soften the joint surface and reduce residual stress.
The solution improves the peel strength and delayed fracture resistance of the projection welded joints by alleviating stress concentration and reducing residual stress, effectively addressing the brittleness and hydrogen embrittlement issues associated with high-strength steel plates.
Smart Images

Figure JP2024016151_31102024_PF_FP_ABST
Abstract
Description
Projection welded joint and its manufacturing method
[0001] The present invention relates to a projection-welded joint formed by projection-welding a steel plate and a nut having a protrusion via the protrusion, and to a method for manufacturing the same.
[0002] In recent years, the use of various high-strength steel plates (hi-tensile steel) has been promoted in automobile bodies from the viewpoints of weight reduction for improved fuel economy and ensuring collision safety. Furthermore, when resistance spot welding cannot be used in the automobile assembly process, arc welding and bolt fastening are used. Furthermore, bolt fastening is also widely used to join dissimilar materials such as steel plates and aluminum. In bolt fastening, a nut with a projection (protruding portion) is projection-welded (resistance-welded) to the steel plate, and then other plates are fastened with bolts to complete the assembly.
[0003] One of the quality assurance criteria for projection welding is the push-in peel strength (also simply referred to as peel strength). As the strength of steel sheets has increased in recent years, the joint between the steel sheet and the nut has become more brittle, making it difficult to ensure peel strength. Furthermore, as the strength of steel sheets has increased, their susceptibility to delayed fracture, or hydrogen embrittlement, has also become an issue. Another issue is that hydrogen is absorbed into the weld due to the influence of rust-preventive oils and plating layers on the steel sheet surface, making delayed fracture more likely.
[0004] Patent Document 1 describes a projection-welded joint in which the area ratio between the joint and the nominal diameter portion of the nut or bolt satisfies a predetermined relationship and the maximum hardness of the joint and heat-affected zone is 550 HV or less. Patent Document 1 also reports that high joint strength can be obtained by increasing the pressure during projection welding. Patent Document 2 also reports that high joint strength can be obtained by tempering the joint after projection welding by post-energizing with a current value lower than the current value during welding.
[0005] JP 2012-157900 A JP 2013-78784 A
[0006] However, conventional methods have had problems such as reduced peel strength and delayed fracture when high-strength steel plates are projection-welded, leaving room for improvement.
[0007] In view of the above problems, an object of the present invention is to provide a projection welded joint having improved peel strength and delayed fracture resistance, and a method for manufacturing the same.
[0008] The present inventors conducted extensive research to solve the above-mentioned problems and have come to the following conclusions. High-strength steel plates have a higher carbon content than conventional steel plates, which makes the joint more susceptible to embrittlement, resulting in reduced peel strength of projection-welded joints. To improve the peel strength of projection-welded joints using high-strength steel plates, it is effective to alleviate stress concentration by softening the joint surface between the nut and the steel plate. Delayed fracture is also caused by the hardness of the joint, which is the fracture initiation point, and the influence of segregation and inclusions present in the joint. Therefore, to suppress delayed fracture, it is effective to prevent hardening of the joint and reduce residual stress. In particular, the region near the boundary between the steel plate and the nut and including a portion of the joint is designated as region c. By reducing the hardness of region c, delayed fracture resistance can be improved. This is because softening the hardness of region c improves the toughness of region c, and further reduces residual stress, making delayed fracture less likely to occur.
[0009] That is, the gist and configuration of the present invention are as follows.
[0010] [1] A projection welded joint formed by projection welding a steel plate and a nut having a protrusion via the protrusion, wherein the steel plate contains, in mass%, C: 0.05 to 0.50%, Si: 0.1 to 2.0%, Mn: 1.5 to 4.0%, P: 0.10% or less, S: 0.005% or less, N: 0.010% or less, and O: 0.030% or less, and optionally further contains Al: 2.00% or less, B: 0.0050% or less, Ca: 0.005% or less, Cr: 1.00% or less, Cu: 0.80% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ti: 0.200% or less, V: 0.500% or less, A projection welded joint having a chemical composition containing at least one element selected from the group consisting of Nb: 0.080% or less, Sb: 0.200% or less, and Sn: 0.200% or less, with the balance consisting of Fe and unavoidable impurities, wherein the minimum hardness Hvc (HV) of the steel plate in a region c defined below and the base metal hardness Hvm (HV) of the steel plate satisfy the following formula (1): Hvc / Hvm≦0.85 (1) Region c is specified as follows in a cross section of the projection welded joint that includes the center line of the nut and passes through the center of the joint between the steel plate and the nut. The end point of the nut on the inner surface side that contacts the steel plate is A, the end point on the outer surface side is B, the thickness of the steel plate at the cross section is t (mm), points inside the steel plate that are moved 0.20 mm and 2 / 3t from point A in the thickness direction of the steel plate are A1 and A2, respectively, and points inside the steel plate that are moved 0.20 mm and 2 / 3t from point B in the thickness direction of the steel plate are B1 and B2, respectively, and the inside of the rectangle formed by connecting points A1, B1, B2, and A2 is defined as region c.
[0011] [2] A method for manufacturing a projection welded joint by projection welding a steel plate and a nut having a protrusion via the protrusion, wherein the steel plate contains, in mass%, C: 0.05 to 0.50%, Si: 0.1 to 2.0%, Mn: 1.5 to 4.0%, P: 0.10% or less, S: 0.005% or less, N: 0.010% or less, and O: 0.030% or less, and optionally further contains Al: 2.00% or less, B: 0.0050% or less, Ca: 0.005% or less, Cr: 1.00% or less, Cu: 0.80% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ti: 0.200% or less, V: 0.500% or less, The steel sheet has a composition containing at least one element selected from the group consisting of Nb: 0.080% or less, Sb: 0.200% or less, and Sn: 0.200% or less, with the balance being Fe and unavoidable impurities, and the projection welding is performed at a current value I 1 (kA) and current flow time t 1 a main current application process in which current is applied for a period of time t (ms) to form a joint between the steel plate and the nut; and a non-current application process in which current is applied for a period of time t (ms) to satisfy the following formula (2). c1 a non-energizing step in which a non-energizing period of (ms) is provided, and a current value I that satisfies the following formula (3) 2 (kA), and the current application time t satisfies the following formula (4) 2 a first post-energization step of energizing the coil for a period of time equal to or longer than 1 ms; and a current value I satisfying the following formula (5): 3 (kA), and the current application time t satisfies the following formula (6) 3 (ms)。 (ms) after the second current application process. c1 ...(2) 1.10I 1 ≦I 2 ≦1.80I 1 ... (3) 50≦t 2 ≦200...(4) I 3 ≦0.70I 2 ... (5) 300≦t 3 ≦1000 (6)
[0012] The present invention can provide a projection welded joint with improved peel strength and delayed fracture resistance.
[0013] Fig. 1 is a cross-sectional view, including the center line, of a nut used in one embodiment of the present invention. Fig. 2 is a partial cross-sectional view, including the center line of the nut and passing through the center of the joint between the steel plate and the nut, of a projection-welded joint according to one embodiment of the present invention. Fig. 3 is a top view of (a) a nut provided with three protrusions and (b) a nut provided with four protrusions, used in one embodiment of the present invention. Fig. 4 is a diagram showing region c and hardness measurement points in region c in a cross-section of a projection-welded joint according to one embodiment of the present invention. Fig. 5 is a diagram showing a measurement region 30 for base metal hardness Hvm and hardness measurement points in region 30 in a cross-section of a projection-welded joint according to one embodiment of the present invention.
[0014] Hereinafter, an embodiment of a projection welded joint and a manufacturing method thereof according to the present invention will be described. Note that the embodiment described below is an example of a specific embodiment of the present invention, and the configuration of the present invention is not limited to this specific example.
[0015] [Steel Plate] First, the chemical composition of the steel plate in the projection welded joint according to the present invention will be described. In the following description, the "%" designation for the chemical composition refers to "mass %" unless otherwise specified.
[0016] C: 0.05 to 0.50% C is an element that contributes to strengthening the steel plate. If the C content of the steel plate is less than 0.05%, the strength of the steel plate will be low, making it extremely difficult to produce a steel plate with a tensile strength of 780 MPa or more. Therefore, the C content of the steel plate is set to 0.05% or more. The C content of the steel plate is preferably set to 0.10% or more. On the other hand, if the C content of the steel plate exceeds 0.50%, the strength of the steel plate will increase, but the amount of hard martensite will become excessive, resulting in an increase in microvoids. Furthermore, the joint will become excessively hardened and embrittlement will progress, making it difficult to improve peel strength. Therefore, the C content of the steel plate is set to 0.50% or less. The C content of the steel plate is preferably set to 0.45% or less.
[0017] Si: 0.1 to 2.0% When the Si content of the steel plate is 0.1% or more, it effectively strengthens the steel plate. Furthermore, since Si is a ferrite-forming element, it favors the formation of ferrite at the end of the weld. Therefore, the Si content of the steel plate is set to 0.1% or more. The Si content of the steel plate is preferably set to 0.2% or more. On the other hand, if the Si content of the steel plate exceeds 2.0%, the steel plate is strengthened, but this may have a negative effect on toughness. Therefore, the Si content of the steel plate is set to 2.0% or less. The Si content is preferably set to 1.8% or less.
[0018] Mn: 1.5 to 4.0% When the Mn content is 1.5% or more, high peel strength can be obtained without long-term cooling. Therefore, the Mn content of the steel plate is set to 1.5% or more. The Mn content of the steel plate is preferably set to 2.0% or more. On the other hand, when the Mn content of the steel plate exceeds 4.0%, embrittlement of the weld or cracks associated with embrittlement become significant, making it difficult to improve the peel strength. Therefore, the Mn content of the steel plate is set to 4.0% or less. The Mn content of the steel plate is preferably set to 3.5% or less.
[0019] P: 0.10% or less P is an unavoidable impurity, but if the P content of the steel sheet exceeds 0.10%, strong segregation appears at the edge of the welded joint, making it difficult to improve peel strength. Therefore, the P content of the steel sheet is set to 0.10% or less. The P content of the steel sheet is preferably 0.05% or less, and more preferably 0.02% or less. There is no particular lower limit for the P content of the steel sheet. However, since excessive reduction leads to increased costs, the P content of the steel sheet is preferably 0.005% or more.
[0020] S: 0.005% or less S is an element that segregates at grain boundaries and embrittles steel sheets, and is an element that is inevitably contained. Furthermore, if the S content of a steel sheet exceeds 0.005%, sulfides and the local deformability of the steel sheet are reduced. Therefore, the S content of the steel sheet is set to 0.005% or less. The S content of the steel sheet is preferably 0.004% or less, and more preferably 0.003% or less. Note that there is no particular lower limit for the S content of the steel sheet. However, since excessive reduction leads to increased costs, the S content of the steel sheet is preferably 0.001% or more.
[0021] N: 0.010% or less N is an element that is inevitably contained, and if the N content of the steel sheet exceeds 0.010%, the aging resistance of the steel sheet deteriorates. Therefore, the N content of the steel sheet is set to 0.010% or less. The N content of the steel sheet is preferably set to 0.008% or less. There is no particular lower limit for the N content of the steel sheet. However, since an excessive reduction leads to an increase in costs, the N content of the steel sheet is preferably set to 0.001% or more.
[0022] O: 0.030% or less If the O content of a steel plate exceeds 0.030%, non-metallic inclusions are formed, deteriorating the cleanliness and toughness of the steel plate. Therefore, the O content of the steel plate is set to 0.030% or less. The O content of the steel plate is preferably set to 0.020% or less. There is no particular lower limit for the O content of the steel plate. However, since an excessive reduction leads to an increase in costs, the O content of the steel plate is preferably set to 0.005% or more.
[0023] In addition to the above-mentioned chemical composition, the steel sheet used in the present invention may contain, as necessary, one or more elements selected from Al, B, Ca, Cr, Cu, Ni, Mo, Ti, V, Nb, Sb, and Sn, with the remainder consisting of Fe and unavoidable impurities.
[0024] Al: 2.00% or less Al is an element that can control the structure by refining austenite grains, but adding a large amount of Al deteriorates toughness. Therefore, when Al is added, the Al content is set to 2.00% or less. The Al content is preferably set to 1.50% or less. There is no particular lower limit for the Al content, but from the viewpoint of fully obtaining the effects of the addition of Al, the Al content is preferably set to 0.01% or more, and more preferably set to 1.20% or more.
[0025] B: 0.0050% or less B is an element that can improve hardenability and strengthen steel sheets, but if added in large amounts, this effect saturates. Therefore, when B is added, the B content is set to 0.0050% or less. The B content is preferably set to 0.0010% or less. Furthermore, although there is no particular lower limit for the B content, from the viewpoint of fully obtaining the effects of adding B, the B content is preferably set to 0.0003% or more.
[0026] Ca: 0.005% or less Ca is an element that can contribute to improving the workability of steel sheets, but adding a large amount of Ca deteriorates toughness. Therefore, when Ca is added, the Ca content is set to 0.005% or less. The Ca content is preferably set to 0.004% or less. Furthermore, although there is no particular lower limit for the Ca content, from the viewpoint of fully obtaining the effects of adding Ca, the Ca content is preferably set to 0.001% or more.
[0027] Cr: 1.00% or less Cr is an element that can improve the strength of steel sheets by improving hardenability, but adding a large amount may deteriorate the toughness of welded joints. Therefore, when Cr is added, the Cr content is set to 1.00% or less. The Cr content is preferably set to 0.80% or less. Furthermore, although there is no particular lower limit for the Cr content, from the viewpoint of fully obtaining the effects of the addition of Cr, the Cr content is preferably set to 0.01% or more.
[0028] Cu: 0.80% or less Cu is an element that can contribute to improving the strength of steel sheets, but adding a large amount of Cu deteriorates toughness. Therefore, when Cu is added, the Cu content is set to 0.80% or less. The Cu content is preferably set to 0.60% or less. There is no particular lower limit for the Cu content, but from the viewpoint of fully obtaining the effects of adding Cu, the Cu content is preferably set to 0.006% or more.
[0029] Ni: 1.00% or less Ni is an element that can contribute to improving the strength of steel sheets, but adding a large amount of Ni deteriorates toughness. Therefore, when Ni is added, the Ni content is set to 1.00% or less. The Ni content is preferably set to 0.80% or less. Furthermore, although there is no particular lower limit for the Ni content, from the viewpoint of fully obtaining the effects of the addition of Ni, the Ni content is preferably set to 0.005% or more.
[0030] Mo: 1.00% or less Mo is an element that can contribute to improving the strength of steel sheets, but adding a large amount of Mo deteriorates toughness. Therefore, when Mo is added, the Mo content is set to 1.00% or less. The Mo content is preferably set to 0.80% or less. There is no particular lower limit for the Mo content, but from the viewpoint of fully obtaining the effects of adding Mo, the Mo content is preferably set to 0.006% or more.
[0031] Ti: 0.200% or less Ti is an element that can improve hardenability and strengthen steel sheets, but if added in large amounts, it forms carbides, which undergo precipitation hardening, significantly deteriorating toughness. Therefore, when Ti is added, the Ti content is set to 0.200% or less. The Ti content is preferably set to 0.150% or less. Furthermore, although there is no particular lower limit for the Ti content, from the viewpoint of fully obtaining the effects of the addition of Ti, the Ti content is preferably set to 0.003% or more.
[0032] V: 0.500% or less V is an element that can strengthen steel by controlling the structure through precipitation hardening, but adding a large amount leads to a deterioration in the toughness of the weld. Therefore, when V is added, the V content is set to 0.500% or less. The V content is preferably set to 0.300% or less. Furthermore, although there is no particular lower limit for the V content, from the viewpoint of fully obtaining the effect of the addition of V, the V content is preferably set to 0.005% or more.
[0033] Nb: 0.080% or less Nb is an element that can improve cross tensile strength and delayed fracture resistance after resistance welding by forming fine carbonitrides, but adding a large amount of Nb not only significantly reduces elongation but also significantly impairs toughness. Therefore, when Nb is added, the Nb content is set to 0.080% or less. The Nb content is preferably set to 0.070% or less, and more preferably to 0.060% or less. Furthermore, although there is no particular restriction on the lower limit of the Nb content, from the viewpoint of fully obtaining the effects of the addition of Nb, the Nb content is preferably set to 0.005% or more.
[0034] Sb: 0.200% or less Sb is an element that can suppress nitriding and oxidation of the steel sheet surface, but adding a large amount of Sb reduces toughness. Therefore, when Sb is added, the Sb content is set to 0.200% or less. There is no particular lower limit for the Sb content, but from the viewpoint of fully obtaining the effects of the addition of Sb, the Sb content is preferably set to 0.002% or more.
[0035] Sn: 0.200% or less Sn is an element that can suppress nitriding and oxidation of the steel sheet surface, and adding Sn stabilizes the material, but adding a large amount reduces toughness. Therefore, when Sn is added, the Sn content is set to 0.200% or less. There is no particular lower limit for the Sn content, but from the viewpoint of fully obtaining the effects of adding Sn, the Sn content is preferably set to 0.002% or more.
[0036] A steel plate having the above-described chemical composition preferably has a tensile strength of 980 MPa or more, more preferably 1180 MPa or more. However, when the tensile strength of a steel plate is 980 MPa or more, the carbon content is high, which poses a problem of embrittlement of the joint when conventional projection welding is performed, resulting in reduced push-in peel strength. According to the present invention, even in a high-strength steel plate having a tensile strength of 980 MPa or more, softening the hardness of region c can alleviate stress concentration and suppress a decrease in peel strength. Furthermore, reducing the residual stress in region c can improve the peel strength of the projection weld and improve delayed fracture resistance. Note that the above effects can also be achieved when a steel plate having a tensile strength of less than 980 MPa is used. On the other hand, the upper limit of the tensile strength of the steel plate is not particularly limited, but the tensile strength is generally 2000 MPa or less.
[0037] The thickness of the steel sheet is preferably 0.8 mm to 2.3 mm, from the viewpoint of targeting general steel sheets for automobiles.
[0038] The steel sheet used in the present invention may have a plating layer on the surface of the steel sheet, and may be, for example, a steel sheet having a zinc plating layer (galvanized steel sheet). The zinc plating layer includes known zinc plating layers, such as a hot-dip galvanized layer, an electrogalvanized layer, a Zn—Al plating layer, and a Zn—Ni layer. The steel sheet used in the present invention may also be subjected to a zinc plating treatment and then an alloying treatment to form a steel sheet having a zinc alloyed plating layer. The zinc plating layer may be formed on only one side or both sides of the steel sheet.
[0039] [Nut] The nut used in the present invention is a nut having protrusions. FIG. 1 shows a cross section including a center line 12 of a nut 10 used in one embodiment of the present invention. The nut 10 has protrusions 16 on a surface 14 perpendicular to the center line 12. In FIG. 1, two protrusions 16 are provided symmetrically on the surface 14 perpendicular to the center line 12, spaced 180° apart from each other around the center line 12 as the axis of rotation. Note that the protrusions 16 may be provided at three or four points symmetrically around the center line 12 as the axis of rotation. The shapes of the nut 10 and the protrusions 16 may be, for example, a square weld nut (type 1C) and various protrusion shapes described in JIS B 1196:2010, respectively.
[0040] The component composition of the nut is not particularly limited, but for example, S25C (JIS G4051) may be used. In particular, when the C content in the component composition of the nut is 0.05 mass% or more, the hardness of region c is preferably obtained. Therefore, the C content of the nut is preferably 0.05 mass% or more, and more preferably 0.07 mass% or more. On the other hand, when the C content in the component composition of the nut is 0.40 mass% or less, the hardness of region c is preferably obtained. Therefore, the C content of the nut is preferably 0.40 mass% or less, and more preferably 0.38 mass% or less.
[0041] When three or more protrusions are provided on a surface perpendicular to the center line of the nut used in the present invention, the contact position between the protrusions and the steel plate is three or more times during projection welding, as described below, and the contact state can be suitably stabilized. Therefore, the number of protrusions provided on the surface perpendicular to the center line of the nut used in the present invention is preferably three or more. On the other hand, when four or fewer protrusions are provided on a surface perpendicular to the center line of the nut used in the present invention, the occurrence of weak contact protrusions during projection welding, which can favorably prevent unbalanced heat input, and can suitably suppress a decrease in the strength of the joint. Therefore, the number of protrusions provided on the surface perpendicular to the center line of the nut used in the present invention is preferably four or less.
[0042] [Projection-welded joint] The projection-welded joint according to the present invention is a projection-welded joint formed by projection-welding the above-described steel plate and nut via the protrusion of the nut, whereby a joint between the steel plate and the nut is formed. Here, the "joint between the steel plate and the nut" refers to the portion where the steel plate and the nut are joined by fusion welding or solid-state welding, and is a portion derived from the protrusion of the nut.
[0043] The projection welded joint according to the present invention is characterized in that the minimum hardness Hvc (HV) of the steel plate in region c defined below and the base metal hardness Hvm (HV) of the steel plate satisfy the following formula (1): Hvc / Hvm≦0.85 (1)
[0044] Figure 2 shows a cross section of a projection welded joint 100 according to one embodiment of the present invention, the cross section including the center line 12 of the nut 10 and passing through the center of the joint between the steel plate 20 and the nut 10. The end point of the inner peripheral side of the nut 10 that contacts the steel plate 20 is designated A, the end point of the outer peripheral side is designated B, and the thickness of the steel plate at that cross section is designated t (mm). Points A1 and A2 are located within the steel plate 20 at distances of 0.20 mm and 2 / 3 t, respectively, from point A in the thickness direction of the steel plate 20. Points B1 and B2 are located within the steel plate 20 at distances of 0.20 mm and 2 / 3 t, respectively, from point B in the thickness direction of the steel plate 20. The rectangular area formed by connecting points A1, B1, B2, and A2 is designated region c. Figure 2 also shows a measurement region 30 for the base metal hardness Hvm.
[0045] Because the joint originates from the protrusion of the nut, the center of the joint corresponds to the position where the center of the nut's protrusion was. Figure 3 shows top views of (a) a nut 10A having three protrusions 16 and (b) a nut 10B having four protrusions 16, both of which are used in one embodiment of the present invention. The cutting line shown in Figure 3 is a line passing through the center line of the nut and the center of the protrusions 16. After projection welding the steel plate and the nut, the projection-welded joint is cut along the cutting line shown in Figure 3 to obtain the cross section shown in Figure 2.
[0046] When the ratio Hvc / Hvm of the minimum hardness Hvc of region c to the base metal hardness Hvm of the steel plate is 0.85 or less, region c is sufficiently softened, thereby improving the indentation peel strength and delayed fracture resistance. Therefore, Hvc / Hvm of the projection welded joint according to the present invention is set to 0.85 or less. Hvc / Hvm is preferably 0.83 or less, and more preferably 0.80 or less. On the other hand, when Hvc / Hvm is 0.55 or more, region c can be suitably tempered. Therefore, Hvc / Hvm is preferably 0.55 or more.
[0047] The minimum hardness Hvc of region c is determined as follows. Figure 4 shows an enlarged view of region c. In region c, hardness measurement points 32 are set at 0.20 mm intervals in a direction perpendicular to the thickness direction of the steel plate, starting from a point moved 0.10 mm or 0.30 mm from point B2 toward point B1. At each of the hardness measurement points 32 in region c, a measurement load of 300 gf is applied with an indenter for 15 seconds in accordance with JIS Z 2244 (2020), and the Vickers hardness is measured. The lowest value among the obtained measurement results is defined as the minimum hardness Hvc of region c.
[0048] When the minimum hardness Hvc of region c is 250 HV or more, the stress concentration can be suitably alleviated by softening region c. Therefore, the minimum hardness Hvc of region c is preferably 250 HV or more. On the other hand, when the minimum hardness Hvc of region c is 650 HV or less, the stress concentration can be suitably alleviated by softening region c. Therefore, the minimum hardness Hvc of region c is preferably 650 HV or less.
[0049] The base metal hardness Hvm of the steel plate is determined as follows. As shown in FIG. 2 , in the cross section of the projection welded joint 100, a point C1 is located 7.00 mm away from point B on the line formed by the surface of the steel plate 20. A point C2 is located 0.60 mm further away from point C1 on the line formed by the surface of the steel plate 20. A point C3 is located within the steel plate 20 0.60 mm away from point C2 in the thickness direction of the steel plate 20. A point C4 is located within the steel plate 20 0.60 mm away from point C1 in the thickness direction of the steel plate 20. The area inside the square formed by connecting points C1, C2, C3, and C4 is the measurement area 30 for the base metal hardness Hvm. Point C1 is located 7.00 mm away from point B to avoid thermal effects during welding. FIG. 5 shows an enlarged view of the measurement area 30 for the base metal hardness Hvm. The hardness measurement points 32 are set at 0.20 mm intervals in the thickness direction of the steel plate 20 and in the direction perpendicular to the thickness direction, starting from a point 0.20 mm away from point C1. At the nine hardness measurement points 32 shown in Figure 5, a measurement load of 300 gf is applied for 15 seconds using an indenter in accordance with JIS Z 2244 (2020), and the Vickers hardness is measured at each point. The average value obtained is the base material hardness Hvm. As described above, the base material hardness Hvm of the steel plate is measured at its cross section, and therefore is not affected by the presence or absence of a coating layer.
[0050] When the base material hardness Hvm of the steel plate is 400 HV or more, the softening effect can be suitably obtained in region c. Therefore, the base material hardness Hvm of the steel plate is preferably 400 HV or more. On the other hand, when the base material hardness Hvm of the steel plate is 700 HV or less, the softening effect can be suitably obtained in region c. Therefore, the base material hardness Hvm of the steel plate is preferably 700 HV or less, and more preferably 650 HV or less.
[0051] [Method for manufacturing a projection-welded joint] The method for manufacturing a projection-welded joint according to the present invention is a method for manufacturing a projection-welded joint by projection-welding a steel plate and a nut having a protrusion via the protrusion. The steel plate has the above-described composition, and the projection welding is performed at a current value I 1 (kA) and current flow time t 1(ms) to form a joint between the steel plate and the nut, and a non-energizing time t c1 A non-energizing step in which a non-energizing period of (ms) is provided, and a current value I that satisfies the following formula (3) is provided. 2 (kA), and the current application time t satisfies the following formula (4) 2 A first post-energization step in which current is applied for (ms), and a current value I that satisfies the following formula (5) 3 (kA), and the current application time t satisfies the following formula (6) 3 and a second post-energization step of energizing the semiconductor substrate for 800 <t (ms). c1 ...(2) 1.10I 1 ≦I 2 ≦1.80I 1 ... (3) 50≦t 2 ≦200...(4) I 3 ≦0.70I 2 ... (5) 300≦t 3 ≦1000 (6)
[0052] [Main Current-Applying Step] The main current-applying step is a step of forming a joint between the steel plate and the nut. In the main current-applying step, a current value I 1 The current flow time is t 1 The conditions for the main current application step described below are not particularly limited as long as a joint can be formed.
[0053] Current value I of the main current application process 1 When the current value I is 7.0 kA or more, the steel plate and the nut can be joined together suitably. 1 If the current value I in the main current application step is less than 7.0 kA, when the center of the joint is cut and the cross section is examined under a microscope after joining the steel plate and the nut, a gap is often observed between the steel plate and the nut. 1 is preferably 7.0 kA or more, and more preferably 8.0 kA or more. 1If the current value I is 30.0 kA or less, the joint will expand too much, causing the molten metal to splash out of the nut as spatter, and the projection part of the nut will be completely crushed, preventing it from functioning as a joint. 1 is preferably 30.0 kA or less, and more preferably 28.0 kA or less.
[0054] Current application time t of the main current application process 1 When the main current application time t is 70 ms or more, a stable weld can be obtained. 1 is preferably 70 ms or more, more preferably 100 ms or more, and even more preferably 160 ms or more. 1 If the energization time t of the main energization step is 500 ms or less, the welded portion will expand too much, causing the molten metal to splash out of the nut as spatter, and the projection portion of the nut will be completely crushed, preventing it from functioning as a welded portion. 1 is preferably 500 ms or less, and more preferably 400 ms or less.
[0055] When the pressure applied in the main current application process is 3.0 kN or more, the current diameter is of a suitable size, and the occurrence of expulsion can be suitably prevented. Therefore, the pressure applied in the main current application process is preferably 3.0 kN or more, and more preferably 3.5 kN or more. On the other hand, when the pressure applied in the main current application process is 6.0 kN or less, the current diameter is suitably prevented from expanding, and the weld can be suitably secured. Therefore, the pressure applied in the main current application process is preferably 6.0 kN or less, and more preferably 5.5 kN or less. Note that the pressure applied may be limited by the capacity of the equipment used, and may be adjusted appropriately to obtain the required weld diameter.
[0056] [First de-energization step and first post-energization step] After the main energization step, softening is performed on the projection welded joint, particularly on region c. Specifically, after the main energization step, a de-energization step, a first post-energization step, and a second post-energization step are performed. Softening region c alleviates stress concentration during a peel test and reduces residual stress, thereby preventing delayed fracture.
[0057] In the first de-energizing step, the projection welded joint is cooled to sufficiently lower the temperature of region c in order to obtain a softening effect.
[0058] In the first non-energizing step, the cooling time t c1 The weld is cooled by maintaining a non-energized state for 800 <t (ms). c1 (2) Cooling time t in the first de-energizing step c1 If the cooling time t is less than 800 ms, the region c cannot be sufficiently softened. As a result, even if subsequent processes are performed, the region c will have an embrittlement structure, which will easily cause stress concentration during the indentation peel test and make it easier for cracks to grow. Therefore, the cooling time t c1 The cooling time t c1 is preferably 850 ms or more, and more preferably 900 ms or more. c1 If the cooling time t is long, the processing time will increase. c1 is preferably 2500 ms or less.
[0059] Following the first non-energizing step, a first post-energizing step is performed. An electric current is applied to raise the temperature of the region c to an appropriate temperature range. The "appropriate temperature range" refers to a temperature range for softening the hardness of the region c. In the first post-energizing step, a current value I that satisfies the following formula (3) is applied. 2 (kA), and the current application time t satisfies the following formula (4) 2 (ms) 1.10I 1 ≦I 2 ≦1.80I 1 ... (3) 50≦t 2 ≦200 ... (4)
[0060] The inventors have found that region c can be softened by performing the first post-current step at a current value equal to or greater than that of the main current step. The post-current step softens region c, reducing its hardness, thereby alleviating the stress concentration applied to region c during a push-through peel test.
[0061] Current value I of the first post-current application step 2 is 1.10I 1 If the current value I is less than 1000 W, the region c cannot be effectively softened. 2 is 1.10I 1 That's it, 1.20I 1 On the other hand, the current value I 2 But 1.80I 1 If the temperature of region c exceeds A c3 The temperature at which the transformation from ferrite to austenite is completed is likely to be exceeded, resulting in embrittlement. As a result, the welded joint cannot be toughened. Therefore, the current value I 2 is 1.80I 1 Below, 1.70I 1 It is preferable that:
[0062] As described above, in the first post-current application step, the temperature is rapidly increased in a short time. Therefore, the current application time t 2 The energization time t must be 50 ms or more. 2 On the other hand, the current application time t 2 When the time exceeds 200 ms, the temperature of area c becomes A c3 Therefore, the current flow time t 2 is 200 ms or less, and preferably 180 ms or less.
[0063] In the projection welding according to the present invention, after the first post-current application step, a current value I that satisfies the following formula (5) is applied. 3 (kA), and the current application time t satisfies the following formula (6) 3A second post-current process is performed in which current is applied for a period of time equal to or longer than 100 ms. By performing the second post-current process, the region c can be softened more effectively, and residual stress can be reduced, facilitating relaxation of stress concentration. 3 ≦0.70I 2 ... (5) 300≦t 3 ≦1000 (6)
[0064] Current value I of the second post-current application process 3 is 0.70I 2 If the current value I in the second post-current application step is greater than 1000 W, it is not possible to perform appropriate temperature control to more effectively soften the region c. 3 is 0.70I 2 or less, 0.65I 2 It is preferable that the value is 0.60I or less. 2 On the other hand, the current value I in the second post-current application step is more preferably set to be equal to or less than the above. 3 But 0.15I 2 In the above case, the stress concentration is preferably alleviated by softening the region c. 3 is 0.15I 2 It is preferable that the value is 0.20I or more. 2 More preferably, it is set to be equal to or greater than this.
[0065] The second post-energization step is a step for softening the region c, and the energization time t 3 Therefore, when the energization time t of the second post-energization step is 300 ms or more, the softening can be effectively performed. 3 is 300 ms or more, preferably 350 ms or more, and more preferably 400 ms or more. 3 If the energization time t of the second post-energization step exceeds 1000 ms, the temperature will rise and there is a possibility that the temperature will rise again to near the melting point. 3 is set to 1000 ms or less, and preferably 900 ms or less.
[0066] Following the second post-current step, a de-energization step and a post-current step may be further repeatedly performed. Repeating the de-energization step and the post-current step is preferable because it enhances the effect of softening the region b. On the other hand, if the de-energization step and the post-current step are repeated too many times, the effect saturates, so the number of times these steps are repeated is preferably less than 10 times, and more preferably less than 4 times.
[0067] As described above, the projection welding method of the present invention can soften region c by appropriately controlling the welding conditions in the post-heat treatment step, thereby alleviating stress concentration and reducing residual stress. In other words, the projection-welded joint obtained by this welding method can improve the push-in peel strength. Therefore, even when welding steel sheets containing a relatively large amount of C in their chemical composition, specifically high-strength steel sheets with a tensile strength of 980 MPa or more and a C content of 0.05 to 0.50 mass %, as described above, the peel strength can be further improved.
[0068] For steps and conditions not described in this specification, conventional methods can be used.
[0069] As an example of the present invention, a projection welded joint was produced by projection welding a steel plate and a nut. The test specimens used were steel plates (Steel Plates A to M) with tensile strengths of 780 MPa to 1800 MPa and thicknesses of 1.0 to 1.8 mm. Table 1 shows the tensile strength (TS), thickness, and chemical composition of the steel plates A to M used. The remainder of the chemical composition listed in Table 1 is Fe and unavoidable impurities, and "-" indicates that the content of that element is below the detection limit.
[0070] Cold-rolled steel sheets or GA steel sheets (galvannealed steel sheets) of each steel sheet were prepared as test specimens. The test specimens had a long side of 50 mm and a short side of 50 mm, and an 11 mm diameter hole was drilled in the center of the test specimen. An M8 welding nut was also prepared, with three protrusions symmetrically spaced 120° apart from the centerline of the nut. The test specimen was set in an AC welding machine so that the center of the hole in the test specimen coincided with the center of the screw hole in the nut, and welded under the welding conditions shown in Table 2 to obtain a welded body. The steel type of the M8 welding nut was S25C (JIS G4051). Resistance welding was performed using a servomotor-pressurized single-phase AC (50 Hz) resistance welding machine attached to a welding gun, and projection-welded joints were produced. The pair of electrode tips used were flat 30 mm diameter electrodes. A bolt was fixed into the nut hole of the resulting projection-welded joint to prepare a bolted test specimen.
[0071]
[0072]
[0073] The hardness, peel strength and delayed fracture resistance of the base material and region c of the obtained projection welded joints and bolted test pieces were measured by the methods described below.
[0074] [Hardness Evaluation] The hardness of the base material and region c was measured as follows. The projection welded joint was cut at a position including the center line of the nut and passing through the center of the joint between the steel plate and the nut to obtain a test piece. The test piece was ultrasonically cleaned and then embedded in resin to obtain a sample. The thickness cross section of the obtained sample was polished and etched using a picric acid solution. The hardness of the thickness cross section of the etched sample was measured as described above, and the results are shown in Table 2. In the "Hardness Evaluation" column in Table 2, if the hardness measurement result satisfied formula (1) (i.e., if Hvc / Hvm≦0.85), it was marked as passing, and if it did not satisfy formula (1), it was marked as failing, with "○".
[0075] [Peel Strength Evaluation] Using the obtained bolt fastening test specimen, the maximum load when the nut peeled from the steel plate was measured by a push-peel test in accordance with JIS B1196:2010, and this measured value was taken as the peel strength (kN). In the present invention, the lower limit value (3.73 kN) of JIS B1196:2010 was used as the standard for peel strength, and peel strengths of less than 3.73 kN were evaluated as poor, with a rating of "x." Peel strengths of 3.73 kN or more but less than 6.00 kN were evaluated as equivalent to conventional peel strengths, with a rating of "△." Peel strengths of 6.00 kN or more were evaluated as excellent, with a rating of "○." Table 2 shows the measured peel strengths and their evaluation results.
[0076] [Evaluation of delayed fracture resistance] After leaving the projection welded joint for 24 hours, the joint was cut and embedded in resin, and the cross section of the weld was observed. The cross section was visually inspected to evaluate the occurrence of delayed fracture. Those in which delayed fracture occurred were evaluated as "x", and those in which delayed fracture did not occur were evaluated as "○".
[0077] As shown in Table 2, the projection-welded joints of the invention examples were good welded joints with excellent peel strength and delayed fracture resistance. In contrast, good projection-welded joints were not obtained in the comparative examples.
[0078] The present invention can provide a projection welded joint with improved peel strength and delayed fracture resistance.
[0079] 100 Projection welded joint 10 Nut 10A Nut with three protrusions 10B Nut with four protrusions 12 Center line of nut 14 Surface perpendicular to center line of nut 16 Protrusion 20 Steel plate 30 Measurement area for base material hardness Hvm 32 Hardness measurement point
Claims
1. A projection welded joint formed by projection welding a steel plate and a nut having a protrusion via the protrusion, wherein the steel plate contains, by mass%, C: 0.05-0.50%, Si: 0.1-2.0%, Mn: 1.5-4.0%, P: 0.10% or less, S: 0.005% or less, N: 0.010% or less, and O: 0.030% or less, and optionally further contains Al: 2.00% or less, B: 0.0050% or less, Ca: 0.005% or less, Cr: 1.00% or less, Cu: 0.80% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ti: 0.200% or less, V: 0.500% or less, A projection welded joint having a composition containing at least one element selected from the group consisting of Nb: 0.080% or less, Sb: 0.200% or less, and Sn: 0.200% or less, with the balance being Fe and unavoidable impurities, wherein a minimum hardness Hvc (HV) of a region c in the steel plate defined below and a base metal hardness Hvm (HV) of the steel plate satisfy the following formula (1): Hvc / Hvm≦0.85 ... (1) The region c is specified as follows in a cross section of the projection welded joint that includes the center line of the nut and passes through the center of the joint between the steel plate and the nut. The end point on the inner surface side of the nut that contacts the steel plate is A, the end point on the outer surface side is B, the thickness of the steel plate at the cross section is t (mm), points within the steel plate that are moved 0.20 mm and 2 / 3t from point A in the thickness direction of the steel plate are A1 and A2, respectively, and points within the steel plate that are moved 0.20 mm and 2 / 3t from point B in the thickness direction of the steel plate are B1 and B2, respectively, and the inside of the rectangle formed by connecting points A1, B1, B2, and A2 is defined as region c.
2. A method for manufacturing a projection welded joint by projection welding a steel plate and a nut having a protrusion via the protrusion, wherein the steel plate contains, by mass%, C: 0.05 to 0.50%, Si: 0.1 to 2.0%, Mn: 1.5 to 4.0%, P: 0.10% or less, S: 0.005% or less, N: 0.010% or less, and O: 0.030% or less, and optionally further contains Al: 2.00% or less, B: 0.0050% or less, Ca: 0.005% or less, Cr: 1.00% or less, Cu: 0.80% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ti: 0.200% or less, V: 0.500% or less, The steel sheet has a composition containing at least one element selected from the group consisting of Nb: 0.080% or less, Sb: 0.200% or less, and Sn: 0.200% or less, with the balance being Fe and unavoidable impurities, and the projection welding is performed at a current value I 1 (kA) and current flow time t 1 a main current application process in which a current is applied for a period of time t (ms) to form a joint between the steel plate and the nut; and c1 a non-energizing step in which a non-energizing period of 100 ms is provided; and a current value I 2 (kA), and the current application time t 2 A first post-current application step of applying current for a period of time of (ms), and a current value I satisfying the following formula (5): 3 (kA), and the current application time t 3 (ms), and a second post-current application step of applying current for 800<t c1 ...(2) 1.10I 1 ≦I 2 ≦1.80I 1 ... (3) 50 ≦ t 2 ≦200...(4) I 3 ≦0.70I 2 ... (5) 300 ≦ t 3 ≦1000 ... (6)
Citation Information
Patent Citations
Projection welding method
JP2004050280A
Nut projection-welding coupling
JP2010116592A
Projection welding joint and projection welding method
JP7020597B1
Method for producing rivet joint, rivet joint, and automobile part
WO2023047840A1
Cited By
Joint member manufacturing method
WO2026163521A1