Production method for recycled aluminum metal lump

Microwave irradiation and compression of aluminum scrap address the inefficiencies in current recycling methods, enhancing melting yield and reducing CO2 emissions, resulting in high-density recycled aluminum ingots with improved properties.

WO2024225447A1PCT designated stage expired Publication Date: 2024-10-31TOYOTA JIDOSHA KK +6
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016481
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current methods for recycling aluminum scrap into ingots are inefficient, with low dissolution yields and high energy consumption, and generate carbon dioxide, which contributes to global warming.

Method used

A method involving the irradiation of aluminum scrap with microwaves, combined with compression, to produce recycled aluminum metal ingots, which reduces energy requirements and improves melting efficiency while minimizing CO2 emissions.

Benefits of technology

This method enhances the melting yield of aluminum scrap, reduces the formation of oxides, and produces high-density recycled aluminum metal ingots with improved properties, such as increased density and reduced voids, thereby improving the recycling efficiency and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016481_31102024_PF_FP_ABST
    Figure JP2024016481_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for efficiently producing a recycled aluminum metal lump from aluminum scrap. The present invention relates to a production method for a recycled aluminum metal lump that includes a step for irradiating microwaves at aluminum metal that includes aluminum scrap.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method for recycled aluminum metal blocks

[0001] The present invention relates to a method for producing recycled aluminum ingots.

[0002] Lighter automotive parts can improve fuel efficiency and reduce power consumption, so there are currently studies being conducted to replace conventional iron-based materials with aluminum-based materials.

[0003] Aluminum bullion (ingot), which is the raw material for such aluminum-based materials, can be produced by refining bauxite, a raw ore, but refining requires a huge amount of energy. Therefore, in recent years, attempts have been made to recycle aluminum scrap generated from ingots and products to produce aluminum ingots or products.

[0004] For example, Patent Document 1 describes a method for refining aluminum scrap, in which aluminum scrap is melted in a melting furnace, refined to remove impurities from the melt, tapped, and cast into ingots of a predetermined size to be recycled into aluminum ingots again, by separating the melting step of the aluminum scrap from the refining step and connecting the refining step with the casting step, in which only the aluminum scrap is melted in the melting furnace and tapped into a ladle, the ladle is covered with a refractory lid communicated with an exhaust means, the atmosphere in the ladle is reduced to a predetermined pressure and maintained for a predetermined time, easily volatile components are removed from the molten metal, and then the pressure is restored to atmospheric pressure and the molten metal is continuously poured into a mold.

[0005] JP 2009-108346 A

[0006] Aluminum scrap can be broadly divided into processed scrap and obsolete scrap. Processed scrap mainly includes new aluminum cuttings generated from press factories and chips generated from machine factories.

[0007] In order to reuse such aluminum scrap, it is necessary to first briquette it through pre-treatments such as drying and compression molding, then melt it in molten aluminum, and cast it into aluminum ingots or products.

[0008] However, in the case of chips, for example, the percentage that dissolves in the molten aluminum, i.e., the melting yield, is only about 20%, and even in the case of briquettes, the melting yield in the molten aluminum is only about 40%. For this reason, efforts are being made to improve melting efficiency by stirring the molten aluminum or by inserting chips or briquettes into the gaps in the ingot.

[0009] In addition, the melting of aluminum scrap into molten aluminum increases the temperature of the molten aluminum during refining and by using flux treatment, carbon dioxide (CO 2 ) is generated, and CO 2 It is necessary to reduce CO2 emissions because they can cause global warming.

[0010] Therefore, an object of the present invention is to provide a method for efficiently producing recycled aluminum metal ingots from aluminum scrap.

[0011] The present inventors have investigated various means for solving the above problems, and as a result have discovered that recycled aluminum ingots can be produced by irradiating aluminum scrap with microwaves, thereby completing the present invention.

[0012] That is, the gist of the present invention is as follows: (1) A method for producing recycled aluminum metal ingots, comprising a step of irradiating aluminum metal including aluminum scrap with microwaves. (2) The method according to (1), in which the aluminum scrap is aluminum scrap in one or more forms selected from the group consisting of powder, chips, burrs, and briquettes. (3) The method according to (1) or (2), further comprising a step of compressing the aluminum metal. (4) The method according to (3), in which the step of compressing the aluminum metal is carried out before, during, and / or after microwave irradiation. (5) The method according to (3) or (4), in which the step of compressing the aluminum metal is carried out using a mold. This specification incorporates the disclosure of Japanese Patent Application No. 2023-074519, from which the present application claims priority.

[0013] The present invention provides a method for efficiently producing recycled aluminum ingots from aluminum scrap.

[0014] Photographs of the exterior and interior of Comparative Example 1 and Example 1. Photographs of the cross-sectional structures of Comparative Example 2 and Example 1. Photographs showing the appearance of chips, Comparative Example 2, and Example 1 after melting. Table showing the results of an experiment to melt chips, Comparative Example 2, and Example 1 in molten aluminum.

[0015] Preferred embodiments of the present invention are described in detail below. In this specification, the features of the present invention are described with reference to the drawings as appropriate. The method for producing recycled aluminum metal ingots of the present invention is not limited to the following embodiments, and can be implemented in various forms incorporating modifications and improvements that can be made by those skilled in the art, without departing from the gist of the present invention. Furthermore, in the present invention, the expression "numerical value (lower limit) to numerical value (upper limit)" indicates a range that includes both the lower limit and the upper limit.

[0016] The present invention relates to a method for producing recycled aluminum metal ingots, which includes a step of irradiating aluminum metal containing aluminum scrap with microwaves (a step of irradiating aluminum metal with microwaves).

[0017] In the present invention, aluminum metal refers to a metal and / or alloy containing aluminum (Al) as a main component, and recycled aluminum metal ingot refers to a metal ingot and / or alloy ingot containing aluminum (Al) as a main component.

[0018] The aluminum metal includes aluminum scrap as an aluminum source (aluminum material).

[0019] Examples of aluminum scrap include recycled materials for scrap metals and chips generated during the manufacturing process of aluminum automotive parts, relatively high-quality aluminum scrap foil and printing plates, 5000 series scrap (Al-Mg alloy), 6000 series scrap (Al-Mg-Si alloy), and 7000 series scrap (Al-Zn-Mg alloy) (including, for example, automobile and home appliance panel materials, wrought aluminum materials such as radiators, and aircraft component materials). Depending on the chemical composition of the aluminum scrap, not only one type but two or more types may be used. Aluminum scrap whose composition has not been confirmed may also be used.

[0020] The aluminum scrap is aluminum scrap in one or more forms selected from the group consisting of, for example, powder, chips, burrs, briquettes, etc. Here, briquettes are produced by compressing fine aluminum scrap such as chips and burrs. When the aluminum scrap is a mixture of two or more forms, the mixture may be homogeneous or heterogeneous. In one embodiment, the mixture is homogeneous.

[0021] The proportion of aluminum scrap contained in the aluminum metal is not limited. The aluminum other than aluminum scrap as the aluminum source contained in the aluminum metal may be pure aluminum ingot or metal block and / or aluminum alloy. The proportion of aluminum scrap contained in the aluminum metal may be 100 mass% based on the total mass of the aluminum metal.

[0022] The aluminum metal may contain, in addition to Al as the main component, other modifying alloy elements, such as boron (B), carbon (C), nitrogen (N), silicon (Si), magnesium (Mg), manganese (Mn), iron (Fe), copper (Cu), titanium (Ti), nickel (Ni), zirconium (Zr), cobalt (Co), molybdenum (Mo), tungsten (W), zinc (Zn), lithium (Li), silver (Ag), gallium (Ga), germanium (Ge), scandium (Sc), strontium (Sr), indium (In), vanadium (V), praseodymium (Pr), samarium (Sm), tantalum (Ta), gold (Au), beryllium (Be), and chromium. (Cr), arsenic (As), selenium (Se), yttrium (Y), niobium (Nb), ruthenium (Ru), rhodium (Rh), palladium (Pd), cadmium (Cd), tin (Sn), antimony (Sb), tellurium (Te), cerium (Ce), neodymium (Nd), promethium (Pm), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), lutetium (Lu), hafnium (Hf), rhenium (Re), iridium (Ir), platinum (Pt), mercury (Hg), bismuth (Bi), and thorium (Th).

[0023] The other elements may be added to the aluminum metal as pure metal, compounds, alloys, etc. Basically, metals with high melting points can be added as master alloys with other added elements, and metals with low melting points can be added as pure metals. The addition of the other elements can be carried out before, during, and / or after microwave irradiation. Alternatively, the other elements may be contained in advance as alloy components in aluminum scrap and / or aluminum alloys in the aluminum metal.

[0024] It should be noted that "before, during, and / or after microwave irradiation" refers to one or more time points among before, during, and after microwave irradiation.

[0025] The content of each of the above other elements is not limited. The content of each of the other elements, as metal, is typically 0.0001% by mass to 20% by mass, and in one embodiment, 0.001% by mass to 12% by mass, based on the total mass of the aluminum metal. The content of all of the other elements, as metal, is typically 0.01% by mass to 30% by mass, in one embodiment, 0.01% by mass to 16% by mass, and in another embodiment, 0.01% by mass to 5% by mass, based on the total mass of the aluminum metal. The content of the other elements can be measured by a method known in the art, and although it varies depending on the alloying element, it can be measured, for example, by ICP atomic emission spectroscopy.

[0026] The balance other than aluminum and other elements in the aluminum metal of the present invention consists of unavoidable impurities, organic matter such as coolant (cutting oil) and lubricating oil used in processing aluminum products that may be contained in the aluminum scrap, and moisture.

[0027] Examples of unavoidable impurities include phosphorus (P) and sulfur (S). The contents of phosphorus (P) and sulfur (S) are not limited. The contents of phosphorus (P) and sulfur (S) are usually 0.01 mass% or less based on the total mass of aluminum metal. The contents of phosphorus (P) and sulfur (S) can be measured by methods known in the art, and although the method varies depending on the element being measured, they can be measured, for example, by ICP atomic emission spectroscopy.

[0028] Organic matter and moisture that may be contained in the aluminum scrap may be removed in advance by a method known in the art, such as drying at a temperature of typically 100°C to 600°C.

[0029] The size of the aluminum metal is not limited. When irradiating the aluminum metal with microwaves, the aluminum metal and / or the microwave irradiation source can be moved so that the aluminum metal is evenly irradiated with microwaves.

[0030] The microwaves irradiated onto the aluminum metal are not limited.

[0031] The microwaves are generated by a microwave radiation source (a microwave generator (magnetron)). The microwave radiation source can be either a single-mode system or a multi-mode system.

[0032] The number of microwave irradiation sources is not limited and may be one, two or more.

[0033] The output of the microwave irradiation source is not limited and is generally 1 W to 10 kW, and in one embodiment, the output of the microwave irradiation source is 500 W for home use to 10 kW for industrial use.

[0034] The frequency of the microwaves generated from the microwave irradiation source can be changed as appropriate and is not limited. The microwave frequency is usually 0.9 GHz to 10 GHz, and in one embodiment, 2 GHz to 6 GHz. In one embodiment, the microwave frequency is 2.45 GHz, which is the frequency of an industrial microwave power supply.

[0035] The microwave irradiation time for the aluminum metal is not limited. The microwave irradiation time can be appropriately changed depending on the reaction conditions (composition and amount of aluminum metal, microwave conditions, pressure, atmosphere, temperature during microwave irradiation, etc.). The microwave irradiation time is usually 0.1 to 600 seconds, and in one embodiment, 60 to 300 seconds.

[0036] In one embodiment, the microwave irradiation is uniform during irradiation. In one embodiment, the microwave irradiation conditions are constant during microwave irradiation.

[0037] In the present invention, recycled aluminum ingots can be produced by irradiating aluminum metal, including aluminum scrap, with microwaves, and the high-density energy of microwaves allows recycled aluminum ingots to be produced in a short time.

[0038] Aluminum metal can also be compressed.

[0039] Therefore, the method for producing recycled aluminum metal ingots of the present invention may further include a step of compressing the aluminum metal (aluminum metal compressing step).

[0040] The aluminum metal compaction process is not limited and can be carried out using techniques known in the art, such as uniaxial compaction, cold isostatic pressing (CIP), hot isostatic pressing (HIP), and roller compaction.

[0041] The above-mentioned compression step of the aluminum metal may be carried out using, for example, a mold, which may be made of metal such as aluminum or iron.

[0042] The use of a mold in the above-mentioned aluminum metal compression process can prevent fine aluminum scrap, such as powder or chips, from scattering, particularly during microwave irradiation, i.e., heating. Furthermore, by using a mold in the shape of the product as the mold, the produced recycled aluminum metal ingot can be used as a product as is. The contamination of metal molds and cutting tools that may be used as molds can be avoided by, for example, introducing a magnetic separation process.

[0043] Furthermore, the timing of the aluminum metal compression step is not limited. Thus, the aluminum metal compression step can be carried out before, during, and / or after microwave irradiation. For example, by carrying out the aluminum metal compression step before microwave irradiation and preparing aluminum metal of an appropriate size, it becomes easier to introduce the aluminum metal into a mold that can be used for microwave irradiation, etc. By carrying out the aluminum metal compression step during and / or after microwave irradiation, the density of the resulting recycled aluminum metal block can be increased.

[0044] The pressure in the above-mentioned compressing step of the aluminum metal is not limited, and the pressure in the above-mentioned compressing step of the aluminum metal is usually 10 MPa to 500 MPa.

[0045] The time for the above-mentioned compressing step of aluminum metal is not limited. The time for the above-mentioned compressing step of aluminum metal is until the aluminum metal is formed or shaped by the compressing step of aluminum metal. The time for the above-mentioned compressing step of aluminum metal is usually 0.1 seconds to 60 seconds, and in one embodiment, 2 seconds to 5 seconds.

[0046] The temperature in the above-mentioned aluminum metal compression process is not limited.

[0047] The method for producing recycled aluminum ingots of the present invention includes a compression step of aluminum metal, which makes it possible to remove organic matter and moisture that may be contained in aluminum scrap by leaching (extracting) and separating it, and further prevents the formation of cracks due to gasification in the finally obtained recycled aluminum ingots, thereby increasing the density of the aluminum ingots. The increased density of the recycled aluminum ingots produced by the production method of the present invention makes it possible to improve the melting yield when the aluminum ingots are melted for use.

[0048] The atmosphere in the method for producing recycled aluminum ingots of the present invention is not limited. The method for producing recycled aluminum ingots of the present invention may be carried out in air, an inert gas such as argon (Ar) and / or helium (He), or a neutral gas such as nitrogen (N 2 ), dry hydrogen (dry H 2 ) and / or ammonia (NH 3 ) atmosphere.

[0049] The method for producing recycled aluminum metal ingots of the present invention, particularly the step of irradiating aluminum metal with microwaves, is carried out in a reducing atmosphere, for example, in a hydrogen (H 2 ), carbon monoxide (CO), and / or hydrocarbon gases (e.g., CH 4 , C 3 H 8 , C 4 H 10Alternatively, the method for producing recycled aluminum metal ingots of the present invention, particularly the step of irradiating aluminum metal with microwaves, may be carried out by placing a reducing agent, such as carbon, near the aluminum metal, for example, by mixing the aluminum metal with the reducing agent.

[0050] By carrying out the present invention in a reducing atmosphere or in the presence of a reducing agent, further oxidation of aluminum metal, particularly aluminum scrap, can be prevented or oxidized aluminum metal can be reduced to metallic aluminum, thereby reducing the proportion of oxides in the resulting recycled aluminum metal ingot. Therefore, when the recycled aluminum metal ingot obtained in this manner is melted for use, the amount of slag and slag generated during melting can be reduced, and the melting yield can be improved.

[0051] The method for producing recycled aluminum ingots of the present invention does not necessarily require the preparation of molten aluminum, which is normally carried out when producing recycled aluminum ingots. Therefore, from the viewpoint of life cycle assessment (LCA), the CO generated is 2 The amount can be reduced.

[0052] The density of the recycled aluminum ingot produced by the present invention can be adjusted as needed. For example, the recycled aluminum ingot produced by the present invention can be made high density, and its density is usually 2.00 g / cm 3 ~ True density of aluminum metal (for example, 2.70 g / cm for metallic aluminum) 3 Alternatively, the density of the recycled aluminum ingot produced by the present invention can be typically 99% or more, with 100% being the density when the recycled aluminum ingot is completely metal or alloy.

[0053] Therefore, when the recycled aluminum ingot produced by the present invention is melted and used, the melting yield can be improved. Furthermore, the recycled aluminum ingot produced by the present invention can be used as is as a product such as a part, or can be formed into a product such as a part by processing such as cutting. Furthermore, the high-density recycled aluminum ingot produced by the present invention can be used in the same way as a normal aluminum ingot.

[0054] When the recycled aluminum ingot produced by the present invention contains Si as an additional element, the internal structure is composed of a granular Si phase and an aluminum eutectic. This is because the recycled aluminum ingot produced by the present invention is formed in a short time, and dendrites are not formed (exist) in the internal structure. Furthermore, the recycled aluminum ingot produced by the present invention has boundaries in the internal structure. Note that the recycled aluminum ingot produced by the present invention also has voids in the internal structure. However, the recycled aluminum ingot produced by the present invention can be made high-density, and its density can be within the above-mentioned range, so the volume of the voids can be reduced.

[0055] Hereinafter, several examples of the present invention will be described, but it is not intended that the present invention be limited to those shown in these examples.

[0056] I. Sample Preparation Example 1 Aluminum chips (Cu: 1.5% by mass to 3.5% by mass, Si: 9.6% by mass to 12% by mass, Mg: 0.3% by mass or less, Zn: 1.0% by mass or less, Fe: 1.3% by mass or less, Mn: 0.5% by mass or less, Ni: 0.5% by mass or less, Sn: 0.2% by mass or less, Pb: 0.2% by mass or less, Ti: 0.3% by mass or less, Al: balance) as aluminum scrap were irradiated with microwaves at 1 kW while applying a pressure of 5 MPa using a silicon nitride mold in an argon atmosphere, to produce the recycled aluminum metal ingot of Example 1.

[0057] Comparative Example 1 Briquettes of Comparative Example 1 were produced by compressing aluminum chips (Cu: 1.5% by mass to 3.5% by mass, Si: 9.6% by mass to 12% by mass, Mg: 0.3% by mass or less, Zn: 1.0% by mass or less, Fe: 1.3% by mass or less, Mn: 0.5% by mass or less, Ni: 0.5% by mass or less, Sn: 0.2% by mass or less, Pb: 0.2% by mass or less, Ti: 0.3% by mass or less, Al: balance) as aluminum scrap at a pressure of 5 MPa in an argon atmosphere.

[0058] Comparative example 2 As Comparative Example 2, aluminum ingot (ADC12, cut product, Cu: 1.5% by mass to 3.5% by mass, Si: 9.6% by mass to 12% by mass, Mg: 0.3% by mass or less, Zn: 1.0% by mass or more) Below, Fe: 1.3% by mass or less, Mn: 0.5% by mass or less, Ni: 0.5% by mass or less, Sn: 0.2% by mass or less, Pb: 0.2% by mass or less, Ti: 0.3% by mass or less, Al: remainder).

[0059] II. Evaluation (External Appearance and Internal Observation) The external appearance and internal observation using an optical microscope were carried out for the briquette of Comparative Example 1 and the recycled aluminum metal ingot of Example 1. The results are shown in FIG.

[0060] 1, the appearance of the briquette of Comparative Example 1 was that it had internal voids and was low density, whereas the appearance of the recycled aluminum ingot of Example 1 had a metallic luster like that of metallic aluminum, and internal observation confirmed that it was high density.

[0061] (Cross-sectional structure observation) Cross-sectional structure observation was carried out with an optical microscope for the aluminum ingot of Comparative Example 2 and the recycled aluminum metal block of Example 1. The results are shown in FIG.

[0062] 2 reveals the following: In the aluminum ingot of Comparative Example 2, the internal structure was composed of an acicular Si phase and an aluminum eutectic, and dendrites were formed in the internal structure.

[0063] On the other hand, the recycled aluminum metal ingot of Example 1 had an internal structure consisting of a granular Si phase and aluminum eutectic, and no dendrites were formed in the internal structure. Furthermore, the recycled aluminum metal ingot of Example 1 had clearer boundaries and voids in the internal structure compared to the aluminum ingot of Comparative Example 2. However, the recycled aluminum metal ingot of Example 1 had a high density, with its density being 99% or more, with 100% being the density when the aluminum metal ingot was completely metal (alloy), and therefore the volume of the voids was small.

[0064] In other words, in the aluminum ingot of Comparative Example 2, dendrites are formed as the molten metal solidifies slowly when placed in a mold and formed, whereas in the recycled aluminum metal block of Example 1, dendrites are not formed because the recycled aluminum metal block is formed in a short time by microwave irradiation.

[0065] Furthermore, in Example 1, melting is not required in the manufacturing process, making it possible to manufacture metal ingots on-site, and furthermore, oxidation of the attached coolant can be prevented. Therefore, Example 1 is a CO 2 This allows for reduction.

[0066] When aluminum alloys were used as aluminum scrap, the boundary tended to be thinner in aluminum alloys having an alloy composition used as a wrought material, such as A6061, which has fewer impurities, compared to aluminum alloys having an alloy composition with a higher impurity content.

[0067] Approximately 28 g each of the cutting chips, the aluminum ingot of Comparative Example 2, and the recycled aluminum metal block of Example 1 was placed in a furnace at a temperature of 800° C. and melted for approximately 30 minutes, and the gas and oxidation conditions in the furnace were confirmed. The results are shown in FIG.

[0068] As can be seen from Figure 3, the chips contained a large amount of oxides even during melting, resulting in a very poor melting yield, while the recycled aluminum metal block of Example 1 contained slightly more oxides than the aluminum ingot of Comparative Example 2, but no gas was generated.

[0069] (Melting test in molten aluminum) Approximately 28 g each of the cutting chips, the aluminum ingot of Comparative Example 2, and the recycled aluminum metal lump of Example 1 was dissolved in molten aluminum. The results are shown in FIG.

[0070] 4, it can be seen that although the chips floated on the molten metal and the melting yield was less than 40%, the melting yield of the recycled aluminum metal ingot in Example 1 was improved to 60% or more. All publications, patents, and patent applications cited herein are hereby incorporated by reference in their entirety.

Claims

1. A method for producing recycled aluminum metal ingot, comprising the step of irradiating aluminum metal, including aluminum scrap, with microwaves.

2. The method according to claim 1, wherein the aluminum scrap is in one or more forms selected from the group consisting of powder, chips, burrs and briquettes.

3. The method of claim 1 or 2, further comprising the step of compressing the aluminum metal.

4. The method of claim 3, wherein the step of compressing the aluminum metal is carried out before, during, and / or after microwave irradiation.

5. The method of claim 3, wherein the step of compressing the aluminum metal is carried out using a form.

6. The method of claim 4, wherein the step of compressing the aluminum metal is carried out using a form.

Citation Information

Patent Citations

  • Method and apparatus for refining aluminum scrap

    JP2009108346A

  • Patterning method of quantum dot, manufacturing method of optical element, manufacturing method of backlight unit and manufacturing method of image display device

    JP2023074519A

  • Manufacturing method of aluminum-scandium alloy

    JP2018178180A

  • Process for producing microcrystalline α-alumina by microwave calcination

    JP2022171629A

  • Method for recovering processed aluminum scraps of aeronautical aluminum alloy