Thermoelectric conversion element and thermoelectric conversion method

The thermoelectric conversion element with electrodes of differing conductivities and an organic semiconductor layer enables efficient electrical energy conversion in constant temperature environments, overcoming the limitations of conventional methods by using abundant materials and achieving high electromotive forces.

WO2024225487A1PCT designated stage expired Publication Date: 2024-10-31TSUJIUCHI YUTAKA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016610
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional thermoelectric conversion methods require a temperature difference between electrodes, which is not always feasible, and rely on rare metals like bismuth tellurium, making them economically inefficient.

Method used

A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials with different conductivities, along with an organic semiconductor layer that generates electrons and holes through thermal excitation, allowing for electrical energy conversion in a constant temperature environment without the need for a temperature gradient, using materials like indium tin oxide, carbon, and phthalocyanine-based compounds.

Benefits of technology

This approach enables efficient conversion of thermal energy into electrical energy in environments without temperature differences, using abundant and cost-effective materials, and achieves electromotive forces significantly higher than traditional thermocouples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016610_31102024_PF_FP_ABST
    Figure JP2024016610_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a thermoelectric conversion element including a positive electrode and a negative electrode made of materials different in conductivity and capable of converting thermal energy to electric energy even in an environment having no temperature difference and comprising an organic semiconductor layer provided, between the positive electrode and the negative electrode, with a material that generates electrons and holes when thermally excited. Also provided is a thermoelectric conversion method using the thermoelectric conversion element.
Need to check novelty before this filing date? Find Prior Art

Description

Thermoelectric conversion element and thermoelectric conversion method

[0001] The present invention relates to a thermoelectric conversion element and a thermoelectric conversion method, and more particularly to a thermoelectric conversion element that can be used in an isothermal environment and a thermoelectric conversion method using the thermoelectric conversion element.

[0002] A conventional technique for directly converting thermal energy into electrical energy utilizes the phenomenon of generating a voltage proportional to a temperature difference between two ends of a rod-shaped metal or semiconductor sample by heating one end and cooling the other. This phenomenon was discovered by T.J. Seebeck in 1821 and was named the Seebeck effect (Non-Patent Documents 1-3). Conversely, a phenomenon in which heating or cooling occurs depending on the direction of current when a current is passed through one end is known. This phenomenon was discovered by J.C. Peltier in 1834 and is named the Peltier effect (Non-Patent Document 4).

[0003] Furthermore, based on the principle of the Seebeck effect, when an n-type semiconductor and a p-type semiconductor are placed side by side and a temperature difference is applied, the carriers that carry electric charges in the semiconductor are diffused by the heat, which generates an electromotive force. As an example of a method that has been known to generate a large electromotive force, a method that uses a bismuth-tellurium material containing the elements bismuth and tellurium is known (Non-Patent Document 5).

[0004] Seebeck, TJ (1822). "On the Magnetism of the Galvanic Chain." Proceedings of the Physical Class of the Royal Prussian Academy of Sciences from the years 1820-1821: 289-346. Seebeck, TJ (1825). "Magnetic Polarization of Metals and Minerals by Temperature Differences." Treatises of the Royal Academy of Sciences in Berlin, pp. 265-373. Seebeck (1826) "On the Magnetic Polarization of Metals and Minerals by Temperature Differences." (On the magnetic polarization of metals and minerals by temperature differences), Annals of Physics and Chemistry, 6: 1-20, 133-160, 253-286.Peltier (1834). "Nouvelles experiences sur la caloricite des courants electrique" [New experiments on the heat effects of electric currents]. Annales de Chimie et de Physique (in French). 56: 371-386.FD Rosi, B. Abeles and RV Jensen, J. Phys.Chem. Solids, 10, 191-200 (1959).

[0005] However, the methods of References 1 to 3 always require a low-temperature section and a high-temperature section, and it cannot be said that an environment that widely satisfies such conditions can be ensured. Furthermore, the technology of Reference 5 requires the use of rare metals, bismuth and tellurium, making it less economical. The present invention aims to provide a thermoelectric conversion element that can convert thermal energy into electrical energy even in an environment without a temperature difference, and a thermoelectric conversion method using the thermoelectric conversion element.

[0006] The present inventors have conducted extensive research to solve the above problems and have completed the following invention.

[0007] [1] A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials with different electrical conductivities, and an organic semiconductor layer between the positive electrode and the negative electrode, the organic semiconductor layer comprising a material that generates electrons and holes upon thermal excitation. [2] The thermoelectric conversion element according to [1], wherein the difference in electrical conductivity between the high-conductivity material constituting the negative electrode and the low-conductivity material constituting the positive electrode is 50 S / m or more and 10,000 S / m or less.

[0008] [3] The thermoelectric conversion element according to [1] or [2], wherein the positive electrode is indium tin oxide or a carbon material, and the negative electrode is a metal material. [4] The thermoelectric conversion element according to any one of [1] to [3], wherein the material that generates electrons and holes upon thermal excitation is a viscous liquid containing a material that generates electrons and holes upon thermal excitation.

[0009] [5] The thermoelectric conversion element according to [4], wherein the viscous liquid is a viscous liquid capable of transporting ions as charge carriers. [6] The thermoelectric conversion element according to any one of [1] to [5], wherein the material that generates electrons and holes upon thermal excitation is iron phthalocyanine or zinc phthalocyanine.

[0010] [7] A thermoelectric conversion method comprising a step of placing the thermoelectric conversion element according to any one of [1] to [6] in a thermal environment.

[0011] [8] A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials with different electrical conductivities, and an organic semiconductor layer between the positive electrode and the negative electrode, the organic semiconductor layer comprising a material that generates electrons and holes upon thermal excitation, wherein the organic semiconductor layer comprises a first organic semiconductor layer on the positive electrode side and a second semiconductor layer on the negative electrode side, and wherein the energy level of a HOMO of the first organic semiconductor layer is higher than the energy level of a HOMO of the second semiconductor layer.

[0012] [9] The thermoelectric conversion element according to [8], wherein the difference in conductivity between the high conductivity material constituting the negative electrode and the low conductivity material constituting the positive electrode is 50 S / m or more and 10,000 S / m or less.

[10] The thermoelectric conversion element according to [8] or [9], wherein the positive electrode is made of indium tin oxide or a carbon material, and the negative electrode is made of a metal material.

[0013]

[11] The thermoelectric conversion element according to any one of [8] to

[10] , wherein the material that generates electrons and holes upon thermal excitation is a viscous liquid containing a material that generates electrons and holes upon thermal excitation.

[12] The thermoelectric conversion element according to

[11] , wherein the viscous liquid is a viscous liquid that can transport ions as charge carriers.

[0014]

[13] The thermoelectric conversion element according to any one of [8] to

[12] , wherein the material that generates electrons and holes upon thermal excitation is iron phthalocyanine or zinc phthalocyanine.

[14] The thermoelectric conversion element according to any one of [8] to

[13] , wherein the material that generates electrons and holes upon thermal excitation contained in the first organic semiconductor layer is iron phthalocyanine, and the material that generates electrons and holes upon thermal excitation contained in the second organic semiconductor layer is zinc phthalocyanine.

[0015]

[15] A thermoelectric conversion method, comprising placing the thermoelectric conversion element according to any one of [8] to

[14] in a thermal environment.

[0016]

[16] A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials with different electrical conductivities, and an organic semiconductor layer between the positive electrode and the negative electrode, the organic semiconductor layer comprising a material that generates electrons and holes upon thermal excitation, the organic semiconductor layer further comprising ions of a transition metal.

[17] The thermoelectric conversion element according to

[16] , wherein the difference in electrical conductivity between the high-conductivity material constituting the negative electrode and the low-conductivity material constituting the positive electrode is 50 S / m or more and 10,000 S / m or less.

[0017]

[18] The thermoelectric conversion element according to

[16] or

[17] , wherein the positive electrode is indium tin oxide or a carbon material, and the negative electrode is a metal material.

[19] The thermoelectric conversion element according to any one of

[16] to

[18] , wherein the material that generates electrons and holes upon thermal excitation is a viscous liquid containing a material that generates electrons and holes upon thermal excitation.

[20] The thermoelectric conversion element according to

[19] , wherein the viscous liquid is a viscous liquid that can transport ions as charge carriers.

[0018]

[21] The thermoelectric conversion element according to any one of

[16] to

[20] , wherein the material that generates electrons and holes upon thermal excitation is iron phthalocyanine or zinc phthalocyanine.

[22] The thermoelectric conversion element according to any one of

[16] to

[21] , wherein the transition metal ions are one or more ions selected from iron ions, manganese ions, zinc ions, copper ions, cobalt ions, and nickel ions.

[23] A thermoelectric conversion method comprising a step of placing the thermoelectric conversion element according to any one of

[16] to

[22] in a thermal environment.

[0019]

[24] A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials with different electrical conductivities, and an organic semiconductor layer between the positive electrode and the negative electrode, the organic semiconductor layer comprising a material that generates electrons and holes upon thermal excitation, wherein the organic semiconductor layer comprises a first organic semiconductor layer on the positive electrode side and a second semiconductor layer on the negative electrode side, and further comprising a layer made of a carbon-based substance between the first organic semiconductor layer and the second semiconductor layer.

[0020]

[25] The thermoelectric conversion element according to

[24] , wherein the difference in conductivity between the high conductivity material constituting the negative electrode and the low conductivity material constituting the positive electrode is 50 S / m or more and 10,000 S / m or less.

[26] The thermoelectric conversion element according to

[24] or

[25] , wherein the positive electrode is made of indium tin oxide or a carbon material, and the negative electrode is made of a metal material.

[0021]

[27] The thermoelectric conversion element according to any one of

[24] to

[26] , wherein the material that generates electrons and holes upon thermal excitation is a viscous liquid containing a material that generates electrons and holes upon thermal excitation.

[28] The thermoelectric conversion element according to

[27] , wherein the viscous liquid is a viscous liquid that can transport ions as charge carriers.

[0022]

[29] The thermoelectric conversion element according to any one of

[24] to

[28] , wherein the HOMO energy level of the first organic semiconductor layer is higher than the HOMO energy level of the second semiconductor layer.

[30] The thermoelectric conversion element according to any one of

[24] to

[29] , wherein the material that generates electrons and holes upon thermal excitation is iron phthalocyanine or zinc phthalocyanine.

[0023]

[31] The thermoelectric conversion element according to any one of

[24] to

[30] , wherein the material contained in the first organic semiconductor layer that generates electrons and holes upon thermal excitation is iron phthalocyanine, and the material contained in the second organic semiconductor layer that generates electrons and holes upon thermal excitation is zinc phthalocyanine.

[32] The thermoelectric conversion element according to any one of

[24] to

[31] , wherein the layer made of a carbon-based substance is a layer made of graphite.

[33] A thermoelectric conversion method comprising a step of placing the thermoelectric conversion element according to any one of

[24] to

[32] in a thermal environment.

[0024] According to the thermoelectric conversion element and the thermoelectric conversion method of the present invention, thermal energy can be converted into electrical energy even in an environment without a temperature difference.

[0025] FIG. 1 is a schematic diagram of a thermoelectric conversion element of the first embodiment of the present invention. FIG. 2 is a model diagram for theoretically explaining the thermoelectric conversion element of the first embodiment of the present invention. FIG. 3 is an optical absorption spectrum measured for iron phthalocyanine (FePc). FIG. 4 is an optical absorption spectrum measured for zinc phthalocyanine (ZnPc). FIG. 5 is a circuit diagram assembled to measure electrical energy for elements prepared in Examples and Comparative Examples. FIG. 6(a) shows the voltage measurement results for the element of Comparative Example 1-1, and FIG. 6(b) shows the current measurement results for the element of Comparative Example 1-1. FIG. 7(a) shows the voltage measurement results for the element of Comparative Example 1-2, and FIG. 7(b) shows the current measurement results for the element of Comparative Example 1-2. FIG. 8(a) shows the voltage measurement results for the element of Example 1-1, and FIG. 8(b) shows the current measurement results for the element of Example 1-1. FIG. 9(a) shows the voltage measurement results for the element of Example 1-2, and FIG. 9(b) shows the current measurement results for the element of Example 1-2. FIG. 10 shows the measurement results of the current and voltage of the element of Comparative Example 1-3. FIG. 11 shows the measurement results of the current and voltage of the element of Comparative Example 1-4. FIG. 12 is a schematic diagram of a thermoelectric conversion element of the second embodiment of the present invention. FIG. 13 is a model diagram for theoretically explaining the thermoelectric conversion element of the second embodiment of the present invention. FIG. 14 shows the optical absorption spectrum measured for iron phthalocyanine (FePc). FIG. 15 shows the optical absorption spectrum measured for zinc phthalocyanine (ZnPc). FIG. 16 is a circuit diagram assembled to measure the electrical energy of the elements prepared in the examples and comparative examples. FIG. 17(a) shows the measurement results of the voltage of the element of Comparative Example 2-1, and FIG. 17(b) shows the measurement results of the current of the element of Comparative Example 2-1. FIG. 18(a) shows the measurement results of the voltage of the element of Comparative Example 2-2, and FIG. 18(b) shows the measurement results of the current of the element of Comparative Example 2-2. FIG. 19 shows the measurement results of the current and voltage of the element of Comparative Example 2-3. Fig. 20 shows the measurement results of the current and voltage of the element of Comparative Example 2-4. Fig. 21(a) shows the measurement results of the current value versus temperature of Example 2-1, Fig. 21(b) shows the measurement results of the voltage value versus temperature of Example 2-1, and Fig. 21(c) shows the measurement results of the power value versus temperature of Example 2-1.Figure 22(a) shows the measurement results of current values ​​versus temperature for Comparative Example 2-5, Figure 22(b) shows the measurement results of voltage values ​​versus temperature for Comparative Example 2-5, and Figure 22(c) shows the measurement results of power values ​​versus temperature for Comparative Example 2-5. Figure 23(a) shows a comparison of power between the thermoelectric conversion element of Example 2-1 and the thermoelectric conversion element of Comparative Example 2-5 at 10 kΩ, where power is calculated to be particularly large, and Figure 23(b) shows a similar comparison at 100 kΩ. Figure 24 shows the changes in current and voltage values ​​when multiple thermoelectric conversion elements of Example 2-1 are connected. Figures 25(a) and (b) are schematic diagrams of a thermoelectric conversion element of the third embodiment of the present invention. Figures 26(a) and (b) are model diagrams for theoretical explanation of the thermoelectric conversion element of the third embodiment of the present invention. Figure 27 is a model diagram for theoretical explanation of the improvement in electromotive force due to the addition of transition metal ions. Figure 28 shows the optical absorption spectrum measured for iron phthalocyanine (FePc). Figure 29 shows the optical absorption spectrum measured for zinc phthalocyanine (ZnPc). Figure 30 shows the current measurement results for the element fabricated in Example 3-1 when the temperature was repeatedly increased and stopped. Figure 31 shows a circuit diagram assembled to measure the electrical energy of the element fabricated in Comparative Example 3-1. Figure 32(a) shows the voltage measurement results for the element in Comparative Example 3-1, and Figure 32(b) shows the current measurement results for the element in Comparative Example 3-1. Figure 33(a) shows the voltage measurement results for the element in Comparative Example 3-2, and Figure 33(b) shows the current measurement results for the element in Comparative Example 3-2. Figure 34 shows the current and voltage measurement results for the element in Comparative Example 3-3. Figure 35 shows the current and voltage measurement results for the element in Comparative Example 3-4. Figure 36 is a schematic diagram of a thermoelectric conversion element according to the fourth embodiment of the present invention. Figure 37 is a model diagram for theoretically explaining the thermoelectric conversion element according to the fourth embodiment of the present invention. Figure 38 shows the optical absorption spectrum measured for iron phthalocyanine (FePc). Figure 39 shows the optical absorption spectrum measured for zinc phthalocyanine (ZnPc). Figure 40 is a circuit diagram assembled to measure the electrical energy of the elements fabricated in the examples and comparative examples. Figure 41(a) shows the measurement results of the voltage of the element of comparative example 4-1, and Figure 41(b) shows the measurement results of the current of the element of comparative example 4-1.Figure 42(a) shows the voltage measurement results for the element of Comparative Example 4-2, and Figure 42(b) shows the current measurement results for the element of Comparative Example 4-2. Figure 43 shows the current and voltage measurement results for the element of Comparative Example 4-3. Figure 44 shows the current and voltage measurement results for the element of Comparative Example 4-4. Figure 45(a) shows the current value versus temperature measurement results for Example 4-1, Figure 45(b) shows the voltage value versus temperature measurement results for Example 4-1, and Figure 45(c) shows the power value versus temperature measurement results for Example 4-1. Figure 46 is a diagram illustrating the performance improvement observed in a small resistance circuit at temperatures between 20°C and 60°C due to the insertion of graphite. Figure 47 is a schematic diagram showing an experiment to prove that the thermoelectric conversion method of the present invention is not a phenomenon due to ionization tendency. Figure 48 shows the voltage measurement results of the above experiment. Figure 49 is a schematic diagram showing an experiment to prove that the thermoelectric conversion method of the present invention is not a phenomenon involving a chemical reaction. Figure 50 shows the voltage measurement results of the above experiment. Figure 51 is a schematic diagram showing an experiment on charge transfer due to the thinning of the negative electrode of the element and the correlation between area and power generation. Figure 52 shows the current measurement results of the above experiment. Figure 53 shows the current measurement results (enlarged view) of the above experiment. Figure 54 is a schematic diagram of the element used in an experiment demonstrating the effect of series connection by stacking elements. Figure 55 shows the voltage and current measurement results of the above experiment. Figure 56 is a schematic diagram of the element used in an experiment demonstrating the effect of series connection by stacking elements. Figure 57 shows the voltage and current measurement results of the above experiment. Figure 58 shows the current change measured when five elements obtained by constituting the third type of thermoelectric conversion element are connected in series. Figure 59 shows the current change measured when five elements obtained by constituting the third type of thermoelectric conversion element are connected in parallel. Figure 60 shows the current measured with an ammeter and voltmeter after placing elements in an electric furnace and changing the temperature inside the furnace using a program. Figure 61 shows the measurement results when an element generating a larger current was used. Figure 62 shows the results of measuring the current generated by the element under conditions in which the temperature change was programmed to vary between periods of gradual, step-like rise and periods of sudden rise. Figure 63 shows the results of an experiment attempting to measure the upper limit of the power generation capacity of the thermoelectric conversion element of the present invention.Fig. 64 shows the results showing the possibility of scaling up the thermoelectric conversion element of the present invention. Fig. 65 is a diagram showing the power generation effect at around room temperature. Fig. 66 is a schematic diagram showing the stages of sealing the element and the state of an experiment on durability. Fig. 67 is a diagram showing the value of the open circuit voltage (change over time) after applying heat flow flux in the above experiment.

[0026] [First embodiment] <Thermoelectric conversion element (first embodiment)> As shown in the schematic diagram of FIG. 1 , a thermoelectric conversion element 1100 of the present invention includes a positive electrode 110 and a negative electrode 120 made of materials with different electrical conductivities, and an organic semiconductor layer 130 between the positive electrode 110 and the negative electrode 120, the organic semiconductor layer 130 containing a material that is thermally excited to generate electrons and holes.

[0027] (Positive and negative electrodes made of materials with different electrical conductivities) The thermoelectric conversion element of the present invention uses positive and negative electrodes made of materials with different electrical conductivities. This generates an internal electric field between the electrodes, and electrons and holes, which are charge carriers generated by thermal excitation in the organic semiconductor layer, migrate to the negative and positive electrodes, respectively, due to the internal electric field, thereby generating an electromotive force. In this way, the thermoelectric conversion element of the present invention generates an electromotive force even when the positive and negative electrodes are in the same temperature environment, and is based on a theory different from the conventional Seebeck effect.

[0028] A model diagram is shown in Figure 2, and a theoretical explanation of the thermoelectric conversion element of the present invention is provided. The most fundamental phenomenon is the generation of an internal electric field between two electrode materials with different electrical conductivities. Directly joining two different electrode materials would be equivalent to the well-known thermocouple technology, i.e., the configuration of a Seebeck element. However, in the present invention, instead of joining two different electrode materials, we fabricated an element in which the electrode with higher electrical conductivity serves as the negative electrode and the electrode with lower electrical conductivity serves as the positive electrode. We sandwiched an organic semiconductor layer between these electrodes, containing a material that emits electrons and holes upon thermal excitation. This successfully generated a large internal electric field. The resulting electromotive force was 100,000 to 1,000,000 times greater than that generated by a thermocouple. This structure, in which charge carriers move and are polarized, facilitates the movement of electrons to the negative electrode and holes to the positive electrode due to the heat flow from the outside world, demonstrating a method for generating a large electromotive force.

[0029] Referring to Figure 2, the energy levels of the positive and negative electrodes in the figure are Fermi levels. The energy levels of organic semiconductors are, from top to bottom, the lowest unoccupied molecular orbital (LUMO) and the highest occupied molecular orbital (HOMO). When discussing the energy levels of organic semiconductors, it is permissible to compare the band gaps of the LUMO and HOMO with the energy levels of inorganic materials.

[0030] In the thermoelectric conversion element of the present invention, electrons emitted by the organic semiconductor due to thermal excitation caused by receiving ambient thermal energy migrate. Specifically, carriers (electrons, holes) generated by charge separation in the organic semiconductor migrate between the inside of the element and the external circuit according to the energy levels of each substance. That is, electrons in the LUMO of the organic semiconductor acquire energy exceeding the Fermi level of the negative electrode and migrate to the conduction band. Concomitantly, holes in the HOMO of the organic semiconductor acquire energy exceeding the Fermi level of the positive electrode and migrate to the conduction band. This carrier migration generates an electromotive force.

[0031] Thus, with the thermoelectric conversion element of the present invention, electromotive force can be generated even when the negative and positive electrodes are at the same temperature. The phenomenon of electromotive force generation in a thermocouple is reflected by the temperature difference between the reference point of the measurement system and the point of contact with the heat flow. However, in the present invention, measurements are performed by placing all copper wires, instruments, and elements in the measurement system in the same temperature environment and applying a heat flow, and results equivalent to electromotive force and power generation measurements performed with only the element in contact with the heat flow are obtained. This means that in the thermoelectric conversion element of the present invention, thermally excited electrons and holes function as an element with diode characteristics that exhibit the same behavior as photoexcited electrons and holes inside a photovoltaic cell generated by photoelectric conversion, generating electromotive force. This is a fundamentally novel feature that differs from conventional Seebeck elements.

[0032] Among materials with different conductivities, an electrode made of a material with low conductivity that results in a high hole density becomes the positive electrode, and an electrode made of a material with high conductivity that results in a high electron density becomes the negative electrode. Here, high conductivity and low conductivity are determined by comparing the material that constitutes the positive electrode with the material that constitutes the negative electrode.

[0033] The greater the difference in conductivity between the positive electrode 110 and the negative electrode 120, the stronger the internal electric field generated between the electrodes. Therefore, the lower limit of the difference in conductivity between the positive electrode 110 and the negative electrode 120 is preferably 50 S / m or more, more preferably 100 S / m or more. However, if the difference in conductivity is too large, the electrode itself begins to exhibit resistance, causing energy loss and also leading to a decrease in performance, such as a slowdown in the thermoelectric conversion rate. Furthermore, although there are no particular limitations on the upper limit, from the viewpoint of the materials that can be selected, it is usually preferably 10,000 S / m or less, more preferably 1,000 S / m or less.

[0034] The conductivity of the negative electrode 120 with high conductivity is 1×10 7 ~1 x 10 8 S / m, and the conductivity of the positive electrode 110 having low conductivity is preferably 1×10 3 ~1 x 10 5 It is preferable to set it to S / m.

[0035] Examples of materials constituting the electrodes include metals, conductive organic substances, carbon materials such as amorphous carbon, ceramics, amorphous metals, etc. Examples of materials constituting the positive electrode 10 include, for example, tin-doped indium oxide (ITO), an oxide of indium and tin, carbon-based materials, and carbon black. Examples of materials constituting the negative electrode 20 include, for example, metal materials such as aluminum, gold, silver, platinum, and copper. In the thermoelectric conversion element of the present invention, it is important to generate an internal electric field between the electrodes. As long as the desired internal electric field can be generated, various conductive materials can be appropriately selected and applied. For example, the same type of conductive material can be used for both the positive and negative electrodes. For example, pencils obtained by blending carbon and clay have different conductivity depending on the blending ratio. An electrode obtained by applying a pencil with a high conductivity can be used as the negative electrode, and an electrode obtained by applying a pencil with a low conductivity can be used as the positive electrode.

[0036] (Organic Semiconductor Layer) The organic semiconductor layer may be any layer that has the function of generating electrons and holes upon thermal excitation and the function of transporting the generated electrons and holes to the respective electrodes, and layers made of various materials may be used as long as they have these functions. For example, an organic semiconductor may be used as a material that generates electrons and holes upon thermal excitation.

[0037] Examples of organic semiconductors include organic charge transfer complexes such as complexes of phthalocyanine and various transition metals. More specifically, examples include magnetic metal-containing organic complex compounds such as iron phthalocyanine (FePc), nickel phthalocyanine (NiPc), manganese phthalocyanine (MnPc), cobalt phthalocyanine (CoPc), iron porphyrin complexes, nickel porphyrin complexes, manganese porphyrin complexes, and cobalt porphyrin complexes, and diamagnetic metal-containing organic complex compounds such as copper phthalocyanine (CuPc), zinc phthalocyanine (ZnPc), copper porphyrin complexes, and zinc porphyrin complexes.

[0038] In addition, the organic semiconductor layer preferably contains a medium that transports electrons and holes emitted by the organic semiconductor upon thermal excitation to the negative electrode and the positive electrode. As such a charge carrier transport medium, for example, polyoxyethylene sorbitan monostearate can be used.

[0039] <Method for producing thermoelectric conversion element (first embodiment)> The thermoelectric conversion element of the present invention can be produced, for example, by the following steps: preparing a mixed solution containing an organic semiconductor; forming an organic semiconductor layer on an electrode surface; and forming a thermoelectric conversion element.

[0040] (Preparation of Mixed Solution Containing Organic Semiconductor) A mixed solution containing an organic semiconductor can be obtained by mixing an organic semiconductor, a charge carrier transport medium, and a solvent capable of dissolving the transport medium, and stirring as necessary. The amount of solvent can be appropriately adjusted so that the solution is easy to handle (applicable), and if there is no problem with applicability, a solvent may not be added. The solvent is not particularly limited, but for example, chloroform can be used.

[0041] (Step of forming an organic semiconductor layer on the electrode surface) The mixed solution formed above is applied to the surfaces of the positive electrode and the negative electrode and dried, thereby forming an organic semiconductor layer on the electrode surface. In a preferred embodiment, the mixed solution is applied to the surfaces of the positive electrode and the negative electrode, respectively, to form an organic semiconductor layer on each of the positive electrode surface and the negative electrode surface, and the formed organic semiconductor layers are bonded together, pressed, and heated as necessary to form a single-layer organic semiconductor layer. In this manufacturing method, it is possible to improve the adhesion between the positive electrode and the negative electrode and the organic semiconductor layer.

[0042] Alternatively, an element may be formed by forming an organic semiconductor layer on one of the positive electrode or negative electrode and bonding this to the other electrode on which no organic semiconductor layer is formed. In this case, however, when bonding the electrodes together, it becomes necessary to adjust the pressing force or the heating temperature so as to ensure adhesion between the electrodes and the organic semiconductor layer.

[0043] (Step of forming thermoelectric conversion element) The organic semiconductor layers formed on the surfaces of the positive electrode and negative electrode obtained above are bonded together to form a thermoelectric conversion element. A pressing force of preferably about 1,200 hPa to 1,500 hPa is applied to the bonded positive electrode / organic semiconductor layer / organic semiconductor layer / negative electrode, and the pressure is maintained for preferably 60 to 120 minutes, thereby integrating the organic semiconductor layer / organic semiconductor layer and forming a thermoelectric conversion element consisting of the positive electrode / organic semiconductor layer / negative electrode.

[0044] Furthermore, by simultaneously heating the laminate during lamination, the organic semiconductor layer can be more effectively integrated. Heating can be preferably performed within a range of 50° C. or higher and 140° C. or lower.

[0045] <Thermoelectric Conversion Method (First Aspect)> According to the thermoelectric conversion method of the present invention, it is possible to convert thermal energy into electrical energy simply by placing the above-described thermoelectric conversion element in the presence of a thermal energy flow that creates a certain thermal environment. In other words, while conventional methods based on the Seebeck effect require a temperature difference between the positive electrode and the negative electrode, the method of the present application does not require a temperature difference, and it is sufficient to simply place the thermoelectric conversion element in a thermal environment of a constant temperature in the presence of a thermal energy flow.

[0046] The term "constant-temperature thermal environment in the presence of thermal energy flow" refers to any thermal environment that can impart constant thermal energy to the thermoelectric conversion element, preferably in an atmosphere at 20°C (room temperature) or higher, more preferably in an atmosphere at 25°C or higher, even more preferably in an atmosphere at 30°C or higher, particularly preferably in an atmosphere at 35°C or higher, and most preferably in an atmosphere at 40°C or higher. This phenomenon can be understood in comparison with the movement of electrons and holes excited by light energy within a solar cell under a constant light irradiation environment in the presence of light energy flow, and is a physically understandable phenomenon. Furthermore, when the light energy flow stops, the solar cell ceases to generate electromotive force. However, in the thermoelectric conversion method of the present invention, a decrease in the inflow of thermal energy flow corresponds to the cessation of light energy flow in a solar cell, and can be understood in comparison with the decline in the electromotive force generation function. However, unlike the cessation of light irradiation, the energy distribution of atoms and molecules mediating the thermal energy flow does not instantly become zero but gradually decays, so the phenomenon of generating electromotive force does not suddenly become zero.

[0047] Furthermore, even in a gaseous atmosphere other than air, for example, in an inert gas such as nitrogen, it can be said that the environment is capable of imparting thermal energy to the thermoelectric conversion element as long as the temperature is similar to that described above. Furthermore, the thermoelectric conversion element may be placed in an atmosphere other than gas, for example, in a liquid such as water. From the viewpoint of efficiently imparting thermal energy to the thermoelectric conversion element, it can be said that it is preferable to place the thermoelectric conversion element in an underwater atmosphere at a predetermined temperature. The underwater thermal environment can be preferably water at 20°C (room temperature) or higher, more preferably water at 25°C or higher, even more preferably water at 30°C or higher, particularly preferably water at 35°C or higher, and most preferably water at 40°C or higher. Furthermore, organic solvents such as alcohols at temperatures above the above temperatures can also be used, even if they are not water. In other words, it is sufficient that thermal vibrations of atoms and molecules are conducted.

[0048] [Second form]

[0049] <Thermoelectric Conversion Element (Second Form)> As shown in the schematic diagram of FIG. 12 , a thermoelectric conversion element 2100 of the present invention is a thermoelectric conversion element that includes a positive electrode 210 and a negative electrode 220 made of materials with different electrical conductivities, and an organic semiconductor layer between the positive electrode 210 and the negative electrode 220, the organic semiconductor layer including a material that generates electrons and holes upon thermal excitation, the organic semiconductor layer including a first organic semiconductor layer 232 on the positive electrode side and a second semiconductor layer 234 on the negative electrode side, and the energy level of the HOMO of the first organic semiconductor layer 232 is higher than the energy level of the HOMO of the second semiconductor layer 234.

[0050] (Positive and negative electrodes made of materials with different electrical conductivities) The thermoelectric conversion element of the present invention uses positive and negative electrodes made of materials with different electrical conductivities. This generates an internal electric field between the electrodes, and electrons and holes, which are charge carriers generated by thermal excitation in the organic semiconductor layer, migrate to the negative and positive electrodes, respectively, due to the internal electric field, thereby generating an electromotive force. In this way, the thermoelectric conversion element of the present invention generates an electromotive force even when the positive and negative electrodes are in the same temperature environment, and is based on a theory different from the conventional Seebeck effect.

[0051] A model diagram is shown in Figure 13, and a theoretical explanation of the thermoelectric conversion element of the present invention is provided. The most fundamental phenomenon is that two electrode materials with different electrical conductivities generate an internal electric field between the electrodes. If two different electrode materials were directly joined, this would be the well-known thermocouple technology, i.e., the configuration of a Seebeck element. However, in the present invention, instead of joining two different electrode materials, we fabricated an element in which the electrode with higher electrical conductivity serves as the negative electrode and the electrode with lower electrical conductivity serves as the positive electrode. We sandwiched an organic semiconductor layer between these electrodes, containing a material that emits electrons and holes upon thermal excitation. This successfully generated a large internal electric field. The resulting electromotive force was 100,000 to 1,000,000 times greater than that generated by a thermocouple. It was revealed that by creating a structure in which charge carriers move and are polarized, electrons can easily move to the negative electrode and holes to the positive electrode due to the heat flow from the outside, thereby generating a large electromotive force.

[0052] Explaining based on Figure 13, the energy levels of the positive and negative poles in the figure are Fermi levels. The energy levels of organic semiconductors are, from top to bottom, the lowest unoccupied molecular orbital (LUMO) and the highest occupied molecular orbital (HOMO). When discussing the energy levels of organic semiconductors, it is permissible to compare the band gaps of the LUMO and HOMO with the energy levels of inorganic materials.

[0053] In the thermoelectric conversion element of the present invention, electrons emitted by the organic semiconductor due to thermal excitation caused by receiving ambient thermal energy migrate. Specifically, carriers (electrons, holes) generated by charge separation in the organic semiconductor migrate between the inside of the element and the external circuit according to the energy levels of each substance. That is, electrons in the LUMO of the second organic semiconductor layer acquire energy exceeding the Fermi level of the negative electrode and migrate to the conduction band. Accordingly, holes in the HOMO of the second organic semiconductor layer migrate to the HOMO of the first organic semiconductor layer, and then further acquire energy exceeding the Fermi level of the positive electrode and migrate to the conduction band. This type of carrier migration generates an electromotive force.

[0054] In the present invention, the HOMO energy level of the first organic semiconductor layer is higher than the HOMO energy level of the second organic semiconductor layer. Therefore, the energy level of holes is stepped toward the positive electrode, allowing smooth movement of holes. This results in a large electromotive force.

[0055] Furthermore, the energy difference between the HOMO and LUMO of the second organic semiconductor layer is larger than the energy difference between the HOMO and LUMO of the first organic semiconductor layer, and electrons that have acquired a large amount of energy are located on the negative electrode side where the internal electric field is large, resulting in a large electromotive force.

[0056] Thus, with the thermoelectric conversion element of the present invention, electromotive force can be generated even when the negative and positive electrodes are at the same temperature. The phenomenon of electromotive force generation in a thermocouple is reflected by the temperature difference between the reference point of the measurement system and the point of contact with the heat flow. However, with the present invention, even when measurements are performed by applying a heat flow while all copper wires, instruments, and elements in the measurement system are placed in the same temperature environment, results equivalent to those obtained by measuring electromotive force and power generation when only the element is in contact with the heat flow can be obtained. This means that in the thermoelectric conversion element of the present invention, thermally excited electrons and holes function as an element with diode characteristics that exhibit the same behavior as photoexcited electrons and holes inside a photovoltaic cell generated by photoelectric conversion, thereby generating electromotive force. This is a fundamentally novel feature that differs from conventional Seebeck elements.

[0057] Among materials with different conductivities, an electrode made of a material with low conductivity that results in a high hole density becomes the positive electrode, and an electrode made of a material with high conductivity that results in a high electron density becomes the negative electrode. Here, high conductivity and low conductivity are determined by comparing the material that constitutes the positive electrode with the material that constitutes the negative electrode.

[0058] The greater the difference in conductivity between the positive electrode 210 and the negative electrode 220, the stronger the internal electric field generated between the electrodes. Therefore, the lower limit of the difference in conductivity between the positive electrode 210 and the negative electrode 220 is preferably 50 S / m or more, more preferably 100 S / m or more. However, if the difference in conductivity is too large, the electrodes themselves begin to exhibit resistance, causing not only energy loss but also a decrease in performance, such as a slowdown in the thermoelectric conversion rate. Furthermore, although there are no particular limitations on the upper limit, from the viewpoint of the materials that can be selected, it is usually preferably 10,000 S / m or less, more preferably 1,000 S / m or less.

[0059] The conductivity of the negative electrode 220 with high conductivity is 1×10 7 ~1 x 10 8 S / m, and the conductivity of the positive electrode 210 having low conductivity is preferably 1×10 3 ~1 x 10 5 It is preferable to set it to S / m.

[0060] Examples of materials constituting the electrodes include metals, conductive organic substances, carbon materials such as amorphous carbon, ceramics, amorphous metals, etc. Examples of materials constituting the positive electrode 210 include tin-doped indium oxide (ITO), an oxide of indium and tin, carbon-based materials, and carbon black. Examples of materials constituting the negative electrode 220 include metal materials such as aluminum, gold, silver, platinum, and copper. In the thermoelectric conversion element of the present invention, it is important to generate an internal electric field between the electrodes. As long as the desired internal electric field can be generated, various conductive materials can be appropriately selected and applied. For example, the same type of conductive material can be used for both the positive and negative electrodes. For example, pencils obtained by blending carbon and clay have different conductivity depending on the blending ratio. An electrode obtained by applying a pencil with a high conductivity can be used as the negative electrode, and an electrode obtained by applying a pencil with a low conductivity can be used as the positive electrode.

[0061] (Organic Semiconductor Layer) The organic semiconductor layer may be any layer that has the function of generating electrons and holes upon thermal excitation and the function of transporting the generated electrons and holes to the respective electrodes, and layers made of various materials may be used as long as they have these functions. For example, an organic semiconductor may be used as a material that generates electrons and holes upon thermal excitation.

[0062] Examples of organic semiconductors include organic charge transfer complexes such as complexes of phthalocyanine and various transition metals. More specifically, examples include magnetic metal-containing organic complex compounds such as iron phthalocyanine (FePc), nickel phthalocyanine (NiPc), manganese phthalocyanine (MnPc), cobalt phthalocyanine (CoPc), iron porphyrin complexes, nickel porphyrin complexes, manganese porphyrin complexes, and cobalt porphyrin complexes, and diamagnetic metal-containing organic complex compounds such as copper phthalocyanine (CuPc), zinc phthalocyanine (ZnPc), copper porphyrin complexes, and zinc porphyrin complexes.

[0063] In addition, the organic semiconductor layer preferably contains a medium that transports electrons and holes emitted by the organic semiconductor upon thermal excitation to the negative electrode and the positive electrode. As such a charge carrier transport medium, for example, polyoxyethylene sorbitan monostearate can be used.

[0064] In addition, in the present invention, the organic semiconductor layer is composed of two layers: a first organic semiconductor layer 232 on the positive electrode 210 side and a second organic semiconductor layer 234 on the negative electrode 220 side. As described above, the HOMO energy level of the first organic semiconductor layer 232 is higher than the HOMO energy level of the second semiconductor layer 234, which results in a configuration in which a high electromotive force can be obtained.

[0065] An example of a combination of organic semiconductors that can achieve such a configuration is a combination in which the organic semiconductor contained in the first organic semiconductor layer is iron phthalocyanine, and the organic semiconductor contained in the second organic semiconductor layer is copper phthalocyanine, cobalt phthalocyanine, nickel phthalocyanine, or zinc phthalocyanine.

[0066] <Method for manufacturing thermoelectric conversion element (second embodiment)> The thermoelectric conversion element of the present invention can be manufactured, for example, by the following steps: preparing a mixed solution containing an organic semiconductor; forming an organic semiconductor layer on an electrode surface; and forming a thermoelectric conversion element.

[0067] (Preparation of Mixed Solution Containing Organic Semiconductor) A mixed solution containing an organic semiconductor can be obtained by mixing an organic semiconductor, a charge carrier transport medium, and a solvent capable of dissolving the transport medium, and stirring as necessary. The amount of solvent can be appropriately adjusted so that the solution is easy to handle (applicable), and if there is no problem with applicability, a solvent may not be added. The solvent is not particularly limited, but for example, chloroform can be used.

[0068] (Step of forming an organic semiconductor layer on the electrode surface) The mixed solution formed above is applied to the surfaces of the positive electrode and the negative electrode and dried, thereby forming an organic semiconductor layer on the electrode surface. A preferred embodiment is to apply the mixed solution to the surfaces of the positive electrode and the negative electrode, respectively, to form a first organic semiconductor layer on the surface of the positive electrode and a second organic semiconductor layer on the surface of the negative electrode. In this embodiment, it is possible to improve the adhesion between the positive electrode and the negative electrode and the respective organic semiconductor layers.

[0069] Alternatively, a device can be formed by sequentially forming a first organic semiconductor layer and a second organic semiconductor layer on the surface of a positive electrode and then bonding the second organic semiconductor layer to the surface of a negative electrode. Similarly, a device can be formed by sequentially forming a second organic semiconductor layer and a first organic semiconductor layer on the surface of a negative electrode and then bonding the first organic semiconductor layer to the surface of a positive electrode. However, in this case, it becomes necessary to adjust the pressing force and heating temperature when bonding the electrodes so as to ensure adhesion between the electrodes and the organic semiconductor layers.

[0070] (Step of forming thermoelectric conversion element) The thermoelectric conversion element is formed by bonding the first organic semiconductor layer formed on the positive electrode surface and the second organic semiconductor layer formed on the negative electrode surface obtained above. A pressing force of preferably about 1,200 hPa to 1,500 hPa is applied to the bonded positive electrode / first organic semiconductor layer / second organic semiconductor layer / negative electrode, and the bonded positive electrode / first organic semiconductor layer / second organic semiconductor layer / negative electrode is maintained for preferably 60 to 120 minutes, thereby allowing the first organic semiconductor layer / second organic semiconductor layer to adhere to each other.

[0071] Furthermore, by simultaneously heating the laminate during lamination, the organic semiconductor layer can be more effectively integrated. Heating can be preferably performed within a range of 50° C. or higher and 140° C. or lower.

[0072] <Thermoelectric Conversion Method (Second Embodiment)> According to the thermoelectric conversion method of the present invention, it is possible to convert thermal energy into electrical energy simply by placing the above-mentioned thermoelectric conversion element in the presence of a thermal energy flow that creates a certain thermal environment. In other words, while conventional methods based on the Seebeck effect require a temperature difference between the positive electrode and the negative electrode, the method of the present application does not require a temperature difference, and it is sufficient to simply place the thermoelectric conversion element in a thermal environment of a constant temperature in the presence of a thermal energy flow.

[0073] The term "constant-temperature thermal environment in the presence of thermal energy flow" refers to any thermal environment that can impart constant thermal energy to the thermoelectric conversion element, preferably in an atmosphere at 20°C (room temperature) or higher, more preferably in an atmosphere at 25°C or higher, even more preferably in an atmosphere at 30°C or higher, particularly preferably in an atmosphere at 35°C or higher, and most preferably in an atmosphere at 40°C or higher. This phenomenon can be understood in comparison with the movement of electrons and holes excited by light energy within a solar cell under a constant light irradiation environment in the presence of light energy flow, and is a physically understandable phenomenon. Furthermore, when the light energy flow stops, the solar cell ceases to generate electromotive force. However, in the thermoelectric conversion method of the present invention, a decrease in the inflow of thermal energy flow corresponds to the cessation of light energy flow in a solar cell, and can be understood in comparison with the decline in the electromotive force generation function. However, unlike the cessation of light irradiation, the energy distribution of atoms and molecules mediating the thermal energy flow does not instantly become zero but gradually decays, so the phenomenon of generating electromotive force does not suddenly become zero.

[0074] Furthermore, even in a gaseous atmosphere other than air, for example, in an inert gas such as nitrogen, it can be said that the environment is capable of imparting thermal energy to the thermoelectric conversion element as long as the temperature is similar to that described above. Furthermore, the thermoelectric conversion element may be placed in an atmosphere other than gas, for example, in a liquid such as water. From the viewpoint of efficiently imparting thermal energy to the thermoelectric conversion element, it can be said that it is preferable to place the thermoelectric conversion element in an underwater atmosphere at a predetermined temperature. The underwater thermal environment can be preferably water at 20°C (room temperature) or higher, more preferably water at 25°C or higher, even more preferably water at 30°C or higher, particularly preferably water at 35°C or higher, and most preferably water at 40°C or higher. Furthermore, organic solvents such as alcohols at temperatures above the above temperatures can also be used, even if they are not water. In other words, it is sufficient that thermal vibrations of atoms and molecules are conducted.

[0075] 25( a), a thermoelectric conversion element 3100A of the present invention includes a positive electrode 310 and a negative electrode 320 made of materials with different electrical conductivities, and an organic semiconductor layer 330 made of a material that generates electrons and holes upon thermal excitation, between the positive electrode 310 and the negative electrode 320. Also, a thermoelectric conversion element 3100B of a preferred embodiment of the present invention includes a positive electrode 310 and a negative electrode 320 made of materials with different electrical conductivities, and includes a first organic semiconductor layer 332 on the positive electrode 310 side and a second semiconductor layer 334 on the negative electrode 320 side, as organic semiconductor layers made of a material that generates electrons and holes upon thermal excitation, between the positive electrode 310 and the negative electrode 320, as shown in the schematic diagram of FIG.

[0076] (Positive and negative electrodes made of materials with different electrical conductivities) The thermoelectric conversion element of the present invention uses positive and negative electrodes made of materials with different electrical conductivities. This generates an internal electric field between the electrodes, and electrons and holes, which are charge carriers generated by thermal excitation in the organic semiconductor layer, migrate to the negative and positive electrodes, respectively, due to the internal electric field, thereby generating an electromotive force. In this way, the thermoelectric conversion element of the present invention generates an electromotive force even when the positive and negative electrodes are in the same temperature environment, and is based on a theory different from the conventional Seebeck effect.

[0077] Figure 26(a) shows a model diagram of a single-layer organic semiconductor layer, and Figure 26(b) shows a model diagram of a two-layer organic semiconductor layer. The theoretical explanation of the thermoelectric conversion element of the present invention is provided below. The most fundamental phenomenon is that two electrode materials with different conductivities generate an internal electric field between the electrodes. If two different electrode materials were directly joined, this would be the well-known thermocouple technology, i.e., the configuration of a Seebeck element. However, in the present invention, two different electrode materials are not joined, but rather the electrode with higher conductivity becomes the negative electrode and the electrode with lower conductivity becomes the positive electrode. By sandwiching an organic semiconductor layer containing a material that is thermally excited to emit electrons and holes between these electrodes, we have succeeded in generating a large internal electric field. The electromotive force obtained in this way is equivalent to 100,000 to 1,000,000 times the electromotive force generated by a thermocouple, and it has become clear that by creating a structure in which charge carriers move and become polarized, electrons can easily move to the negative electrode and holes to the positive electrode due to the heat flow coming in from the outside, thereby generating a large electromotive force.

[0078] 26(a), the energy levels of the positive and negative poles in the figure are Fermi levels. The energy levels of organic semiconductors are, from top to bottom, the lowest unoccupied molecular orbital (LUMO) and the highest occupied molecular orbital (HOMO). When discussing the energy levels of organic semiconductors, it is permissible to compare the band gaps of the LUMO and HOMO with the energy levels of inorganic materials.

[0079] In the thermoelectric conversion element of the present invention, electrons emitted by the organic semiconductor due to thermal excitation caused by receiving ambient thermal energy migrate. Specifically, carriers (electrons, holes) generated by charge separation in the organic semiconductor migrate between the inside of the element and the external circuit according to the energy levels of each substance. That is, electrons in the LUMO of the organic semiconductor acquire energy exceeding the Fermi level of the negative electrode and migrate to the conduction band. Concomitantly, holes in the HOMO of the organic semiconductor acquire energy exceeding the Fermi level of the positive electrode and migrate to the conduction band. This carrier migration generates an electromotive force.

[0080] 26(b), the energy levels of the positive and negative poles in the figure are Fermi levels. The energy levels of organic semiconductors are, from top to bottom, the lowest unoccupied molecular orbital (LUMO) and the highest occupied molecular orbital (HOMO). When discussing the energy levels of organic semiconductors, it is permissible to compare the band gaps of the LUMO and HOMO with the energy levels of inorganic materials.

[0081] In the thermoelectric conversion element of the present invention, electrons emitted by the organic semiconductor due to thermal excitation caused by receiving ambient thermal energy migrate. Specifically, carriers (electrons, holes) generated by charge separation in the organic semiconductor migrate between the inside of the element and the external circuit according to the energy levels of each substance. That is, electrons in the LUMO of the second organic semiconductor layer acquire energy exceeding the Fermi level of the negative electrode and migrate to the conduction band. Accordingly, holes in the HOMO of the second organic semiconductor layer migrate to the HOMO of the first organic semiconductor layer, and then further acquire energy exceeding the Fermi level of the positive electrode and migrate to the conduction band. This type of carrier migration generates an electromotive force.

[0082] In the configuration shown in Figure 26(b), the HOMO energy level of the first organic semiconductor layer is higher than the HOMO energy level of the second organic semiconductor layer. Therefore, the energy level of holes is stepped toward the positive electrode, allowing smooth movement of holes. This results in a large electromotive force.

[0083] Furthermore, the energy difference between the HOMO and LUMO of the second organic semiconductor layer is larger than the energy difference between the HOMO and LUMO of the first organic semiconductor layer, and electrons that have acquired a large amount of energy are located on the negative electrode side where the internal electric field is large, resulting in a large electromotive force.

[0084] Thus, with the thermoelectric conversion element of the present invention, electromotive force can be generated even when the negative and positive electrodes are at the same temperature. The phenomenon of electromotive force generation in a thermocouple is reflected by the temperature difference between the reference point of the measurement system and the point of contact with the heat flow. However, with the present invention, even when measurements are performed by applying a heat flow while all copper wires, instruments, and elements in the measurement system are placed in the same temperature environment, results equivalent to those obtained by measuring electromotive force and power generation when only the element is in contact with the heat flow can be obtained. This means that in the thermoelectric conversion element of the present invention, thermally excited electrons and holes function as an element with diode characteristics that exhibit the same behavior as photoexcited electrons and holes inside a photovoltaic cell generated by photoelectric conversion, thereby generating electromotive force. This is a fundamentally novel feature that differs from conventional Seebeck elements.

[0085] Among materials with different conductivities, an electrode made of a material with low conductivity that results in a high hole density becomes the positive electrode, and an electrode made of a material with high conductivity that results in a high electron density becomes the negative electrode. Here, high conductivity and low conductivity are determined by comparing the material that constitutes the positive electrode with the material that constitutes the negative electrode.

[0086] The greater the difference in conductivity between the positive electrode 310 and the negative electrode 320, the stronger the internal electric field generated between the electrodes. Therefore, the lower limit of the difference in conductivity between the positive electrode 10 and the negative electrode 20 is preferably 50 S / m or more, more preferably 100 S / m or more. However, if the difference in conductivity is too large, the electrodes themselves begin to exhibit resistance, causing not only energy loss but also a decrease in performance, such as a slowdown in the thermoelectric conversion rate. Furthermore, while there are no particular limitations on the upper limit, from the perspective of the materials that can be selected, it is usually preferably 10,000 S / m or less, more preferably 1,000 S / m or less.

[0087] The conductivity of the negative electrode 320 with high conductivity is 1×10 7 ~1 x 10 8 S / m, and the conductivity of the positive electrode 310 having low conductivity is preferably 1×10 3 ~1 x 10 5 It is preferable to set it to S / m.

[0088] Examples of materials constituting the electrodes include metals, conductive organic substances, carbon materials such as amorphous carbon, ceramics, amorphous metals, etc. Examples of materials constituting the positive electrode 10 include tin-doped indium oxide (ITO), an oxide of indium and tin, and carbon-based materials. Examples of materials constituting the negative electrode 320 include metal materials such as aluminum, gold, silver, platinum, and copper. In the thermoelectric conversion element of the present invention, it is important to generate an internal electric field between the electrodes. As long as the desired internal electric field can be generated, various conductive materials can be appropriately selected and applied. For example, the same type of conductive material can be used for both the positive and negative electrodes. For example, pencils obtained by blending carbon and clay have different conductivity depending on the blending ratio. An electrode obtained by applying a pencil with a high conductivity can be used as the negative electrode, and an electrode obtained by applying a pencil with a low conductivity can be used as the positive electrode.

[0089] (Organic Semiconductor Layer) The organic semiconductor layer may be any layer that has the function of generating electrons and holes upon thermal excitation and the function of transporting the generated electrons and holes to the respective electrodes, and layers made of various materials may be used as long as they have these functions. For example, an organic semiconductor may be used as a material that generates electrons and holes upon thermal excitation.

[0090] Examples of organic semiconductors include organic charge transfer complexes such as complexes of phthalocyanine and various transition metals. More specifically, examples include magnetic metal-containing organic complex compounds such as iron phthalocyanine (FePc), nickel phthalocyanine (NiPc), manganese phthalocyanine (MnPc), cobalt phthalocyanine (CoPc), iron porphyrin complexes, nickel porphyrin complexes, manganese porphyrin complexes, and cobalt porphyrin complexes, and diamagnetic metal-containing organic complex compounds such as copper phthalocyanine (CuPc), zinc phthalocyanine (ZnPc), copper porphyrin complexes, and zinc porphyrin complexes.

[0091] The organic semiconductor layer preferably contains a medium that transports electrons and holes emitted by the organic semiconductor upon thermal excitation to the negative electrode and positive electrode. As such a charge carrier transport medium, for example, an emulsifier such as polyoxyethylene sorbitan monostearate can be used.

[0092] 25(b), the organic semiconductor layer 330 is preferably configured to include two layers: a first organic semiconductor layer 332 on the positive electrode 310 side, and a second organic semiconductor layer 334 on the negative electrode 320 side. As described above, the HOMO energy level of the first organic semiconductor layer 332 is preferably higher than the HOMO energy level of the second semiconductor layer 334, thereby providing a configuration in which a high electromotive force can be obtained.

[0093] An example of a combination of organic semiconductors that can achieve such a configuration is a combination in which the organic semiconductor contained in the first organic semiconductor layer is iron phthalocyanine and the organic semiconductor contained in the second organic semiconductor layer is zinc phthalocyanine.

[0094] (Addition of Transition Metal Ions to Organic Semiconductor Layer) In the thermoelectric conversion element of the present invention, the organic semiconductor layer contains transition metal ions. The present inventors speculate that the inclusion of transition metal ions causes the transition metal ions to generate excitons (electrons + holes) through thermal excitation, which then capture the excitons in the organic semiconductor, thereby improving the electromotive force of the thermoelectric conversion element of the present invention.

[0095] The mechanism of the above-mentioned increase in electromotive force will be explained below with reference to Fig. 27. A transition element (e.g., Fe is shown in the figure) in a phthalocyanine (Pc) complex, which is an organic semiconductor, is thermally excited to generate excitons (electrons + holes), which are polarized by an internal electric field. 2 and FeCl 3 When a transition metal ion (for example, Fe ion) is introduced by adding Fe, the number density of Fe elements around the phthalocyanine (Pc) increases. 2+(which can be considered as the presence of 2 x holes) is excited in the same way as the Fe in the phthalocyanine complex, generating an exciton (3 x holes + electrons). The electrons then travel to the negative electrode, and the Fe 3+ (It can be considered as 3 x holes.) is Fe 2+ A positive hole is generated, and the remaining hole moves to the positive electrode. This phenomenon is repeated in the field created by the phthalocyanine, functioning as a thermally excited diode type power generation element. In addition, the following examples have confirmed that the amount of power generation depends on the number density of the added Fe ions.

[0096] Examples of the transition metal ions added to the organic semiconductor layer, that is, the transition metal ions further contained in the organic semiconductor layer, include iron ions, zinc ions, manganese ions, nickel ions, copper ions, and cobalt ions; ions of first transition elements such as scandium, titanium, vanadium, and chromium; ions of second transition elements such as yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, and silver; and ions of third transition elements such as lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, hafnium, tantalum, tungsten, rhenium, osmium, iridium, platinum, and gold. Among these, iron ions are preferred in terms of their effect of increasing the electromotive force of the thermoelectric conversion element and their availability on Earth. These transition metal ions can be added in the form of halides such as chlorides and bromides, hydroxides, etc., but from the viewpoint of ease of handling, they are preferably added as chlorides. They are also preferably added as anhydrides. The amount of the transition metal ions added is preferably a mass ratio of 0.5 to 1.5, more preferably 0.8 to 1.2, relative to the phthalocyanine complex, which is an organic semiconductor.

[0097] <Method for manufacturing thermoelectric conversion element (third embodiment)> The thermoelectric conversion element of the present invention can be manufactured, for example, by the following steps: preparing a mixed solution containing an organic semiconductor; forming an organic semiconductor layer on an electrode surface; and forming a thermoelectric conversion element.

[0098] (Preparation of Mixed Solution Containing Organic Semiconductor) A mixed solution containing an organic semiconductor can be obtained by mixing an organic semiconductor, a transition metal halide, a charge carrier transport medium, and a solvent capable of dissolving the transport medium, and stirring as necessary. The amount of solvent can be adjusted appropriately to improve the handleability (applicability) of the solution, and if there are no problems with applicability, a solvent need not be added. The solvent is not particularly limited, but chloroform, for example, can be used. In addition, the mixed solution containing an organic semiconductor may further contain a carbonate compound such as lithium carbonate, sodium carbonate, or calcium carbonate, which makes it possible to neutralize hydrogen halide that may be generated when the contained components contain water of hydration.

[0099] (Step of forming an organic semiconductor layer on the electrode surface) The mixed solution formed above can be applied to the surfaces of the positive electrode and the negative electrode and dried to form an organic semiconductor layer on the electrode surface. A preferred embodiment is a method in which the mixed solution is applied to the surfaces of the positive electrode and the negative electrode, respectively, to form an organic semiconductor layer on each, and then the layers are bonded together in a later step. In addition, in a form in which two organic semiconductor layers are formed, a first organic semiconductor layer can be formed on the surface of the positive electrode, and a second organic semiconductor layer can be formed on the surface of the negative electrode. In these embodiments, it is possible to improve the adhesion between the positive electrode and the negative electrode and the respective organic semiconductor layers.

[0100] Alternatively, a device can be formed by sequentially forming a first organic semiconductor layer and a second organic semiconductor layer on the surface of a positive electrode and then bonding the second organic semiconductor layer to the surface of a negative electrode. Similarly, a device can be formed by sequentially forming a second organic semiconductor layer and a first organic semiconductor layer on the surface of a negative electrode and then bonding the first organic semiconductor layer to the surface of a positive electrode. However, in this case, it becomes necessary to adjust the pressing force and heating temperature when bonding the electrodes so as to ensure adhesion between the electrodes and the organic semiconductor layers.

[0101] (Thermoelectric conversion element formation process) The organic semiconductor layer formed on the positive electrode surface and the organic semiconductor layer formed on the negative electrode surface obtained above are bonded together, or the first organic semiconductor layer formed on the positive electrode surface and the second organic semiconductor layer formed on the negative electrode surface are bonded together to form a thermoelectric conversion element. A pressing force of about 1,200 hPa to 1,500 hPa is preferably applied to the bonded positive electrode / organic semiconductor layer / organic semiconductor layer / negative electrode, or positive electrode / first organic semiconductor layer / second organic semiconductor layer / negative electrode, and preferably maintained for 60 to 120 minutes, thereby allowing the organic semiconductor layers to adhere to each other.

[0102] Furthermore, by simultaneously heating the laminate during lamination, the organic semiconductor layer can be more effectively integrated. Heating can be preferably performed within a range of 50° C. or higher and 140° C. or lower.

[0103] <Thermoelectric Conversion Method (Third Form)> According to the thermoelectric conversion method of the present invention, it is possible to convert thermal energy into electrical energy simply by placing the above-mentioned thermoelectric conversion element in the presence of a thermal energy flow that creates a certain thermal environment. In other words, while conventional methods based on the Seebeck effect require a temperature difference between the positive electrode and the negative electrode, the method of the present application does not require a temperature difference, and it is sufficient to simply place the thermoelectric conversion element in a thermal environment of a constant temperature in the presence of a thermal energy flow.

[0104] The term "constant-temperature thermal environment in the presence of thermal energy flow" refers to any thermal environment that can impart constant thermal energy to the thermoelectric conversion element, preferably in an atmosphere at 20°C (room temperature) or higher, more preferably in an atmosphere at 25°C or higher, even more preferably in an atmosphere at 30°C or higher, particularly preferably in an atmosphere at 35°C or higher, and most preferably in an atmosphere at 40°C or higher. This phenomenon can be understood in comparison with the movement of electrons and holes excited by light energy within a solar cell under a constant light irradiation environment in the presence of light energy flow, and is a physically understandable phenomenon. Furthermore, when the light energy flow stops, the solar cell ceases to generate electromotive force. However, in the thermoelectric conversion method of the present invention, a decrease in the inflow of thermal energy flow corresponds to the cessation of light energy flow in a solar cell, and can be understood in comparison with the decline in the electromotive force generation function. However, unlike the cessation of light irradiation, the energy distribution of atoms and molecules mediating the thermal energy flow does not instantly become zero but gradually decays, so the phenomenon of generating electromotive force does not suddenly become zero.

[0105] Furthermore, even in a gaseous atmosphere other than air, for example, in an inert gas such as nitrogen, it can be said that the environment is capable of imparting thermal energy to the thermoelectric conversion element as long as the temperature is similar to that described above. Furthermore, the thermoelectric conversion element may be placed in an atmosphere other than gas, for example, in a liquid such as water. From the viewpoint of efficiently imparting thermal energy to the thermoelectric conversion element, it can be said that it is preferable to place the thermoelectric conversion element in an underwater atmosphere at a predetermined temperature. The underwater thermal environment can be preferably water at 20°C (room temperature) or higher, more preferably water at 25°C or higher, even more preferably water at 30°C or higher, particularly preferably water at 35°C or higher, and most preferably water at 40°C or higher. Furthermore, organic solvents such as alcohols at temperatures above the above temperatures can also be used, even if they are not water. In other words, it is sufficient that thermal vibrations of atoms and molecules are conducted.

[0106] [Fourth Form] <Thermoelectric Conversion Element (Fourth Form)> As shown in the schematic diagram of FIG. 36 , a thermoelectric conversion element 4100 of the present invention includes a positive electrode 410 and a negative electrode 420 made of materials with different electrical conductivities, and an organic semiconductor layer between the positive electrode 410 and the negative electrode 420, the organic semiconductor layer including a material that generates electrons and holes upon thermal excitation, the organic semiconductor layer including a first organic semiconductor layer 432 on the positive electrode side and a second semiconductor layer 434 on the negative electrode side, and further including a layer 440 made of a carbon-based substance between the first organic semiconductor layer 432 and the second semiconductor layer 434.

[0107] (Positive and negative electrodes made of materials with different electrical conductivities) The thermoelectric conversion element of the present invention uses positive and negative electrodes made of materials with different electrical conductivities. This generates an internal electric field between the electrodes, and electrons and holes, which are charge carriers generated by thermal excitation in the organic semiconductor layer, migrate to the negative and positive electrodes, respectively, due to the internal electric field, thereby generating an electromotive force. In this way, the thermoelectric conversion element of the present invention generates an electromotive force even when the positive and negative electrodes are in the same temperature environment, and is based on a theory different from the conventional Seebeck effect.

[0108] A model diagram is shown in Figure 37, and a theoretical explanation of the thermoelectric conversion element of the present invention is provided. The most fundamental phenomenon is that two electrode materials with different electrical conductivities generate an internal electric field between the electrodes. If two different electrode materials were directly joined, this would be the well-known thermocouple technology, i.e., the configuration of a Seebeck element. However, in the present invention, instead of joining two different electrode materials, we fabricated an element in which the electrode with the higher conductivity serves as the negative electrode and the electrode with the lower conductivity serves as the positive electrode. We sandwiched an organic semiconductor layer between these electrodes, containing a material that emits electrons and holes upon thermal excitation. This successfully generated a large internal electric field. The resulting electromotive force was equivalent to 100,000 to 1,000,000 times that generated by a thermocouple. It was revealed that by creating a structure in which charge carriers move and are polarized, electrons can easily move to the negative electrode and holes to the positive electrode due to the heat flow from the outside, thereby generating a large electromotive force.

[0109] Explaining based on Figure 37, the energy levels of the positive and negative poles in the figure are Fermi levels. The energy levels of organic semiconductors are, from top to bottom, the lowest unoccupied molecular orbital (LUMO) and the highest occupied molecular orbital (HOMO). When discussing the energy levels of organic semiconductors, it is permissible to compare the band gaps of the LUMO and HOMO with the energy levels of inorganic materials.

[0110] In the thermoelectric conversion element of the present invention, electrons emitted by the organic semiconductor due to thermal excitation caused by receiving ambient thermal energy migrate. Specifically, carriers (electrons, holes) generated by charge separation in the organic semiconductor migrate between the inside of the element and the external circuit according to the energy levels of each substance. That is, electrons in the LUMO of the second organic semiconductor layer acquire energy exceeding the Fermi level of the negative electrode and migrate to the conduction band. Accordingly, holes in the HOMO of the second organic semiconductor layer migrate to the HOMO of the first organic semiconductor layer, and then further acquire energy exceeding the Fermi level of the positive electrode and migrate to the conduction band. This type of carrier migration generates an electromotive force.

[0111] In the present invention, it is preferable that the HOMO energy level of the first organic semiconductor layer is higher than the HOMO energy level of the second organic semiconductor layer. Therefore, the energy level of holes is stepped toward the positive electrode, allowing smooth movement of holes. As a result, a large electromotive force can be obtained.

[0112] Furthermore, it is preferable that the energy difference between the HOMO and LUMO of the second organic semiconductor layer is larger than the energy difference between the HOMO and LUMO of the first organic semiconductor layer, and electrons that have acquired a large amount of energy are located on the negative electrode side where the internal electric field is large, thereby increasing the resulting electromotive force.

[0113] Thus, with the thermoelectric conversion element of the present invention, electromotive force can be generated even when the negative and positive electrodes are at the same temperature. The phenomenon of electromotive force generation in a thermocouple is reflected by the temperature difference between the reference point of the measurement system and the point of contact with the heat flow. However, with the present invention, even when measurements are performed by applying a heat flow while all copper wires, instruments, and elements in the measurement system are placed in the same temperature environment, results equivalent to those obtained by measuring electromotive force and power generation when only the element is in contact with the heat flow can be obtained. This means that in the thermoelectric conversion element of the present invention, thermally excited electrons and holes function as an element with diode characteristics that exhibit the same behavior as photoexcited electrons and holes inside a photovoltaic cell generated by photoelectric conversion, thereby generating electromotive force. This is a fundamentally novel feature that differs from conventional Seebeck elements.

[0114] Among materials with different conductivities, an electrode made of a material with low conductivity that results in a high hole density becomes the positive electrode, and an electrode made of a material with high conductivity that results in a high electron density becomes the negative electrode. Here, high conductivity and low conductivity are determined by comparing the material that constitutes the positive electrode with the material that constitutes the negative electrode.

[0115] The greater the difference in conductivity between the positive electrode 410 and the negative electrode 420, the stronger the internal electric field generated between the electrodes; therefore, the lower limit of the difference in conductivity between the positive electrode 410 and the negative electrode 420 is preferably 50 S / m or more, more preferably 100 S / m or more. However, if the difference in conductivity is too large, the electrodes themselves begin to exhibit resistance, causing not only energy loss but also a decrease in performance, such as a slowdown in the thermoelectric conversion rate. Furthermore, although there are no particular limitations on the upper limit, from the viewpoint of the materials that can be selected, it is generally preferably 10,000 S / m or less, more preferably 1,000 S / m or less.

[0116] The conductivity of the negative electrode 420 with high conductivity is 1×10 7 ~1 x 10 8 S / m, and the conductivity of the positive electrode 410 having low conductivity is preferably 1×10 3 ~1 x 10 5 It is preferable to set it to S / m.

[0117] Examples of materials constituting the electrodes include metals, conductive organic substances, carbon materials such as amorphous carbon, ceramics, amorphous metals, etc. Examples of materials constituting the positive electrode 10 include, for example, tin-doped indium oxide (ITO), an oxide of indium and tin, carbon-based materials, and carbon black. Examples of materials constituting the negative electrode 20 include, for example, metal materials such as aluminum, gold, silver, platinum, and copper. In the thermoelectric conversion element of the present invention, it is important to generate an internal electric field between the electrodes. As long as the desired internal electric field can be generated, various conductive materials can be appropriately selected and applied. For example, the same type of conductive material can be used for both the positive and negative electrodes. For example, pencils obtained by blending carbon and clay have different conductivity depending on the blending ratio. An electrode obtained by applying a pencil with a high conductivity can be used as the negative electrode, and an electrode obtained by applying a pencil with a low conductivity can be used as the positive electrode.

[0118] (Organic Semiconductor Layer) The organic semiconductor layer may be any layer that has the function of generating electrons and holes upon thermal excitation and the function of transporting the generated electrons and holes to the respective electrodes, and layers made of various materials may be used as long as they have these functions. For example, an organic semiconductor may be used as a material that generates electrons and holes upon thermal excitation.

[0119] Examples of organic semiconductors include organic charge transfer complexes such as complexes of phthalocyanine and various transition metals. More specifically, examples include magnetic metal-containing organic complex compounds such as iron phthalocyanine (FePc), nickel phthalocyanine (NiPc), manganese phthalocyanine (MnPc), cobalt phthalocyanine (CoPc), iron porphyrin complexes, nickel porphyrin complexes, manganese porphyrin complexes, and cobalt porphyrin complexes, and diamagnetic metal-containing organic complex compounds such as copper phthalocyanine (CuPc), zinc phthalocyanine (ZnPc), copper porphyrin complexes, and zinc porphyrin complexes.

[0120] The organic semiconductor layer preferably contains a medium that transports electrons and holes emitted by the organic semiconductor upon thermal excitation to the negative electrode and positive electrode. As such a charge carrier transport medium, for example, an emulsifier such as polyoxyethylene sorbitan monostearate can be used.

[0121] In the present invention, the organic semiconductor layer is composed of two layers: a first organic semiconductor layer 432 on the positive electrode 410 side, and a second organic semiconductor layer 434 on the negative electrode 420 side. As described above, the HOMO energy level of the first organic semiconductor layer 432 is preferably higher than the HOMO energy level of the second semiconductor layer 434, which results in a configuration that can obtain a high electromotive force.

[0122] An example of a combination of organic semiconductors that can achieve such a configuration is a combination in which the organic semiconductor contained in the first organic semiconductor layer is iron phthalocyanine, and the organic semiconductor contained in the second organic semiconductor layer is copper phthalocyanine, cobalt phthalocyanine, nickel phthalocyanine, or zinc phthalocyanine.

[0123] (Layer made of carbon-based material) The present invention further includes a layer made of a carbon-based material between the first organic semiconductor layer and the second semiconductor layer. In the organic semiconductor layer, the polyoxyethylene sorbitan monostearate described above acts as a thickener, maintaining the shape of the organic semiconductor layer itself. However, as the temperature increases, the viscosity of polyoxyethylene sorbitan monostearate decreases, and the thickening effect weakens. This can cause component flow between the first organic semiconductor and the second organic semiconductor. In the present invention, by including a layer made of a carbon-based material between the first organic semiconductor layer and the second semiconductor layer, component flow is suppressed, allowing electromotive force to be maintained for a long period of time even under high-temperature conditions.

[0124] Furthermore, the element of the present invention, in which a layer made of a carbon-based material is laminated between organic semiconductors, not only suppresses the fluidity of the organic semiconductor layer but also enhances the charge transport efficiency in low-temperature, low-resistance circuits, and as shown in the following examples, a clear increase in the amount of power generated was observed in a temperature environment of 60° C. or less. This effect can be understood by considering two elements, namely, a positive electrode / first organic semiconductor layer / layer made of a carbon-based material and a layer made of a carbon-based material / second organic semiconductor layer / negative electrode, connected in series.

[0125] Examples of carbon-based materials constituting the carbon-based layer include graphite, graphene, and fullerene. It is also possible to sandwich a Teflon filter having pores of 10 nm to 100 nm between the carbon-based layer and the first organic semiconductor layer and / or the second organic semiconductor layer. This makes it possible to suppress the diffusion of the carbon-based material, the diffusion of the first organic semiconductor material on the positive electrode side, and the diffusion of the second organic semiconductor material on the negative electrode side without interfering with the movement of charge carriers (ions, electrons, and holes).

[0126] <Method for manufacturing thermoelectric conversion element (fourth embodiment)> The thermoelectric conversion element of the present invention can be manufactured, for example, by the following steps: a step of preparing a mixed solution containing an organic semiconductor; a step of forming an organic semiconductor layer on an electrode surface; and a step of forming a thermoelectric conversion element.

[0127] (Preparation of Mixed Solution Containing Organic Semiconductor) A mixed solution containing an organic semiconductor can be obtained by mixing an organic semiconductor, a charge carrier transport medium, and a solvent capable of dissolving the transport medium, and stirring as necessary. The amount of solvent can be appropriately adjusted so that the solution is easy to handle (applicable), and if there is no problem with applicability, a solvent may not be added. The solvent is not particularly limited, but for example, chloroform can be used.

[0128] (Step of forming an organic semiconductor layer on the electrode surface) The mixed solution formed above is applied to the surfaces of the positive electrode and the negative electrode and dried, thereby forming an organic semiconductor layer on the electrode surface. A preferred embodiment is to apply the mixed solution to the surfaces of the positive electrode and the negative electrode, respectively, to form a first organic semiconductor layer on the surface of the positive electrode and a second organic semiconductor layer on the surface of the negative electrode. In this embodiment, it is possible to improve the adhesion between the positive electrode and the negative electrode and the respective organic semiconductor layers.

[0129] Alternatively, a device can be formed by sequentially forming a first organic semiconductor layer, a layer made of a carbon-based material, and a second organic semiconductor layer on the surface of a positive electrode, and then bonding the second organic semiconductor layer to the surface of a negative electrode. Similarly, a device can be formed by sequentially forming a second organic semiconductor layer, a layer made of a carbon-based material, and a first organic semiconductor layer on the surface of a negative electrode, and then bonding the first organic semiconductor layer to the surface of a positive electrode. However, in this case, it becomes necessary to adjust the pressing force and heating temperature when bonding the electrodes so as to ensure adhesion between the electrodes and the organic semiconductor layer.

[0130] (Step of Forming Thermoelectric Conversion Element) The thermoelectric conversion element of the present invention is formed by bonding the first organic semiconductor layer formed on the positive electrode surface and the second organic semiconductor layer formed on the negative electrode surface, obtained as described above, via a layer made of a carbon-based material. That is, the thermoelectric conversion element of the present invention can be formed by bonding the first organic semiconductor layer formed on the positive electrode surface to one side of the layer made of a carbon-based material and bonding the second organic semiconductor layer formed on the negative electrode surface to the other side. Specifically, with the first organic semiconductor layer on the positive electrode side facing up, a carbon-based material such as graphite powder is scattered on the first organic semiconductor layer, preferably to a thickness of 1 μm to 20 μm, more preferably 5 μm to 15 μm, and then bonded to the second organic semiconductor layer on the negative electrode side.

[0131] As described above, it is also possible to form a device by laminating a Teflon filter having pores of 10 nm to 100 nm on the layer made of a carbon-based substance formed on the first organic semiconductor layer, and then bonding the second organic semiconductor layer on the negative electrode side thereon. Alternatively, it is also possible to form a device by laminating a Teflon filter on the first organic semiconductor layer, forming a layer made of a carbon-based substance thereon, and then laminating a Teflon filter on top of that, and then bonding the second organic semiconductor layer on the negative electrode side thereon.

[0132] That is, the layer configuration can be as follows: positive electrode / first organic semiconductor layer / layer made of carbon-based material / Teflon filter / second organic semiconductor layer / negative electrode positive electrode / first organic semiconductor layer / Teflon filter / layer made of carbon-based material / second organic semiconductor layer / negative electrode positive electrode / first organic semiconductor layer / Teflon filter / layer made of carbon-based material / Teflon filter / second organic semiconductor layer / negative electrode

[0133] These forms are preferable from the viewpoint of suppressing the diffusion of the carbon-based material in the intermediate layer, the diffusion of the organic semiconductor material on the positive electrode side, and the diffusion of the organic semiconductor material on the negative electrode side, without interfering with the movement of charge carriers (ions, electrons, and holes).

[0134] A pressing force of preferably about 1,200 hPa to 1,500 hPa is applied to the laminated structure of positive electrode / first organic semiconductor layer / layer made of carbon-based material / second organic semiconductor layer / negative electrode, and the pressure is maintained for preferably 60 minutes to 120 minutes, thereby allowing the first organic semiconductor layer / layer made of carbon-based material / second organic semiconductor layer to adhere tightly to each other.

[0135] Furthermore, by simultaneously heating the laminate during lamination, the organic semiconductor layer can be more effectively integrated. Heating can be preferably performed within a range of 50° C. or higher and 140° C. or lower.

[0136] <Thermoelectric Conversion Method (Fourth Form)> According to the thermoelectric conversion method of the present invention, it is possible to convert thermal energy into electrical energy simply by placing the above-mentioned thermoelectric conversion element in the presence of a thermal energy flow that creates a certain thermal environment. In other words, while conventional methods based on the Seebeck effect require a temperature difference between the positive electrode and the negative electrode, the method of the present application does not require a temperature difference, and it is sufficient to simply place the thermoelectric conversion element in a thermal environment of a constant temperature in the presence of a thermal energy flow.

[0137] The term "constant-temperature thermal environment in the presence of thermal energy flow" refers to any thermal environment that can impart constant thermal energy to the thermoelectric conversion element, preferably in an atmosphere at 20°C (room temperature) or higher, more preferably in an atmosphere at 25°C or higher, even more preferably in an atmosphere at 30°C or higher, particularly preferably in an atmosphere at 35°C or higher, and most preferably in an atmosphere at 40°C or higher. This phenomenon can be understood in comparison with the movement of electrons and holes excited by light energy within a solar cell under a constant light irradiation environment in the presence of light energy flow, and is a physically understandable phenomenon. Furthermore, when the light energy flow stops, the solar cell ceases to generate electromotive force. However, in the thermoelectric conversion method of the present invention, a decrease in the inflow of thermal energy flow corresponds to the cessation of light energy flow in a solar cell, and can be understood in comparison with the decline in the electromotive force generation function. However, unlike the cessation of light irradiation, the energy distribution of atoms and molecules mediating the thermal energy flow does not instantly become zero but gradually decays, so the phenomenon of generating electromotive force does not suddenly become zero.

[0138] Furthermore, even in a gaseous atmosphere other than air, for example, in an inert gas such as nitrogen, it can be said that the environment is capable of imparting thermal energy to the thermoelectric conversion element as long as the temperature is similar to that described above. Furthermore, the thermoelectric conversion element may be placed in an atmosphere other than gas, for example, in a liquid such as water. From the viewpoint of efficiently imparting thermal energy to the thermoelectric conversion element, it can be said that it is preferable to place the thermoelectric conversion element in an underwater atmosphere at a predetermined temperature. The underwater thermal environment can be preferably water at 20°C (room temperature) or higher, more preferably water at 25°C or higher, even more preferably water at 30°C or higher, particularly preferably water at 35°C or higher, and most preferably water at 40°C or higher. Furthermore, organic solvents such as alcohols at temperatures above the above temperatures can also be used, even if they are not water. In other words, it is sufficient that thermal vibrations of atoms and molecules are conducted.

[0139] Examples of the resin composition of the present invention are shown below, but the present invention is not limited to the following examples as long as the gist of the invention is not exceeded.

[0140] [First Form] <Materials Used> The materials used in the following examples are as follows. (Iron Phthalocyanine (FePc)) Phthalocyanine (hereinafter sometimes abbreviated as Pc) is a cyclic compound with a structure in which four phthalic acid imides are bridged by nitrogen atoms, and has a structure similar to porphyrin. The central part forms a complex with various elements including transition metals, forming a stable complex. Because the π-electron conjugated system extends throughout the molecule, it has a planar structure and exhibits a strong color. The molecule in which the central part of this phthalocyanine forms a complex with an iron atom is iron phthalocyanine (FePc). Molecular formula C 32 H 16 N 8 Fe is a dark purple powder with a molecular weight of 568.38 and is insoluble in water. It is also used as an organic semiconductor, similar to copper phthalocyanine (CuPc). In the present invention, it is used as an organic semiconductor that emits electrons and holes upon thermal excitation (hole, electron emitting material), and Tokyo Chemical Industry Co., Ltd.'s P0774 was used.

[0141] The structural formula of iron phthalocyanine (FePc) is as follows: The measured optical absorption spectrum is shown in FIG.

[0142]

[0143] (Zinc phthalocyanine (ZnPc)) Zinc phthalocyanine (ZnPc) is a molecule in which the central part of phthalocyanine is complexed with a zinc atom. Molecular formula C 32 H 16 N 8 Zn is a dark red to dark purple to dark blue powder with a molecular weight of 577.92, and is insoluble in water. It is also used as an organic semiconductor, similar to copper phthalocyanine (CuPc). In the present invention, it is used as an organic semiconductor, a material that emits electrons and holes upon thermal excitation (hole, electron emitting material), and P0767 from Tokyo Chemical Industry Co., Ltd. was used.

[0144] The structural formula of zinc phthalocyanine (ZnPc) and the measured optical absorption spectrum are shown below: The measured optical absorption spectrum is also shown in FIG.

[0145]

[0146] (Tin-doped indium oxide (ITO) glass) Tin-doped indium oxide (ITO) glass is a type of transparent conductive glass. When a thin film of tin-doped indium oxide is formed on an insulating glass substrate, it becomes conductive and is used as a transparent electrode. In the present invention, TCO 1001 manufactured by Geomatec Co., Ltd. was used as the electrode substrate.

[0147] (Chloroform) Chloroform is a type of alkyl halide and its IUPAC name is trichloromethane. It has a molecular weight of 119.38 and a molecular formula of CHCl 3 It is a colorless, transparent liquid with a sweet taste and a strong, sweet aroma. Although it is highly volatile, it dissolves many organic compounds well and is therefore widely used as a solvent. In this invention, Nacalai Tesque's 08402-55 was used as the organic solvent.

[0148] (Polyoxyethylene sorbitan monostearate) Polyoxyethylene sorbitan monostearate is a pale yellow solid. Its melting point is 20-24°C, and it is stored as a Vaseline-like solid at room temperature. Its main uses are as an emulsifier, solubilizer, colorant solubilizer, and emulsion polymerization stabilizer for pharmaceuticals and cosmetics. In the present invention, it is used to adjust the viscosity of a chloroform suspension of a material that emits electrons and holes upon thermal excitation (hole, electron emitting material, organic semiconductor), and as a transport medium for charge carriers emitted from the dispersed organic semiconductor. The polyoxyethylene sorbitan monostearate used was 35702-85 from Nacalai Tesque.

[0149] (Graphite) Graphite, also known as graphite, is a dark gray-black powder that is practically insoluble in water. It has electrical conductivity and lubricity, and its main uses include synthetic raw materials, functional materials, synthetic resin additives, lubricants, and release agents. In the present invention, 070-01325 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used for the charge transport layer.

[0150] <Preparation of Mixed Solutions Containing Organic Semiconductors> The FePc solution was prepared by mixing 0.5 g of FePc powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate in a vial. The ZnPc solution was prepared by mixing 1.0 g of ZnPc powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate in a vial. After stirring each solution in a vortex mixer, the solution was kept at 40°C or higher to prevent the polyoxyethylene sorbitan monostearate from solidifying.

[0151] <Formation of Organic Semiconductor Layer> 60 μL of the mixed solution prepared above was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy electric furnace, long type, programmable type, ROP-002P. This process produced ITO substrate / organic semiconductor layer (FePc), ITO substrate / organic semiconductor layer (ZnPc), Al substrate / organic semiconductor layer (FePc), and Al substrate / organic semiconductor layer (ZnPc).

[0152] Example 1-1: The ITO substrate / organic semiconductor layer (FePc) and Al substrate / organic semiconductor layer (FePc) prepared above were bonded together so that the organic semiconductor layers overlapped, to produce a thermoelectric conversion element consisting of ITO substrate / organic semiconductor layer (FePc) / organic semiconductor layer (FePc) / Al substrate. The produced thermoelectric conversion element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0153] Example 1-2: The ITO substrate / organic semiconductor layer (ZnPc) and Al substrate / organic semiconductor layer (ZnPc) prepared above were bonded together so that the organic semiconductor layers overlapped, to produce a thermoelectric conversion element consisting of ITO substrate / organic semiconductor layer (ZnPc) / organic semiconductor layer (ZnPc) / Al substrate. The produced thermoelectric conversion element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0154] Comparative Example 1-1: Two Al substrates / organic semiconductor layer (FePc) prepared as described above were bonded together so that the organic semiconductor layers overlapped, to prepare an element consisting of Al substrate / organic semiconductor layer (FePc) / organic semiconductor layer (FePc) / Al substrate. The prepared element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0155] Comparative Example 1-2: Two ITO substrates / organic semiconductor layers (ZnPc) prepared as described above were bonded together so that the organic semiconductor layers overlapped, to produce an element consisting of ITO substrate / organic semiconductor layer (ZnPc) / organic semiconductor layer (ZnPc) / ITO substrate. The produced element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0156] Comparative Example 1-3: In Comparative Example 1-3, a device was fabricated by sandwiching only metal-free phthalocyanine between electrodes, and thermoelectric conversion measurements were performed. 0.5 g of phthalocyanine (Pc) powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate were mixed in a vial. 60 μL of this mixture was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy long-type programmable electric furnace, model ROP-002P. This process produced an ITO substrate / phthalocyanine layer (Pc) and an Al substrate / phthalocyanine layer (Pc).

[0157] The ITO substrate / phthalocyanine layer (Pc) and the Al substrate / phthalocyanine layer (Pc) prepared above were bonded together so that the phthalocyanine layers overlapped, to prepare an element consisting of ITO substrate / phthalocyanine layer (Pc) / phthalocyanine layer (Pc) / Al substrate. The prepared element was sealed with a silicone resin to prevent the phthalocyanine layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0158] Comparative Example 1-4 In Comparative Example 1-4, a device was fabricated by sandwiching phthalonitrile, a metal-free phthalocyanine component, between electrodes, and thermoelectric conversion measurements were performed. 0.5 g of phthalonitrile (PN) powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate were mixed in a vial. 60 μL of this mixture was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy long-type programmable electric furnace, ROP-002P. This process produced an ITO substrate / phthalonitrile layer (PN) and an Al substrate / phthalonitrile layer (PN).

[0159] The ITO substrate / phthalonitrile layer (PN) and the Al substrate / phthalonitrile layer (PN) prepared above were bonded together so that the phthalonitrile layers overlapped, to prepare an element consisting of an ITO substrate / phthalonitrile layer (PN) / phthalonitrile layer (PN) / Al substrate. The prepared element was sealed with a silicone resin to prevent the phthalonitrile layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0160] <Measurement of Electrical Energy in Thermoelectric Conversion> For the elements fabricated in the above Examples and Comparative Examples, a measurement circuit such as that shown in FIG. 5 was constructed to measure the electrical energy that can be extracted from thermal energy in a thermal equilibrium state under a constant thermal environment at a specific temperature T (K). Here, two digital multimeter and PC units were connected, and a measurement system was constructed so that changes in the measured values ​​over time could be observed when measuring current and voltage. The circuit was then designed with a variable resistor incorporated, and the resistance was set to 110 Ω. The ambient temperature including the element was set to 20°C (room temperature).

[0161] Figure 6(a) shows the measurement results of the voltage of the element of Comparative Example 1-1, and Figure 6(b) shows the measurement results of the current of the element of Comparative Example 1-1. Figure 7(a) shows the measurement results of the voltage of the element of Comparative Example 1-2, and Figure 7(b) shows the measurement results of the current of the element of Comparative Example 1-2.

[0162] Figure 8(a) shows the measurement results of the voltage of the element of Example 1-1, and Figure 8(b) shows the measurement results of the current of the element of Example 1-1. Figure 9(a) shows the measurement results of the voltage of the element of Example 1-2, and Figure 9(b) shows the measurement results of the current of the element of Example 1-2.

[0163] 10 shows the measurement results of the current and voltage of the element of Comparative Example 1-3, and FIG. 11 shows the measurement results of the current and voltage of the element of Comparative Example 1-4.

[0164] From the above results, it was found that in the elements of Examples 1-1 and 1-2, both the voltage and current were constant and electric power was obtained. In contrast, in the elements of Comparative Examples 1-1 and 1-2, the voltage attenuated, the current was zero, and no electric power was obtained. In other words, it was shown that in order to generate an electromotive force, it is necessary to construct the positive and negative electrodes with materials having different electrical conductivities and generate an internal electric field between the electrodes. Furthermore, it was found that in the elements of Comparative Examples 3 and 4, the voltage attenuated, the current was zero, and no electric power was obtained. In other words, it was shown that in order to generate an electromotive force, an organic semiconductor layer comprising a material that is thermally excited to generate electrons and holes between the specified electrodes is necessary. Furthermore, it was shown that by using the thermoelectric conversion element of the present invention, it is possible to convert thermal energy into electrical energy in a certain thermal environment in the presence of a thermal energy flow.

[0165] [Second embodiment] <Materials used> The materials used in the following examples are as follows. (Iron phthalocyanine (FePc)) Phthalocyanine (hereinafter sometimes abbreviated as Pc) is a cyclic compound with a structure in which four phthalic acid imides are bridged by nitrogen atoms, and has a structure similar to porphyrin. The central part forms a complex with various elements including transition metals, forming a stable complex. Because the π-electron conjugated system extends throughout the molecule, it has a planar structure and exhibits a strong color. The molecule in which the central part of this phthalocyanine forms a complex with an iron atom is iron phthalocyanine (FePc). Molecular formula C 32 H 16 N 8Fe is a dark purple powder with a molecular weight of 568.38 and is insoluble in water. It is also used as an organic semiconductor, similar to copper phthalocyanine (CuPc). In the present invention, it is used as an organic semiconductor that emits electrons and holes upon thermal excitation (hole, electron emitting material), and Tokyo Chemical Industry Co., Ltd.'s P0774 was used.

[0166] The structural formula of iron phthalocyanine (FePc) is as follows: The measured optical absorption spectrum is shown in FIG.

[0167]

[0168] (Zinc phthalocyanine (ZnPc)) Zinc phthalocyanine (ZnPc) is a molecule in which the central part of phthalocyanine is complexed with a zinc atom. Molecular formula C 32 H 16 N 8 Zn is a dark red to dark purple to dark blue powder with a molecular weight of 577.92, and is insoluble in water. It is also used as an organic semiconductor, similar to copper phthalocyanine (CuPc). In the present invention, it is used as an organic semiconductor, a material that emits electrons and holes upon thermal excitation (hole, electron emitting material), and P0767 from Tokyo Chemical Industry Co., Ltd. was used.

[0169] The structural formula of zinc phthalocyanine (ZnPc) and the measured optical absorption spectrum are shown below: The measured optical absorption spectrum is also shown in FIG.

[0170]

[0171] (Tin-doped indium oxide (ITO) glass) Tin-doped indium oxide (ITO) glass is a type of transparent conductive glass. When a thin film of tin-doped indium oxide is formed on an insulating glass substrate, it becomes conductive and is used as a transparent electrode. In the present invention, TCO 1001 manufactured by Geomatec Co., Ltd. was used as the electrode substrate.

[0172] (Chloroform) Chloroform is a type of alkyl halide and its IUPAC name is trichloromethane. It has a molecular weight of 119.38 and a molecular formula of CHCl 3 It is a colorless, transparent liquid with a sweet taste and a strong, sweet aroma. Although it is highly volatile, it dissolves many organic compounds well and is therefore widely used as a solvent. In this invention, Nacalai Tesque's 08402-55 was used as the organic solvent.

[0173] (Polyoxyethylene sorbitan monostearate) Polyoxyethylene sorbitan monostearate is a pale yellow solid. Its melting point is 20-24°C, and it is stored as a Vaseline-like solid at room temperature. Its main uses are as an emulsifier, solubilizer, colorant solubilizer, and emulsion polymerization stabilizer for pharmaceuticals and cosmetics. In the present invention, it is used to adjust the viscosity of a chloroform suspension of a material that emits electrons and holes upon thermal excitation (hole, electron emitting material, organic semiconductor), and as a transport medium for charge carriers emitted from the dispersed organic semiconductor. The polyoxyethylene sorbitan monostearate used was 35702-85 from Nacalai Tesque.

[0174] (Graphite) Graphite, also known as graphite, is a dark gray-black powder that is practically insoluble in water. It has electrical conductivity and lubricity, and its main uses include synthetic raw materials, functional materials, synthetic resin additives, lubricants, and release agents. In the present invention, 070-01325 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used for the charge transport layer.

[0175] <Preparation of Mixed Solutions Containing Organic Semiconductors> The FePc solution was prepared by mixing 0.5 g of FePc powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate in a vial. The ZnPc solution was prepared by mixing 1.0 g of ZnPc powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate in a vial. After stirring each solution in a vortex mixer, the solution was kept at 40°C or higher to prevent the polyoxyethylene sorbitan monostearate from solidifying.

[0176] <Formation of Organic Semiconductor Layer> 60 μL of the mixed solution prepared above was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy electric furnace, long type, programmable type, ROP-002P. This process produced ITO substrate / organic semiconductor layer (FePc), ITO substrate / organic semiconductor layer (ZnPc), Al substrate / organic semiconductor layer (FePc), and Al substrate / organic semiconductor layer (ZnPc).

[0177] Example 2-1: The ITO substrate / organic semiconductor layer (FePc) and the Al substrate / organic semiconductor layer (ZnPc) prepared above were bonded together so that the organic semiconductor layers overlapped, to produce a thermoelectric conversion element consisting of an ITO substrate / organic semiconductor layer (FePc) / organic semiconductor layer (ZnPc) / Al substrate. The produced thermoelectric conversion element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0178] Comparative Example 2-1: Two Al substrates / organic semiconductor layer (FePc) prepared as described above were bonded together so that the organic semiconductor layers overlapped, to produce an element consisting of Al substrate / organic semiconductor layer (FePc) / organic semiconductor layer (FePc) / Al substrate. The produced element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0179] Comparative Example 2-2: Two ITO substrates / organic semiconductor layer (ZnPc) prepared as described above were bonded together so that the organic semiconductor layers overlapped, to produce an element consisting of ITO substrate / organic semiconductor layer (ZnPc) / organic semiconductor layer (ZnPc) / ITO substrate. The produced element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0180] Comparative Example 2-3 In Comparative Example 3, a device was fabricated by sandwiching only metal-free phthalocyanine between electrodes, and thermoelectric conversion measurements were performed. 0.5 g of phthalocyanine (Pc) powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate were mixed in a vial. 60 μL of this mixture was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy long-type programmable electric furnace, model ROP-002P. This process produced an ITO substrate / phthalocyanine layer (Pc) and an Al substrate / phthalocyanine layer (Pc).

[0181] The ITO substrate / phthalocyanine layer (Pc) and the Al substrate / phthalocyanine layer (Pc) prepared above were bonded together so that the phthalocyanine layers overlapped, to prepare an element consisting of ITO substrate / phthalocyanine layer (Pc) / phthalocyanine layer (Pc) / Al substrate. The prepared element was sealed with a silicone resin to prevent the phthalocyanine layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0182] Comparative Example 2-4 In Comparative Example 2-4, a device was fabricated by sandwiching phthalonitrile, a metal-free phthalocyanine component, between electrodes, and thermoelectric conversion measurements were performed. 0.5 g of phthalonitrile (PN) powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate were mixed in a vial. 60 μL of this mixture was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy long-type programmable electric furnace, ROP-002P. This process produced an ITO substrate / phthalonitrile layer (PN) and an Al substrate / phthalonitrile layer (PN).

[0183] The ITO substrate / phthalonitrile layer (PN) and the Al substrate / phthalonitrile layer (PN) prepared above were bonded together so that the phthalonitrile layers overlapped, to prepare an element consisting of an ITO substrate / phthalonitrile layer (PN) / phthalonitrile layer (PN) / Al substrate. The prepared element was sealed with a silicone resin to prevent the phthalonitrile layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0184] Comparative Example 2-5: The ITO substrate / organic semiconductor layer (ZnPc) and Al substrate / organic semiconductor layer (FePc) prepared above were bonded together so that the organic semiconductor layers overlapped, to produce a thermoelectric conversion element consisting of an ITO substrate / organic semiconductor layer (ZnPc) / organic semiconductor layer (FePc) / Al substrate. The produced thermoelectric conversion element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0185] <Measurement of Electrical Energy in Thermoelectric Conversion> For the elements fabricated in the above Examples and Comparative Examples, a measurement circuit such as that shown in Figure 16 was constructed to measure the electrical energy that can be extracted from thermal energy in a thermal equilibrium state in a constant thermal environment at a specific temperature T (K). Here, two digital multimeter and PC units were connected, and a measurement system was constructed so that changes in the measured values ​​over time could be observed when measuring current and voltage. The circuit was then designed with a variable resistor incorporated, and the ambient temperature including the element was set to 20°C (room temperature).

[0186] In Comparative Examples 2-1 to 2-4, the resistance was set to 110 Ω. In Example 2-1 and Comparative Example 2-5, the resistance was changed to 110 Ω, 10 kΩ, 100 kΩ, and 500 kΩ, and measurements were performed.

[0187] Figure 17(a) shows the measurement results of the voltage of the element of Comparative Example 2-1, and Figure 17(b) shows the measurement results of the current of the element of Comparative Example 2-1. Figure 18(a) shows the measurement results of the voltage of the element of Comparative Example 2-2, and Figure 18(b) shows the measurement results of the current of the element of Comparative Example 2-2.

[0188] 19 shows the measurement results of the current and voltage of the element of Comparative Example 2-3, and FIG. 20 shows the measurement results of the current and voltage of the element of Comparative Example 2-4.

[0189] FIG. 21(a) shows the current value versus temperature for Example 2-1, FIG. 21(b) shows the voltage value versus temperature for Example 2-1, and FIG. 21(c) shows the power value versus temperature for Example 2-1.

[0190] Fig. 22(a) shows the current value versus temperature for Comparative Example 2-5, Fig. 22(b) shows the voltage value versus temperature for Comparative Example 2-5, and Fig. 22(c) shows the power value versus temperature for Comparative Example 2-5. Fig. 23(a) shows the power obtained versus temperature for Example 2-1 and Comparative Example 2-5 at a variable resistance of 10 kΩ, and Fig. 23(b) shows the power value obtained versus temperature for Example 2-1 and Comparative Example 2-5 at a variable resistance of 100 kΩ.

[0191] From the above results, it was found that in the elements of Comparative Examples 2-1 and 2-2, the voltage attenuated, the current was zero, and no power was obtained. In other words, it was shown that in order to generate an electromotive force, it is necessary to construct the positive and negative electrodes with materials having different electrical conductivities and to generate an internal electric field between the electrodes. Furthermore, it was found that in the elements of Comparative Examples 2-3 and 2-4, the voltage attenuated, the current was zero, and no power was obtained. In other words, it was shown that in order to generate an electromotive force, an organic semiconductor layer comprising a material that is thermally excited to generate electrons and holes is required between the specified electrodes.

[0192] In contrast, in Example 2-1, as shown in Figures 21(a) and 21(b), it was confirmed that the measured current and voltage values ​​increased depending on the temperature, reaching a maximum at 120°C or 140°C when the resistance was low and then decreasing at higher temperatures. It was also confirmed that the measured current and voltage values ​​increased at 100°C or 120°C when the resistance was high and then decreasing at higher temperatures. Figure 21(c) shows that the highest power generation was achieved when 10 kΩ was applied at 120°C, with a calculated value of 11.868 μW. It was also found that greater power could be extracted at 100 kΩ than at 10 kΩ between 20°C and 80°C.

[0193] Furthermore, in Comparative Example 2-5, Figures 22(a) and 22(b) show changes in measured values ​​roughly similar to those of the ITO / FePc / ZnPc / Al type element of Example 2-1. However, the current and voltage values ​​were relatively low at all temperatures. Figure 22(c) shows that the largest amount of power generation was achieved when 10 kΩ was applied at 140°C, with a calculated value of 5.244 μW. It was also found that measurements at 100 kΩ were greater than measurements at 10 kΩ below 100°C, and that measurements at 500 kΩ were greater than measurements at 40°C below. In other words, the lower the temperature, the more power a circuit with a higher resistance can generate.

[0194] 23(a) and 23(b) show a comparison of the power between the thermoelectric conversion element of Example 2-1 and the thermoelectric conversion element of Comparative Example 5 at 10 kΩ and 100 kΩ, where the power is calculated to be particularly large. It can be seen that the difference in power generation amount becomes large at high temperatures, with the difference being several times greater. Thus, comparing the power values ​​of Example 1 and Comparative Example 5, it can be seen that the thermoelectric conversion element of the present invention generates power more efficiently.

[0195] <Example 2-2> We investigated the change in performance when multiple thermoelectric conversion elements of Example 2-1 were connected. Figure 24 shows the changes in current and voltage when multiple thermoelectric conversion elements of Example 2-1 were connected. In a 500 kΩ circuit at room temperature (21°C), when the number of elements was increased to 3, 4, 6, and 8, the measured values ​​of both current and voltage increased linearly in proportion to the number of elements. Therefore, it can be said that we were able to confirm that each element functions as a battery.

[0196] [Third Form] <Materials Used> The materials used in the following examples are as follows. (Iron Phthalocyanine (FePc)) Phthalocyanine (hereinafter sometimes abbreviated as Pc) is a cyclic compound with a structure in which four phthalic acid imides are bridged by nitrogen atoms, and has a structure similar to porphyrin. The central part forms a complex with various elements including transition metals, forming a stable complex. Because the π-electron conjugated system extends throughout the molecule, it has a planar structure and exhibits a strong color. The molecule in which the central part of this phthalocyanine forms a complex with an iron atom is iron phthalocyanine (FePc). Molecular formula C 32 H 16 N 8 Fe is a dark purple powder with a molecular weight of 568.38 and is insoluble in water. It is also used as an organic semiconductor, similar to copper phthalocyanine (CuPc). In the present invention, it is used as an organic semiconductor that emits electrons and holes upon thermal excitation (hole, electron emitting material), and Tokyo Chemical Industry Co., Ltd.'s P0774 was used.

[0197] The structural formula of iron phthalocyanine (FePc) is as follows: The measured optical absorption spectrum is shown in FIG.

[0198]

[0199] (Zinc phthalocyanine (ZnPc)) Zinc phthalocyanine (ZnPc) is a molecule in which the central part of phthalocyanine is complexed with a zinc atom. Molecular formula C 32 H 16 N 8 Zn is a dark red to dark purple to dark blue powder with a molecular weight of 577.92, and is insoluble in water. It is also used as an organic semiconductor, similar to copper phthalocyanine (CuPc). In the present invention, it is used as an organic semiconductor, a material that emits electrons and holes upon thermal excitation (hole, electron emitting material), and P0767 from Tokyo Chemical Industry Co., Ltd. was used.

[0200] The structural formula of zinc phthalocyanine (ZnPc) and the measured optical absorption spectrum are shown below: The measured optical absorption spectrum is also shown in FIG.

[0201]

[0202] (Tin-doped indium oxide (ITO) glass) Tin-doped indium oxide (ITO) glass is a type of transparent conductive glass. When a thin film of tin-doped indium oxide is formed on an insulating glass substrate, it becomes conductive and is used as a transparent electrode. In the present invention, TCO 1001 manufactured by Geomatec Co., Ltd. was used as the electrode substrate.

[0203] (Chloroform) Chloroform is a type of alkyl halide and its IUPAC name is trichloromethane. It has a molecular weight of 119.38 and a molecular formula of CHCl 3 It is a colorless, transparent liquid with a sweet taste and a strong, sweet aroma. Although it is highly volatile, it dissolves many organic compounds well and is therefore widely used as a solvent. In this invention, Nacalai Tesque's 08402-55 was used as the organic solvent.

[0204] (Polyoxyethylene sorbitan monostearate) Polyoxyethylene sorbitan monostearate is a pale yellow solid. Its melting point is 20-24°C, and it is stored as a Vaseline-like solid at room temperature. Its main uses are as an emulsifier, solubilizer, colorant solubilizer, and emulsion polymerization stabilizer for pharmaceuticals and cosmetics. In the present invention, it is used to adjust the viscosity of a chloroform suspension of a material that emits electrons and holes upon thermal excitation (hole, electron emitting material, organic semiconductor), and as a transport medium for charge carriers emitted from the dispersed organic semiconductor. The polyoxyethylene sorbitan monostearate used was 35702-85 from Nacalai Tesque.

[0205] (Graphite) Graphite, also known as graphite, is a dark gray-black powder that is practically insoluble in water. It has electrical conductivity and lubricity, and its main uses include synthetic raw materials, functional materials, synthetic resin additives, lubricants, and release agents. In the present invention, 070-01325 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used for the charge transport layer.

[0206] <Preparation of Mixed Solutions Containing Organic Semiconductors> The FePc solution was prepared by mixing 0.5 g of FePc powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate in a vial. The ZnPc solution was prepared by mixing 1.0 g of ZnPc powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate in a vial. After stirring each solution in a vortex mixer, the solution was kept at 40°C or higher to prevent the polyoxyethylene sorbitan monostearate from solidifying.

[0207] <Formation of Organic Semiconductor Layer> 60 μL of the mixed solution prepared above was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy electric furnace, long type, programmable type, ROP-002P. This process produced ITO substrate / organic semiconductor layer (FePc), ITO substrate / organic semiconductor layer (ZnPc), Al substrate / organic semiconductor layer (FePc), and Al substrate / organic semiconductor layer (ZnPc).

[0208] Example 3-1 (Preparation of a mixed solution containing Fe ions and an organic semiconductor) 0.5 g of FePc powder was mixed with an equivalent weight of iron (III) chloride (FeCl 3 0.5 g of ZnPc powder and 0.1 g of 10 wt% lithium carbonate were mixed together, followed by 6 mL of chloroform and 2 mL of polyoxyethylene sorbitan monostearate in a 30 mL beaker. The mixture was heated to 50°C and degassed in a vacuum dryer to remove water molecules, to prepare a reagent mixture (mixed solution (A)). Also, 0.5 g of ZnPc powder and an equivalent weight of iron(II) chloride (FeCl 2) and 0.1 g of 10 wt % lithium carbonate were mixed, and then 6 mL of chloroform and 2 mL of polyoxyethylene sorbitan monostearate were added to a 30 mL beaker. The mixture was degassed in a vacuum dryer while being heated to 50°C to remove water molecules, thereby preparing a reagent designated as mixed solution (B).

[0209] (Formation of an organic semiconductor layer containing Fe ions and a thermoelectric conversion element) Next, 0.1 g of the mixed solution (A) was laminated on an ITO glass substrate, and 0.1 g of the mixed solution (B) was laminated on an Al substrate, and the two were stacked to form an element. The area of ​​the element was 10 cm. 2 The inside was sealed with silicone resin to prevent leakage of the compound.

[0210] (Measurement of Electrical Energy in Thermoelectric Conversion) 24 hours after the sealing, the following measurement was carried out to measure the power generation performance. Two digital multimeters as measuring instruments, all of the conductors constituting the circuit, and the element were placed in the same large tray (50 cm x 30 cm x 20 cm), and the temperature was raised to 50°C and then stopped repeatedly. The circuit load was 110 Ω.

[0211] The results shown in Figure 30 were obtained. The current value reached 1,800 μA, and decreased during the period when the inflow of heat flow stopped, and then increased during the temperature rise process due to the re-inflow of heat flow. Performance evaluation of this element revealed that the generated electrical energy exceeded 1 milliwatt. This power generation performance shows greater thermoelectric conversion characteristics than previously known thermoelectric elements.

[0212] Comparative Example 3-1: Two Al substrates / organic semiconductor layer (FePc) prepared as described above were bonded together so that the organic semiconductor layers overlapped, to produce an element consisting of Al substrate / organic semiconductor layer (FePc) / organic semiconductor layer (FePc) / Al substrate. The produced element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0213] Comparative Example 3-2: Two ITO substrates / organic semiconductor layer (ZnPc) prepared as described above were bonded together so that the organic semiconductor layers overlapped, to produce an element consisting of ITO substrate / organic semiconductor layer (ZnPc) / organic semiconductor layer (ZnPc) / ITO substrate. The produced element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0214] Comparative Example 3-3 In Comparative Example 3-3, a device was fabricated by sandwiching only metal-free phthalocyanine between electrodes, and thermoelectric conversion measurements were performed. 0.5 g of phthalocyanine (Pc) powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate were mixed in a vial. 60 μL of this mixture was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy long-type programmable electric furnace, model ROP-002P. This process produced an ITO substrate / phthalocyanine layer (Pc) and an Al substrate / phthalocyanine layer (Pc).

[0215] The ITO substrate / phthalocyanine layer (Pc) and the Al substrate / phthalocyanine layer (Pc) prepared above were bonded together so that the phthalocyanine layers overlapped, to prepare an element consisting of ITO substrate / phthalocyanine layer (Pc) / phthalocyanine layer (Pc) / Al substrate. The prepared element was sealed with a silicone resin to prevent the phthalocyanine layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0216] Comparative Example 3-4 In Comparative Example 3-4, a device was fabricated by sandwiching phthalonitrile, a metal-free phthalocyanine component, between electrodes, and thermoelectric conversion measurements were performed. 0.5 g of phthalonitrile (PN) powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate were mixed in a vial. 60 μL of this mixture was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy electric furnace, long type, programmable, ROP-002P. This process produced an ITO substrate / phthalonitrile layer (PN) and an Al substrate / phthalonitrile layer (PN).

[0217] The ITO substrate / phthalonitrile layer (PN) and the Al substrate / phthalonitrile layer (PN) prepared above were bonded together so that the phthalonitrile layers overlapped, to prepare an element consisting of an ITO substrate / phthalonitrile layer (PN) / phthalonitrile layer (PN) / Al substrate. The prepared element was sealed with a silicone resin to prevent the phthalonitrile layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0218] <Measurement of Electrical Energy in Thermoelectric Conversion> For the elements produced in Comparative Examples 3-1 to 3-4 above, a measurement circuit such as that shown in Figure 7 was constructed to measure the electrical energy that can be extracted from thermal energy in a thermal equilibrium state in a constant thermal environment at a specific temperature T (K). Here, two digital multimeter and PC units were connected, and a measurement system was constructed so that changes in the measured values ​​over time could be observed when measuring current and voltage. The circuit was then designed with a variable resistor incorporated, and the ambient temperature including the element was set to 20°C (room temperature).

[0219] In Comparative Examples 3-1 to 3-4, the resistance was set to 110Ω.

[0220] Figure 32(a) shows the measurement results of the voltage of the element of Comparative Example 3-1, and Figure 32(b) shows the measurement results of the current of the element of Comparative Example 3-1. Figure 33(a) shows the measurement results of the voltage of the element of Comparative Example 3-2, and Figure 33(b) shows the measurement results of the current of the element of Comparative Example 3-2.

[0221] Fig. 34 shows the measurement results of the current and voltage of the element of Comparative Example 3-3. Fig. 35 shows the measurement results of the current and voltage of the element of Comparative Example 3-4.

[0222] From the above results, it was found that in the elements of Comparative Examples 3-1 and 3-2, the voltage attenuated, the current was zero, and no power was obtained. In other words, it was shown that in order to generate an electromotive force, it is necessary to configure the positive and negative electrodes with materials having different conductivities and generate an internal electric field between the electrodes. Furthermore, it was found that in the elements of Comparative Examples 3-3 and 3-4, the voltage attenuated, the current was zero, and no power was obtained. In other words, it was shown that in order to generate an electromotive force, an organic semiconductor layer comprising a material that is thermally excited to generate electrons and holes is required between the specified electrodes.

[0223] [Fourth Form] <Materials Used> The materials used in the following examples are as follows. (Iron Phthalocyanine (FePc)) Phthalocyanine (hereinafter sometimes abbreviated as Pc) is a cyclic compound with a structure in which four phthalic acid imides are bridged by nitrogen atoms, and has a structure similar to porphyrin. The central part forms a complex with various elements including transition metals, forming a stable complex. Because the π-electron conjugated system extends throughout the molecule, it has a planar structure and exhibits a strong color. The molecule in which the central part of this phthalocyanine forms a complex with an iron atom is iron phthalocyanine (FePc). Molecular formula C 32 H 16 N 8 Fe is a dark purple powder with a molecular weight of 568.38 and is insoluble in water. It is also used as an organic semiconductor, similar to copper phthalocyanine (CuPc). In the present invention, it is used as an organic semiconductor that emits electrons and holes upon thermal excitation (hole, electron emitting material), and Tokyo Chemical Industry Co., Ltd.'s P0774 was used.

[0224] The structural formula of iron phthalocyanine (FePc) is as follows: The measured optical absorption spectrum is shown in FIG.

[0225]

[0226] (Zinc phthalocyanine (ZnPc)) Zinc phthalocyanine (ZnPc) is a molecule in which the central part of phthalocyanine is complexed with a zinc atom. Molecular formula C 32 H 16 N 8 Zn is a dark red to dark purple to dark blue powder with a molecular weight of 577.92, and is insoluble in water. It is also used as an organic semiconductor, similar to copper phthalocyanine (CuPc). In the present invention, it is used as an organic semiconductor, a material that emits electrons and holes upon thermal excitation (hole, electron emitting material), and P0767 from Tokyo Chemical Industry Co., Ltd. was used.

[0227] The structural formula of zinc phthalocyanine (ZnPc) and the measured optical absorption spectrum are shown below: The measured optical absorption spectrum is also shown in FIG.

[0228]

[0229] (Tin-doped indium oxide (ITO) glass) Tin-doped indium oxide (ITO) glass is a type of transparent conductive glass. When a thin film of tin-doped indium oxide is formed on an insulating glass substrate, it becomes conductive and is used as a transparent electrode. In the present invention, TCO 1001 manufactured by Geomatec Co., Ltd. was used as the electrode substrate.

[0230] (Chloroform) Chloroform is a type of alkyl halide and its IUPAC name is trichloromethane. It has a molecular weight of 119.38 and a molecular formula of CHCl 3It is a colorless, transparent liquid with a sweet taste and a strong, sweet aroma. Although it is highly volatile, it dissolves many organic compounds well and is therefore widely used as a solvent. In this invention, Nacalai Tesque's 08402-55 was used as the organic solvent.

[0231] (Polyoxyethylene sorbitan monostearate) Polyoxyethylene sorbitan monostearate is a pale yellow solid. Its melting point is 20-24°C, and it is stored as a Vaseline-like solid at room temperature. Its main uses are as an emulsifier, solubilizer, colorant solubilizer, and emulsion polymerization stabilizer for pharmaceuticals and cosmetics. In the present invention, it is used to adjust the viscosity of a chloroform suspension of a material that emits electrons and holes upon thermal excitation (hole, electron emitting material, organic semiconductor), and as a transport medium for charge carriers emitted from the dispersed organic semiconductor. The polyoxyethylene sorbitan monostearate used was 35702-85 from Nacalai Tesque.

[0232] (Graphite) Graphite, also known as graphite, is a dark gray-black powder that is practically insoluble in water. It has electrical conductivity and lubricity, and its main uses include synthetic raw materials, functional materials, synthetic resin additives, lubricants, and release agents. In the present invention, 070-01325 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used for the charge transport layer.

[0233] <Preparation of Mixed Solutions Containing Organic Semiconductors> The FePc solution was prepared by mixing 0.5 g of FePc powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate in a vial. The ZnPc solution was prepared by mixing 1.0 g of ZnPc powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate in a vial. After stirring each solution in a vortex mixer, the solution was kept at 40°C or higher to prevent the polyoxyethylene sorbitan monostearate from solidifying.

[0234] <Formation of Organic Semiconductor Layer> 60 μL of the mixed solution prepared above was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy electric furnace, long type, programmable type, ROP-002P. This process produced ITO substrate / organic semiconductor layer (FePc), ITO substrate / organic semiconductor layer (ZnPc), Al substrate / organic semiconductor layer (FePc), and Al substrate / organic semiconductor layer (ZnPc).

[0235] Example 4-1: 0.08 g of graphite was laminated on the surface of the organic semiconductor layer (FePc) of the ITO substrate / organic semiconductor layer (FePc) prepared above to form a graphite layer measuring 10 mm x 15 mm, and the organic semiconductor layer (ZnPc) of the Al substrate / organic semiconductor layer (ZnPc) was then superimposed on top of this to prepare a thermoelectric conversion element consisting of ITO substrate / organic semiconductor layer (FePc) / graphite layer / organic semiconductor layer (ZnPc) / Al substrate. The prepared thermoelectric conversion element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0236] Comparative Example 4-1: Two Al substrates / organic semiconductor layer (FePc) prepared as described above were bonded together so that the organic semiconductor layers overlapped, to produce an element consisting of Al substrate / organic semiconductor layer (FePc) / organic semiconductor layer (FePc) / Al substrate. The produced element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0237] Comparative Example 4-2: Two ITO substrates / organic semiconductor layer (ZnPc) prepared as described above were bonded together so that the organic semiconductor layers overlapped, to produce an element consisting of ITO substrate / organic semiconductor layer (ZnPc) / organic semiconductor layer (ZnPc) / ITO substrate. The produced element was sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0238] Comparative Example 4-3 In Comparative Example 4-3, a device was fabricated by sandwiching only metal-free phthalocyanine between electrodes, and thermoelectric conversion measurements were performed. 0.5 g of phthalocyanine (Pc) powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate were mixed in a vial. 60 μL of this mixture was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy long-type programmable electric furnace, ROP-002P. This process produced an ITO substrate / phthalocyanine layer (Pc) and an Al substrate / phthalocyanine layer (Pc).

[0239] The ITO substrate / phthalocyanine layer (Pc) and the Al substrate / phthalocyanine layer (Pc) prepared above were bonded together so that the phthalocyanine layers overlapped, to prepare an element consisting of ITO substrate / phthalocyanine layer (Pc) / phthalocyanine layer (Pc) / Al substrate. The prepared element was sealed with a silicone resin to prevent the phthalocyanine layer from protruding when heated for subsequent thermoelectric conversion measurements.

[0240] Comparative Example 4-4 In Comparative Example 4-4, a device was fabricated by sandwiching phthalonitrile, a metal-free phthalocyanine component, between electrodes, and thermoelectric conversion measurements were performed. 0.5 g of phthalonitrile (PN) powder, 3 mL of chloroform, and 1 mL of polyoxyethylene sorbitan monostearate were mixed in a vial. 60 μL of this mixture was dropped onto a 10 mm x 15 mm area in the center of an ITO glass substrate and an Al substrate. After air drying, each substrate was heated in an electric furnace at 140°C for 2 hours. The electric furnace used was an AS ONE Corporation economy long-type programmable electric furnace, ROP-002P. This process produced an ITO substrate / phthalonitrile layer (PN) and an Al substrate / phthalonitrile layer (PN).

[0241] The ITO substrate / phthalonitrile layer (PN) and the Al substrate / phthalonitrile layer (PN) prepared above were bonded together so that the phthalonitrile layers overlapped, to prepare an element consisting of an ITO substrate / phthalonitrile layer (PN) / phthalonitrile layer (PN) / Al substrate. The prepared element was sealed with a silicone resin to prevent the phthalonitrile layer from protruding when heated during subsequent thermoelectric conversion measurements.

[0242] <Measurement of Electrical Energy in Thermoelectric Conversion> For the elements fabricated in the above Examples and Comparative Examples, a measurement circuit such as that shown in Figure 5 was constructed to measure the electrical energy that can be extracted from thermal energy in a thermal equilibrium state in a constant thermal environment at a specific temperature T (K). Here, two digital multimeter and PC units were connected, and a measurement system was constructed so that changes in the measured values ​​over time could be observed when measuring current and voltage. The circuit was then designed with a variable resistor incorporated, and the ambient temperature including the element was set to 20°C (room temperature).

[0243] In Comparative Examples 4-1 to 4-4, the resistance was set to 110 Ω. In Example 4-1, the resistance was changed to 110 Ω, 10 kΩ, 100 kΩ, and 500 kΩ, and measurements were performed.

[0244] Figure 41(a) shows the measurement results of the voltage of the element of Comparative Example 4-1, and Figure 41(b) shows the measurement results of the current of the element of Comparative Example 4-1. Figure 42(a) shows the measurement results of the voltage of the element of Comparative Example 4-2, and Figure 42(b) shows the measurement results of the current of the element of Comparative Example 4-2.

[0245] Fig. 43 shows the measurement results of the current and voltage of the element of Comparative Example 4-3. Fig. 44 shows the measurement results of the current and voltage of the element of Comparative Example 4-4.

[0246] FIG. 45(a) shows the current value versus temperature for Example 4-1, FIG. 45(b) shows the voltage value versus temperature for Example 4-1, and FIG. 45(c) shows the power value versus temperature for Example 4-1.

[0247] From the above results, it was found that in the elements of Comparative Examples 4-1 and 4-2, the voltage attenuated, the current was zero, and no power was obtained. In other words, it was shown that in order to generate an electromotive force, it is necessary to construct the positive and negative electrodes with materials having different electrical conductivities and to generate an internal electric field between the electrodes. Furthermore, it was found that in the elements of Comparative Examples 4-3 and 4-4, the voltage attenuated, the current was zero, and no power was obtained. In other words, it was shown that in order to generate an electromotive force, an organic semiconductor layer comprising a material that is thermally excited to generate electrons and holes is required between the specified electrodes.

[0248] In contrast, in Example 4-1, as shown in Figures 45(a) and 45(b), when the resistance was low, the measured value increased depending on the temperature (110 Ω), but when the resistance was high, the measured value peaked between 100 and 120 °C and then dropped at 140 °C. From Figure 45(c), it was found that the largest amount of power generation was achieved when 10 kΩ was applied at 120 °C, and was calculated to be 7.156 μW. It was also found that at temperatures below 60 °C, greater power could be extracted when measured at 100 kΩ than when measured at 10 kΩ.

[0249] The fact that the insertion of graphite improved the performance of small resistance circuits at temperatures between 20°C and 60°C can be understood as a phenomenon as follows, as depicted in Figure 46. When Gr is inserted into the intermediate layer to form ITO / FePc / Gr / ZnPc / Al, the electrical conductivity of Gr (σ ≈ 105 S / m) is smaller than that of Al (σ ≈ 108 S / m), but it is conductive and Gr can also function as an electrode.

[0250] Generally, the electrical resistance of a material changes with temperature. While the resistance of metal conductors increases with increasing temperature, the resistance of semiconductors and carbon decreases. Therefore, if we consider that Gr has electrode-like properties and functions as a doublet series element, such as an ITO / FePc / Gr element and a Gr / ZnPc / Al element, the performance improvement at 20°C can be understood. Furthermore, Gr is a carbon atom aggregate, realizing continuous charge transfer in the organic semiconductors ZnPc and FePc via the vacant p orbitals. As the temperature increases, the resistance of Gr decreases, the energy band gap narrows, and the available potential energy becomes relatively small. Therefore, it is thought that the power will decrease at high temperatures above 60°C.

[0251] [Common features of the first to fourth embodiments] <Experimental data for proving the theoretical framework of the present invention> (Proof that the thermoelectric conversion method of the present invention is not a phenomenon caused by ionization tendency) As shown in Figure 47, a conductor having platinum foil fixed to a 0.3 mm thick aluminum plate was prepared as one electrode, and a conductor having a carbon electrode fixed to a glass plate with double-sided tape was prepared as the other electrode. A substance obtained by drying a mixed solution containing organic semiconductor iron phthalocyanine and ferrous chloride under reduced pressure was laminated as the thermoelectric conversion material of the present invention, and the platinum electrode was connected to the (-) terminal of a voltmeter, and a carbon black electrode was connected to the (+) terminal of the voltmeter, and the electromotive force was measured at a variable resistance of 500 kΩ.

[0252] As a result, a positive change was obtained, as shown in Figure 48. This means that the platinum electrode is operating as a negative electrode, and it became clear that this does not follow the commonly known rule that "in the case of a phenomenon due to ionization tendency, platinum, which has the smallest ionization tendency, acts as a positive electrode." Therefore, it was proven that the thermoelectric conversion method of the present invention is not a phenomenon due to ionization tendency.

[0253] (Proof that the thermoelectric conversion method of the present invention is not a phenomenon involving a chemical reaction) As shown in Figure 49, a conductor was prepared in which one electrode was a high-resistance carbon electrode with a value of 2 kOhm, obtained by applying HB pencil light to a piece of paper, and attached with double-sided tape to a 1.1 mm thick glass plate, and the other electrode was a low-resistance carbon electrode with a value of 0.4 kOhm, obtained by applying 8B pencil light to a piece of paper, and attached with double-sided tape to a glass plate.As the thermoelectric conversion material of the present invention, a substance obtained by drying a mixed solution containing organic semiconductor iron phthalocyanine and ferrous chloride under reduced pressure was laminated as the conversion material, and the low-resistance carbon electrode was connected to the (-) terminal of a voltmeter, and the high-resistance carbon electrode was connected to the (+) terminal of the voltmeter, and the electromotive force was measured at a variable resistance of 500 kOhm.

[0254] As a result, a positive change was obtained, as shown in Figure 50. This means that the low-resistance carbon electrode is operating as the negative electrode, and it has become clear that the operation is based on the physical principle proposed by the present invention between carbon electrodes that are not chemically reactive. This also proves that the thermoelectric conversion method of the present invention is not a phenomenon caused by a chemical reaction due to ionization tendency or the like.

[0255] The results of the above two proofs are shown in Table 1. Here, the thermoelectric conversion element of the present invention is sometimes referred to as a thermovoltaic cell. In the table, this is referred to as TV cell, and hereafter TV cell is an abbreviation for the thermoelectric conversion element of the present invention.

[0256]

[0257] (Charge transfer phenomenon due to thinning of the negative electrode of the element and the correlation between area and power generation) Figure 51 shows the element design when aluminum foil was used for the aluminum negative electrode in the fourth embodiment element fabrication, and the element width (W) was changed to 3 mm, 6 mm, 9 mm, 12 mm, and 15 mm. A comparison was conducted to determine whether there were any differences in the current characteristics. The results were as shown in Figure 52. To observe the changes immediately after circuit connection in detail, a magnified comparison was performed in Figure 53. It was revealed that as the value of W increased, the current value flowing immediately after circuit connection increased, and then the current value decayed and approached 9 μA in both cases. This revealed that thinning the negative electrode and reducing its area resulted in differences in the number of electrons moving from the conversion material to the negative electrode. This means that exciton generation and charge separation due to thermal excitation occur in the element of the present invention even before circuit connection.

[0258] <Experimental data showing power generation effect> (Effect of series connection by stacking elements) Figure 54 shows that in the production of the fourth form of element, by using a carbon electrode such as carbon black as the positive electrode, it is possible to connect elements continuously in series without using a conductor, and three sets of elements were successfully connected. The measured values ​​of the voltage and current of the element obtained in this way, when a variable resistance of 500 kΩ was used, were as shown in Figure 55.

[0259] Next, in a similar manner, the case of connecting four sets of elements is described in Figure 56. The results are shown in Figure 57. The results in Figures 55 and 57 make it clear that there is a proportional relationship to the number of layers.

[0260] (Scaling up power generation capacity by connecting power generation elements in series and in parallel) Figure 58 shows the current change when five elements obtained by configuring a thermoelectric conversion element of the third type described below are connected in series, and Figure 59 shows the change when they are connected in parallel. In configuring this element, the (+) electrode / ITO substrate / organic semiconductor layer (FePc) + transition element (FeCl 2 ・nH 2A thermovoltaic cell (referred to as TV cell in the figures as a thermoelectric conversion element of the present invention, hereafter TV cell will be abbreviated as the thermoelectric conversion element of the present invention) was fabricated by coating a substrate with a size of 10 mm x 10 mm x 0.03 mm thick and sealing it. The three elements other than the two ends were conductively connected in series by overlapping the (+) electrodes of each element with the (-) electrodes of the adjacent element. For parallel connections, the (+) electrodes were connected together in a circuit using a cord with alligator clips on both ends, and the (-) electrodes were similarly connected together to form a parallel configuration. The fabricated elements were sealed with a silicone resin to prevent the organic semiconductor layer from protruding when heated during subsequent thermoelectric conversion measurements. When connected in series, the electromotive force was 4.4 to 5.6 V, about five times the approximately 1 V of a single element, and when connected in parallel, the electromotive force was a single value, but the current value was scaled up five times to 10,000 μA.

[0261] (Inflow of heat flow flux and temperature change, and change in power generation amount) It can be confirmed that the thermoelectric conversion element of the present invention operates in an environment without temperature difference. Figure 60 shows the results of using an electric furnace (As One, ROP-002P), changing the temperature inside the furnace using a program, placing the element inside, and measuring the current with an ammeter and voltmeter. The element used here was (+) pole / ITO substrate / organic semiconductor layer (FePc) + transition element (FeCl 2 ・nH 2 A TV cell consisting of a 10mm x 10mm x 0.03mm thick aluminum substrate (-) electrode was coated on a substrate, and one of these was fabricated and placed in an electric furnace. The furnace was connected to an external measurement circuit via a thin lead. The measurement results showed that the current increased over a long period of time in response to temperature changes, and then decreased as the temperature in the furnace decreased.

[0262] Figure 61 shows the case where a larger current is generated using an element. Here, (+) pole / ITO substrate / first organic semiconductor layer (FePc) + transition element (FeCl 3 ・Anhydrous) addition / second organic semiconductor layer (ZnPc) + transition element (FeCl2 ・nH 2 A TV cell consisting of a 10 mm x 10 mm x 0.03 mm thick substrate with a 0.03 mm thick coating was prepared and placed in an electric furnace. The furnace was connected to an external measurement circuit via a thin lead.

[0263] FIG. 62 shows a (+) pole / ITO substrate / first organic semiconductor layer (FePc)+transition element (FeCl 3 ・Anhydrous) addition / second organic semiconductor layer (ZnPc) + transition element (FeCl 2 ・nH 2 A TV cell consisting of a 10mm x 10mm x 0.03mm thick substrate with a 0.03mm thick coating was fabricated and placed in an electric furnace. The furnace was connected to an external measurement circuit via a thin wire, and the current generated by the element was measured under conditions in which the temperature was programmed to rise gradually in steps and then rise sharply. The time lag between the generation of the heat flux generated when the temperature was raised stepwise in the electric furnace and the time required for the heat flux to spread to the element was confirmed. This characteristic indicates that power generation increases in an environment where the temperature rises gradually over a long period of time.

[0264] (Sustained power generation state close to the maximum value) Measurements were conducted to approach the upper limit of the power generation amount of the thermoelectric conversion element of the present invention. (+) pole / ITO substrate / first organic semiconductor layer (FePc)+transition element (FeCl 3 ・Anhydrous) addition / second organic semiconductor layer (ZnPc) + transition element (FeCl 2 ・nH 2A TV cell consisting of a 10 mm x 10 mm x 0.03 mm thick substrate with a ZnO-doped aluminum substrate (-) electrode was fabricated. A 1200 W dryer was used to continuously irradiate the cell with heat flux. Figure 63 shows the results when the heat flux irradiation was turned on and off. The current increased from 50 s after the heat flux irradiation was turned on until approximately 120 s, but then stopped increasing and reached a maximum. As the heat flux irradiation continued, the power generation remained constant even near the maximum. After 225 s after the heat flux irradiation was turned off, the current decreased over time.

[0265] (Scale-up) A device ((+) electrode / ITO substrate / organic semiconductor layer (FePc) + transition element (FeCl)) was fabricated by applying 50 mg of the thermoelectric conversion material of the third embodiment to an application area of ​​1 square cm. 3 A TV cell consisting of an anhydrous (added) / Al substrate (-) electrode (constructed by applying a film of 10 mm x 10 mm x 0.03 mm thickness to a substrate) with a resistance of 110 Ω in a work system reached a current value of 2 mA when exposed to a heat flux of 50 seconds. When 14 of these were connected in parallel, we investigated the power generation observed when exposed to a heat flux of 50 seconds. As a result, an output of 28 mA was measured, as shown in Figure 64. This suggests that the thermoelectric conversion element of the present invention, as a thermally pumped diode, can be scaled up in the same way as a photo-pumped solar cell.

[0266] (Power generation effect near room temperature) Figure 65 shows a device ((+) pole / ITO substrate / first organic semiconductor layer (FePc) + transition element (FeCl 3 ・Anhydrous) addition / second organic semiconductor layer (ZnPc) + transition element (FeCl 2 ・nH 2When six TV cells consisting of a 10mm x 10mm x 0.03mm thick substrate with a ZnO doped / Al substrate (-) electrode are connected in series, the blue light-emitting diode lights up at room temperature of 20°C. When a heat flux is irradiated onto this, the blue light-emitting diode emits light with increased brightness.

[0267] <Experimental Data Demonstrating Durability> (Element Sealing Stage and Durability) The simplest configuration of the element of the present invention is a structure in which a resin-containing double-sided tape is used between the electrodes to maintain a distance of approximately 15 to 30 μm, and a thermoelectric conversion material is inserted between the electrodes. Figure 66 shows a conceptual diagram of the resin and tape frame required for element construction. Preventing pressure drop between the thermoelectric conversion material and the electrodes is important. If a fibrous material such as paper is used in a carbon-carbon electrode construction, the material will seep into the gaps between the fibers, causing a drop in pressure. Furthermore, the double-sided tape used as a spacer to maintain the electrode spacing also contains fibers as a base material, which can cause similar problems.

[0268] (Relationship between element sealing and durability: Open circuit voltage value after application of heat flow flux (change over time)) Figure 67 shows the change over time of the open circuit voltage measured and recorded after applying heat flow flux every day for 100 days using three types of elements with different sealing levels. The following three types of element configurations were fabricated and compared. "Electrodes fixed with double-sided tape on a paper substrate (element A)": (+) electrode / ITO substrate / organic semiconductor layer (FePc) + transition element (FeCl 3 An element in which a TV cell consisting of an organic semiconductor layer (FePc) + transition element (FeCl) was applied to a substrate in a size of 10 mm x 10 mm x 0.03 mm thick, and a double-sided tape (NW10S manufactured by Nichiban Co., Ltd.) made of paper was cut to a width of 2 mm and attached to the substrate as a spacer and adhesive between the electrodes, but no resin or other sealing was applied to the periphery, "Electrodes fixed with silicone resin (element B)": (+) electrode / ITO substrate / organic semiconductor layer (FePc) + transition element (FeCl 3An element in which a TV cell consisting of an organic semiconductor layer (FePc) containing an anhydrous material and an Al substrate (-) electrode was applied to a substrate in a size of 10 mm x 10 mm x 0.03 mm thick, and a paper-based double-sided tape (NW10S manufactured by Nichiban Co., Ltd.) was cut to a width of 2 mm and adhered to the electrodes as a spacer and adhesive, and then the periphery was sealed with silicone resin, and the electrodes were fixed with a nonwoven fabric-based double-sided tape, and the periphery was fixed with a glass-to-metal fixing resin (element C): (+) electrode / ITO substrate / organic semiconductor layer (FePc) + transition element (FeCl 3 A TV cell consisting of a thermoelectric conversion material / Al substrate (-) electrode, which had been treated with anhydrous water and then dried under reduced pressure for 3 weeks to remove solvent molecules, was applied to a substrate in a size of 10 mm x 10 mm x 0.03 mm thick, and a nonwoven double-sided tape (MKRC-30, manufactured by Moritoku Co., Ltd.) was cut to a width of 2 mm and tightly adhered to the substrate as a spacer and adhesive between the electrodes, and then sealed with an epoxy-based adhesive (Araldite Cartridge Adhesive 2011, manufactured by Huntsman, Germany) which hardens into a glassy state.

[0269] The results were as shown in Figure 67. Element A had the poorest durability and deteriorated rapidly because the electrodes were only secured with double-sided tape on a paper substrate. This was thought to be due to its susceptibility to atmospheric moisture and other factors. Next, Element B, which secured the electrodes with silicone resin, had improved durability compared to Element A, but its performance halved over 100 days. This was thought to be due to the soft resin causing loosening between the electrodes and a decrease in pressure between the conversion material and the electrodes. It is desirable for the thermoelectric conversion material to be tightly attached to the electrodes without coming into contact with the outside world. Therefore, Element C, which was secured with thin double-sided tape and then completely secured around the device using a resin (Araldite Cartridge Adhesive 2011, Huntsman, Germany) that simultaneously secures the glass and metal and is highly resistant to thermal expansion and contraction, was found to maintain stable performance over 100 days without infiltration, deformation, or deterioration of the contents.

[0270] By using the thermoelectric conversion element of the present invention, it is possible to convert thermal energy into electrical energy even in a thermal environment of constant temperature in the presence of thermal energy flow. Therefore, this can contribute to the effective use of low-temperature waste heat from human living environments, geothermal energy, ocean heat, and atmospheric heat in temperate climates, regardless of season, location, or latitude. Furthermore, to cite a more recent example, in the extreme summer heat caused by global warming in recent years, if heat stored in homes, for example, in attics, can be effectively utilized, it can be used as an auxiliary power source for air conditioners in the summer, an auxiliary power source for electric vehicles that require charging, and especially as an auxiliary power source for solar power generation.

Claims

1. A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials with different electrical conductivities, and an organic semiconductor layer between the positive electrode and the negative electrode, the organic semiconductor layer comprising a material that can be thermally excited to generate electrons and holes.

2. A thermoelectric conversion element as described in claim 1, wherein the difference in conductivity between the high conductivity material constituting the negative electrode and the low conductivity material constituting the positive electrode is 50 S / m or more and 10,000 S / m or less as the materials with different electrical conductivity.

3. The thermoelectric conversion element according to claim 1 or 2, wherein the positive electrode is indium tin oxide or a carbon material, and the negative electrode is a metal material.

4. A thermoelectric conversion element according to claim 1 or 2, wherein the material that generates electrons and holes when thermally excited is a viscous liquid containing a material that generates electrons and holes when thermally excited.

5. The thermoelectric conversion element according to claim 4, wherein the viscous liquid is a viscous liquid capable of transporting ions as charge carriers.

6. A thermoelectric conversion element according to claim 1 or 2, wherein the material that is thermally excited to generate electrons and holes is iron phthalocyanine or zinc phthalocyanine.

7. A thermoelectric conversion method comprising the step of placing the thermoelectric conversion element according to claim 1 or 2 in a thermal environment.

8. A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials having different electrical conductivities, and an organic semiconductor layer between the positive electrode and the negative electrode, the organic semiconductor layer comprising a material that generates electrons and holes upon thermal excitation, the organic semiconductor layer comprising a first organic semiconductor layer on the positive electrode side and a second semiconductor layer on the negative electrode side, and the energy level of the HOMO of the first organic semiconductor layer is higher than the energy level of the HOMO of the second semiconductor layer.

9. A thermoelectric conversion element according to claim 8, wherein the difference in conductivity between the high conductivity material constituting the negative electrode and the low conductivity material constituting the positive electrode, as the materials with different electrical conductivity, is 50 S / m or more and 10,000 S / m or less.

10. The thermoelectric conversion element according to claim 8 or 9, wherein the positive electrode is indium tin oxide or a carbon material, and the negative electrode is a metal material.

11. A thermoelectric conversion element according to claim 8 or 9, wherein the material that generates electrons and holes when thermally excited is a viscous liquid containing a material that generates electrons and holes when thermally excited.

12. The thermoelectric conversion element according to claim 11, wherein the viscous liquid is a viscous liquid capable of transporting ions as charge carriers.

13. The thermoelectric conversion element according to claim 8 or 9, wherein the material that is thermally excited to generate electrons and holes is iron phthalocyanine or zinc phthalocyanine.

14. A thermoelectric conversion element according to claim 8 or 9, wherein the material contained in the first organic semiconductor layer that is thermally excited to generate electrons and holes is iron phthalocyanine, and the material contained in the second organic semiconductor layer that is thermally excited to generate electrons and holes is zinc phthalocyanine.

15. A thermoelectric conversion method comprising the step of placing the thermoelectric conversion element according to claim 8 or 9 in a thermal environment.

16. A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials having different electrical conductivities, and an organic semiconductor layer between the positive electrode and the negative electrode, the organic semiconductor layer comprising a material that is thermally excited to generate electrons and holes, the organic semiconductor layer further containing ions of a transition metal.

17. A thermoelectric conversion element as described in claim 16, wherein the difference in conductivity between the high conductivity material constituting the negative electrode and the low conductivity material constituting the positive electrode, as the materials with different electrical conductivity, is 50 S / m or more and 10,000 S / m or less.

18. The thermoelectric conversion element according to claim 16 or 17, wherein the positive electrode is indium tin oxide or a carbon material, and the negative electrode is a metal material.

19. A thermoelectric conversion element according to claim 16 or 17, wherein the material that generates electrons and holes when thermally excited is a viscous liquid containing a material that generates electrons and holes when thermally excited.

20. The thermoelectric conversion element according to claim 19, wherein the viscous liquid is a viscous liquid capable of transporting ions as charge carriers.

21. The thermoelectric conversion element according to claim 16 or 17, wherein the material that is thermally excited to generate electrons and holes is iron phthalocyanine or zinc phthalocyanine.

22. The thermoelectric conversion element according to claim 16 or 17, wherein the transition metal ions are at least one ion selected from the group consisting of iron ions, manganese ions, copper ions, cobalt ions and nickel ions.

23. A thermoelectric conversion method comprising the step of placing the thermoelectric conversion element according to claim 16 or 17 in a thermal environment.

24. A thermoelectric conversion element comprising a positive electrode and a negative electrode made of materials having different electrical conductivities, and an organic semiconductor layer between the positive electrode and the negative electrode, the organic semiconductor layer comprising a material that generates electrons and holes upon thermal excitation, the organic semiconductor layer comprising a first organic semiconductor layer on the positive electrode side and a second semiconductor layer on the negative electrode side, and further comprising a layer made of a carbon-based material between the first organic semiconductor layer and the second semiconductor layer.

25. A thermoelectric conversion element as described in claim 24, wherein the difference in conductivity between the high conductivity material constituting the negative electrode and the low conductivity material constituting the positive electrode, as the materials with different electrical conductivity, is 50 S / m or more and 10,000 S / m or less.

26. The thermoelectric conversion element according to claim 24 or 25, wherein the positive electrode is indium tin oxide or a carbon material, and the negative electrode is a metal material.

27. A thermoelectric conversion element according to claim 24 or 25, wherein the material that generates electrons and holes when thermally excited is a viscous liquid containing a material that generates electrons and holes when thermally excited.

28. The thermoelectric conversion element according to claim 27, wherein the viscous liquid is a viscous liquid capable of transporting ions as charge carriers.

29. A thermoelectric conversion element according to claim 24 or 25, wherein the energy level of the HOMO of the first organic semiconductor layer is higher than the energy level of the HOMO of the second organic semiconductor layer.

30. A thermoelectric conversion element according to claim 24 or 25, wherein the material that is thermally excited to generate electrons and holes is iron phthalocyanine or zinc phthalocyanine.

31. A thermoelectric conversion element according to claim 24 or 25, wherein the material contained in the first organic semiconductor layer that is thermally excited to generate electrons and holes is iron phthalocyanine, and the material contained in the second organic semiconductor layer that is thermally excited to generate electrons and holes is zinc phthalocyanine.

32. The thermoelectric conversion element according to claim 24 or 25, wherein the layer made of a carbon-based material is a layer made of graphite.

33. A thermoelectric conversion method comprising the step of placing the thermoelectric conversion element according to claim 24 or 25 in a thermal environment.

Citation Information

Patent Citations

  • x-y addressable electrical microswitch array and sensor matrix using it

    JP2002502128A

  • Power generating element

    JP2016100374A

  • Vehicle illumination device

    JP2017228675A

  • Thermoelectric conversion material and thermoelectric conversion device

    JP2021100064A

  • Heat utilization power generation module and manufacturing method for the same

    JP2023037269A