Furnace brazing-based corrugated metal hose

By forming a limiting part and clamping structure on the circular tubular connection section of the corrugated metal hose, combined with high-temperature solder and self-fusion welding, the problems of high difficulty and low welding quality of traditional corrugated metal hose are solved, and welding is achieved Improved strength and sealing.

WO2024227280A1PCT designated stage expired Publication Date: 2024-11-07ZHUJI SPIDER METAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/091981
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

During the welding process, traditional corrugated metal hoses have problems such as difficult welding, low weld quality, uneven welding gap, uneven solder penetration and difficult assembly. Especially, thin-walled corrugated pipes are prone to deform after brazing in the furnace and lead to welding. The pass rate is low and the processing is difficult.

Method used

Using a corrugated metal hose structure based on brazing in the furnace, the limit part is formed on the circular tubular connection section, combined with the clamping method of reinforced sleeve and connector, ensure uniform distribution of solder and welding quality, and use high-temperature melting point solder to improve Welding strength and sealing, and fixing the mesh sleeves through self-fusion welding or mechanical connections to improve connection strength.

Benefits of technology

It effectively solves the problems of uneven welding gap, uneven solder distribution and assembly difficulties, improves welding strength and sealing, reduces welding difficulty and process complexity, and ensures efficient welding and service performance of corrugated metal hoses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023091981_07112024_PF_FP_ABST
    Figure CN2023091981_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a furnace brazing-based corrugated metal hose, comprising a corrugated pipe, reinforcing sleeves, connecting pipes, a net sleeve fitted outside the corrugated pipe, and outer sleeves wrapping the ends of the net sleeve. Limiting parts are formed on the two circular pipe-shaped connecting sections of the corrugated pipe. The manufacturing method for the corrugated metal hose comprises the following processes: sleeving one circular pipe-shaped connecting section with the reinforcing sleeve, so as to form a soldering section used for soldering the connecting pipe; machining, on the circular pipe-shaped connecting section, a limiting part used for limiting the axial displacement of the reinforcing sleeve relative to the circular pipe-shaped connecting section in a direction towards a port of the circular pipe-shaped connecting section; fixing the soldering section by means of a tool to insert the connecting pipe into the soldering section; assembling the reinforcing sleeve and the connecting pipe on the other circular pipe-shaped connecting section by adopting the process steps; placing solder at each soldering joint between the inner peripheral wall of the circular pipe-shaped connecting section and the outer peripheral wall of the connecting pipe and at each soldering joint between the outer peripheral wall of the circular pipe-shaped connecting section and the inner peripheral wall of the reinforcing sleeve; and performing furnace brazing on the assembly undergoing the above-mentioned processes.
Need to check novelty before this filing date? Find Prior Art

Description

Corrugated metal hose based on furnace brazing Technical Field

[0001] The present invention relates to piping systems, and in particular to a corrugated metal hose based on furnace brazing. Background Art

[0002] Corrugated metal hoses are used in piping systems to compensate for displacement and installation deviations, absorb vibration, and reduce noise. They are widely used in piping systems in refrigeration, petrochemicals, steel, and transportation industries. Traditional corrugated metal hoses primarily consist of a bellows, a mesh sleeve, an inner sleeve, an outer sleeve, and a copper joint. The bellows, inner sleeve, and copper joint are brazed together using a brass flame brazing process to form two welds, A1 and A2. The outer sleeve, mesh sleeve, and inner sleeve are then joined using argon arc welding (A3), as shown in Figure 1. Because the bellows are made of thin-walled stainless steel, oxidation easily occurs during flame brazing. Even with the addition of flux, oxidation cannot be completely eliminated, leading to weld problems such as cold or broken welds. Furthermore, the three-step process of welding creates two welds, making it difficult to weld and guarantee quality. Furthermore, the low melting point of the welds formed by flame brazing makes secondary melting very likely when the corrugated metal hose is subsequently flame brazed with the system piping, leading to leaks.

[0003] In order to solve the problem of difficulty in welding traditional corrugated metal hoses, an improved corrugated metal hose has been proposed. As shown in Figure 2, the inner sleeve is a turned part, one end of which is connected to the bellows and then brazed in a furnace (at B1), and then the outer sleeve, mesh sleeve and inner sleeve are argon arc welded (at B2); finally, the copper tube is connected to the inner sleeve and flame brazed (at B3). Although this structure uses the turned inner sleeve as a transition piece to achieve step-by-step welding to reduce the difficulty of welding, it still has the problem of low weld quality after flame brazing of stainless steel products. Furthermore, the turned inner sleeve structure in this structure is not only complex in process and difficult to process, but also has very low processing efficiency. In order to further solve the problems brought about by flame brazing, Chinese patent CN108526636B proposes a corrugated metal hose formed by integrated furnace welding. In this structure, the bellows connection section is socketed and welded to the mating portion of the adapter on the corresponding side. The thin-walled bellows inserted into the brazing process can deform after prolonged, high-temperature furnace brazing, resulting in an uneven weld gap and a significant reduction in weld pass rate. Furthermore, the inner sleeve in this structure is still a difficult-to-machine turned part.

[0004] In order to solve the problems of difficult processing and low efficiency caused by turning the inner liner, Chinese patent CN218883236U discloses a metal hose structure in which the inner liner is formed by bending and rolling, and the metal hose can also be formed by integrated furnace welding. Although this structure effectively solves the problems caused by turning the inner liner, the bellows is located at the innermost side in this structure, and furnace brazing will still cause the thin-walled bellows to deform, resulting in uneven welding gap size and low welding qualification rate. In addition, since the solder will penetrate between the mesh sleeve and the bellows during integrated furnace brazing, the solidified solder layer will harden the corrugated metal hose, which will make it difficult for its static bending performance and dynamic bending performance to meet the standard requirements.

[0005] In addition, Chinese patent CN218348154U proposes a corrugated shock-absorbing pipe that improves the quality of welds by setting steps on the connecting pipe. In this structure, the setting of the two steps forms welds between the first step and the bellows, between the bellows and the steel bushing, and between the second step and the steel bushing. The multi-weld connection structure causes the flow of solder to be very random. During the actual welding process, it is difficult for the solder to penetrate according to the design expectation, resulting in problems such as cold welds, broken welds, and uneven distribution of solder in the necessary welds with sealing requirements. Furthermore, the multi-layer structure will also bring about the problem of difficulty in controlling the gaps between layers. In addition, this structure also has the problem of difficult assembly; specifically, in this structure, the connecting pipe, bellows and steel bushing need to be socketed in sequence, but there is no limit on the entire product.

[0006] Summary of the Invention

[0007] In order to overcome at least one deficiency of the prior art, the present invention provides a corrugated metal hose based on furnace brazing.

[0008] To achieve the above-mentioned object, the present invention provides a corrugated metal hose based on furnace brazing, which includes a corrugated pipe, a reinforcement sleeve, a connecting pipe, a mesh sleeve wrapped around the corrugated pipe, and an outer sleeve covering the end of the mesh sleeve; the corrugated pipe includes a central corrugated section and two circular tubular connecting sections located at both ends of the corrugated section, and each circular tubular connecting section is formed with a limiting portion;

[0009] The manufacturing method of the corrugated metal hose based on furnace brazing includes the following steps:

[0010] The reinforcing sleeve is placed outside the circular tubular connecting section of the corrugated pipe to form a welding section for welding the connecting pipe;

[0011] A limiting portion is machined on the circular tubular connecting section for limiting the axial displacement of the reinforcement sleeve relative to the circular tubular connecting section in a direction pointing to the end of the circular tubular connecting section;

[0012] Fixing the welding section by a tool to press the pipe into the welding section;

[0013] Using the above steps, assemble the reinforcement sleeve and the connecting pipe on the other circular tubular connecting section of the corrugated pipe;

[0014] Placing solder at the weld between the inner circumferential wall of the circular tubular connecting section and the outer circumferential wall of the connecting pipe, and at the weld between the outer circumferential wall of the circular tubular connecting section and the inner circumferential wall of the reinforcing sleeve;

[0015] The assembled parts that have completed the above steps are brazed in a furnace.

[0016] According to one embodiment of the present invention, after the reinforcing sleeve is sleeved, the connecting section of the bellows is expanded internally to ensure a tight fit between the two.

[0017] According to one embodiment of the present invention, a flared or flanged limiting portion is processed at the end of the circular tubular connecting section during or after the internal expansion.

[0018] Alternatively, after the internal expansion is completed, a limiting portion is formed radially outward on the inner wall of the circular tubular connecting section in the form of raised dots or ribs;

[0019] Alternatively, after the internal expansion is completed, the limiting portion is formed by welding the circular tubular connecting section and the reinforcement sleeve.

[0020] According to one embodiment of the present invention, when the limiting portion is in a flared or flanging shape, solder is placed on the inner and outer sides of the limiting portion respectively, and the solder located on the inner side penetrates into the weld between the inner circumferential wall of the circular tubular connecting section and the outer circumferential wall of the connecting pipe; the solder located on the outer side penetrates into the weld between the outer circumferential wall of the circular tubular connecting section and the inner circumferential wall of the reinforcement sleeve.

[0021] According to an embodiment of the present invention, the liquidus of the deposited solder is not lower than 950 degrees Celsius.

[0022] According to one embodiment of the present invention, the method for manufacturing a corrugated metal hose based on furnace brazing further includes:

[0023] Place the mesh sleeve over the assembled part after brazing in the furnace;

[0024] Use self-fluxing welding or mechanical connection to fix the mesh sleeve and reinforcement sleeve;

[0025] The outer sleeves are respectively inserted into the two ends of the mesh sleeve and the mesh sleeve is crimped by reducing the diameter.

[0026] According to one embodiment of the present invention, the method for manufacturing a corrugated metal hose based on furnace brazing further includes:

[0027] Place the mesh sleeve over the assembled part after brazing in the furnace;

[0028] Insert outer sleeves into both ends of the net sleeve to cover the two ends of the net sleeve;

[0029] The reinforcement sleeve, mesh sleeve and outer sleeve are connected by argon arc welding or laser welding.

[0030] According to one embodiment of the present invention, a plurality of axially extending drawing lines or knurling patterns are distributed on the outer peripheral wall of one end of the connecting pipe connected to the circular tubular connecting section.

[0031] According to an embodiment of the present invention, the connecting pipe is any one of a quick connector type, a pipe thread type, a flange type or a connecting pipe type.

[0032] According to an embodiment of the present invention, the connecting pipe is a copper pipe or a stainless steel pipe; or, the connecting pipe is a combination of a copper pipe and a stainless steel pipe.

[0033] According to one embodiment of the present invention, the welding insertion depth L between the connecting pipe and the circular tubular connecting section satisfies: 0.2D≤L≤0.7D; wherein D is the outer diameter of the straight section of the upper main body of the connecting pipe.

[0034] In summary, in the corrugated metal hose based on furnace brazing provided by the present invention, the reinforcing sleeve is placed outside the circular tubular connection section of the corrugated tube to support the outer peripheral wall of the circular tubular connection section and limit its deformation space in the radial direction during furnace brazing. The connecting pipe is socketed in the circular tubular connection and inserted into the welding section. The connecting pipe and the reinforcing sleeve clamp the circular tubular connection section from the inside and outside to effectively solve the problem of uneven welding gap caused by deformation of the circular tubular connection section during furnace brazing. By forming a limiting portion on the circular tubular connection section, the limiting portion limits the axial displacement of the reinforcing sleeve relative to the circular tubular connection section in the direction pointing to the port of the circular tubular connection section when the connecting pipe is inserted to achieve the assembly of the connecting pipe. At the same time, the limiting portion effectively isolates the two welds on the inner and outer circumferential walls of the circular tubular connecting section, allowing the solder placed at the two welds to penetrate into the corresponding welds in a directionally controlled manner. This ensures that sufficient solder penetrates and is evenly distributed into the key weld between the inner circumferential wall of the circular tubular connecting section and the outer circumferential wall of the connecting pipe after welding. This effectively solves welding quality issues such as broken welds, flow soldering, and cold welds caused by the random flow of solder due to the connection of multiple welds. In addition, the limiting portion provides space for the solder to be placed stably, providing the basic conditions for the solder to penetrate into the corresponding welds and greatly reducing the difficulty of solder assembly.

[0035] In order to make the above and other objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below with reference to the accompanying drawings for detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] FIG1 and FIG2 are schematic structural diagrams of existing corrugated metal hoses.

[0037] FIG3 is a schematic structural diagram of a corrugated metal hose based on furnace brazing provided by one embodiment of the present invention.

[0038] FIG4 is a schematic diagram showing the assembly of the bellows and the mesh sleeve in FIG3 .

[0039] FIG5 is an enlarged schematic diagram of point C in FIG3 .

[0040] FIG6 is a partial schematic diagram showing the assembly of the reinforcement sleeve and the bellows in FIG3 .

[0041] FIG7 is a schematic diagram showing the force analysis of the circular tubular connection section clamped by the reinforcement sleeve and the pipe.

[0042] FIG8 is a schematic diagram showing the assembly of the corrugated metal hose provided by the present invention by pressing the connecting pipe into the circular tubular connecting section based on furnace brazing.

[0043] FIG9 is a schematic diagram showing the movement direction of the connecting pipe and the reinforcement sleeve when the connecting pipe is pressed in. FIG.

[0044] FIG10 is a schematic diagram showing a structure in which the inner diameter of a circular tubular connecting section is increased by using a conventional axial expansion process.

[0045] FIG11 is a schematic diagram showing a structure of a circular tubular connecting section with radially enlarged inner diameter provided by the present invention.

[0046] 12 , 13 , 14 , 15 and 16 are schematic structural diagrams showing a position limiting portion in another embodiment of the present invention.

[0047] FIG. 17A is a schematic diagram of a pipe connecting structure provided by an embodiment of the present invention.

[0048] 17B , 17C and 17D are schematic diagrams showing a pipe connection of a pipe connection type structure provided by another embodiment of the present invention.

[0049] FIG. 18 is a schematic diagram of a quick connector pipe according to another embodiment of the present invention.

[0050] FIG. 19A is a schematic diagram of a flange-type connecting pipe according to another embodiment of the present invention.

[0051] FIG19B is a schematic structural diagram of FIG19A from another perspective.

[0052] 20A and 20B are schematic diagrams showing a pipe thread type connecting pipe provided in another embodiment of the present invention.

[0053] 21 and 22 are schematic structural diagrams of a corrugated metal hose based on furnace brazing according to another embodiment of the present invention.

[0054] FIG23 is a schematic diagram showing a process for manufacturing a corrugated metal hose based on furnace brazing according to an embodiment of the present invention. DETAILED DESCRIPTION

[0055] Both traditional corrugated metal hoses and improved corrugated metal hoses with turned parts as transition pieces need to be welded by flame brazing. For stainless steel bellows, the welds after flame brazing are very prone to welding problems such as cold welds, broken welds, and secondary welding, which pose welding hazards. For this reason, some people have proposed corrugated metal hoses that can improve the quality of welds by brazing in a furnace or by setting steps on the pipe. For corrugated metal hoses brazed in a furnace, there is a problem that the thin-walled bellows will deform after welding, resulting in uneven welding gaps and welding leakage; and the multiple steps on the pipe result in multiple welds connected, resulting in random solder flow, and thus problems such as cold welds, broken welds, and assembly difficulties in key welds.

[0056] In view of this, the present embodiment provides a corrugated metal hose which is welded using an intensive furnace brazing process, wherein after welding, the thin-walled bellows does not deform, the key welds are full, and the solder is evenly distributed.

[0057] As shown in Figures 3 to 6, the corrugated metal hose based on furnace brazing provided in this embodiment includes a bellows 1, a reinforcement sleeve 2, a pipe 3, a mesh sleeve 4 externally mounted on the bellows 1, and an outer sleeve 5 covering the end of the mesh sleeve 4. The bellows 1 includes a central corrugated section 11 and two circular tubular connecting sections 12 located at both ends of the bellows section 11. Each circular tubular connecting section 12 is formed with a limiting portion 121. The limiting portion 121 limits the axial displacement of the reinforcement sleeve 2 relative to the circular tubular connecting section 12 in the direction of the end of the circular tubular connecting section 12. The two reinforcement sleeves 2 are respectively externally mounted on the two circular tubular connecting sections 12 of the bellows 1. The reinforcement sleeves 2 reinforce the circular tubular connecting sections 12 to form a welding section 10 for welding the pipes. The two pipes 3 are respectively inserted into the two circular tubular connecting sections 12 of the bellows and inserted into the welding section 10. A solder layer 101 is formed between the pipe 3 and the circular tubular connecting section 12.

[0058] Preferably, the welding insertion depth L between the connecting pipe 3 and the circular tubular connecting section 12 satisfies the following conditions: 0.2D ≤ L ≤ 0.7D. D is the outer diameter of the main straight section 30 of the connecting pipe 3. The main straight section 30 refers to the straight section of the connecting pipe 3 not connected to the circular tubular connecting section 12. Setting this welding insertion depth ensures excellent weld strength after welding the connecting pipe 3. However, this invention is not limited to this.

[0059] In this embodiment, the two reinforcement sleeves 2 have the same structure, and both are formed by bending and rolling the liner. However, the present invention does not impose any limitation on this. In other embodiments, the reinforcement sleeve can also be obtained by blanking a circular pipe; if the assembly accuracy of the reinforcement sleeve after direct blanking does not meet the requirements, simple turning can be performed to improve the assembly accuracy of its inner hole. Although this embodiment is described as an example of two reinforcement sleeves with the same structure. However, the present invention does not impose any limitation on this. In other embodiments, the structures of the two reinforcement sleeves can also be different, and both can adopt any of the above forms.

[0060] In this embodiment, the bellows 1 is made of thin-walled stainless steel, the two reinforcing sleeves 2 are also made of stainless steel, and the two connecting pipes 3 are identical in structure and are both stainless steel pipes. However, the present invention is not limited to this. In other embodiments, the structures of the two connecting pipes may differ, and the materials of the two connecting pipes may also vary depending on the connection requirements of the external pipeline. For example, one connecting pipe may be a copper pipe and the other a stainless steel pipe, or a combination of copper and stainless steel pipes; alternatively, both connecting pipes may be copper pipes.

[0061] The processing process of the corrugated metal hose based on furnace brazing provided in this embodiment includes: placing the reinforcement sleeve 2 obtained after bending and rolling or blanking the round pipe on the outer surface of the circular tubular connecting section 12 of the corrugated pipe to form a welding section 10 for welding the pipe (step S10). A limit portion 121 is processed on the circular tubular connecting section 12 to limit the axial displacement of the reinforcement sleeve 2 relative to the circular tubular connecting section 12 in the direction of the port of the circular tubular connecting section 12 (step S20). The welding section 10 is fixed by a tool to press the pipe 3 into the welding section 10 (step S30). The above process steps are used to assemble another reinforcement sleeve 2 and another pipe 3 on the other circular tubular connecting section 12 of the corrugated pipe. Solder is placed at the weld between the inner circumferential wall of the circular tubular connecting section 12 and the outer circumferential wall of the pipe 3 and at the weld between the outer circumferential wall of the circular tubular connecting section 12 and the inner circumferential wall of the reinforcement sleeve 2 (step S40). The assembled parts after the above steps are brazed in a furnace (step S50).

[0062] In the corrugated metal hose based on furnace brazing provided in this embodiment, a reinforcing sleeve 2 is provided on the outside of the circular tubular connection section 12, and the rigidity of the reinforcing sleeve 2 is used to support the thin-walled circular tubular connection section 12 to effectively prevent the circular tubular connection section 12 from deforming during the welding process. Specifically, the thin-walled circular tubular connection section 12 may be deformed due to high temperature and long-term welding during furnace brazing. At this time, as shown in Figure 7, the reinforcing sleeve 2 will generate a supporting force F1 pointing to the inner side of the circular tubular connection section 12 to prevent the peripheral wall of the circular tubular connection section from bulging outward. Similarly, the connecting pipe 3 inserted into the circular tubular connection section 12 will also generate a supporting force F2 pointing outward when the circular tubular connection section 12 is deformed. The opposing supporting forces F1 and F2 clamp the thin-walled circular tubular connecting section 12, effectively preventing it from deforming during furnace brazing. This in turn ensures that the solder penetration gaps on both sides of the circular tubular connecting section 12 (the weld between the inner circumferential wall of the circular tubular connecting section 12 and the outer circumferential wall of the connecting pipe 3, and the weld between the outer circumferential wall of the circular tubular connecting section 12 and the inner circumferential wall of the reinforcing sleeve 2) are evenly distributed. This effectively solves the leakage problem caused by uneven weld gaps caused by deformation of the thin-walled circular tubular connecting section after furnace brazing in existing corrugated metal hoses. In addition, when assembling the circular tubular connecting section 12 and the connecting pipe 3, the insertion of the connecting pipe 3 will also cause the circular tubular connecting section 12 to deform, and the reinforcing sleeve 2 can also support the circular tubular connecting section 12 during this process.

[0063] In this embodiment, the reinforcement sleeve 2, the circular tubular connecting section 12 and the connecting pipe 3 are sequentially sleeved and assembled. Since the corrugated tube 1 is made of thin-walled stainless steel material and has a corrugated section 11, this structure will make it difficult to apply stable pressure in the axial direction to press it into the connecting pipe 3. Therefore, in step S30, the end of the reinforcement sleeve 2 is positioned using a tool to press the connecting pipe 3 into the circular tubular connecting section 12. Based on this positioning method, when the connecting pipe 3 is pressed in the direction indicated by the arrow K in Figures 8 and 9, the reinforcement sleeve 2 at the welding section 10 will move relative to the circular tubular connecting section 12 toward the end of the circular tubular connecting section 12 (i.e., the direction indicated by the arrow K' in Figure 9), causing the reinforcement sleeve 2 to detach from the circular tubular connecting section 12. To address this assembly issue, this embodiment forms a stopper 121 on the circular tubular connecting section 12 to limit the axial displacement of the reinforcing sleeve 2 relative to the circular tubular connecting section 12 in the direction toward the end of the circular tubular connecting section 12 during assembly of the connecting pipe 3, thereby preventing the reinforcing sleeve 2 from detaching during assembly of the connecting pipe 3. The provision of the stopper 121 allows for press-fitting of the connecting pipe 3 without applying force to the corrugated pipe 1, thereby preventing deformation of the corrugated pipe 1 during assembly.

[0064] In addition, as shown in Figures 5 and 6, the limiting portion 121, which is bent, flanged, or raised in the direction of the reinforcement sleeve 2, effectively isolates the weld on the inner wall side of the circular tubular connecting section 12 (the weld between the inner wall of the circular tubular connecting section 12 and the outer wall of the connecting pipe 3) and the weld on the outer wall side (the weld between the outer wall of the circular tubular connecting section 12 and the inner wall of the reinforcement sleeve 2). During welding, it is difficult for the solder between the two welds to flow across the bent, inclined, or arc-shaped raised surface of the limiting portion. That is, the solder placed on the inner wall side of the circular tubular connecting section 12 will only penetrate into the weld between the inner wall of the circular tubular connecting section 12 and the outer wall of the connecting pipe 3; while the solder placed on the outer wall side of the circular tubular connecting section 12 will only penetrate into the weld between the outer wall of the circular tubular connecting section 12 and the inner wall of the reinforcement sleeve 2. The isolation of the limiting portion 121 eliminates the random flow of solder between the two connected welds, allowing the solder to penetrate in a targeted manner into the corresponding welds. This ensures that the solder is evenly distributed within the key weld formed between the inner circumferential wall of the circular tubular connecting section 12 and the outer circumferential wall of the connecting pipe 3, and that the weld is full after welding. This in turn ensures that the welded corrugated metal hose has excellent weld strength and weld sealing. Furthermore, the limiting portion 121, which is bent, flanged, or raised in the direction of the reinforcement sleeve 2, provides space for the placement of the solder. The stable placement of the solder further facilitates the targeted penetration of the solder. Specifically, as shown in Figures 5 and 6, the limiting portion 121 is flared, and its inner and outer sides are formed with accommodating grooves for placing solder. The solder placed in the inner accommodating groove 1211 penetrates into the weld between the inner circumferential wall of the circular tubular connecting section 12 and the outer circumferential wall of the connecting pipe 3 to form a solder layer 101; the solder placed in the outer accommodating groove 1212 penetrates into the weld between the outer circumferential wall of the circular tubular connecting section 12 and the inner circumferential wall of the reinforcement sleeve 2 to form a solder layer 102.

[0065] Furthermore, in order to allow the molten solder to better penetrate into the weld during welding, the corrugated metal hose middle pipe 3 based on furnace brazing provided in this embodiment has a plurality of axially extending drawn wires or knurling 310 distributed on the outer peripheral wall of the part connected to the circular tubular connecting section 12.

[0066] The following will describe in detail the processing steps of the corrugated metal hose based on furnace brazing provided by this embodiment with reference to the accompanying drawings.

[0067] As mentioned above, the assembly of the reinforcement sleeve 2 in step S10 can effectively avoid the problem of uneven welding gap caused by deformation of the thin-walled circular tubular connecting section 12 after brazing in the furnace. Therefore, when assembling the reinforcement sleeve 2, it is hoped that the transition fit between it and the circular tubular connecting section 12 meets the solder penetration requirement. Transition fit refers to the overlap of the inner diameter tolerance band of the reinforcement sleeve 2 and the outer diameter tolerance band of the circular tubular connecting section 12. The two may be a clearance fit or an interference fit, but the gap amount and the interference amount are both very small. The very small gap amount and interference amount limit the deformation space of the circular tubular connecting section 12 so that it is not easy to deform during brazing in the furnace and affect the welding gap between the inner circumferential wall of the circular tubular connecting section 12 and the outer circumferential wall of the pipe 3. However, the thin-walled corrugated pipe 1 has an elliptical shape after processing and the difference between the long and short radii of the ellipse is large, which will bring difficulties to the sleeve assembly of the reinforcement sleeve 2. In addition, as mentioned above, the thin-walled characteristics and the presence of the corrugated section 11 make it difficult to apply stable pressure to the corrugated tube in the axial direction to perform transition fit press-fitting of the reinforcement sleeve 2 .

[0068] To address this technical problem, the furnace brazing-based corrugated metal hose provided in this embodiment employs the following assembly steps in step S10: The corrugated tube connecting section 12 and the reinforcement sleeve 2 are first assembled with clearance; after assembly, the inner diameter of the thin-walled circular tubular connecting section 12 is enlarged through an internal expansion process, thereby achieving a tight fit between the circular tubular connecting section 12 and the reinforcement sleeve 2. Figure 10 illustrates a conventional process for increasing the inner diameter of a pipe by axial expansion. In this process, an expansion punch 100 gradually extends into the circular tubular connecting section 12' along the axial direction of the circular tubular connecting section 12'. The inner wall of the circular tubular connecting section 12' is subjected to axial compression, generating a lateral expansion force that gradually deforms the circumferential wall. This gradually uneven force causes the circular tubular connecting section 12' to crack due to expansion. To this end, this embodiment employs an internal expansion process that applies only radial pressure to the circular tubular connecting section 12 to synchronously expand its inner diameter as a whole. Specifically, as shown in Figure 11, the inner expansion head is first inserted into the tubular connecting section 12 with a clearance fit. Once inserted, the inner expansion head expands to apply radial pressure F11 to the tubular connecting section 12 as a whole, thereby simultaneously expanding its inner diameter. In other words, during expansion, all parts of the tubular connecting section 12 are subjected to the same radial pressure F11, causing them to expand simultaneously. The uniform force applied to the tube wall ensures that the circumferential wall of the tubular connecting section 12 remains intact and crack-free after expansion. Compared to the traditional process of axially expanding the inner diameter of the pipe, the expansion process of applying radial pressure to simultaneously expand the inner diameter as a whole, adopted in this embodiment, not only has a high expansion qualification rate, but also a simple process and high efficiency.

[0069] As shown in Figures 5 and 6, in this embodiment, the limiting portion 121 is a flared section formed at the end of the circular tubular connecting section 12. Therefore, in step S10, the flared limiting portion 121 is machined at the end of the circular tubular connecting section 12 while the circular tubular connecting section 12 is internally expanded. However, the present invention does not impose any restrictions on the specific forming process of the limiting portion. In other embodiments, the limiting portion can be machined in a separate step after the circular tubular connecting section is internally expanded; alternatively, the limiting portion can be machined first after the reinforcing sleeve is sleeved, and then the circular tubular connecting section is internally expanded.

[0070] In addition, the present invention does not impose any restrictions on the shape of the limiting portion. In other embodiments, the shape of the limiting portion may also be a flange section 121 formed at the end of the circular tubular connecting section 12, which may be formed when the circular tubular connecting section is internally expanded or after the internal expansion (as shown in FIG12 ). In other embodiments, after the internal expansion is completed, an outwardly protruding limiting portion 121 may be formed on the outer wall of the circular tubular connecting section 12 in the form of raised dots or ribs radially outward on the inner wall of the circular tubular connecting section. The raised limiting portion 121 may be one or more raised dots distributed on the outer circumferential wall of the circular tubular connecting section (as shown in FIG13 ) or a circumferentially continuous raised ring (as shown in FIG14 and FIG15 ). The raised limiting portion 121 can be formed on the outer peripheral wall of the circular tubular connecting section 12 near its end (as shown in Figures 13 and 14); or it can be formed in the middle area of ​​the outer peripheral wall of the circular tubular connecting section 12 (as shown in Figure 15). In this case, the reinforcing sleeve 2 has a groove 21 that matches the raised limiting portion 121. The limiting portion 121 limits the two side walls of the groove 21 in the axial direction of the corrugated pipe. Alternatively, in other embodiments, the limiting portion 121 is formed by welding the circular tubular connecting section 12 and the reinforcing sleeve 2 after the internal expansion is completed (as shown in Figure 16); the welding method can be any one of argon arc welding, laser welding or resistance welding.

[0071] After the assembly of the reinforcement sleeve 2 and the processing of the limiting portion 121 are completed, step S30 is performed, and the welding section 10 is fixed by the tooling to press the connecting pipe 3 into the welding section 10. As mentioned above, the thin wall of the corrugated tube 1 and the arrangement of the corrugated section 11 thereon make it difficult to apply stable pressure in the axial direction to assemble the connecting pipe 3. Therefore, this embodiment will fix the tooling based on the reinforcement sleeve 2 at the welding section 10. Specifically, the tooling can be clamped to the reinforcement sleeve 2 in the radial direction, and the friction between the tooling and the reinforcement sleeve 2 can realize the positioning of the reinforcement sleeve 2 and the corrugated tube 1 so that the connecting pipe 3 is pressed into the circular tubular connecting section 12. Alternatively, the tooling can also be inserted into the end of the reinforcement sleeve 2 close to one end of the corrugated section 11, and the tooling can be used to position the end of the reinforcement sleeve 2 to press the connecting pipe 3 into the circular tubular connecting section 12. Although the circular tubular connecting section 12 and the reinforcement sleeve 2 are tightly fitted, the axial pressure during insertion of the connecting pipe 3 will still cause relative axial displacement between the circular tubular connecting section 12 and the reinforcement sleeve 2 (as shown in Figures 8 and 9). At this time, the outer peripheral wall of the stopper 121 will prevent the reinforcement sleeve 2 from axially displacing the circular tubular connecting section 12 in the direction toward the end of the circular tubular connecting section 12, thereby maintaining the welded section 10 formed between the two to meet the requirements of the welded connection of the connecting pipe 3.

[0072] At this point, the assembly of the reinforcement sleeve 2 and the connecting pipe 3 on one of the circular tubular connecting sections 12 of the corrugated tube is completed, and the reinforcement sleeve 2 and the connecting pipe 3 are assembled on the other circular tubular connecting section 12 of the corrugated tube 1 using the above-mentioned process steps. In the actual assembly process, the assembly of the same parts will be carried out in the same process steps. Specifically, after the assembly of the reinforcement sleeve 2 on one of the circular tubular connecting sections 12 is completed, the reinforcement sleeve 2 will be assembled on the other circular tubular connecting section 12, and then the connecting pipe 3 will be press-fitted. However, the invention does not impose any limitation on this. In other embodiments, the reinforcement sleeve and the connecting pipe can also be assembled on one of the circular tubular connecting sections separately, and then the reinforcement sleeve and the connecting pipe can be assembled in sequence on the other circular tubular connecting section.

[0073] After the bellows 1, the two reinforcement sleeves 2, and the two connecting pipes 3 are assembled, step S40 is performed, in which solder is placed in the welds between the inner circumferential wall of the circular tubular connecting section 12 and the outer circumferential wall of the connecting pipe 3, and in the welds between the outer circumferential wall of the circular tubular connecting section 12 and the inner circumferential wall of the reinforcing sleeve 2. In this embodiment, as shown in Figures 5 and 6, the stopper 121 is a flared section formed at the end of the circular tubular connecting section 12. An inner accommodating groove 1211 formed between the inner side of the stopper 121 and the connecting pipe 3 connects the welds between the inner circumferential wall of the circular tubular connecting section 12 and the outer circumferential wall of the connecting pipe 3; while an outer accommodating groove 1212 formed between the outer side of the stopper 121 and the end of the reinforcing sleeve 2 connects the welds between the outer circumferential wall of the circular tubular connecting section 12 and the inner circumferential wall of the reinforcing sleeve 2. The stopper 121 isolates the two solder rings located in the accommodating grooves on either side of it, thereby allowing the two solder rings to penetrate into their corresponding welds in a directionally controlled manner to ensure welding quality.

[0074] In other embodiments, although the shape of the limiting portion is different from that of this embodiment, it can still form a receiving groove for accommodating solder on both its inner and outer sides and isolate the solder. As shown in Figure 12, the limiting portion 121 is a flanged section formed at the end of the circular tubular connecting section 12. An inner receiving groove 1211 is formed between the inner surface of the flanged section and the connecting pipe 3, and an outer receiving groove 1212 is formed between the outer surface of the flanged section and the end of the reinforcement sleeve 2. As shown in Figure 14, the limiting portion 12 is a convex ring. The inner groove of the limiting portion 121 (the inner wall groove corresponding to the convex ring) forms an inner receiving groove 1211, and the outer receiving groove 1212 is formed between the outer side of the limiting portion 121 and the end of the reinforcement sleeve 2.

[0075] In other embodiments, if the limiting portion 121 does not form a receiving groove for placing solder, such as the limiting portion 121 shown in FIG13 , which is a protrusion or a soldering point structure as shown in FIG16 , the solder at the weld between the inner circumferential wall of the circular tubular connecting section 12 and the outer circumferential wall of the connecting pipe 3 can be placed on the step formed between the insertion end of the connecting pipe 3 and the inner circumferential wall of the circular tubular connecting section 12. Preferably, a chamfer can be provided at the insertion end of the connecting pipe 3, and an inner groove 1211' is formed between the chamfer and the inner circumferential wall of the circular tubular connecting section 12. The solder at the weld between the outer circumferential wall of the circular tubular connecting section 12 and the inner circumferential wall of the reinforcing sleeve 2 can be placed on the step between the end of the reinforcing sleeve 2 and the outer circumferential wall of the circular tubular connecting section 12. Preferably, a chamfer can be provided at the end of the reinforcing sleeve 2, and an outer groove 1212' is formed between the chamfer and the outer circumferential wall of the circular tubular connecting section 12. At this time, the peripheral wall of the circular tubular connecting section 12 isolates the solder in the inner groove 1211 ′ and the outer groove 1212 ′ to achieve directional penetration of each solder.

[0076] In step S50, the assembled components, after soldering, are placed in a brazing furnace for integrated furnace brazing of the bellows 1, reinforcement sleeve 2, and connecting pipe 3. This furnace brazing can be performed using a mesh belt tunnel furnace, a vacuum brazing furnace, or a gas shielded brazing furnace. Furnace brazing not only provides consistent welding and a clean, bright surface, but also effectively eliminates internal stress in the bellows during brazing, thereby extending the bellows' lifespan and ensuring vibration resistance.

[0077] The existing metal hoses processed by brass flame brazing mostly use brass brazing materials or silver-containing copper-based solders when welding. The liquidus lines of such solders are all below 900 degrees Celsius, so the melting point of the weld formed is relatively low. Taking the copper-zinc solder in the brass brazing material as an example, its liquidus line is 890 degrees Celsius and its welding temperature is 905 degrees Celsius. When the existing corrugated metal hose is flame brazed to connect with the system pipeline, the low-melting-point weld formed on the metal hose during processing will easily produce secondary welding and cause leakage. The liquidus line of the brazing material placed in the corrugated metal hose formed by furnace brazing provided in this embodiment is not lower than 950 degrees Celsius. This setting greatly increases the heat-affected temperature of the weld when the system pipeline is welded to the connecting pipe 3, thereby effectively avoiding the problem of secondary welding of the weld. Specifically, in this embodiment, the bellows 1, the reinforcement sleeve 2, and the connecting pipe 3 are all made of stainless steel. During welding, oxygen-free copper brazing material with a melting point of approximately 1080°C can be used. This temperature is much higher than the temperature (905°C) for flame brazing the connecting pipe 3 and the system piping. The weld formed by the oxygen-free copper brazing material will not be affected by heat and will not produce secondary welding, thus ensuring the performance of the corrugated metal hose after welding to the system piping. In other embodiments, if the connecting pipe 3 is a copper pipe or a combination of a copper pipe and a stainless steel pipe, tin-bronze brazing material with a liquidus above 950°C can be selected for furnace brazing. Similarly, this temperature is much higher than the temperature for flame brazing the connecting pipe 3 and the system piping, and the weld formed by the tin-bronze brazing material will not be affected by heat and will not produce secondary welding.

[0078] In this embodiment, both pipes 3 are of pipe type and have a necking section 311 at one end 31 inserted into the circular tubular connecting section 12 of the corrugated pipe, and knurling 310 is formed on the necking section 311 (as shown in FIG17A ). However, the present invention does not impose any limitation on this. In other embodiments, a wire drawing line 310 'may also be formed on the necking section 311 (as shown in FIG17B ); or, no groove may be formed (as shown in FIG17C ). In other embodiments, the pipe 3 may also be a straight pipe without a necking section at one end 31 inserted into the circular tubular connecting section 12 of the corrugated pipe (as shown in FIG17D ).

[0079] In other embodiments, the connecting pipe 3 may also be a quick connector type, as shown in Figure 18, the connecting pipe 3 includes a ball valve joint 3A, a nut 3B and a ball head slip-on joint seat 3C connected to the external system pipeline, and the end 31 of the ball valve joint 3A close to the bellows 1 is inserted into the circular tubular connecting section 12.

[0080] Alternatively, the connecting pipe 3 may be a flange type as shown in FIG. 19 and FIG. 19A , and the connecting pipe 3 further includes a flange body 3A′ and a flange gasket 3B′ connected to an external system pipeline.

[0081] Alternatively, connecting pipe 3 can be of the pipe thread type shown in Figure 20A or Figure 20B. In Figure 20A, connecting pipe 3 includes a ball valve joint 3A, a nut 3B, and a ball-end slip-on joint seat 3C' for connecting to the external system pipeline. The ball-end slip-on joint seat 3C' has a threaded portion 3D for connection. The end 31 of the ball valve joint 3A, which is adjacent to the bellows 1, is inserted into the circular tubular connecting section 2. In Figure 20B, connecting pipe 3 also has a threaded portion 3D for connecting to the external system pipeline. Furthermore, the connecting pipe can be straight or curved.

[0082] The mesh sleeve is a key component of a corrugated metal hose. It's typically woven from a series of intersecting metal strands or strips of metal, and placed over the outer surface of the bellows at a specified angle, providing both reinforcement and shielding. The mesh sleeve not only distributes the static load of the corrugated metal hose in the axial and radial directions but also ensures safe and reliable operation under the pulsating action of fluid flowing through the pipe. It also protects the corrugated portion of the bellows from direct mechanical damage from friction, impact, and other factors. The strength of a bellows with a mesh sleeve can be increased by dozens of times, and its shielding capacity can reach 99.95%.

[0083] Based on the axial and radial static load requirements that the mesh sleeve needs to bear during operation, the two ends of the mesh sleeve need to be fixed during production. In traditional corrugated metal hoses, the two ends of the mesh sleeve are mainly fixed by direct closing or argon arc welding. The mechanical connection strength of simple closing fixation is low, and the connection strength will gradually decrease with the continuous vibration of the corrugated metal hose, which will cause the two ends of the mesh sleeve to loosen, thereby seriously shortening the service life of the corrugated metal hose. As for argon arc welding fixation, based on the requirements of argon arc welding for the flatness of the welding point, the braided tube wire at the end of the mesh sleeve needs to be cut before welding to make it flush with the outer bushing, and then the bushing, mesh sleeve and outer sleeve are argon arc welded in an integrated manner. This connection method not only takes a long time to weld, but also requires the outer sleeve to be polished to remove the blackened surface after the argon arc welding is completed. Therefore, there are problems such as low welding efficiency, argon gas consumption and complicated welding process.

[0084] In order to solve the problem of low mesh fixing strength or complex fixing process in existing corrugated metal hoses, the corrugated metal hose based on furnace brazing provided in this embodiment also adopts a new mesh fixing method, which not only has high fixing strength but also is very convenient to process. Specifically, the processing steps of the corrugated metal hose based on furnace brazing also include:

[0085] After the bellows 1, the reinforcement sleeve 2 and the connecting pipe 3 are brazed in the furnace, the mesh sleeve 4 is placed over the furnace-brazed assembly (step S60). Specifically, the end of the mesh sleeve 4 completely or partially covers the reinforcement sleeve 2 corresponding to the end.

[0086] Afterwards, the mesh sleeve 4 and the reinforcement sleeve 2 are secured together using autogenous welding or mechanical connection (step S70). In this step, resistance welding can be used to form a circumferential weld in the overlapping region of the mesh sleeve 4 and the reinforcement sleeve 2. However, the present invention is not limited to this. In other embodiments, resistance welding or other autogenous welding methods can also be used to form multiple circumferentially distributed weld spots in the overlapping region of the mesh sleeve and the reinforcement sleeve.

[0087] Finally, outer sleeves 5 are inserted into both ends of the mesh sleeve 4. The outer sleeves 5 are compressed against the mesh sleeve 4 by reducing their diameter. The front end of the outer sleeve 5 has a closing step 51 that bends toward the reinforcement sleeve 2 (step S80), as shown in FIG5 . In other embodiments, a closing section 51' that bends toward the reinforcement sleeve 2 can also be formed at the front end of the outer sleeve 5 (as shown in FIG21 ). The front end of the outer sleeve 5 refers to the end of the outer sleeve 5 that is away from the corrugated section 11.

[0088] In the furnace-brazed corrugated metal hose provided in this embodiment, the mesh sleeve 4 is not furnace-brazed with the bellows 1, reinforcement sleeve 2, and connecting pipe 3. In other words, the mesh sleeve 4 is unaffected by the brazing material, and thus does not suffer from the problem of reduced bending performance caused by the hardening of the brazing material. In addition, the self-fluxing welding or mechanical connection between the mesh sleeve 4 and the reinforcement sleeve 2 has basically fixed the ends of the mesh sleeve 4. The reduced diameter press-fit of the outer sleeve 5 further enhances the connection strength of the mesh sleeve 4 while also covering the ends of the mesh sleeve 4 to prevent the mesh from unraveling.

[0089] In the mesh sleeve 4 fixing structure provided in this embodiment, the outer sleeve 5 does not require welding during the fixed connection, nor does the front mesh wire of the mesh sleeve 4 need to be processed. This not only provides high fixing strength but also simplifies the processing process. Taking a DN25 furnace-brazed corrugated metal hose as an example, the mesh sleeve 4, after being circumferentially welded using resistance welding to form a circumferential weld seam, has a burst pressure of up to 24.6 MPa. For a furnace-brazed corrugated metal hose that uses resistance welding for spot welding for local fixation, the burst pressure can reach 20.2 MPa when the number of weld points reaches 16. Both far exceed the standard burst pressure of 16.6 MPa.

[0090] Although this embodiment illustrates a method in which the outer sleeve 5 is reduced in diameter and press-fitted with the mesh sleeve 4 after self-fluxing welding of the reinforcement sleeve 2 and the mesh sleeve 4, the present invention does not impose any limitations on the method for securing the mesh sleeve. In other embodiments, when the circular tubular connecting section 12, the reinforcement sleeve 2, and the connecting pipe 3 are welded in a three-in-one furnace using the structure provided in this embodiment, and the circular tubular connecting section 12 has a stopper 121, the mesh sleeve 4 can also be press-fitted using the traditional, complex argon arc welding method (as shown in Figure E), as shown in Figure 22.

[0091] In summary, in the corrugated metal hose based on furnace brazing provided by the present invention, the reinforcing sleeve is placed outside the circular tubular connection section of the corrugated tube to support the outer peripheral wall of the circular tubular connection section and limit its deformation space in the radial direction during furnace brazing. The connecting pipe is socketed in the circular tubular connection and inserted into the welding section. The connecting pipe and the reinforcing sleeve clamp the circular tubular connection section from the inside and outside to effectively solve the problem of uneven welding gap caused by deformation of the circular tubular connection section during furnace brazing. By forming a limiting portion on the circular tubular connection section, the limiting portion limits the axial displacement of the reinforcing sleeve relative to the circular tubular connection section in the direction pointing to the port of the circular tubular connection section when the connecting pipe is inserted to achieve the assembly of the connecting pipe. At the same time, the limiting portion effectively isolates the two welds on the inner and outer circumferential walls of the circular tubular connecting section, allowing the solder placed at the two welds to penetrate into the corresponding welds in a directionally controlled manner. This ensures that sufficient solder penetrates and is evenly distributed into the key weld between the inner circumferential wall of the circular tubular connecting section and the outer circumferential wall of the connecting pipe after welding. This effectively solves welding quality issues such as broken welds, flow soldering, and cold welds caused by the random flow of solder due to the connection of multiple welds. In addition, the limiting portion provides space for the solder to be placed stably, providing the basic conditions for the solder to penetrate into the corresponding welds and greatly reducing the difficulty of solder assembly.

[0092] Although the present invention has been disclosed above by means of preferred embodiments, this is not intended to limit the present invention. Anyone skilled in the art may make slight changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the scope of protection required by the claims.

Claims

1. A corrugated metal hose based on furnace brazing, characterized in that: The corrugated metal hose comprises a corrugated tube, a reinforcement sleeve, a connecting pipe, a mesh sleeve disposed on the corrugated tube, and an outer sleeve covering the end of the mesh sleeve; the corrugated tube comprises a middle corrugated section and two circular tubular connecting sections located at both ends of the corrugated section, and a limited position portion is formed on each circular tubular connecting section; The manufacturing method of the corrugated metal hose based on furnace brazing comprises the following steps: The reinforcing sleeve is placed outside the circular tubular connecting section of the corrugated pipe to form a welding section for welding the connecting pipe; A limiting portion is machined on the circular tubular connecting section to limit the axial displacement of the reinforcement sleeve relative to the circular tubular connecting section in a direction pointing to the port of the circular tubular connecting section; Fixing the welding section by a tool to press the pipe into the welding section; Using the above process steps, a reinforcement sleeve and a connecting pipe are assembled on another circular tubular connecting section of the corrugated pipe; Placing solder at the weld between the inner circumferential wall of the circular tubular connecting section and the outer circumferential wall of the connecting pipe and at the weld between the outer circumferential wall of the circular tubular connecting section and the inner circumferential wall of the reinforcing sleeve; The assembled parts that have completed the above steps are brazed in a furnace.

2. The corrugated metal hose based on furnace brazing according to claim 1, characterized in that: After the reinforcing sleeve is sleeved, the connecting section of the bellows is expanded internally to make the two fit tightly.

3. The corrugated metal hose based on furnace brazing according to claim 2, characterized in that: During or after the internal expansion, a flared or flanged limiting portion is processed at the end of the circular tubular connecting section; Alternatively, after the internal expansion is completed, a limiting portion is formed radially outwardly on the inner wall of the circular tubular connecting section in the form of convex points or convex ribs; Alternatively, after the internal expansion is completed, the limiting portion is formed by welding the circular tubular connecting section and the reinforcement sleeve.

4. The corrugated metal hose based on furnace brazing according to claim 1 or 3, characterized in that: When the limiting portion is in a flared or flanged shape, solder is placed on the inner and outer sides of the limiting portion respectively, and the solder on the inner side penetrates into the weld between the inner circumferential wall of the circular tubular connecting section and the outer circumferential wall of the connecting pipe; the solder on the outer side penetrates into the weld between the outer circumferential wall of the circular tubular connecting section and the inner circumferential wall of the reinforcing sleeve.

5. The corrugated metal hose based on furnace brazing according to claim 1, characterized in that: The liquidus of the solder placed is not less than 950 degrees Celsius.

6. The corrugated metal hose based on furnace brazing according to claim 1, characterized in that: The method for manufacturing the corrugated metal hose based on furnace brazing also includes: Put the mesh sleeve over the assembled part after brazing in the furnace; The mesh sleeve and the reinforcement sleeve are fixed by self-melting welding or mechanical connection; The outer sleeves are respectively inserted into the two ends of the mesh sleeve and the mesh sleeve is crimped by reducing the diameter.

7. The corrugated metal hose based on furnace brazing according to claim 1, characterized in that: The manufacturing method of the corrugated metal hose based on furnace brazing also includes: Put the mesh sleeve over the assembled part after brazing in the furnace; Insert outer sleeves at both ends of the mesh sleeve to cover the two ends of the mesh sleeve; The reinforcement sleeve, mesh sleeve and outer sleeve are connected by argon arc welding or laser welding.

8. The corrugated metal hose based on furnace brazing according to claim 1, characterized in that: A plurality of drawing lines or knurling patterns extending in the axial direction are distributed on the outer peripheral wall of one end of the connecting pipe connected to the circular tubular connecting section.

9. The corrugated metal hose based on furnace brazing according to claim 1, characterized in that: The connecting pipe is any one of a quick connector type, a pipe thread type, a flange type or a connecting pipe type.

10. The furnace brazing based corrugated metal hose according to claim 1, characterized in that: The connecting pipe is a copper pipe or a stainless steel pipe; or, the connecting pipe is a combination of a copper pipe and a stainless steel pipe.

11. The furnace brazing based corrugated metal hose according to claim 1, characterized in that: The welding insertion depth L between the connecting pipe and the circular tubular connecting section satisfies: 0.2D≤L≤0.7D; wherein D is the outer diameter of the straight section of the main body on the connecting pipe.

Citation Information

Patent Citations

  • Shock insulation pipe for refrigerant transmission

    CN108167557A

  • Corrugated flexible metal pipe's welded structure for locomotive

    CN207112170U

  • High-precision metal hose

    CN217177754U

  • Metal hose and air conditioning system

    CN218883236U

  • Vibration absorbing pipe device

    JP2002195474A