Modified solid-state electrolyte and preparation method therefor, solid-state battery, and electric device
By introducing phase change toughener to the solid electrolytes distributed along the grain boundary, the fragility and dendrite problems of traditional solid electrolytes are solved, the toughness and conductivity of solid-state batteries are improved, and their application performance is enhanced.
Patent Information
- Application Number
- PCT/CN2023/132662
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2023-11-20
- Publication Date
- 2024-11-07
AI Technical Summary
Traditional solid electrolytes have fragile ceramic properties and are prone to cracking. Especially when they are combined with lithium metal negative electrodes, the formation of dendrites leads to short-circuiting and failure of solid-state batteries, making it difficult to meet the practical application needs.
By distributing phase change toughening agents in solid electrolyte substrates, they are mainly distributed along the grain boundaries. The phase change toughening agents generate stress transitions under external force stimulation, improving the mechanical strength and toughness of solid electrolytes. Avoid internal defects and dendrites growth.
It improves the toughness and ionic conductivity of solid electrolytes, reduces the risk of dendrites piercing the electrodes, and enhances the efficiency and reliability of solid-state batteries.
Smart Images

Figure CN2023132662_07112024_PF_FP_ABST
Abstract
Description
Modified solid electrolyte and preparation method thereof, solid-state battery and electrical device
[0001] Cross-references
[0002] This application refers to Chinese patent application No. 202310484801.9 filed on May 4, 2023, entitled “Modified solid electrolyte, preparation method thereof, solid-state battery and electrical device”, which is incorporated into this application in its entirety by reference. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to a modified solid electrolyte and a preparation method thereof, a solid-state battery and an electrical device. Background Art
[0004] In recent years, solid-state batteries prepared with solid-state electrolytes have received increasing attention. On the one hand, solid-state batteries can avoid the flammable and explosive problems of liquid batteries due to the presence of organic electrolytes. Solid-state batteries can use metals as negative electrode materials, which can reduce the probability of side reactions occurring at high temperatures. Therefore, safety is considered to be one of the most fundamental driving forces for the development of solid-state batteries. Solid-state electrolytes give solid-state batteries the characteristics of compact structure, adjustable scale, and great design flexibility. They can be used to drive microelectronic devices, as well as in the fields of power and energy storage.
[0005] Traditional solid-state electrolytes often have the fragile characteristics of ceramics, with poor mechanical strength and easy cracking. They are prone to cracking during use, especially when used with lithium metal negative electrodes. Lithium metal will form dendrites at the solid-state electrolyte interface. The formation of dendrites will cause the solid-state electrolyte to break and even penetrate the solid-state electrolyte, causing short circuits and failure of solid-state batteries, making it difficult to meet actual application needs.
[0006] Therefore, traditional technologies still need to be improved.
[0007] Summary of the Invention
[0008] According to various embodiments of the present application, the present application provides a modified solid electrolyte and a preparation method thereof, a solid-state battery and an electrical device, aiming to improve the toughness of the solid-state electrolyte and thereby improve the efficiency of the solid-state battery.
[0009] This application is achieved through the following technical solutions.
[0010] In a first aspect of the present application, a modified solid electrolyte is provided, comprising a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate; wherein in the modified solid electrolyte, the phase change toughening agent is mainly distributed at the grain boundaries in the solid electrolyte;
[0011] The phase change toughening agent can undergo phase change under the action of external force.
[0012] The above-mentioned modified solid electrolyte includes a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate. When subjected to external force, stress will be generated accordingly inside the phase change toughening agent. Under the stimulation of stress, the phase change toughening agent will undergo a phase change. The stress transformation brought about by this phase change process can improve the mechanical strength and toughness of the solid electrolyte substrate. The phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. In this way, the generation of internal defects of the solid electrolyte can be avoided more accurately, and the toughness can be further improved.
[0013] In some embodiments, among the total number of particles of the phase change toughening agent in the modified solid electrolyte, the number of particles of the phase change toughening agent distributed at the grain boundaries in the solid electrolyte accounts for ≥50%.
[0014] In some embodiments, in the same cross section of the modified solid electrolyte, the total number of particles of the phase change toughening agent is N1, and the number of particles of the phase change toughening agent distributed at the grain boundaries in the same cross section is N2, then the orientation degree of the phase change toughening agent distributed along the grain boundaries is A=N2 / N1×100%, and A satisfies: A≥50%;
[0015] Optionally, A satisfies: 50%<A≤100%;
[0016] Optionally, A satisfies: 50%<A<100%.
[0017] In the above-mentioned modified solid electrolyte, on the same cross-section, the orientation degree H of the phase change toughening agent along the grain boundary is ≥50%, which can be regarded as that in the modified solid electrolyte, the phase change toughening agent is mainly distributed along the grain boundary in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. Therefore, the phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte, which can more accurately avoid the generation of internal defects in the solid electrolyte and further improve the toughness.
[0018] In some embodiments, the same cross section is a cross section or a longitudinal section of the modified solid electrolyte.
[0019] Specifically, a cross section is a section formed by cutting perpendicular to the height or thickness direction, and a longitudinal section is a section formed by cutting parallel to the height or thickness direction. For example, a cylinder's cross section is a section formed by cutting perpendicular to the height direction, which is a circle, and its longitudinal section is a section formed by cutting parallel to the height direction, which is a rectangle. The height of a cylinder can also be called its thickness. If the height of the cylinder is relatively low, for example, the height is less than the diameter of the ground, then the cylinder is a disc, in which case the height is usually called the thickness.
[0020] In some embodiments, the step of testing the orientation degree A comprises:
[0021] Taking the sample to be tested of the modified solid electrolyte, cutting the sample to be tested along a direction perpendicular to the thickness of the wafer, and the cut cross section formed when cutting the sample to be tested is the cross section to be tested;
[0022] An X-ray energy spectrometer is used to mark the key elements contained in the phase change toughening agent in the cross section to be measured so that the key elements emit signal points, and a scanning electron microscope image of the cross section to be measured is obtained:
[0023] Obtaining a total number M1 of the signal points in the scanning electron microscope image and a number M2 of the signal points contained in the grain boundaries in the scanning electron microscope image;
[0024] According to M1 and M2, we get A;
[0025] Specifically, A=M2 / M1×100%.
[0026] The key element is an element contained in the phase change toughening agent but not contained in the solid electrolyte substrate.
[0027] In some embodiments, the phase change toughening agent contains zirconium oxide, and the key element is zirconium.
[0028] In some embodiments, the phase change toughening agent further contains a stabilizer, and the mass proportion of the stabilizer in the phase change toughening agent is 0.01% to 50%;
[0029] Optionally, the stabilizer contains at least one element selected from the group consisting of yttrium, scandium, magnesium, calcium, and cesium;
[0030] Optionally, the stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide;
[0031] Optionally, the stabilizer comprises yttrium oxide.
[0032] Although the specific toughening mechanism of phase change toughening agents remains to be studied, technicians speculate as follows: Phase change toughening agents have a metastable state, that is, the phase change toughening agents exist in a high-temperature stable crystal structure at room temperature. This allows the phase change toughening material to undergo a phase change and volume change when stimulated by external forces, thereby inhibiting the fracture of the solid electrolyte and playing a phase change toughening role. For example, when pure ZrO2 is cooled from high temperature to room temperature, it will generally undergo the following phase transitions: cubic phase (c), tetragonal phase (t) to monoclinic phase (m), of which the t to m phase transition occurs at around 1150°C, accompanied by a volume change of about 5%. If the t and m phase transition points of ZrO2 are stabilized at room temperature, it can produce a tm phase transition when induced by external stress at room temperature. Due to the volume effect generated by the phase transition, a large amount of fracture energy is absorbed, resulting in the material exhibiting an abnormally high fracture toughness, achieving the effect of phase change toughening.
[0033] In some embodiments, in the modified solid electrolyte, the mass proportion of the phase change toughening agent is 2% to 25%;
[0034] Optionally, the mass proportion of the phase change toughening agent is 5% to 25%;
[0035] Optionally, the mass proportion of the phase change toughening agent is 10% to 25%;
[0036] Optionally, the mass proportion of the phase change toughening agent is 15% to 25%.
[0037] The mass proportion of the phase change toughening agent is regulated to further improve the toughness of the modified solid electrolyte.
[0038] In some embodiments, in the modified solid electrolyte, the mass of the solid electrolyte substrate is m1 and the theoretical density is ρ1, the mass of the phase change toughening agent is m2 and the theoretical density is ρ2, then the theoretical volume Vt of the modified solid electrolyte satisfies: Vt = [m1 / ρ1] + [m2 / ρ2];
[0039] The actual volume of the modified solid electrolyte is Vr, and the density of the modified solid electrolyte is K=Vt / Vr×100%;
[0040] Optionally, K satisfies: K≥70%; optionally, K satisfies: 90%≤K≤100%.
[0041] It can be understood that the theoretical density ρ1 and the theoretical density ρ2 are the densities of the pure solid electrolyte substrate and the pure phase change toughening agent respectively. It can also be understood as the density of the solid electrolyte substrate raw material and the phase change toughening agent raw material used in the preparation. Then Vt represents the volume of the modified solid electrolyte. The larger the K value, the greater the difference between its actual volume and the theoretical volume, which means that the actual distribution inside the modified solid electrolyte is more compact and dense. The above-mentioned modified solid electrolyte has a high density. When used in the preparation of solid-state batteries, it can reduce the defects and pores on the surface of the electrolyte sheet / membrane and can further improve the ionic conductivity of the modified solid electrolyte.
[0042] In some embodiments, the solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.
[0043] In a second aspect of the present application, a method for preparing a modified solid electrolyte is provided, comprising the following steps:
[0044] mixing a solid electrolyte substrate and a phase change toughening agent to prepare a mixture;
[0045] The mixture is sintered under a protective gas atmosphere to prepare the modified solid electrolyte.
[0046] In the above preparation method, during the sintering period, the grains of the mixture grow and the grain boundaries fuse with each other. At the same time, the phase change toughening agent, which originally tends to be evenly distributed in the mixture, enters the grain boundary area under the promotion of grain growth and is distributed along the grain boundary orientation.
[0047] Furthermore, under the action of grain growth and grain boundary fusion, the defects and pores of the modified solid electrolyte are greatly reduced, and the density is improved.
[0048] In some embodiments, the sintering process satisfies at least one of the following conditions (1) to (2):
[0049] (1) The sintering temperature is 90°C to 600°C, and the sintering time is 10 minutes to 120 hours;
[0050] By regulating the temperature and time of the sintering treatment, the phase change toughening agent is further promoted to enter the grain boundary area under the promotion of grain growth, and the structural stability of the solid electrolyte substrate and the phase change toughening agent is ensured.
[0051] (2) The protective gas atmosphere is formed by filling a protective gas, wherein the protective gas includes at least one of an inert gas and nitrogen;
[0052] Optionally, the protective gas comprises helium;
[0053] Optionally, the water content in the protective gas is less than 0.1 ppm, and the oxygen content is less than 0.1 ppm.
[0054] In some embodiments, after the sintering process, the method further comprises the step of pressing the product obtained by the sintering process;
[0055] Optionally, the pressure T1 used in the pressing step satisfies: T1≤400 MPa;
[0056] Optionally, T1 satisfies: 400 MPa≤T1≤600 MPa.
[0057] In some embodiments, the mixing step adopts dry mixing, and before the mixture is sintered, the following steps are further included:
[0058] Pressing the mixture into a sheet-like mixture; optionally, the thickness of the sheet-like mixture is 200 μm to 2 mm; optionally, the pressure used when pressing the mixture into the sheet-like mixture is 400 MPa to 600 MPa; or
[0059] The mixing step adopts wet mixing, and before the mixture is sintered, the following steps are also included:
[0060] The mixture is coated and dried to form a film-like mixture; optionally, the thickness of the film-like mixture is 10 μm to 200 μm.
[0061] In a third aspect of the present application, a solid-state battery is provided, comprising the modified solid-state electrolyte of the first aspect or the modified solid-state electrolyte prepared by the preparation method of the modified solid-state electrolyte of the second aspect.
[0062] In a fourth aspect of the present application, an electrical device is provided, comprising the solid-state battery of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive work. In the drawings:
[0064] FIG1 is a schematic diagram of a solid-state battery according to one embodiment;
[0065] FIG2 is a schematic diagram of an embodiment of a battery pack;
[0066] FIG3 is an exploded view of FIG2 ;
[0067] FIG4 is a schematic diagram of an embodiment of an electrical device using a solid-state battery as a power source;
[0068] FIG5 is an electron microscope image of a cross section of the modified solid electrolyte prepared in Example 1.
[0069] Figure numerals: 1. battery pack; 2. upper box; 3. lower box; 4. solid-state battery; 5. electrical device. DETAILED DESCRIPTION
[0070] To make the above-mentioned objects, features, and advantages of the present application more clearly understood, the specific embodiments of the present application are described in detail below. The following description sets forth many specific details to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the scope of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0071] In this application, unless otherwise specified or limited, the terms "installed," "connected," "connect," "fixed," etc. should be understood in a broad sense. For example, they can refer to fixed connection, detachable connection, or integration; mechanical connection or electrical connection; direct connection or indirect connection through an intermediate medium; internal communication between two elements or interaction between two elements, unless otherwise specified. Those skilled in the art will understand the specific meanings of the above terms in this application based on specific circumstances.
[0072] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of such features. Throughout the description of this application, "plurality" means at least two, for example, two, three, etc., unless otherwise specifically defined.
[0073] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0074] Given the aforementioned background, traditional solid-state electrolytes often share the fragile characteristics of ceramics. Traditionally, researchers have focused on developing new solid-state electrolytes or improving solid-state battery structures, but to date, no significant breakthroughs or progress have been achieved.
[0075] The technical personnel of this application have found that the contact interface formed when crystals with different orientations in the solid electrolyte contact each other, namely the grain boundary, is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and is also the area where dendrites are most likely to grow and spread.
[0076] Based on this, the technical personnel of this application, after a lot of creative exploration, obtained the modified solid electrolyte with excellent toughness in this application.
[0077] One embodiment of the present application provides a modified solid electrolyte, which includes a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate, and in the modified solid electrolyte, the phase change toughening agent is mainly distributed at the grain boundaries in the modified solid electrolyte.
[0078] Phase change toughening agents can undergo phase change under the action of external forces.
[0079] The above-mentioned modified solid electrolyte includes a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate. When stimulated by external force, tensile stress is generated inside. Under the stimulation of tensile stress, the phase change toughening agent will undergo a phase change. The stress transformation brought about by this phase change process can improve the mechanical strength and toughness of the solid electrolyte substrate. The phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. In this way, the generation of internal defects in the solid electrolyte can be avoided more accurately and the toughness can be improved.
[0080] It can be understood that the external force in the above-mentioned "phase change toughening agent will undergo phase change under the action of external force" refers to the effect exerted on the phase change toughening agent by the external environment outside the phase change toughening agent itself. Furthermore, when the external force acts on the phase change toughening agent, it causes the phase change toughening agent to deform, and the various parts within the phase change toughening agent then generate interacting internal forces to resist the action of the external force and attempt to restore the phase change toughening agent from the deformed position to the position before deformation. This internal force is stress. Driven by the stress, a phase change will occur inside the phase change toughening agent, and a large amount of fracture energy will be absorbed due to the volume change caused by the phase change, thereby achieving the effect of phase change toughening.
[0081] It can be understood that the grain boundary is the interface between grains with the same structure but different orientations. At the crystal interface, the atomic arrangement transitions from one orientation to another, so the atomic arrangement at the grain boundary is in a transitional state. When observed under the bright field of a scanning electron microscope (SEM), the grain boundary can be seen to be dark and black.
[0082] In some embodiments, among the total number of phase change toughening agent particles in the modified solid electrolyte, the number of phase change toughening agent particles distributed at the grain boundaries in the solid electrolyte accounts for ≥50%.
[0083] In some embodiments, in the same cross section of the modified solid electrolyte, the total number of phase change toughening agent particles is N1, and the number of phase change toughening agent particles distributed at the grain boundaries in the same cross section is N2, then the orientation degree of the phase change toughening agent distributed along the grain boundaries is A=N2 / N1×100%, and A satisfies: A≥50%;
[0084] Optionally, A satisfies: 50%<A≤100%;
[0085] Optionally, A satisfies: 50%<A<100%.
[0086] In the above-mentioned modified solid electrolyte, on the same cross-section, the orientation degree A of the phase change toughening agent along the grain boundary is ≥50%, which can be regarded as that in the modified solid electrolyte, the phase change toughening agent is mainly distributed along the grain boundary in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. Therefore, the phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte, which can more accurately avoid the generation of internal defects in the solid electrolyte and further improve the toughness.
[0087] It can be understood that the distribution of the phase change toughening agent on the plane can reflect the distribution of the phase change toughening agent in the overall modified fixed electrolyte.
[0088] In the above “50%<A≤100%”, the value of A includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 51%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99%, 100%; or a range consisting of any two values, for example, 51%~99%, 55%~99%, 60%~99%, 65%~99%, 70%~99%, 75%~99%, 80%~99%, 51%~95%, 55%~95%, 60%~95%, 65%~95%, 70%~95%, 75%~ 95%, 80%-95%, 51%-90%, 55%-90%, 60%-90%, 65%-90%, 70%-90%, 75%-90%, 80%-90%, 51%-85%, 55%-85%, 60%-85%, 65%-85%, 70%-85%, 75%-85%, 80%-85%, 51%-80%, 55%-80%, 60%-80%, 65%-80%, 70%-80%, 75%-80%, 51%-75%, 55%-75%, 60%-75%, 65%-75%, 70%-75%, 51%-70%, 55%-70%, 60%-70%, 65%-70%.
[0089] In some embodiments, the same cross section is a cross section or a longitudinal section of the modified solid electrolyte.
[0090] Specifically, a cross section is a section formed by cutting perpendicular to the height or thickness direction, and a longitudinal section is a section formed by cutting parallel to the height or thickness direction. For example, a cylinder's cross section is a section formed by cutting perpendicular to the height direction, which is a circle, and its longitudinal section is a section formed by cutting parallel to the height direction, which is a rectangle. The height of a cylinder can also be called its thickness. If the height of the cylinder is relatively low, for example, the height is less than the diameter of the ground, then the cylinder is a disc, in which case the height is usually called the thickness.
[0091] Optionally, the same cross section is a cross section of the modified solid electrolyte. Further optionally, the modified solid electrolyte is a cylinder.
[0092] In some embodiments, the steps for testing the orientation degree A include:
[0093] Taking the modified solid electrolyte disc, cutting the disc along a direction perpendicular to the thickness of the disc, and the cut section formed when cutting the disc is the cross section to be measured;
[0094] An X-ray spectrometer is used to mark key elements contained in the phase change toughening agent in the cross section to be measured, so that the key elements emit signal points, and a scanning electron microscope image of the cross section to be measured is obtained: wherein the key elements are elements contained in the phase change toughening agent but not in the solid electrolyte substrate;
[0095] Obtaining the total number M1 of signal points in the scanning electron microscope image and the number M2 of signal points contained in the grain boundaries in the scanning electron microscope image;
[0096] According to M1 and M2, we get A.
[0097] Specifically, A=M2 / M1×100%.
[0098] It can be understood that the total number of signal points emitted by the key elements in the scanning electron microscope image can be regarded as the total number of particles of the phase change toughening agent in the cross section to be measured;
[0099] The number of signal points emitted by the key elements contained in the grain boundaries in the scanning electron microscope image is counted, which can be regarded as the number N2 of phase change toughening agent particles distributed at the grain boundaries in the cross section to be measured.
[0100] Specifically, in the electron microscope energy spectrum (SEM-EDS) analysis, the electron microscope is equipped with an EDS probe. Taking Zr as an example, the key element, the Zr signal comes from the EDS probe of the SEM. Its mechanism of action is to emit electrons, excite the surface material, and then detect the characteristic X-ray radiation. Therefore, the scanning electron microscope image is divided into 1μm squares. The number of Zr element signal points output by EDS in the squares is regarded as the number of particles of the phase change toughening agent.
[0101] Specifically, an accelerating voltage of 10 kV was used for EDS scanning, and the EDS probe was an Oxford Instrument AZtechOne.
[0102] Optionally, the thickness of the wafer is 200 μm to 2 mm.
[0103] In some embodiments, when the wafer is cut perpendicular to the thickness of the wafer, the cutting point is located at 1 / 2 of the thickness of the wafer.
[0104] In some embodiments, the magnification of the scanning electron microscope image is 1k to 5k.
[0105] In some embodiments, the area of the measured cross section is grid-divided into n unit grid areas, where n is an integer ≥ 2; each unit grid area is placed under a scanning electron microscope for observation to form a scanning electron microscope image, and then the total number of signal points emitted by the key elements in the scanning electron microscope image of each grid area and the number of signal points emitted by the key elements at the grain boundaries in the grid area are counted, and the orientation degree An corresponding to each grid area is calculated, and then the average value is taken to obtain the orientation degree A in the measured cross section: A = (A1+....+An) / n.
[0106] In some embodiments, n satisfies: 3≤n≤10, and n is an integer.
[0107] In some embodiments, n=5.
[0108] When n=5, the grid is divided into five grid units by referring to the five-point sampling method: that is, the midpoint of the diagonal is first determined as the central sampling point grid, and then four grid units with equal distances from the central sampling point grid are selected on the diagonal.
[0109] Furthermore, when the cross section to be measured is placed under a scanning electron microscope for observation, the placement position of the cross section to be measured can be changed multiple times to perform the above steps to obtain the orientation degrees of multiple areas of the cross section to be measured, and then the average value of the orientation degrees of multiple areas is calculated, which is regarded as the orientation degree of the phase change toughening agent distributed along the grain boundary in the cross section to be measured.
[0110] In some embodiments, the phase change toughening agent contains zirconium oxide, with zirconium being the key element.
[0111] In some embodiments, the phase change toughening agent further contains a stabilizer, and the mass proportion of the stabilizer in the phase change toughening agent is 0.1% to 50%;
[0112] Optionally, the stabilizer contains at least one element selected from the group consisting of yttrium, scandium, magnesium, calcium, and cesium.
[0113] In some embodiments, the stabilizer component includes an oxide.
[0114] Optionally, the stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide.
[0115] When the stabilizers are yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide, the toughening agents are recorded as YSZ, SSZ, MSZ, CSZ, and CsSZ, respectively.
[0116] Optionally, the stabilizer comprises yttrium oxide.
[0117] Although the specific toughening mechanism of phase change toughening agents remains to be studied, technicians speculate as follows: Phase change toughening agents have a metastable state, that is, the phase change toughening agents exist in a high-temperature stable crystal structure at room temperature. This allows the phase change toughening material to undergo a phase change and volume change when stimulated by external forces, thereby inhibiting the fracture of the solid electrolyte and playing a phase change toughening role. For example, when pure ZrO2 is cooled from high temperature to room temperature, it will generally undergo the following phase transitions: cubic phase (c), tetragonal phase (t) to monoclinic phase (m), of which the t to m phase transition occurs at around 1150°C, accompanied by a volume change of about 5%. If the t and m phase transition points of ZrO2 are stabilized at room temperature, it can produce a tm phase transition when induced by external stress at room temperature. Due to the volume effect generated by the phase transition, a large amount of fracture energy is absorbed, resulting in the material exhibiting an abnormally high fracture toughness, achieving the effect of phase change toughening.
[0118] In the above “0.01% to 50%”, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include, but are not limited to, the point values in the embodiments and the following point values: 0.01%, 0.05%, 0.1%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%; or a range consisting of any two values, for example, 1% to 50%, 5% to 50%, 10% to 50%, 15% to 50%, 20% to 50%, 25% to 50%, 30% to 50%, 35% to 50%, 40% to 50%, 45% to 50%, 1% to 45%, 5% to 45%, 10% to 50%, 15% to 50%, 20% to 50%, 25% to 50%, 30% to 50%, 35% to 50%, 40% to 50%, 45% to 50%, %~45%, 15%~45%, 20%~45%, 25%~45%, 30%~45%, 35%~45%, 40%~45%, 1%~40%, 5%~40%, 10%~40%, 15%~40%, 20%~40%, 25%~40%, 30%~40%, 35%~40%, 1%~35%, 5%~35%, 10%~35%, 15%~35%, 20%~35%, 25%~35%, 30%~35%, 1%~30%, 5%~30%, 10%~30%, 15%~30%, 20%~30%, 1%~25%, 5%~25%, 10%~25%, 15%~25%, 20%~25%.
[0119] In some embodiments, in the modified solid electrolyte, the mass proportion of the phase change toughening agent is 2% to 25%;
[0120] In some embodiments, the mass proportion of the phase change toughening agent is 5% to 25%;
[0121] In some embodiments, the mass proportion of the phase change toughening agent is 10% to 25%;
[0122] In some embodiments, the mass proportion of the phase change toughening agent is 15% to 25%.
[0123] The mass proportion of the phase change toughening agent is regulated to further improve the toughness of the modified solid electrolyte.
[0124] In the above-mentioned "2% to 25%", the values include the minimum and maximum values of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and the following point values: 2%, 5%, 10%, 15%, 20%, 25%; or a range consisting of any two numerical values, for example, it can be 2% to 5%, 2% to 10%, 2% to 15%, 2% to 20%, 2% to 25%, 5% to 10%, 5% to 15%, 5% to 20%, 5% to 25%, 10% to 15%, 10% to 20%, 10% to 25%, 15% to 20%, 15% to 25%, 20% to 25%.
[0125] In some embodiments, in the modified solid electrolyte, the mass of the solid electrolyte substrate is M1, the theoretical density is ρ1, the mass of the phase change toughening agent is M2, and the theoretical density is ρ2, then the theoretical volume Vt of the modified solid electrolyte satisfies: Vt = [M1 / ρ1] + [M2 / ρ2];
[0126] The actual volume of the modified solid electrolyte is Vr, then the density of the modified solid electrolyte is K = Vt / Vr × 100%;
[0127] Optionally, K satisfies: K≥70%; optionally, K satisfies: 90%≤K≤100%.
[0128] It can be understood that the theoretical density ρ1 and the theoretical density ρ2 are the densities of the pure solid electrolyte substrate and the pure phase change toughening agent respectively. It can also be understood as the density of the solid electrolyte substrate raw material and the phase change toughening agent raw material used in the preparation. Then Vt represents the volume of the modified solid electrolyte. The larger the K value, the greater the difference between its actual volume and the theoretical volume, which means that the actual distribution inside the modified solid electrolyte is more compact and dense. The above-mentioned modified solid electrolyte has a high density. When used in the preparation of solid-state batteries, it can reduce the defects and pores on the surface of the electrolyte sheet / membrane and can further improve the ionic conductivity of the modified solid electrolyte.
[0129] In some embodiments, the actual volume Vr of the modified solid electrolyte is obtained by measuring the actual modified solid electrolyte using the Archimedean method or a micrometer.
[0130] In some embodiments, the solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.
[0131] The above-mentioned lithium ion solid electrolyte, sodium ion solid electrolyte and potassium ion solid electrolyte can be various lithium ion solid electrolytes, sodium ion solid electrolytes and potassium ion solid electrolytes commonly used in the art.
[0132] In some embodiments, the solid electrolyte substrate is a lithium-ion solid electrolyte.
[0133] Examples of lithium-ion solid electrolytes are provided here, including but not limited to:
[0134] LISICON type: such as γ-Li3PO4, etc.;
[0135] NASICON type; such as Li (1+x1) Q x M (2-x1) (PO4)3, 0≤x1<1, Q includes at least one of Al, Cr, Ba, Fe, Sc, In, Lu, Y, and La;
[0136] Garnet type; for example, Li (7-x2) La3Zr (2-x2) M x2 O 12 etc., 0≤x2<1, M includes at least one of Sb, Nb, Ta, Te, and W;
[0137] LIPON type: such as Li x3 PO y1 N z1 ; 0<x3≤1, 0<y1≤1, 0<z1≤1;
[0138] Perovskite type: such as Li3 x 4Q (2 / 3-x4) MO3, etc., 0.04<x4<0.17, Q includes at least one of La, Sr, Ba, Nd, and M includes at least one of Al, Ti, and Ge;
[0139] Anti-Perovskite type: such as Li3OCl, etc.; Thio-LiSICON type: such as Li (3+x5) My2A (1-y2) Q (4-z2) T z2 ,, wherein -1<x5<2, 0≤y2≤1, 0≤z2≤2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, and Mo, A includes at least one of P, As, Sb, and Bi, Q includes at least one of S and Se, and T includes at least one of F, Cl, Br, and I;
[0140] Sulfide solid electrolytes, including: Thiophosphate type: Li3PS4, Argyrodite type: Li6PS5Cl, Halide type: Li3InCl6, Hydrode type: 0.7Li(CB9H 10 )-0.3Li(CB 11 H 12 ) at least one; for example, Li (10+x6) M (1+y3) A (2-y3) Q (12-z3) H z3 Type: where -2<x6<2, 0≤y3≤2, 0≤z3≤2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo; A includes at least one of P, As, Sb, Bi, Q includes at least one of S, Se, H includes at least one of F, Cl, Br, I: (100-x7)Li2S·x7M·y4Q type: where 20≤x7≤30, 0≤y4≤50, M includes B2S3, Al2S3, In2S3, SiS2, GeS2 , SnS2, P2S5, As2S3, Sb2S5, Bi2S3, WS2, MoS2, Q includes at least one of B2O3, Al2O3, In2O3, SiO2, GeO2, SnO2, P2O5, Sb2O5, Bi2O3, WO2, WO3, MoO2, MoO3, Fe2O3, ZnO, MgO, CuO, CaO, LiN, Li2O, LiF, LiCl, LiBr, LiI; Argyrodite type: Li (6+x8) M y5 A (1-y5) Q (5-z5) T (1+z5) , where -1≤x8≤1, 0≤y5≤1, -1<z5≤1, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, and Mo, A includes at least one of P, As, Sb, and Bi, Q includes at least one of S and Se, and T includes at least one of F, Cl, Br, and I; Halide type: Li3MJ or Li2Sc 2 / 3 J; M includes at least one of Y, Er, In, Sc, and Ga, and J includes at least one of F, Cl, Br, and I.
[0141] When the above-mentioned sulfide solid electrolyte is a sulfide-type solid electrolyte, it includes but is not limited to: argyrodite electrolyte; binary sulfide-type solid systems such as Li2S-P2S5, Li2S-SiS2, Li2S-GeS and Li2S-B2S3, and Li2S-Me-P2S5 ternary system, wherein Me is selected from Si, Ge, Sn or Al, etc.
[0142] Specifically, the above-mentioned sulfide electrolyte is selected from at least one of Li2S-P2S5, Li2S-SiS2, Li2S-GeS, Li2S-B2S3 and Li2S-Me-P2S5.
[0143] Sodium ion solid electrolytes include but are not limited to: NASICON type: Na(1+x9+2y5)Zr (2-y5) M y5 P (3-x9) Si x9 O 12 , 0≤x9≤3, 0≤y5≤1, M includes at least one of Zn, Mg, Ca; Na-β-Alumina type: Na2O·2Al2O3 or Na2O·3Al2O3, etc.; Na (3+x10) M y6 A (1-y6) Q (4-z6) T z6 Type, wherein -1<x10<2, 0≤y6≤1, 0≤z6≤2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, and Mo, A includes at least one of P, As, Sb, and Bi, Q includes at least one of S and Se, and T includes at least one of F, Cl, Br, and I; Na (11+x11) M (2-y7) A (1+y7) Q (12-z7) T z7 Type wherein -1<x11<1, 0≤y7≤2, 0≤z7≤2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo, A includes P, As, Sb, Bi; Q=at least one of S, Se, T includes at least one of F, Cl, Br, I; antiperovskite type Na3OX, X includes at least one of Cl, Br, I, BH4.
[0144] Potassium ion solid electrolytes include but are not limited to: β-Alumina type such as K2O·x13Al2O3, where x13 is any number from 8 to 11, Anti-Perovskite type such as K3OI, and at least one of K2Fe4O7 and KSi2P3 types.
[0145] One embodiment of the present application further provides a method for preparing a modified solid electrolyte, comprising the following steps S10 to S20.
[0146] Step S10: Mixing a solid electrolyte substrate and a phase change toughening agent to prepare a mixture.
[0147] Step S20: sintering the mixture in a protective gas atmosphere to prepare a modified solid electrolyte.
[0148] In the above preparation method, during the sintering period, the grains of the mixture grow and the grain boundaries fuse with each other. At the same time, the phase change toughening agent, which originally tends to be evenly distributed in the mixture, enters the grain boundary area under the promotion of grain growth and is distributed along the grain boundary orientation.
[0149] Furthermore, under the action of grain growth and grain boundary fusion, the defects and pores of the modified solid electrolyte are greatly reduced, and the density is improved.
[0150] The types and further mass ratios of the solid electrolyte substrate and the phase change toughening agent are as described above and will not be repeated here.
[0151] In some embodiments, the sintering temperature is 90° C. to 600° C., and the sintering time is 10 minutes to 120 hours.
[0152] By regulating the temperature and time of the sintering treatment, the phase change toughening agent is further promoted to enter the grain boundary area under the promotion of grain growth.
[0153] In some embodiments, the sintering temperature is 90°C to 550°C.
[0154] The sintering temperature is further adjusted to ensure that most of the phase change toughening agent enters the grain boundary area while maintaining the structural stability of the solid electrolyte substrate and the phase change toughening agent.
[0155] In the above "90℃~600℃", the temperature value includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and the following point values: 90℃, 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, 240℃, 250℃, 260℃, 270℃, 280℃, 290℃ , 300℃, 310℃, 320℃, 330℃, 340℃, 350℃, 360℃, 370℃, 380℃, 390℃, 400℃, 410℃, 420℃, 430℃, 440℃, 450℃, 460℃, 470℃, 480℃, 490℃, 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, 600℃; or a range consisting of any two values, for example, it can be 100 ℃~600℃、100℃~550℃、100℃~500℃、100℃~450℃、100℃~400℃、100℃~350℃、100℃~300℃、100℃~250℃、100℃~200℃、150℃~600℃、150℃~500℃、150℃~400℃、150℃~350℃、150℃~300℃、150℃~250℃、150℃~200℃、200℃~600℃、200℃~500℃、2 00℃~400℃, 200℃~350℃, 200℃~300℃, 200℃~250℃, 250℃~600℃, 250℃~500℃, 250℃~400℃, 250℃~350℃, 250℃~300℃, 300℃~600℃, 300℃~500℃, 300℃~400℃, 300℃~350℃, 400℃~600℃, 400℃~500℃, 450℃~600℃, 450℃~500℃, 500℃~600℃.
[0156] In the above "10min~120h", the time value includes the minimum and maximum values of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and the following point values: 110h, 100h, 95h, 90h, 85h, 80h, 75h, 70h, 65h, 60h, 55h, 50h, 45h, 40h, 35h, 30h, 25h, 20h, 15h, 10h, 9h, 8h, 7h, 6h, 5h, 4h, 3h, 2h, 1h, 0.5h, 20min, and 10min.
[0157] In some embodiments, in the sintering step of step S20 , the temperature is raised to the sintering temperature at a heating rate of 10° C. / min.
[0158] It should be noted that the sintering time is counted from the time when the temperature reaches the sintering temperature.
[0159] In some embodiments, the protective gas atmosphere is formed by filling a protective gas, wherein the protective gas includes at least one of an inert gas and nitrogen.
[0160] Optionally, the protective gas comprises helium.
[0161] Optionally, the water content in the protective gas is less than 0.1 ppm, and the oxygen content is less than 0.1 ppm.
[0162] In some embodiments, after the sintering process, the method further comprises the step of pressing the product obtained by the sintering process;
[0163] Optionally, the pressure T1 used in the pressing step satisfies: T1≤400 MPa;
[0164] Optionally, T1 satisfies: 400 MPa≤T1≤600 MPa.
[0165] Through further pressing treatment, the components of the modified solid electrolyte are distributed more densely, and the phase change toughening agent is further squeezed into the grain boundary area.
[0166] Further adjusting the pressing pressure can further increase the orientation degree A of the phase change toughening agent distributed along the grain boundaries.
[0167] In some embodiments, the mixing step in step S10 is dry mixing, and before the mixture is sintered, the following steps are further included:
[0168] The mixture is compressed into a sheet-like mixture.
[0169] Optionally, the thickness of the sheet-like mixture is 200 μm to 2 mm.
[0170] In some embodiments, the pressure used when pressing the mixture into a sheet-shaped mixture is 400 MPa to 600 MPa.
[0171] In some embodiments, the mixing step in step S10 is wet mixing, and before the mixture is sintered, the following steps are further included:
[0172] The mixture is coated and dried to form a film-like mixture; optionally, the thickness of the film-like mixture is 10 μm to 200 μm.
[0173] It can be understood that dry mixing is to directly mix the solid electrolyte substrate and the phase change toughening agent; wet mixing is to mix the solid electrolyte substrate, the phase change toughening agent, the solvent and the binder to form a mixture slurry.
[0174] Optionally, the solvent may be at least one of water, a small molecule alcohol, a benzene solvent, and an alcohol ether solvent. Further optionally, the small molecule alcohol includes ethanol, propanol, etc., and the benzene solvent includes toluene, xylene, etc.
[0175] The binder can be a binder commonly used in the art, including but not limited to: styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), carboxymethyl chitosan (CMCS), and at least one of polyvinylidene fluoride (PVDF).
[0176] Furthermore, the mixing is carried out under stirring; the stirring method can be various stirring methods commonly used in the art, such as stirring with a ball mill, and the stirring time includes but is not limited to: 0.5h~6h, and further, the stirring speed is 100rpm~300rpm.
[0177] The purpose of the drying step is to dry the solvent in the wet film formed by coating. There are no special requirements for the drying temperature or drying time. It is sufficient to evaporate the solvent in the wet film formed by coating and dry it. Specifically, the drying methods commonly used in the art can be used, including but not limited to: vacuum drying, heating drying, etc.
[0178] It should be noted that the solvent in the mixture after wet mixing will evaporate during the sintering process, and the binder will carbonize and form gas that evaporates during the sintering process. Therefore, the content of solvent and binder residues in the modified solid electrolyte obtained after sintering is extremely small and can be almost ignored.
[0179] One embodiment of the present application provides a solid-state battery, which includes the above-mentioned modified solid-state electrolyte.
[0180] In the above-mentioned modified solid electrolyte, the phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. Therefore, it can more accurately avoid the generation of internal defects in the solid electrolyte, improve toughness and inhibit dendrites from further piercing the electrode. It also has high ionic conductivity, thereby improving the efficiency of solid-state batteries.
[0181] In some embodiments, in the above-mentioned solid-state battery, the modified solid-state electrolyte exists in the form of a membrane; further, the above-mentioned solid-state battery also includes a positive electrode sheet and a negative electrode sheet, and the modified solid-state electrolyte membrane is arranged between the electrode sheet and the negative electrode sheet.
[0182] The positive electrode sheet and the negative electrode sheet may be those commonly used in the art, and the positive electrode sheet and the negative electrode sheet are described herein by way of non-limiting examples.
[0183] negative electrode
[0184] The negative electrode sheet includes a positive electrode current collector and a negative electrode active layer loaded on the surface of the positive electrode current collector.
[0185] The components of the negative electrode active layer include a negative electrode active material.
[0186] The negative electrode active material may be any common negative electrode active material in this application, including at least one of metallic lithium negative electrode materials, carbon-based negative electrode materials, oxide negative electrode materials, and silicon-based negative electrode materials.
[0187] In any embodiment of the present application, the above-mentioned negative electrode active material includes metallic lithium, lithium-containing alloys, lithium-containing composites, mesophase carbon microspheres, graphite, glassy carbon, carbon nanotubes, carbon-carbon composites, carbon fibers, hard carbon, soft carbon, magnesium oxide, silicon-carbon composites, TiO2, MoO2, In2O3, Al2O3, Cu2O, VO2, SnO x 、SiO x , Ga2O3, Sb2O5, Bi2O.
[0188] In any embodiment of the present application, the mass proportion of the negative electrode active material in the negative electrode active layer is 70% to 99.5%.
[0189] In any embodiment of the present application, the components of the negative electrode active layer further include a negative electrode conductive agent and a negative electrode binder.
[0190] In any embodiment of the present application, the negative electrode conductive agent may be a conductive material commonly used in the art, including but not limited to at least one of graphite, carbon nanotubes, nanofibers, carbon black, and graphene. Specifically, the negative electrode conductive agent may be selected from at least one of SP, KS-6, acetylene black, branched Ketjen black ECP, SFG-6, vapor-grown carbon fiber VGCF, carbon nanotubes CNTs, graphene, and composite conductive agents thereof.
[0191] The weight ratio of the negative electrode conductive agent in the negative electrode active layer is 0 to 20 wt % based on the total weight of the negative electrode active layer.
[0192] The negative electrode binder may be a binder commonly used in the art, and may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), carboxymethyl chitosan (CMCS), and polyvinylidene fluoride (PVDF).
[0193] The weight ratio of the negative electrode binder in the negative electrode active layer is 0 to 30 wt % based on the total weight of the negative electrode active layer.
[0194] In any embodiment of the present application, the negative electrode active layer may further optionally include other additives, such as a thickener, such as sodium carboxymethyl cellulose (CMC-Na), etc. Based on the total weight of the negative electrode active layer, the weight ratio of the other additives in the negative electrode active layer is 0 to 15 wt%.
[0195] In any embodiment of the present application, the current collector in the negative electrode sheet may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0196] In any embodiment of the present application, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained. The solid content of the negative electrode slurry is 30wt% to 70wt%, and the viscosity at room temperature is adjusted to 2000mPa·s to 10000mPa·s; the obtained negative electrode slurry is coated on the negative electrode current collector, and after a drying process, cold pressing such as a roller, a negative electrode sheet is obtained. The negative electrode powder coating unit surface density is 75mg / m 2 ~220 mg / m 2 , the compaction density of the negative electrode is 1.2g / m 3 ~2.0g / m 3 .
[0197] positive electrode
[0198] The positive electrode sheet includes a positive electrode current collector and a positive electrode active layer loaded on the surface of the positive electrode current collector.
[0199] The components of the positive electrode active layer include a positive electrode active material.
[0200] In some embodiments, the mass proportion of the positive electrode active material in the positive electrode active layer is 70% to 100%.
[0201] In some embodiments, the positive electrode active material may be a positive electrode active material for a secondary battery known in the art.
[0202] In any embodiment of the present application, the positive electrode active material includes any one of a sodium ion positive electrode active material and a lithium ion positive electrode active material.
[0203] Further, as an example, the lithium ion active material may include at least one of the following materials: lithium phosphates containing olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries can also be used. These positive electrode active materials can be used alone or in combination of two or more. Examples of lithium transition metal oxides may include but are not limited to lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.80 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium manganese phosphate (such as LiMnPO4), and lithium manganese iron phosphate.
[0204] In any embodiment of the present application, the molecular formula of the lithium ion active material is: LiFe x Mn (1-x) PO4, x is any number from 0 to 1.
[0205] It can be understood that when x is 0, LiFe x Mn (1-x) PO4 is LiMnPO4 lithium manganese phosphate, and when x is 1, LiFePO4 is LiFePO4 lithium iron phosphate (LFP).
[0206] As an example, the sodium ion positive electrode active material may include at least one of the following materials: at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as sodium ion battery positive electrode active materials may also be used. In any embodiment of the present application, the positive electrode active material includes at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound;
[0207] Optionally, the positive electrode active material includes at least one of a sodium transition metal oxide and a polyanionic compound.
[0208] Sodium transition metal oxides have a layered transition metal structure. Compared to the rhombohedral phase of Prussian blue compounds, theoretically, layered transition metal structures should have a greater thickness rebound rate. However, in practice, Prussian blue compounds easily absorb water, forming crystalline water and vacancy defects, which increase the thickness rebound rate and even cause structural collapse. Therefore, when sodium transition metal oxides are used as positive electrode active materials, the thickness rebound rate of the positive electrode sheet is actually smaller.
[0209] The anionic structural units in the polyanionic compound are connected into a three-dimensional structure through covalent bonds, and the structure has good stability. When it is used as a positive electrode active material, the thickness rebound rate of the positive electrode sheet is low.
[0210] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Sodium transition metal oxide is, for example, Na x MO2, wherein M includes at least one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.
[0211] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n-A class of compounds with anionic units. Transition metals include at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y includes at least one of P, S, and Si; n represents (YO4) n- valence.
[0212] Polyanionic compounds can also be sodium ions, transition metal ions, tetrahedral (YO4) n- A class of compounds containing anion units and halogen anions. The transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y includes at least one of P, S, and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.
[0213] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedron unit (ZO y ) m+ and an optional halogen anion. Y includes at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, including at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce, m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.
[0214] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2(P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).
[0215] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ). The transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' each independently include at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.
[0216] In any embodiment of the present application, the components of the positive electrode active layer further include a positive electrode binder, and the mass proportion of the positive electrode binder in the positive electrode active layer is 0.05% to 10%.
[0217] Optionally, the mass proportion of the positive electrode binder in the positive electrode active layer is 0.1% to 8%.
[0218] The positive electrode binder can be any of various binders commonly used in the art. As an example, the positive electrode binder includes at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorine-containing acrylate resin, sodium carboxymethyl cellulose, hydroxypropyl cellulose, sodium hydroxymethyl cellulose, potassium hydroxymethyl cellulose, diacetyl cellulose, polyacrylic acid, sodium alginate, styrene-butadiene rubber, acrylic butadiene rubber, polypyrrole, polyaniline, epoxy resin, and guardo gum.
[0219] In any embodiment of the present application, the components of the positive electrode active layer further include a positive electrode conductive agent, and the mass proportion of the positive electrode conductive agent in the positive electrode active layer is 0.05% to 8%.
[0220] Optionally, the mass proportion of the positive electrode conductive agent in the positive electrode active layer is 0.1% to 6%.
[0221] As an example, the positive electrode conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0222] The positive electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0223] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the positive electrode conductor, the positive electrode binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0224] In some embodiments, the solid-state battery is an all-solid-state battery or a semi-solid-state battery.
[0225] In some embodiments, in a solid-state battery, the modified solid electrolyte exists in the form of a modified solid electrolyte membrane, which is located between the positive electrode sheet and the negative electrode sheet.
[0226] Furthermore, the solid-state battery further includes a shell for packaging the positive electrode sheet, the negative electrode sheet, and the modified solid electrolyte membrane.
[0227] In some embodiments, the housing may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the housing may be a soft package, such as a bag-type soft package. The soft package may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0228] The present application has no particular limitation on the shape of the battery, which can be cylindrical, square, or any other shape. For example, FIG1 shows a solid-state battery 4 with a square structure as an example.
[0229] The present application also provides an electrical device, which includes the above-mentioned solid-state battery.
[0230] Furthermore, in the above-mentioned electrical device, the solid-state battery may exist in the form of a battery cell, or may be further assembled into a battery pack.
[0231] Figures 2 and 3 illustrate an example battery pack 1. Battery pack 1 includes a battery case and one or more solid-state batteries 4 disposed within the case. The case comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for the batteries 4.
[0232] Multiple solid-state batteries 4 can be arranged in the battery box in any manner.
[0233] The above-mentioned solid-state battery or the battery pack assembled therefrom can be used as a power source for an electrical device or as an energy storage unit for an electrical device.
[0234] The above-mentioned electrical devices may be, but are not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0235] Figure 4 shows an example of an electric device 5. The electric device 5 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the electric device 5, a battery pack can be used.
[0236] As another example, the power-consuming device may be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and may use a battery as a power source.
[0237] The present application will be described below in conjunction with specific embodiments, but the present application is not limited to the following embodiments. It should be understood that the attached claims summarize the scope of the present application. Under the guidance of the concept of the present application, those skilled in the art should realize that certain changes made to the various embodiments of the present application will be covered by the spirit and scope of the claims of the present application.
[0238] The following are specific examples.
[0239] Example 1
[0240] 1. Preparation of modified solid electrolyte. The specific steps are as follows:
[0241] S1: The solid electrolyte substrate (Li6PS5Cl) and the phase change toughening agent were dry-mixed using a Fritsch Pulverisette planetary ball mill at a rotation speed of 100 rpm for 0.5 h to obtain a mixture.
[0242] The phase change toughening agent includes zirconium oxide and a stabilizer. The mass of the phase change toughening agent is used as the calculation basis, and the mass proportion of the stabilizer is recorded as Y1. The mass proportion of the phase change toughening agent is used as the calculation basis, and the mass proportion of the phase change toughening agent is recorded as Y2. Specific parameters are shown in Table 1.
[0243] S2: The mixture was placed in a mold and pressed at a pressure of 500 MPa to a thickness of 1 mm and a surface area of 19.63 mm. 2 of a disc-shaped mixture.
[0244] S3: The sheet mixture is placed in an argon environment (H2O < 0.1 ppm, O2 < 0.1 ppm), heated to 350°C at a heating rate of 10°C / min, and sintered at this temperature for 10 hours, followed by natural cooling to obtain a modified solid electrolyte.
[0245] S4: Performance testing of modified solid electrolytes
[0246] Test of the orientation degree A of the phase change toughening agent distributed along the grain boundaries in the modified solid electrolyte:
[0247] 1. Cut the wafer perpendicular to its thickness. The cutting point is located at 1 / 2 of the thickness of the wafer. The cross section formed when cutting the wafer is the cross section to be measured.
[0248] 2. The area of the cross section is gridded into 5 unit grid areas, and each unit grid area is placed under a scanning electron microscope for observation to form a scanning electron microscope image; then the total number of signal points emitted by the key elements in the scanning electron microscope image of each grid area is counted, which is regarded as the number of phase change toughening agent particles in each grid area, and recorded as M11, M12, M13, M14, and M15 respectively; at the same time, the number of signal points emitted by the key elements at the grain boundaries in each grid area is counted, which is regarded as the number of phase change toughening agent particles at the grain boundaries in each grid area, and recorded as M21, M22, M23, M24, and M25 respectively, and the orientation degree of the phase change toughening agent along the grain boundary in the modified solid electrolyte in each grid area is calculated, which is recorded as A1, A2, A3, A4, and A5 respectively, and the calculation method is as follows: A1=M21 / M11×100%; A2=M22 / M12×100%; A3=M23 / M 13×100%; A4=M 24 / M 14×100%; A5=M 25 / M 15×100%;
[0249] The orientation degree A of the phase change toughening agent distributed along the grain boundaries in the modified solid electrolyte is calculated according to the following formula:
[0250] A=(A1+A2+A3+A4+A5) / 5.
[0251] Among them, the grid is divided by referring to the five-point sampling method, and five grid units are divided: that is, the midpoint of the diagonal is first determined as the central sampling point grid, and then four grid units with equal distances from the central sampling point grid are selected on the diagonal.
[0252] Specifically, each grid area was analyzed using SEM-EDS analysis. The resulting scanning electron microscope image was divided into 1-μm squares. The number of Zr elemental signal points in the EDS output within the squares was considered the number of phase change toughening agent particles. Detailed results are shown in Table 1. EDS scanning was performed using an accelerating voltage of 10 kV and an Oxford Instrument AZtechOne probe.
[0253] Among them, the scanning electron microscope image of the cross section of the modified solid electrolyte to be tested is shown in Figure 5. It can be clearly seen from the figure that the phase change toughening agent particles are mainly concentrated and distributed along the electrolyte grain boundaries.
[0254] Fracture toughness test of modified solid electrolyte:
[0255] Fracture toughness is a parameter that describes the ability of a material to absorb strain energy before fracture. The fracture toughness value (K IC) indicates a stronger resistance to crack propagation, which also reflects the modified solid electrolyte's ability to resist cracking and short circuiting caused by dendrites. Fracture toughness can be measured using a four-point bending test or a Vickers cone indentation test. The Vickers cone indentation test is used here. The specific process is as follows:
[0256] In an argon atmosphere, the surface of the modified solid electrolyte disc is polished with sandpaper, starting from 800 mesh, then to 2000 mesh, then to 4000 mesh, and finally to 8000 mesh, until the disc surface shows mirror properties without obvious defects. Then, the polished surface is subjected to an indentation test using a Vickers cone indentation tester. The indentation tester is driven with an appropriate load P until radial cracks appear at the four corners of the cone indentation. According to the indentation load P, radial crack extension length C, and microhardness H obtained during the test, the microhardness of the disc is determined. V , the fracture toughness value K is further calculated by the following formula IC :
[0257] Where P is the indentation load when cracks appear, in N; C is the extension length of radial cracks, in mm; H V is the microhardness, unit is kgf / mm 2 ; E is Young's modulus, unit is GPa; K IC is the fracture toughness of the solid electrolyte, the unit is MPa·m 1 / 2 .
[0258] (3) Critical current density test of modified solid electrolyte
[0259] The critical current density (CCD) refers to the minimum current density at which dendrites and short circuits occur during electrochemical deposition of a solid electrolyte material in combination with a corresponding alkali metal electrode. In other words, when electrochemically depositing a modified solid electrolyte below the CCD, dendrites and short circuits do not occur. Critical current density is a core indicator of a solid electrolyte material's ability to suppress dendrites and short circuits.
[0260] The critical current density of the modified solid electrolyte is measured by the traditional symmetric battery step-by-step current density cycle method. Taking lithium-ion solid electrolyte as an example, the process is as follows:
[0261] Two lithium metal discs with 8mm long dendrites and 50μm thickness were placed at the center of the modified solid electrolyte disc on both sides. Mechanical pressure was used to make the lithium metal discs and electrolyte discs fit tightly together to form a lithium / solid electrolyte / lithium symmetrical battery. After the symmetrical battery was assembled and packaged, the symmetrical battery was tested from 0.25mA / cm 2 Starting with a current of 1 mAh / cm, 1 mAh / cm2 After lithium, the current was increased to 0.5 mA / cm 2 , maintain 1mAh / cm 2 After the surface capacity deposition and stripping, the current is increased to 0.75mA / cm 2 , 1.0mA / cm 2 , 1.25mA / cm 2 ...to 10mA / cm 2 , and monitor the voltage change during the process. The current density when the voltage suddenly drops sharply is recorded as the critical current density (Jc). The specific results are shown in Table 1.
[0262] (4) Ionic conductivity test of modified solid electrolyte
[0263] Ionic conductivity is a core indicator for measuring the ability of solid electrolytes to conduct corresponding metal ions. Ionic conductivity is generally tested by electrochemical impedance spectroscopy, and the corresponding ionic conductivity is calculated. The specific process is as follows:
[0264] A 200 nm thick nickel metal layer was deposited on both sides of the solid electrolyte wafer by magnetron sputtering PVD. The current collector was then attached to the nickel metal layer and connected to the electrochemical workstation via the tabs. 6 The solid electrolyte sheet was subjected to electrochemical impedance spectroscopy (EIS) testing at 0.1 Hz to 0.1 Hz. The Z' coordinate of the point closest to the Z' axis from right to left in the low-frequency band of the EIS curve was used as the resistance R. The ionic conductivity σ can be calculated using the following formula:
[0265] Wherein, d is the thickness of the solid electrolyte sheet, and A is the contact area between the solid electrolyte sheet and the current collector.
[0266] (5) The density of the modified solid electrolyte material is tested as follows:
[0267] 1. The mass of the solid electrolyte substrate (Li6PS5Cl) used in the preparation is m1, the theoretical density is ρ1, the mass of the phase change toughening agent is m2, and the theoretical density is ρ2. The theoretical volume Vt of the modified solid electrolyte is calculated according to the following formula: Vt = [m1 / ρ1] + [m2 / ρ2];
[0268] Among them, m1 and m2 can both be obtained by weighing on a balance, the solid electrolyte substrate and the phase change toughening agent are both purchased commodities, and ρ1 and ρ2 are recorded in the parameter table of the commodity.
[0269] 2. The real volume Vr of the modified solid electrolyte is obtained by the Archimedes method or by measuring the actual modified solid electrolyte.
[0270] 3. Density of modified solid electrolyte K = Vt / Vr. See Table 1 for specific results.
[0271] S5: Preparation and performance testing of solid-state batteries
[0272] (1) Preparation of positive electrode sheet
[0273] The positive electrode active material NCM811, the binder nitrile rubber (NBR), the conductive agent VGCF and the electrolyte Li6PS5Cl were mixed in a mass ratio of 80:1.5:0.5:18, and p-xylene was added and stirred to form a uniformly dispersed slurry; the slurry was evenly coated on one surface of the aluminum foil and then transferred to a vacuum drying oven for complete drying; the obtained electrode sheet was roll-pressed and then punched to obtain the positive electrode sheet.
[0274] (2) Preparation of negative electrode sheet
[0275] Lithium metal is used as the negative electrode active material, and the preparation method of the negative electrode sheet is as follows:
[0276] The lithium metal foil is rolled and thinned to a thickness of 50 μm, and the lithium metal foil is covered on one surface of the copper foil by rolling again, and then cut to obtain a negative electrode sheet.
[0277] The solid electrolyte membrane is placed between the negative electrode sheet and the positive electrode sheet, and they are bonded to ensure close contact at the interface to form a solid-state battery.
[0278] (3) Maximum charging current density test: The maximum charging current density of the solid-state battery can be measured by cycling the current density in a step-by-step manner until failure: After the above-mentioned all-solid-state battery is assembled and packaged, the full battery is charged from 0.25 mA / cm 2 At the beginning, charge and discharge were performed separately, and the capacity was controlled at 1 mAh / cm 2 To ensure constant test surface capacity during the cycle test, increase the current to 0.5 mA / cm after completing the first cycle. 2 , maintain 1mAh / cm 2 After the surface capacity is charged and discharged for a cycle, the 2 The gradient is 0.75 mA / cm 2 , 1.0mA / cm 2 , 1.25mA / cm 2 ...to 10mA / cm 2 Perform all-solid-state battery cycling and record the current density at which the voltage suddenly drops sharply or exhibits obvious jitter as the maximum charging current density.
[0279] In fact, the maximum charging current density has a similar physical meaning to the critical current density of the composite solid electrolyte, and their values are almost the same.
[0280] Example 2
[0281] Example 2 is basically the same as Example 1, except that the type of stabilizer in step S1 is different from that in Example 1. Please see Table 1 for specific conditions.
[0282] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0283] Examples 3 to 6
[0284] Examples 3 to 6 are basically the same as Example 1, except that in step S1, the mass proportion of the phase change toughening agent in the mixture is denoted as Y2, which is different from Example 1. For specific conditions, see Table 1.
[0285] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0286] Examples 7 to 13
[0287] Examples 7 to 13 are basically the same as Example 1, and the only difference is the temperature or time of the sintering treatment in step S3. Please see Table 1 for specific conditions.
[0288] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0289] Examples 14 to 16
[0290] Examples 14 to 16 are basically the same as Example 1, except that the mass proportion Y1 of the stabilizer in the phase change toughening agent in step S1 is different from that in Example 1. Please see Table 1 for specific conditions.
[0291] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0292] Comparative Example 1
[0293] Comparative Example 1 is substantially the same as Example 1, except that: in Comparative Example 1, a solid electrolyte substrate (Li6PS5Cl) is directly provided to perform step S4 and subsequent steps.
[0294] Comparative Example 2
[0295] Comparative Example 2 is substantially the same as Example 1, except that step S3 is not performed in Comparative Example 2. Specific conditions are shown in Table 1.
[0296] The remaining steps are the same as those in Example 1.
[0297] The relevant physical parameters and test results in each embodiment and comparative example are shown in Table 1, wherein the mass of the phase change toughening agent is used as the calculation basis, the mass proportion of the stabilizer is recorded as Y1, the total mass of the modified solid electrolyte is used as the calculation basis, the mass proportion of the phase change toughening agent is recorded as Y2, the orientation degree of the phase change toughening agent along the grain boundary in the modified solid electrolyte is A, KIC, Jc, σ and K are the fracture toughness, critical current density, ionic conductivity and density of the modified solid electrolyte, respectively.
[0298] Table 1
[0299] Note: “ / ” means that the step processing or the substance or parameter does not exist.
[0300] From the experimental results in the above table, analysis and comparison of the data of Example 1 and Comparative Examples 1 to 2 show that in the modified solid electrolyte of the present application, the phase change toughening agent is mainly distributed along the grain boundary region in the modified solid electrolyte, and the grain boundary is the defective area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. Therefore, the phase change toughening agent is mainly distributed along the grain boundary region in the modified solid electrolyte, which can more accurately avoid the generation of internal defects in the solid electrolyte and further improve the toughness.
[0301] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0302] The above-described embodiments merely represent several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make a number of variations and improvements without departing from the concept of the present application, and these variations and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the patent application shall be based on the appended claims, and the description and drawings may be used to interpret the content of the claims.
Claims
1. A modified solid electrolyte, the components of which include a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate, and in the modified solid electrolyte, the phase change toughening agent is mainly distributed at the grain boundaries in the solid electrolyte; The phase change toughening agent can undergo phase change under the action of external force.
2. The modified solid electrolyte according to claim 1, wherein Among the total number of particles of the phase change toughening agent in the modified solid electrolyte, the number of particles of the phase change toughening agent distributed at the grain boundaries in the solid electrolyte accounts for ≥50%.
3. The modified solid electrolyte according to claim 1, wherein In the same cross section of the modified solid electrolyte, the total number of particles of the phase change toughening agent is N1, and the number of particles of the phase change toughening agent distributed at the grain boundary in the same cross section is N2, then the orientation degree of the phase change toughening agent distributed along the grain boundary is A=N2 / N1×100%, and A satisfies: A≥50%; Optionally, A satisfies: 50%<A≤100%; Optionally, A satisfies: 50%<A<100%.
4. The modified solid electrolyte according to claim 3, wherein The same cross section is a cross section or a longitudinal section of the modified solid electrolyte.
5. The modified solid electrolyte according to claim 3, wherein The test steps of the orientation degree A include: Taking the sample to be tested of the modified solid electrolyte, cutting the sample to be tested along a direction perpendicular to the thickness of the sample to be tested, and the cutting section formed when cutting the sample to be tested is the cross section to be tested; An X-ray spectrometer is used to mark the key elements contained in the phase change toughening agent in the cross section to be measured, so that the key elements emit signal points, and a scanning electron microscope image of the cross section to be measured is obtained: Obtaining a total number M1 of the signal points in the scanning electron microscope image and a number M2 of the signal points contained at the grain boundaries in the scanning electron microscope image; According to M1 and M2, we get A; The key element is an element contained in the phase change toughening agent but not contained in the solid electrolyte substrate.
6. The modified solid electrolyte according to claim 5, wherein The phase change toughening agent contains zirconium oxide, and the key element is zirconium.
7. The modified solid electrolyte according to claim 6, wherein The phase change toughening agent further contains a stabilizer, and the mass proportion of the stabilizer in the phase change toughening agent is 0.01% to 50%; Optionally, the stabilizer contains at least one element selected from the group consisting of yttrium, scandium, magnesium, calcium, and cesium; Optionally, the stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide; Optionally, the stabilizer comprises yttrium oxide.
8. The modified solid electrolyte according to any one of claims 1 to 7, wherein In the modified solid electrolyte, the mass proportion of the phase change toughening agent is 2% to 25%; Optionally, the mass proportion of the phase change toughening agent is 5% to 25%; Optionally, the mass proportion of the phase change toughening agent is 10% to 25%; Optionally, the mass proportion of the phase change toughening agent is 15% to 25%.
9. The modified solid electrolyte according to any one of claims 1 to 8, wherein In the modified solid electrolyte, the mass of the solid electrolyte substrate is m1, the theoretical density is ρ1, the mass of the phase change toughening agent is m2, the theoretical density is ρ2, then the theoretical volume Vt of the modified solid electrolyte satisfies: Vt = [m1 / ρ1] + [m2 / ρ2]; The actual volume of the modified solid electrolyte is Vr, and the density of the modified solid electrolyte is K=Vt / Vr×100%; Optionally, K satisfies: K≥70%; Optionally, K satisfies: 90%≤K≤100%.
10. The modified solid electrolyte according to any one of claims 1 to 9, wherein The solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte and a potassium ion solid electrolyte.
11. A method for preparing a modified solid electrolyte, comprising the following steps: Mixing a solid electrolyte substrate and a phase change toughening agent to prepare a mixture; The mixture is sintered under a protective gas atmosphere to prepare a modified solid electrolyte.
12. The method for preparing a modified solid electrolyte according to claim 11, wherein: The sintering process satisfies at least one of the following conditions (1) to (2): (1) The sintering treatment temperature is 90°C to 600°C, and the sintering time is 10 minutes to 120 hours; (2) The protective gas atmosphere is formed by filling with a protective gas, wherein the protective gas comprises at least one of an inert gas and nitrogen; Optionally, the protective gas comprises helium; Optionally, the water content in the protective gas is less than 0.1 ppm, and the oxygen content is less than 0.1 ppm.
13. The method for preparing a modified solid electrolyte according to any one of claims 11 to 12, wherein: After the sintering process, the method further comprises the step of pressing the product obtained by the sintering process; Optionally, the pressure T1 used in the pressing step satisfies: T1 ≥ 400 MPa; Optionally, T1 satisfies: 400MPa≤T1≤600MPa.
14. The method for preparing a modified solid electrolyte according to any one of claims 11 to 12, wherein: The mixing step adopts dry mixing, and before the mixture is sintered, the following steps are also included: The mixture is pressed into a sheet-like mixture; optionally, the thickness of the sheet-like mixture is 200 μm to 2 mm; optionally, the pressure used when the mixture is pressed into the sheet-like mixture is 400 to 600 MPa; or The mixing step adopts wet mixing, and before the mixture is sintered, the following steps are also included: The mixture is coated and dried to form a film-like mixture; optionally, the thickness of the film-like mixture is 10 μm to 200 μm.
15. A solid-state battery, comprising the modified solid electrolyte according to any one of claims 1 to 10 or the modified solid electrolyte prepared by the method for preparing the modified solid electrolyte according to any one of claims 11 to 14.
16. An electrical device, comprising the solid-state battery according to claim 15.
Citation Information
Patent Citations
Composite solid electrolyte membrane, preparation method thereof and solid-state battery
CN114142082A
Ceramic lamination body and its manufacture
JP2000292406A
Zirconia-based ceramic and method of producing the same
JP2002145663A
High Voltage Electrolyte for 5V Solid State Lithium-ion Battery Cell
US20230013068A1
Cited By
Doping modified sulfide electrolyte and preparation method thereof
CN120657236A
Metal tungsten interface modification layer, preparation method and solid-state battery