Coating mixture for coating of substrates, process for producing coated substrates, and coated substrate and its use
The coating mixture with silane, oligosiloxane, and specific additives forms a polysiloxane xerogel matrix that actively inhibits corrosion, addressing the limitations of chromium(VI) compounds by providing effective, environmentally friendly corrosion protection for metals, even after coating damage.
Patent Information
- Application Number
- PCT/EP2024/061925
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-07
AI Technical Summary
Current corrosion protection methods for metals, particularly in industries like automotive and aerospace, rely heavily on toxic chromium(VI) compounds, which are regulated due to environmental and health concerns, necessitating the development of environmentally friendly and effective alternatives that can provide both passive and active protection, especially in scenarios where coatings are physically damaged.
A coating mixture comprising silane, oligosiloxane, a complexing agent functioning as a reducing agent, and a metal-containing ion, which forms a polysiloxane xerogel matrix that actively inhibits corrosion by altering the redox potential and forming protective layers, offering both passive and active corrosion protection without using chromium(VI).
The solution achieves excellent corrosion resistance with a thin, dense coating that remains effective even after physical damage, reducing material usage and manufacturing costs, while being environmentally friendly and compatible with various metal substrates.
Smart Images

Figure IMGF000009_0001 
Figure IMGF000010_0001 
Figure IMGF000027_0001
Abstract
Description
[0001] Zitt GmbH & Co.KG
[0002] 249 PCT 1033
[0003] Coating mixture for coating substrates, method for producing coated substrates, as well as coated substrate and its use The present invention relates to a coating mixture for coating substrates which contain or consist of material to be protected against corrosion, wherein the material to be protected against corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; copper; alloys containing iron, copper and / or aluminum; intermetallic phases containing iron, copper and / or aluminum; composite materials containing iron, copper and / or aluminum;and mixtures thereof, wherein the coating mixture contains at least one silane and / or at least one oligosiloxane formed from the at least one silane, at least one complexing agent for complexing cations of at least one metal contained in the material to be protected from corrosion, at least one metal-containing ion, and at least one solvent. The present invention also relates to a process for producing coated substrates, as well as to a coated substrate and its use.
[0004] Due to the excessive growth of the world population and the high demands of various industries, today's researchers are expected to develop new, innovative, and durable materials. For metals, corrosion is the most significant problem to be solved. Therefore, innovative corrosion protection techniques and methods should be continuously developed. One of these is various coatings: e.g., conversion coatings, primers, resins, and paint systems.
[0005] In certain industrial applications, such as hydraulics, components are only treated in the assembled state, i.e., after components made of different materials, such as aluminum, steel, sealing material, or plastic, have been joined together. Contact between two metals creates a galvanic element, which leads to increased corrosion, which is also problematic.
[0006] Many conventional anti-corrosive coatings are banned or planned to be banned due to environmental, sustainability, and health concerns. For example, the automotive industry has already restricted the use of chromium(VI)-based passivation processes due to their toxicity and carcinogenicity, and these restrictions are being extended to the aerospace industry. The search for new environmentally friendly materials and processes could lead to more effective corrosion protection of coatings at lower costs. For example, a specific additive or a targeted blend of additives could be found that, when incorporated into a coating system, could significantly improve corrosion resistance.Increased corrosion resistance could make it possible to reduce the thickness of the coatings or, in the case of a multi-layer system, the number of coatings required, which would of course be an important economic aspect.
[0007] Furthermore, mechanically damaged coatings, e.g., due to breakage, are no longer able to protect against corrosion, as the bare metal surface at the fracture site comes into contact with atmospheric moisture and also with corrosive species: This leads to progressive corrosion under the coating and to corrosion damage to the metal substrate itself. Therefore, novel corrosion protection coatings should be able to continue to protect against corrosion even in the event of physical or mechanical damage to the coating.
[0008] All these facts are of great importance and therefore there is a great need for innovative solutions in the following industries, for example: automotive, aerospace, precision machining, defense and shipbuilding, as they must avoid highly toxic compounds while maintaining adequate corrosion protection.
[0009] Corrosion protection of metal substrates has been the subject of intensive research in recent decades, but the problem has not yet been satisfactorily resolved. Various industries are affected, as corrosion control is a very important issue to ensure the safety and reliability of manufactured metal parts, particularly in the automotive and aerospace industries. These industries use various aluminum and steel alloys, which require different approaches depending on their composition.
[0010] A generally accepted and proven effective corrosion protection method is chromium(VI) compounds, which are used for the pretreatment of metal substrates and also in conversion coatings. These compounds offer excellent corrosion protection due to the formation of oxides and hydroxides. However, because they are highly toxic and carcinogenic, their use is strictly regulated and in some cases prohibited, requiring the development of new materials.
[0011] Based on this, the object of the present invention was to provide a mixture for coating substrates, with which coatings with very good corrosion protection can be obtained, and to specify a method for producing coated substrates with which coated substrates can be obtained that have very good corrosion protection. This object is achieved with regard to a coating mixture for coating substrates with the features of patent claim 1, with regard to a method for producing coated substrates with the features of patent claim 6, and with regard to a coated substrate with the features of patent claim 10. Claim 15 specifies possible uses of the coated substrate according to the invention. The dependent claims represent advantageous developments.
[0012] According to the invention, a coating mixture (or mixture) is thus provided for coating substrates which contain or consist of material to be protected from corrosion, wherein the material to be protected from corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; copper; alloys containing iron, copper and / or aluminum, intermetallic phases containing iron, copper and / or aluminum; composite materials containing iron, copper and / or aluminum; and mixtures thereof, wherein the coating mixture
[0013] • at least one silane and / or at least one oligosiloxane formed from the at least one silane (by cross-linking),
[0014] • at least one complexing agent for complexing cations of at least one metal contained in the material to be protected from corrosion,
[0015] • at least one metal-containing ion, and
[0016] • comprises at least one solvent, wherein the at least one silane has at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, and wherein the at least one complexing agent comprises at least one complexing agent which (additionally) functions as a reducing agent and which is the reduced form of a (corresponding) redox pair which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a lower (or more negative) redox potential (or electrode potential) in this aqueous solution than the (corresponding) redox pair(s) of a metal contained in the material to be protected from corrosion, preferably than the (corresponding) redox pair(s).corresponding) redox pair(s) of the metal contained in the material to be protected from corrosion, and / or the coating mixture additionally contains at least one reducing agent which is the reduced form of a (corresponding) redox pair which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a lower (or more negative) redox potential (or electrode potential) in this aqueous solution than the (corresponding) redox pair(s) of a metal contained in the material to be protected from corrosion, preferably than the (corresponding) redox pair(s) of each metal contained in the material to be protected from corrosion.
[0017] The (corresponding) redox pair(s) of a metal contained in the material to be protected from corrosion is / are understood to be the (corresponding) redox pair(s) in which the metal contained in the material to be protected from corrosion is in its reduced form. For the metal aluminum, for example, this would be the (corresponding) redox pair Al / Al. 3+ For the metal iron, for example, these would be the (corresponding) redox pairs Fe / Fe 2+ and Fe / Fe 3+ .
[0018] By combining the special components of the coating mixture according to the invention, coatings can be produced with the coating mixture that offer very good corrosion protection. The coatings produced with the coating mixture according to the invention are capable of protecting the material to be protected from corrosion not only passively but also actively. This means that – even in the event of physical damage to the coating – the coating can continue to protect the material to be protected from corrosion in a complex chemical manner.
[0019] This exploits the fact that, during the production of a coating or a coated substrate using the coating mixture according to the invention, a polymeric network, a so-called xerogel or polysiloxane xerogel, can be formed (by crosslinking the at least one silane and / or the at least one oligosiloxane), to which the other components of the mixture can be advantageously added (e.g. adsorbed) and / or bound (e.g. covalently bonded), so that a very good homogeneous distribution of the components over the entire coating can be achieved. The polysiloxane xerogel thus functions in the produced coating as a type of matrix to which the other components can be added and / or bonded.
[0020] Silane or polysiloxane materials have so far only been used as sealing layers for corrosion protection. Examples can also be found in which various metal oxide nanoparticles, plant extracts, or 2D materials such as graphene oxide or carbon nanotubes have been incorporated. However, these only utilize the passive corrosion protection properties of these fillers / additives, aiming for, among other things, increased hydrophobicity or simple diffusion barrier properties with corresponding mechanistic interpretations. As discovered within the scope of the present invention, the special structure of polysiloxane xerogels, with their high specific surface area and small pore size, offers even further possibilities for effectively modifying the corrosion chemistry on a given substrate in a targeted combination, whereby the specific interactions of different processes can be finely tuned.As a result, various possibilities for active corrosion-inhibiting chemical and electrochemical processes can be initiated, which have not yet been explored in the state of the art.
[0021] With the coating mixture according to the invention, coatings with a low thickness (similar to typical conversion coatings) can be developed. On the one hand, this has a clearly positive economic effect, since thinner layers require less material and therefore have lower production costs. On the other hand, the thinner coatings have a positive influence on the mechanical properties of the coated substrates.
[0022] The polysiloxane xerogel (or polysiloxane network) obtained by crosslinking the at least one silane can act as a matrix for the other components of the coating, e.g., instead of water or other solvents that evaporate after coating. This is particularly important with regard to the following aspects:
[0023] • The polysiloxane network is able to create nanocavities in which additives find their place, chemical reactions can take place locally without affecting the entire surface.
[0024] • A coating without polysiloxane xerogel, e.g. water-based, would only lead to a sporadic occurrence of the other components on the substrate surface, while the intact polysiloxane network as a reservoir for the other components enables a homogeneous distribution of these components in the coating.
[0025] • Thanks to the polysiloxane xerogel, the resulting coating is dense, homogeneous, and covers the entire surface. Since at least one silane can be selected, modified, or functionalized for the specific application, a subsequent primer layer is unnecessary: the coating itself can serve as both a conversion layer and adhesion promoter. This has a clearly positive economic effect, while also positively influencing the mechanical properties of the coated substrates.
[0026] • The polysiloxane network acts as a physical diffusion barrier for corrosive agents and substances, including oxygen, hydrogen, water, etc. Through functionalization with other (possibly polycyclic) molecules, this effect can be thought of as a kind of "labyrinth" that makes it difficult for these substances to access the metal surface by lengthening the diffusion path. This is a passive form of corrosion protection.
[0027] By combining at least one silane, which is cross-linked in the form of a polysiloxane xerogel in the produced coating, with the other components of the mixture or the produced coating, not only passive but also active corrosion protection of the material to be protected from corrosion can be achieved.
[0028] Firstly, active corrosion protection is obtained by the reducing agent and / or the complexing agent acting as a reducing agent. Due to the presence of the specific reducing agent or the specific complexing agent acting as a reducing agent in the produced coating, which is the reduced form of a redox couple which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a lower (or more negative) redox potential (or electrode potential) in this aqueous solution than the redox couple(s) of the metal to be protected (or of a metal contained in the material to be protected from corrosion), according to the laws of electrochemistry, this reducing agent is used instead of the metal to be protected (or of the metal to be protected) in a coated substrate produced with the coating mixture according to the invention.of the metal contained in the material to be protected from corrosion). In other words, the reducing agent sacrifices itself for this metal in order to protect it from oxidation or corrosion. If the metal to be protected is aluminum, for example, the oxidation of aluminum does not occur according to reaction AI. Al 3+ + 3e, but instead oxidation of the reducing agent, such as ascorbic acid, vanillin, melamine, and / or readily oxidizable groups, including those with N or S atoms on silane or siloxane molecules. In this way, the material to be protected from corrosion can be actively protected against corrosion.
[0029] In addition, the at least one metal-containing ion can lead to active corrosion protection in two different ways. For example, the metal contained in the metal-containing ion can be the oxidized form of a redox couple, which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a higher (or more positive) redox potential (or electrode potential) in this aqueous solution than the redox couple O2 / H2O and / or the redox couple Ch / OH (depending on the pH value). In this case, in a coated substrate produced with the coating mixture according to the invention, the metal contained in the metal-containing ion would be reduced instead of oxygen according to the laws of electrochemistry. Thus, the reduction of oxygen according to the reaction 1 O2 + 2e + 2 H + - H2O or the reaction 1 O2 + 2e _ + H2O 2 OH- (depending on the pH value), but instead reduces the metal contained in the metal-containing ion. This prevents the reduction of oxygen and thus the cathodic reaction of corrosion, thus achieving active corrosion protection.
[0030] For kinetic reasons, as well as because the electrode potential in the aqueous medium has a limit, or if the metal contained in the metal-containing ion is not the oxidized form of a redox couple, which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a higher (or more positive) redox potential (or electrode potential) in this aqueous solution than the redox couple O2 / H2O and / or the redox couple Ch / OH (depending on the pH value), the added metal-containing ion can also act differently, or lead to active corrosion protection in a different way. In this case, oxygen is reduced, i.e. the cathodic reaction of the corrosion is not stopped. But theThe hydroxide ions resulting from the reduction of oxygen will not form a corrosion product with the metal cation of the metal to be protected, but will form a protective metal oxide and / or metal hydroxide layer with the metal contained in the metal-containing ion, which leads to active corrosion protection.
[0031] The reducing agent or the complexing agent acting as a reducing agent, as well as the metal-containing ion, can accelerate certain beneficial oxidation and reduction reactions and suppress other harmful ones, ultimately resulting in active corrosion protection. It should be noted that the various components of the coating influence or change the redox potential of the redox pair of the reducing agent or the complexing agent acting as a reducing agent, the redox potential of the redox pair of the metal contained in the metal-containing ion, and also the redox potential of the redox pair of the metal contained in the material to be protected from corrosion.The redox potential conditions can thus be finely tuned via the various components of the coating, so that the redox potentials of the redox pairs of the individual components are in such a relationship to each other that the desired advantageous oxidation and reduction reactions take place and the undesired oxidation and reduction reactions are suppressed.
[0032] Furthermore, the at least one complexing agent (regardless of any possible additional function of the complexing agent as a reducing agent) also contributes to active corrosion protection. For kinetic reasons, and because the electrode potential in an aqueous medium has a limit, the metal contained in the material to be protected from corrosion can also dissolve to a certain extent, i.e., the metal can be reduced to a certain extent in the produced coating despite the presence of the reducing agent (or the complexing agent acting as a reducing agent). The at least one complexing agent complexes the oxidized cations of the metal contained in the material to be protected from corrosion, so that the cations are bound by the complexing agent and can therefore no longer contribute to the corrosion process.In other words, no corrosion product can form from the cations of the metal contained in the material to be protected from corrosion and the oxide and / or hydroxide ions present. Furthermore, the coating prevents cations from diffusing away from the metal surface through the coating due to corrosion phenomena, which would lead to the complete destruction of the protective layer after electrochemical or chemical reactions. However, since the cations are trapped by the complexation with the at least one complexing agent, such diffusion can be prevented. In this context, the at least one complexing agent can also be considered a potential ion exchanger.
[0033] The presence of the reducing agent or the complexing agent acting as a reducing agent and the metal-containing ion in the mixture and thus in the produced coating can ensure that a redox reaction no longer takes place (or only to a minimal extent) between oxygen and a metal contained in the material to be protected from corrosion, but rather between oxygen and the reducing agent and / or between the metal of the metal-containing ion and the reducing agent. Since oxidation of the metal contained in the material to be protected from corrosion by the reducing agent (or the complexing agent acting as a reducing agent) may not be completely prevented, the presence of the complexing agent ensures that the metal cations formed by such oxidation are complexed or oxidized by the complexing agent.so that they cannot diffuse away and contribute to a corrosion process. Furthermore, the metal-containing ion can also contribute to corrosion protection by forming a metal oxide layer and / or metal hydroxide layer that protects against corrosion.
[0034] The polysiloxane matrix or polysiloxane xerogel present in the produced coating, which is formed (or produced) by crosslinking the at least one silane and / or the at least one oligosiloxane, ultimately acts as a kind of "container" for the components, which, due to the network structure of the polysiloxane matrix, are evenly distributed over the entire surface and can thus provide optimal protection against corrosion. The physical barrier effect of the polysiloxane xerogel effectively keeps corrosive species away from the surface. On the one hand, polysiloxanes can be applied macroscopically densely, with a homogeneous layer thickness, to metallic surfaces, while on the microscopic level they exhibit internal cavities (pores). This allows oxygen, water, chloride ions, etc., to diffuse longer distances to the surface, which enables further kinetic prevention of corrosion processes.The polysiloxane network structure also enables the immobilization of the above components: by functionalizing the side chains, it is possible to covalently bind reducing agents or complexing agents.
[0035] The components present in the mixture (e.g., the complexing agent, the reducing agent, and / or the at least one silane) can contain functional groups that are residues of weak acids. This would also provide a certain buffering capacity: OH ions are formed, which promote the formation of the protective layers discussed above with the metal from the metal-containing ion. As residues of weak acids, oxygen-containing functional groups of the at least one silane can provide a certain buffering capacity in the low alkaline pH range. Furthermore, alkaline-hydrolyzing ions also act as buffering agents. In alkaline media, the effects of acids, which make a significant contribution to corrosion, can be counteracted. Furthermore, the presence of hydroxide ions can shift the equilibria of corrosion reactions according to the Le Châtelier principle, preferably the oxygen reduction reactions H2O + 1 / 2O2 + 2 e- -> 2 OH- and 2 H2O + O2 + 2 e- -> H2O2 + 2 OH-, which leads to a slowdown of cathodic delamination.
[0036] The coating composition according to the invention is characterized in particular by the following advantageous properties:
[0037] Excellent storage stability, no sedimentation or precipitation phenomena observed
[0038] Simple application using common techniques (dipping, squeegeeing, rolling, spinning, etc.) in a robust and fast manner
[0039] Possibility of local application / repair (spraying, brushing) Environmentally friendly, sustainable, and energy / environmentally friendly (low-temperature process, low rinsing water requirement and thus less wastewater)
[0040] Easy adaptation to specific customer requirements, search for new high-performance additives
[0041] A coating produced with the coating composition according to the invention can have the following advantageous properties: very small pore size very thin layers (thickness similar to that of typical conversion coatings) possible, e.g. 500 nm to 800 nm, or layers with a thickness down to the pm range dense layer with granular morphology; very good adhesion, particles remain on the surface after fracture (cryogenic fracture)
[0042] Excellent corrosion resistance
[0043] Improved mechanical resistance
[0044] Excellent adhesion to all metal surfaces as well as to all underlying or overlying coatings (enabling application on multi-material systems) Optional: elastic properties, which makes the coating suitable for potential damping against thermal expansion discrepancy-related mechanical stresses
[0045] -> increased compatibility with typical coatings in the automotive and aerospace industries
[0046] -> Any combination with common compositions of basecoats, topcoats is conceivable to form multi-layer systems or hybrid systems of sandwich structures or composite structures
[0047] Diffusion barrier effect for water and other corrosive substances
[0048] Possibility of painting, gluing, printing
[0049] Possibility of chemically controlled (active) corrosion protection (a type of self-healing) low inspection and repair requirements
[0050] Preferably, the material to be protected from corrosion is selected from the group consisting of
[0051] aluminum; anodized aluminum; iron;
[0052] Copper;
[0053] Alloys comprising or consisting of
[0054] • Aluminium and / or iron, as well as
[0055] • at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof;
[0056] Alloys comprising or consisting of copper and zinc; intermetallic phases comprising or consisting of
[0057] • Aluminium and / or iron, as well as
[0058] • at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof;
[0059] Composite materials comprising or consisting of
[0060] • Aluminium, iron and / or copper, as well as
[0061] • at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof; as well as mixtures thereof.
[0062] Particularly preferably, the material to be protected against corrosion is selected from the group consisting of
[0063] aluminum; anodized aluminum;
[0064] Iron;
[0065] Copper;
[0066] Steel; alloys consisting of aluminum and at least one substance selected from the group consisting of copper, magnesium, iron, zinc, silicon, chromium, manganese, and mixtures thereof; preferably AI 2024-T3, AI 7075-T6, AIMgl, AIMg3, AI99.5 (EN AW 1050A), and mixtures thereof; intermetallic phases consisting of aluminum and at least one substance selected from the group consisting of copper, magnesium, iron, zinc, silicon, chromium, manganese, and mixtures thereof;
[0067] Alloys consisting of iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, and mixtures thereof; preferably low-alloy steel (E), steel 1.4301 (S), HDG steel (Z275); intermetallic phases consisting of iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, and mixtures thereof;
[0068] Alloys consisting of copper and zinc;
[0069] Composite materials consisting of aluminum and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof;
[0070] Composite materials consisting of iron and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof;
[0071] Composite materials consisting of copper and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber-reinforced plastics, glass fiber-reinforced plastics, and mixtures thereof; as well as mixtures thereof.
[0072] The composite materials could, for example, be carbon fiber reinforced plastic (CFRP) composites with integrated copper mesh. This would offer the following advantages:
[0073] Corrosion protection on copper
[0074] Compensation of the discrepancy in the thermal expansion coefficients of copper and carbon fiber reinforced plastics (a(Cu)» a(CFRP)) - Reduction of mechanical stresses
[0075] Adhesion mediation between copper and carbon fiber reinforced plastic
[0076] In the event that CFRP-AI contacts are also present, a coating according to the invention on the multi-material system could prevent contact corrosion
[0077] The substrate is preferably a composite made up of several subcomponents, at least one of the subcomponents being made of the material to be protected against corrosion. Such a composite can particularly preferably comprise at least one subcomponent made of the material to be protected against corrosion (e.g. at least one subcomponent made of aluminum and / or at least one subcomponent made of steel) and at least one subcomponent made of at least one plastic, and optionally additionally at least one subcomponent made of at least one sealing material. The at least one plastic is preferably selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof.The at least one sealing material is preferably selected from the group consisting of polyurethane and 1K and 2K epoxy materials, in particular thermoplastic polyurethanes, polytetrafluoroethylene, acrylonitrile butadiene rubber, vulcanized rubber, and mixtures thereof. For example, the composite can comprise at least one subcomponent made of a first material to be protected against corrosion (e.g., aluminum), at least one subcomponent made of a second material to be protected against corrosion (e.g., steel), and at least one subcomponent made of the at least one plastic, and optionally additionally at least one subcomponent made of the at least one sealing material.
[0078] Such composites can be used, for example, in the hydraulics sector. There, components are only treated in their assembled state, i.e., after components made of different materials, such as aluminum, steel, sealing material, or plastic, have been bonded together. Contact between two metals creates a galvanic element, which leads to increased corrosion. Coating the composite with the coating mixture enables a universal coating on the multiple (sub-)components with good adhesion and good corrosion protection properties. The electrical potential difference resulting from contact between two metals can be chemically compensated by the active corrosion protection effect of the coating described.
[0079] The coating mixture according to the invention comprises at least one silane and / or at least one oligosiloxane formed from the at least one silane (by crosslinking). The at least one oligosiloxane can, for example, have 2 to 50, preferably 2 to 30, (monomeric) subunits (or siloxane units).
[0080] Preferably, the at least one silane has at least two, particularly preferably at least three, alkoxy groups having 1 to 4 carbon atoms bonded to the Si atom.
[0081] The at least one complexing agent is suitable for complexing cations of at least one metal contained in the material to be protected from corrosion. Preferably, the at least one complexing agent for complexing cations of at least one metal contained in the material to be protected from corrosion is at least one complexing agent for complexing cations selected from the group consisting of iron cations, aluminum cations, copper cations, magnesium cations, zinc cations, chromium cations, manganese cations, and mixtures and combinations thereof. Particularly preferably, the at least one complexing agent for complexing cations of at least one metal contained in the material to be protected from corrosion is at least one complexing agent for complexing aluminum cations and / or iron cations.
[0082] According to the invention, the at least one complexing agent comprises at least one complexing agent acting as a reducing agent, which is the reduced form of a (corresponding) redox pair which, upon contact of an aqueous solution (e.g. an aqueous salt solution or an aqueous buffer solution) with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a lower (or more negative) redox potential in this aqueous solution (preferably at a temperature of 5 °C to 50 °C, e.g. at a temperature of 25 °C) than the (corresponding) redox pair or pairs of a metal contained in the material to be protected from corrosion, and / or the coating mixture additionally contains at least one reducing agent which is the reduced form of a (corresponding) redox pair which, upon contact of an aqueous solution (e.g.an aqueous salt solution or an aqueous buffer solution) with a coating produced with the coating mixture (on a substrate made of the material to be protected against corrosion) in this aqueous solution (preferably at a temperature of 5 °C to 50 °C, e.g. at a temperature of 25 °C) has a lower redox potential than the (corresponding) redox pair or the (corresponding) redox pairs of a metal contained in the material to be protected against corrosion.
[0083] The aqueous salt solution can (in both of the aforementioned cases) preferably have a salt content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a salt content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 3 to 11, preferably of 5 to 9 (e.g. a pH of 7). For example, the aqueous salt solution (in both of the aforementioned cases) can be an aqueous NaCl solution, which preferably has an NaCl content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a NaCl content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 3 to 11, preferably of 5 to 9 (e.g. a pH of 7).
[0084] The aqueous buffer solution may (in both of the above-mentioned cases) preferably have a buffer content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a buffer content of 3.5 wt.%), based on the total mass of the solution, and / or a pH value of 7 to 10, preferably of 8 to 9 (e.g. a pH value of 8.5). For example, the aqueous buffer solution (in both of the above-mentioned cases) may be an aqueous sodium tetraborate / boric acid buffer solution, which preferably has a sodium tetraborate / boric acid buffer content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a sodium tetraborate / boric acid buffer content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 7 to 10, preferably of 8 to 9 (e.g. a pH of 8.5).
[0085] The feature that the at least one reducing agent or the at least one complexing agent acting as a reducing agent is the reduced form of a redox pair which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a lower (or more negative) redox potential in this aqueous solution than the redox pair(s) of a metal contained in the material to be protected from corrosion, can be detected using cyclic voltammetry. In this case, cyclic voltammetry can be used to determine which redox reaction takes place and to what extent. If it is determined that only the at least one reducing agent orIf at least one complexing agent acting as a reducing agent is oxidized, whereas the metal contained in the material to be protected from corrosion is not oxidized, this is clear evidence that the aforementioned feature is met. For example, a voltage sweep (scan rate) of 20 mV / s and a 3-electrode system can be used, whereby the measurement can be carried out, for example, at a temperature of 25 °C and / or, for example, in an aqueous NaCl solution with an NaCl content of 3.5 wt.%, based on the total mass of the solution, and / or a pH of 7; or an aqueous sodium tetraborate / boric acid buffer solution with a sodium tetraborate / boric acid buffer content of 3.5 wt.%, based on the total mass of the solution, and / or a pH of 8.5.
[0086] Cyclic voltammetry is used to track electrochemical (redox) reactions under specific conditions. A potential range (both anodic - oxidative and cathodic - reductive directions) is scanned, and the current is measured as a function of the potential. This can be understood as a non-stationary state, where the different reactions manifest themselves as "current peaks": the individual peaks are characteristic of a specific reaction, with the location of the peak providing a qualitative statement (i.e., which reaction? which substance?) and the height of the peak providing a quantitative statement (i.e., how intense is the reaction?). If the appearance of certain peaks can be used to determine the dissolution of aluminum and the oxygen reduction reaction in the case of an uncoated sample, but for the coated sample, these peaks disappear and others appear (e.g.,the peaks for the added metal-containing ion and / or the peaks for the reducing agent or the complexing agent acting as a reducing agent), this is clear evidence that these substances in the coating (i.e. the metal-containing ion and / or the reducing agent or the complexing agent acting as a reducing agent) are the actual reactants (of the ongoing redox process), while the corrosion processes (i.e. corrosion of the substrate material to be protected from corrosion) are suppressed and thus the metal contained in the material to be protected from corrosion is not oxidized. Such measurements are usually carried out under defined conditions, e.g. 3.5% (w / w) NaCl solution (or sodium tetraborate / boric acid buffer, pH 8.5), 25 °C, 20 mV / s voltage sweep (scan rate), 3-electrode system.
[0087] The feature that the at least one reducing agent or the at least one complexing agent acting as a reducing agent is the reduced form of a redox pair which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a lower (or more negative) redox potential in this aqueous solution than the redox pair(s) of a metal contained in the material to be protected from corrosion, is to be understood that the at least one reducing agent or the at least one complexing agent acting as a reducing agent is the reduced form of a redox pair which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a redox potential in this aqueous solution which is lower (or more negative).more negative) than the redox potential of the redox couple or the redox potentials of the redox couples of a (preferably each) metal contained in the material to be protected from corrosion (which is in contact with this aqueous solution).
[0088] Preferably, the at least one metal-containing ion contains at least one metal which is the oxidized form of a (corresponding) redox pair which, upon contact of an aqueous solution (e.g. an aqueous salt solution or an aqueous buffer solution) with a coating produced with the coating mixture (on a substrate made of the material to be protected against corrosion), has a higher (or more positive) redox potential in this aqueous solution (preferably at a temperature of 5 °C to 50 °C, e.g. at a temperature of 25 °C) than the (corresponding) redox pair O2 / H2O and / or the (corresponding) redox pair Ch / OH (depending on the pH value), and / or can form a metal hydroxide and / or metal oxide layer with hydroxide anions and / or oxide anions.upon contact of an aqueous solution with a coated substrate prepared with the coating mixture containing hydroxide anions and / or oxide anions, a metal hydroxide and / or metal oxide layer is formed).
[0089] The aqueous salt solution can preferably have a salt content of 0.1 wt.% to 20 wt.%, preferably from 0.5 wt.% to 15 wt.% (e.g. a salt content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 3 to 11, preferably from 5 to 9 (e.g. a pH of 7). For example, the aqueous salt solution can be an aqueous NaCl solution, which preferably has an NaCl content of 0.1 wt.% to 20 wt.%, preferably from 0.5 wt.% to 15 wt.% (e.g. a NaCl content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 3 to 11, preferably from 5 to 9 (e.g. a pH of 7).
[0090] The aqueous buffer solution may preferably have a buffer content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a buffer content of 3.5 wt.%), based on the total mass of the solution, and / or a pH value of 7 to 10, preferably of 8 to 9 (e.g. a pH value of 8.5). For example, the aqueous buffer solution can be an aqueous sodium tetraborate / boric acid buffer solution which preferably has a sodium tetraborate / boric acid buffer content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a sodium tetraborate / boric acid buffer content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 7 to 10, preferably of 8 to 9 (e.g. a pH of 8.5).
[0091] The characteristic that the metal contained in the at least one metal-containing ion is the oxidized form of a redox couple, which, upon contact of an aqueous solution with a coating produced with the coating mixture (on a substrate made of the material to be protected from corrosion), has a higher (or more positive) redox potential in this aqueous solution than the redox couple O2 / H2O and / or the redox couple Ch / OH (depending on the pH value), can be demonstrated using cyclic voltammetry. Cyclic voltammetry can be used to determine which redox reaction occurs and to what extent. If it is determined that only the metal contained in the at least one metal-containing ion is reduced, whereas oxygen is not, this is clear evidence that the aforementioned characteristic is met. For example, a voltage sweep (scan rate) of 20 mV / s and a 3-electrode system can be used, whereby the measurement can be carried out, for example,at a temperature of 25 °C and / or e.g. in an aqueous NaCl solution with an NaCl content of 3.5 wt.%, based on the total mass of the solution, and / or a pH of 7; or an aqueous sodium tetraborate / boric acid buffer solution with a sodium tetraborate / boric acid buffer content of 3.5 wt.%, based on the total mass of the solution, and / or a pH of 8.5.
[0092] Preferably, the at least one metal-containing ion is at least one metal cation, at least one (metal) oxoanion, or a mixture (or combination) of at least one metal cation and at least one (metal) oxoanion.
[0093] Preferably, the at least one metal-containing ion comprises a metal that can assume several, preferably at least three, particularly preferably at least four, positive oxidation states. Particularly preferably, the at least one metal-containing ion is a (metal) oxoanion that comprises a metal that can assume several, preferably at least three, particularly preferably at least four, positive oxidation states.
[0094] Preferably, the at least one metal-containing ion contains no Cr(III) and no Cr(VI). Particularly preferably, the at least one metal-containing ion contains no chromium (i.e., no chromium in any oxidation state), in particular neither in the form of chromium cations nor in the form of chromium oxoanions or chromate.
[0095] The coating mixture according to the invention preferably contains no Cr(III) and no Cr(VI). The coating mixture according to the invention particularly preferably contains no chromium (ie, no chromium in any oxidation state), in particular neither in the form of chromium cations nor in the form of chromium oxoanions or chromate.
[0096] Preferably, the coating mixture according to the invention contains no toxic compounds, no chromium species, no fluorine-containing substances, and / or no phosphate-containing compounds.
[0097] Preferably, the at least one solvent is water, at least one oxygen-containing organic solvent, or a mixture of water and at least one oxygen-containing organic solvent.
[0098] The coating mixture can be in the form of a solution or a dispersion (e.g., suspension). Preferably, the coating mixture is in the form of a solution or colloidal solution.
[0099] The coating mixture according to the invention can be produced, for example, by mixing the individual components of the coating mixture to be produced with one another. With regard to the at least one silane, it should be noted that this can optionally be at least partially crosslinked to form at least one oligosiloxane during the production of the coating mixture. This can be achieved, for example, by setting an acidic pH in the mixture with an acid (e.g., acetic acid) during production, which promotes crosslinking, and by setting an alkaline pH in the mixture with a base (e.g., sodium carbonate) at the end of production, which stops crosslinking. Should the coating mixture contain a silane with an epoxy group, a catalyst (e.g., boron trifluoride etherate catalyst) can additionally be used to open the epoxy groups, i.e.added to the coating mixture during production.
[0100] A preferred embodiment of the coating mixture according to the invention is characterized in that the at least one silane comprises at least one first silane and at least one second silane, wherein the at least one first silane and the at least one second silane each have at least one, preferably at least two, particularly preferably at least three, alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, and wherein the at least one first silane and / or the at least one second silane each additionally has a group bonded to the Si atom, each of which is independently selected from the group consisting of alkyl groups having 1 to 4 carbon atoms, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups and combinations thereof, and alkoxyalkyl groups which may have one or more groups selected from amino groups, organosulfonyl groups,epoxy groups and combinations thereof, and / or the at least one silane is at least one functionalized silane, wherein the at least one silane is preferably functionalized with the at least one complexing agent, with the at least one reducing agent, and / or with a substance selected from the group consisting of phenol hydroxides, lactates, carboxylates, and combinations thereof.
[0101] At least one silane can be functionalized. Functionalized molecules can carry various functional groups, such as phenol hydroxides, lactates, and carboxylates, which are deprotonated at different, usually higher, pH values defined by pKa values. This means they can be counterions of various cations (salt formation). Furthermore, due to the various oxygen-containing functional groups, they are capable of forming complexes with cations; particularly important in this regard are iron, aluminum, and other alloying elements. Several multidentate functionalized molecules, arranged closely together at the molecular level, can even behave like cryptands, the term for a family of synthetic bicyclic and polycyclic multidentate ligands for complexing cations (used particularly in bioinorganic chemistry).
[0102] It is possible that the at least one complexing agent is partially functionalized to the at least one silane and partially separate (i.e., not functionalized to the at least one silane) in the coating mixture.
[0103] It is possible that the at least one reducing agent is partially functionalized to the at least one silane and partially separate (i.e., not functionalized to the at least one silane) in the coating mixture.
[0104] Preferably, the silane comprises a silane according to one of the following structural formulas (I) to (III) or several silanes according to one or more of the following structural formulas (I) to (III): where the R 1 , R 2 , R 3 and R 4 are each independently selected from the group consisting of methyl, ethyl, propyl and butyl.
[0105] A further preferred embodiment of the coating mixture according to the invention is characterized in that the at least one complexing agent is at least one complexing agent for complexing cations selected from the group consisting of aluminum cations, iron cations, copper cations, magnesium cations, zinc cations, chromium cations, manganese cations, and mixtures thereof, wherein the at least one complexing agent is preferably selected from the group consisting of Alizarin S (Alizarin Red); 2,2',2",2"'-(ethane-1,2-diyldinitrilo)tetraacetic acid (EDTA) and salts thereof; 2,2',2",2"'-[(1R,2R)-1,2-cyclohexanediyldinitrilo]tetraacetic acid (CDTA) and salts thereof; Ethylene glycol bis(ß-aminoethyl ether)-N,N,N',N'-tetraacetic acid (EGTA) and its salts; ascorbic acid ((5R)-[(1S)-1,2-dihydroxyethyl]-3,4-dihydroxyfuran-2(5H)-one) and its isomers, conjugates and salts; cyanic acid (1,3,5-triazinan-2,4,6-trione) and its isomers and salts;Tartaric acid (2,3-dihydroxysuccinic acid) and its isomers and salts; 1,4-dioxane; melamine (1,3,5-triazine-2,4,6-triamine) and its isomers and derivatives; thiourea; cysteine; and mixtures thereof, and / or the at least one complexing agent acting as a reducing agent is selected from the group consisting of ascorbic acid and its isomers, conjugates and salts; melamine; thiourea; cysteine; TI and its isomers and derivatives;and mixtures thereof, and / or the at least one reducing agent is selected from the group consisting of vanillin (4-hydroxy-3-methoxybenzaldehyde) and its isomers (e.g. isovaniline or 3-hydroxy-4-methoxybenzaldehyde) and homologues (e.g. ethylvanillin or 3-ethoxy-4-hydroxybenzaldehyde), bisulfites, sulphites, dithionites, glutathione, polyphenols, and mixtures thereof, and / or the at least one metal-containing ion is selected from the group consisting of alkali metal cations, alkaline earth metal cations, transition metal cations, lanthanide cations, oxoanions, and mixtures thereof, wherein the at least one metal-containing ion is preferably selected from the group consisting of cerium(III) cations, cerium(IV) cations, lithium cations, sodium cations, molybdenum oxoanions, manganese oxoanions, and mixtures thereof thereof, and / or the at least one solvent is selected from the group consisting of water; alcohols, preferably ethanol, isopropanol;Butyl acetate; fruit acid esters, and mixtures thereof, and / or the material to be protected against corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; copper; alloys comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; alloys comprising or consisting of copper and zinc; intermetallic phases comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon and mixtures thereof;Composite materials comprising or consisting of aluminum, iron and / or copper and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof; and mixtures thereof. The at least one complexing agent can preferably be selected from the group consisting of carboxylates; lactates; phenol hydroxides; crown ethers (e.g. 1,4-dioxane); Alizarin S (Alizarin Red); 2,2',2",2"'-(ethane-1,2-diyldinitrilo)tetraacetic acid (EDTA) and salts thereof; 2,2',2",2"'-[(lR,2R)-l,2-cyclohexanediyldinitrilo]tetraacetic acid (CDTA) and its salts; ethylene glycol bis(ß-aminoethyl ether)-N,N,N',N'-tetraacetic acid (EGTA) and its salts;Ascorbic acid ((5R)-[(1S)-1,2-dihydroxyethyl]-3,4-dihydroxyfuran-2(5H)-one) and its isomers, conjugates and salts; cyanic acid (1,3,5-triazinane-2,4,6-trione) and its isomers and salts; tartaric acid (2,3-dihydroxysuccinic acid) and its isomers and salts; 1,4-dioxane; melamine and its isomers and derivatives; and mixtures thereof.
[0106] The composite materials can, for example, be composite materials made of carbon fiber reinforced plastic (CFRP) with an integrated copper mesh.
[0107] According to a further preferred embodiment of the coating mixture according to the invention, the coating mixture contains
[0108] Nanoparticles, which are preferably selected from the group consisting of titanium oxide nanoparticles, tungsten oxide nanoparticles, aluminum oxide nanoparticles, silicon dioxide nanoparticles, and mixtures thereof, and / or at least one base, which is preferably selected from the group consisting of sodium carbonate, lithium carbonate, potassium carbonate, and mixtures thereof, and / or at least one additive selected from the group consisting of adhesion promoters, pigments, fillers, and mixtures thereof.
[0109] The at least one coating mixture may contain nanoparticles.
[0110] This can improve the appearance and / or printability of the coating produced.
[0111] Depending on the specific use of the coating mixture according to the invention, suitable additives (adhesion promoters, pigments, fillers) can be used to meet the specific needs of a particular application.
[0112] A further preferred embodiment of the coating mixture according to the invention is characterized in that the coating mixture
[0113] 5 wt.% to 60 wt.%, preferably 5 wt.% to 25 wt.%, of the at least one silane and / or of the at least one oligosiloxane, based on the total mass of the mixture, and / or
[0114] 100 ppm to 5000 ppm, preferably 100 ppm to 250 ppm, of the at least one complexing agent, based on the total mass of the mixture, and / or
[0115] 100 ppm to 5000 ppm, preferably 100 ppm to 250 ppm, of the at least one reducing agent, based on the total mass of the mixture, and / or
[0116] 1 to 100 ppm, preferably 5 to 10 ppm, of the at least one metal-containing ion, based on the total mass of the mixture, and / or
[0117] 100 ppm to 1000 ppm, preferably 100 ppm to 250 ppm, nanoparticles, based on the total mass of the mixture, and / or,
[0118] 100 ppm to 5000 ppm wt.%, preferably 100 ppm to 500 ppm wt.%, of at least one additive, based on the total mass of the mixture.
[0119] In addition, the present invention also relates to a method for producing coated substrates, in which a) at least one layer of a coating mixture according to one of the preceding claims is applied to at least one region of a surface of at least one substrate which contains or consists of material to be protected against corrosion, wherein the material to be protected against corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; copper; alloys containing iron, copper and / or aluminum; intermetallic phases containing iron, copper and / or aluminum; composite materials containing iron, copper and / or aluminum; and mixtures thereof, and b) the at least one applied layer is subjected to at least one curing process in which the at least one silane and / or the at least one oligosiloxane is crosslinked to form a (polysiloxane) xerogel.
[0120] A preferred variant of the method according to the invention is characterized in that the application of the at least one layer in step a) is carried out by means of at least one application process which is selected from the group consisting of dipping, doctor blade coating, rolling, spinning, spraying, brushing, painting, and combinations thereof, and / or the substrate is subjected to at least one pretreatment before step a), which is preferably selected from the group consisting of cleaning, sandblasting, polishing, degreasing, alkaline etching, acid etching, plasma treatment, laser treatment, and combinations thereof.
[0121] A further preferred variant of the method according to the invention is characterized in that the at least one curing process in step b) is carried out at a temperature of 60 °C to 120 °C, preferably from 70 °C to 100 °C, particularly preferably from 80 °C to 90 °C, and / or for a duration of 5 min to 8 h, preferably from 30 min to 4 h, particularly preferably from 45 min to 2 h.
[0122] According to a further preferred variant of the method according to the invention, the at least one layer is applied in a thickness of 500 nm to 800 nm. A further preferred variant of the method according to the invention is characterized in that the material to be protected against corrosion is selected from the group consisting of
[0123] aluminum; anodized aluminum;
[0124] Iron;
[0125] Copper;
[0126] Alloys comprising or consisting of
[0127] • Aluminium and / or iron, as well as
[0128] • at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof;
[0129] Alloys comprising or consisting of copper and zinc; intermetallic phases comprising or consisting of
[0130] • Aluminium and / or iron, as well as
[0131] • at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon and mixtures thereof;
[0132] Composite materials comprising or consisting of
[0133] • Aluminium, iron and / or copper, as well as
[0134] • at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof; as well as mixtures thereof.
[0135] A particularly preferred variant of the method according to the invention is characterized in that the material to be protected against corrosion is selected from the group consisting of aluminum; anodized aluminum;
[0136] Iron;
[0137] Copper;
[0138] Steel;
[0139] Alloys consisting of aluminum and at least one substance selected from the group consisting of copper, magnesium, iron, zinc, silicon, chromium, manganese, and mixtures thereof; preferably AI 2024-T3, AI 7075-T6, AIMgl, AIMg3, AI99.5 (EN AW 1050A), and mixtures thereof; intermetallic phases consisting of aluminum and at least one substance selected from the group consisting of copper, magnesium, iron, zinc, silicon, chromium, manganese, and mixtures thereof;
[0140] Alloys consisting of iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, and mixtures thereof; preferably low-alloy steel (E), steel 1.4301 (S), HDG steel (Z275); intermetallic phases consisting of iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, and mixtures thereof;
[0141] Alloys consisting of copper and zinc;
[0142] Composite materials consisting of aluminum and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof;
[0143] Composite materials consisting of iron and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof;
[0144] Composite materials consisting of copper and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber-reinforced plastics, glass fiber-reinforced plastics, and mixtures thereof; as well as mixtures thereof.
[0145] The composite materials can, for example, be composite materials made of carbon fiber reinforced plastic (CFRP) with an integrated copper mesh.
[0146] The at least one substrate is preferably at least one composite comprising a plurality of subcomponents, wherein at least one of the subcomponents consists of the material to be protected against corrosion. Particularly preferably, such at least one composite can have at least one subcomponent made of the material to be protected against corrosion (e.g. at least one subcomponent made of aluminum and / or at least one subcomponent made of steel) and at least one subcomponent made of at least one plastic, and optionally additionally at least one subcomponent made of at least one sealing material. The at least one plastic is preferably selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof.The at least one sealing material is preferably selected from the group consisting of polyurethane and 1K and 2K epoxy materials, in particular thermoplastic polyurethanes, polytetrafluoroethylene, acrylonitrile butadiene rubber, vulcanized rubber, and mixtures thereof. For example, the at least one composite can comprise at least one subcomponent made of a first material to be protected against corrosion (e.g., aluminum), at least one subcomponent made of a second material to be protected against corrosion (e.g., steel), and at least one subcomponent made of the at least one plastic, and optionally additionally at least one subcomponent made of the at least one sealing material.
[0147] Possible substrate materials include, for example, aluminum alloys of the 2000, 5000, 6000, and 7000 series, especially AA2024, AA7075, but also AlMg1, AlMg3, and Al99.5 compositions, as well as low-alloy steel, e.g., S355, DC04, and stainless steel, e.g., 1.4301. Of particular importance is the aluminum composition AA2024-T3, with its main alloying element copper (3.8–4.9%), which forms fine intermetallic particles (hardening precipitates, dispersoids, inclusions), essential for a high strength-to-weight ratio and good fatigue resistance in the aerospace industry. Intermetallic phases that initiate corrosion processes can lead to pitting and stress corrosion cracking (as they are active cathodic sites where the oxygen reduction reaction can take place).
[0148] The substrates to which the coatings according to the invention can be applied can have any shape: simple (metal) parts or complex, machined parts, and all geometric compositions thereof. Depending on the requirements of a particular industry, the substrates can be subjected to pretreatment before application of the coating according to the invention. The pretreatment can consist of mechanical steps, e.g., sandblasting, polishing, and also chemical steps. The latter can include degreasing techniques, alkaline and acid etching (pickling), alkaline conditioning using chemicals, and other commercial products approved and certified in the respective industry. Physical pretreatment methods are also conceivable, e.g., plasma or laser technologies.
[0149] Furthermore, the present invention also relates to a coated substrate comprising a metal-containing substrate which contains or consists of a material to be protected from corrosion, wherein the material to be protected from corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; copper; alloys containing iron, copper and / or aluminum; intermetallic phases containing iron, copper and / or aluminum; composite materials containing iron, copper and / or aluminum; and mixtures thereof, and at least one coating arranged on at least one region of a surface of the substrate containing a (polysiloxane) xerogel and at least one complexing agent for complexing cations of at least one metal contained in the material to be protected from corrosion, and at least one metal-containing ion,wherein the (polysiloxane) xerogel is formed (or produced) (by crosslinking) from at least one silane (and / or at least one oligosiloxane formed from the at least one silane), wherein the at least one silane has at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, and wherein the at least one complexing agent comprises at least one complexing agent (additionally) acting as a reducing agent, which is the reduced form of a (corresponding) redox couple which, upon contact of an aqueous solution (e.g., an aqueous salt solution or an aqueous buffer solution) with the at least one coating in this aqueous solution (preferably at a temperature of 5°C to 50°C, e.g., at a temperature of 25°C), has a lower redox potential than the (corresponding) redox couple(s) of a metal contained in the material to be protected from corrosion,preferably as the (corresponding) redox couple(s) of each metal contained in the material to be protected from corrosion, and / or the coating additionally contains at least one reducing agent which is the reduced form of a (corresponding) redox couple which, upon contact of an aqueous solution (e.g. an aqueous salt solution or an aqueous buffer solution) with the at least one coating in this aqueous solution (preferably at a temperature of 5 °C to 50 °C, e.g. at a temperature of 25 °C), has a lower redox potential than the (corresponding) redox couple(s) of a metal contained in the material to be protected from corrosion, preferably as the (corresponding) redox couple(s) of each metal contained in the material to be protected from corrosion.
[0150] The aqueous salt solution can (in both of the aforementioned cases) preferably have a salt content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a salt content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 3 to 11, preferably of 5 to 9 (e.g. a pH of 7). For example, the aqueous salt solution (in both of the aforementioned cases) can be an aqueous NaCl solution, which preferably has an NaCl content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a NaCl content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 3 to 11, preferably of 5 to 9 (e.g. a pH of 7).
[0151] The aqueous buffer solution may (in both of the above-mentioned cases) preferably have a buffer content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a buffer content of 3.5 wt.%), based on the total mass of the solution, and / or a pH value of 7 to 10, preferably of 8 to 9 (e.g. a pH value of 8.5). For example, the aqueous buffer solution (in both of the above-mentioned cases) may be an aqueous sodium tetraborate / boric acid buffer solution, which preferably has a sodium tetraborate / boric acid buffer content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a sodium tetraborate / boric acid buffer content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 7 to 10, preferably of 8 to 9 (e.g. a pH of 8.5).
[0152] The feature that the at least one reducing agent or the at least one complexing agent acting as a reducing agent is the reduced form of a redox couple, which, upon contact of an aqueous solution with the at least one coating in this aqueous solution, has a lower (or more negative) redox potential than the redox couple(s) of a metal contained in the material to be protected from corrosion, can be demonstrated using cyclic voltammetry. Cyclic voltammetry can be used to determine which redox reaction occurs and to what extent. If it is determined that only the at least one reducing agent or the at least one complexing agent acting as a reducing agent is oxidized, whereas the metal contained in the material to be protected from corrosion is not oxidized, this is clear evidence that the feature mentioned is met. For example,a voltage feed (scan rate) of 20 mV / s and a 3-electrode system are used, whereby the measurement can be carried out, for example, at a temperature of 25 °C and / or, for example, in an aqueous NaCl solution with an NaCl content of 3.5 wt.%, based on the total mass of the solution, and / or a pH of 7; or an aqueous sodium tetraborate / boric acid buffer solution with a sodium tetraborate / boric acid buffer content of 3.5 wt.%, based on the total mass of the solution, and / or a pH of 8.5.
[0153] The feature that the at least one reducing agent or the at least one complexing agent acting as a reducing agent is the reduced form of a redox pair which, upon contact of an aqueous solution with the at least one coating in this aqueous solution, has a lower (or more negative) redox potential than the redox potential(s) of a metal contained in the material to be protected against corrosion, is to be understood that the at least one reducing agent or the at least one complexing agent acting as a reducing agent is the reduced form of a redox pair which, upon contact of an aqueous solution with the at least one coating in this aqueous solution, has a redox potential which is lower (or more negative) than the redox potential of the redox pair orthe redox potentials of the redox pairs of one (preferably each) metal contained in the material to be protected from corrosion (which is in contact with this aqueous solution).
[0154] A preferred embodiment of the coated substrate according to the invention is characterized in that the at least one complexing agent and / or the at least one reducing agent is / are covalently bound to the (polysiloxane) xerogel and / or is / are adsorbed to the (polysiloxane) xerogel. A further preferred embodiment of the coated substrate according to the invention is characterized in that the at least one metal-containing ion contains at least one metal which is the oxidized form of a (corresponding) redox pair which, upon contact of an aqueous solution (e.g. an aqueous salt solution or an aqueous buffer solution) with the at least one coating, in this aqueous solution (preferably at a temperature of 5 °C to 50 °C, e.g. at a temperature of 25 °C), has a higher (ormore positive) redox potential than the (corresponding) redox pair O2 / H2O and / or the (corresponding) redox pair Ch / OI-r (depending on the pH value), and / or can form a metal hydroxide and / or metal oxide layer with hydroxide anions and / or oxide anions (or forms a metal hydroxide and / or metal oxide layer upon contact of an aqueous solution with a coated substrate produced with the coating mixture with hydroxide anions and / or oxide anions).
[0155] The aqueous salt solution can preferably have a salt content of 0.1 wt.% to 20 wt.%, preferably from 0.5 wt.% to 15 wt.% (e.g. a salt content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 3 to 11, preferably from 5 to 9 (e.g. a pH of 7). For example, the aqueous salt solution can be an aqueous NaCl solution, which preferably has an NaCl content of 0.1 wt.% to 20 wt.%, preferably from 0.5 wt.% to 15 wt.% (e.g. a NaCl content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 3 to 11, preferably from 5 to 9 (e.g. a pH of 7).
[0156] The aqueous buffer solution may preferably have a buffer content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a buffer content of 3.5 wt.%), based on the total mass of the solution, and / or a pH value of 7 to 10, preferably of 8 to 9 (e.g. a pH value of 8.5). For example, the aqueous buffer solution can be an aqueous sodium tetraborate / boric acid buffer solution which preferably has a sodium tetraborate / boric acid buffer content of 0.1 wt.% to 20 wt.%, preferably of 0.5 wt.% to 15 wt.% (e.g. a sodium tetraborate / boric acid buffer content of 3.5 wt.%), based on the total mass of the solution, and / or a pH of 7 to 10, preferably of 8 to 9 (e.g. a pH of 8.5).
[0157] The feature that the metal contained in the at least one metal-containing ion is the oxidized form of a redox couple, which, upon contact of an aqueous solution with the at least one coating in this aqueous solution, has a higher (or more positive) redox potential than the O2 / H2O redox couple and / or the CH / OH redox couple (depending on the pH value), can be detected using cyclic voltammetry. Cyclic voltammetry can be used to determine which redox reaction occurs and to what extent. If it is determined that only the metal contained in the at least one metal-containing ion is reduced, whereas oxygen is not reduced, this is clear evidence that the aforementioned feature is met. For example, a voltage sweep (scan rate) of 20 mV / s and a 3-electrode system can be used, with the measurement being carried out, for example, at a temperature of 25 °C and / orin an aqueous NaCl solution with an NaCl content of 3.5 wt.%, based on the total mass of the solution, and / or a pH of 7; or an aqueous sodium tetraborate / boric acid buffer solution with a sodium tetraborate / boric acid buffer content of 3.5 wt.%, based on the total mass of the solution, and / or a pH of 8.5.
[0158] A further preferred embodiment of the coated substrate according to the invention is characterized in that the (polysiloxane) xerogel is formed (or is formed) (by crosslinking) from at least one silane (and / or at least one oligosiloxane formed from the at least one silane).manufactured), wherein the at least one silane is functionalized and / or has at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, wherein the at least one silane preferably has at least one group bonded to the Si atom, each of which is independently selected from the group consisting of alkyl groups having 1 to 4 carbon atoms, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups and combinations thereof, and alkoxyalkyl groups, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups and combinations thereof, and / or the material to be protected from corrosion is selected from the group consisting of.
[0159] • Aluminum;
[0160] • anodized aluminum;
[0161] • Iron;
[0162] • Copper;
[0163] • Alloys comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof;
[0164] • Alloys comprising or consisting of copper and zinc;
[0165] • intermetallic phases comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon and mixtures thereof;
[0166] • Composite materials comprising or consisting of aluminum, iron and / or copper and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof;
[0167] • and mixtures thereof, and / or the at least one complexing agent is at least one complexing agent for complexing cations selected from the group consisting of aluminum cations, iron cations, copper cations, magnesium cations, zinc cations, chromium cations, manganese cations, silicon cations, and mixtures thereof, wherein the at least one complexing agent is preferably selected from the group consisting of Alizarin S; 2,2',2",2"'-(ethane-1,2-diyldinitrilo)tetraacetic acid and salts thereof; 2,2',2",2"'-[(1R,2R)-1,2-cyclohexanediyldinitrilo]tetraacetic acid and salts thereof; ethylene glycol bis(ß-aminoethyl ether)-N,N,N',N'-tetraacetic acid and salts thereof; ascorbic acid and isomers, conjugates and salts thereof; Cyanic acid and its isomers and salts; tartaric acid and its isomers and salts; 1,4-dioxane; melamine and its isomers and derivatives; thiourea; cysteine;and mixtures thereof, and / or the at least one complexing agent acting as a reducing agent is selected from the group consisting of ascorbic acid and its isomers, conjugates and salts; melamine and its isomers and derivatives; thiourea; cysteine; and mixtures thereof, and / or the at least one reducing agent is selected from the group consisting of vanillin and its isomers and homologues, bisulfites, sulphites, dithionites, glutathione, polyphenols, and mixtures thereof, and / or the at least one metal-containing ion is selected from the group consisting of alkali metal cations, alkaline earth metal cations, transition metal cations, lanthanide cations, and mixtures thereof, preferably selected from cerium(II) cations, cerium(IV) cations, lithium cations, sodium cations, molybdenum oxoanions, manganese oxoanions, and mixtures thereof.;
[0168] Particularly preferably, the material to be protected against corrosion is selected from the group consisting of
[0169] aluminum; anodized aluminum
[0170] Iron;
[0171] copper; steel;
[0172] Alloys consisting of aluminum and at least one substance selected from the group consisting of copper, magnesium, iron, zinc, silicon, chromium, manganese, and mixtures thereof; preferably AI 2024-T3, AI 7075-T6, AIMgl, AIMg3, AI99.5 (EN AW 1050A), and mixtures thereof; intermetallic phases consisting of aluminum and at least one substance selected from the group consisting of copper, magnesium, iron, zinc, silicon, chromium, manganese, and mixtures thereof;
[0173] Alloys consisting of iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, and mixtures thereof; preferably low-alloy steel (E), steel 1.4301 (S), HDG steel (Z275); intermetallic phases consisting of iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, and mixtures thereof;
[0174] Alloys consisting of copper and zinc;
[0175] Composite materials consisting of aluminum and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof;
[0176] Composite materials consisting of iron and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof;
[0177] Composite materials consisting of copper and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber-reinforced plastics, glass fiber-reinforced plastics, and mixtures thereof; as well as mixtures thereof.
[0178] The composite materials can, for example, be composite materials made of carbon fiber reinforced plastic (CFRP) with an integrated copper mesh.
[0179] The metal-containing substrate is preferably a composite comprising a plurality of subcomponents, at least one of the subcomponents consisting of the material to be protected against corrosion. Such a composite can particularly preferably comprise at least one subcomponent made of the material to be protected against corrosion (e.g. at least one subcomponent made of aluminum and / or at least one subcomponent made of steel) and at least one subcomponent made of at least one plastic, and optionally additionally at least one subcomponent made of at least one sealing material. The at least one plastic is preferably selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof.The at least one sealing material is preferably selected from the group consisting of polyurethane and 1K and 2K epoxy materials, in particular thermoplastic polyurethanes, polytetrafluoroethylene, acrylonitrile butadiene rubber, vulcanized rubber, and mixtures thereof. For example, the composite can comprise at least one subcomponent made of a first material to be protected against corrosion (e.g., aluminum), at least one subcomponent made of a second material to be protected against corrosion (e.g., steel), and at least one subcomponent made of the at least one plastic, and optionally additionally at least one subcomponent made of the at least one sealing material.
[0180] A further preferred embodiment of the coated substrate according to the invention is characterized in that the at least one coating is a single layer, a multi-layer, a part of a multi-layer system in combination with at least one further coating, a primer, a conversion coating, a clear coat, or a combination thereof.
[0181] A further preferred embodiment of the coated substrate according to the invention is characterized in that the coated substrate can be produced or is produced by the method according to the invention.
[0182] Preferably, the at least one coating of the coated substrate according to the invention contains no Cr(III) and no Cr(VI). Particularly preferably, the at least one coating of the coated substrate according to the invention contains no chromium (i.e., no chromium in any oxidation state), in particular neither in the form of chromium cations nor in the form of chromium oxoanions or chromate. This can be achieved by producing the coating with a coating mixture that contains no Cr(III) and no Cr(VI), preferably no chromium (i.e., no chromium in any oxidation state), in particular neither in the form of chromium cations nor in the form of chromium oxoanions or chromate.
[0183] It should be noted that after extended use of the coated substrate, any chromium contained in the substrate material may dissolve from the substrate material and enter the coating, so that the coating would then still contain minimal amounts of chromium, even if it was produced with a coating mixture that does not contain chromium. However, since chromium dissolves from the substrate material (and can then enter the coating) much later than other components of the substrate material for thermodynamic reasons, minimal amounts of chromium would only be present in the coating after a very long period of use of the coated substrate.
[0184] Preferably, the at least one coating of the coated substrate according to the invention can be produced or is produced with a coating mixture that contains no Cr(III) and no Cr(VI). Particularly preferably, the at least one coating of the coated substrate according to the invention can be produced or is produced with a coating mixture that contains no chromium (ie, no chromium in any oxidation state), in particular neither in the form of chromium cations nor in the form of chromium oxoanions or chromate.
[0185] According to a further preferred embodiment of the coated substrate according to the invention, the at least one coating has a thickness of 500 nm to 800 nm.
[0186] The present invention also relates to the use of a coated substrate according to the invention as a component in the aerospace industry, in the automotive industry, in shipbuilding, and in precision engineering.
[0187] The present invention can be applied in various fields, for example in one or more of the following fields:
[0188] Corrosion protection of structural steel
[0189] Corrosion protection of alloyed steel
[0190] Corrosion protection of (hot-) galvanized steel
[0191] Corrosion protection of aluminum for the aviation industry
[0192] Corrosion protection of aluminum for other industries, possible substitution of anodizing
[0193] Corrosion protection of multi-material systems (e.g. composites of several metals, sealing materials, plastics)
[0194] Adhesion promoting in composite materials
[0195] Compensation interface in composites when combining materials with non-conforming material parameters, e.g., thermal expansion coefficient, electrical and ionic conductivity, magnetic susceptibility
[0196] Digital printing of metallic substrates with typical water-based printing inks In the aviation industry, the coatings according to the invention are conceivable, for example, for aircraft made of carbon fiber reinforced polymers with integrated copper mesh as lightning protection.
[0197] The coating of the coated substrate according to the invention can have the following advantageous properties:
[0198] - very small pore size
[0199] - very thin layers (thickness similar to that of typical conversion coatings) possible, e.g. 500 nm to 800 nm
[0200] - Dense layer with granular morphology; very good adhesion, particles remain on the surface after fracture (cryogenic fracture)
[0201] - Excellent corrosion resistance
[0202] - Improved mechanical resistance
[0203] - Excellent adhesion to all metal surfaces as well as to all underlying or overlying coatings
[0204] -> increased compatibility with typical coatings in the automotive and aerospace industries
[0205] -> Any combination with common compositions of basecoats, topcoats is conceivable to form multi-layer systems or hybrid systems or sandwich structures or composite structures
[0206] Diffusion barrier effect for water and other corrosive substances
[0207] Possibility of painting, gluing, printing
[0208] Possibility of chemically controlled (active) corrosion protection (a type of self-healing) low inspection and repair requirements
[0209] The formation of the siloxane polymers or polysiloxane xerogel, ie the sol-gel process, can be monitored using Fourier transform infrared spectroscopy.
[0210] The concentration of the meta II ions present can be determined by inductively coupled plasma optical emission spectroscopy, where the solutions are analyzed based on their spectral lines.
[0211] Bound complexing agents and / or reducing agents can be determined by measuring the residue in the solution by titration or other specific analytical methods.
[0212] The morphology, structure, coverage, and adhesion strength of the substrate can be determined using scanning electron microscopy on fractured samples (cryogenic fracture). Adhesion can be further analyzed using cross-cut testing according to DIN EN ISO 2409:2020.
[0213] To determine corrosion inhibition / protection properties (or corrosion resistance), the salt spray test (or neutral salt spray test) according to DIN EN ISO 9227:2017 or DIN EN ISO 9227:2022 can be used. During the test, the specimens are placed in a chamber in which a 5 wt% NaCl solution is continuously sprayed at a temperature of 35 °C. The mist condenses on the specimen surfaces and has a corrosive effect. The test duration is selected based on the expected corrosion resistance of the material or coating. The specimens are visually inspected at regular intervals for initial signs of corrosion. If no corrosion occurs after the specified time, sufficient corrosion protection can be assumed. The process of anodic infiltration and cathodic delamination can be investigated if a blade cut is also performed on the coating before the test begins.
[0214] The scanning Kelvin probe can be used to investigate active protection mechanisms, i.e. whether limited corrosion occurs even in the event of layer damage, compared to a coating where only passive effects are assumed. Cathodic delamination and anodic infiltration are the most common failure mechanisms of a metal-polymer bond in corrosive atmospheres and when exposed to corrosive electrolyte solutions and are described in detail. There are several techniques for investigating them, which are recommended by Stratman et al. The scanning Kelvin probe has proven to be the most powerful tool for understanding the complexity of all the processes taking place. In contrast to conventional electrochemical techniques, the scanning Kelvin probe is a local electrochemical measurement method for determining the potential distribution on a surface, e.g., a metal or polymer-metal interface.
[0215] Electrochemical measurements, i.e., open circuit potential, potentiodynamic measurements, and electrochemical impedance spectroscopic studies can be performed to evaluate the corrosion protection capabilities of the present inventive coating in comparison to uncoated samples or other types of coatings.
[0216] The determination of water absorption can be carried out, for example, using electrochemical impedance spectroscopy.
[0217] Raman spectroscopy can be used to determine and qualitatively analyze precipitates and molecules (as protective agents or corrosion products) directly on the surface.
[0218] The present invention also relates to the following aspects:
[0219] Aspect 1
[0220] Coating mixture for coating substrates made of material to be protected from corrosion, selected from the group consisting of aluminum, iron, alloys containing iron and / or aluminum, intermetallic phases containing iron and / or aluminum, and mixtures thereof, wherein the coating mixture contains at least one silane and / or at least one oligosiloxane formed from the at least one silane, at least one complexing agent for complexing cations of at least one metal contained in the material to be protected from corrosion, at least one metal-containing ion, and at least one solvent, wherein the at least one silane has at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, and wherein the at least one complexing agent comprises at least one complexing agent acting as a reducing agent, which is the reduced form of a redox couple,which, upon contact of an aqueous solution with a coating produced with the coating mixture, has a lower redox potential in this aqueous solution than the redox pair(s) of a metal contained in the material to be protected from corrosion, and / or the coating mixture additionally contains at least one reducing agent which is the reduced form of a redox pair which, upon contact of an aqueous solution with a coating produced with the coating mixture, has a lower redox potential in this aqueous solution than the redox pair(s) of a metal contained in the material to be protected from corrosion.
[0221] Aspect 2 Coating mixture according to the preceding aspect, characterized in that the at least one silane comprises at least one first silane and at least one second silane, wherein the at least one first silane and the at least one second silane each have at least one alkoxy group bonded to the Si atom having 1 to 4 carbon atoms, and wherein the at least one first silane and / or the at least one second silane each additionally has a group bonded to the Si atom, each of which is independently selected from the group consisting of alkyl groups having 1 to 4 carbon atoms, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups, and combinations thereof, and alkoxyalkyl groups, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups, and combinations thereof,and / or the at least one silane is at least one functionalized silane, wherein the at least one silane is preferably functionalized with the at least one complexing agent, with the at least one reducing agent, and / or with a substance selected from the group consisting of phenol hydroxides, lactates, carboxylates, and combinations thereof.
[0222] Aspect 3
[0223] Coating mixture according to one of the preceding aspects, characterized in that the at least one complexing agent is at least one complexing agent for complexing cations selected from the group consisting of aluminum cations, iron cations, copper cations, magnesium cations, zinc cations, chromium cations, manganese cations, and mixtures thereof, wherein the at least one complexing agent is preferably selected from the group consisting of Alizarin S; 2,2',2",2"'-(ethane-1,2-diyldinitrilo)tetraacetic acid and salts thereof;
[0224] 2,2',2",2"'-[(lR,2R)-l,2-cyclohexanediyldinitrilo]tetraacetic acid and its salts; ethylene glycol bis(ß-aminoethyl ether)-N,N,N',N'-tetraacetic acid and its salts; ascorbic acid and its isomers, conjugates and salts; cyanic acid and its isomers and salts; tartaric acid and its isomers and salts; 1,4-dioxane; melamine and its isomers and derivatives; thiourea; cysteine; and mixtures thereof, and / or the at least one complexing agent acting as a reducing agent is selected from the group consisting of ascorbic acid and its isomers, conjugates and salts; melamine and its isomers and derivatives; thiourea; cysteine;and mixtures thereof, and / or the at least one reducing agent is selected from the group consisting of vanillin and its isomers and homologues, bisulfites, sulphites, dithionites, glutathione, polyphenols, and mixtures thereof, and / or the at least one metal-containing ion is selected from the group consisting of alkali metal cations, alkaline earth metal cations, transition metal cations, lanthanide cations, oxoanions, and mixtures thereof, wherein the at least one metal-containing ion is preferably selected from the group consisting of cerium(III) cations, cerium(IV) cations, lithium cations, sodium cations, molybdenum oxoanions, manganese oxoanions, and mixtures thereof, and / or the at least one solvent is selected from the group consisting of water; alcohols, preferably ethanol, isopropanol; butyl acetate;Fruit acid esters, and mixtures thereof, and / or the material to be protected from corrosion is selected from the group consisting of aluminum; iron; alloys comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; intermetallic phases comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon and mixtures thereof; and mixtures thereof.
[0225] Aspect 4
[0226] Coating mixture according to one of the preceding aspects, characterized in that the coating mixture
[0227] Nanoparticles, which are preferably selected from the group consisting of titanium oxide nanoparticles, tungsten oxide nanoparticles, aluminum oxide nanoparticles, silicon dioxide nanoparticles, and mixtures thereof, and / or at least one base, which is preferably selected from the group consisting of sodium carbonate, lithium carbonate, potassium carbonate, and mixtures thereof, and / or at least one additive selected from the group consisting of adhesion promoters, pigments, fillers, and mixtures thereof.
[0228] Aspect 5
[0229] Coating mixture according to one of the preceding aspects, characterized in that the coating mixture contains 5 wt.% to 60 wt.%, preferably 5 wt.% to 25 wt.%, of the at least one silane and / or of the at least one oligosiloxane, based on the total mass of the mixture, and / or
[0230] 100 ppm to 5000 ppm, preferably 100 ppm to 250 ppm, of the at least one complexing agent, based on the total mass of the mixture, and / or
[0231] 100 ppm to 5000 ppm, preferably 100 ppm to 250 ppm, of the at least one reducing agent, based on the total mass of the mixture, and / or
[0232] 1 to 100 ppm, preferably 5 to 10 ppm, of the at least one metal-containing ion, based on the total mass of the mixture, and / or
[0233] 100 ppm to 1000 ppm, preferably 100 ppm to 250 ppm, nanoparticles, based on the total mass of the mixture, and / or,
[0234] 100 ppm to 5000 ppm wt.%, preferably 100 ppm to 500 ppm wt.%, of at least one additive, based on the total mass of the mixture.
[0235] Aspect 6
[0236] A method for producing coated substrates, in which a) at least one layer of a coating mixture according to one of the preceding aspects is applied to at least one region of a surface of at least one substrate made of material to be protected from corrosion selected from the group consisting of aluminum, iron, alloys containing iron and / or aluminum, intermetallic phases containing iron and / or aluminum, and mixtures thereof, and b) the at least one applied layer is subjected to at least one curing process in which the at least one silane and / or the at least one oligosiloxane is / are crosslinked to form a xerogel.
[0237] Aspect 7 Method according to aspect 6, characterized in that the application of the at least one layer in step a) takes place by means of at least one application process which is selected from the group consisting of dipping, doctor blade coating, rolling, spinning, spraying, brushing, painting, and combinations thereof, and / or the substrate is subjected to at least one pretreatment before step a), which is preferably selected from the group consisting of cleaning, sandblasting, polishing, degreasing, alkaline etching, acid etching, plasma treatment, laser treatment, and combinations thereof.
[0238] Aspect 8
[0239] Method according to aspect 6 or 7, characterized in that the at least one curing process in step b) takes place at a temperature of 60 °C to 120 °C, preferably from 70 °C to 100 °C, particularly preferably from 80 °C to 90 °C, and / or for a duration of 5 min to 8 h, preferably from 30 min to 4 h, particularly preferably from 45 min to 2 h.
[0240] Aspect 9
[0241] Method according to one of aspects 6 to 8, characterized in that the material to be protected against corrosion is selected from the group consisting of
[0242] Aluminum;
[0243] Iron;
[0244] Alloys comprising or consisting of
[0245] • Aluminium and / or iron, as well as
[0246] • at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; intermetallic phases comprising or consisting of
[0247] • Aluminum and / or iron, as well as at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon and mixtures thereof; as well as mixtures thereof.
[0248] Aspect 10
[0249] A coated substrate comprising a metal-containing substrate made of a material to be protected from corrosion selected from the group consisting of aluminum, iron, alloys containing iron and / or aluminum, intermetallic phases containing iron and / or aluminum, and mixtures thereof, and at least one coating arranged on at least one area of a surface of the substrate, containing a xerogel and at least one complexing agent for complexing cations of at least one metal contained in the material to be protected from corrosion, and at least one metal-containing ion, wherein the xerogel is formed from at least one silane having at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, and wherein the at least one complexing agent comprises at least one complexing agent acting as a reducing agent, which is the reduced form of a redox couple,which, upon contact of an aqueous solution with the at least one coating, has a lower redox potential in this aqueous solution than the redox couple(s) of a metal contained in the material to be protected from corrosion, and / or the coating additionally contains at least one reducing agent which is the reduced form of a redox couple which, upon contact of an aqueous solution with the at least one coating in this aqueous solution, has a lower redox potential than the redox couple(s) of a metal contained in the material to be protected from corrosion. Aspect 11,
[0250] Coated substrate according to aspect 10, characterized in that the at least one complexing agent and / or the at least one reducing agent is / are covalently bound to the xerogel and / or is / are adsorbed to the xerogel.
[0251] Aspect 12
[0252] Coated substrate according to aspect 10 or 11, characterized in that the xerogel is formed from at least one silane which is functionalized and / or has at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, wherein the at least one silane preferably has at least one group bonded to the Si atom, each of which is independently selected from the group consisting of alkyl groups having 1 to 4 carbon atoms, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups and combinations thereof, and alkoxyalkyl groups which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups and combinations thereof, and / or the material to be protected against corrosion is selected from the group consisting of aluminum; iron;Alloys comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; intermetallic phases comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; and mixtures thereof, and / or the at least one complexing agent is at least one complexing agent for complexing cations selected from the group consisting of aluminum cations, iron cations, copper cations, magnesium cations, zinc cations, chromium cations, manganese cations, silicon cations, and mixtures thereof, wherein the at least one complexing agent is preferably selected from the group consisting of Alizarin S; 2,2',2",2"'-(ethane-1,2-diyldinitrilo)tetraacetic acid and salts thereof;2,2',2",2"'-[(lR,2R)-l,2-cyclohexanediyldinitrilo]tetraacetic acid and salts thereof; ethylene glycol bis(ß-aminoethyl ether)-N,N,N',N'-tetraacetic acid and salts thereof; ascorbic acid and isomers, conjugates and salts thereof; cyanic acid and isomers and salts thereof; tartaric acid and isomers and salts thereof; 1,4-dioxane; melamine and its isomers and derivatives; thiourea; cysteine; and mixtures thereof, and / or the at least one complexing agent acting as a reducing agent is selected from the group consisting of ascorbic acid and its isomers, conjugates and salts; melamine and its isomers and derivatives; thiourea; cysteine;and mixtures thereof, and / or the at least one reducing agent is selected from the group consisting of vanillin and its isomers and homologues, bisulfites, sulphites, dithionites, glutathione, polyphenols, and mixtures thereof, and / or the at least one metal-containing ion is selected from the group consisting of alkali metal cations, alkaline earth metal cations, transition metal cations, lanthanide cations, and mixtures thereof, preferably selected from cerium(lII) cations, cerium(IV) cations, lithium cations, sodium cations, molybdenum oxoanions, manganese oxoanions, and mixtures thereof.;
[0253] Aspect 13
[0254] Coated substrate according to any one of aspects 10 to 12, characterized in that the at least one coating is a single layer, a multilayer, a part of a multilayer system in combination with at least one further coating, a primer, a conversion coating, a clearcoat layer, or a combination thereof. Aspect 14
[0255] Coated substrate according to one of aspects 10 to 13, characterized in that the coated substrate can be produced or is produced by a method according to one of aspects 6 to 9.
[0256] Aspect 15
[0257] Use of a coated substrate according to any one of aspects 10 to 14 as a component in the aerospace industry, in the automotive industry, in shipbuilding, in precision engineering.
[0258] The present invention is explained in more detail with reference to the following figures and examples, without limiting the invention to the specifically illustrated parameters.
[0259] Example 1
[0260] To explain the invention in more detail, we focus, as an example, on the support material AA2024-T3 with an Alizarin S-functionalized (3-glycidyloxypropyl)trimethoxysilane (GPTMS) coating with cerium(III) ions and cerium(IV) ions, ascorbic acid and sodium carbonate (the latter being used to stop the synthesis process by shifting the pH value into the alkaline range).
[0261] Preparation of the coating mixture:
[0262] All chemicals were purchased from Merck (Sigma-Aldrich), and the purity of the chemicals is the highest available unless otherwise stated. In this example, 400 ml of deionized water is taken and 79.2 ml of GPTMS (3-glycidyloxypropyl)trimethoxysilane and 39.6 ml of tetraethylorthosilicate are added. 25 ml of 1 mol-l 1Acetic acid solution is added. The solution initially appears slightly cloudy, but then quickly becomes colorless and clear. It is allowed to stand on a stir plate for 30 minutes. In a separate, smaller container, 80 ml of deionized water is mixed with 4.104 g of Alizarin S. This is also magnetically stirred for 15 minutes. The solution is homogeneous and has an amber color. In a separate container, 7.2 ml of boron trifluoride etherate catalyst is dispersed in 120 ml of water. After the first and second solutions have been stirred for the required time, the Alizarin S dispersion is first added to the GPTMS solution, followed by the boron trifluoride etherate dispersion as catalyst. Next, 10 mg of Ce(III) nitrate, 10 mg of Ce(IV) nitrate, and 1 g of L-ascorbic acid are added. The reaction is allowed to run for one hour with constant stirring.After one hour, we add sodium carbonate to the solution in small increments while monitoring the pH until it reaches 7. At this point, the solution should be clear and have a deep amber color. We strain the solution and then add 117.6 ml of ethanol. The approximately 800 ml of solution can now be diluted 1:5 with distilled water and used to coat surfaces.
[0263] Production of the coated substrate:
[0264] The starting substrate was an aluminum alloy with copper-containing intermetallic phases (substrate material: AA2024-T3). Pretreatment consisted of degreasing, alkaline etching, and acid etching (pickling) of the substrate to be coated, with a rinsing process with distilled water between each step. After pretreatment, the coating process was carried out using the coating mixture prepared as described above.
[0265] The exact steps in detail in the order applied:
[0266] Degrease the substrate (substrate material: AA2024) by immersing the substrate in distilled water + ENPREP 144 (60 g / l, McDermid, Inc.) at 60 °C for 15 min
[0267] Rinsing by immersing the substrate in distilled water for 5 min Alkaline etching by immersing the substrate in distilled water + 10% NaOH at 60 °C for 1 min
[0268] Rinsing by immersing the substrate in distilled water for 5 min Acid etching (pickling) by immersing the substrate in distilled water + 22% HNO3 + 15% Alfideox 79 (Alufinish GmbH & Co. KG) at room temperature for 10 min
[0269] Rinse by immersing the substrate in distilled water for 5 min
[0270] Apply the coating mixture by immersing the substrate in the coating mixture at room temperature for 10 min
[0271] Curing at 80 °C for lh
[0272] The following summarizes the roles of the main components in this example:
[0273] Incorporation of Ce(IV) as a metal-containing ion or metal cation, which can be reduced to Ce(III) and thereby forms an oxide / hydroxide precipitate
[0274] Integration of ascorbic acid as a reducing agent that donates electrons for the reduction of Ce(IV)
[0275] Incorporation of Alizarin S and functionalization of silanes with Alizarin S, which undergoes alkaline hydrolysis to form OH- and can form kinetically and thermodynamically stable aluminum complexes. Alizarin S was selected as an excellent and specific complexing agent for aluminum. Furthermore, covalent bonding to silanes can be achieved using epoxy rings.
[0276] Incorporation of ascorbic acid as a sacrificial agent to be oxidized
[0277] Use of sodium carbonate for neutralization after acid-catalyzed polysiloxane formation: COs 2- produces OH"
[0278] The polysiloxane network acts as a physical diffusion barrier for corrosive agents and substances, impairing the corrosion reaction kinetics and acting as a reservoir for the additives used to achieve a homogeneous corrosion protection effect
[0279] In the untreated substrate, the copper-rich intermetallic phase would initiate pitting corrosion: It is the cathodic site where the oxygen reduction reaction begins and generates electrons. This leads to the anodic oxidation of aluminum at another location on the substrate surface by absorbing these electrons. These processes are stopped by the applied coating.
[0280] The metal cations (cerium(III)) form cerium oxides / hydroxides (precipitates), which serve as protective agents on the surface. For this purpose, an alkaline medium is generated through an oxygen reduction reaction. However, the corresponding counter-reaction is aluminum oxidation. To prevent aluminum oxidation, a redox reaction takes place between a sacrificial species and oxygen.
[0281] The sacrificial species is the strong reducing agent. When electrons are donated by other species (not aluminum), an oxygen reduction reaction can occur and the formation of a protective cerium oxide / hydroxide layer occurs. Therefore, the strongly reducing additive (ascorbic acid) receives a redox potential due to the redox potential relation E(AI 3+ / AI) > E (Ox / Red) ("victim" / susceptible species) the electrons.
[0282] The complexing agent Alizarin S, which is very specific for aluminum ions, manipulates E(AI 3+ / AI) in a more positive direction to avoid being oxidized.
[0283] The suppression of the oxygen reduction reaction is achieved by the strongly oxidizing cerium(IV), whose reduction takes over the electron donation.
[0284] The formation of oxide / hydroxide precipitates is achieved through local hydrogen peroxide or hydroxide ion formation. This can be achieved by adding cider functional groups that can shift the pH. As described above, phenolic OH groups covalently bind Alizarin S and CO3. 2 ' ions.
[0285] The matrix of the polysiloxane network also plays an important role. The kinetics of corrosion reactions are strongly influenced by the limited supply of species from the atmosphere. A water-based coating would lead to a sporadic appearance of additives on the substrate surface. The polysiloxane network or polysiloxane xerogel used as a reservoir enables homogeneous distribution even in the case of a damaged coating. The polysiloxane network is capable of forming small "capsules," cavities, in which the processes can take place locally without affecting the entire surface. Polysiloxane itself would only be a sealing layer with passive corrosion protection. However, together with the other components used, various possibilities for active corrosion-inhibiting chemical and electrochemical processes are initiated.
[0286] The processes just described are summarized schematically in Fig. 1.
[0287] Excellent storage stability, no sedimentation or precipitation phenomena observed
[0288] Simple application using common techniques (dipping, squeegeeing, rolling, spinning, etc.) in a robust and fast manner
[0289] Possibility of local application / repair (spraying, brushing)
[0290] Environmentally friendly, sustainable and energy / environmentally friendly (low-temperature process, low rinse water requirement and therefore less wastewater)
[0291] Easy adaptation to specific customer requirements, search for new high-performance additives On the substrate: very small pore size, very thin layers (thickness similar to that of typical conversion coatings) possible, 500-800 nm according to scanning electron microscopy: dense layer with granular morphology; very good adhesion, particles remain on the surface after fracture (cryogenic fracture)
[0292] Excellent corrosion resistance (scientifically and technically proven effect, 1.5 - 2 times better performance in the salt spray test according to DIN ISO 9227:2017 compared to conventional conversion coatings on AA2024) - no corrosion up to 960 hours
[0293] Improved mechanical resistance (conical bending test with the following SEM: deformability of the substrate without cracking in the coating layer of the coating composition according to the invention, scratch resistance)
[0294] Excellent adhesion to all metal surfaces as well as to all underlying or overlying coatings
[0295] -> increased compatibility with typical coatings in the automotive and aerospace industries
[0296] -> Any combination with common compositions of basecoats, topcoats is conceivable to form multi-layer systems or hybrid systems or sandwich structures or composite structures
[0297] Diffusion barrier effect for water and other corrosive substances
[0298] Possibility of painting, gluing, printing
[0299] Possibility of chemically controlled (active) corrosion protection (a type of self-healing) low inspection and repair requirements
[0300] Fig. 2 shows a photograph of the coated substrate produced in this example after a salt spray test according to DIN ISO 9227:2017 after 960 hours. As can be clearly seen, there are no signs of corrosion. The coated substrate therefore exhibits excellent corrosion resistance.
[0301] Fig. 3 shows a diagram of a potentiodynamic measurement of the coating according to the invention produced in this exemplary embodiment compared to a Cr(III)-based coating produced according to the prior art on an AA2024 substrate (pH 9 borate buffer, room temperature, feed rate: 0.05 mV s-1, start: -50 mV vs. OCP, end: 1500 mV vs. OCP, 3-electrode system, AE: coated plate, RE: Ag / AgCl / sat.KCl, GE: platinum sheet). As can be seen from the diagram, the electrochemical measurement indicates a significantly better corrosion protection effect compared to the Cr(III)-containing coating. Flat part of the curve: formation of protective passive layer, shift of the resting potential: other redox system takes over (through complex formation and reducing agent), the much lower currents: slow reactions (diffusion barrier effect).
[0302] Example 2
[0303] First, a coating mixture was prepared as in Example 1, except that no Alizarin S was used. Alizarin S is a complexing agent for Al 3+ .
[0304] Using the prepared coating mixture, a semi-coated substrate was produced, using a mild steel substrate as the starting substrate. Only approximately half of the surface of the mild steel substrate was coated, with the coating process otherwise being carried out as in Example 1.
[0305] Fig. 4 shows the semi-coated structural steel substrate after 168 hours of neutral salt spray testing according to DIN ISO 9227:2017. The lower part of the substrate shown in Fig. 4 is coated, whereas the upper part is uncoated. The structural steel material was tested as a raw material for rotors in electric vehicles. No signs of corrosion are apparent on the coated part of the substrate, demonstrating the excellent anti-corrosion properties of the coating.
[0306] For example, a coating as shown in Fig. 4 is also suitable for the maritime industry as an intermediate storage solution: Parts are stored in a corrosive atmosphere and treated for corrosion only after assembly. In this case, the upper part would represent the surface without the coating during storage, while the lower part would represent the surface with the coating. The coating then serves as corrosion protection and forms an excellent base for further coatings (adhesion promotion), eliminating the need for expensive and laborious blasting processes.
[0307] Example 3
[0308] Using the coating according to the invention, it has also been possible to digitally print steel and aluminum substrates with water-based inks containing a styrene acrylate binder with a relatively high carboxyl group content and a high-molecular-weight resin. This is of great importance for front panels and control cabinets, as well as for other information signs.
[0309] Figure 5 shows an exemplary coated substrate according to the invention that has been printed accordingly. It is a coated structural steel substrate that has been digitally printed.
[0310] The preparation of the coating mixture and the subsequent production of the coated substrate were carried out as described in Example 2.
[0311] Example 4
[0312] Preparation of the coating mixture:
[0313] All chemicals were purchased from Merck (Sigma-Aldrich), and the purity of the chemicals is the highest available unless otherwise stated. In this example, 400 ml of deionized water is taken and 79.2 ml of GPTMS (3-glycidyloxypropyl)trimethoxysilane and 39.6 ml of tetraethylorthosilicate are added. 25 ml of 1 mol-l 1Acetic acid solution is added. The solution initially appears slightly cloudy, but then quickly becomes colorless and clear. It is allowed to stand on a stir plate for 30 minutes. In a separate, smaller container, 80 ml of deionized water is mixed with 4.104 g of Alizarin S. This is also magnetically stirred for 15 minutes. The solution is homogeneous and has an amber color. In a separate container, 7.2 ml of boron trifluoride etherate catalyst is dispersed in 120 ml of water. After the first and second solutions have been stirred for the required time, the Alizarin S dispersion is first added to the GPTMS solution, followed by the boron trifluoride etherate dispersion as catalyst. Next, 10 mg of Ce(III) nitrate, 10 mg of Ce(IV) nitrate, and 1 g of L-ascorbic acid are added. The reaction is allowed to run for one hour with constant stirring.After one hour, we add sodium carbonate to the solution in small increments while monitoring the pH until it reaches 7. At this point, the solution should be clear and have a deep amber color. We strain the solution and then add 117.6 ml of ethanol. The approximately 800 ml of solution can now be diluted 1:5 with distilled water and used to coat surfaces.
[0314] Production of the coated substrate:
[0315] Various substrates were used as starting substrates for the coating: two substrates made of different aluminum alloys with copper-containing intermetallic phases (substrate material: AI2024 or AI2024-T3, AI7075 or AI7075-T6), substrates made of various aluminum alloys with a high magnesium content (AIMgl, AIMg3), and a substrate made of pure aluminum (AI99.5 or EN AW 1050A). In all cases, the substrate pretreatment consisted of degreasing, alkaline etching, and acid etching (pickling) of the substrate to be coated, with a rinsing process with distilled water between the individual steps. After pretreatment, the coating process was carried out using the coating mixture prepared as described above.
[0316] The exact steps in detail in the order applied:
[0317] Degrease the substrate by immersing it in distilled water + ENPREP 144 (60 g / l, McDermid, Inc.) at 60 °C for 15 min
[0318] Rinse by immersing the substrate in distilled water for 5 min
[0319] Alkaline etching by immersing the substrate in distilled water + 10% NaOH at 60 °C for 1 min. Rinsing by immersing the substrate in distilled water for 5 min.
[0320] Acid etching (pickling) by immersing the substrate in distilled water + 22% HNO3 + 15% Alfideox 79 (Alufinish GmbH & Co. KG) at room temperature for 10 min
[0321] Rinse by immersing the substrate in distilled water for 5 min
[0322] Apply the coating mixture by immersing the substrate in the coating mixture at room temperature for 10 min
[0323] Curing at 80 °C for lh
[0324] The resulting coated substrates are subjected to a salt spray test or a neutral salt spray test according to DIN EN ISO 9227:2022. For comparison, a corresponding salt spray test or a corresponding neutral salt spray test according to DIN EN ISO 9227:2022 is carried out with uncoated substrates made of the same material. 150 mm x 80 mm panels are used for both the coating and the tests. The coated samples are prepared as follows: To avoid edge effects, the back or edges are taped with galvanic adhesive tape, leaving an approximately 140 mm x 70 mm window for the test.
[0325] The results of the salt spray test are shown in Fig. 6, which shows images of the coated and uncoated substrates side by side after each test, with the duration of the salt spray test and the neutral salt spray test indicated in each case. In the comparative images, the coated substrates are shown on the right and the uncoated substrates on the left.
[0326] It is clearly visible in Fig. 6 that the uncoated substrates show significant signs of corrosion after just a few hours, whereas the coated substrates show no or only very few signs of corrosion after a significantly longer period. Example 5
[0327] All chemicals were purchased from Merck (Sigma-Aldrich), and the purity of the chemicals is the highest available unless otherwise stated. In this example, 400 ml of deionized water is taken and 79.2 ml of GPTMS (3-glycidyloxypropyl)trimethoxysilane and 39.6 ml of tetraethylorthosilicate are added. 25 ml of 1 mol-l 1Acetic acid solution is added. The solution initially appears slightly cloudy, but then quickly becomes colorless and clear. It is allowed to stand on a stir plate for 30 minutes. In a separate, smaller container, 80 ml of deionized water is mixed with 4.104 g of Alizarin S. This is also stirred magnetically for 15 minutes. The solution is homogeneous and has an amber color. In a separate container, 7.2 ml of boron trifluoride etherate catalyst is dispersed in 120 ml of water. After the first and second solutions have been stirred for the required time, the boron trifluoride etherate dispersion is added dropwise as a catalyst. Next, 10 mg of Ce(II) nitrate and 10 mg of Ce(IV) nitrate are added. The reaction is allowed to run for one hour with constant stirring. After one hour, we add sodium carbonate to the solution in small steps while monitoring the pH until the pH reaches 7.At this point, the solution should be clear and have a deep amber color. Strain the solution and then add 117.6 ml of ethanol. The approximately 800 ml solution can now be diluted 1:5 with distilled water and used to coat surfaces.
[0328] Production of the coated substrate:
[0329] The starting substrate is made of an iron alloy (steel: 1.4301), low-alloy steel, or hot-dip galvanized (HDG 20 um Zn). Pretreatment of the substrate consisted of degreasing, followed by two rinses with distilled water. Following pretreatment, the coating process was carried out using the coating mixture prepared as described above.
[0330] The exact steps in detail in the applied order: Degrease the substrate (substrate material: AA2024) by immersing the substrate in distilled water + ENPREP 144 (60 g / l, McDermid, Inc.) at 60 °C for 15 min
[0331] Rinse by immersing the substrate in distilled water for two 5 min periods
[0332] Apply the coating mixture by immersing the substrate in the coating mixture at room temperature for 10 min
[0333] Curing at 80 °C for lh
Claims
Patent claims 1. A coating mixture for coating substrates containing or consisting of material to be protected from corrosion, wherein the material to be protected from corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; copper; alloys containing iron, copper, and / or aluminum; intermetallic phases containing iron, copper, and / or aluminum; composite materials containing iron, copper, and / or aluminum; and mixtures thereof, wherein the coating mixture contains at least one silane and / or at least one oligosiloxane formed from the at least one silane, at least one complexing agent for complexing cations of at least one metal contained in the material to be protected from corrosion, at least one metal-containing ion, and at least one solvent, wherein the at least one silane has at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom,and wherein the at least one complexing agent comprises at least one complexing agent acting as a reducing agent, which is the reduced form of a redox couple which, upon contact of an aqueous solution with a coating produced with the coating mixture in this aqueous solution, has a lower redox potential than the redox couple(s) of a metal contained in the material to be protected from corrosion, and / or the coating mixture additionally contains at least one reducing agent which is the reduced form of a redox couple which, upon contact of an aqueous solution with a coating produced with the coating mixture in this aqueous, solution has a lower redox potential than the redox pair(s) of a metal contained in the material to be protected from corrosion.
2. Coating mixture according to the preceding claim, characterized in that the at least one silane comprises at least one first silane and at least one second silane, wherein the at least one first silane and the at least one second silane each have at least one alkoxy group bonded to the Si atom having 1 to 4 carbon atoms, and wherein the at least one first silane and / or the at least one second silane each additionally has a group bonded to the Si atom, each of which is independently selected from the group consisting of alkyl groups having 1 to 4 carbon atoms, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups, and combinations thereof, and alkoxyalkyl groups, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups, and combinations thereof,and / or the at least one silane is at least one functionalized silane, wherein the at least one silane is preferably functionalized with the at least one complexing agent, with the at least one reducing agent, and / or with a substance selected from the group consisting of phenol hydroxides, lactates, carboxylates, and combinations thereof.
3. Coating mixture according to one of the preceding claims, characterized in that the at least one complexing agent is at least one complexing agent for complexing cations selected from the group consisting of aluminum cations, iron cations, copper cations, magnesium cations, zinc cations, chromium cations, manganese cations- and mixtures thereof, wherein the at least one complexing agent is preferably selected from the group consisting of Alizarin S; 2,2',2",2"'-(ethane-1,2-diyldinitrilo)tetraacetic acid and salts thereof; 2,2',2",2"'-[(1R,2R)-1,2-cyclohexanediyldinitrilo]tetraacetic acid and salts thereof; ethylene glycol bis(ß-aminoethyl ether)-N,N,N',N'-tetraacetic acid and salts thereof; ascorbic acid and isomers, conjugates and salts thereof; cyanic acid and isomers and salts thereof; tartaric acid and isomers and salts thereof; 1,4-dioxane; melamine and its isomers and derivatives; thiourea; cysteine; and mixtures thereof, and / or the at least one complexing agent acting as a reducing agent is selected from the group consisting of ascorbic acid and its isomers, conjugates and salts; melamine and its isomers and derivatives; thiourea; cysteine;and mixtures thereof, and / or the at least one reducing agent is selected from the group consisting of vanillin and its isomers and homologues, bisulfites, sulphites, dithionites, glutathione, polyphenols, and mixtures thereof, and / or the at least one metal-containing ion is selected from the group consisting of alkali metal cations, alkaline earth metal cations, transition metal cations, lanthanide cations, oxoanions, and mixtures thereof, wherein the at least one metal-containing ion is preferably selected from the group consisting of cerium(III) cations, cerium(IV) cations, lithium cations, sodium cations, molybdenum oxoanions, manganese oxoanions, and mixtures thereof, and / or the at least one solvent is selected from the group consisting of water; alcohols, preferably ethanol, isopropanol; butyl acetate;Fruit acid esters, and mixtures thereof, and / or the material to be protected from corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; Copper; alloys comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; alloys comprising or consisting of copper and zinc; intermetallic phases comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; composite materials comprising or consisting of aluminum, iron and / or copper and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof; and mixtures thereof.
4. Coating mixture according to one of the preceding claims, characterized in that the coating mixture Nanoparticles, which are preferably selected from the group consisting of titanium oxide nanoparticles, tungsten oxide nanoparticles, aluminum oxide nanoparticles, silicon dioxide nanoparticles, and mixtures thereof, and / or at least one base, which is preferably selected from the group consisting of sodium carbonate, lithium carbonate, potassium carbonate, and mixtures thereof, and / or at least one additive selected from the group consisting of adhesion promoters, pigments, fillers, and mixtures thereof.
5. Coating mixture according to one of the preceding claims, characterized in that the coating mixture 5 wt.% to 60 wt.%, preferably 5 wt.% to 25 wt.%, of the at least one silane and / or of the at least one oligosiloxane, based on the total mass of the mixture, and / or 100 ppm to 5000 ppm, preferably 100 ppm to 250 ppm, of the at least one complexing agent, based on the total mass of the mixture, and / or 100 ppm to 5000 ppm, preferably 100 ppm to 250 ppm, of the at least one reducing agent, based on the total mass of the mixture, and / or 1 to 100 ppm, preferably 5 to 10 ppm, of the at least one metal-containing ion, based on the total mass of the mixture, and / or 100 ppm to 1000 ppm, preferably 100 ppm to 250 ppm, nanoparticles, based on the total mass of the mixture, and / or, Contains 100 ppm to 5000 ppm wt.%, preferably 100 ppm to 500 ppm wt.%, of at least one additive, based on the total mass of the mixture.
6. A method for producing coated substrates, in which a) at least one layer of a coating mixture according to one of the preceding claims is applied to at least one area of a surface of at least one substrate which contains or consists of material to be protected from corrosion, wherein the material to be protected from corrosion is selected from the group consisting of aluminum, anodized aluminum; iron; copper; alloys containing iron, copper and / or aluminum; intermetallic phases containing iron; copper and / or aluminum; composite materials containing iron, copper and / or aluminum; and mixtures thereof, and b) the at least one applied layer is subjected to at least one curing process, in which the at least a silane and / or the at least one oligosiloxane is / are crosslinked to form a xerogel.
7. The method according to claim 6, characterized in that the application of the at least one layer in step a) is carried out by means of at least one application process which is selected from the group consisting of dipping, doctor blade coating, rolling, spinning, spraying, brushing, painting, and combinations thereof, and / or the substrate is subjected to at least one pretreatment before step a), which is preferably selected from the group consisting of cleaning, sandblasting, polishing, degreasing, alkaline etching, acid etching, plasma treatment, laser treatment, and combinations thereof.
8. The method according to claim 6 or 7, characterized in that the at least one curing process in step b) takes place at a temperature of 60 °C to 120 °C, preferably from 70 °C to 100 °C, particularly preferably from 80 °C to 90 °C, and / or for a duration of 5 min to 8 h, preferably from 30 min to 4 h, particularly preferably from 45 min to 2 h.
9. Method according to one of claims 6 to 8, characterized in that the material to be protected against corrosion is selected from the group consisting of aluminum; anodized aluminum; Iron; Copper; Alloys comprising or consisting of • Aluminium and / or iron, as well as • at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; Alloys comprising or consisting of copper and zinc; intermetallic phases comprising or consisting of • Aluminium and / or iron, as well as • at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon and mixtures thereof; Composite materials comprising or consisting of • Aluminium, iron and / or copper, as well as • at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber reinforced plastics, glass fiber reinforced plastics, and mixtures thereof; as well as mixtures thereof.
10. A coated substrate comprising a metal-containing substrate containing or consisting of material to be protected from corrosion, wherein the material to be protected from corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; copper; alloys containing iron, copper and / or aluminum; intermetallic phases containing iron, copper and / or aluminum; composite materials containing iron, copper and / or aluminum; and mixtures thereof, and at least one coating arranged on at least one area of a surface of the substrate containing a xerogel and at least one complexing agent for complexing cations at least one metal contained in the material to be protected from corrosion, and at least one metal-containing ion, wherein the xerogel is formed from at least one silane having at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, and wherein the at least one complexing agent comprises at least one complexing agent acting as a reducing agent, which is the reduced form of a redox couple which, upon contact of an aqueous solution with the at least one coating in this aqueous solution, has a lower redox potential than the redox couple(s) of a metal contained in the material to be protected from corrosion, and / or the coating additionally contains at least one reducing agent which is the reduced form of a redox couple,which, upon contact of an aqueous solution with the at least one coating in this aqueous solution, has a lower redox potential than the redox pair(s) of a metal contained in the material to be protected from corrosion.
11. Coated substrate according to claim 10, characterized in that the at least one complexing agent and / or the at least one reducing agent is / are covalently bound to the xerogel and / or is / are adsorbed to the xerogel.
12. Coated substrate according to claim 10 or 11, characterized in that the xerogel is formed from at least one silane which is functionalized and / or has at least one alkoxy group having 1 to 4 carbon atoms bonded to the Si atom, wherein the at least one silane preferably has at least one alkoxy group bonded to the Si- atom-bonded group, each of which is independently selected from the group consisting of alkyl groups having 1 to 4 carbon atoms, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups and combinations thereof, and alkoxyalkyl groups, which may have one or more groups selected from amino groups, organosulfonyl groups, epoxy groups and combinations thereof, and / or the material to be protected from corrosion is selected from the group consisting of aluminum; anodized aluminum; iron; copper; alloys comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; alloys comprising or consisting of copper and zinc;intermetallic phases comprising or consisting of aluminum and / or iron and at least one substance selected from the group consisting of copper, magnesium, zinc, silicon, chromium, manganese, carbon, and mixtures thereof; composite materials comprising or consisting of aluminum, iron and / or copper and at least one substance selected from the group consisting of polyurethanes, in particular thermoplastic polyurethanes, epoxy resins, polytetrafluoroethylene, acrylonitrile-butadiene rubber, polycarbonates, polyethylene, in particular HD polyethylene, carbon fiber-reinforced plastics, glass fiber-reinforced plastics, and mixtures thereof;and mixtures thereof, and / or the at least one complexing agent is at least one complexing agent for complexing cations selected from the group consisting of aluminum cations, iron cations, copper cations, magnesium cations, zinc cations, chromium cations, manganese cations, silicon cations, and mixtures thereof, wherein the at least one complexing agent is preferably selected from the; Group consisting of Alizarin S; 2,2',2",2"'-(ethane-1,2-diyldinitrilo)tetraacetic acid and its salts; 2,2',2",2"'-[(lR,2R)-1,2-cyclohexanediyldinitrilo]tetraacetic acid and its salts; ethylene glycol bis(ß-aminoethyl ether)-N,N,N',N'-tetraacetic acid and its salts; ascorbic acid and its isomers, conjugates and salts; cyanic acid and its isomers and salts; tartaric acid and its isomers and salts; 1,4-dioxane; melamine and its isomers and derivatives; thiourea; cysteine; and mixtures thereof, and / or the at least one complexing agent acting as a reducing agent is selected from the group consisting of ascorbic acid and its isomers, conjugates and salts; melamine and its isomers and derivatives; thiourea; cysteine;and mixtures thereof, and / or the at least one reducing agent is selected from the group consisting of vanillin and its isomers and homologues, bisulfites, sulphites, dithionites, glutathione, polyphenols, and mixtures thereof, and / or the at least one metal-containing ion is selected from the group consisting of alkali metal cations, alkaline earth metal cations, transition metal cations, lanthanide cations, and mixtures thereof, preferably selected from cerium(III) cations, cerium(IV) cations, lithium cations, sodium cations, molybdenum oxoanions, manganese oxoanions, and mixtures thereof.; 13. Coated substrate according to one of claims 10 to 12, characterized in that the at least one coating is a single layer, a multi-layer, a part of a multi-layer system in combination with at least one further coating, a primer, a conversion coating, a clear coat, or a combination thereof.
14. Coated substrate according to one of claims 10 to 13, characterized in that the coated substrate can be produced or is produced by a process according to one of claims 6 to 9.
15. Use of a coated substrate according to one of claims 10 to 14 as a component in the aerospace industry, in the automotive industry, in shipbuilding, in precision engineering.
Citation Information
Patent Citations
Coating composition with titanium dioxide-generating agent, nanoscale coating based on titanium dioxide, its production, further processing and use
DE102010032619A1
Hydrogel and xerogelactive ingredient carriers made from dendritic polymers and silica for solid substrate coating applications
GR1010001B
Organosiloxane-grafted natural polymer coatings
US5844058A
Composition and use of this composition for forming a sol-gel coating on a metal surface
WO2022023685A1