Lithium secondary battery

By integrating oxide-based solid electrolyte particles with specific particle diameters into the positive electrode active material layer, the lithium secondary battery enhances desolvation and conductivity, overcoming the limitations of high-concentration lithium salt compositions and achieving improved output and low-temperature performance.

WO2024228487A1PCT designated stage expired Publication Date: 2024-11-07LG ENERGY SOLUTION LTD

Patent Information

Application Number
PCT/KR2024/004873
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-04
Filing Date
2024-04-11
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Lithium secondary batteries face challenges in achieving high output characteristics and maintaining excellent low-temperature performance due to increased electrolyte viscosity and decreased ionic conductivity when using high-concentration lithium salt compositions, which hinder the desolvation process of lithium ions.

Method used

Incorporating oxide-based solid electrolyte particles with specific average particle diameters into the positive electrode active material layer, which accelerates the desolvation process and improves lithium ion conductivity, thereby enhancing output characteristics without the need for high-concentration lithium salt compositions.

Benefits of technology

The solution effectively improves the output characteristics and low-temperature performance of lithium secondary batteries by reducing activation energy and maintaining high ionic conductivity, even at low temperatures, thus addressing the limitations of high-concentration lithium salt compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004873_07112024_PF_FP_ABST
    Figure KR2024004873_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium secondary battery with improved output characteristics and low-temperature characteristics. The lithium secondary battery comprises a cathode, an anode, and an electrolyte containing a lithium salt and a non-aqueous organic solvent. The cathode comprises: a cathode current collector; and an active material layer formed on the cathode current collector and containing a cathode active material, a conductive material, and an oxide-based solid electrolyte having a lithium ion source. The cathode active material and the oxide-based solid electrolyte are dispersed in the form of particles within the active material layer, and the average particle diameter (D50) of the particles satisfies a predetermined ratio.
Need to check novelty before this filing date? Find Prior Art

Description

lithium secondary battery

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0058563, filed May 4, 2023, and Korean Patent Application No. 10-2023-0131540, filed October 4, 2023, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to a lithium secondary battery having improved output characteristics and low-temperature characteristics.

[0004] Recently, as the application areas of lithium secondary batteries have rapidly expanded to include not only power supply for electronic devices such as electric, electronic, communication, and computer devices, but also power storage for large-area devices such as automobiles and power storage devices, the demand for lithium secondary batteries with high capacity, high output, long life, and high stability is increasing.

[0005] A lithium secondary battery is generally composed of a positive electrode, a negative electrode, a separator, and an electrolyte including a lithium salt and an organic solvent, and lithium ions move through the electrolyte during the charging and discharging process.

[0006] Within the electrolyte, lithium ions exist in a solvated state, surrounded by an organic solvent. Therefore, for the lithium ions within the electrolyte to migrate and be inserted into the electrode active material, they must undergo a desolvation process, in which the lithium ions are separated or desorbed from the organic solvent molecules. Therefore, the smooth progress of this desolvation process can affect the output, resistance, or stability of a lithium secondary battery.

[0007] Meanwhile, with the recent demand for higher capacity and higher output in lithium secondary batteries, the development of novel electrolytes is actively underway. In particular, novel electrolyte compositions have been proposed, such as those that include high concentrations of lithium salts or that change the composition of the organic solvent to form localized, high-concentration regions of lithium salts around the electrode, to accelerate the desolvation of lithium ions and thereby increase the output of lithium secondary batteries.

[0008] However, when applying the above novel electrolyte composition including a high concentration of lithium salt, there is a disadvantage in that the problem of reduced fluidity due to increased viscosity of the electrolyte may occur, and in particular, the ion conductivity of the electrolyte may decrease at low temperatures, resulting in increased resistance or reduced battery output, thereby deteriorating the low-temperature characteristics of the lithium secondary battery.

[0009] Accordingly, there is a continuous demand for the development of technology that can improve the output characteristics of lithium secondary batteries by accelerating the desolvation of lithium ions within the electrolyte while maintaining excellent low-temperature characteristics.

[0010] Accordingly, the present invention provides a lithium secondary battery that exhibits improved output characteristics by accelerating the desolvation of lithium ions in an electrolyte, while maintaining excellent low-temperature characteristics such as high output at low temperatures.

[0011] The present invention comprises a positive electrode, a negative electrode, and an electrolyte including a lithium salt and a non-aqueous organic solvent,

[0012] The positive electrode comprises a positive electrode current collector; and an active material layer formed on the positive electrode current collector and including an oxide-based solid electrolyte having a positive electrode active material, a conductive material, and a lithium ion source,

[0013] The above-mentioned positive electrode active material and the above-mentioned oxide-based solid electrolyte are dispersed in the active material layer in the form of particles, and the average particle diameter (D50) of the particles is provided in a lithium secondary battery in which the oxide-based solid electrolyte and the above-mentioned positive electrode active material have a ratio of 1:4 to 1:90.

[0014] In the lithium secondary battery of the present invention, the positive electrode includes oxide-based solid electrolyte particles dispersed within an active material layer, and the oxide-based solid electrolyte particles may have an average particle diameter (D50) of a certain ratio with respect to the positive electrode active material particles. The oxide-based solid electrolyte particles may be uniformly distributed around the positive electrode active material particles within the active material layer, and may be distributed in large numbers near the interface between the active material layer and the electrolyte.

[0015] These oxide-based solid electrolyte particles can reduce the activation energy involved in the desolvation process of lithium ions in the electrolyte at the interface where the active material layer and the electrolyte come into contact, and can accelerate the desolvation of lithium ions, thereby improving the output characteristics of a lithium secondary battery.

[0016] Furthermore, since the output characteristics of a lithium secondary battery can be improved without applying a new electrolyte composition including a high concentration of lithium salt, problems such as increased electrolyte viscosity, decreased fluidity, and decreased ion conductivity of the electrolyte and output of the battery at low temperatures due to the application of the new electrolyte composition can be solved, and excellent low-temperature characteristics of a lithium secondary battery can be achieved.

[0017] Additionally, even when applying an electrolyte composition including the above-described high-concentration lithium salt, etc., the application of the positive electrode can facilitate the desolvation of lithium ions, thereby improving lithium ion conductivity and reducing resistance. Accordingly, the output characteristics of a lithium secondary battery can be further improved by using the high-concentration lithium salt, etc., while reducing the deterioration of low-temperature characteristics.

[0018] Accordingly, the present invention can greatly contribute to the development of next-generation lithium secondary batteries exhibiting improved output characteristics and low-temperature characteristics.

[0019] Figure 1 is a graph comparing the degree of voltage drop according to the discharge time while discharging from a state of charge (SOC) of 50% at -10°C for 30 seconds for the lithium secondary batteries of Comparative Example 1 and Example 1.

[0020] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical spirit of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best possible manner.

[0021] It should be understood that the terms “include,” “comprising,” or “having” used in this specification are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0022] According to one embodiment of the invention, there is provided a battery comprising a positive electrode, a negative electrode, and an electrolyte including a lithium salt and a non-aqueous organic solvent,

[0023] The positive electrode comprises a positive electrode current collector; and an active material layer formed on the positive electrode current collector and including an oxide-based solid electrolyte having a positive electrode active material, a conductive material, and a lithium ion source,

[0024] A lithium secondary battery is provided in which the positive electrode active material and the oxide-based solid electrolyte are dispersed in the active material layer in the form of particles, and the average particle diameter (D50) of the particles is such that the oxide-based solid electrolyte: the positive electrode active material has a ratio of 1:4 to 1:90.

[0025] In such a lithium secondary battery, oxide-based solid electrolyte particles are dispersed together with positive electrode active material particles within the active material layer of the positive electrode, and the oxide-based solid electrolyte particles can satisfy an average particle diameter (D50) ratio with respect to positive electrode active material particles of 1:4 to 1:90, or 1:5 to 1:80, or 1:10 to 1:60, or 1:15 to 1:40, or 1:16 to 1:25, or 1:20 to 1:35.

[0026] According to the experimental results of the present inventors, when oxide-based solid electrolyte particles satisfying the D50 ratio are included in the active material layer of the positive electrode, these oxide-based solid electrolyte particles can be uniformly distributed around the positive electrode active material particles within the active material layer, and in particular, can be distributed in large numbers near the interface between the active material layer and the electrolyte. Accordingly, the oxide-based solid electrolyte particles can accelerate the desolvation process of lithium ions by reducing the activation energy involved in the desolvation process of lithium ions within the electrolyte at the interface where the active material layer and the electrolyte come into contact. In addition, this can improve the movement speed of lithium ions and lithium ion conductivity around the positive electrode active material particles.

[0027] Therefore, a lithium secondary battery including such a positive electrode according to one embodiment can accelerate the desolvation of lithium ions and improve the lithium ion movement speed and conductivity within the active material layer, thereby lowering the resistance and improving the output characteristics of the lithium secondary battery, even without applying an electrolyte composition including a high-concentration lithium salt. As a result, problems such as increased electrolyte viscosity, decreased fluidity, and decreased ion conductivity of the electrolyte and output of the battery at low temperatures due to the application of the high-concentration lithium salt can be solved, and excellent low-temperature characteristics of the lithium secondary battery can be achieved at the same time.

[0028]

[0029] Hereinafter, a lithium secondary battery according to an embodiment will be described in more detail.

[0030] In the lithium secondary battery according to the above embodiment, the positive electrode includes a positive electrode current collector. The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used.

[0031] Additionally, the active material layer on the positive electrode current collector may include an oxide-based solid electrolyte having a positive electrode active material, a conductive material, and a lithium ion source, and may optionally further include a binder.

[0032] At this time, the positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically may include a lithium metal oxide containing lithium and one or more metals such as iron, cobalt, manganese, nickel, or aluminum.

[0033] Specifically, the lithium metal oxide is a lithium-manganese oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt oxide (e.g., LiCoO2, etc.), a lithium-nickel oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese oxide (e.g., LiNi 1-Y Mn Y O2 (here, 0 <Y<1), LiMn 2-Z Ni Z O4 (where 0<Z<2), etc.), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y1 Co Y1 O2 (here, 0 <Y1<1) 등), 리튬-망간-코발트계 산화물(예를 들면, LiCo 1-Y2 Mn Y2 O2 (here, 0 <Y2<1), LiMn 2-Z1 Co Z1O4 (wherein, 0<Z1<2) etc.), lithium-nickel-manganese-cobalt oxides (e.g., Li(Ni p Co q Mn r )O2(wherein, 0<p<1, 0<q<1, 0<r<1, p+q+r=1) or Li(Ni p1 Co q1 Mn r1 )O4 (wherein, 0<p1<2, 0<q1<2, 0<r1<2, p1+q1+r1=2) etc.), lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r2 M s2 )O2 (wherein, M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r2 and s2 are atomic fractions of independent elements, respectively, 0<p2<1, 0<q2<1, 0<r2<1, 0<s2<1, p2+q2+r2+s2=1), etc.), or lithium iron phosphate (e.g., Li 1+a Fe 1-x M x (PO 4-b )X b (Here, M is at least one selected from Al, Mg, and Ti, X is at least one selected from F, S, and N, -0.5≤a≤+0.5, 0≤x≤0.5, 0≤b≤0.1), and any one or two or more compounds thereof may be included.

[0034] Among these, the positive electrode active material includes a lithium metal oxide including lithium and two or more metals selected from the group consisting of nickel, manganese, cobalt, and aluminum, and the lithium metal oxide may include nickel in an amount of 60 mol% or more, or 60 to 99 mol%, or 70 to 95 mol%, based on the total metal content excluding lithium. Such a lithium metal oxide may be represented by, for example, the following chemical formula 1:

[0035] [Chemical Formula 1]

[0036] Li x Ni a Co b M 1 c M 2 d O2

[0037] In the above chemical formula 1, the M 1 Mn and Al may be one or more selected from or a combination thereof, and M 2 may be at least one selected from the group consisting of Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S, and may be 0.90≤x≤1.1, or 0.95≤x≤1.08, or 1.0≤x≤1.08, and may be 0.60≤a<1.0, or 0.70≤a≤0.99, or 0.80≤a≤0.95.

[0038] By using lithium metal oxide containing such a high nickel content as a cathode active material and combining it with an oxide-based solid electrolyte, the output and capacity characteristics of a lithium secondary battery can be further improved.

[0039] The above-described positive electrode active material may be included in an amount of 60 to 99 wt%, or 70 to 99 wt%, or 80 to 98 wt% based on the total weight of the active material layer.

[0040] In addition, as the above oxide-based solid electrolyte, any solid electrolyte having a lithium ion source including lithium in its structure and having the form of a lithium metal oxide or lithium metal phosphate can be used.

[0041] Specific examples thereof include at least one lithium metal oxide or lithium metal phosphate selected from a Nasicon-type solid electrolyte, a Lisicon-type solid electrolyte, a Garnet-type solid electrolyte, a Perovskite-type solid electrolyte, and a LiPON-type solid electrolyte, and more specific examples thereof include at least one selected from the group consisting of a LAGP (lithium aluminum germanium phosphate) compound, an LLZO (lithium lanthanum zirconium oxide) compound, a LATP (lithium aluminum titanium phosphate) compound, an LLZTO (lithium lanthanum zirconium tantalum oxide) compound, an LLTO (lithium lanthanum titanium oxide) compound, a LSTP (lithium silicon titanium phosphate) compound, and a LGPO (lithium germanium phosphate) compound.

[0042] Among these, a NASICON-type solid electrolyte such as the LAGP-type compound or LATP-type compound can be appropriately used in terms of accelerating the desolvation of lithium ions at the interface between the active material layer and the electrolyte and improving the ion conductivity and output of a lithium secondary battery.

[0043] In the positive electrode described above, the positive electrode active material and the oxide-based solid electrolyte can be dispersed in the form of particles within the active material layer, and each has a predetermined average particle diameter (D50), thereby satisfying the above-described D50 ratio. At this time, the average particle diameter (D50) of each particle can be calculated as a particle diameter corresponding to 50% of the volume accumulation amount in the particle size distribution curve when the particle size distribution of the positive electrode active material or the oxide-based solid electrolyte is measured using a laser diffraction method and a laser diffraction particle size measuring device, for example.

[0044] Specifically, the positive electrode active material may have an average particle diameter (D50) of 5 to 15 μm, or 7 to 13 μm, or 8 to 12 μm, and the oxide-based solid electrolyte may have an average particle diameter (D50) of 100 nm to 1.2 μm, or 120 nm to 1 μm, or 150 to 800 nm, or 200 to 600 nm. When these components satisfy the above-described average particle diameter (D50) and the above-described D50 ratio, the lithium secondary battery of one embodiment may exhibit better capacity and output characteristics, and lower resistance and low-temperature characteristics.

[0045] In addition, the oxide-based solid electrolyte may be included in an amount of 0.1 to 5 parts by weight, or 0.5 to 4 parts by weight, or 1 to 3.5 parts by weight, based on 100 parts by weight of the positive electrode active material, in order to accelerate the desolvation of lithium ions at the interface between the active material layer and the electrolyte and improve the lithium ion movement speed and conductivity, etc., without inhibiting the insertion and desorption process of lithium ions by the positive electrode active material.

[0046] Meanwhile, the conductive material included in the active material layer is a component for further improving the conductivity of the positive electrode active material. The conductive material is not particularly limited as long as it has conductivity without causing chemical changes in the battery. For example, carbon powder such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive nanomaterials such as carbon nanofibers or carbon nanotubes; fluorinated carbon powder; conductive powder such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. can be used. Among these, the conductive material can further lower the resistance of the lithium secondary battery of one embodiment and improve the output characteristics, etc. by including a conductive nanomaterial such as carbon nanotubes or carbon nanofibers.

[0047] Typically, the conductive material may be included in an amount of 1 to 20 wt%, or 1 to 15 wt%, or 1 to 10 wt% based on the total weight of the active material layer.

[0048] The binder optionally included in the above active material layer is a component that assists in the bonding of the positive electrode active material and the conductive material, and the bonding to the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, nitrile rubber, styrene-butadiene rubber, or fluororubber, and a mixture or copolymer of two or more selected from these may also be used.

[0049] Typically, the binder may be included in an amount of 1 to 20 wt%, or 1 to 15 wt%, or 1 to 10 wt% based on the total weight of the positive electrode active material layer.

[0050] Additionally, a filler may be optionally added to the positive electrode as a component that suppresses its expansion. Such filler is not particularly limited as long as it can suppress the expansion of the electrode without causing chemical changes in the battery. Examples of fillers that can be used include olefin polymers such as polyethylene and polypropylene; fibrous materials such as glass fiber and carbon fiber; and the like.

[0051] The above-described positive electrode can be manufactured, for example, by dispersing and mixing the positive electrode active material, oxide-based solid electrolyte, binder, and conductive agent in a dispersion medium (solvent) to make a slurry, applying the slurry on a positive electrode current collector, and then drying and rolling. At this time, the dispersion medium may be NMP (N-methyl-2-pyrrolidone), DMF (Dimethyl formamide), DMSO (Dimethyl sulfoxide), ethanol, isopropanol, water, and mixtures thereof, but is not necessarily limited thereto.

[0052] Meanwhile, in the lithium secondary battery of one embodiment, the negative electrode may have a conventional configuration known in the art. For example, the negative electrode may include an negative electrode current collector and an negative electrode active material layer formed on the negative electrode current collector, and the negative electrode active material layer may include, for example, an negative electrode active material and, if necessary, additives such as a conductive material, a binder, and a filler. In addition, the negative electrode may be formed by a general method of dispersing and mixing each component of the negative electrode active material layer in a dispersion medium (solvent) to make a slurry, applying the slurry on the negative electrode current collector, and then drying and rolling the slurry.

[0053] At this time, the negative electrode current collector may be, but is not limited to, platinum (Pt), gold (Au), palladium (Pd), iridium (Ir), silver (Ag), ruthenium (Ru), nickel (Ni), stainless steel (STS), copper (Cu), molybdenum (Mo), chromium (Cr), carbon (C), titanium (Ti), tungsten (W), ITO (In doped SnO2), FTO (F doped SnO2), and alloys thereof, as well as copper (Cu) or stainless steel surface-treated with carbon (C), nickel (Ni), titanium (Ti), or silver (Ag). The negative electrode current collector may have a form such as a foil, a film, a sheet, a punched form, a porous body, or a foam.

[0054] In addition, a compound capable of reversible intercalation and deintercalation of lithium may be used as the negative electrode active material. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Sb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; metallic oxides capable of doping and dedoping lithium such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may also be used as the negative electrode active material.

[0055] In addition, both low-crystalline carbon and high-crystalline carbon can be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include amorphous, plate-like, flaky, spherical or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.

[0056] The above-described negative electrode active material may be included in an amount of 60 to 99 wt%, or 70 to 99 wt%, or 80 to 98 wt% based on the total weight of the negative electrode active material layer.

[0057] In another embodiment, the negative electrode may not include a negative electrode active material layer, but may only include a negative electrode current collector. In such a negative electrode, lithium ions moved from the positive electrode during the charge and discharge process may be deposited on the negative electrode current collector to form a lithium metal layer, and this lithium metal layer may function as a negative electrode active material.

[0058] Meanwhile, the binder and conductive material included in the negative electrode active material layer may be the same as those described above for the positive electrode, and therefore, further description thereof will be omitted. In addition, similar to the positive electrode described above, the negative electrode active material layer may further include an oxide-based solid electrolyte having the lithium ion source described above, and in this case, the oxide-based solid electrolyte may satisfy the D50 ratio described above for the negative electrode active material particles.

[0059] The lithium secondary battery described above further includes an electrolyte comprising a lithium salt and a non-aqueous organic solvent. This electrolyte acts as a transport medium for lithium ions between the positive and negative electrodes. These lithium ions exist in the electrolyte in a solvated state, while at the interface between the electrolyte and the electrode, they can be desolvated and inserted into the electrode active material. As described above, in one embodiment of the secondary battery, this desolvation is accelerated, thereby exhibiting improved output characteristics, etc.

[0060] The lithium salt included in the above electrolyte is used as a medium for transferring ions within a lithium secondary battery. The lithium salt is, for example, Li as a cation. + Including, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO2 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P- , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - and SCN - It may include an anion selected from the group consisting of .

[0061] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (lithium bis(fluorosulfonyl) imide, LiN(SO2F)2), LiBETI (lithium bis(perfluoroethanesulfonyl) imide, LiN(SO2CF2CF3)2) and LiTFSI (lithium bis(trifluoromethanesulfonyl) imide, LiN(SO2CF3)2).

[0062] The concentration of the above lithium salt can be appropriately changed within a commonly usable range, and can be included in the electrolyte at a concentration of 0.5 M to 6 M, or a concentration of 1 M to 5 M.

[0063] In a more specific embodiment, the electrolyte may include a lithium salt in a relatively low concentration of 0.5 M or more and less than 2 M, or 0.7 M to 1.5 M. Even in this case, since the desolvation of lithium ions is accelerated by the action of the positive electrode described above, the lithium secondary battery of one embodiment may exhibit improved output characteristics. As a result, problems such as increased electrolyte viscosity, decreased fluidity, and decreased ionic conductivity of the electrolyte and battery output at low temperatures due to the application of an electrolyte composition including a high concentration of lithium salt can be solved, and excellent low-temperature characteristics of the lithium secondary battery can be achieved at the same time.

[0064] Meanwhile, in another embodiment of the invention, the electrolyte may contain a lithium salt at a high concentration of 2 M to 6 M, or 2.5 M to 5.5 M. In this case, the desolvation of lithium ions can be further accelerated by the inclusion of a high-concentration lithium salt and the application of the above-described positive electrode, and the output characteristics of the secondary battery can be further improved.

[0065] In addition, by applying the above-mentioned positive electrode, lithium ion conductivity can be improved and resistance can be reduced even at low temperatures. This can reduce the deterioration of low-temperature output characteristics due to high-concentration lithium salts, etc.

[0066] Meanwhile, the type of non-aqueous organic solvent that can be included in the electrolyte is not particularly limited, and any organic solvent previously known to be applicable to electrolytes of lithium ion batteries, etc., can be used. Examples of such organic solvents include at least one selected from the group consisting of carbonate solvents, ether solvents, nitrile solvents, phosphate solvents, and sulfone solvents.

[0067] More specifically, as the carbonate solvent, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, methyl propyl carbonate, ethyl methyl carbonate, ethyl propyl carbonate or methyl (2,2,2-trifluoroethyl) carbonate can be used, and as the phosphate solvent, trimethyl phosphate, triethyl phosphate or 2-(2,2,2-trifluoroethoxy)-1,3,2-dioxaphosphorane 2-oxide can be used.

[0068] In addition, as the ether solvent, dibutyl ether, tetraglyme, diglyme, dimethoxy ethane, or tetrahydrofuran derivatives such as 2-methyl tetrahydrofuran can be used, and as the nitrile solvent, succinonitrile, adiponitrile, sebaconitrile, acetonitrile, or propionitrile can be used. In addition, as the sulfone solvent, dimethyl sulfone, ethylmethyl sulfone, or sulforane can be used.

[0069] Meanwhile, the electrolyte may further include, in addition to the lithium salt and the non-aqueous organic solvent described above, a diluent that exhibits a solubility in the lithium salt that is at least 10 times lower than that of the non-aqueous organic solvent. The diluent may be an organic solvent that is miscible with the non-aqueous organic solvent while exhibiting substantially no solubility in the lithium salt, for example, an ether solvent having a fluorine-substituted alkyl group, and more specifically, may include at least one selected from the group consisting of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl) ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), methoxynonafluorobutane (MOFB), and ethoxynonafluorobutane (EOFB).

[0070] When such a diluent is further included, a high-concentration lithium salt may be locally present in the non-aqueous organic solvent within the electrolyte, and substantially no lithium salt may be present within the diluent. In this way, since a high-concentration lithium salt is locally present in a solvated form within the electrolyte, the output characteristics of the lithium secondary battery can be further improved, while the increase in viscosity and decrease in fluidity of the electrolyte can be reduced. In addition, when the positive electrode described above is applied together with such a high-concentration salt electrolyte, lithium ion conductivity can be improved and resistance can be reduced even at low temperatures, thereby reducing the deterioration of low-temperature output characteristics caused by high-concentration lithium salts, etc.

[0071] The amount of the diluent used can be adjusted depending on the type of non-aqueous organic solvent and lithium salt, or the overall concentration of the lithium salt, and for example, the diluent: non-aqueous organic solvent can be included in the electrolyte in a molar ratio of 1:0.2 to 1:5, or 1:0.5 to 1:2.

[0072] Meanwhile, the lithium secondary battery of the above-described embodiment may further include a porous separator interposed between the positive electrode and the negative electrode.

[0073] These porous membranes can be made of olefin polymers such as polyethylene and polypropylene, glass fibers, etc. in the form of sheets, multi-membranes, microporous films, woven fabrics, and non-woven fabrics, but are not necessarily limited thereto. However, it may be preferable to use porous polyethylene or porous glass fiber non-woven fabric (glass filter) as the membrane, and it may be more preferable to use porous glass filter (glass fiber non-woven fabric) as the membrane. The membrane may be an insulating thin film having high ion permeability and mechanical strength, and the pore diameter of the membrane may generally be in the range of 0.01 to 10 ㎛, and the thickness may generally be in the range of 5 to 300 ㎛, but is not limited thereto.

[0074] In addition, in another example of the lithium secondary battery, the separator may not be interposed, and the electrolyte described above may be interposed between the positive and negative electrodes in the form of an electrolyte membrane or electrolyte film. In this case, the electrolyte membrane or electrolyte film may be in the form of a polymer matrix containing the lithium salt and a non-aqueous organic solvent described above, and the polymer matrix may use a well-known polymer-based solid electrolyte or a crosslinked polymer obtained by crosslinking a multifunctional acrylate monomer. In this case, the lithium secondary battery of the above embodiment may be a semi-solid battery that uses a liquid electrolyte and a solid electrolyte in combination.

[0075] Meanwhile, the lithium secondary battery of the above embodiment can be manufactured according to a conventional method in the art. For example, the electrode assembly including the positive electrode, negative electrode, and separator (or electrolyte membrane) can be manufactured by housing it in a case and injecting and impregnating the electrolyte described above.

[0076] These lithium secondary batteries can be applied to battery cells used as power sources for small devices, and are particularly suitable for use as unit cells in battery modules that serve as power sources for medium- to large-sized devices.

[0077]

[0078] The invention will be described in more detail below through specific examples. However, the following examples are provided solely to aid understanding of the invention and do not limit the scope of the invention.

[0079]

[0080] Example 1: Manufacturing of a lithium secondary battery

[0081] As a cathode active material, lithium nickel cobalt manganese composite oxide (NCM 811; D50: 10㎛) containing 80 mol% of nickel among the total transition metals was used, carbon nanotubes were used as a conductive material, polyvinylidene fluoride (PVdF) was used as a binder, and LiAl with D50: 300nm was used as an oxide-based solid electrolyte. 0.3 Ti 1.7 (PO4)3(LATP system) compound particles were used respectively (oxide system solid electrolyte: D50 ratio of the above electrode active material: 1:33.3).

[0082] The above positive electrode active material: conductive material: binder: oxide-based solid electrolyte was mixed in a weight ratio of 94:1.5:2:2.5, dispersed in an NMP solvent at 2500 to 3000 rpm to prepare a slurry, and then coated with a uniform thickness on a 25 ㎛ thick aluminum foil (Al foil) using a blade-type coating machine, a Mathis coater (Labdryer / coater type LTE, Werner Mathis AG), dried in a vacuum oven at 110 to 130°C for 12 to 24 hours, and rolled using a roll press machine to prepare a positive electrode for a lithium secondary battery.

[0083] Graphite was used as the negative active material, and the negative active material: conductive material: binder was mixed in a weight ratio of 96.5:1.5:2 without using an oxide-based solid electrolyte, and the negative electrode was manufactured by performing the same process as the positive electrode.

[0084] After the positive and negative electrodes were each formed, a separator made of a porous polyethylene (PE) film was interposed between them to manufacture an electrode assembly.

[0085] After positioning the manufactured electrode assembly inside the battery case, an electrolyte was injected into the case to manufacture a lithium secondary battery. At this time, the electrolyte was prepared by dissolving 1.0 M LiFSI in an organic solvent consisting of ethylene carbonate / ethyl methyl carbonate (EC / EMC mixing volume ratio of 3 / 7).

[0086]

[0087] Example 2: Manufacturing of a lithium secondary battery

[0088] In the above Example 1, the oxide-based solid electrolyte is LiAl with D50: 600 nm. 0.3 Ti 1.7 A positive electrode and a lithium secondary battery were manufactured in the same manner as in Example 1, except that (PO4)3(LATP) compound particles were used (oxide-based solid electrolyte: D50 ratio of the electrode active material: 1:16.7).

[0089]

[0090] Example 3: Manufacturing of a lithium secondary battery

[0091] The positive and negative electrodes were each manufactured in the same manner as in Example 1.

[0092] Meanwhile, 4 parts by weight of trimethylolpropane triacrylate (ETPTA) and 0.6 parts by weight of AIBN as thermal initiators were added to 100 parts by weight of an electrolyte prepared by dissolving 1.0 M LiFSI in an organic solvent consisting of ethylene carbonate / ethyl methyl carbonate (EC / EMC mixing volume ratio of 3 / 7), respectively. Subsequently, the mixture was heat-treated at 60°C for 3 hours in an oxygen-blocking atmosphere to carry out a crosslinking reaction, thereby preparing a gel electrolyte containing the electrolyte on a crosslinked polymer of the ETPTA.

[0093] After the positive and negative electrodes were each formed by pressing, the gel electrolyte was interposed between them to manufacture an electrode assembly. The manufactured electrode assembly was placed inside a battery case to manufacture a lithium secondary battery.

[0094]

[0095] Comparative Example 1: Manufacturing of a cathode and lithium secondary battery

[0096] A positive electrode and a lithium secondary battery including the same were manufactured in the same manner as in Example 1, except that oxide-based solid electrolyte particles were not used in the manufacture of the positive electrode.

[0097]

[0098] Comparative Example 2: Manufacturing of a positive electrode and a lithium secondary battery

[0099] A positive electrode and a lithium secondary battery including the same were manufactured in the same manner as in Example 3, except that oxide-based solid electrolyte particles were not used in the manufacture of the positive electrode.

[0100]

[0101] Experimental Example 1 - Battery Resistance Evaluation by State of Charge (SOC) for Small Cells

[0102] First, the lithium secondary batteries of Examples 1 and 2 and Comparative Example 1 were manufactured as small cells with a capacity of 60 mAh. For the lithium secondary batteries of Examples 1 and 2 and Comparative Example 1 in the form of such small cells, charge and discharge tests were repeatedly performed at room temperature (approximately 25°C) under the conditions of 1) 0.2C - 0.33C charge (cut-off: 4.2 V, 0.05 C) and 2) 0.2C - 0.33C discharge (cut-off: 2.5 V), and the resistance was measured according to the state of charge (SOC).

[0103] Specifically, the above charge-discharge test was repeatedly performed under the SOC setting of 10% to 90%, and the DC resistance (2.5C discharge (cut-off: 10 s or 2 V)) was measured after each charge-discharge.

[0104] As a result of the resistance measurement according to the state of charge, the resistance evaluation results at SOC 10%, 50%, and 90% are shown in Table 1 below:

[0105] SOC(%) Comparative Example 1(Ω) Example 2(Ω) Example 1(Ω) 900.750.7260.718500.6960.6890.672101.2621.2251.198

[0106] Referring to Table 1 above, it was confirmed that the lithium secondary batteries of Examples 1 and 2 exhibited lower resistance and higher ionic conductivity at different charge states compared to Comparative Example 1.

[0107]

[0108] Experimental Example 2 - Battery Resistance Evaluation by State of Charge (SOC) for Large Cells

[0109] The lithium secondary batteries of Examples 1 and 3 and Comparative Examples 1 and 2 were manufactured as large cells with a capacity of 40 Ah to confirm the characteristics by type of electrolyte. For the lithium secondary batteries of Examples 1 and 3 and Comparative Examples 1 and 2 in this large cell type, charge and discharge tests were repeatedly performed at room temperature (approximately 25°C) under the conditions of 1) 0.2 C - 0.33 C charge (cut-off: 4.2 V, 0.05 C) and 2) 0.2 C - 0.33 C discharge (cut-off: 2.5 V), and the resistance was measured by state of charge (SOC).

[0110] Specifically, the above charge-discharge test was repeatedly performed under the SOC setting of 10% to 90%, and the DC resistance (2.5C discharge (cut-off: 10 s or 2 V)) was measured after each charge-discharge.

[0111] As a result of the resistance measurement according to the state of charge, the resistance evaluation results at SOC 10%, 50%, and 90% are shown in Table 2 below:

[0112] SOC(%)Comparative Example 1(Ω)Comparative Example 2(Ω)Example 1(Ω)Example 2(Ω)901.9812.2521.8712.098501.8792.1871.8011.98103.4683.6413.1723.609

[0113] Referring to Table 2 above, compared to the batteries of Comparative Example 1 and Example 1, which applied an electrolyte and a separator, the batteries of Comparative Example 2 and Example 2, which applied a gel electrolyte, appear to have a generally increased resistance due to the difference in the electrolyte form, which appears to be due to the relatively low ionic conductivity of the gel electrolyte.

[0114] However, regardless of the form of the electrolyte, it was confirmed that the lithium secondary batteries of Examples 1 and 2, in which an oxide-based solid electrolyte was added to the positive electrode as in the examples, exhibited lower resistance and higher ionic conductivity at each state of charge compared to Comparative Examples 1 and 2, respectively.

[0115]

[0116] Experimental Example 2 - Low-Temperature Characteristics Evaluation

[0117] For the lithium secondary batteries of Example 1 and Comparative Example 1, a discharge test was conducted for 30 seconds starting from an SOC of 50% at a temperature of -10°C.

[0118] Specifically, first, charging was performed up to 50% SOC under the conditions of 0.1C - 0.33C at a temperature of 25℃. Then, the lithium secondary battery with 50% SOC was stored in a chamber at -10℃ for 3 to 5 hours to cool the temperature of the lithium secondary battery to -10℃. Then, discharge was performed under the condition of 1C with a cut-off of 30 s or 2.5 V, and the degree of voltage drop according to the discharge time was measured.

[0119] Next, the battery was recharged to the same amount of discharge as above under the conditions of -10℃ and 0.1C, and the discharge test was repeated while changing the discharge rate condition from 1C to 2C, 3C, 3.5C, 4.5C, 6C, and 8C. Through the above process, the voltage drop for each discharge time was measured while the discharge was performed for 30 seconds at each discharge rate, and the results are shown in Figure 1. The low-temperature output characteristics calculated from this are shown in Table 3 below:

[0120] Discharge rate comparison example 1 Output (@-10℃; Wh) Example 1 (@-10℃; Wh) 1 C 1.067 1.088 2 C 1.968 2.020 3 C 2.755 2.852 3.5 C 3.093 3.172 4.5 C 2.262 2.718 6 C 0.146 1.223 8 C 0.021 0.022

[0121] Referring to Fig. 1 and Table 3, it was confirmed that the lithium secondary battery of Example 1 exhibited a lower voltage drop at the beginning of discharge and superior output characteristics compared to Comparative Example 1 at a low temperature of -10°C.

Claims

1. Containing a positive electrode, a negative electrode, and an electrolyte including a lithium salt and a non-aqueous organic solvent, The positive electrode comprises a positive electrode current collector; and an active material layer formed on the positive electrode current collector and including an oxide-based solid electrolyte having a positive electrode active material, a conductive material, and a lithium ion source, A lithium secondary battery in which the positive electrode active material and the oxide-based solid electrolyte are dispersed in the active material layer in the form of particles, and the average particle diameter (D50) of the particles is such that the oxide-based solid electrolyte: the positive electrode active material has a ratio of 1:4 to 1:

90.

2. In the first paragraph, the positive electrode active material comprises a lithium metal oxide including lithium and two or more metals selected from the group consisting of nickel, manganese, cobalt, and aluminum, A lithium secondary battery wherein the lithium metal oxide contains nickel in an amount of 60 mol% or more based on the total metal content excluding lithium.

3. A lithium secondary battery according to claim 1, wherein the oxide-based solid electrolyte comprises at least one lithium metal oxide or lithium metal phosphate selected from a Nasicon-type solid electrolyte, a Lisicon-type solid electrolyte, a Garnet-type solid electrolyte, a Perovskite-type solid electrolyte, and a LiPON-type solid electrolyte.

4. A lithium secondary battery according to claim 1, wherein the oxide-based solid electrolyte comprises at least one selected from the group consisting of a LAGP (lithium aluminum germanium phosphate)-based compound, an LLZO (lithium lanthanum zirconium oxide)-based compound, a LATP (lithium aluminum titanium phosphate)-based compound, an LLZTO (lithium lanthanum zirconium tantalum oxide)-based compound, an LLTO (lithium lanthanum titanium oxide)-based compound, a LSTP (lithium silicon titanium phosphate)-based compound, and a LGPO (lithium germanium phosphate)-based compound.

5. In the first paragraph, the positive electrode active material has an average particle diameter (D50) of 5 to 15㎛, A lithium secondary battery in which the above oxide-based solid electrolyte has an average particle diameter (D50) of 100 nm to 1.2 μm.

6. A lithium secondary battery according to claim 1, wherein the oxide-based solid electrolyte is included in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the positive electrode active material.

7. A lithium secondary battery according to claim 1, wherein the conductive material comprises carbon nanotubes or carbon nanofibers, and the active material layer further comprises a binder.

8. In the first paragraph, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 A lithium secondary battery comprising at least one selected from the group consisting of LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (lithium bis(fluorosulfonyl) imide, LiN(SO2F)2), LiBETI (lithium bis(perfluoroethanesulfonyl) imide, LiN(SO2CF2CF3)2) and LiTFSI (lithium bis(trifluoromethanesulfonyl) imide, LiN(SO2CF3)2).

9. A lithium secondary battery according to claim 1, wherein the lithium salt is included in the electrolyte at a concentration of 0.5 M to 6 M.

10. A lithium secondary battery according to claim 1, wherein the electrolyte further comprises a diluent having a solubility for the lithium salt that is at least 10 times lower than that of the non-aqueous organic solvent.

11. A lithium secondary battery in claim 10, wherein the diluent comprises at least one selected from the group consisting of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl) ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), methoxynonafluorobutane (MOFB), and ethoxynonafluorobutane (EOFB).

12. In the first paragraph, further comprising a separator interposed between the positive and negative electrodes, or A lithium secondary battery in which the electrolyte has the form of an electrolyte membrane or electrolyte film containing the lithium salt and a non-aqueous organic solvent within a polymer matrix and is interposed between the positive electrode and the negative electrode.

Citation Information

Patent Citations

  • Mixed powder for all-solid-state lithium-ion battery, mixed paste for all-solid-state lithium-ion battery, electrode, and all-solid-state lithium-ion battery

    JP2021114407A

  • Low-flammability electrolyte for stable operation of electrochemical devices

    JP2021500704A

  • Active material composite particles, electrode composite comprising the same and method of producing the same and all solid battery

    KR1020180043887A

  • Cosmetic composition for improving atopic dermatitis and dry skin containing Taraxacum Coreanum Phytoplacenta Culture Extract

    KR102552616B1

  • Apparatus for measuring crack depth for safety inspection, precise safety diagnosis, and performance evaluation

    KR102591428B1

Cited By

  • Lithium ion battery

    CN119400963A

  • Medium-concentration electrolyte suitable for extremely cold environment, preparation method and lithium metal soft package battery

    CN119627228A

  • Lithium ion secondary battery

    CN119890407A

  • A lithium-ion secondary battery

    CN119890407B

  • Lithium-ion secondary battery

    US12506173B1