Method for preparing lithium extraction electrode and use thereof
By forming a porous carbon network and a uniform mass transfer channel in the electrode, the problem of low lithium ion transmission efficiency in electrochemical lithium extraction technology is solved, the recovery rate of lithium and the stability of the electrode are improved, and efficient lithium ion lithium extraction is achieved .
Patent Information
- Application Number
- PCT/CN2023/092281
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-14
AI Technical Summary
The existing electrochemical lithium extraction technology has low lithium ion transmission efficiency in salt lakes, resulting in low lithium extraction efficiency and uneven mass transfer channels, affecting the recovery rate and cost of lithium.
By dispersing the lithium iron phosphate synthetic raw materials in the polymer network at high temperature calcination to form a carbon conductive network, and reacting with CO2 at high temperature to form a porous carbon network, combining the adsorption and drying process of ammonium bicarbonate to form a uniform mass transfer channel, improving Conductivity and cyclic stability of the electrode.
It significantly improves the transmission rate of lithium ions and the efficiency of lithium extraction, improves the conductivity of the electrode, promotes the mass transfer of solution, and improves the recovery rate of lithium and the stability of the electrode.
Smart Images

Figure CN2023092281_14112024_PF_FP_ABST
Abstract
Description
Preparation method of lithium extraction electrode and its application Technical Field
[0001] The present disclosure belongs to the technical field of lithium extraction from salt lakes, and particularly relates to a preparation method of a lithium extraction electrode and its application. Background Art
[0002] Lithium is widely used in lithium batteries. With the rapid development of the new energy sector, market demand for lithium resources is rapidly increasing. Low-cost, efficient lithium resource development has become a key factor in ensuring companies' ability to compete in this market. Discovered lithium resources in nature are primarily found in salt lake brines, seawater, and ores, with salt lake lithium accounting for approximately 70%. Due to the high cost and difficulty of mining lithium ore, and its increasing depletion and depletion with continued mining, extracting lithium from salt lake brines has become a trend in lithium resource development.
[0003] Currently, the main methods for extracting lithium from brine at home and abroad include precipitation, solvent extraction, evaporative crystallization, electrodialysis, and ion exchange adsorption. Precipitation, a mature lithium extraction technology, has the disadvantages of high energy consumption, complex process flow, and high cost, and the lithium recovery rate is also low. Extraction methods offer rapid lithium extraction rates, but the dissolution of the extractant in the brine can easily lead to environmental pollution. Adsorption methods also suffer from low adsorption capacity, adsorbent loss, and high water consumption. In recent years, many researchers at home and abroad have conducted extensive research and exploration into new lithium extraction processes, and electrochemical lithium extraction technology has shown promising value and application prospects.
[0004] The principle of electrochemical lithium extraction is to charge the working electrode to release lithium ions, forming a lithium ion sieve. Discharging the working electrode in brine allows lithium ions to selectively enter the lithium ion sieve, and lithium enrichment is achieved through a cyclic charge-discharge process. However, due to the low lithium concentration in brine, the presence of large amounts of impurities such as magnesium and sodium, and the high viscosity of the brine, mass transfer within the electrode is slow, resulting in low efficiency of electrochemical lithium extraction. Therefore, improving the ion transport rate of the electrode is of great significance.
[0005] The conductivity and cycle stability of the electrode are usually improved by coating the surface of the electrode active material with a layer of carbon. However, ordinary carbon coatings are dense or have tiny pores. When used for lithium extraction from salt lakes, they cannot form uniform mass transfer channels, resulting in slow solution transfer and reduced lithium extraction efficiency.
[0006] Summary of the Invention
[0007] The present disclosure aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present disclosure proposes a preparation method and application of a lithium extraction electrode, firstly dispersing the synthetic raw materials of lithium iron phosphate in a polymer network, calcining at high temperature to generate lithium iron phosphate while carbonizing the polymer into a carbon conductive network, then combining with CO2 high temperature treatment to form a porous carbon network, and finally mixing with a pore-forming agent so that the pore-forming agent is uniformly adsorbed on the conductive carbon. When the electrode is dried, the pore-forming agent volatilizes to form a uniform mass transfer channel, thereby improving the lithium extraction efficiency.
[0008] According to one aspect of the present disclosure, a method for preparing a lithium extraction electrode is proposed, comprising the following steps:
[0009] S1: mixing a lithium source, an iron source, a phosphorus source and a polymer in a solvent, and drying the obtained mixture to obtain a dry material;
[0010] S2: The dry material is first calcined at a temperature of 600-900° C. under a protective atmosphere, and then carbon dioxide or water vapor is introduced and calcined for a second time at a temperature of 750-900° C. to obtain lithium iron phosphate;
[0011] S3: soaking the lithium iron phosphate in an ammonium bicarbonate solution, and performing solid-liquid separation to obtain a solid material;
[0012] S4: mixing the solid material, the conductive agent, the binder and N-methylpyrrolidone to prepare a slurry, coating the slurry on a current collector, and heating and drying the mixture to obtain the lithium extraction electrode.
[0013] In some embodiments of the present disclosure, in step S1, the lithium source is at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium dihydrogen phosphate, or lithium acetate.
[0014] In some embodiments of the present disclosure, in step S1, the iron source is at least one of ferrous oxalate, ferric nitrate or ferric phosphate.
[0015] In some embodiments of the present disclosure, in step S1, the phosphorus source is at least one of ammonium dihydrogen phosphate or phosphoric acid.
[0016] In some embodiments of the present disclosure, in step S1, the polymer is at least one of polypyrrole, polyethylene, polypropylene, polystyrene, polycarbonate or polyaniline.
[0017] In some embodiments of the present disclosure, in step S1, the solvent is at least one of ethanol, acetone, methanol or water.
[0018] In some embodiments of the present disclosure, in step S1, the lithium source, iron source, and phosphorus source are mixed in a molar ratio of Li:Fe:P=(1.2-2):(1-1.1):1.
[0019] In some embodiments of the present disclosure, in step S1, the amount of the polymer added is 1%-10% of the mass of the synthesized lithium iron phosphate.
[0020] In some embodiments of the present disclosure, in step S1, the mixing method is ball milling, and the ball milling time is 4-12 hours. Ball milling can refine the raw material particles and make the raw materials mixed more uniformly.
[0021] In some embodiments of the present disclosure, in step S2, the first calcination time is 12-24 hours.
[0022] In some embodiments of the present disclosure, in step S2, the temperature is increased to the temperature of the first calcination at a heating rate of 5-10°C / min.
[0023] In some embodiments of the present disclosure, in step S2, the flow rate of the carbon dioxide or water vapor is 0.05-0.5 L / min.
[0024] In some embodiments of the present disclosure, in step S2, the second calcination time is 1-4 hours.
[0025] In some embodiments of the present disclosure, in step S2, the temperature is increased to the temperature of the second calcination at a heating rate of 2-8°C / min.
[0026] In some embodiments of the present disclosure, in step S3, the concentration of the ammonium bicarbonate solution is 0.1-1 mol / L, and the solid-to-liquid ratio of the lithium iron phosphate to the ammonium bicarbonate solution is 1 g / (2-6) mL.
[0027] In some embodiments of the present disclosure, in step S3, the soaking time is 2-6 hours.
[0028] In some embodiments of the present disclosure, in step S4, the density of the slurry coating is 150-200 mg / cm 2 .
[0029] In some embodiments of the present disclosure, in step S4, the heating and drying temperature is 50-80° C. and the time is 4-8 hours.
[0030] The present disclosure also provides the use of the lithium extraction electrode prepared by the preparation method in extracting lithium from salt lakes.
[0031] According to the embodiments of the present disclosure, there are at least the following beneficial effects:
[0032] The present invention first mixes and grinds a lithium source, an iron source, a phosphorus source and a polymer, and then calcines them at high temperature. While generating lithium iron phosphate, the polymer is carbonized to form a carbon conductive network, so that the synthesized lithium iron phosphate is distributed in the carbon conductive network. Then, at high temperature, part of the carbon reacts with CO2 / water vapor to convert it into CO gas to escape, forming a porous carbon network. When the lithium iron phosphate embedded with the porous carbon network is mixed with an ammonium bicarbonate solution, the ammonium bicarbonate is easily adsorbed on the porous carbon, so that a large amount of ammonium bicarbonate is evenly distributed around the lithium iron phosphate particles. During the electrode drying process, the ammonium bicarbonate is thermally decomposed to produce a large amount of gas, forming a uniform mass transfer channel between the lithium iron phosphate particles. Therefore, the present invention can not only improve the conductive properties of the material and accelerate the migration of electrons, but also promote solution mass transfer and improve lithium extraction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The present disclosure is further described below with reference to the accompanying drawings and embodiments, wherein:
[0034] FIG1 is a comparison of the lithium extraction efficiency of the electrodes of the embodiment of the present disclosure and the comparative example. DETAILED DESCRIPTION
[0035] The following will clearly and completely describe the concept and technical effects of the present disclosure in conjunction with embodiments to fully understand the purpose, features and effects of the present disclosure.
[0036] Example 1
[0037] This example prepares a salt lake lithium extraction electrode using the electrochemical deintercalation method. The specific process is as follows:
[0038] (1) Weigh 29 g of lithium hydroxide, 144 g of ferrous oxalate, 115 g of ammonium dihydrogen phosphate, and 15 g of polyaniline into a ball mill, add anhydrous ethanol as a dispersant, and mix and ball mill for 12 h.
[0039] (2) After the ball-milled material of step (1) is dried, it is placed in a tubular furnace, and in a nitrogen atmosphere, the temperature is raised to 900°C at a rate of 10°C / min, and calcined for 12 hours. Then, CO2 gas is introduced at a flow rate of 0.5L / min and kept at 900°C for 2 hours to allow part of the carbon to react with CO2 to obtain lithium iron phosphate.
[0040] (3) Dissolve ammonium bicarbonate in deionized water to prepare a 1 mol / L solution, place the lithium iron phosphate obtained in step (2) in the ammonium bicarbonate solution at a solid-liquid ratio of 1 g: 2 mL, mix well, let stand for 3 h, filter, and air-dry to obtain a solid material.
[0041] (4) The solid material, acetylene black and PVDF of step (3) were weighed in a mass ratio of 8:1:1, added to N-methylpyrrolidone (NMP), stirred thoroughly to form a slurry, and the slurry was evenly coated on the titanium mesh current collector with a coating density of 200 mg / cm 2 , and dried at 80 °C for 5 h to obtain a porous electrode.
[0042] Example 2
[0043] This example prepares a salt lake lithium extraction electrode using the electrochemical deintercalation method. The specific process is as follows:
[0044] (1) Weigh 45 g of lithium carbonate, 242 g of ferric nitrate, 115 g of ammonium dihydrogen phosphate, and 8 g of polyaniline into a ball mill, add anhydrous ethanol as a dispersant, and mix and ball mill for 8 h.
[0045] (2) After the ball-milled material of step (1) is dried, it is placed in a tube furnace and heated to 600°C at a rate of 5°C / min in a nitrogen atmosphere, calcined for 24 hours, and then CO2 gas is introduced at a flow rate of 0.1 L / min, and the temperature is raised to 800°C at a rate of 5°C / min. The temperature is kept at this temperature for 4 hours to allow part of the carbon to react with CO2 to obtain lithium iron phosphate.
[0046] (3) Dissolve ammonium bicarbonate in deionized water to prepare a 0.1 mol / L solution, place the lithium iron phosphate obtained in step (2) into the ammonium bicarbonate solution at a solid-liquid ratio of 1 g:6 mL, mix well, let stand for 2 h, filter, and air-dry to obtain a solid material.
[0047] (4) The solid material, acetylene black and PVDF of step (3) were weighed in a mass ratio of 8:1:1, added to N-methylpyrrolidone (NMP), stirred thoroughly to form a slurry, and the slurry was evenly coated on the titanium mesh current collector with a coating density of 150 mg / cm 2 , and dried at 65 °C for 8 h to obtain a porous electrode.
[0048] Example 3
[0049] This example prepares a salt lake lithium extraction electrode using the electrochemical deintercalation method. The specific process is as follows:
[0050] (1) Weigh 36 g of lithium hydroxide, 152 g of ferrous oxalate, 121 g of ammonium dihydrogen phosphate, and 2.2 g of polyaniline into a ball mill, add anhydrous ethanol as a dispersant, and mix and ball mill for 12 h.
[0051] (2) After the ball-milled material of step (1) is dried, it is placed in a tubular furnace, and in a nitrogen atmosphere, the temperature is raised to 800°C at a rate of 8°C / min, and calcined for 15 hours. Then, water vapor is introduced at a flow rate of 0.05 L / min and kept at 800°C for 1 hour to allow part of the carbon to react with the water vapor to obtain lithium iron phosphate.
[0052] (3) Dissolve ammonium bicarbonate in deionized water to prepare a 0.5 mol / L solution, place the lithium iron phosphate obtained in step (2) in the ammonium bicarbonate solution at a solid-liquid ratio of 1 g:4 mL, mix well, let stand for 4 hours, filter, and air-dry to obtain a solid material.
[0053] (4) The solid material, acetylene black and PVDF of step (3) were weighed in a mass ratio of 8:1:1, added to N-methylpyrrolidone (NMP), stirred thoroughly to form a slurry, and the slurry was evenly coated on the titanium mesh current collector with a coating density of 150 mg / cm 2 , and dried at 60 °C for 8 h to obtain a porous electrode.
[0054] Comparative Example 1
[0055] This comparative example prepared a salt lake lithium extraction electrode using the electrochemical deintercalation method. The difference from Example 1 is that no CO2 gas treatment was introduced. The specific process is as follows:
[0056] (1) Weigh 29 g of lithium hydroxide, 144 g of ferrous oxalate, 115 g of ammonium dihydrogen phosphate, and 15 g of polyaniline into a ball mill, add anhydrous ethanol as a dispersant, and mix and ball mill for 12 h.
[0057] (2) After the ball-milled material of step (1) is dried, it is placed in a tube furnace, heated to 900° C. at a rate of 10° C. / min under a nitrogen atmosphere, and calcined for 12 h to obtain lithium iron phosphate.
[0058] (3) Dissolve ammonium bicarbonate in deionized water to prepare a 1 mol / L solution, place the lithium iron phosphate obtained in step (2) in the ammonium bicarbonate solution at a solid-liquid ratio of 1 g: 2 mL, mix well, let stand for 3 h, filter, and air-dry to obtain a solid material.
[0059] (4) The solid material, acetylene black and PVDF of step (3) were weighed in a mass ratio of 8:1:1, added to N-methylpyrrolidone (NMP), stirred thoroughly to form a slurry, and the slurry was evenly coated on the titanium mesh current collector with a coating density of 200 mg / cm 2 , and dried at 80 °C for 5 h to obtain a porous electrode.
[0060] Comparative Example 2
[0061] This example prepares a salt lake lithium extraction electrode using the electrochemical deintercalation method. The difference from Example 1 is that the electrode is not immersed in an ammonium bicarbonate solution. The specific process is as follows:
[0062] (1) Weigh 29 g of lithium hydroxide, 144 g of ferrous oxalate, 115 g of ammonium dihydrogen phosphate, and 15 g of polyaniline into a ball mill, add anhydrous ethanol as a dispersant, and mix and ball mill for 12 h.
[0063] (2) After the ball-milled material of step (1) is dried, it is placed in a tubular furnace, and in a nitrogen atmosphere, the temperature is raised to 900°C at a rate of 10°C / min, and calcined for 12 hours. Then, CO2 gas is introduced at a flow rate of 0.5L / min and kept at 900°C for 2 hours to allow part of the carbon to react with CO2 to obtain lithium iron phosphate.
[0064] (3) Lithium iron phosphate, acetylene black and PVDF from step (2) were weighed in a mass ratio of 8:1:1, added to N-methylpyrrolidone (NMP), stirred thoroughly to form a slurry, and the slurry was evenly coated on the titanium mesh current collector at a coating density of 200 mg / cm 2 , and dried at 80 °C for 5 h to obtain a porous electrode.
[0065] Comparative Example 3
[0066] This example prepares a salt lake lithium extraction electrode using the electrochemical deintercalation method. The difference from Example 1 is that no CO2 gas treatment is introduced and no ammonium bicarbonate solution is immersed. The specific process is as follows:
[0067] (1) Weigh 29 g of lithium hydroxide, 144 g of ferrous oxalate, 115 g of ammonium dihydrogen phosphate, and 15 g of polyaniline into a ball mill, add anhydrous ethanol as a dispersant, and mix and ball mill for 12 h.
[0068] (2) After the ball-milled material of step (1) is dried, it is placed in a tube furnace, heated to 900° C. at a rate of 10° C. / min under a nitrogen atmosphere, and calcined for 12 h to obtain lithium iron phosphate.
[0069] (3) Lithium iron phosphate, acetylene black and PVDF from step (2) were weighed in a mass ratio of 8:1:1, added to N-methylpyrrolidone (NMP), stirred thoroughly to form a slurry, and the slurry was evenly coated on the titanium mesh current collector at a coating density of 200 mg / cm 2 , and dried at 80 °C for 5 h to obtain a porous electrode.
[0070] Test example
[0071] Lithium extraction experiment: Using the electrodes prepared in the examples and comparative examples as the positive electrode, the AgCl electrode as the negative electrode, and a 0.05 mol / L KCl solution as the electrolyte, the lithium-rich electrode was delithiated at a constant voltage of 1.0 V to obtain a lithium-poor electrode. The electrolysis apparatus was separated into an anode chamber and a cathode chamber by an anion exchange membrane. The lithium-rich electrode and the lithium-poor electrode were placed in the anode chamber and the cathode chamber, respectively. Brine with a lithium concentration of 1.52 g / L was injected into the cathode chamber, and NaCl solution was injected into the anode chamber. A voltage of 0.3 V was applied to the anode and cathode to extract lithium.
[0072] The lithium extraction efficiency during the lithium extraction process of the electrodes of the embodiment and the comparative example is shown in FIG1 , and the changes of the anode lithium concentration and the brine lithium concentration over time are shown in Table 1 .
[0073] Table 1 Anode lithium concentration and brine lithium concentration at different time points of lithium extraction
[0074] The results of Examples 1-3 in Table 1 show that the electrodes prepared using the lithium iron phosphate materials provided in Examples 1-3 exhibit high lithium extraction efficiency. This is because the porous carbon embedded in the lithium iron phosphate material can adsorb a large number of ammonium bicarbonate molecules, which easily decomposes during electrode drying to form mass transfer channels, thereby improving the adsorption and desorption efficiency of lithium ions. The amount of ammonium bicarbonate adsorbed significantly affects the lithium extraction efficiency of the electrode. When the carbon network is more pore-rich and the ammonium bicarbonate solution concentration is higher, the porous carbon easily adsorbs a large amount of ammonium bicarbonate, resulting in a high porosity during electrode preparation and better lithium extraction efficiency. After lithium extraction, the lithium concentration in the brine is lower, while the lithium concentration in the anolyte is higher.
[0075] From the results of Example 1 and Comparative Example 1, it can be seen that the lithium extraction efficiency of the electrode of Comparative Example 1 is low because Comparative Example 1 does not remove part of the carbon network, forming a porous structure, resulting in a small amount of ammonium bicarbonate adsorption, a low pore formation rate, and fewer mass transfer channels.
[0076] From the results of Example 1 and Comparative Example 2, it can be seen that the lithium extraction efficiency of the electrode of Comparative Example 2 is low because ammonium bicarbonate is not adsorbed on the porous carbon in Comparative Example 2, and further pores cannot be formed, and the solution only transfers mass through the porous carbon.
[0077] From the results of Comparative Examples 1, 2, and 3, it can be seen that the lithium extraction efficiency of the electrode in Comparative Example 3 is the lowest. This is because Comparative Example 3 neither removes part of the carbon network to form pores nor adsorbs ammonium bicarbonate on the carbon network. Mass transfer channels cannot be formed between the particles, resulting in low lithium extraction efficiency of the electrode.
Claims
1. A method for preparing a lithium extraction electrode, characterized in that: The following steps are involved: S1: mixing a lithium source, an iron source, a phosphorus source and a polymer in a solvent, and drying the obtained mixture to obtain a dry material; S2: the dry material is first calcined at a temperature of 600-900° C. under a protective atmosphere, and then carbon dioxide or water vapor is introduced to perform a second calcination at a temperature of 750-900° C. to obtain lithium iron phosphate; S3: soaking the lithium iron phosphate in an ammonium bicarbonate solution to obtain a solid material by solid-liquid separation; S4: mixing the solid material, the conductive agent, the binder and N-methylpyrrolidone to prepare a slurry, coating the slurry on a current collector, and heating and drying to obtain the lithium extraction electrode.
2. The preparation method according to claim 1, characterized in that: In step S1, the lithium source is at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium dihydrogen phosphate or lithium acetate.
3. The preparation method according to claim 1, characterized in that: In step S1, the iron source is at least one of ferrous oxalate, ferric nitrate or ferric phosphate.
4. The preparation method according to claim 1, characterized in that: In step S1, the phosphorus source is at least one of diammonium phosphate or phosphoric acid.
5. The preparation method according to claim 1, characterized in that: In step S1, the polymer is at least one of polypyrrole, polyethylene, polypropylene, polystyrene, polycarbonate or polyaniline.
6. The preparation method according to claim 1, characterized in that: In step S1, the solvent is at least one of ethanol, acetone, methanol or water.
7. The preparation method according to claim 1, characterized in that: In step S1, the lithium source, iron source and phosphorus source are mixed in a molar ratio of Li:Fe:P=(1.2-2):(1-1.1):
1.
8. The preparation method according to claim 1, characterized in that: In step S1, the amount of the polymer added is 1%-10% of the mass of the synthesized lithium iron phosphate.
9. The preparation method according to claim 1, characterized in that: In step S1, the mixing method is ball milling, and the ball milling time is 4-12 hours.
10. The preparation method according to claim 1, characterized in that: In step S2, the first calcination time is 12-24 hours.
11. The preparation method according to claim 1, characterized in that: In step S2, the temperature is raised to the first calcination temperature at a heating rate of 5-10°C / min.
12. The preparation method according to claim 1, characterized in that: In step S2, the flow rate of the carbon dioxide or water vapor is 0.05-0.5 L / min.
13. The preparation method according to claim 1, characterized in that: In step S2, the second calcination time is 1-4 hours.
14. The preparation method according to claim 1, characterized in that: In step S2, the temperature is raised to the second calcination temperature at a heating rate of 2-8°C / min.
15. The preparation method according to claim 1, characterized in that: In step S3, the concentration of the ammonium bicarbonate solution is 0.1-1 mol / L, and the solid-to-liquid ratio of the lithium iron phosphate to the ammonium bicarbonate solution is 1 g / (2-6) mL.
16. The preparation method according to claim 1, characterized in that: In step S3, the soaking time is 2-6 hours.
17. The preparation method according to claim 1, characterized in that: In step S4, the density of the slurry coating is 150-200 mg / cm 2 .
18. The preparation method according to claim 1, characterized in that: In step S4, the heating and drying is performed at a temperature of 50-80° C. for 4-8 hours.
19. Use of the lithium extraction electrode prepared by the preparation method according to any one of claims 1 to 18 in extracting lithium from salt lakes.
Citation Information
Patent Citations
Preparing method of anode active material lithium iron phosphate for lithium ionic secondary cell
CN101399343A
Preparation method of lithium iron phosphate / carbon composite cathode material
CN101931073A
Preparation method of high-conductivity porous electrode for extracting lithium from salt lake
CN113265538A
Preparation method of lithium iron phosphate, lithium iron phosphate material and lithium ion battery
CN114906831A
Methods for Synthesizing Lithium Iron Phosphate as a Material for the Cathode of Lithium Batteries
US20090035204A1