Lithium battery positive electrode material, and preparation method therefor and use thereof

WO2024229646A1PCT designated stage expired Publication Date: 2024-11-14GUANGDONG BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
PCT/CN2023/092669
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-14

Smart Images

  • Figure CN2023092669_14112024_PF_FP_ABST
    Figure CN2023092669_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure belongs to the technical field of lithium batteries, and in particular relates to a lithium battery positive electrode material, and a preparation method therefor and use thereof. The lithium battery positive electrode material provided by the present disclosure is doped with an R element and an M element. The R element is doped into the bulk phase, and the M element is doped on the surface. By means of optimizing a selection range of the R and M elements, R is controlled to be selected from at least one of Ni, Co, Mn, Zr, Al, Mg, Ti, Sr, W, Y, Mo, Sb, Nb, Sn, Zn, La, Ce, Ta, B, and F, M is controlled to be selected from at least five of Li, B, Al, Ti, Ni, Co, Mn, Ce, La, W, Nb, Mo, Zr, Mg, Zn, Sb, Sn, Ta, and Y, and an ion radius difference value of any two elements is controlled, so as to enable various kinds of atoms to enter surface lattices of the positive electrode material and share crystallization sites, thereby forming a single-phase solid solution structure.
Need to check novelty before this filing date? Find Prior Art

Description

A lithium battery positive electrode material, preparation method and application thereof Technical Field

[0001] The present disclosure belongs to the technical field of lithium batteries, and in particular relates to a lithium battery positive electrode material, a preparation method thereof, and applications. Background Art

[0002] At present, lithium-ion power batteries have been widely used in new energy vehicles. Improving the energy density of automotive lithium-ion power batteries and alleviating travel anxiety are urgent issues that need to be addressed. To further improve the energy density, we can start from two aspects: improving the operating voltage platform and capacity. When the battery material system does not change, the former is relatively fixed, so it is more important to further improve the gram capacity of the positive electrode material. Increasing the operating voltage of the positive electrode material so that more lithium ions can be released from the lattice of the positive electrode material is the most direct and effective way to increase the gram capacity of the positive electrode material. As lithium ions are released, the side reactions between the surface interface of the material and the electrolyte are significantly enhanced, accompanied by gas production and other phenomena, which pose a huge safety hazard. Therefore, the risk of gas production must be reduced.

[0003] Currently, methods to suppress gas production in cathode materials under high voltages typically involve doping, coating, and electrolyte additives. Effective process measures include iso-gradient structures and core-shell structures. The coating process plays a crucial role in suppressing side reactions between the cathode material surface and the electrolyte, phase transitions on the cathode material surface, and the release of active oxygen from the lattice at high operating voltages. Chinese patent CN 106935911B discloses a method for improving gas production during high-temperature storage of cathode materials using a gas-suppressing additive, but this method does not fundamentally reduce the gas production of the cathode material.

[0004] The currently proposed methods for inhibiting gas production of positive electrode materials under high voltage cannot effectively reduce the gas production of positive electrode materials during circulation and storage, and cannot fundamentally reduce the risk of gas production.

[0005] In view of this, the present disclosure is proposed.

[0006] Summary of the Invention

[0007] The purpose of the present disclosure includes providing a lithium battery positive electrode material, a preparation method and application thereof, aiming to effectively reduce the gas production of the positive electrode material during circulation and storage.

[0008] In order to achieve the above-mentioned purpose of the present disclosure, the following technical solutions can be adopted:

[0009] In the first aspect, the solution provided by the present disclosure includes a lithium battery positive electrode material, the general formula of the lithium battery positive electrode material is LiNi x Co y Mn z R a O2+δ @M b where R is a bulk doping element and M is a surface doping element;

[0010] wherein, R is selected from at least one of Ni, Co, Mn, Zr, Al, Mg, Ti, Sr, W, Y, Mo, Sb, Nb, Sn, Zn, La, Ce, Ta, B and F;

[0011] M is selected from at least five of Li, B, Al, Ti, Ni, Co, Mn, Ce, La, W, Nb, Mo, Zr, Mg, Zn, Sb, Sn, Ta and Y, and for several elements corresponding to M, the ratio of the difference in ionic radii between any two elements to the larger ionic radius between the two is less than 0.15;

[0012] In the general formula, 0 < x < 1, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 0.6, 0.001 ≤ a ≤ 0.03, 0.001 ≤ b ≤ 0.05, x + y + z + a = 1, and δ changes with the value of b to satisfy electroneutrality.

[0013] In some embodiments of the present disclosure, R is selected from at least one of Zr, Al, Ti, Sr, W, Y, Mo, Ta and La.

[0014] In some embodiments of the present disclosure, M is selected from at least five of Li, Al, Ti, Ni, Co, Ce, W, Mo, Zr, Mg, Zn, Sb and Ta.

[0015] In some embodiments of the present disclosure, 0.3 < x ≤ 1, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 0.4, 0.001 ≤ a ≤ 0.03, 0.001 ≤ b ≤ 0.05.

[0016] In some embodiments of the present disclosure, for several elements corresponding to M, the number of doped atoms of each element accounts for 5% - 35% of the total number of doped atoms corresponding to M.

[0017] In some embodiments of the present disclosure, the morphology of the lithium battery cathode material includes at least one of polycrystalline materials, quasi-single crystal materials and single crystal materials, and the particle size D50 of the quasi-single crystal materials and single crystal materials is 2 μm - 6 μm.

[0018] In a second aspect, the solution provided by the present disclosure further includes a method for preparing a lithium battery cathode material, including: using a nickel-cobalt-manganese hydroxide precursor, a lithium salt, a first additive containing R element and a second additive containing M element as raw materials to prepare the lithium battery cathode material.

[0019] In some embodiments of the present disclosure, the process includes: mixing a nickel-cobalt-manganese hydroxide precursor, a lithium salt, and a first additive and performing a primary sintering; and mixing the sintered product with a second additive and LiNO 3 and performing a secondary sintering.

[0020] In some embodiments of the present disclosure, the doping amount of the doping element in the first additive is 2000 ppm-5000 ppm, calculated based on the mass ratio of the doping element in the first additive to the nickel-cobalt-manganese hydroxide precursor.

[0021] In some embodiments of the present disclosure, the total doping amount of several doping elements in the second additive is 5000 ppm-10000 ppm, calculated as the mass ratio of the total amount of doping elements in the second additive to the mass of the product after the primary sintering.

[0022] In some embodiments of the present disclosure, the sintering temperature of the primary sintering is 750° C.-1050° C., and the sintering time is 20 h-40 h.

[0023] In some embodiments of the present disclosure, the secondary sintering process includes: first subjecting the material to be sintered to high-temperature pulse sintering, and then subjecting the material to be sintered to low-temperature sintering after cooling;

[0024] The sintering temperature of the high-temperature pulse sintering is 700° C.-980° C., the sintering temperature of the low-temperature sintering is 450° C.-950° C., and the sintering temperature of the high-temperature pulse sintering is controlled to be higher than the sintering temperature of the low-temperature sintering.

[0025] In some embodiments of the present disclosure, the sintering time of high temperature pulse sintering is 5 min-60 min.

[0026] In some embodiments of the present disclosure, the sintering time of low-temperature sintering is 3 hours to 8 hours.

[0027] In some embodiments of the present disclosure, by controlling the amount of LiNO 3 added, the molar ratio of the added lithium to the molar ratio of the residual lithium in the product after the primary sintering is 20-50:100.

[0028] In some embodiments of the present disclosure, the lithium salt is selected from at least one of LiOH and Li2CO3.

[0029] In some embodiments of the present disclosure, the amount of lithium salt added is controlled so that the molar ratio of lithium to the total amount of nickel, cobalt and manganese is 1.03-1.07:1.

[0030] In some embodiments of the present disclosure, the first additive is selected from at least one of oxides, hydroxides, oxyhydroxides, and carbonates corresponding to the doping element.

[0031] In some embodiments of the present disclosure, the second additive is selected from at least one of oxides, hydroxides, oxyhydroxides, and carbonates corresponding to the doping element.

[0032] In some embodiments of the present disclosure, the product obtained after the primary sintering is crushed and then mixed with the second additive and LiNO3 for secondary sintering.

[0033] In some embodiments of the present disclosure, the crushing process is to control the particle size D50 after crushing to be 2 μm-6 μm.

[0034] In some embodiments of the present disclosure, both the primary sintering and the secondary sintering are performed in an oxygen atmosphere.

[0035] In some embodiments of the present disclosure, the oxygen atmosphere is controlled to have an oxygen volume fraction of 22%-99.99%.

[0036] In some embodiments of the present disclosure, after the secondary sintering is completed, the product is screened, iron removed, and packaged to obtain a finished product.

[0037] In a third aspect, the solution provided by the present disclosure also includes a positive electrode sheet prepared using the lithium battery positive electrode material in the above embodiment as an active material.

[0038] In a fourth aspect, the solution provided by the present disclosure also includes a lithium battery, including the positive electrode plate in the above embodiment.

[0039] In a fifth aspect, the solution provided by the present disclosure also includes an electrical device, including the lithium battery in the above embodiment.

[0040] The lithium battery positive electrode material provided by the present invention is doped with R elements and M elements, where R elements are bulk doped and M is surface doped. By optimizing the selection range of R and M elements, M is controlled to select at least five of Li, B, Al, Ti, Ni, Co, Mn, Ce, La, W, Nb, Mo, Zr, Mg, Zn, Sb, Sn, Ta and Y, and controlling the difference in ionic radius between any two elements, multiple atoms enter the surface lattice of the positive electrode material, share crystallization sites, and form a single-phase solid solution structure, the entropy of which increases with the increase in the number of elements. When the increase in entropy is greater than the increase in enthalpy, the Gibbs free energy of the system decreases, thereby improving the stability of the crystal structure, thereby effectively reducing the gas production of the positive electrode material during circulation and storage, and helping to further improve the electrochemical properties of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0042] FIG1 is a schematic diagram of the surface confined doping principle provided by the present disclosure;

[0043] FIG2 is a process flow chart of the preparation method provided by the present disclosure;

[0044] FIG3 is an overall schematic diagram of the coating effect of the positive electrode material in Example 1 of the present disclosure;

[0045] FIG4 is a schematic diagram showing the effect of forming an island-shaped coating in Comparative Example 1 of the present disclosure;

[0046] FIG5 is a schematic diagram showing the effect of forming an island-shaped coating in Comparative Example 8 of the present disclosure;

[0047] FIG6 is a comparison chart of gas production between Example 1 and Comparative Example 1 when stored at 70° C. DETAILED DESCRIPTION

[0048] The embodiments of the present disclosure will be described in detail below with reference to the examples. However, those skilled in the art will appreciate that the following examples are intended only to illustrate the present disclosure and should not be construed as limiting the scope of the present disclosure. Where specific conditions are not specified in the examples, the experiments were performed under conventional conditions or the conditions recommended by the manufacturer. Where the manufacturer of the reagents or instruments is not specified, all are commercially available conventional products.

[0049] The endpoints of the ranges and any values ​​disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.

[0050] Conventional dry coating processes typically result in a point-like coating on the surface of cathode materials, forming a discontinuous coating layer. The exposed surface interface is a highly susceptible site for various side reactions. The high-entropy material derived from a high-entropy alloy (HEA) disclosed herein is a multi-component, single-phase solid solution characterized by shared crystallization sites among multiple elements. Its entropy increases with the number of elements present. When the increase in entropy is greater than the increase in enthalpy, the Gibbs free energy of the system decreases, thereby enhancing the stability of the crystal structure and ultimately forming a continuous surface coating.

[0051] Referring to FIG1 , the present disclosure provides a lithium battery positive electrode material, the general formula of which is LiNi x Co y Mn z R a O 2+δ @M b , R is the bulk doping element, and M is the surface doping element; most of the bulk doping elements are distributed inside the material, and most of the surface doping elements are distributed on the surface of the material.

[0052] In the general formula, R is selected from at least one of Ni, Co, Mn, Zr, Al, Mg, Ti, Sr, W, Y, Mo, Sb, Nb, Sn, Zn, La, Ce, Ta, B, and F; M is selected from at least five of Li, B, Al, Ti, Ni, Co, Mn, Ce, La, W, Nb, Mo, Zr, Mg, Zn, Sb, Sn, Ta, and Y. Among the elements corresponding to M, the ratio of the difference in ionic radius between any two elements to the larger ionic radius between the two is less than 0.15. Only when the ionic radius difference is less than 15% (i.e., 0.15) can an infinite solid solution be formed. When it is greater than 15%, a limited solid solution is generally formed or no solid solution can be formed. By controlling the selection range of R and M and precisely controlling the ionic radius difference between any two elements among the elements corresponding to M, the final product can fully utilize the advantages of surface confinement doping and the "entropy stabilization effect", effectively reducing gas production of the positive electrode material during cycling and storage.

[0053] Specifically, R can be selected from any one or several of the above elements; M can be selected from any five, any six or more of the above elements, but it is necessary to satisfy that the ratio of the difference between the ionic radius of any two elements and the larger ionic radius between the two is less than 0.15, that is, the difference between the ionic radius of any two elements should not be too large.

[0054] It should be added that the ionic radius of an element can be queried based on its valence state. Various ionic radii can be queried by searching for shannon radii.

[0055] Optionally, R is selected from at least one of Zr, Al, Ti, Sr, W, Y, Mo, Ta, and La; and M is selected from at least five of Li, Al, Ti, Ni, Co, Ce, W, Mo, Zr, Mg, Zn, Sb, and Ta. Selecting the above elements for R and M further improves the stability of the crystal structure.

[0056] In the general formula, 0 < x < 1, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 0.6, 0.001 ≤ a ≤ 0.03, 0.001 ≤ b ≤ 0.05, x + y + z + a = 1, and δ changes with the value of b to satisfy electroneutrality. Further optionally, 0.3 < x ≤ 1, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 0.4, 0.001 ≤ a ≤ 0.03, 0.001 ≤ b ≤ 0.05. By further controlling the doping amount of elements, the electrochemical performance of the cathode material product is improved.

[0057] Specifically, the value of x is greater than 0 and can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.8, 1.0, etc.; the value of y can be 0.0, 0.1, 0.2, 0.3, etc.; the value of z can be 0.0, 0.2, 0.4, 0.6, etc.; the value of a can be 0.001, 0.005, 0.01, 0.02, 0.03, etc.; the value of b can be 0.001, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, etc. δ changes with the value of b to satisfy electroneutrality.

[0058] In some embodiments, among the several elements corresponding to M, the number of doped atoms of each element accounts for 5% - 35% of the total number of doped atoms corresponding to M. The doping amount of each element should not be too much, and it is appropriate to control within the above range to improve the stability of the product and reduce the gas generation amount. Specifically, the proportion of the number of doped atoms of each element to the total number of doped atoms corresponding to M can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, etc.

[0059] In some embodiments, the morphology of the lithium - ion cathode material includes at least one of polycrystalline materials, near - single - crystal materials, and single - crystal materials. The D50 of the near - single - crystal materials and single - crystal materials is 2μm - 6μm. The form of the product is diverse, including the above several types of crystals, and there is an obvious inheritance between the morphology of the cathode material and the precursor. Among them, the polycrystalline material means that the cathode material is a spherical aggregate composed of primary particles with a size of several hundred nanometers; the near - single - crystal material means an aggregate composed of 3 - 10 small primary particles; the single - crystal material means a material system mainly composed of single primary particles (allowing the existence of a small amount of aggregated particles).

[0060] Please refer to Figure 2. The present disclosure also provides a method for preparing a lithium - ion cathode material. Using nickel - cobalt - manganese hydroxide precursor, lithium salt, a first additive containing element R, and a second additive containing element M as raw materials, the steps for preparing the lithium - ion cathode material are as follows:

[0061] S1. Primary sintering

[0062] The nickel-cobalt-manganese hydroxide precursor, lithium salt and the first additive are mixed and sintered once to enable the R element to form bulk doping. The type of the R element is described above, and the doping amount is described in the general formula.

[0063] Specifically, the nickel-cobalt-manganese hydroxide precursor can be a commercially available material, Ni x Co y Mn z (OH)2, the values ​​of x, y, and z refer to the above introduction to the positive electrode material products. The product after one sintering is recorded as LiNi x Co y Mn z R a O2.

[0064] In some embodiments, the lithium salt is selected from at least one of LiOH and Li2CO3, and the particle size is not limited, such as at least one of micro-powder LiOH, coarse-particle LiOH, battery-grade Li2CO3, quasi-battery-grade Li2CO3, and industrial Li2CO3, specifically one or more.

[0065] In some embodiments, the amount of lithium salt added is controlled to achieve a molar ratio of lithium to the total amount of nickel, cobalt, and manganese of 1.03-1.07:1, such as 1.03:1, 1.04:1, 1.05:1, 1.06:1, 1.07:1, etc. A slight excess of lithium is controlled to improve the utilization of nickel, cobalt, and manganese.

[0066] In some embodiments, the first additive is selected from at least one of oxides, hydroxides, oxyhydroxides, and carbonates corresponding to the doping element, and may be any one or more of the above. For example, when R is nickel, the first additive may be selected from specific raw materials such as nickel oxide, nickel hydroxide, nickel oxyhydroxide, and nickel carbonate. Based on the mass ratio of the doping element in the first additive to the nickel-cobalt-manganese hydroxide precursor, the doping amount of the doping element in the first additive is 2000ppm-5000ppm, such as 2000ppm, 3000ppm, 4000ppm, 5000ppm, etc.

[0067] In some embodiments, the sintering temperature of the primary sintering is 750° C.-1050° C., and the sintering time is 20 h-40 h. The sintering temperature of the primary sintering is controlled within the above range, and specifically can be 750° C., 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C., etc. The sintering time can be 20 h, 25 h, 30 h, 35 h, 40 h, etc.

[0068] In some embodiments, the primary sintering is carried out in an oxygen atmosphere, and the oxygen atmosphere can be a controlled oxygen volume fraction of 22%-99.99%, that is, it can be a pure oxygen atmosphere or a mixed gas containing oxygen, and the oxygen volume fraction can be 22%, 30%, 50%, 70%, 99.99%, etc.

[0069] S2. Crushing

[0070] In order to improve the uniformity of the product obtained by the secondary sintering, the product obtained after the primary sintering can be crushed and then subjected to the secondary sintering. The product obtained after the primary sintering is crushed to a particle size D50 of 2μm-6μm.

[0071] Specifically, the particle size D50 after the crushing process can be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, etc.

[0072] S3, secondary sintering

[0073] The sintered product is mixed with a second additive and LiNO3 for secondary sintering. The second additive containing M is introduced during the secondary sintering to achieve the effect of surface confined high-entropy doping. LiNO3 has a low melting point and can form a low-eutectic phase with the residual lithium on the surface of the positive electrode material at a lower temperature, thereby promoting the diffusion of the high-entropy coating agent into the interior of the material.

[0074] In some embodiments, the second additive is selected from at least one of oxides, hydroxides, oxyhydroxides, and carbonates corresponding to the doping element, and may be any one or more of the above. The amount of the element used is determined based on the product formula, with the number of doping atoms of each element being controlled to account for 5% to 35% of the total number of doping atoms corresponding to M.

[0075] In actual operation, based on the mass ratio of the total amount of doping elements in the second additive to the crushed product after the primary sintering, the total amount of doping elements in the second additive is 5000ppm-10000ppm.

[0076] In some embodiments, by controlling the amount of LiNO3 added, the ratio of the molar amount of lithium added to the molar amount of residual lithium in the product after the primary sintering is 20-50:100, and by precisely controlling the amount of LiNO3 added, a better surface confined high entropy doping effect is formed. If the amount is too large, it will cause a waste of raw materials and affect product performance. If the amount is too small, it will affect the formation of the low eutectic phase. Specifically, by controlling the amount of LiNO3 added, the ratio of the molar amount of lithium added to the molar amount of residual lithium in the product after the primary sintering can be 20:100, 30:100, 40:100, 50:100, etc.

[0077] In some embodiments, the secondary sintering process includes: first subjecting the material to be sintered to a short period of high-temperature pulse sintering, and then subjecting it to low-temperature sintering after cooling. The diffusion depth of the second additive on the surface of the positive electrode material can be controlled by the short-term high-temperature pulse sintering, and the surface coating agent is partially diffused to the surface of the positive electrode material, which can achieve surface confined doping of several atomic layers on the surface of the material, thereby achieving continuous coating of the surface. A variety of additive atoms enter the surface lattice of the positive electrode material, share crystallization sites, and form a single-phase solid solution structure, thereby increasing the diversity and distortion energy of the local structure of the positive electrode material, and synergistically exerting the "entropy stabilization effect". When the increase in entropy is greater than the increase in enthalpy, the Gibbs free energy of the system decreases, and the stability of the structure and surface interface of the positive electrode material is improved, thereby effectively improving the gas production during the circulation and storage of the positive electrode material.

[0078] In some embodiments, the sintering temperature of high-temperature pulse sintering is 700°C-980°C, and the sintering temperature of low-temperature sintering is 450°C-950°C, and the sintering temperature of high-temperature pulse sintering is controlled to be greater than the sintering temperature of low-temperature sintering when sintering the same material. The high temperature provided by the pulse sintering process can accelerate the diffusion of the coating agent to the surface and sub-surface of the positive electrode material, and the diffusion depth can be effectively controlled by changing the pulse sintering time and temperature. The uniqueness of the pulse sintering process is reflected in: if the coating process is carried out at high temperature for a long time, the coating process is close to bulk doping, and the positive electrode material is prone to oxygen loss, resulting in structural degradation; if the coating temperature is low, the coating effect is a conventional island coating, and the additives are rarely or almost not diffused to the surface of the positive electrode material.

[0079] Specifically, the sintering temperature of high-temperature pulse sintering can be 700℃, 750℃, 800℃, 850℃, 900℃, 950℃, 980℃, etc.; the sintering temperature of low-temperature sintering can be 450℃, 550℃, 600℃, 650℃, 700℃, 750℃, 800℃, 850℃, 900℃, 950℃, etc., and the temperature needs to be controlled for different materials. For the same material, the sintering temperature of high-temperature pulse sintering is controlled to be greater than the sintering temperature of low-temperature sintering.

[0080] In some embodiments, the sintering time of high-temperature pulse sintering is 5 min to 60 min, such as 5 min, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, etc. The sintering time of low-temperature sintering is 3 h to 8 h, such as 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, etc. After sintering, the material is naturally cooled to room temperature in the furnace.

[0081] Specifically, the sintering process involves first heating to a high temperature, holding it for a short period, and then cooling to a relatively low temperature for a longer period. High-temperature pulse sintering refers to a short high-temperature sintering phase during the sintering process, which is equivalent to a pulse in the overall sintering process.

[0082] In some embodiments, the secondary sintering is also carried out under the conditions of an oxygen atmosphere, and the oxygen atmosphere can be a controlled oxygen volume fraction of 22%-99.99%, that is, it can be a pure oxygen atmosphere or a mixed gas containing oxygen, and the volume fraction of oxygen can be 22%, 30%, 50%, 70%, 99.99%, etc.

[0083] S4. Post-processing

[0084] After the secondary sintering is completed, the product is post-processed to obtain the finished product.

[0085] The specific operation steps of post-processing are not limited and can be adjusted according to product requirements, such as including screening, iron removal and packaging.

[0086] The present disclosure also provides a positive electrode plate, which is prepared using the above-mentioned lithium battery positive electrode material as an active material. Through the improvement of the active material, the final positive electrode plate has excellent electrochemical performance when used in lithium batteries.

[0087] It should be noted that the preparation process can adopt the existing preparation process, mixing the active material with raw materials such as the conductive agent, binder, and dispersant to form a slurry, coating it on the positive electrode current collector, and then drying it.

[0088] The present disclosure also provides a lithium battery, comprising the positive electrode plate in the above embodiment. The lithium battery produces less gas during circulation and storage and has excellent electrochemical performance.

[0089] The present disclosure also provides an electrical device, including the lithium battery in the above embodiment. The type of the electrical device is not limited. The lithium battery is used for power supply, and the performance of the electrical device is improved by improving the electrochemical performance of the lithium battery.

[0090] The features and performance of the present disclosure are further described in detail below with reference to the embodiments.

[0091] It should be noted that the precursors used in the following examples and comparative examples are all commercially available raw materials.

[0092] Example 1

[0093] This embodiment provides a method for preparing a lithium battery positive electrode material, comprising the following steps:

[0094] (1) Primary sintering

[0095] Using nickel cobalt manganese hydroxide precursor Ni 0.70 Co 0.05 Mn 0.25 (OH)2, mixed with powdered LiOH (particle size of about D50 = 6μm), additives ZrO2, Y2O3, and sintered at high temperature in an oxygen atmosphere. 0.70 Co 0.05 Mn 0.25 The molar ratio of (OH)2 to LiOH was 1.05, with a Li / (Ni+Co+Mn) ratio. ZrO2 and Y2O3 additives were added in amounts of 3000 ppm and 1000 ppm, respectively (based on the mass of Zr / Y in the precursor). The sintering process was conducted at an oxygen volume fraction of 95%, a temperature of 925°C, and a sintering time of 28 hours.

[0096] (2) Crushing

[0097] The sintered product enters the next process after coarse crushing pretreatment, and the particle size Dv50 after coarse crushing is controlled at 4.0±0.3μm.

[0098] (3) Secondary sintering

[0099] The material after crushing and pre-treatment in step (2) is mixed evenly with additives MoO3, Sb2O5, Al2O3, Co(OH)2, TiO2, and LiNO3, and then subjected to secondary sintering. The additives MoO3, Sb2O5, Al2O3, Co(OH)2, TiO2, and LiNO3 are added in amounts of 1000ppm, 500ppm, 1500ppm, 3000ppm, 600ppm, and 700ppm, respectively (based on the mass of the crushed positive electrode material in MoO3 / Sb2O5 / Al2O3 / Co(OH)2 / TiO2 / LiNO3). The sintering temperature of the high-temperature pulse sintering section in the secondary sintering is 800°C, the holding time is 30 minutes, and then the temperature is lowered to 650°C and held for 6 hours. The oxygen volume fraction in the atmosphere is controlled to be 95% during the sintering process. After the holding period is completed, the furnace is naturally cooled.

[0100] It should be added that the ionic radii of Mo / Sb / Al / Co / Ti are The ratio of the difference in ionic radius between any two elements to the larger ionic radius between the two elements is less than 0.15.

[0101] (4) Post-processing

[0102] The product after sintering in step (3) is screened, iron removed and packaged to obtain the finished product.

[0103] Example 2

[0104] This embodiment provides a method for preparing a lithium battery positive electrode material, comprising the following steps:

[0105] (1) Primary sintering

[0106] Using nickel cobalt manganese hydroxide precursor Ni 0.82 Co 0.06 Mn 0.12 (OH)2 precursor, coarse particles of LiOH (D50 = 20μm), additives SrCO3, Al2O3 are mixed evenly and sintered at high temperature in an oxygen atmosphere. 0.82 Co 0.06 Mn 0.12 The molar ratio of (OH)2 to LiOH was 1.03, and the additives SrCO3 and Al2O3 were added in amounts of 1200 ppm and 1000 ppm, respectively (based on the Sr / Al ratio in SrCO3 / Al2O3 relative to the precursor mass). The oxygen volume fraction during sintering was 98%, the sintering temperature was 840°C, and the sintering time was 30 hours.

[0107] (2) Crushing

[0108] The sintered product enters the next process after coarse crushing pretreatment, and the particle size Dv50 after coarse crushing is controlled at 4.0±0.3μm.

[0109] (3) Secondary sintering

[0110] The crushed pre-treated material in step (2) is mixed evenly with additives Nb2O5, WO3, Sb2O5, NiOOH, Ta2O5, and LiNO3, and then subjected to secondary sintering. The additive amounts of Nb2O5, WO3, Sb2O5, NiOOH, Ta2O5, and LiNO3 are 1000ppm, 1500ppm, 1000ppm, 2500ppm, 500ppm, and 800ppm, respectively (based on the mass of the crushed positive electrode material in step (2) in terms of Nb / W / Ga / Ni / Ta / Li in Nb2O5 / WO3 / Ga2O3 / NiOOH / Ta2O5 / LiNO3). The sintering temperature of the high-temperature pulse sintering section in the secondary sintering is 700°C, and the holding time is 60 minutes. The temperature is then lowered to 400°C and held for 7 hours. During the sintering process, the oxygen volume fraction in the atmosphere is controlled to be 95%. After the holding period is completed, the furnace is naturally cooled.

[0111] It should be added that the ionic radius of Nb / W / Sb / Ni / Ta is The ratio of the difference in ionic radius between any two elements to the larger ionic radius between the two elements is less than 0.15.

[0112] (4) Post-processing

[0113] The product after sintering in step (3) is screened, iron removed and packaged to obtain the finished product.

[0114] Example 3

[0115] This embodiment provides a method for preparing a lithium battery positive electrode material, comprising the following steps:

[0116] (1) Primary sintering

[0117] Using nickel cobalt manganese hydroxide precursor Ni 0.55 Co 0.12 Mn 0.33 (OH)2 precursor, mixed with battery grade Li2CO3, additives Ta2O5, La2O3, and then sintered at high temperature in an oxygen atmosphere. 0.55 Co 0.12 Mn 0.33 The (OH)2 and Li2CO3 were added at a Li / (Ni+Co+Mn) molar ratio of 1.06. The additives Ta2O5 and La2O3 were added in amounts of 2000 ppm and 1000 ppm, respectively (based on the mass of Ta / La in Ta2O5 / La2O3 relative to the precursor). The oxygen volume fraction during sintering was 22%, the sintering temperature was 950°C, and the sintering time was 35 hours.

[0118] (2) Crushing

[0119] The sintered product enters the next process after coarse crushing pretreatment, and the particle size Dv50 after coarse crushing is controlled at 4.0±0.3μm.

[0120] (3) Secondary sintering

[0121] S2. The crushed and pre-treated material of step S1 is mixed evenly with additives Sb2O5, TiO2, AlOOH, CoOOH, WO3, and LiNO3, and then subjected to secondary sintering. The additive amounts of Sb2O5, TiO2, AlOOH, CoOOH, WO3, and LiNO3 are 1000ppm, 2000ppm, 1500ppm, 4000ppm, 600ppm, and 500ppm, respectively (based on the mass of the crushed positive electrode material in step (2) in terms of Sb / Ti / Al / Co / W / Li in Sb2O5 / TiO2 / AlOOH / CoOOH / WO3 / LiNO3). The sintering temperature of the high-temperature pulse sintering section in the secondary sintering is 900°C, and the holding time is 15 minutes. The temperature is then lowered to 500°C and held for 8 hours. The oxygen volume fraction in the atmosphere is controlled to be 95% during the sintering process. After the holding period is completed, the mixture is allowed to cool naturally with the furnace.

[0122] It should be added that the ionic radius of Sb / Ti / Al / Co / W is The ratio of the difference in ionic radius between any two elements to the larger ionic radius between the two elements is less than 0.15.

[0123] (4) Post-processing

[0124] The product after sintering in step (3) is screened, iron removed and packaged to obtain the finished product.

[0125] Example 4

[0126] This embodiment provides a method for preparing a lithium battery positive electrode material, comprising the following steps:

[0127] (1) Primary sintering

[0128] Using nickel cobalt manganese hydroxide precursor Ni 0.60 Co 0.07 Mn 0.33 (OH)2 precursor, mixed with battery grade Li2CO3, additives ZrO2, MoO3, SrO, and then sintered at high temperature in an oxygen atmosphere. 0.60 Co 0.07 Mn 0.33 The molar ratio of (OH)2 to Li2CO3 was 1.05, and the additive amounts of ZrO2, MoO3, and SrO were 2500ppm, 1000ppm, and 1000ppm, respectively (based on the mass of Zr / Mo / Sr in ZrO2 / MoO3 / SrO). The oxygen volume fraction during sintering was 22%, the sintering temperature was 950°C, and the sintering time was 25h.

[0129] (2) Crushing

[0130] The sintered product enters the next process after coarse crushing pretreatment, and the particle size Dv50 after coarse crushing is controlled at 4.0±0.3μm.

[0131] (3) Secondary sintering

[0132] S2. The crushed and pre-treated material from step S1 is uniformly mixed with additives ZrO2, MgCO3, ZnO, SnO2, LiOH, and LiNO3, and then subjected to secondary sintering. The additive amounts of ZrO2, MgCO3, ZnO, SnO2, LiOH, and LiNO3 are 1000ppm, 1000ppm, 1000ppm, 1000ppm, 1000ppm, and 600ppm, respectively (based on the mass of the crushed positive electrode material in ZrO2 / MgCO3 / ZnO / SnO2 / LiOH / LiNO3 relative to the mass of the crushed positive electrode material in step (2)). The secondary sintering is performed at a high-temperature pulse sintering stage of 750°C for 45 minutes, followed by cooling to 600°C and holding for 5 hours. During the sintering process, the oxygen volume fraction in the atmosphere is controlled to be 95%. After the holding period is completed, the material is allowed to cool naturally with the furnace.

[0133] It should be added that the ionic radii of Zr / Mg / Zn / Bi / Li are The ratio of the difference in ionic radius between any two elements to the larger ionic radius between the two elements is less than 0.15.

[0134] (4) Post-processing

[0135] The product after sintering in step (3) is screened, iron removed and packaged to obtain the finished product.

[0136] Comparative Example 1

[0137] This comparative example provides a method for preparing a positive electrode material, which differs from Example 1 only in that the temperature of the secondary sintering in step (3) is 450° C., the sintering time is 6 h, and no pulse is introduced during the process.

[0138] Comparative Example 2

[0139] This comparative example provides a method for preparing a positive electrode material, which differs from Example 1 only in that the additive used in step (3) is only 1500 ppm Al2O3.

[0140] Comparative Example 3

[0141] This comparative example provides a method for preparing a positive electrode material, which differs from Example 1 only in that the secondary sintering process in step (3) is adjusted to 800° C. for 6.5 h, and no pulse is introduced during the process.

[0142] Comparative Example 4

[0143] This comparative example provides a method for preparing a positive electrode material, which differs from Example 2 in that the selection of additives in step (3) does not follow the principle that the difference in ionic radius should be within 15%. The selected additives are Y2O3, SrO, Al2O3, B2O3, LiOH, and LiNO3, which are mixed evenly and then sintered for the second time. The addition amounts of the additives Y2O3, SrO, Al2O3, B2O3, LiOH, and LiNO3 are 1000ppm, 1500ppm, 1000ppm, 2500ppm, 500ppm, and 800ppm, respectively (based on the mass of the crushed positive electrode material in step (2) of Y / Sr / Al / B / Li / Li in Y2O3 / SrO / Al2O3 / B2O3 / LiOH / LiNO3). It should be added that the ionic radii of Y / Sr / Al / B / Li are The ratio of the difference between the ionic radii of any two elements to the larger ionic radius between the two elements is not less than 0.15.

[0144] Comparative Example 5

[0145] This comparative example provides a method for preparing a positive electrode material. The difference from Example 2 is that the amount of additives added in step (3) does not follow the principle that the atomic percentage of each additive element is between 5 and 35%. The additives selected are Nb2O5, WO3, Al2O3, NiOOH, Ta2O5, and LiNO3, and the addition amounts are 3000ppm, 900ppm, 100ppm, 200ppm, 800ppm, and 800ppm, respectively (based on the mass of Nb / W / Al / Ni / Ta / Li in Nb2O5 / WO3 / Al2O3 / NiOOH / Ta2O5 / LiNO3 relative to the mass of the crushed positive electrode material in step (2)).

[0146] It should be added that the doping amount of Nb in this comparative example is too large, and the ratio of Nb to the total atomic number of doping elements exceeds 35%.

[0147] Comparative Example 6

[0148] This comparative example provides a method for preparing a positive electrode material. The only difference from Example 1 is that in step (3), the material pre-treated by crushing in step (2) is mixed evenly with four additives, namely, MoO3, Sb2O5, Al2O3, and Co(OH)2, and LiNO3, and then subjected to secondary sintering. The amounts of the additives added remain unchanged.

[0149] Since the number of additives added is less than five, the high entropy coating effect cannot be achieved.

[0150] Comparative Example 7

[0151] This comparative example provides a method for preparing a positive electrode material. The only difference from Example 1 is that in step (3), the material pre-treated by crushing in step (2) is mixed evenly with five additives, namely, MoO₃, Sb₂O₅, Al₂O₃, Co(OH)₂, and TiO₂, and LiNO₃, and then subjected to secondary sintering. The amount of each of the five additives is increased by 50%.

[0152] Comparative Example 8

[0153] This comparative example provides a method for preparing a positive electrode material. The only difference from Example 1 is that in step (3), the material pre-treated by crushing in step (2) is mixed uniformly with five additives, namely, MoO₃, Sb₂O₅, Al₂O₃, Co(OH)₂, and TiO₂, and LiNO₃, and then subjected to secondary sintering. The amount of each of the five additives is 50% of that in Example 1.

[0154] Comparative Example 9

[0155] This comparative example provides a method for preparing a positive electrode material, which differs from Example 1 only in that the secondary sintering heat treatment process in step (3) is as follows: the sintering temperature of the high-temperature pulse sintering section in the secondary sintering is 800°C, the holding time is 3h, and then the temperature is lowered to 650°C and kept for 6h.

[0156] Comparative Example 10

[0157] This comparative example provides a method for preparing a positive electrode material, which differs from Example 1 only in that in step (3), the pulse sintering section of 800°C for 30 minutes is eliminated during the secondary sintering process, and the temperature is directly raised to 650°C for 6 hours.

[0158] Test Example 1

[0159] This test example tested the charge and discharge test results of the positive electrode materials of Examples 1 to 4 and Comparative Examples 1 and 2. The test results are shown in Table 1.

[0160] Testing method: Using N-methylpyrrolidone as a solvent, the positive electrode material, acetylene black, and PVDF were mixed uniformly in a mass ratio of 9.2:0.5:0.3 to form a slurry. The slurry was then coated onto aluminum foil and dried with forced air at 80°C for 8 hours, followed by vacuum drying at 120°C for 12 hours to obtain the positive electrode. The battery was assembled in an argon-protected glove box. The negative electrode was a lithium metal sheet, the separator was a polypropylene film, and the electrolyte was 1M LiPF6-EC / DMC (1:1, v / v). A 2032 button cell case was used. The resulting button cell was subjected to electrochemical performance testing, and the initial charge and discharge capacity and efficiency were recorded.

[0161] Table 1 Performance test results

[0162] In Examples 1 to 4, the present invention discloses that at least five coating agents are co-coated by two sintering at high temperature. At high temperature, the coating agents diffuse to the surface of the material to achieve surface doping of the positive electrode material. At the same time, the "entropy stabilization effect" synergistically produced by the additives further enhances the structural stability of the material, thereby effectively inhibiting the side reactions at the surface interface between the positive electrode material and the electrolyte, and reducing the gas production of the material during circulation and storage.

[0163] Comparative Example 1 still uses conventional low-temperature coating, and the additive is still attached to the material surface in the form of island coating, rather than diffusing into the material surface layer to form surface doping, which is not continuous coating. The coating effect diagrams of Example 1, Comparative Example 1, and Comparative Example 8 are shown in Figures 3, 4, and 5, respectively. The surface of the positive electrode material particles is relatively smooth under high-temperature coating, while the additive adhesion effect is obvious under conventional low-temperature coating. Example 1 can form a film-like coating, without obvious additive enrichment on the particle surface, and can form a continuous coating.

[0164] Test Example 2

[0165] This test example tests the gas generation detection results of soft-pack batteries made of the positive electrode materials of Example 1 and Comparative Example 1 stored at 70°C in a fully charged state. The test results are shown in Figure 6.

[0166] The gas production test method follows the following process: slurry preparation - coating - roller pressing - winding - packaging - liquid injection - formation - testing. The cathode material slurry is prepared by stirring at a mass ratio of 96:2:2 (cathode material: PVDF: SP). The amount of NMP added is approximately 0.8 times the mass of the cathode material. Stirring is performed at 2000 rpm for 8 hours to ensure a slurry viscosity of ~4000 mPa·s.

[0167] The negative electrode slurry was prepared according to the mass ratio of graphite: SBR: CMC: SP of 90:1:4:5, and deionized water 1.5 times the mass of graphite was added, and stirred at 2000r / min for 6h.

[0168] The coating process controls the surface density of the positive electrode to 1.6g / dm 2 The surface density of the negative electrode is 1.1g / dm 2 .

[0169] The roller pressing process controls the areal density of the positive electrode to 3.9g / cc and the areal density of the negative electrode to 1.6g / cc.

[0170] The positive electrode sheet, negative electrode sheet and separator are wound into a bare battery cell using an automatic winding machine. During the process, the positive electrode sheet and the negative electrode sheet should be prevented from shifting.

[0171] The bare cell was encapsulated in aluminum-plastic film for top and side sealing, and dried at 90°C for 12 h in a vacuum dryer to remove excess moisture in the cell.

[0172] After injecting 5g of commercial electrolyte, the cell is evacuated and pre-packaged.

[0173] The cells were aged at 45°C to form an SEI film on the negative electrode. The process was as follows: After the cells were left to rest for 2 hours, they were charged at a constant current of 0.02C to 3.4V. After resting for another 5 minutes, they were charged at a constant current of 0.33C to 3.75V. After resting for another 5 minutes, they were charged at a constant current of 0.33C to 4.4V.

[0174] Place the soft pack battery in the test cabinet and set up the charging system according to the test steps.

[0175] The gas production of soft-pack battery storage is tested once every 5 days, and the gas volume is measured using the drainage method.

[0176] As can be seen from FIG6 , the gas production of the cathode material prepared in the embodiment is significantly less than that in the comparative example.

[0177] At the same time, the prepared soft pack was subjected to a charge-discharge cycle test at a certain voltage and a 1C / 1C rate. The capacity retention rates of some embodiments and comparative examples after 100 cycles are shown in Table 2.

[0178] Table 2 Soft pack cycle capacity retention rate

[0179] It can be seen that the capacity retention rates of the products prepared in the examples are significantly better than those in the comparative examples.

[0180] The preferred embodiments of the present disclosure are described in detail above, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed by the present disclosure and fall within the scope of protection of the present disclosure. Industrial Applicability

[0181] The lithium battery cathode material provided by the present disclosure is doped with R and M elements. The R element is bulk doped, and the M element is surface doped. The doping is achieved through a secondary sintering process. During the secondary sintering, a short high-temperature pulse sintering is introduced. The M element contains at least five elements, and the difference in the ionic radius of any two elements is controlled. Multiple atoms enter the surface lattice of the cathode material, sharing crystallization sites and forming a single-phase solid solution structure. This can effectively reduce gas production during the circulation and storage process of the cathode material, which is conducive to further improving the electrochemical performance of the material. The preparation process is simple to operate and has excellent industrial applicability.

Claims

1. A lithium battery positive electrode material, characterized in that: The general formula of lithium battery positive electrode material is LiNi x Co y Mn z R a O 2+δ @M b , R is the bulk doping element, M is the surface doping element; Among them, R is selected from at least one of Ni, Co, Mn, Zr, Al, Mg, Ti, Sr, W, Y, Mo, Sb, Nb, Sn, Zn, La, Ce, Ta, B, and F; M is selected from at least five of Li, B, Al, Ti, Ni, Co, Mn, Ce, La, W, Nb, Mo, Zr, Mg, Zn, Sb, Sn, Ta, and Y. Among the several elements corresponding to M, the ratio of the difference in ionic radii between any two elements to the larger ionic radius between the two is less than 0.15; In the general formula, 0 < x < 1, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 0.6, 0.001 ≤ a ≤ 0.03, 0.001 ≤ b ≤ 0.05, x + y + z + a = 1, and δ changes with the value of b to satisfy electrical neutrality.

2. The lithium battery positive electrode material according to claim 1, characterized in that: R is selected from at least one of Zr, Al, Ti, Sr, W, Y, Mo, Ta, and La.

3. The lithium battery positive electrode material according to claim 1 or 2, characterized in that: M is selected from at least five of Li, Al, Ti, Ni, Co, Ce, W, Mo, Zr, Mg, Zn, Sb, and Ta.

4. The lithium battery positive electrode material according to any one of claims 1 to 3, characterized in that 0.3 < x ≤ 1, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 0.4, 0.001 ≤ a ≤ 0.03, 0.001 ≤ b ≤ 0.

05.

5. The lithium battery positive electrode material according to any one of claims 1 to 4, characterized in that: Among the several elements corresponding to M, the doping atom number of each element accounts for 5% - 35% of the total doping atom number corresponding to M.

6. The lithium battery positive electrode material according to any one of claims 1 to 5, characterized in that The morphology of the lithium battery cathode material includes at least one of polycrystalline materials, quasi-single crystal materials, and single crystal materials. The particle sizes D50 of the quasi-single crystal materials and the single crystal materials are both 2 μm - 6 μm.

7. A method for preparing the lithium battery positive electrode material according to any one of claims 1 to 6, characterized in that: Including: Using nickel-cobalt-manganese hydroxide precursor, lithium salt, a first additive containing R element, and a second additive containing M element as raw materials to prepare the lithium battery cathode material.

8. The preparation method according to claim 7, characterized in that: Including: Mixing the nickel-cobalt-manganese hydroxide precursor, lithium salt, and the first additive for primary sintering, and mixing the sintered product with the second additive and LiNO3 for secondary sintering.

9. The preparation method according to claim 8, characterized in that: Calculated by the mass ratio of the doping element in the first additive to the nickel-cobalt-manganese hydroxide precursor, the doping amount of the doping element in the first additive is 2000 ppm - 5000 ppm.

10. The preparation method according to claim 8 or 9, characterized in that: Calculated by the mass ratio of the total amount of doping elements in the second additive to the crushed product after primary sintering, the total doping amount of several doping elements in the second additive is 5000 ppm - 10000 ppm.

11. The preparation method according to any one of claims 8 to 10, characterized in that: The sintering temperature of the primary sintering is 750 °C - 1050 °C, and the sintering time is 20 h - 40 h.

12. The preparation method according to any one of claims 8 to 11, characterized in that: The process of the secondary sintering includes: first performing high-temperature pulse sintering on the material to be sintered, and then performing low-temperature sintering after cooling; Among them, the sintering temperature of the high-temperature pulse sintering is 700 °C - 980 °C, the sintering temperature of the low-temperature sintering is 450 °C - 950 °C, and it is controlled that the sintering temperature of the high-temperature pulse sintering is higher than the sintering temperature of the low-temperature sintering.

13. The preparation method according to claim 12, characterized in that: The sintering time of the high-temperature pulse sintering is 5 min - 60 min.

14. The preparation method according to claim 12 or 13, characterized in that: The sintering time of the low-temperature sintering is 3 h - 8 h.

15. The preparation method according to any one of claims 8 to 14, characterized in that: By controlling the addition amount of LiNO3, the ratio of the molar amount of added lithium to the molar amount of residual lithium in the product after primary sintering is 20 - 50:

100.

16. The preparation method according to any one of claims 8 to 15, characterized in that: The lithium salt is selected from at least one of LiOH and Li2CO3.

17. The preparation method according to claim 16, characterized in that: By controlling the amount of the lithium salt added, the molar ratio of lithium to the total amount of nickel, cobalt and manganese is 1.03-1.07:

1.

18. The preparation method according to any one of claims 8 to 17, characterized in that: The first additive is selected from at least one of oxides, hydroxides, oxyhydroxides and carbonates corresponding to the doping element.

19. The preparation method according to any one of claims 8 to 18, characterized in that: The second additive is selected from at least one of oxides, hydroxides, oxyhydroxides and carbonates corresponding to the doping element.

20. The preparation method according to any one of claims 8 to 19, characterized in that: The product obtained after the primary sintering is crushed and then mixed with the second additive and LiNO3 for secondary sintering.

21. The preparation method according to claim 20, characterized in that: The crushing process is to control the particle size D50 after crushing to be 2μm-6μm.

22. The preparation method according to any one of claims 8 to 21, characterized in that: The primary sintering and the secondary sintering are both performed in an oxygen atmosphere.

23. The preparation method according to claim 22, characterized in that: The oxygen atmosphere is controlled to have an oxygen volume fraction of 22%-99.99%.

24. The preparation method according to any one of claims 8 to 23, characterized in that: After the secondary sintering is completed, the product is screened, iron removed and packaged to obtain the finished product.

25. A positive electrode plate, characterized in that: The active material is prepared by using the lithium battery positive electrode material described in any one of claims 1 to 6 or the lithium battery positive electrode material prepared by the preparation method described in any one of claims 7 to 24.

26. A lithium battery, characterized in that: Includes the positive electrode sheet as described in claim 25.

27. An electrical device, characterized in that: Includes the lithium battery described in claim 26.

Citation Information

Patent Citations

  • Positive electrode material and preparation method therefor, positive electrode plate and lithium ion battery

    CN107681123A

  • Cathode material for lithium-ion battery as well as preparation method and application thereof

    CN108232150A

  • NCM ternary cathode material doped with Mo element in surface layer and bulk phase, and preparation method thereof

    CN108878868A

  • Self-coated and dual-modification structure lithium ion battery positive electrode material during doping process and preparation method thereof

    CN109920996A

  • Positive electrode material and lithium ion battery

    CN110277539A

Cited By

  • High-entropy high-nickel single crystal lithium ion battery positive electrode material and preparation method thereof

    CN119495740A

  • Ultrahigh nickel layered oxide positive electrode material and application thereof

    CN120089737A