Method and system for preparing superfine tungsten trioxide
Through the calcination and physical crushing of ammonium paratungstate crystals, the problems of low productivity and high cost in the preparation process of tungsten trioxide in the prior art are solved, and the efficient and low-cost ultra-fine tungsten trioxide preparation is achieved, providing high-quality tungsten trioxide Tungsten oxide material.
Patent Information
- Application Number
- PCT/CN2023/116003
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2023-08-31
- Publication Date
- 2024-11-14
AI Technical Summary
The existing tungsten trioxide preparation methods have low productivity, high cost and difficult to control, resulting in unstable product quality.
Ultrafine tungsten trioxide is prepared by calcining ammonium paratungstate crystals and physical crushing methods. By adjusting the calcining temperature section and physical crushing method, an efficient and low-cost production process is achieved.
The ultrafine tungsten trioxide preparation without the addition of auxiliary materials is realized, which reduces production costs, improves product quality and production efficiency, and produces high-quality tungsten trioxide materials with an average particle size of 0.5-1.0μm.
Smart Images

Figure CN2023116003_14112024_PF_FP_ABST
Abstract
Description
A method and system for preparing ultrafine tungsten trioxide
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 9, 2023, with application number 202310515547.4 and invention name “A method and system for preparing ultrafine tungsten trioxide”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention belongs to the technical field of tungsten trioxide, and in particular relates to a preparation method and system of ultrafine tungsten trioxide. Background Art
[0003] Tungsten trioxide has high density, a high melting point, high hardness, high wear resistance, a low coefficient of thermal expansion, excellent electrical and thermal conductivity, good corrosion resistance, and semiconductor properties, making it a highly promising sensitive material and sensitive to a variety of gases. Ultrafine tungsten trioxide, in addition to these properties, has a large specific surface area, significant surface effects, and strong electromagnetic wave absorption, making it an excellent solar energy absorber and stealth material for use in the battery industry. Furthermore, tungsten trioxide exhibits exceptional catalytic properties, making it widely used in the chemical and petrochemical industries.
[0004] There are many methods for preparing tungsten trioxide. Commonly used preparation methods include gas phase method, liquid phase method (including precipitation method, hydrothermal method, sol-gel method, etc.) and solid phase method. These methods all have disadvantages such as low productivity, high cost and difficult production control.
[0005] Summary of the Invention
[0006] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a method for preparing ultrafine tungsten trioxide.
[0007] The technical solutions of the present invention are as follows:
[0008] In order to solve the problems in the prior art, the present invention provides a method for preparing ultrafine tungsten trioxide. No other auxiliary materials need to be added during the production process, the production process is mature and easy to control, and the cost is low.
[0009] To this end, the present invention provides a method for preparing ultrafine tungsten trioxide, comprising the following steps:
[0010] A method for preparing ultrafine tungsten trioxide comprises the following steps:
[0011] Step S1: calcining ammonium paratungstate crystals to obtain tungsten trioxide powder;
[0012] wherein the calcination comprises at least three gradually increasing temperature sections;
[0013] Step S2: Physically crushing the tungsten trioxide powder obtained in step S1 to obtain ultrafine tungsten trioxide powder.
[0014] As a preferred embodiment of the present invention, in step S1, the preparation method of the ammonium paratungstate crystals is: evaporating and crystallizing a high-purity ammonium tungstate solution to obtain ammonium paratungstate crystals;
[0015] The evaporation and crystallization are stirred at the same time, and the stirring speed is 90-110 r / min 1-3 hours before crystallization and 60-89 r / min after 1-3 hours.
[0016] As a preferred embodiment of the present invention, the terminal crystallization rate of evaporative crystallization is 85-95%.
[0017] As a preferred embodiment of the present invention, the high-purity ammonium tungstate solution is produced by at least one of an ion exchange process, an acid extraction process, an alkaline extraction process, and a sulfur-phosphorus mixed acid process.
[0018] As a preferred embodiment of the present invention, in step S1, the at least three gradually increasing temperature sections are specifically:
[0019] The temperature of the first temperature control zone is 250-450°C, the temperature of the second temperature control zone is 400-600°C; and the temperature of the third temperature control zone is 600-800°C.
[0020] As a preferred embodiment of the present invention, in step S1, the at least three gradually increasing temperature sections are specifically:
[0021] The temperature of the first temperature control zone is 200-300°C, the temperature of the second temperature control zone is 300-400°C; the temperature of the third temperature control zone is 450-600°C; and the temperature of the fourth temperature control zone is 650-800°C.
[0022] As a preferred embodiment of the present invention, in step S1, the at least three gradually increasing temperature sections are specifically:
[0023] The temperature of the first temperature control zone is 250-350℃, the temperature of the second temperature control zone is 350-450℃; the temperature of the third temperature control zone is 450-550℃; the temperature of the fourth temperature control zone is 550-650℃; the temperature of the fifth temperature control zone is 650-800℃.
[0024] As a preferred embodiment of the present invention, in step S1, the at least three gradually increasing temperature sections are specifically:
[0025] The temperature of the first temperature control zone is 250-300℃, the temperature of the second temperature control zone is 300-400℃; the temperature of the third temperature control zone is 450-600℃; the temperature of the fourth temperature control zone is 550-700℃; the temperature of the fifth temperature control zone is 600-750℃; and the temperature of the sixth temperature control zone is 650-800℃.
[0026] As a preferred embodiment of the present invention, in step S1, the calcination is carried out in a calcination furnace, and the rotation speed of the calcination furnace tube is 1.8-2.7 r / min.
[0027] As a preferred embodiment of the present invention, in step S2, the physical crushing method includes: grinding and / or air flow crushing.
[0028] The present invention also provides an ultrafine tungsten trioxide obtained by any of the above preparation methods, wherein the average particle size is 0.5-1.0 μm.
[0029] The present invention also discloses a preparation system for ultrafine tungsten trioxide, comprising: an APT silo, a calcining furnace, a tungsten trioxide silo, a vibrating screen, and a jet mill arranged in sequence along the feeding direction; wherein the calcining furnace comprises at least three heating sections.
[0030] Preferably, the discharge port of the jet mill is connected to a material collecting device;
[0031] The bottom of the air flow mill and air flow crushing bin is connected to an air supply system that provides high-pressure air, and the discharge port of the air flow crushing bin is connected to a material collecting device through a pipeline.
[0032] The beneficial effects of the present invention are:
[0033] (1) The preparation method of the present invention does not require the addition of auxiliary materials during the entire process, which reduces production costs and avoids unqualified products caused by incomplete processing of auxiliary materials.
[0034] (2) The production process of the present invention is stable, the production efficiency is high, and the product quality is stable.
[0035] (3) The present invention produces tungsten trioxide with a small original particle size by adjusting the crystallization process, crystallization rate, heating temperature of the calcination process and furnace tube speed. After physical crushing, tungsten trioxide with an average particle size of 0.5-1.0μm can be produced, providing the tungsten industry with a high-quality ultrafine tungsten trioxide material.
[0036] (4) The preparation system of the present invention sequentially uses a calcining furnace with at least three heating sections, a vibrating screen machine and a jet mill, which solves the problem of coarse tungsten trioxide particles in traditional equipment and produces ultrafine tungsten trioxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] FIG1 is a schematic diagram of a system for preparing ultrafine tungsten trioxide according to the present invention;
[0038] FIG2 is a structural schematic diagram of a calcining furnace according to the present invention;
[0039] FIG3 is a second structural diagram of a calcining furnace according to the present invention;
[0040] FIG4 is a third structural diagram of the calcining furnace of the present invention;
[0041] FIG5 is a fourth structural diagram of the calcining furnace of the present invention;
[0042] FIG6 is an electron microscope photograph of tungsten trioxide generated by calcining APT in Example 5;
[0043] FIG7 is an electron microscope photograph of ultrafine tungsten trioxide in Example 5;
[0044] FIG8 is an electron microscope photograph of tungsten trioxide generated by calcining APT in Example 6;
[0045] FIG9 is an electron microscope photograph of ultrafine tungsten trioxide in Example 6.
[0046] In the figure, 1-APT silo, 2-calcining furnace, 201-first heating section, 202-second heating section, 203-third heating section, 204-fourth heating section, 205-fifth heating section, 206-sixth heating section, 3-tungsten trioxide silo, 4-vibrating screen, 5-air jet mill, 6-material collecting device, 7-maintenance window. DETAILED DESCRIPTION
[0047] A method for preparing ultrafine tungsten trioxide comprises the following steps:
[0048] A high-purity ammonium tungstate solution is added to an evaporation crystallization pot, and then a stirring paddle and steam are activated to obtain ammonium paratungstate (APT) crystals. Specifically, the evaporation crystallization pot is a batch evaporation crystallization pot, and the stirring paddle speed is 60-110 r / min. The stirring paddle speed is 90-110 r / min for the first two hours of crystallization, and in step S1, the stirring paddle speed is 60-89 r / min after two hours of crystallization. The crystallization endpoint yield is 85-95%. The high-purity ammonium tungstate solution is produced through an ion exchange process, an acid extraction process, an alkaline extraction process, and a sulfur-phosphorus mixed acid process.
[0049] The APT crystal obtained above is calcined in a calcining furnace to obtain tungsten trioxide powder; wherein the calcining furnace is a rotary kiln with a furnace tube speed of 1.8-2.7r / min. The calcining furnace has at least 3 temperature control zones:
[0050] The temperature of the first temperature control zone is 250-450°C, the temperature of the second temperature control zone is 400-600°C; the temperature of the third temperature control zone is 600-800°C;
[0051] In some other embodiments, the temperature of the first temperature control zone is 200-300°C, the temperature of the second temperature control zone is 300-400°C; the temperature of the third temperature control zone is 450-600°C; the temperature of the fourth temperature control zone is 650-800°C;
[0052] In some other embodiments, the temperature of the first temperature control zone is 250-350°C, the temperature of the second temperature control zone is 350-450°C; the temperature of the third temperature control zone is 450-550°C; the temperature of the fourth temperature control zone is 550-650°C; the temperature of the fifth temperature control zone is 650-800°C.
[0053] In some other embodiments, the temperature of the second temperature control zone is 300-400°C; the temperature of the third temperature control zone is 450-600°C; the temperature of the fourth temperature control zone is 550-700°C; the temperature of the fifth temperature control zone is 600-750°C; and the temperature of the sixth temperature control zone is 650-800°C.
[0054] In step S3, the tungsten trioxide powder obtained in step 2 is physically crushed to obtain ultrafine tungsten trioxide powder. Specifically, the physical crushing method includes: grinding and / or air flow crushing.
[0055] There is another preferred embodiment, the preparation system of the ultrafine tungsten trioxide is as follows, referring to Figures 1-5;
[0056] A system for preparing ultrafine tungsten trioxide comprises: an APT silo 1, a calcining furnace 2, a tungsten trioxide silo 3, a vibrating screen 4, and a jet mill 5, which are arranged in sequence along a feeding direction; wherein the calcining furnace 2 comprises at least three heating sections, specifically, a first heating section 201, a second heating section 202, a third heating section 203, a fourth heating section 204, a fifth heating section 205, and a sixth heating section 206; different temperatures can be set in different heating sections to meet the above-mentioned process requirements, which is more conducive to the formation of ultrafine tungsten trioxide.
[0057] Specifically, the discharge port of the air flow mill 5 is connected to a material collecting device 6; more specifically, the material collecting device 6 is a bag dust collector, which is provided with an inspection window 7 to facilitate timely inspection of the tank.
[0058] The jet mill 5 includes a jet crushing chamber, which is connected to the material collection device 6 through a pipeline. The bottom of the jet crushing chamber is connected to an air supply system that provides high-pressure air to crush the material. The jet mill 5 is used to grind tungsten trioxide more evenly.
[0059] The technical solution of the present invention is further described below with reference to specific embodiments.
[0060] APT: ammonium paratungstate.
[0061] Example 1
[0062] APT is placed in a rotary furnace, and the temperature is controlled as follows: 300℃ in the first temperature control zone, 500℃ in the second temperature control zone, and 700℃ in the third temperature control zone. The furnace tube speed is 1.8r / min. Tungsten trioxide is obtained by sieving. The tungsten trioxide is then ground to obtain ultrafine tungsten trioxide.
[0063] Example 2
[0064] APT is placed in a rotary furnace, and the temperature is controlled as follows: 300°C in the first temperature control zone, 450°C in the second temperature control zone, 600°C in the third temperature control zone, and 750°C in the fourth temperature control zone. The furnace tube speed is 2.5r / min, and tungsten trioxide is obtained through screening. The tungsten trioxide is then crushed by air flow to obtain ultrafine tungsten trioxide.
[0065] Example 3
[0066] APT is placed in a rotary furnace, and the temperature is controlled as follows: 250°C in the first temperature control zone, 350°C in the second temperature control zone, 500°C in the third temperature control zone, 650°C in the fourth temperature control zone, and 750°C in the fifth temperature control zone. The furnace tube speed is 2.2r / min, and tungsten trioxide is obtained through screening. The tungsten trioxide is then crushed by air flow to obtain ultrafine tungsten trioxide.
[0067] Example 4
[0068] APT is placed in a rotary furnace, and the temperature is controlled as follows: 250°C in the first temperature control zone, 350°C in the second temperature control zone, 500°C in the third temperature control zone, 650°C in the fourth temperature control zone, 700°C in the fifth temperature control zone, and 750°C in the sixth temperature control zone. The furnace tube speed is 2.5r / min, and tungsten trioxide is obtained through screening. The tungsten trioxide is then crushed by air flow to obtain ultrafine tungsten trioxide.
[0069] Example 5
[0070] APT is placed in a rotary furnace, and the temperature is controlled as follows: 250°C in the first temperature control zone, 380°C in the second temperature control zone, 520°C in the third temperature control zone, 680°C in the fourth temperature control zone, 720°C in the fifth temperature control zone, and 780°C in the sixth temperature control zone. The furnace tube speed is 2.2r / min, and tungsten trioxide is obtained through screening. The tungsten trioxide is then crushed by air flow to obtain ultrafine tungsten trioxide.
[0071] The tungsten trioxide after calcination and after airflow crushing in this embodiment was scanned by electron microscope, referring to Figures 6 and 7. As can be seen from Figure 1, the tungsten trioxide after calcination of APT is composed of multiple grains combined into tungsten trioxide crystals. The particle size of each grain is less than 1μm, and the grains are closely connected. After the tungsten trioxide in Figure 6 is crushed by airflow, each grain is basically dispersed to form a single tiny nano-scale crystal.
[0072] Example 6
[0073] The ammonium tungstate solution produced by acid extraction (test results are shown in Table 1) was placed in an intermittent crystallization pot. The stirring speed was controlled at 90 r / min for two hours before crystallization and at 100 r / min for two hours after crystallization.
[0074] 60r / min, controlling the crystallization rate to 85% to obtain APT; placing the APT in a rotary furnace, controlling the temperatures as follows: 250°C in the first temperature control zone, 300°C in the second temperature control zone, 450°C in the third temperature control zone, 550°C in the fourth temperature control zone, 600°C in the fifth temperature control zone, and 650°C in the sixth temperature control zone, with the furnace tube rotating speed at 1.8r / min, and sieving to obtain tungsten trioxide; and grinding the tungsten trioxide to obtain tungsten trioxide.
[0075] Table 1 Test results of acidic extraction of ammonium tungstate solution (g / L)
[0076] The tungsten trioxide after calcination and after airflow crushing in this embodiment was scanned by electron microscope, referring to Figures 8 and 9. As can be seen from Figure 1, the tungsten trioxide after calcination of APT is composed of multiple grains combined into tungsten trioxide crystals. The particle size of each grain is less than 1μm, and the grains are closely connected. The ultrafine tungsten trioxide powder shown in Figure 9 is generated by airflow crushing the tungsten trioxide in Figure 8. Each grain is basically dispersed to form a single tiny nano-scale crystal.
[0077] Comparative Example 1
[0078] APT was placed in a rotary furnace, and the temperature was controlled as follows: 300°C in the first temperature control zone, 500°C in the second temperature control zone, and 700°C in the third temperature control zone. The furnace tube speed was 1.8 r / min, and tungsten trioxide was obtained after sieving.
[0079] Comparative Example 2
[0080] APT is placed in a rotary furnace, the temperature is controlled at 750°C, the furnace tube speed is 1.8r / min, and tungsten trioxide is obtained after screening; the tungsten trioxide is crushed by air flow to obtain tungsten trioxide.
[0081] Comparative Example 3
[0082] APT is placed in a rotary furnace, and the temperature is controlled as follows: 350°C in the first temperature control zone, 750°C in the second temperature control zone, and the furnace tube speed is 1.8r / min. Tungsten trioxide is obtained by sieving; and tungsten trioxide is obtained by air flow crushing.
[0083] Comparative Example 4
[0084] APT is placed in a rotary furnace, and the temperature is controlled as follows: 750°C in the first temperature control zone, 650°C in the second temperature control zone, and 550°C in the third temperature control zone. The furnace tube speed is 1.8r / min. Tungsten trioxide is obtained by sieving. The tungsten trioxide is then crushed by air flow to obtain tungsten trioxide.
[0085] Comparative Example 5
[0086] APT is placed in a rotary furnace, and the temperature is controlled as follows: 750°C in the first temperature control zone, 700°C in the second temperature control zone, 650°C in the third temperature control zone, and 550°C in the fourth temperature control zone. The furnace tube speed is 1.8r / min, and tungsten trioxide is obtained after sieving. The tungsten trioxide is then crushed by air flow to obtain tungsten trioxide.
[0087] Comparative Example 6
[0088] APT is placed in a rotary furnace, and the temperature is controlled as follows: 300°C in the first temperature control zone, 500°C in the second temperature control zone, and 700°C in the third temperature control zone. The furnace tube speed is 1.5r / min, and tungsten trioxide is obtained after sieving. The tungsten trioxide is then crushed by air flow to obtain tungsten trioxide.
[0089] The average particle size of the samples of the above embodiments and comparative examples was tested, and the test results are shown in Table 1.
[0090] Table 2 Average particle size of examples and comparative examples
[0091] As can be seen from the table above, the average particle size of the tungsten trioxide prepared in Examples 1-6 reached 0.5-1 μm, i.e., nanometer-scale, which is superior to that of Comparative Examples 1-6. The main reasons may be as follows: in the initial stage of evaporative crystallization, rapid stirring can quickly generate a large number of crystal nuclei. In the later stages of crystallization, as the supersaturation of the solution decreases, reducing the stirring speed reduces the growth of solute on the existing crystal nuclei, thereby producing fine-grained APT. When APT decomposes at slightly lower temperatures and water vapor and ammonia escape from the interior of the particles, a large number of microcracks will form in the particles. Ammonia and water generated by excessively rapid heating or high temperatures do not evaporate quickly, thus hindering the decomposition of APT and preventing the production of fine-grained tungsten trioxide. Therefore, the present invention produces tungsten trioxide with a small initial particle size by adjusting the crystallization process, crystallization rate, calcination heating temperature, and furnace speed. After physical pulverization, tungsten trioxide with an average particle size of 0.5-1.0 μm can be produced, providing a high-quality ultrafine tungsten trioxide material for the tungsten industry.
[0092] The above-described embodiments merely represent preferred implementations of the present invention. While the descriptions thereof are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that a person skilled in the art would be able to make various other corresponding changes and modifications based on the technical solutions and concepts described above, and all such changes and modifications should fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing ultrafine tungsten trioxide, characterized in that: The following steps are involved: Step S1: calcining ammonium paratungstate crystals to obtain tungsten trioxide powder; wherein the calcination comprises at least three gradually increasing temperature sections; Step S2, physically crushing the tungsten trioxide powder obtained in step S1 to obtain ultrafine tungsten trioxide powder.
2. The method for preparing ultrafine tungsten trioxide according to claim 1, characterized in that: Step S1 at least includes the following technical features: The preparation method of the ammonium paratungstate crystal is as follows: evaporating and crystallizing a high-purity ammonium tungstate solution to obtain the ammonium paratungstate crystal; Stirring is performed during the evaporation and crystallization, the stirring speed is 90-110 r / min 1-3 h before crystallization, and the stirring speed is 60-89 r / min after 1-3 h; The terminal crystallization rate of the evaporation crystallization is 85-95%; The calcination is carried out in a calcination furnace, and the rotation speed of the calcination furnace tube is 1.8-2.7r / min; and / or; In step S2, the physical crushing method includes: grinding and / or air flow crushing.
3. The method for preparing ultrafine tungsten trioxide according to claim 2, characterized in that: The high-purity ammonium tungstate solution is produced by at least one of an ion exchange process, an acid extraction process, an alkaline extraction process, and a sulfur-phosphorus mixed acid process.
4. The method for preparing ultrafine tungsten trioxide according to claim 1, characterized in that: In step S1, the at least three gradually increasing temperature sections are specifically: The temperature of the first temperature control zone is 250-450°C, the temperature of the second temperature control zone is 400-600°C; and the temperature of the third temperature control zone is 600-800°C.
5. The method for preparing ultrafine tungsten trioxide according to claim 1, characterized in that: In step S1, the at least three gradually increasing temperature sections are specifically: The temperature of the first temperature control zone is 200-300°C, the temperature of the second temperature control zone is 300-400°C; the temperature of the third temperature control zone is 450-600°C; the temperature of the fourth temperature control zone is 650-800°C.
6. The method for preparing ultrafine tungsten trioxide according to claim 1, characterized in that: In step S1, the at least three gradually increasing temperature sections are specifically: The temperature of the first temperature control zone is 250-350°C, the temperature of the second temperature control zone is 350-450°C; the temperature of the third temperature control zone is 450-550°C; the temperature of the fourth temperature control zone is 550-650°C; the temperature of the fifth temperature control zone is 650-800°C.
7. The method for preparing ultrafine tungsten trioxide according to claim 1, characterized in that: In step S1, the at least three gradually increasing temperature sections are specifically: The temperature of the first temperature control zone is 250-300℃, the temperature of the second temperature control zone is 300-400℃; the temperature of the third temperature control zone is 450-600℃; the temperature of the fourth temperature control zone is 550-700℃; the temperature of the fifth temperature control zone is 600-750℃; the temperature of the sixth temperature control zone is 650-800℃.
8. An ultrafine tungsten trioxide obtained by any preparation method of claims 1-7, characterized in that: Its average particle size is 0.5-1.0 μm.
9. A system for preparing ultrafine tungsten trioxide, characterized in that: include: An APT silo (1), a calcining furnace (2), a tungsten trioxide silo (3), a vibrating screen (4) and a jet mill (5) are arranged in sequence along the feeding direction; wherein the calcining furnace (2) comprises at least three heating sections.
10. The system for preparing ultrafine tungsten trioxide according to claim 9, characterized in that: The at least three heating sections are a first heating section (201), a second heating section (202), a third heating section (203), a fourth heating section (204), a fifth heating section (205) and a sixth heating section (206).
11. The system for preparing ultrafine tungsten trioxide according to claim 9, characterized in that: The discharge port of the jet mill (5) is connected to a material collecting device (6); The air flow mill (5) comprises an air flow crushing chamber, the bottom of which is connected to an air supply system for providing high-pressure air, and the discharge port of the air flow crushing chamber is connected to a material collecting device (6) through a pipeline.
12. The system for preparing ultrafine tungsten trioxide according to claim 11, characterized in that: The material collecting device (6) is a bag dust collector.
Citation Information
Patent Citations
Preparation method for high-purity ammonium paratungstate
CN102674460A
Preparation method of high fluidity tungsten oxide
CN104944472A
System and method for preparing blue tungsten high in specific surface area
CN105016393A
Preparation method and system of superfine tungsten trioxide
CN116282175A
High-purity ammonium paratungstate preparation system
CN202688007U
Cited By
Spongy tungsten trioxide and preparation method thereof
CN120736566A
Ultra-thick tabular tungsten oxide and preparation method thereof
CN121377119A