Biodegradable polyester composition, and preparation method therefor and use thereof
By using inorganic rigid particles with specific particle size distribution in biodegradable polyester, combining copolyester and polylactic acid, the high cost problem in the prior art is solved, and bioavailable with high mechanical properties and low apparent density is achieved Degrading polyester films reduces the cost of materials.
Patent Information
- Application Number
- PCT/CN2023/133479
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2023-11-22
- Publication Date
- 2024-11-14
AI Technical Summary
The prior art improves the mechanical properties of biodegradable polyester by adding inorganic rigid particles, but it is difficult to reduce the cost of material while ensuring performance.
Using a mixture of acid-etchable and non-etchable inorganic rigid particles with specific particle size distribution, combined with biodegradable copolyester and polylactic acid, the weight ratio and particle size distribution are adjusted to prepare a table with better mechanical properties and lower surfaces. A biodegradable polyester composition of considerable density.
It is achieved to improve the mechanical properties of the film with the same apparent thickness, and at the same time reduce the cost of materials. By adjusting the distribution of inorganic particles, the toughness and dimensional stability of the composition are enhanced, and the tensile strength and impact are improved. Strength while maintaining a low apparent density.
Smart Images

Figure PCTCN2023133479-FTAPPB-I100001 
Figure PCTCN2023133479-FTAPPB-I100002 
Figure PCTCN2023133479-FTAPPB-I100003
Abstract
Description
A biodegradable polyester composition and its preparation method and application Technical Field
[0001] The present invention belongs to the field of biodegradable polyesters, and in particular relates to a biodegradable polyester composition, a preparation method and an application thereof. Background Art
[0002] Biodegradable polyester is a type of polymer material derived from biological resources. Compared to petroleum-based polymers derived from petrochemical resources, biodegradable polyester is able to degrade through biological or biochemical processes or in the biological environment. It is currently one of the most actively researched and marketed biodegradable materials for biodegradable plastics. Biodegradable polyester film is currently one of the most important applications for biodegradable polyester. Biodegradable polyester features a soft texture, is non-toxic, is easy to process, exhibits good chemical stability, possesses a certain strength, and exhibits excellent resistance to chemical solvents and cold weather. It is widely used in shopping bags, kitchen waste bags, food packaging films, agricultural mulch films, and other applications.
[0003] With increasing demand and tight supply of chemical raw materials, the price of biodegradable polyester has skyrocketed. Adding inorganic rigid particles is a key approach to improving performance and reducing costs. However, existing biodegradable polyesters produced by adding inorganic rigid particles cannot achieve both good mechanical properties and low material costs.
[0004] Summary of the Invention
[0005] The present invention aims to overcome the shortcomings of the prior art by providing a biodegradable polyester composition, preparation method, and application thereof. Films made from this biodegradable polyester composition, with similar inorganic content, exhibit improved mechanical properties and lower apparent density at the same apparent thickness, thereby reducing material costs.
[0006] In order to achieve the above object, the present invention adopts the following technical solution: a biodegradable polyester composition comprising the following components in percentage by weight:
[0007] i. 75 to 100 weight percent of a biodegradable copolyester, based on the total weight of components i to ii;
[0008] ii. 0 to 25 weight percent polylactic acid, based on the total weight of components i to ii;
[0009] iii. 15 to 30 weight percent of acid-etchable inorganic rigid particles, based on the total weight of components i to iv;
[0010] iv. 1 to 15 weight percent of non-acid-etchable inorganic rigid particles, based on the total weight of components i to iv.
[0011] The mixed particle size of the acid-etchable inorganic rigid particles and the non-acid-etchable inorganic rigid particles conforms to the following distribution: D90 < 12 μm, D95 = 15-25 μm, wherein D90 and D95 are measured by the laser particle size multimodal distribution particle size of the residue calcined at 500°C.
[0012] It can be understood that in the present invention, D90<12μm, can be understood as including but not limited to 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm; D95=15~25μm, can be understood as including but not limited to 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm.
[0013] Preferably, the mixed particle size of the acid-etchable inorganic rigid particles and the non-acid-etchable inorganic rigid particles conforms to the following distribution: D90≤7.5 μm, D95=16.3-21.5 μm.
[0014] More preferably, the mixed particle size of the acid-etchable inorganic rigid particles and the non-acid-etchable inorganic rigid particles conforms to the following distribution: D90 = 6.2-7.3 μm, D95 = 17.4-20.8 μm.
[0015] Preferably, the biodegradable polyester composition comprises the following components in percentage by weight:
[0016] i. 90-95% by weight of a biodegradable copolyester, based on the total weight of components i-ii;
[0017] ii. 5 to 10 weight percent polylactic acid, based on the total weight of components i to ii;
[0018] iii. 21 to 24 weight percent of acid-etchable inorganic rigid particles, based on the total weight of components i to iv;
[0019] iv. 5 to 8 weight percent of non-acid-etchable inorganic rigid particles, based on the total weight of components i to iv.
[0020] Preferably, the biodegradable copolyester is at least one of a copolymer of butylene adipate and butylene terephthalate, and a copolymer of butylene sebacate and butylene terephthalate.
[0021] More preferably, the molar percentage of butylene terephthalate in the copolymer of butylene adipate and butylene terephthalate is 40 to 60%; the molar percentage of butylene terephthalate in the copolymer of butylene sebacate and butylene terephthalate is 40 to 60%.
[0022] Preferably, the biodegradable polyester composition comprises the following two items (1) and (2):
[0023] (1) The acid-etchable inorganic rigid particles refer to inorganic rigid particles that can be completely dissolved in 1M hydrochloric acid; the acid-etchable inorganic rigid particles are at least one of calcium carbonate and calcite;
[0024] (2) The non-acid-etchable inorganic rigid particles refer to inorganic rigid particles that cannot be completely dissolved in 1M hydrochloric acid; the non-acid-etchable inorganic rigid particles include at least one of talc, silicon dioxide, barium sulfate, and titanium dioxide.
[0025] Preferably, the biodegradable polyester composition further comprises an opening agent, which accounts for 0 to 0.5% of the total weight of components i to iv. The opening agent is a common component in the art.
[0026] A method for preparing the biodegradable polyester composition comprises the following steps:
[0027] The biodegradable copolyester and polylactic acid are firstly uniformly mixed and dried, and then stirred and mixed with acid-etchable inorganic rigid particles, non-acid-etchable inorganic rigid particles and an opener. The uniform mixture is melt-plasticized, extruded and granulated to obtain a biodegradable polyester composition.
[0028] Preferably, the drying temperature is 70-90° C., and the drying time is 4-6 hours.
[0029] Preferably, the stirring and mixing time is 1 to 5 minutes.
[0030] Preferably, the set temperature for melt plasticization, extrusion and granulation is 60-190° C., the rotation speed is 250-320 rpm, and the extrusion speed is 550-630 kg / h.
[0031] A use of the biodegradable polyester composition in preparing a biodegradable film product, wherein the biodegradable film product includes any one of a shopping bag, a kitchen waste bag, a food packaging film, and an agricultural mulch film.
[0032] The acid-etchable inorganic rigid particles selected in the present invention have better dispersibility in the weakly acidic environment of the biodegradable polyester melt and can effectively increase the toughness of the composition; the non-acid-etchable inorganic rigid particles have better dimensional stability in the weakly acidic environment of the biodegradable polyester melt and can effectively increase the rigidity of the composition. Inorganic rigid particles with smaller particle sizes are more easily encapsulated by the resin matrix, which can enhance the continuous phase but significantly increase the apparent density of the resulting film; inorganic rigid particles with larger particle sizes are not easily encapsulated by the resin matrix and protrude from the surface of the resulting film, which is beneficial to reducing the apparent density but causes a decrease in mechanical properties due to the destruction of the continuous phase. By adjusting the weight ratio and particle size distribution of the acid-etchable inorganic rigid particles and the non-acid-etchable inorganic rigid particles, the resulting biodegradable polyester composition can have good mechanical properties such as tensile strength and impact strength, while having a lower apparent density.
[0033] All inorganic rigid particles mentioned in the present invention refer to the sum of acid-etchable inorganic rigid particles and non-acid-etchable inorganic rigid particles.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The present invention uses inorganic rigid particles with a specific particle size distribution in a biodegradable polyester composition so that the mixed particle size distribution satisfies the following conditions: D90 < 12 μm, D95 = 15-25 μm. Films with similar inorganic matter content prepared from the biodegradable polyester composition have better mechanical properties and lower apparent density at similar apparent thickness, effectively reducing the amount of material used and thus further lowering the material cost. DETAILED DESCRIPTION
[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0037] In the following examples and comparative examples, the experimental methods used are conventional methods unless otherwise specified. Unless otherwise specified, the opener is commercially available and the same one is used in parallel experiments.
[0038] The raw materials used in the examples and comparative examples are shown in Table 1.
[0039] Table 1
[0040] In the embodiment of the present invention, the weight ratio of the acid-etchable inorganic rigid particles to the non-acid-etchable inorganic rigid particles is adjusted to thereby adjust the sizes of the mixed particle size distribution D90 and D95 of the acid-etchable inorganic rigid particles and the non-acid-etchable inorganic rigid particles.
[0041] Examples 1 to 6 and Comparative Examples 1 to 5
[0042] The components and weight proportions of the biodegradable polyester compositions of Examples 1 to 6 and Comparative Examples 1 to 5 are shown in Table 2.
[0043] The preparation method of the biodegradable polyester composition of Examples 1 to 6 and Comparative Examples 1 to 5 comprises the following steps:
[0044] First, the biodegradable copolyester and polylactic acid are uniformly mixed, dried at 80°C for 5 hours, and then stirred and mixed with acid-etchable inorganic rigid particles, non-acid-etchable inorganic rigid particles and an opener for 3 minutes. The resulting uniform mixture is fed into a twin-screw extruder for melt plasticization, extrusion and granulation to obtain a biodegradable polyester composition.
[0045] Among them, the twin-screw extruder is a co-rotating parallel twin-screw extruder with a screw length-diameter ratio of 40:1. Its set temperatures are: zone 1: 80°C, zone 2: 130°C, zone 3: 150°C, zone 4: 180°C, zone 5: 180°C, zone 6: 180°C, zone 7: 180°C, zone 8: 180°C, zone 9: 180°C, die head: 180°C, screw speed: 300rpm, extrusion speed: 600kg / h.
[0046] Inorganic rigid particle content and multi-peak particle size determination
[0047] A certain amount of the biodegradable polyester composition was placed in a covered crucible and calcined in a muffle furnace at 500°C to constant weight. The resulting solid was weighed to determine the total ash content (inorganic rigid particles). A portion was added to an excess of 1M hydrochloric acid and stirred thoroughly. After no bubbles were generated, the precipitate was centrifuged to obtain a precipitate. The precipitate was washed with deionized water until the pH of the eluate reached 7, dried under vacuum, and weighed to determine the non-acid-etchable inorganic rigid particle content. The acid-etchable inorganic rigid particle content was determined by subtracting the non-acid-etchable inorganic rigid particle content from the total inorganic rigid particle content. The multimodal particle size of the inorganic rigid particles was measured on a Malvern Panalytical Mastersizer laser particle size analyzer using water or ethanol as the dispersion phase.
[0048] Table 2 Component dosage in Examples and Comparative Examples (parts by weight)
[0049] Performance Testing
[0050] The biodegradable polyester compositions prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were subjected to relevant performance tests. The test methods and standards are as follows. The experimental results are shown in Table 3.
[0051] (1) Thickness and apparent density
[0052] The biodegradable polyester composition was formed into a 20±2 μm film using a single-screw film blowing machine with a screw diameter of 45 cm and an aspect ratio of 20:1. The apparent thickness was controlled uniformly using a thickness gauge. The average apparent thickness was measured according to ISO 4593:1993. The meter weight was measured and the apparent density was calculated.
[0053] (2) Mechanical properties of membrane materials
[0054] The tensile strength and elongation at break were tested using ISO 527-3:2018, the tear strength was tested using ISO 6383-2:2004, and the dart impact strength was tested using ISO 7765-1:1998.
[0055] Table 3 Performance test results
[0056] From the experimental data in Table 3, it can be seen that the films made from the biodegradable polyester compositions of the embodiments of the present invention can well balance mechanical properties and apparent density at similar thicknesses, achieving low apparent density while having good mechanical properties, thereby reducing material costs. The apparent density can be maintained at 0.891 to 0.989 g·cm -3 The longitudinal tensile strength can be maintained at 19-20 MPa, the transverse tensile strength can be maintained at 10-13 MPa, the longitudinal tear strength can be maintained at 1862-1937 mN, the transverse tear strength can be maintained at 2103-2460 mN, and the drop impact strength can be maintained at 188-205 g.
[0057] The weight fractions of the etchable inorganic rigid particles and the non-etchable inorganic rigid particles added in Comparative Examples 1 to 3 are inappropriate, resulting in mechanical properties such as tensile strength, tear strength, and impact strength being worse than those in the examples; Comparative Example 4 only adds a single etchable inorganic rigid particle, resulting in a larger apparent density; Comparative Example 5 only adds a single non-etchable inorganic rigid particle, and has a lower apparent density, but its mechanical properties such as tensile strength, tear strength, and impact strength are all poor, and are significantly worse than those in the examples. This shows that only under the joint action of etchable and non-etchable inorganic rigid particles can it be achieved to have better mechanical properties while maintaining a lower apparent density, which is beneficial to reducing material costs at the terminal.
[0058] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the present invention. Anyone skilled in the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by one of ordinary skill in the art without departing from the spirit and technical principles disclosed herein are intended to be covered by the claims of the present invention.
Claims
1. A biodegradable polyester composition, characterized in that The following components are included in weight percentage: i. 75 to 100 weight percent of a biodegradable copolyester, based on the total weight of components i to ii; ii. 0 to 25% by weight of polylactic acid, based on the total weight of components i to ii; iii. 15 to 30 weight percent of acid-etchable inorganic rigid particles, based on the total weight of components i to iv; iv. 1 to 15 weight percent of non-acid-etchable inorganic rigid particles, based on the total weight of components i to iv; The mixed particle size of the acid-etchable inorganic rigid particles and the non-acid-etchable inorganic rigid particles conforms to the following distribution: D90<12 μm, D95=15-25 μm.
2. The biodegradable polyester composition according to claim 1, characterized in that The following components are included in weight percentage: i. 90-95 wt % of a biodegradable copolyester, based on the total weight of components i-ii; ii. 5 to 10 wt% polylactic acid, based on the total weight of components i to ii; iii. 21 to 24 weight percent of acid-etchable inorganic rigid particles, based on the total weight of components i to iv; iv. 5 to 8 wt% of non-acid-etchable inorganic rigid particles, based on the total weight of components i to iv.
3. The biodegradable polyester composition according to claim 1 or 2, characterized in that: The biodegradable copolyesters are copolymers based on aliphatic and / or aromatic dicarboxylic acids and on aliphatic dihydroxy compounds.
4. The biodegradable polyester composition according to claim 1, characterized in that The biodegradable copolyester includes at least one of a copolymer of butylene adipate and butylene terephthalate and a copolymer of butylene sebacate and butylene terephthalate.
5. The biodegradable polyester composition according to claim 1, characterized in that It includes the following two items (1) and (2): (1) The acid-etchable inorganic rigid particles are at least one of calcium carbonate and calcite; (2) The non-acid-erodible inorganic rigid particles include at least one of talc, silicon dioxide, barium sulfate, and titanium dioxide.
6. The biodegradable polyester composition according to claim 1, characterized in that The biodegradable polyester composition further comprises an opening agent which accounts for 0 to 0.5% of the total weight of components i to iv.
7. A method for preparing the biodegradable polyester composition according to any one of claims 1 to 6, characterized in that: The following steps are involved: The biodegradable copolyester and polylactic acid are firstly uniformly mixed and dried, and then stirred and mixed with acid-etchable inorganic rigid particles, non-acid-etchable inorganic rigid particles and an opening agent, and the uniform mixture is melt-plasticized, extruded and granulated to obtain a biodegradable polyester composition.
8. The preparation method according to claim 7, characterized in that: At least one of the following (1) and (2): (1) The drying temperature is 70 to 90° C. and the drying time is 4 to 6 hours; (2) The stirring and mixing time is 1 to 5 minutes.
9. The preparation method according to claim 7, characterized in that: The setting temperature of the melt plasticization, extrusion and granulation is 60-190° C., the rotation speed is 250-320 rpm, and the extrusion speed is 550-630 kg / h.
10. Use of the biodegradable polyester composition according to any one of claims 1 to 6 in the preparation of biodegradable film products.
Citation Information
Patent Citations
Novel heat-resistant high-toughness polylactic acid composite material and preparation method thereof
CN103819884A
Biodegradable polyester foam material and preparation method thereof
CN110591304A
PLA / PBAT biodegradable composite material and product thereof
CN111718566A
PBAT composite material film as well as preparation method and application thereof
CN112341763A
High-rate PBAT foamed bead and preparation method thereof
CN113736228A
Cited By
Polyester composition as well as preparation method and application thereof
CN119955264A
A polyester composition, its preparation and use
CN119955264B