Composite current collector having cold-resistance and Anti-adhesion functions

By using cold-resistant polymer base film and metal foil layer in the composite liquid collection of lithium-ion batteries, combining specific ester compounds and antiblocking agents, the problem of reducing reactivity and preparation of easy adhesion in low temperature environments is solved, and high Performance and low-cost composite fluid collection, suitable for use in low temperature areas.

WO2024230186A1PCT designated stage expired Publication Date: 2024-11-14YANGZHOU NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/141154
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2023-12-22
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Lithium-ion batteries have reduced reactivity in low temperature environments, resulting in attenuation of charge and discharge performance, and the composite liquid collector is prone to stick to each other during the preparation process, with low product yield and high production cost.

Method used

A cold-resistant polymer base film consisting of 92-95 parts of polymer resin and 5-8 parts of cold-resistant agent is used, and a metal foil layer is prepared on both sides of it, through specific ester compounds, organic antiblocking agents and cold-resistant polycarbonate Aids improve performance, increase surface area and bonding, avoid adhesions, and reduce costs by improving metal foil layer processing technology.

Benefits of technology

The excellent performance of composite fluid collectors at low temperatures of -20 to -40°C is achieved, which reduces the problem of adhesion, improves flexibility and anti-extrusion pressure, reduces the preparation cost, and increases the energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023141154-FTAPPB-I100001
    Figure PCTCN2023141154-FTAPPB-I100001
Patent Text Reader

Abstract

The present application relates to the technical field of lithium-ion batteries, and specifically relates to a composite current collector having cold-resistance and anti-adhesion functions. In order to improve the performance of a composite current collector at a low temperature, a cold-resistant agent is prepared, such that various disadvantages, such as easy breakage, increased brittleness and reduced elongation, of a conventional plastic product under low-temperature conditions can be overcome, thereby enabling a prepared composite current collector to have extremely strong cold resistance, good flexibility, and high strength against pressure. On this basis, an organic anti-adhesion agent of a specific cross-linking structure is further added to the cold-resistant agent, and can form protrusions having a certain height on the surface of a thin film after directional stretching is performed, thereby achieving the effects of increasing surface roughness and preventing adhesion. Moreover, by means of improving a metal foil layer processing technique, the use of metal raw materials is reduced, and the cost and weight are reduced, thereby promoting an increase in the energy density of a battery.
Need to check novelty before this filing date? Find Prior Art

Description

A composite current collector with cold-resistant and anti-adhesion functions Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a composite current collector with cold-resistant and anti-adhesion functions. Background Art

[0002] Lithium-ion batteries, with their high energy density, long cycle life, and zero pollution, are currently the most ideal power source for 3C batteries, power batteries, and energy storage batteries. The rapid expansion of the new energy industry has led to a growing demand for lithium-ion batteries, further highlighting the advantages of new composite current collectors.

[0003] A composite current collector is a multilayer composite material prepared by depositing a metal layer on the surface of a polymer film. Compared with traditional current collectors, composite current collectors have the following advantages: ① Less metal raw material usage, which promotes lower battery costs; ② The unique multilayer structure promotes improved battery safety performance; ③ Lighter weight, which promotes increased battery energy density.

[0004] However, lithium-ion batteries are sensitive to changes in ambient temperature. Generally, the optimal operating temperature range for lithium-ion batteries is 20-30°C. The composite current collector, a battery component, generally functions relatively stably within the range of 0-45°C, and the current collector has the best conductivity. However, in extremely cold regions, the average winter temperature is below 0°C, which reduces the internal reaction activity of the battery. At the same time, in this case, the substandard performance of the composite current collector will lead to a decrease in the charge and discharge performance of the lithium-ion battery. In addition, compared with conventional current collectors, the composite current collector uses a polymer film as a substrate during the preparation process. Due to the limitations of the polymer's own properties, the composite current collector is prone to adhesion during the preparation process, resulting in low product yield and high preparation costs. Therefore, it is necessary to conduct research on the above shortcomings to meet market demand.

[0005] Summary of the Invention

[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0007] The purpose of this application is to provide a composite current collector with cold-resistant and anti-adhesion functions to solve the problems raised in the above background technology.

[0008] In order to solve the above technical problems, the present application provides the following technical solutions: a composite current collector with cold-resistant and anti-adhesion functions, having the following characteristics: the composite current collector with cold-resistant functions is composed of a cold-resistant polymer base film and metal foil layers on both sides thereof;

[0009] Wherein, the cold-resistant polymer base film is composed of 92-95 parts of polymer resin and 5-8 parts of cold-resistant agent in parts by weight.

[0010] Optionally, the cold-resistant polymer base film has a thickness of 2-6 microns.

[0011] Optionally, the polymer resin is any one or more of polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyimide, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene, polycarbonate, polyetheretherketone, polyamide, and polyimide.

[0012] Optionally, the cold-resistant agent is composed of 1-2 parts of ester compounds, 3-4 parts of organic anti-blocking agents, and 1-2 parts of cold-resistant polycarbonate additives, calculated by weight.

[0013] Optionally, the ester compound is any one or more of dioctyl adipate, diisodecyl adipate, dioctyl azelaic acid, dibutyl sebacate, dioctyl sebacate, diisooctyl sebacate, di(2-ethylbutyric acid) triethylene glycol ester, dioctyl phthalate, diisooctyl phthalate, diisodecyl phthalate, dibutyl phthalate, diisobutyl phthalate, butyl benzyl phthalate, dimethyl phthalate, diethyl phthalate, dicyclohexyl phthalate, and dioctyl terephthalate.

[0014] Optionally, the organic anti-blocking agent is any one of an organic silicon polymer or a methacrylate polymer.

[0015] Optionally, the cold-resistant polycarbonate auxiliary agent is any one or more of methyl methacrylate-butadiene-styrene copolymer, ethylene-butyl acrylate copolymer, butyl acrylate (BA) and methyl methacrylate.

[0016] Optionally, the metal foil layer is any one of copper foil and aluminum foil.

[0017] A method for preparing a composite current collector with cold-resistant and anti-adhesion functions comprises the following steps:

[0018] S1. Preparation of cold-resistant agent;

[0019] The ester compound, the organic anti-blocking agent and the cold-resistant polycarbonate additive are mixed, heated to 80-120° C., stirred for 10-15 minutes, then the heating is stopped and the mixture is cooled to room temperature to obtain a cold-resistant agent;

[0020] S2. The polymer resin is mixed with a cold-resistant agent, heated to 150-400 ℃, stirred for 5-8min, extruded, and stretched to obtain a cold-resistant polymer base film;

[0021] S3. Prepare metal foil layers on both sides of the cold-resistant polymer base film to obtain a composite current collector with cold-resistant and anti-adhesion functions.

[0022] Optionally, in step S3, when the metal foil layer is copper foil, the preparation method includes the following steps:

[0023] Magnetron sputtering copper layers on both sides of the cold-resistant polymer base film prepared in step S2, after the thickness of the copper layer on one side reaches 0.25-0.35 microns, metallizing the base film, removing it, and electroplating it with copper until the overall thickness reaches 5.5-6.5 microns, removing it, washing the surface with acetone, and drying it to obtain a composite current collector with cold-resistant and anti-adhesion functions;

[0024] When the metal foil layer is aluminum foil, the preparation method thereof comprises the following steps:

[0025] Aluminum layers are evaporated on both sides of the cold-resistant polymer base film obtained in step S2 until the thickness reaches 7-9 microns, and then the evaporation is stopped to obtain a composite current collector with cold-resistant and anti-adhesion functions.

[0026] Compared with the prior art, the beneficial effects achieved by the present application are: the present application prepares a cold-resistant agent, which can solve the various disadvantages of traditional plastic products such as easy breakage, increased brittleness, and reduced elongation under low temperature conditions, so that the composite current collector prepared by the present application has extremely strong cold resistance, excellent flexibility, and high strength anti-extrusion force, and can still maintain the excellent performance of the current collector product at low temperatures of -20 to -40°C, and is suitable for use in low temperature areas. On this basis, in order to reduce the problem of easy adhesion in the preparation of the composite current collector, the present application also adds an organic anti-adhesion agent with a specific cross-linking structure, which, after mixing with the polymer resin, will form a cross-linking agent on the surface of the film after directional stretching. The cold-resistant polymer base film is formed into protrusions of a certain height, thereby greatly increasing the surface area of ​​the cold-resistant polymer base film, thereby increasing the contact area with the plated metal. After the metal foil layer is evaporated, the surface of the composite current collector finally prepared can have a certain roughness, thereby effectively avoiding the adhesion of the composite current collector; at the same time, the present application also adds acid ester compounds when preparing the cold-resistant agent, which can effectively improve the surface polarity of the polymer base film, thereby further enhancing the adhesion between the base film and the metal foil layer, and avoiding the peeling of the metal foil layer; afterwards, the present application also reduces the use of metal raw materials, reduces cost and quality, and promotes the improvement of battery energy density by improving the metal foil layer processing technology.

[0027] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION

[0028] The following is a clear and complete description of the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0029] In the examples and comparative examples of the present application, the diisodecyl adipate used is CAS No. 27178-16-1; the methacrylate polymer used is CAS No. 921214-61-1; the methyl methacrylate-butadiene-styrene copolymer used is CAS No. 25053-09-2; and the polypropylene resin used is CAS No. 86403-32-9.

[0030] Example 1:

[0031] A method for preparing a composite current collector with cold-resistant and anti-adhesion functions comprises the following steps:

[0032] S1. Preparation of cold-resistant agent;

[0033] Mix 1 part of diisodecyl adipate, 3 parts of methacrylate polymer, and 1 part of methyl methacrylate-butadiene-styrene copolymer by weight, heat to 95° C., stir for 10 minutes, stop heating, and cool to room temperature to obtain a cold-resistant agent;

[0034] S2. In parts by weight, 95 parts of polypropylene resin and 5 parts of the cold-resistant agent obtained in step S1 were mixed, heated to 135 ℃, stirred for 5min, extruded, and stretched to obtain a cold-resistant polymer base film having a thickness of 4.5 microns;

[0035] S3. Prepare metal foil layers on both sides of the cold-resistant polymer base film by using magnetron sputtering technology. The general cooling temperature in the magnetron sputtering chamber is -15°C and the deep cooling temperature is -125°C. A layer of copper foil with a thickness of 0.3 microns is sputtered on the cold-resistant polymer base film to realize base film metallization. Then, the copper foil electroplating process is adopted. The electroplating temperature is 25°C, the electroplating thickening time is 10 minutes, the working voltage is 3V, and the relative movement speed of the plastic film with respect to the brush roller is 5m / min. The thickness of the composite copper foil is increased to obtain a composite copper foil with an overall thickness of 5.5 microns. After the electroplating is completed, the surface is cleaned with acetone. After drying, a composite current collector with cold-resistant and anti-adhesion functions is obtained.

[0036] Example 2.

[0037] A method for preparing a composite current collector with cold-resistant and anti-adhesion functions comprises the following steps:

[0038] S1. Preparation of cold-resistant agent;

[0039] Mix 2 parts of diisodecyl adipate, 4 parts of methacrylate polymer, and 2 parts of methyl methacrylate-butadiene-styrene copolymer by weight, heat to 95° C., stir for 10 minutes, stop heating, and cool to room temperature to obtain a cold-resistant agent;

[0040] S2. In parts by weight, 92 parts of polypropylene resin and 8 parts of the cold-resistant agent obtained in step S1 were mixed, heated to 135 ℃, stirred for 5min, extruded, and stretched to obtain a cold-resistant polymer base film having a thickness of 4.5 microns;

[0041] S3. Prepare metal foil layers on both sides of the cold-resistant polymer base film by using magnetron sputtering technology. The general cooling temperature in the magnetron sputtering chamber is -15°C and the deep cooling temperature is -130°C. A layer of copper foil with a thickness of 0.3 microns is sputtered on the cold-resistant polymer base film to realize base film metallization. Then, the copper foil electroplating process is adopted. The electroplating temperature is 25°C, the electroplating thickening time is 10 minutes, the working voltage is 3V, and the relative movement speed of the plastic film with respect to the brush roller is 5m / min. The thickness of the composite copper foil is increased to obtain a composite copper foil with an overall thickness of 5.5 microns. After the electroplating is completed, the surface is cleaned with acetone. After drying, a composite current collector with cold-resistant and anti-adhesion functions is obtained.

[0042] Example 3.

[0043] A method for preparing a composite current collector with cold-resistant and anti-adhesion functions comprises the following steps:

[0044] S1. Preparation of cold-resistant agent;

[0045] Mix 1 part of diisodecyl adipate, 3 parts of methacrylate polymer, and 1 part of methyl methacrylate-butadiene-styrene copolymer by weight, heat to 95° C., stir for 10 minutes, stop heating, and cool to room temperature to obtain a cold-resistant agent;

[0046] S2. In parts by weight, 95 parts of polypropylene resin and 5 parts of the cold-resistant agent obtained in step S1 were mixed, heated to 135 ℃, stirred for 5min, extruded, and stretched to obtain a cold-resistant polymer base film having a thickness of 6 microns;

[0047] S3. The cold-resistant polymer base film and 99.9% high-purity aluminum ingot were placed in a vacuum evaporation device. The concentration of aluminum vapor was maintained at 30 mol / L, the temperature of the evaporated aluminum metal was 800 ° C, and the vacuum degree was 5 × 10 -2 Pa, evaporate an aluminum foil layer with a thickness of 1 micron on the cold-resistant polymer base film, take it out, and obtain a composite current collector with cold-resistant and anti-adhesion functions.

[0048] Example 4.

[0049] A method for preparing a composite current collector with cold-resistant and anti-adhesion functions comprises the following steps:

[0050] S1. Preparation of cold-resistant agent;

[0051] Mix 2 parts of diisodecyl adipate, 4 parts of methacrylate polymer, and 2 parts of methyl methacrylate-butadiene-styrene copolymer by weight, heat to 95° C., stir for 10 minutes, stop heating, and cool to room temperature to obtain a cold-resistant agent;

[0052] S2. In parts by weight, 92 parts of polypropylene resin and 8 parts of the cold-resistant agent obtained in step S1 were mixed, heated to 135 ℃, stirred for 5min, extruded, and stretched to obtain a cold-resistant polymer base film having a thickness of 6 microns;

[0053] S3. The cold-resistant polymer base film and 99.9% high-purity aluminum ingot were placed in a vacuum evaporation device. The concentration of aluminum vapor was maintained at 30 mol / L, the temperature of the evaporated aluminum metal was 800 ° C, and the vacuum degree was 5 × 10 -2 Pa, evaporate an aluminum foil layer with a thickness of 1 micron on the cold-resistant polymer base film, take it out, and obtain a composite current collector with cold-resistant and anti-adhesion functions.

[0054] Comparative Example 1.

[0055] A method for preparing a current collector comprises the following steps:

[0056] S1. The polypropylene resin was heated to 135°C, stirred for 5 minutes, extruded, and stretched to obtain a cold-resistant polymer base film having a thickness of 4.5 microns;

[0057] S2. Prepare metal foil layers on both sides of the cold-resistant polymer base film by using magnetron sputtering technology. The general cooling temperature in the magnetron sputtering chamber is -15°C and the deep cooling temperature is -150°C. A layer of copper foil with a thickness of 0.1 microns is sputtered on the cold-resistant polymer base film to achieve base film metallization. Then, the copper foil electroplating process is adopted. The electroplating temperature is 25°C, the electroplating thickening time is 10 minutes, the working voltage is 3V, and the relative movement speed of the plastic film with respect to the brush roller is 5m / min. The thickness of the composite copper foil is increased to obtain a composite copper foil with an overall thickness of 5.5 microns. After the electroplating is completed, the surface is cleaned with acetone and dried to obtain a composite current collector.

[0058] Comparative Example 2.

[0059] A method for preparing a current collector comprises the following steps:

[0060] S1. The polypropylene resin was heated to 135°C, stirred for 5 minutes, extruded, and stretched to obtain a cold-resistant polymer base film having a thickness of 6 microns;

[0061] S2 puts the cold-resistant polymer base film and 99.9% high-purity aluminum ingot into the vacuum evaporation device respectively. The concentration of aluminum vapor is maintained at 30 mol / L, the temperature of evaporating metal aluminum is 800℃, and the vacuum degree is 5×10 -2 Pa, evaporate an aluminum foil layer with a thickness of 1 micron on the cold-resistant polymer base film, take it out, and obtain a composite current collector.

[0062] Testing: The composite current collector was placed in a -20°C environment for 30 minutes and then subjected to mechanical property testing. The testing method is as follows:

[0063] The room temperature tensile strength and elongation at break were measured using an electronic universal material testing machine with the following test conditions: gauge length 100 mm, tensile speed 100 mm / min, and width 15 mm;

[0064] Coating peel strength test: The test method is as follows: Take a test sample with a size of 15*100mm, stick 3M-9080A-15mm tape on a stainless steel plate, then evenly stick the test sample on the double-sided tape and squeeze it back and forth twice with a 2kg standard small pressure roller. Then stick 3M-9080A-14mm tape on the sample surface and squeeze it back and forth twice with a 2kg standard small pressure roller. Then, take the pressed sample to a tensile testing machine and stretch it 180° at a speed of 100mm / min and a width of 14mm. The maximum value is taken.

[0065] Comparing the tensile strength and elongation of the composite copper foil and composite aluminum foil made with two kinds of cold-resistant agent components, the test results are shown in the table below;

[0066] Finally, it should be noted that the above description is merely a preferred embodiment of the present application and is not intended to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art may still modify the technical solutions described in the aforementioned embodiments or substitute equivalents for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included within the scope of protection of the present application.

Claims

1. A composite current collector with cold-resistant and anti-adhesion function, consisting of a cold-resistant polymer base film and metal foil layers on both sides thereof; in, The cold-resistant polymer base film is composed of 92-95 parts of polymer resin and 5-8 parts of cold-resistant agent by weight.

2. The composite current collector having cold-resistant and anti-adhesion function according to claim 1, wherein: The thickness of the cold-resistant polymer base film is 2-6 microns.

3. The composite current collector having cold-resistant and anti-adhesion function according to claim 1 or 2, wherein: The polymer resin is any one or more of polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyimide, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene ether, polystyrene, polycarbonate, polyetheretherketone, polyamide, and polyimide.

4. The composite current collector having cold-resistant and anti-adhesion functions according to any one of claims 1 to 3, wherein: In terms of weight, the cold-resistant agent is composed of 1-2 parts of ester compounds, 3-4 parts of organic anti-adhesion agents, and 1-2 parts of cold-resistant polycarbonate additives.

5. The composite current collector having cold-resistant and anti-adhesion function according to claim 4, wherein: The ester compound is any one or more of dioctyl adipate, diisodecyl adipate, dioctyl azelaic acid, dibutyl sebacate, dioctyl sebacate, diisooctyl sebacate, di(2-ethylbutyric acid) triethylene glycol ester, dioctyl phthalate, diisooctyl phthalate, diisodecyl phthalate, dibutyl phthalate, diisobutyl phthalate, butyl benzyl phthalate, dimethyl phthalate, diethyl phthalate, dicyclohexyl phthalate, and dioctyl terephthalate.

6. The composite current collector with cold-resistant and anti-adhesion function according to claim 4 or 5, wherein: The organic anti-blocking agent is any one of an organic silicon polymer or a methacrylate polymer.

7. The composite current collector having cold-resistant and anti-adhesion functions according to any one of claims 4 to 6, wherein: The cold-resistant polycarbonate auxiliary agent is any one or more of methyl methacrylate-butadiene-styrene copolymer, ethylene-butyl acrylate copolymer, butyl acrylate (BA) and methyl methacrylate.

8. The composite current collector having cold-resistant and anti-adhesion functions according to any one of claims 1 to 7, wherein: The metal foil layer is any one of copper foil and aluminum foil.

9. A method for preparing a composite current collector having cold-resistant and anti-adhesion functions as claimed in claims 1 to 8, comprising the following steps: S1. Preparation of cold-resistant agent; The ester compound, the organic anti-blocking agent and the cold-resistant polycarbonate additive are mixed, heated to 80-120°C, stirred for 10-15 minutes, then the heating is stopped and cooled to room temperature to obtain a cold-resistant agent; S2. The polymer resin and the cold-resistant agent are mixed, heated to 150-400°C, stirred for 5-8min, extruded, and stretched to obtain a cold-resistant polymer base film; S3. Prepare metal foil layers on both sides of the cold-resistant polymer base film to obtain a composite current collector with cold-resistant and anti-adhesion functions.

10. The method for preparing a composite current collector having cold-resistant and anti-adhesion functions according to claim 9, wherein: In step S3, when the metal foil layer is copper foil, the preparation method includes the following steps: The copper layer is magnetron sputtered on both sides of the cold-resistant polymer base film prepared in step S2. After the thickness of the copper layer on one side reaches 0.25-0.35 microns, the base film is metallized, taken out, and electroplated with copper until the overall thickness is 5.5-6.5 microns. After that, the composite current collector with cold-resistant and anti-adhesion function is obtained after washing the surface with acetone and drying. When the metal foil layer is aluminum foil, the preparation method thereof comprises the following steps: Aluminum layers are deposited on both sides of the cold-resistant polymer base film obtained in step S2 until the thickness reaches 7-9 microns. Then the evaporation is stopped to obtain a composite current collector with cold-resistant and anti-adhesion functions.

Citation Information

Patent Citations

  • Improved cold-resistant polycarbonate and ABS (Acrylonitrile Butadiene Styrene) alloy and preparation method thereof

    CN103265802A

  • Composite cathode material of low-temperature lithium ion battery, cathode plate of low-temperature lithium ion battery, preparation method thereof, and lithium ion battery

    CN105914394A

  • Lithium ion secondary battery, battery cell and negative pole piece

    CN111180737A

  • Highly cold-resistant polyvinyl chloride artificial leather and preparation method thereof

    CN113417149A

  • Aluminum composite current collector and preparation method and application thereof

    CN115149000A