Method for forming semiconductor substrate layer, and method for preparing heterojunction cell

By forming a buffer semiconductor layer on the semiconductor substrate layer and performing diffusion annealing treatment, the problem of insufficient miscible absorption capacity in the prior art is solved, more efficient impurity removal is achieved, and the performance of heterojunction batteries is improved.

WO2024230190A1PCT designated stage expired Publication Date: 2024-11-14ANHUI HUASUN ENERGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/141441
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2023-12-25
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The prior art has poor mist absorption capacity of semiconductor substrate layers, which affects the electrical performance of heterojunction batteries.

Method used

A buffered semiconductor layer is formed on the initial surface of the semiconductor substrate layer, and it is converted from amorphous state to a crystal by diffusion annealing treatment, forming a doped layer and an oxide layer, and after removal, the semiconductor substrate layer is formed to enhance the mist absorption capacity.

Benefits of technology

The impurity absorption capacity of the semiconductor substrate layer is significantly improved, and the metal impurity concentration is reduced by 10%-20%, thereby improving the efficiency of heterojunction batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023141441_14112024_PF_FP_ABST
    Figure CN2023141441_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of the preparation of solar cells, and particularly provides a method for forming a semiconductor substrate layer, and a method for preparing a heterojunction cell. The method for forming a semiconductor substrate layer comprises: providing an initial semiconductor substrate layer; forming a buffer semiconductor layer on the surface of at least one side of the initial semiconductor substrate layer, wherein the buffer semiconductor layer is in an amorphous state; after the buffer semiconductor layer is formed, performing diffusion annealing treatment so as to form a doped layer in partial thickness of the buffer semiconductor layer in the process that the buffer semiconductor layer gradually converts from the amorphous state to a crystalline state; in the process of performing diffusion annealing treatment, further forming an oxide layer located on the surface of the side of the doped layer facing away from the buffer semiconductor layer; and removing the oxide layer and the doped layer, so that the initial semiconductor substrate layer and the remaining buffer semiconductor layer jointly form a semiconductor substrate layer. The method for forming a semiconductor substrate layer provided by the present application can improve the capability of gettering for semiconductor substrate layers.
Need to check novelty before this filing date? Find Prior Art

Description

Method for forming semiconductor substrate layer and method for preparing heterojunction battery

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on May 9, 2023, with application number 202310524359.8 and invention name “Method for forming a semiconductor substrate layer and method for preparing a heterojunction battery”, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the technical field of solar cell preparation, and in particular to a method for forming a semiconductor substrate layer and a method for preparing a heterojunction cell. Background Art

[0004] Heterojunction cells use N-type crystalline silicon wafers as their substrate material. Impurities, especially metallic impurities, in the crystalline silicon substrate directly affect the electrical performance of the resulting heterojunction cell. Currently, a common method for reducing impurities is to perform gettering on the crystalline silicon wafers before proceeding with subsequent process steps, such as texturing and cleaning, semiconductor layer deposition, and transparent conductive layer formation. Gettering involves high-temperature phosphorus diffusion, or applying a liquid phosphorus source to the surface of the crystalline silicon wafer. This process then uses chain heating equipment to precipitate impurities from the crystalline silicon and concentrate them in an impurity-rich layer, which is then cleaned and removed.

[0005] As heterojunction cell cost reduction and efficiency improvement standards gradually increase, further reducing impurities in the crystalline silicon substrate has become one of the key challenges in improving heterojunction cell efficiency. However, existing methods for getting impurities in the semiconductor substrate layer have poor gettering capabilities.

[0006] Summary of the Invention

[0007] Therefore, the technical problem to be solved by the present application is to overcome the defect of poor doping ability of the semiconductor substrate layer in the prior art, thereby providing a method for forming a semiconductor substrate layer and a method for preparing a heterojunction battery.

[0008] The present application provides a method for forming a semiconductor substrate layer, comprising: providing an initial semiconductor substrate layer; forming a buffer semiconductor layer on at least one side surface of the initial semiconductor substrate layer, the buffer semiconductor layer being in an amorphous state; the defect concentration within the buffer semiconductor layer being greater than the defect concentration within the initial semiconductor substrate layer; after forming the buffer semiconductor layer, performing a diffusion annealing treatment to form a doped layer in a portion of the buffer semiconductor layer during the process of the buffer semiconductor layer gradually transforming from an amorphous state to a crystalline state; during the diffusion annealing treatment, also forming an oxide layer on a side surface of the doped layer facing away from the buffer semiconductor layer; removing the oxide layer and the doped layer, whereby the initial semiconductor substrate layer and the remaining buffer semiconductor layer together form a semiconductor substrate layer.

[0009] Optionally, the buffer semiconductor layer contains phosphorus atoms, the process of forming the buffer semiconductor layer includes a chemical vapor deposition process, and the thickness of the buffer semiconductor layer is 10 nm-50 nm.

[0010] Optionally, before the buffer semiconductor layer is formed on the surface of at least one side of the initial semiconductor substrate layer, both sides of the initial semiconductor substrate layer have a damaged layer; the method for forming the semiconductor substrate layer also includes: before the buffer semiconductor layer is formed on the surface of at least one side of the initial semiconductor substrate layer, performing surface pre-cleaning treatment on the initial semiconductor substrate layer to remove the damaged layer; wherein, the surface pre-cleaning treatment uses an alkaline solution, the alkaline solution includes a KOH solution or a NaOH solution, the mass percentage concentration of the alkaline solution is 1%-5%, the temperature is 65°C-80°C, and the time of the surface pre-cleaning treatment is 60s-400s.

[0011] Optionally, the process of removing the doping layer includes a wet etching process; wherein the etching solution used is an alkaline solution, the alkaline solution includes a KOH solution or a NaOH solution, the mass percentage concentration of the alkaline solution is 2%-5%, the temperature is 75°C-85°C, and the time for removing the doping layer is 30s-300s.

[0012] Optionally, the process of removing the oxide layer includes a wet etching process; wherein the etching solution used is an acid solution, the acid solution includes an HF solution, the mass percentage concentration of HF is 5%-8%, the temperature is 15°C-30°C, and the time for removing the oxide layer is 60s-600s.

[0013] Optionally, the buffer semiconductor layer includes a first buffer semiconductor layer located on the front side of the initial semiconductor substrate layer and a second buffer semiconductor layer located on the back side of the initial semiconductor substrate layer; the doping layer includes a first doping layer located on the side of the first buffer semiconductor layer away from the initial semiconductor substrate layer and a second doping layer located on the side of the second buffer semiconductor layer away from the initial semiconductor substrate layer; the oxide layer includes a first oxide layer located on the side of the first doping layer away from the first buffer semiconductor layer and a second oxide layer located on the side of the second doping layer away from the second buffer semiconductor layer.

[0014] Optionally, the conductivity type of the doped layer is the same as the conductivity type of the initial semiconductor substrate layer before the diffusion annealing treatment; before the diffusion annealing treatment, the conductivity type of the initial semiconductor substrate layer is N-type, and the conductivity type of the doped layer is N-type.

[0015] Optionally, the gas source used in the diffusion annealing treatment is a phosphorus-containing gas source, and the phosphorus-containing gas source includes POCl3; the doping layer contains phosphorus atoms; the temperature used in the diffusion annealing treatment is 700℃-850℃; the time used in the diffusion annealing treatment is 5min-15min.

[0016] Optionally, it also includes: after forming the semiconductor substrate layer, performing a texturing treatment on at least one side surface of the semiconductor substrate layer; wherein the texturing treatment uses an alkaline texturing solution, the alkaline texturing solution includes a KOH solution or a NaOH solution, the mass percentage concentration of the alkaline texturing solution is 2%-5%, the temperature is 75°C-85°C, and the time is 300s-700s.

[0017] The present application also provides a method for preparing a heterojunction battery, which is based on a semiconductor substrate layer, and is prepared by sequentially forming an intrinsic semiconductor layer, a doped semiconductor layer, a transparent conductive film and a gate electrode on at least one side surface of the semiconductor substrate layer. The characteristic is that the preparation of the semiconductor substrate layer adopts the method for forming the semiconductor substrate layer described in the present application.

[0018] The beneficial effects of this application are:

[0019] The present application provides a method for forming a semiconductor substrate layer, in which a buffer semiconductor layer is formed on at least one side of the surface of the initial semiconductor substrate layer. Since the buffer semiconductor layer is initially amorphous and is a semiconductor layer without regular crystal orientation, its own lattice distortion is very large, and the buffer semiconductor layer has a high defect density. In other words, the buffer semiconductor layer is initially arranged in a disordered manner, with a large number of dangling bonds and vacancy defects. The disordered arrangement energy state is higher, and the ordered arrangement energy state is lower; the defect concentration inside the buffer semiconductor layer is greater than the defect concentration inside the initial semiconductor substrate layer; in the method for forming a semiconductor substrate layer of the present application, under the high temperature state of diffusion annealing, specifically during the heating process, the disordered arrangement portion of the buffer semiconductor layer will gradually transform into a more stable ordered arrangement, so that the buffer semiconductor layer gradually transforms from an amorphous state to a crystalline state. This process will further generate a large number of defects, so that the defect concentration difference between the buffer semiconductor layer and the initial semiconductor substrate layer is increased from the existing 10 5-6 pieces / cm 3 Increased to 10 15-16 pieces / cm 3 (Compared to the existing technology, an increase of about 10 10 times), due to the aggravation of the concentration difference, the diffusion driving force of the metal impurities is enhanced, driving the metal impurities in the initial semiconductor substrate layer to gradually diffuse into the buffer semiconductor layer, so that the metal impurity concentration in the initial semiconductor substrate layer is reduced from 6ppma-7ppma to 4ppma-5ppma, a decrease of 10%-20%, thereby achieving a better impurity gettering effect; secondly, during the diffusion annealing process, the metal impurities are enriched in the buffer semiconductor layer, so that a doped layer is formed in a portion of the thickness of the buffer semiconductor layer. The metal impurities further transfer and diffuse toward the side away from the initial semiconductor substrate layer, and also form an oxide layer on the surface of the doped layer away from the buffer semiconductor layer. Finally, the remaining buffer semiconductor layer, doped layer, and oxide layer are formed in sequence on the surface of the initial semiconductor substrate layer. After removing the oxide layer and the doped layer, the initial semiconductor substrate layer and the remaining buffer semiconductor layer together form a semiconductor substrate layer. In summary, the impurity gettering ability of the semiconductor substrate layer is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the following is a brief introduction to the drawings required for use in the specific implementation methods or the description of the prior art. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0021] FIG1 is a flow chart of a method for forming a semiconductor substrate layer in Example 1 of the present application;

[0022] 2 to 8 are schematic structural diagrams of various processes in the method for forming a semiconductor substrate layer in Example 1 of the present application;

[0023] Explanation of reference numerals: 100 - initial semiconductor substrate layer; 110 - damaged layer; 120 - first buffer semiconductor layer; 130 - second buffer semiconductor layer; 140 - first doped layer; 150 - second doped layer; 160 - first oxide layer; 170 - second oxide layer; 200 - semiconductor substrate layer; 210 - light-trapping surface. DETAILED DESCRIPTION

[0024] The following will clearly and completely describe the technical solution of this application in conjunction with the accompanying drawings. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of this application.

[0025] In the description of this application, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings and are intended solely to facilitate the description of this application and simplify the description. They do not indicate or imply that the devices or components referred to must have a specific orientation, be constructed, or operate in a specific orientation. Therefore, they should not be construed as limitations on this application. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0026] In the description of this application, it should be noted that, unless otherwise expressly specified or limited, the terms "mounted," "connected," and "connected" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integral connections; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; and internal connections between two components. Those skilled in the art will understand the specific meanings of the above terms in this application based on the specific circumstances.

[0027] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0028] Example 1

[0029] The technical concept of this application is to cleverly utilize the disadvantage that a large number of defects are further generated in the buffer semiconductor layer during the process of gradually transforming from an amorphous state to a crystalline state under high-temperature diffusion annealing, turning a disadvantage into an advantage to achieve a better gettering effect. A method for forming a semiconductor substrate layer is provided, referring to FIG1 , and the method includes the following steps:

[0030] S1: providing an initial semiconductor substrate layer;

[0031] S2: forming a buffer semiconductor layer on at least one side of the initial semiconductor substrate layer, wherein the buffer semiconductor layer is amorphous; and the defect concentration within the buffer semiconductor layer is greater than the defect concentration within the initial semiconductor substrate layer;

[0032] S3: After forming the buffer semiconductor layer, performing a diffusion annealing process to form a doped layer in a portion of the buffer semiconductor layer during the process of the buffer semiconductor layer gradually transforming from an amorphous state to a crystalline state; during the diffusion annealing process, an oxide layer is also formed on a surface of the doped layer facing away from the buffer semiconductor layer;

[0033] S4: removing the oxide layer and the doping layer, and the initial semiconductor substrate layer and the remaining buffer semiconductor layer together form a semiconductor substrate layer.

[0034] In this embodiment, a buffer semiconductor layer is formed on at least one side of the surface of the initial semiconductor substrate layer. Since the buffer semiconductor layer is initially amorphous and is a semiconductor layer without regular crystal orientation, its own lattice distortion is very large, and the buffer semiconductor layer has a high defect density. In other words, the buffer semiconductor layer is initially arranged in a disordered manner, with a large number of dangling bonds and vacancy defects. The disordered arrangement energy state is higher, and the ordered arrangement energy state is lower. The defect concentration inside the buffer semiconductor layer is greater than the defect concentration inside the initial semiconductor substrate layer. In the method for forming the semiconductor substrate layer of the present application, under the high temperature state of diffusion annealing, specifically during the heating process, the disordered arrangement portion of the buffer semiconductor layer will gradually transform into a more stable ordered arrangement, so that the buffer semiconductor layer gradually transforms from an amorphous state to a crystalline state. This process will further generate a large number of defects, so that the defect concentration difference between the buffer semiconductor layer and the initial semiconductor substrate layer is increased from the existing 10 5-6 pieces / cm 3 Increased to 10 15-16 pieces / cm 3 (Compared to the existing technology, an increase of about 10 10times), due to the aggravation of the concentration difference, the diffusion driving force of the metal impurities is enhanced, driving the metal impurities in the initial semiconductor substrate layer to gradually diffuse into the buffer semiconductor layer, so that the metal impurity concentration in the initial semiconductor substrate layer is reduced from 6ppma-7ppma to 4ppma-5ppma, a decrease of 10%-20%, thereby achieving a better impurity gettering effect; secondly, during the diffusion annealing process, the metal impurities are enriched in the buffer semiconductor layer, so that a doped layer is formed in a portion of the thickness of the buffer semiconductor layer. The metal impurities further transfer and diffuse toward the side away from the initial semiconductor substrate layer, and also form an oxide layer on the surface of the doped layer away from the buffer semiconductor layer. Finally, the remaining buffer semiconductor layer, doped layer, and oxide layer are formed in sequence on the surface of the initial semiconductor substrate layer. After removing the oxide layer and the doped layer, the initial semiconductor substrate layer and the remaining buffer semiconductor layer together form a semiconductor substrate layer. In summary, the impurity gettering ability of the semiconductor substrate layer is improved.

[0035] Before forming a buffer semiconductor layer on at least one side surface of the initial semiconductor substrate layer, both sides of the initial semiconductor substrate layer have a damaged layer; the method for forming the semiconductor substrate layer also includes: before forming a buffer semiconductor layer on at least one side surface of the initial semiconductor substrate layer, performing a surface pre-cleaning treatment on the initial semiconductor substrate layer to remove the damaged layer.

[0036] The method for forming a semiconductor substrate layer further includes: after forming the semiconductor substrate layer, performing a texturing process on at least one side surface of the semiconductor substrate layer.

[0037] The method for forming the semiconductor substrate layer will be described in detail below with reference to FIG. 2 to FIG. 8 .

[0038] 2 , an initial semiconductor substrate layer 100 is provided.

[0039] The material of the initial semiconductor substrate layer 100 includes silicon. In other embodiments, the material of the initial semiconductor substrate layer is other semiconductor materials, such as single crystal silicon or silicon germanium. The material of the initial semiconductor substrate layer can also be other semiconductor materials.

[0040] In this embodiment, both sides of the initial semiconductor substrate layer 100 have damaged layers 110. In a specific embodiment, both the front and back sides of the initial semiconductor substrate layer 100 have damaged layers 110.

[0041] The damaged layer 110 is formed during the process of cutting a single crystal silicon raw material to form the initial semiconductor substrate layer 100. The damaged layer 110 always exists before a buffer semiconductor layer is formed on at least one side of the surface of the initial semiconductor substrate layer 100.

[0042] 3 , a surface pre-cleaning process is performed on the initial semiconductor substrate layer 100 .

[0043] The surface of the initial semiconductor substrate layer 100 is pre-cleaned to remove the damaged layer. Specifically, the surface pre-cleaning of the initial semiconductor substrate layer 100 can not only clean the front surface of the initial semiconductor substrate layer 100, but also clean the back surface of the initial semiconductor substrate layer 100.

[0044] The surface pre-cleaning treatment also includes removing organic matter and metal impurities on the surface of the initial semiconductor substrate layer 100 .

[0045] In one embodiment, the surface pre-cleaning treatment uses an alkali solution, which includes a KOH solution or a NaOH solution, and the mass percentage concentration of the alkali solution is 1%-5%, for example, 1%, 3% or 5%, and the temperature is 65°C-80°C, for example, 65°C, 70°C or 80°C, and the time of the surface pre-cleaning treatment is 60s-400s, for example, 60s, 200s or 400s.

[0046] The surface pre-cleaning process can remove the damaged layer and reduce the thickness of the initial semiconductor substrate layer 100 .

[0047] In one embodiment, the surface pre-cleaning treatment reduces the weight of the initial semiconductor substrate layer 100 by 2‰-4‰ of the initial semiconductor substrate layer 100, for example, 2‰, 3‰ or 4‰.

[0048] In other embodiments, the damaged layer may be removed by using a dry etching process.

[0049] 4 , a buffer semiconductor layer is formed on the surface of the initial semiconductor substrate layer 100 , and the buffer semiconductor layer is in an amorphous state.

[0050] After pre-cleaning the surface of the initial semiconductor substrate layer 100, a buffer semiconductor layer is formed on the surface of the initial semiconductor substrate layer 100. The buffer semiconductor layer includes a first buffer semiconductor layer 120 located on the front surface of the initial semiconductor substrate layer 100 and a second buffer semiconductor layer 130 located on the back surface of the initial semiconductor substrate layer 100. Specifically, the first buffer semiconductor layer 120 is in an amorphous state, and the second buffer semiconductor layer 130 is in an amorphous state.

[0051] In this embodiment, when the material of the initial semiconductor substrate layer 100 is silicon, the buffer semiconductor layer is an amorphous silicon layer. Specifically, the first buffer semiconductor layer 120 is a first amorphous silicon layer, and the second buffer semiconductor layer 130 is a second amorphous silicon layer.

[0052] During the process of forming the buffer semiconductor layer on the surface of the initial semiconductor substrate layer 100, a sub-doped layer (not shown in the figure) is formed in a portion of the thickness of the initial semiconductor substrate layer 100. Specifically, a first sub-doped layer (not shown in the figure) is formed between the initial semiconductor substrate layer 100 and the first buffer semiconductor layer 120, and a second sub-doped layer (not shown in the figure) is formed between the initial semiconductor substrate layer 100 and the second buffer semiconductor layer 130.

[0053] Because the buffer semiconductor layer lacks a regular crystal orientation and exhibits significant lattice distortion, the buffer semiconductor layer exhibits a high defect density. This results in a significant difference in defect concentration between the buffer semiconductor layer and the initial semiconductor substrate layer 100, causing metal impurities within the initial semiconductor substrate layer 100 to migrate into the buffer semiconductor layer. Specifically, the metal impurities within the initial semiconductor substrate layer 100 migrate into the first and second sub-doped layers, increasing the solubility of the metal impurities in the first and second sub-doped layers, thereby reducing the metal impurity content within the initial semiconductor substrate layer 100.

[0054] In one embodiment, the buffer semiconductor layer contains phosphorus ions. Specifically, the first buffer semiconductor layer 120 contains phosphorus atoms, and the second buffer semiconductor layer 130 contains phosphorus atoms. During the subsequent gettering process, the phosphorus atoms in the buffer semiconductor layer diffuse into the initial semiconductor substrate layer 100, increasing the doping concentration, enhancing the lattice distortion effect, and thereby improving the gettering effect on the initial semiconductor substrate layer 100.

[0055] The process for forming the buffer semiconductor layer includes a chemical vapor deposition process. Specifically, the process for forming the first buffer semiconductor layer 120 on the front surface of the initial semiconductor substrate layer 100 includes a chemical vapor deposition process, and the process for forming the second buffer semiconductor layer 130 on the back surface of the initial semiconductor substrate layer 100 includes a chemical vapor deposition process.

[0056] In one embodiment, the buffer semiconductor layer has a thickness of 10 nm to 50 nm, for example, 10 nm, 30 nm, or 50 nm. If the buffer semiconductor layer is too thick, it takes a long time to deposit the buffer semiconductor layer, increasing the production process time. If the buffer semiconductor layer is too thin, the ability of impurities within the initial semiconductor substrate layer 100 to migrate into the buffer semiconductor layer is insufficient.

[0057] 5 , a diffusion annealing process is performed on the initial semiconductor substrate layer 100 and the buffer semiconductor layer on the surface of the initial semiconductor substrate layer 100 .

[0058] After forming a buffer semiconductor layer on the surface of the initial semiconductor substrate layer 100, a diffusion annealing process is performed on the initial semiconductor substrate layer 100 and the buffer semiconductor layer on the surface of the initial semiconductor substrate layer 100 to form a doped layer in a portion of the thickness of the buffer semiconductor layer. The doped layer includes a first doped layer 140 located on a side of the first buffer semiconductor layer 120 facing away from the initial semiconductor substrate layer 100, and a second doped layer 150 located on a side of the second buffer semiconductor layer 130 facing away from the initial semiconductor substrate layer 100.

[0059] In this embodiment, during the diffusion annealing process, the buffer semiconductor layer gradually transforms from an amorphous state to a crystalline state. Specifically, the buffer semiconductor layer gradually crystallizes from the amorphous state, then transforms into a microcrystalline state, and then continues to heat up to transform into a crystalline state. The defect density of the buffer semiconductor layer, from low to high, is as follows: amorphous buffer semiconductor layer - microcrystalline buffer semiconductor layer - crystalline buffer semiconductor layer. In this step, when the buffer semiconductor layer is in the amorphous state, the defect concentration is high. At this time, when a phosphorus source is introduced, the phosphorus source diffuses more easily, and the concentration of phosphorus atoms in the amorphous buffer semiconductor layer is much higher than that in the initial semiconductor substrate layer. After the temperature is raised, the buffer semiconductor layer gradually crystallizes from the amorphous state to the microcrystalline state, and the defect concentration decreases. However, since a large number of doped phosphorus atoms have already entered the amorphous buffer semiconductor layer, the phosphorus atoms in the microcrystalline buffer semiconductor layer still introduce many defect sites, but the order of magnitude of the defects is much smaller than that in the amorphous buffer semiconductor layer. The buffer semiconductor layer is completely crystallized into a crystalline state: the phosphorus atom and defect density in the crystalline buffer semiconductor layer are slightly higher than those in the initial semiconductor substrate layer 100.

[0060] During the diffusion annealing treatment, the sub-doping layer is enriched in the buffer semiconductor layer so that a doping layer is formed in a partial thickness of the buffer semiconductor layer. Specifically, the first sub-doping layer is enriched in the first buffer semiconductor layer 120 so that a first doping layer 140 is formed in a partial thickness of the first buffer semiconductor layer 120, and the second sub-doping layer is enriched in the second buffer semiconductor layer 130 so that a second doping layer 150 is formed in a partial thickness of the second buffer semiconductor layer 130.

[0061] During the diffusion annealing process, an oxide layer is formed on the surface of the doped layer facing away from the buffer semiconductor layer. The oxide layer includes a first oxide layer 160 located on the side of the first doped layer 140 facing away from the first buffer semiconductor layer 120 and a second oxide layer 170 located on the side of the second doped layer 150 facing away from the second buffer semiconductor layer 130.

[0062] In this embodiment, the material of the oxide layer includes phosphosilicate glass (PSG). In other embodiments, the material of the oxide layer is other materials, such as silicon dioxide. The material of the oxide layer can also be other materials.

[0063] Through diffusion annealing treatment, the impurities inside the initial semiconductor substrate layer 100 are gradually diffused into the first buffer semiconductor layer 120 and the second buffer semiconductor layer 130. The impurities are enriched in the first buffer semiconductor layer 120 and the second buffer semiconductor layer 130, so that a first doping layer 140 is formed in a partial thickness of the first buffer semiconductor layer 120, and a second doping layer 150 is formed in a partial thickness of the second buffer semiconductor layer 130. The impurities are further transferred and diffused to the two sides away from the initial semiconductor substrate layer 100 to the first oxide layer 160 and the second oxide layer 170.

[0064] Furthermore, the solid solubility of the first oxide layer 160 for impurities in the initial semiconductor substrate layer 100 is greater than the solid solubility of the first doping layer 140 for impurities in the initial semiconductor substrate layer 100, and the solid solubility of the second oxide layer 170 for impurities in the initial semiconductor substrate layer 100 is greater than the solid solubility of the second doping layer 150 for impurities in the initial semiconductor substrate layer 100. In this way, during the diffusion annealing process, the first doping layer 140 enriched in the first buffer semiconductor layer 120 is further transferred and diffused to the first oxide layer 160, and the second doping layer 150 enriched in the second buffer semiconductor layer 130 is further transferred and diffused to the second oxide layer 170, so that the impurity content in the first doping layer 140 and the second doping layer 150 is reduced, and the impurity concentrations in the initial semiconductor substrate layer 100, the first doping layer 140 and the first oxide layer 160 form an increasing gradient, and the impurity concentrations in the initial semiconductor substrate layer 100, the second doping layer 150 and the second oxide layer 170 form an increasing gradient, so that the impurities in the initial semiconductor substrate layer 100 are better removed.

[0065] Solid solubility refers to the maximum content of solute in the solid solution, that is, the limiting solubility of impurities (solutes) in the solvent (the first oxide layer 160 , the second oxide layer 170 , the first doping layer 140 , or the second doping layer 150 ).

[0066] The conductivity type of the doped layer is the same as the conductivity type of the initial semiconductor substrate layer 100 before the diffusion annealing process. Optionally, before the diffusion annealing process, the conductivity type of the initial semiconductor substrate layer 100 is N-type, the conductivity type of the doped layer is N-type, and the doping element is phosphorus. Specifically, the conductivity type of the first doped layer 140 is the same as the conductivity type of the initial semiconductor substrate layer 100 before the diffusion annealing process; the conductivity type of the second doped layer 150 is the same as the conductivity type of the initial semiconductor substrate layer 100 before the diffusion annealing process. Optionally, the conductivity type of both the first doped layer 140 and the second doped layer 150 is N-type, and the doping element is phosphorus.

[0067] In this embodiment, the first buffer semiconductor layer 120 , the first doping layer 140 and the first oxide layer 160 all have a gettering function, and the second buffer semiconductor layer 130 , the second doping layer 150 and the second oxide layer 170 all have a gettering function.

[0068] In one embodiment, the diffusion annealing process is performed in a diffusion furnace, which includes a tubular diffusion furnace or a chain diffusion furnace.

[0069] In one embodiment, the gas source used in the diffusion annealing process is a phosphorus-containing gas source; the phosphorus-containing gas source includes POCl 3 .

[0070] In one embodiment, the doping layer contains phosphorus ions. Specifically, the first doping layer 140 contains phosphorus atoms, and the second doping layer 150 contains phosphorus atoms. Since the size of phosphorus atoms is different from that of silicon atoms, the phosphorus atoms in the doping layer exist in the form of solid solution, which will disrupt the original arrangement of silicon atoms, and the initial semiconductor substrate layer 100 will form a lattice distortion. The vacancy defect density in the doping layer increases, attracting impurity atoms in the initial semiconductor substrate layer 100 to move to the vacancies in the doping layer, filling the vacancy defects in the doping layer, thereby achieving an impurity absorption effect. The present application simultaneously diffuses phosphorus atoms at the beginning of the heating stage. Phosphorus atoms will occupy the vacancies in the buffer semiconductor layer. Compared with the prior art of diffusing phosphorus atoms into the initial semiconductor substrate layer 100, the present application diffuses phosphorus atoms into amorphous silicon for better results.

[0071] In one embodiment, the temperature of the diffusion annealing treatment is 700° C.-850° C., for example, 700° C., 800° C. or 850° C.; the time of the diffusion annealing treatment is 5 min-15 min, for example, 5 min, 10 min or 15 min.

[0072] In this embodiment, after the diffusion annealing process, the buffer semiconductor layer is converted into a crystalline semiconductor layer. Since the buffer semiconductor layer is converted into a crystalline semiconductor layer at a temperature above 200°C, and the temperature used in the diffusion annealing process is within the range of 700°C-850°C, the buffer semiconductor layer gradually converts into a crystalline semiconductor layer during the diffusion annealing process. During this conversion process, a large number of defects are generated, which increases the defect concentration difference between the buffer semiconductor layer and the initial semiconductor substrate layer, strengthens the diffusion dynamics of metal impurities, and thus improves the gettering effect.

[0073] 6 , the oxide layer is removed.

[0074] After the diffusion annealing process is performed, the oxide layer is removed. Specifically, after the diffusion annealing process is performed, the first oxide layer 160 and the second oxide layer 170 are removed.

[0075] In this embodiment, the process for removing the oxide layer includes a wet etching process. Specifically, the etching solution used is an acid solution, the acid solution includes an HF solution, and the HF concentration by mass is 5%-8%, for example, 5%, 7%, or 8%; the temperature is 15°C-30°C, for example, 15°C, 20°C, or 30°C; and the time for removing the oxide layer is 60 seconds-600 seconds, for example, 60 seconds, 200 seconds, or 500 seconds.

[0076] In other embodiments, the process of removing the oxide layer includes other etching processes.

[0077] 7 , the doping layer is removed.

[0078] After removing the oxide layer, the doping layer is removed. Specifically, after removing the oxide layer, the first doping layer 140 and the second doping layer 150 are removed.

[0079] In this embodiment, the process for removing the doped layer includes a wet etching process. Specifically, the etching solution used is an alkaline solution, including a KOH solution or a NaOH solution, with a mass percentage concentration of the alkaline solution of 2% to 5%, for example, 2%, 4%, or 4%; the temperature is 75°C to 85°C, for example, 75°C, 80°C, or 85°C; and the time for removing the doped layer is 30 seconds to 300 seconds, for example, 30 seconds, 200 seconds, or 300 seconds.

[0080] In other embodiments, the process of removing the doping layer includes other etching processes.

[0081] In this embodiment, after the doping layer is removed, the initial semiconductor substrate layer 100 and the crystalline semiconductor layer together form a semiconductor substrate layer 200 .

[0082] In other embodiments, after the diffusion annealing process is performed and before the oxide layer is removed, the initial semiconductor substrate layer and the crystalline semiconductor layer together form a semiconductor substrate layer. Alternatively, after the diffusion annealing process is performed and before the doping layer is removed, the initial semiconductor substrate layer and the crystalline semiconductor layer together form a semiconductor substrate layer.

[0083] In other embodiments, after removing the doping layer, the crystalline semiconductor layer is removed, and subsequently texturing is performed on the front and back sides of the initial semiconductor substrate layer.

[0084] 8 , texturing treatment is performed on the front and back surfaces of the semiconductor substrate layer.

[0085] After forming the semiconductor substrate layer 200, a texturing process is performed on the front and back sides of the semiconductor substrate layer 200, so that the front and back sides of the semiconductor substrate layer 200 have light-trapped texture surfaces 210. The semiconductor substrate layer 200 includes the initial semiconductor substrate layer 100 and a crystalline semiconductor layer converted from a buffer semiconductor layer.

[0086] In one embodiment, the texturing treatment uses an alkaline texturing solution, and the alkaline texturing solution includes a KOH solution or a NaOH solution. The mass percentage concentration of the alkaline texturing solution is 2%-5%, for example, 2%, 4% or 5%; the temperature is 75℃-85℃, for example, 75℃, 80℃ or 85℃; the time is 300s-700s, for example, 300s, 500s or 700s.

[0087] During the process of forming a semiconductor substrate layer using the above-mentioned method, a buffer semiconductor layer is first formed on at least one side of the initial semiconductor substrate layer 100. After the buffer semiconductor layer is formed, a diffusion annealing process is performed. Under the high temperature conditions of the diffusion annealing, a portion of the buffer semiconductor layer gradually transforms from an amorphous state to a crystalline state. Metal impurities in the initial semiconductor substrate layer 100 are enriched in the buffer semiconductor layer, forming a doped layer within a portion of the thickness of the buffer semiconductor layer. The metal impurities further migrate and diffuse toward the side away from the initial semiconductor substrate layer 100, achieving the purpose of gettering, and forming the semiconductor substrate layer 200. The concentration of metal impurities in the semiconductor substrate layer 200 directly affects the minority carrier lifetime, and changes in the minority carrier lifetime can indirectly reflect changes in the metal impurity concentration. Typically, the magnitude of metal impurities is very small, generally within 10 ppma. The lower the concentration of metal impurities, the longer the minority carrier lifetime. The existing minority carrier lifetime without impurity gettering treatment is: 1600μs-2000μs, and the minority carrier lifetime after conventional impurity gettering treatment is: 1800μs-2200μs. The method for forming the semiconductor substrate layer of the present application reduces the metal impurity concentration from 6ppma-7ppma to 4ppma-5ppma after impurity gettering treatment, and the minority carrier lifetime in the semiconductor substrate layer is increased from the existing 1600μs-2000μs to 2000μs-2400μs.

[0088] Example 2

[0089] The present application provides a method for preparing a heterojunction battery, which is based on a semiconductor substrate layer 200, and is prepared by sequentially forming an intrinsic semiconductor layer, a doped semiconductor layer, a transparent conductive film and a gate electrode on at least one side surface of the semiconductor substrate layer 200. The preparation of the semiconductor substrate layer adopts the method for the semiconductor substrate layer provided in the above embodiment.

[0090] Specifically, after the front and back sides of the semiconductor substrate layer are textured, a first intrinsic semiconductor layer is formed on the front side of the semiconductor substrate layer; a second intrinsic semiconductor layer is formed on the back side of the semiconductor substrate layer; a first doped semiconductor layer is formed on the side of the first intrinsic semiconductor layer facing away from the semiconductor substrate layer; and a second doped semiconductor layer is formed on the side of the second intrinsic semiconductor layer facing away from the semiconductor substrate layer.

[0091] The process of forming the first intrinsic semiconductor layer includes a vapor deposition process, and the process of forming the second intrinsic semiconductor layer includes a vapor deposition process.

[0092] The process of forming the first doped semiconductor layer includes a vapor deposition process, and the process of forming the second doped semiconductor layer includes a vapor deposition process.

[0093] In one embodiment, the first doped semiconductor layer includes a P-type amorphous silicon layer or a P-type microcrystalline silicon layer, and the second doped semiconductor layer includes an N-type amorphous silicon layer or an N-type microcrystalline silicon layer.

[0094] In one embodiment, the conductivity type of the second doped semiconductor layer is opposite to the conductivity type of the first doped semiconductor layer. In this embodiment, the conductivity type of the first doped semiconductor layer is P type and the conductivity type of the second doped semiconductor layer is N type.

[0095] In this embodiment, the present invention further includes: forming a first transparent conductive film (not specifically shown in the figure) on the side of the first doped semiconductor layer facing away from the semiconductor substrate layer; forming a second transparent conductive film (not specifically shown in the figure) on the side of the second doped semiconductor layer facing away from the semiconductor substrate layer; forming a first gate line electrode (not specifically shown in the figure) on the side of the first transparent conductive film facing away from the semiconductor substrate layer; and forming a second gate line electrode (not specifically shown in the figure) on the side of the second transparent conductive film facing away from the semiconductor substrate layer.

[0096] The heterojunction cell produced using the present invention's heterojunction cell preparation method preforms a buffer semiconductor layer on at least one side of the initial semiconductor substrate layer, followed by a diffusion annealing treatment. This improves the gettering capacity of the initial semiconductor substrate layer, further reducing impurity defects within the semiconductor substrate layer, and ultimately improving the conversion efficiency of the heterojunction cell. Testing has shown that impurity defects within the semiconductor substrate layer were reduced from 6-7 ppma to 4-5 ppma, and the conversion efficiency of the heterojunction cell increased from 25.21% to 25.27%.

[0097] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will readily appreciate that other variations or modifications based on the above descriptions are possible. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications arising therefrom remain within the scope of protection of the present invention.

Claims

1. A method for forming a semiconductor substrate layer, characterized in that: include: providing an initial semiconductor substrate layer; A buffer semiconductor layer is formed on at least one side of the initial semiconductor substrate layer, wherein the buffer semiconductor layer is amorphous; and the defect concentration inside the buffer semiconductor layer is greater than the defect concentration inside the initial semiconductor substrate layer; After forming the buffer semiconductor layer, a diffusion annealing treatment is performed to form a doped layer in a portion of the buffer semiconductor layer in the process of gradually transforming the buffer semiconductor layer from an amorphous state to a crystalline state; during the diffusion annealing treatment, an oxide layer is also formed on a surface of the doped layer facing away from the buffer semiconductor layer; The oxide layer and the doping layer are removed, and the initial semiconductor substrate layer and the remaining buffer semiconductor layer together form a semiconductor substrate layer.

2. The method for forming a semiconductor substrate layer according to claim 1, characterized in that: The buffer semiconductor layer contains phosphorus atoms. The process of forming the buffer semiconductor layer includes a chemical vapor deposition process. The thickness of the buffer semiconductor layer is 10nm-50nm.

3. The method for forming a semiconductor substrate layer according to claim 1, characterized in that: Before forming the buffer semiconductor layer on at least one side surface of the initial semiconductor substrate layer, both sides of the initial semiconductor substrate layer have a damaged layer; The method for forming the semiconductor substrate layer also includes: before forming a buffer semiconductor layer on at least one side of the surface of the initial semiconductor substrate layer, performing a surface pre-cleaning treatment on the initial semiconductor substrate layer to remove the damaged layer; wherein the surface pre-cleaning treatment uses an alkali solution, the alkali solution includes a KOH solution or a NaOH solution, the mass percentage concentration of the alkali solution is 1%-5%, the temperature is 65°C-80°C, and the time of the surface pre-cleaning treatment is 60s-400s.

4. The method for forming a semiconductor substrate layer according to claim 1, characterized in that: The process of removing the doped layer includes a wet etching process; wherein the etching solution used is an alkaline solution, the alkaline solution includes a KOH solution or a NaOH solution, the mass percentage concentration of the alkaline solution is 2%-5%, the temperature is 75°C-85°C, and the time for removing the doped layer is 30s-300s.

5. The method for forming a semiconductor substrate layer according to claim 1, characterized in that: The process of removing the oxide layer includes a wet etching process; wherein the etching solution used is an acid solution, the acid solution includes an HF solution, the mass percentage concentration of HF is 5%-8%, the temperature is 15°C-30°C, and the time for removing the oxide layer is 60s-600s.

6. The method for forming a semiconductor substrate layer according to claim 1, characterized in that: The buffer semiconductor layer includes a first buffer semiconductor layer located on the front side of the initial semiconductor substrate layer and a second buffer semiconductor layer located on the back side of the initial semiconductor substrate layer; The doping layer comprises a first doping layer located on a side of the first buffer semiconductor layer away from the initial semiconductor substrate layer and a second doping layer located on a side of the second buffer semiconductor layer away from the initial semiconductor substrate layer; The oxide layer includes a first oxide layer located on a side of the first doping layer away from the first buffer semiconductor layer and a second oxide layer located on a side of the second doping layer away from the second buffer semiconductor layer.

7. The method for forming a semiconductor substrate layer according to claim 1, characterized in that: The conductivity type of the doped layer is the same as the conductivity type of the initial semiconductor substrate layer before the diffusion annealing process; Before the diffusion annealing process is performed, the conductivity type of the initial semiconductor substrate layer is N-type, and the conductivity type of the doping layer is N-type.

8. The method for forming a semiconductor substrate layer according to claim 1, characterized in that: The gas source used in the diffusion annealing treatment is a phosphorus-containing gas source, and the phosphorus-containing gas source includes POCl3; the doping layer contains phosphorus atoms; The temperature of the diffusion annealing treatment is 700° C.-850° C.; the time of the diffusion annealing treatment is 5 min-15 min.

9. The method for forming a semiconductor substrate layer according to any one of claims 1 to 8, characterized in that: It also includes: after forming the semiconductor substrate layer, performing a texturing treatment on at least one side of the surface of the semiconductor substrate layer; wherein the texturing treatment uses an alkaline texturing solution, the alkaline texturing solution includes a KOH solution or a NaOH solution, the mass percentage concentration of the alkaline texturing solution is 2%-5%, the temperature is 75°C-85°C, and the time is 300s-700s.

10. A method for preparing a heterojunction battery, based on a semiconductor substrate layer, sequentially forming an intrinsic semiconductor layer, a doped semiconductor layer, a transparent conductive film and a gate electrode on at least one side of the semiconductor substrate layer, characterized in that: The semiconductor substrate layer is prepared by using the method for forming a semiconductor substrate layer according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Novel PERC battery and manufacturing method thereof

    CN111710756A

  • Preparation method of heterojunction battery

    CN113675300A

  • Preparation method of ingot casting single crystal or polycrystalline silicon heterojunction solar cell

    CN114388638A

  • Formation method of semiconductor substrate layer and preparation method of heterojunction cell

    CN116525717A

  • Double-sided heterojunction solar cell based on thin epitaxial silicon

    US20110068367A1