Phase-change microcapsule and preparation method therefor, and high-safety lithium battery and preparation method therefor
By introducing high-hardness phase change microcapsules into lithium batteries and improving the positive electrode structure, the thermal runaway problem of lithium-ion batteries under high temperature and pressure is solved, the battery's high safety and stability are achieved, and the battery life is extended.
Patent Information
- Application Number
- PCT/CN2024/088499
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-04-18
- Publication Date
- 2024-11-14
AI Technical Summary
Existing lithium-ion batteries are prone to thermal runaway under high temperature and pressure, resulting in safety accidents. The rupture temperature of existing phase-change microcapsules is low and cannot be kept in a closed state during normal manufacturing and use, resulting in insufficient battery safety.
Using phase-change microcapsules with high capsule wall envelope hardness and crushing resistance, by improving the positive electrode structure and preparation process of lithium battery, phase-change microcapsules are added to the coating material to keep them solid below 110°C. Crack when the set critical temperature or pressure is reached, releasing liquid insulating organic matter and preventing electrochemical reactions.
It effectively solves the problem of thermal runaway control and normal manufacturing process of lithium-ion batteries, improves the safety and stability of lithium batteries, meets the safety requirements of lithium cobalt oxide and ternary lithium batteries, and does not affect the battery performance. Extend battery life under the circumstances.
Smart Images

Figure CN2024088499_14112024_PF_FP_ABST
Abstract
Description
Phase-change microcapsule, high-safety lithium battery and preparation method thereof Technical Field
[0001] The present application relates to the technical field of lithium battery manufacturing, and in particular to a phase change microcapsule, a high-safety lithium battery and a preparation method thereof. Background Art
[0002] Currently, various high-energy-density lithium-ion batteries, such as lithium cobalt oxide (LiCoO2, LCO), ternary lithium-ion batteries such as nickel cobalt manganese oxide (Li(NiCoMnz)O2, NCM), and nickel cobalt aluminum oxide (Li(NiCoAlZ)O2, NCA), have found widespread application in consumer applications, transportation sectors such as new energy vehicles, and new energy fields such as energy storage and base stations. However, issues such as thermal runaway, lithium dendrites, and consistency have long been major limitations on the widespread use of lithium-ion batteries and electric vehicles, and have become a hot topic and focus for the electric vehicle industry and battery companies.
[0003] Lithium-ion batteries, especially lithium cobalt oxide (LCO) and ternary lithium-ion batteries, are highly sensitive to temperature. When temperatures rise excessively high, they are prone to thermal runaway, leading to safety accidents. Thermal runaway in lithium-ion batteries is a major fire hazard in electric vehicles. Thermal runaway, or uncontrollable heat, occurs when a lithium-ion battery's temperature rises rapidly due to various factors. As the rate of temperature rise increases, the battery temperature rises rapidly and becomes uncontrollable. Thermal runaway is one of the most serious failure modes of lithium-ion batteries and poses a significant threat to their safety. The entire reaction process in lithium-ion batteries is exothermic. Thermal runaway occurs when the rate of heat dissipation within the battery is significantly lower than the rate of heat generation. The point at which the heat dissipation rate and heat generation within a lithium-ion battery balance is called the critical point. At this point, heat generation equals heat dissipation. Above this point, heat generation significantly exceeds heat dissipation, leading to thermal runaway. The temperature corresponding to this critical point is also known as the thermal runaway trigger temperature.
[0004] There are many causes of thermal runaway in lithium-ion batteries, which can generally be divided into three categories: mechanical triggering, electrical triggering, and thermal triggering; they can also be divided into internal battery factors and external factors. Specifically, improper use, physical damage, accidental damage, and inherent defects in lithium-ion batteries can all trigger thermal runaway, leading to accidents such as fire, explosion, and fire. While any one or a combination of these factors can trigger thermal runaway, in most cases, thermal runaway in lithium-ion batteries is the result of a combination of internal defects and external factors, with the internal defects often being the more dominant cause.
[0005] Existing research shows that the critical safety temperature (also known as the thermal runaway trigger temperature) of conventional lithium cobalt oxide batteries and ternary lithium batteries is relatively low, generally 160-200°C, with slight differences due to battery materials and structures; 160°C is the critical safety temperature for thermal runaway of most lithium batteries. When the temperature is higher than 160°C, the lithium battery will have a high probability of thermal runaway; at the same time, the higher the internal temperature of the battery, the earlier the thermal runaway will occur; side reactions are one of the direct causes of thermal runaway of lithium-ion batteries, and negative electrode reactions, positive electrode reactions and electrolyte decomposition have a greater impact on thermal runaway; the better the heat dissipation conditions and the higher the material stability, the less likely the battery will experience thermal runaway.
[0006] To address the thermal stability and safety issues of lithium batteries, the document with Chinese invention application number 201811607566.5 discloses a method for preparing phase-change microcapsules for improving the safety of lithium batteries. The conductive polymer monomers coated in the prepared phase-change microcapsules have a rupture temperature of 59-72°C. When the lithium battery is short-circuited, overcharged, or heated, the "skin" of the phase-change microcapsules is easily broken, thereby improving safety. However, the shell rupture temperature of the phase change microcapsule is low, and its compressive strength and hardness are low. During the normal manufacturing process of the battery, it will encounter temperatures higher than 72°C many times (usually the drying temperature of the current collector coating and the electrode is about 100°C) and higher pressures (pressure during the coating process, pressure during electrode winding and compaction). It will inevitably rupture and fail prematurely, resulting in the inability to add it to the coating material or positive and negative electrode materials to manufacture semi-finished or finished lithium batteries; when the lithium battery is fast charged, fast discharged or used in a high temperature environment in summer, its temperature is also likely to reach or exceed 59°C. At this time, the phase change microcapsule ruptures, causing the entire lithium battery to be scrapped, which will inevitably lead to unnecessary losses. Therefore, the technical means of improving battery safety form an insurmountable technical contradiction between the normal preparation and use of lithium batteries.
[0007] Therefore, the above-mentioned patented technical solutions and existing technical solutions are difficult to simultaneously solve the technical contradictions arising from meeting the safety requirements of products such as lithium cobalt oxide and ternary lithium batteries and normal manufacturing processes and normal use during the manufacturing and use of the positive electrode.
[0008] Summary of the Invention
[0009] In order to solve the above-mentioned thermal safety problems of lithium-ion batteries in the prior art, the purpose of this application is to provide a phase change microcapsule, a high-safety lithium battery and a preparation method thereof, introduce a phase change microcapsule with sufficiently high capsule wall hardness and crushing strength (rupture pressure difference), and simultaneously improve the positive electrode structure, materials and preparation process of the lithium battery to improve the mechanical strength, adhesion, thermal stability, surface smoothness of the positive electrode sheet, reduce the internal resistance of the battery, and uniformize its overall thickness. The phase change microcapsule is added to the coating material or the electrode material so that the phase change microcapsule has greater surface hardness and strength during the normal manufacturing and use of the battery, and can withstand high temperatures below 110°C and higher external pressures, so that it can be used in the entire preparation process of the lithium battery. It never softens and maintains a sealed solid shape. Only when the internal temperature of the lithium battery reaches or exceeds the set critical safety temperature (such as 110°C) and continues, so that the volume expansion rate of the capsule core material is greater than 3%, or when the pressure difference between the inside and the outside reaches the rupture pressure difference (that is, the internal and external safety critical pressure difference), the capsule wall membrane will rupture and quickly release the liquid insulating organic matter after the phase change, cutting off the internal electrochemical reaction, and promptly stopping the chain-like accelerated electrochemical reaction inside the battery, controlling the internal temperature and volume of the battery in a safe state. It can quickly, reliably and effectively solve the problem of thermal runaway control and normal manufacturing process being difficult to take into account, and can simultaneously solve the technical contradiction between ensuring the safety requirements of products such as ternary lithium batteries and normal manufacturing and normal use.
[0010] In order to solve the above technical problems, this application provides the following technical solutions:
[0011] A phase-change microcapsule, characterized in that it is a spherical microcapsule with an average particle size of 2-3 μm, comprising a capsule wall membrane and a spherical capsule core completely covered by the capsule wall membrane;
[0012] The capsule core is a phase change material, which is a phase change insulating organic matter with a phase change temperature of 55-70°C, or a mixture of multiple insulating organic matters;
[0013] The capsule wall is a conductive and thermally conductive film formed by a mixture of an organic film-forming resin and a conductive modifier, and has an average thickness of 0.5-1.50 μm;
[0014] The capsule wall membrane, when the temperature of the environment system in which it is located is not higher than the set safety critical temperature, and the pressure difference between the inside and outside of the environment system is not greater than the set safety critical pressure difference (i.e., the rupture pressure difference), maintains the phase change microcapsule shape intact and airtight, and encapsulates the phase change insulating organic matter inside the capsule wall membrane;
[0015] The capsule wall coating obtains a suitable coating hardness and crushing strength tolerance range by adjusting its coating forming components, thickness and hardness, so that when the temperature of the environmental system in which it is located reaches or exceeds the set safety critical temperature, or the pressure difference between the inside and outside of the environmental system reaches or exceeds one of the set safety critical pressure differences, the capsule wall coating ruptures, destroying the integrity and closed form of the phase change microcapsule, and quickly releases the liquid phase change insulating organic matter coated inside the capsule wall coating into the environmental system and diffuses it, quickly increasing the resistance of the environmental system material in which it is located and blocking the continuation of the electrochemical reaction in the environmental system.
[0016] The phase change material forming the capsule core is one of paraffin and polyethylene glycol with a phase change temperature of 55-70°C, or a composite phase change material with a phase change temperature of 55-70°C obtained by mixing paraffin wax with different numbers of carbon atoms with fatty acids and / or fatty alcohols, or a composite phase change material with a phase change temperature of 55-70°C obtained by mixing polyethylene glycols with different molecular weights. The volume expansion rate is ≥3% when the temperature rises to 110°C.
[0017] The conductive modifier forming the capsule wall coating is one of conductive graphite with a particle size D50 of 0.5-2 μm, nickel-plated glass microbeads, or a mixture thereof;
[0018] The organic film-forming resin forming the capsule wall coating is melamine formaldehyde, polystyrene resin or a mixture thereof;
[0019] The mass ratio of the organic film-forming resin to the conductive modifier in the film-forming mixture is 10:(1-20);
[0020] The conductive modifier forming the capsule wall increases in the proportion of the film-forming mixture and the increase in particle size, and reaches the capsule wall.
[0021] The conditions of capsule rupture were negatively correlated;
[0022] The increase in the proportion of the organic film-forming resin in the film-forming mixture and the increase in vitrification are positively correlated with the conditions for achieving rupture of the capsule wall.
[0023] Furthermore, the glass transition temperature of the capsule wall membrane is not lower than 150° C., that is, at a temperature of 150° C. or above, the capsule wall membrane changes from a glassy state to a highly elastic state.
[0024] The set safety critical temperature is 110-150° C., and the set internal and external safety critical pressure difference (rupture pressure difference) is not less than 2.5 MPa.
[0025] The method for preparing the phase change microcapsules is characterized by comprising the following steps:
[0026] (111) preparing or weighing an organic film-forming resin and a conductive modifier according to the materials, proportions, and particle sizes of the capsule wall coating corresponding to the set safety critical temperature and safety critical pressure difference, and mixing them uniformly to obtain a film-forming mixture for forming the capsule wall coating;
[0027] (112) preparing or weighing insulating organic solid particles with a phase transition temperature of 55-70° C. as the capsule core according to the phase change material and its ratio corresponding to the set phase transition temperature and the volume expansion rate at the safety critical temperature;
[0028] (113) The film-forming mixture is uniformly coated on the outer surface of insulating organic solid particles by using one of the spraying process, dipping process, in-situ polymerization process or interfacial polymerization process, and then dried. Particles with a particle size of D50 = 2-3 μm are screened at room temperature to obtain phase change microcapsules.
[0029] A high-safety lithium battery, characterized in that it includes a composite positive electrode current collector, and a safety coating and a positive electrode active layer are provided on at least one side of the surface of the composite positive electrode current collector, which are stacked and bonded in sequence; the safety coating, the positive electrode current collector, and the positive electrode active layer are mutually bonded and compacted to form a composite positive electrode with a stacked structure; wherein the safety coating is an elastic layer with a dense structure made by tightly combining a set proportion of safety particles, the phase change microcapsules according to any one of claims 1 to 4, a conductive agent, and a binder.
[0030] A method for preparing the high-safety lithium battery is characterized in that the composite positive electrode is prepared by the following steps:
[0031] (1) preparing a positive electrode current collector, a safety slurry for a safety coating, and an active slurry for a positive electrode active layer respectively;
[0032] (2) applying the safety slurry of the safety coating to one side of the current collector by a comma blade, spin coating, doctor blading, gravure or micro-gravure printing, and drying at a temperature below 110° C. so that the phase change microcapsules always remain in a solid and sealed state, thereby preparing a positive electrode current collector provided with a safety coating; the thickness of the safety coating on one side after drying is 1.5-5 μm;
[0033] (3) In an environment with an ambient humidity of less than 30%, the active slurry of the positive electrode active layer is applied to the outer surface of the safety coating by a comma scraper method, a roller transfer method, or a slit extrusion method, and then dried and compacted to obtain a positive electrode active layer; after drying and compacting at a temperature below 110°C, the overall thickness of the electrode sheet is 60-110 μm, so that the phase change microcapsule always remains in a solid and sealed state, thereby obtaining a lithium battery composite positive electrode.
[0034] Compared with the prior art, this application has at least the following advantages:
[0035] (1) The high-safety lithium battery, composite positive electrode and preparation method provided by the present application, by introducing phase change microcapsules with sufficiently high capsule wall coating hardness and crushing strength, and then simultaneously improving the lithium battery positive electrode structure, materials and preparation process, the mechanical strength, adhesion, thermal stability, surface smoothness of the positive electrode sheet are improved, the internal resistance of the battery is reduced, and the overall thickness is uniform. The phase change microcapsules are added to the coating material or the electrode material, so that the phase change microcapsules have a large surface hardness and fracture strength tolerance range during the normal manufacturing and use of the battery, and can withstand high temperatures below 110°C and high internal and external pressure differences, so that they do not soften throughout the entire preparation process of the lithium battery (the capsule wall coating can maintain a high hardness below 110°C and have a glass transition temperature above 110°C) and remain sealed The solid shape can meet the processing conditions of various production processes; when the lithium battery has abnormal working conditions, the internal temperature reaches or exceeds 110°C and continues to cause the volume expansion of the phase change material, or the pressure difference between the inside and outside of the capsule wall membrane reaches the rupture pressure difference (the internal and external safety critical pressure difference, not less than 2.5MPa) due to external force, the capsule wall membrane will rupture and quickly release the liquid insulating organic matter after phase change, cutting off the internal electrochemical reaction, and promptly stopping the chain-like accelerated electrochemical reaction inside the battery, and controlling the internal temperature and volume of the battery in a safe state. It can quickly, reliably and effectively solve the problem of thermal runaway control and normal manufacturing process being difficult to balance, and can simultaneously solve the technical contradiction between ensuring the safety requirements of products such as lithium cobalt oxide and ternary lithium batteries and normal manufacturing and normal use.
[0036] (2) The high-safety lithium battery and composite positive electrode provided by the present application have a softening temperature higher than the normal manufacturing and use temperature (within 100°C) and slightly lower than the critical safety temperature of thermal runaway by introducing phase change microcapsules. At the same time, the capsule wall coating has a relatively high hardness, so that the phase change microcapsules can withstand temperature changes and pressure changes in a large range outside during normal manufacturing and use without premature rupture and failure. At the same time, the capsule wall coating material below the glass transition temperature (softening temperature) will be relatively brittle, and the tensile strength will be much smaller than its compressive strength. Therefore, the pressure from the volume expansion of the internal phase change material will reach or exceed the internal and external safety critical pressure difference, resulting in rupture of the capsule wall coating. Only when encountering situations such as internal short circuit, the internal temperature rises sharply, and reaches the set safety temperature (such as 110°C) or above, the internal core material undergoes rapid phase change, volume expansion, and the volume change rate reaches 3% or above, the capsule wall membrane will burst from the inside of the microcapsule, and will not break or release insulating organic matter before reaching the set temperature (such as 110°C) or the internal and external safety critical pressure difference; the phase change microcapsules of the present application have sufficient hardness at room temperature and can meet various external pressures in the manufacturing process (such as the pressure when the electrode is compacted); in the event of unexpected physical and mechanical pressure (such as acupuncture, extrusion ), the cystic membrane will only rupture when it reaches or exceeds the maximum internal and external safety critical pressure difference that the cystic membrane can withstand, that is, only when the external force acting on the battery system reaches the set operating conditions, the external pressure borne by the cystic membrane reaches the maximum pressure limit of the cystic membrane and exceeds the internal and external safety critical pressure difference, that is, exceeds the rupture pressure difference, including when the lithium battery pack is partially subjected to a strong physical collision such as a car accident, the cystic membrane will be fractured under the action of pure external mechanical force, causing the cystic membrane to rupture and release insulating organic matter, blocking the internal electrochemical reaction, thereby quickly, reliably and effectively preventing the lithium battery from thermal runaway.
[0037] (3) The present application provides a phase-change microcapsule in a safety coating, which adopts a core-shell structure. The conductive modifiers of different particle sizes and proportions incorporated into the coating material layer of the capsule wall can cooperate with the organic resin material to enable the coating of the phase-change microcapsule to obtain the required surface hardness, rupture strength, glass transition temperature range and conductive and thermal conductivity, and make it higher than the temperature and pressure in the normal manufacturing and working process, so it does not affect the normal manufacturing and working process of the battery; the capsule wall coating of the phase-change microcapsule is composed of an organic resin and a conductive modifier. Through the combination of its components, ratios, conductive modifier particle size, organic resin glass transition temperature and other properties, comprehensive selection is made to jointly adjust the film thickness, conductive and thermal conductivity and elasticity, heat resistance, and glass transition temperature of the capsule wall coating. Temperature, tolerance to rupture pressure difference and other properties; by making appropriate trade-offs and adjusting the balance between the above-mentioned properties and the rupture conditions and rupture timing of the capsule wall membrane, different surface hardness, rupture strength and glass transition temperature ranges can be obtained, that is, capsule wall membranes with different rupture conditions and rupture timings can be obtained; through the above-mentioned adjustments, the present application can make the capsule wall membrane maintain its shape integrity and airtightness when the set safety temperature or pressure difference is not reached, and quickly rupture when the rupture conditions and rupture timing are reached. On the one hand, the phase change microcapsules can meet the requirements of the entire manufacturing process and the entire use process of lithium batteries, and on the other hand, the phase change microcapsules can prevent and control thermal runaway, thus achieving the unification of two contradictory needs. This application introduces phase change microcapsules to simultaneously improve the structure, materials and preparation process of the lithium battery composite positive electrode. Through the coordinated cooperation of multiple aspects, it solves the problems of thermal runaway and battery performance degradation caused by various reasons in the current lithium battery. On the basis of improving the safety and stability of lithium-ion batteries, it comprehensively guarantees the key needs of battery safety, normal manufacturing, use and capacity density.
[0038] (4) The phase change microcapsules and high-safety lithium batteries provided in the present application are prepared by selecting different mixing ratios of organic film-forming resins and conductive modifiers, and / or simultaneously selecting different particle sizes of conductive modifiers, and then mixing them evenly to obtain film-forming mixtures of various proportions, forming capsule wall coatings of different thicknesses, strengths and glass transition temperatures to match the pre-set safety critical temperature and safety critical pressure difference, so that the phase change temperature and phase change volume expansion rate of the capsule core material, as well as the tolerable external and internal pressure difference, do not soften or passively break during various processes and charge and discharge operations when the temperature, volume expansion rate or internal and external rupture pressure difference of the internal material of the capsule wall coating are not reached; and when the set safety critical temperature or safety critical pressure difference is reached, the internal phase change material of the capsule wall coating has a phase change volume expansion rate exceeding the set value, or when the mechanical action it is subjected to reaches the set internal and external rupture pressure difference, the capsule wall coating actively or passively breaks, quickly releasing liquid phase change insulating organic matter, and preventing the electrochemical reaction of the system material.
[0039] (5) The phase change insulating material in the core of the phase change microcapsule of the present application is solid at room temperature. A single-component phase change material or a composite phase change material formed by multiple components can be used to obtain different phase change temperatures and volume expansion rates, and further obtain the technical effect that the phase change material can reach a set safety critical pressure difference and trigger the rupture of the capsule wall membrane after reaching the set safety critical temperature and volume expansion; under the normal working state of the lithium battery, the phase change material can provide the necessary internal physical support (forming a solid spherical structure) for the capsule wall membrane with strong hardness, so that the capsule wall membrane can continue to maintain its hardness and not collapse inward when subjected to a large external pressure (about 2MPa or less) under normal conditions or during the manufacturing process such as coating and drying. Collapse, maintaining the integrity and airtightness of the overall spherical structure; before reaching the set critical safety temperature, the phase change insulating material in the capsule core is heated and reaches the phase change temperature, gradually changing from solid to liquid and rapidly expanding in volume. Afterwards, as the temperature and internal pressure rise rapidly, the phase change insulating material will quickly melt, change phase, expand rapidly in volume, and even partially vaporize, thereby rapidly increasing the internal pressure and quickly reaching the set critical safety pressure difference, causing the capsule wall membrane to crack and break (or due to external physical effects, the lithium battery is locally fractured when the critical safety pressure difference of the capsule wall membrane reaches 2.5MPa). At this time, the integrity and airtightness of the capsule wall membrane structure are destroyed, and the phase change material quickly flows out or overflows.
[0040] (6) The phase-change microcapsules of the present application can use a variety of resin materials as capsule wall coatings, a variety of conductive solid particle materials as conductive modifiers, and a variety of phase-change organic insulating materials as capsule core materials to produce volume expansion when the phase-change temperature is reached. Since the capsule wall coatings formed by various thicknesses, components, and proportions have different compressive strengths, and the phase-change temperatures and volume expansion coefficients of the various capsule core materials are different, the present application can obtain the capsule wall coating with the required compressive strength and rupture timing by comprehensively balancing and choosing the positive and negative correlations of various factors on the rupture of the coating. For example, by changing the mass ratio of liquid organic resin and solid conductive modifier particles and the particle size of the conductive modifier in the film-forming mixture prepared therefrom, the thickness and compressive strength of the capsule wall membrane formed after film formation can be adjusted to be compatible with the phase change volume expansion coefficient of the internal capsule core material; when the phase change temperature is reached, the total volume expansion of the capsule core material must be greater than 3%, and the internal pressure induced by it is large enough to burst the capsule wall membrane from the inside out; and when the phase change temperature is not reached, the total volume expansion of the phase change material is less than 3%, and the internal pressure induced by its expanded volume is not enough to burst the capsule wall membrane and cannot destroy the membrane, so that the capsule wall membrane maintains a complete spherical and closed structure, avoiding deformation, rupture, and failure of the phase change microcapsules during the coating, drying, compaction, winding and other manufacturing processes, thereby causing the lithium battery to fail as a whole.
[0041] (7) The present application can control the thickness of the safety coating within 0.5-5 μm by rationally controlling the components, formula, shape, structure and size of the safety coating, so as not to reduce the overall energy density of the lithium battery. The safety coating has strong bonding strength, good heat resistance and good lubrication, ensuring that the positive electrode aluminum foil will not directly contact the negative electrode or the needle to cause a short circuit during the needling process and at the high temperature of the needling in the battery. The composite positive electrode provided by the present application is a sandwich structure formed by the outer current collector, the middle safety coating and the inner active material layer. The safety coating has the functions of bonding, lubrication, filling the small defects of the bonding interface on both sides and leveling the thickness. During the long-term cycle process, the middle safety coating can also effectively inhibit the generation and growth of lithium dendrites on the negative electrode side, avoiding the internal short circuit of the battery and battery performance degradation caused by it.
[0042] (8) The high-safety lithium battery and composite positive electrode provided by the present application match the pressure resistance of the phase change microcapsules in the safety coating with the pressure in the compaction step. On the basis of ensuring the normal manufacturing process, the flatness and flexibility of the positive electrode material can be improved, the distance of the lithium ion charge and discharge channels (i.e., the distance between the positive electrode collector and the negative electrode collector) can be balanced, lithium ion nucleation can be avoided, and the generation and growth of lithium dendrites on the negative electrode side can be avoided or inhibited. At the same time, the phase change microcapsules can enhance the strength and flexibility of the positive electrode sheet and the aluminum foil through the elastic deformation of their capsule wall coating, inhibit lithium dendrites that pierce the SEI film from reaching the aluminum foil, and avoid the material shedding and aluminum foil exposure caused by lithium dendrites piercing the positive electrode active material layer, thereby reducing the probability of thermal failure. Therefore, the safety coating provided in this application starts from the positive electrode side and introduces phase change microcapsules with specific structure, strength, composition and passive strain to improve the performance of the positive and negative electrode sides and inhibit the generation and growth of lithium dendrites. By improving the structure, materials and processes of the positive electrode side, the performance of the negative electrode side is improved simultaneously, providing a new idea for solving the balance between the overall manufacturing, consistency and safety of lithium batteries.
[0043] (9) The safety coating in the composite positive electrode provided by this application has a low energy density of safety particles, and its main function is to stabilize and cooperate with the phase change microcapsules, binders, conductive agents and other materials of the safety coating to achieve multiple technical effects such as porosity, elasticity, lubrication, and compensation. The thickness of the safety coating after drying is only 0.5μm, which will not affect the overall energy density of the lithium battery cell. The binder content ratio in the safety coating material is 3-9 times that of the binder in the positive electrode active material, which significantly improves its bonding strength, flexibility and interface flatness. The safety coating has obvious advantages in terms of electrode bonding strength, lubricity, AC impedance, square resistance, rate performance, cycle life, etc., and can increase battery power and extend the life of lithium batteries.
[0044] (10) The safety coating in the composite positive electrode provided by the present application uses safety particles selected from lithium iron phosphate or its modified materials, silicate or its derivative material series, alumina ceramic or its derivative materials. These materials have good thermal stability, which is reflected in the fact that the chemical bond strength in phosphate, silicate and aluminate is much stronger than that of traditional transition metal oxide structures. The strong PO covalent bond in phosphate, Si-O covalent bond in silicate and Al-O metal bond in aluminate stabilize oxygen atoms in the fully charged state. Even at high temperatures or overcharge, they will not collapse and generate heat like lithium cobalt oxide or form strong oxidizing substances, thus preventing them from being oxidized to produce oxygen and release it. Moreover, the decomposition temperature of the material itself is high, all greater than 700°C, and it will not decompose, release gas or catch fire, so it is safer at high temperatures. The safety coating of the present application uses a small amount of safety particles such as lithium iron phosphate, silicate and alumina to cooperate with the positive electrode active material, which can not only solve the safety risks of lithium cobalt oxide and lithium manganese oxide, but also will not cause a significant reduction in battery energy density.
[0045] (11) The safety coating provided in the present application improves the overall flexibility and mechanical strength of the composite positive electrode through its porous structure, strong adhesion, lubrication and elastic deformation of phase change microcapsules, so as to prevent the positive electrode active material from falling off during the manufacturing and use of the composite positive electrode. At the same time, it prevents the positive electrode active material from falling off when it encounters external puncture, physical damage, or internal lithium dendrites piercing the diaphragm, positive electrode active layer or positive electrode current collector.
[0046] (12) The safety coating in the composite positive electrode provided by the present application uses a binder selected from one or more of polyacrylic acid (PAA) or its salts, modified acrylic acid, modified polyacrylonitrile (PAN), and sodium alginate in an aqueous medium, all of which are water-based resin materials with good thermal stability. During a needle puncture test simulating an internal short circuit in a lithium-ion battery, due to the protection of the coating, no material protrudes or falls off, so the heat generated is small and can be diffused in a timely manner, and the heat release caused by the internal short circuit in the battery is not obvious. At this time, the decomposition temperature of the composite positive electrode material used is above 300°C, and strong thermal runaway, side reactions, and thermal runaway diffusion will not occur, thereby improving the overall safety of the battery.
[0047] (13) The safety coating or slurry preparation method for the composite positive electrode provided in this application uses aqueous binders and water as the active slurry medium. The slurry preparation process is simple, highly controllable, low in cost, and more environmentally friendly. The prepared safety coating has high mechanical strength and conductive efficiency. While increasing the specific surface area of the electrochemically active material, it ensures the overall integrity of the metal foil electrode material during battery cycling and ensures good electrical contact between the electrode material and the current collector during cycling.
[0048] (14) The preparation method of the composite positive electrode provided in the present application adopts a double-layer coating for the safety coating and the positive electrode active layer, and places the safety coating with good bonding and lubrication properties between the positive electrode collector (aluminum foil) with poor lubrication properties and the positive electrode active material, so that the electrode formed by this stacked structure has good flexibility and is not prone to breakage during the battery preparation process, thereby improving the battery yield and at the same time helping to control production costs and improve production efficiency.
[0049] (15) The lithium battery prepared by using the composite positive electrode of the present application can also moderately increase the critical safety temperature (thermal runaway trigger temperature) of the battery to 200°C or above by setting a high thermal stability safety coating, a laminated structure and a passively strained phase change microcapsule, which is much higher than the thermal runaway trigger temperature of 150°C-160°C of conventional lithium cobalt oxide and ternary lithium batteries; at the same time, it has obvious advantages in terms of electrode bonding strength, AC impedance, square resistance, rate performance, cycle life, etc. Compared with the battery prepared by the light foil current collector, the AC internal resistance is reduced by more than 20%, and the energy density is not reduced. It is an ideal current collector material for high-power, long-life lithium-ion batteries; at the same time, the composite positive electrode helps the battery as a whole to solve problems such as thermal runaway, lithium dendrites, consistency and performance degradation, which is of great significance to improving the overall performance of the battery, improving the battery thermal management and ensuring the safety of passengers.
[0050] (16) After actual test verification, the lithium battery provided by this application can successfully pass thermal safety tests such as needle puncture, mechanical extrusion, overcharge and over-discharge, and high-temperature heating. The release of insulating organic matter and the process of preventing electrochemical reactions are rapid and reliable. The overall performance of the battery, such as energy density and consistency, is superior to the existing technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] FIG1 is a schematic diagram of the transverse cross-sectional structure of a high-safety composite positive electrode for a lithium battery according to an embodiment of the present invention;
[0052] FIG2 is a schematic diagram of the overall cross-sectional structure of a high-safety lithium battery according to an embodiment of the application.
[0053] In the figure: 1. Positive electrode current collector; 2. Safety coating; 3. Positive electrode active layer; 4. Shell; 5. Separator; 6. Negative electrode current collector; 7. Negative electrode active layer; 8. Phase change microcapsule. DETAILED DESCRIPTION
[0054] The present application is further elaborated below in conjunction with the accompanying drawings and embodiments.
[0055] Example
[0056] 1-2 , the phase-change microcapsules provided in the embodiments of the present application are spherical microcapsules with an average particle size of 2-3 μm, comprising a capsule wall membrane and a spherical capsule core completely covered by the capsule wall membrane;
[0057] The capsule core is a phase change material, which is a phase change insulating organic material with a phase change temperature of 55-70°C, or a mixture of multiple insulating organic materials; the capsule wall is a conductive and thermally conductive coating (i.e., a capsule wall coating) formed by a mixture of an organic film-forming resin and a conductive modifier, and has an average thickness of 0.5-1.50 μm;
[0058] The capsule wall membrane, when the temperature of the environment system in which it is located is not higher than the set safety critical temperature and the pressure difference between the inside and outside of the environment system in which it is located is not greater than the set safety critical pressure difference, maintains the shape of the phase change microcapsule intact and airtight, and encapsulates the phase change insulating organic matter inside the capsule wall membrane;
[0059] When the temperature of the environmental system in which the capsule wall membrane is located reaches or exceeds the set safety critical temperature, or the pressure difference between the inside and outside of the environmental system reaches or exceeds the set safety critical pressure difference (such as 2.5MPa), the capsule wall membrane ruptures, destroying the integrity and closed shape of the phase change microcapsule, and quickly releases the liquid phase change insulating organic matter coated inside the capsule wall membrane into the environmental system and diffuses it, rapidly increasing the resistance of the environmental system material and blocking the continuation of the electrochemical reaction in the environmental system.
[0060] The phase change material forming the capsule core is one of paraffin and polyethylene glycol, or a composite phase change material of paraffin with different numbers of carbon atoms and fatty acids and / or fatty alcohols, or a composite phase change material of polyethylene glycol with different molecular weights, and its volume expansion rate when the temperature rises to 110°C is ≥3%.
[0061] The phase-change material forming the capsule core can be paraffin wax (corresponding to grades 56-70) with a phase transition temperature of 55-70°C and 26-30 carbon atoms, or polyethylene glycol (corresponding to grades 6000-20000) with an average molecular weight of 6000-18500. Alternatively, the phase-change material can be a composite phase-change material comprising a mixture of paraffin waxes with varying carbon numbers and fatty acids and / or fatty alcohols, with a phase transition temperature of 55-70°C, or a composite phase-change material comprising a mixture of polyethylene glycols with varying molecular weights, with a phase transition temperature of 55-70°C. The volume expansion rate at a temperature of 110°C is ≥3%. The specific component monomers or mixtures of the phase-change material can be selected according to conventional techniques.
[0062] In each embodiment of the present application, the core of the phase-change microcapsule is an insulating organic material with a phase-change temperature of 55-70°C. Specifically, a single component or a mixture of multiple components can be selected. The phase-change microcapsules provided in this application can also be used in the manufacture of other products requiring phase change and temperature control.
[0063] It is known from the known technology that the phase transition temperature of a single component of paraffin wax refers to the temperature required for paraffin wax to transform from solid to liquid or from liquid to solid. This phase transition temperature is related to factors such as the chain length, molecular weight and crystal form of the paraffin wax. Generally, the phase transition temperature of paraffin wax varies between 50-80°C, depending on its specific composition. Based on the melting point of the paraffin wax, etc., the paraffin wax with a molecular weight corresponding to the above-mentioned core phase transition temperature of 55-70°C is selected. Specifically, the following can be selected: paraffin wax with 26, 28, 30 carbon atoms, or brand 56 # -70 # One of the solid paraffins, 60 # When refining paraffin oil, the phase transition temperature of the capsule core is 59-61℃.
[0064] As is known in the art, polyethylene glycol (PEG) is a water-soluble polymer compound. Due to different degrees of polymerization, it forms a series of polymers with average relative molecular masses ranging from 200-20,000. The physical form changes from a white viscous liquid to a hard, waxy solid as the molecular weight increases. Because different brands of polyethylene glycol are polymers of PEG with a certain molecular weight range, they melt (phase transition) within a certain temperature range. As the degree of polymerization increases, the phase transition temperature of a series of polyethylene glycols (PEG) with different molecular weights increases successively, and the phase transition temperature corresponding to different molecular weight PEGs ranges from 3.2°C to 70°C. Among them, the phase transition temperature of polyethylene glycol with grade 500 (PEG-500) is 20-25°C, the phase transition temperature of polyethylene glycol with grade 6000 (PEG-6000) is 55-59°C, the phase transition temperature of polyethylene glycol with grade 10000 (PEG-6000) is 59-63°C, and the phase transition temperature of polyethylene glycol with grade 20000 (PEG-20000) is 60-64°C.
[0065] In this embodiment, conventional techniques can be used to mix PEGs of different molecular weights (500-20,000) in appropriate proportions to obtain a PEG composite phase change material having a phase transition temperature of 55-70°C and a volume expansion rate of ≥3% when heated to 110°C. Specifically, conventional techniques can be used to obtain polyethylene glycols of different degrees of polymerization or mixtures thereof as phase change materials at different phase transition temperatures.
[0066] According to known technology, the phase transition temperature of stearic acid (SA) is 51°C. Therefore, when selecting a single component, the phase transition temperature of paraffin with a suitable carbon atomic weight is 55-65°C, the phase transition temperature of polyethylene glycol with a suitable molecular weight range is 55-70°C, and the phase transition temperature of suitable palmitic acid is 60-65°C.
[0067] In each embodiment of the present application, paraffin, fatty acids, and fatty alcohols in different proportions can be used as main raw materials, and paraffin-based composite phase change materials can also be obtained (for example, 10-90wt% paraffin, 10-90wt% fatty acids and / or fatty alcohols;), stearic acid-based composite phase change materials, and palmitic acid-based composite phase change materials, all of which have good thermal stability and thermal conductivity, and are suitable as temperature-controlled phase change materials with a set temperature range phase change and a volume expansion rate of ≥3% when the temperature rises to 110°C.
[0068] The fatty acid is a saturated fatty acid, and the fatty alcohol has 8 to 22 carbon atoms.
[0069] The fatty acid includes one or more of palmitic acid, stearic acid, lauric acid, caprylic acid, capric acid, and myristic acid; the fatty alcohol includes one or more of dodecyl alcohol, tetradecyl alcohol, hexadecanol, and octadecanol.
[0070] If a mixture of two or three of the aforementioned phase change materials is selected, a variety of insulating organic materials can be obtained, each having a phase transition temperature of 55-70°C and a volume expansion rate greater than 3% at 110°C. Persons skilled in the art can determine the composition and ratio of the phase change insulating organic material based on the overall lithium battery preparation process and within the scope described in this application. Alternatively, other organic insulating materials with a phase transition temperature of 55-70°C and a volume expansion rate greater than 3% at 110°C can be selected. Each phase change material is solid before reaching its phase transition temperature and transforms into a liquid upon reaching the phase transition temperature and absorbing heat.
[0071] The conductive modifier forming the capsule wall coating is conductive graphite with a particle size of D50 = 0.5-2 μm, nickel-plated glass beads, or a mixture thereof, and the product prepared by conventional technology can be directly used;
[0072] The organic film-forming resin forming the capsule wall coating is melamine formaldehyde, polystyrene resin or a mixture thereof;
[0073] The mass ratio of the organic film-forming resin to the conductive modifier in the film-forming mixture is 10:(1-20);
[0074] The proportion of the conductive modifier forming the capsule wall in the film-forming mixture increases, and the particle size of the conductive modifier increases.
[0075] It is positively correlated with the conditions for achieving rupture of the capsule wall, that is, if either the proportion or the particle size increases, the thickness of the capsule wall decreases, the compressive strength decreases, the rupture conditions decrease, and the rupture timing is advanced;
[0076] The increase in the proportion of the organic film-forming resin in the film-forming mixture that forms the capsule wall coating, the increase in solid content, the increase in film thickness and the decrease in the particle size of the conductive modifier are all negatively correlated with the conditions for achieving capsule wall coating rupture, that is: if the proportion of the organic film-forming resin in the film-forming mixture increases, the solid content increases, the film thickness increases and the particle size of the conductive modifier decreases, any of these conditions can lead to an increase in the thickness of the capsule wall coating, an increase in the compressive strength, improved rupture conditions and a delay in the timing of rupture.
[0077] In this embodiment, the glass transition temperature of the capsule wall membrane is related to the proportion of the organic film-forming resin that forms the capsule wall membrane, the glass transition temperature of the resin material itself after curing, and the film thickness. Among them, as the proportion of the organic film-forming resin decreases, the glass transition temperature of the resin material itself after film formation and curing decreases, and the film thickness decreases, which is positively correlated with the overall rupture conditions and rupture timing of the capsule wall membrane; conversely, as the proportion of the organic film-forming resin increases, the glass transition temperature of the resin material itself after film formation and curing increases, and the film thickness increases, which is negatively correlated with the overall rupture conditions and rupture timing of the capsule wall membrane.
[0078] Those skilled in the art can, by making appropriate choices among the above-mentioned different correlations, select suitable resin materials, proportions of conductive modifiers and film thicknesses, and obtain the capsule wall coating with the required specific rupture conditions and rupture timing; by combining the phase change temperature and volume expansion rate of the selected phase change material, the required phase change microcapsules that rupture or do not rupture under specific temperature or internal and external pressure difference conditions can be obtained, and the appropriate rupture timing can be obtained.
[0079] Furthermore, the glass transition temperature of the capsule wall membrane is not lower than 150° C., that is, at a temperature of 150° C. or above, the capsule wall membrane changes from a glassy state to a highly elastic state.
[0080] The set safety critical temperature is 110-150° C., and the set internal and external safety critical pressure difference is not less than 2.5 MPa.
[0081] The preparation method of the aforementioned phase change microcapsules comprises the following steps:
[0082] (111) preparing or weighing an organic film-forming resin and a conductive modifier according to the materials, proportions, and particle sizes of the capsule wall coating corresponding to the set safety critical temperature and safety critical pressure difference, and mixing them uniformly to obtain a film-forming mixture for forming the capsule wall coating;
[0083] (112) preparing or weighing insulating organic solid particles with a phase transition temperature of 55-70° C. as the capsule core according to the phase change material and its ratio corresponding to the set phase transition temperature and the volume expansion rate at the safety critical temperature;
[0084] (113) The film-forming mixture is uniformly coated on the outer surface of insulating organic solid particles by using one of the spraying process, dipping process, in-situ polymerization process or interfacial polymerization process, and then dried. Particles with a particle size of D50 = 2-3 μm are screened at room temperature to obtain phase change microcapsules.
[0085] A high-safety lithium battery comprises a composite positive electrode current collector, on at least one side of which a safety coating and a positive electrode active layer are sequentially laminated and bonded together; the safety coating, the positive electrode current collector, and the positive electrode active layer are mutually bonded and compacted to form a composite positive electrode with a laminated structure; the safety coating is an elastic layer with a dense structure made by tightly combining safety particles in a set proportion, the aforementioned phase change microcapsules, a conductive agent, and a binder.
[0086] A method for preparing the high-safety lithium battery, wherein the composite positive electrode is prepared by the following steps:
[0087] (1) preparing a positive electrode current collector, a safety slurry for a safety coating, and an active slurry for a positive electrode active layer respectively;
[0088] (2) applying the safety slurry of the safety coating to one side of the current collector by a comma blade, spin coating, doctor blading, gravure or micro-gravure printing, and drying at a temperature below 110° C. so that the phase change microcapsules always remain in a solid and sealed state, thereby preparing a positive electrode current collector provided with a safety coating; the thickness of the safety coating on one side after drying is 1.5-5 μm;
[0089] (3) In an environment with an ambient humidity of less than 30%, the active slurry of the positive electrode active layer is applied to the outer surface of the safety coating by a comma scraper method, a roller transfer method, or a slit extrusion method, and then dried and compacted to obtain a positive electrode active layer; after drying and compacting at a temperature below 110°C, the overall thickness of the electrode sheet after single-side coating is 60-110 μm, so that the phase change microcapsule always remains in a solid and sealed state, thereby obtaining a lithium battery composite positive electrode.
[0090] The phase change microcapsules and high-safety lithium batteries provided in the present application are prepared by selecting different mixing ratios of organic film-forming resins and conductive modifiers, and / or simultaneously selecting different particle sizes of conductive modifiers, and then mixing them evenly to obtain a variety of film-forming mixtures with different proportions, which can form capsule wall membranes with different thicknesses, surface hardness, rupture strength and glass transition temperatures to match the pre-set safety critical temperature and safety critical pressure difference, thereby obtaining suitable rupture conditions and rupture timing. Specifically, by controlling the composition, thickness, hardness, toughness and glass transition temperature of the capsule wall coating after the film-forming mixture is solidified and formed, it can be matched with the phase change temperature and phase change volume expansion rate of the capsule core material, as well as the tolerable external and internal pressure difference; so that when the phase change microcapsule does not reach the volume expansion rate of the internal material of the capsule wall coating or the internal and external rupture pressure difference, it will not passively break during various processes and charge and discharge operations, and the capsule wall coating will not soften when it does not reach the glass transition temperature and maintain a strong surface hardness; and when the phase change microcapsule reaches the set safety critical temperature or reaches one of the safety critical pressure differences, the capsule wall coating will actively break under the action of the internal pressure generated by the internal phase change material exceeding the set phase change volume expansion rate; in addition, when the mechanical action on the phase change microcapsule reaches the set internal and external rupture pressure difference, the capsule wall coating will also passively break without reaching the set safety critical temperature, quickly releasing liquid phase change insulating organic matter to prevent the electrochemical reaction of the system material.
[0091] The following is a more specific embodiment to illustrate the specific technical solution of this application.
[0092] Example 1
[0093] Please refer to Figures 1 and 2. The phase change microcapsule 8 provided in this embodiment is a spherical microcapsule, comprising a capsule wall membrane and a spherical capsule core completely covered by the capsule wall membrane. The temperature at which the capsule wall membrane breaks (safety critical temperature) is not less than 110°C. The phase change material forming the capsule core is fully refined paraffin wax (corresponding to brand 56 # -70 # ), which are all insulating organic substances with a phase transition temperature of 55-70°C; the capsule wall coating is a conductive and thermally conductive coating formed by a mixture of an organic film-forming resin and a conductive modifier, with a glass transition temperature (i.e., softening temperature) of not less than 150°C, a rupture temperature of not less than 110°C, specifically 160°C, and an internal and external safety critical pressure difference (i.e., coating rupture pressure difference) of not less than 2.5MPa.
[0094] Specifically, the particle size of the phase change microcapsules described in this embodiment is in the range of D50 = 2-2.2 μm; the average thickness of the capsule wall membrane is in the range of 1.2-1.50 μm; the internal and external safety critical pressure difference (i.e., the capsule rupture pressure difference) ΔP ≥ 2.5 MPa, and ΔP can be specifically selected between 2.5-12.5 MPa as needed.
[0095] The conductive modifier forming the capsule wall coating is conductive graphite with a particle size of D50 = 0.5-2 μm; in this embodiment, the conductive graphite particle size D50 = 0.5 μm is selected; the organic film-forming resin forming the capsule wall coating is melamine formaldehyde; the mass ratio of the film-forming mixture of the organic film-forming resin and the conductive modifier forming the capsule wall coating is 10:1; under this ratio, the capsule wall coating has the largest thickness, the highest glass transition temperature (160°C), the largest withstand rupture pressure difference, the capsule wall coating rupture conditions are higher, and the rupture timing is relatively delayed, so that phase change microcapsules with higher tolerance to processing conditions can be obtained.
[0096] It is known from the known technology that the thermal expansion coefficient α of paraffin depends on factors such as its molecular structure, quality and processing technology. However, during the phase change process, the volume change of paraffin will increase sharply. The volume expansion rate of the fully refined paraffin in this embodiment can be higher than 13% when it is heated to 110°C. This volume expansion rate can generate a pressure greater than 9 MPa inside the capsule wall membrane. Moreover, as the temperature continues to rise, the volume expansion rate and internal pressure both rise rapidly, and an internal pressure far greater than 9 MPa can be quickly generated. At this time, the internal pressure of the lithium battery (i.e., the external pressure of the phase change microcapsule) is no more than 1 MPa. Therefore, the phase change material can quickly generate an internal and external safety critical pressure difference greater than 2.5 MPa (i.e., the capsule wall membrane rupture pressure difference) at 110°C, bursting the capsule wall membrane from the inside, causing the liquid paraffin to quickly flow out and diffuse, increasing the internal resistance of the lithium battery, and blocking the electrochemical reaction.
[0097] In other embodiments, the phase change material forming the capsule core may also be selected from 56 # -70 # A mixture of different grades of fully refined paraffin wax is used to obtain more targeted, different phase change temperatures and volume expansion rates to control the rupture conditions (appropriately reduce) and the rupture timing (appropriately advance) of the capsule wall membrane.
[0098] In this embodiment, the phase-change microcapsules, when the ambient temperature is lower than the safety critical temperature of 160°C (below the glass transition temperature of 150°C), the capsule wall membrane remains solid as a whole and has an intact and sealed appearance; when the external temperature (the temperature of the ambient system) reaches or exceeds 160°C, the phase-change material paraffin serving as the capsule core is liquefied by heat and its volume expansion rate rapidly exceeds 3%, causing the internal pressure of the capsule wall membrane to accumulate rapidly and the difference in the internal and external safety critical pressures to rapidly reach greater than 2.5MPa, bursting the membrane from the inside and causing the liquid paraffin to rapidly flow out and diffuse; while the capsule wall membrane is still below the glass transition temperature at this time and does not soften, it has a high compressive strength and a low tensile strength, and when the phase-change material bursts and breaks the capsule wall membrane from the inside, causing it to break, multiple fragments and cracks will be generated, enabling the liquid insulating organic paraffin liquid to rapidly flow out and diffuse.
[0099] The preparation method of the aforementioned phase change microcapsules comprises the following steps:
[0100] (111) According to the aforementioned ratio, the organic film-forming resin melamine formaldehyde and the conductive modifier conductive graphite are weighed and mixed uniformly to prepare a film-forming mixture for forming the capsule wall membrane; by selecting different mixing ratios of the organic film-forming resin and the conductive modifier (10:1 in this embodiment), and / or simultaneously selecting different particle sizes of the conductive modifier, then
[0101] The mixtures are mixed evenly to obtain film-forming mixtures of various proportions, and capsule wall membranes of different thicknesses and strengths are formed, which can match the phase change temperature and phase change volume expansion ratio of the capsule core material in step (112), as well as the external pressure, so that when the internal volume expansion rate or the external rupture pressure difference is reached, the capsule wall membrane does not soften but directly breaks;
[0102] (112) preparing or weighing insulating organic solid particles with a phase transition temperature of 55-70° C. as capsule cores according to a certain ratio;
[0103] (113) The film-forming mixture is uniformly coated on the outer surface of insulating organic solid particles by a spray coating process, a dip coating process, an in-situ polymerization process, or an interfacial polymerization process, and then dried. Particles with a particle size D50 of 2.7-3 μm are screened to obtain phase change microcapsules.
[0104] The high-safety lithium battery composite positive electrode provided in this embodiment is a composite positive electrode of a ternary lithium battery, specifically, a positive electrode of a ternary NCM622 system, comprising a positive electrode collector 1 (a smooth aluminum foil with a thickness of 13 μm), and a safety coating 2 and a positive electrode active layer 3 which are sequentially laminated and bonded on both sides of the positive electrode collector 1; the safety coating 2, the positive electrode collector 1, and the positive electrode active layer 3 are mutually bonded and compacted to form a composite positive electrode with a laminated structure; wherein the safety coating 2 is an elastic layer having a porous structure, strong bonding, lubrication, and density made by tightly combining safety particles, phase change microcapsules 8, a conductive agent, and a binder in a set proportion; the phase change microcapsules comprise a capsule wall membrane and a spherical capsule core which is completely covered by the capsule wall membrane, the capsule wall membrane rupture temperature is not less than 160°C, the capsule core is a phase change material, which is an insulating organic matter with a phase change temperature in the range of 55-70°C and a volume expansion rate greater than 3% when the temperature reaches 160°C; the The safety particles and phase change microcapsules 8 of the safety coating 2 cooperate with the porous structure, binder, and conductive agent to passively strain based on the set temperature or pressure while improving the bonding strength between the layers of the composite positive electrode and reducing the surface resistance. During the entire preparation process of the lithium battery (including the coating, drying, and compaction of the current collector slurry, the coating, drying, and compaction of the positive active slurry, and the winding and packaging with the negative current collector, etc.), the phase change microcapsules do not soften (the processing temperature is lower than 150°C) and maintain a sealed solid shape due to their spherical structure and the hardness of the capsule wall membrane. When the internal temperature of the lithium battery reaches or exceeds 160°C and continues, the capsule core material undergoes a phase change, the volume expands, the capsule wall membrane ruptures, and the liquid insulating organic matter after the phase change is quickly released, which rapidly increases the internal resistance of the battery and eventually cuts off the internal electrochemical reaction, thereby controlling the internal temperature and volume of the battery in a safe state and avoiding adverse consequences such as thermal runaway (explosion).
[0105] Specifically, in this embodiment, the organic film-forming resin forming the capsule wall coating is melamine formaldehyde resin, and the steps for preparing the capsule wall coating are as follows: evenly mix a solution of formaldehyde and melamine with a molar ratio of 2.5:1, adjust the pH to about 8.5, and stir the mixture at 400 rpm at 70°C for 90 minutes to obtain a melamine-formaldehyde prepolymer; mix conductive graphite (modified conductive agent) with a D50 of 0.5 μm with the prepolymer solution, and the ratio of the mass of the conductive graphite to the mass of the prepolymer solid dry matter is 1:10, and disperse at 2000 rpm for 30 minutes to obtain an organic film-forming resin solution mixed with a modifier; slowly add the solution to the pre-dispersed solid paraffin powder (fully refined paraffin, corresponding to the brand 56#-7) while stirring. 0#), the mass of the core material emulsion (paraffin emulsion): the mass of the capsule wall coating material solution (organic film-forming resin solution) = 1:2.4-2.8, (the organic film-forming resin solution can be in the ratio range of 2.4-2.8), an aqueous formaldehyde solution is added to make the formaldehyde: melamine = 2.8:1 (volume ratio), the temperature is raised to 55°C, kept warm for 1 hour, and further raised to 85°C and kept warm for 3.5 hours, that is, the phase change microcapsules are synthesized by an in situ polymerization process; after cooling to room temperature, a small amount of hydrogen peroxide is added to the reaction system to remove residual formaldehyde, the mixture is filtered, rinsed with deionized water and anhydrous ethanol three times, and vacuum dried to obtain solid particles of the phase change microcapsules, and the particles with D50 = 2 μm are screened.
[0106] The method for preparing an aqueous emulsion of paraffin wax powder is as follows: solid paraffin wax powder is added to deionized water at a predetermined ratio. The temperature is then raised to above the melting point of the paraffin wax (e.g., 60°C, depending on the brand of the wax). This temperature is maintained while an appropriate amount of surfactant is added. High-speed dispersion and emulsification are performed for 10-30 minutes. The solution is then allowed to cool naturally to room temperature to obtain an aqueous emulsion of paraffin wax powder. An in-situ resin synthesis process is then employed to directly coat the emulsion phase change material with an organic film-forming resin solution. After the resin material solidifies and forms, the phase change microcapsules are obtained.
[0107] The phase change microcapsules synthesized by this method have a capsule wall coating obtained by curing a mixture of thermosetting melamine formaldehyde resin and conductive graphite. By controlling the composition of the resin, the mass ratio of the resin solid dry weight to the conductive graphite to 10:1, and the average particle size of the conductive graphite (D50 = 0.5 μm), the capsule wall coating can have sufficient temperature control ability and pressure resistance (in other embodiments, when the ratio of conductive graphite added to the resin is adjusted and increased successively between 10: (1-20), the compressive strength of the formed capsule wall coating is not greatly affected, but the degree of resistance to the rupture strength during the volume expansion of the capsule core decreases successively with the increase of the conductive graphite ratio); therefore, by appropriately adjusting By adjusting the mass ratio of the core and wall coating materials and synchronously adjusting the average particle size of the conductive graphite, the thickness of the coating can be controlled between 1.3-1.5 μm, and the coating can be triggered to rupture under the condition of an internal and external pressure difference ΔP (minimum safety critical pressure difference) of not less than 2.5 MPa, and a suitable rupture timing can be obtained; at the same time, in this embodiment, any value within the range of ΔP = 2.5-12.5 MPa or above can cause the coating to rupture; since the temperature and pressure of the battery system materials change very quickly before the critical point of thermal runaway and it is a continuous process, it is impossible to accurately measure the pressure difference value at the actual point of triggering the rupture of the coating, and only the occurrence range of the pressure difference can be known. The core phase change material used in this embodiment can liquefy at 56-70°C. When the microcapsule's external environment is heated to 160°C, the core temperature drops slightly below the external environment due to factors such as heat transfer efficiency. However, the core material's volume expansion rate at 160°C is approximately 13%, and this volume expansion rate increases rapidly with rising temperature. Therefore, at 160°C, the core material can achieve a volume expansion rate significantly greater than 3%, sufficient to induce internal pressure. This expansion ruptures the interface between the resin and the conductive graphite in the capsule wall, causing the entire phase change microcapsule to rupture, releasing the insulating organic material in the core into the battery's internal system and automatically terminating the chemical reaction. However, below 160°C, the internal pressure induced by the volume expansion rate cannot rupture the capsule wall, allowing the microcapsule to maintain its shape.
[0108] In this embodiment, the conductive modifier is conductive graphite with a particle size of D50 = 0.5 μm. The mass ratio of the mixture of the organic film-forming resin and the conductive modifier that form the capsule wall coating is 10:1. The conductive graphite has multiple functions of conductivity, thermal conductivity and affecting the thickness and strength of the film. The organic film-forming resin and the conductive modifier cooperate with each other to obtain a closed membrane surface with the required thickness, thermal conductivity, thermal conductivity and softening temperature, and resistance to rupture pressure difference as the capsule wall coating, and make the surface of the coating hard at room temperature, have large compressive strength and certain elasticity, so as to protect the internal capsule core to maintain its shape integrity and airtightness during the entire battery processing (coating, drying, compacting, winding), and before the set safety critical temperature is reached, the volume expansion rate of the internal phase change material after the phase change is also small, and the internal pressure caused by it is absorbed by the elasticity (toughness) of the coating and cannot burst the capsule wall coating, which can avoid the short-term internal temperature increase of the lithium battery due to other reasons (such as during drying operation) causing the coating to rupture; if the internal temperature of the lithium battery no longer continues to rise at this time, the capsule wall coating continues to remain intact, intact in shape, and airtight. As the internal temperature drops to below the phase change temperature of the capsule core, the capsule core returns to a solid state, and the phase change microgel The capsule automatically returns to its original state without damaging the overall performance of the lithium battery; if the temperature continues to rise after reaching the safety critical temperature, the insulating organic material will completely melt and phase change, and the local organic material will gasify under the rapidly increasing high temperature and high pressure outside, thus rapidly generating a large volume expansion, far greater than 3%, and the internal pressure generated is greater than the absorption capacity of the capsule, thereby bursting the capsule wall from the inside; in addition, under the action of external physical extrusion, when the microcapsule reaches the set internal and external pressure difference of the capsule wall (≥2.5MPa, 3MPa can usually be selected as the benchmark value), the physical effect of the mechanical pressure can cause the capsule to deform significantly, exceed its maximum tolerable rupture strength, and fracture the capsule from the outside, causing the liquid or gaseous insulating organic matter to overflow rapidly, rapidly increase the internal resistance, block the internal electrochemical reaction, and prevent further heat generation and volume increase inside the battery, thereby avoiding catastrophic consequences of thermal runaway such as explosion.
[0109] In other specific embodiments of the present application, resin materials of other different components can be used as film-forming materials to prepare capsule wall coatings, or conductive solid granular materials of other different components can be used as conductive modifiers. And correspondingly, phase-change organic insulating materials of other different components can be used as capsule core materials; since the mechanical strength of the capsule wall coatings formed by various material components, proportions, particle sizes, etc. is different, the phase change temperature and volume expansion coefficient of capsule core materials of different components are also different. Therefore, those skilled in the art can, according to the description of this application, adjust the specific components and mass ratio of the liquid organic resin and the solid conductive modifier particles in the film-forming mixture prepared by the two, and / or adjust the particle size of the conductive modifier at the same time, and reasonably use the interaction of positive correlation and negative correlation to adjust the capsule wall coating formed after film formation. The thickness, hardness, glass transition temperature and fracture resistance strength, etc. can adapt to the volume expansion rate caused by the different temperatures of the core material inside it, so that when the total volume expansion rate of the core material is greater than 3%, the internal pressure caused by the expanded volume is sufficient to quickly burst the envelope (capsule wall envelope) from the inside to the outside; and when the total volume expansion rate is less than 3%, the expansion pressure can be absorbed by the envelope and cannot destroy the envelope, so that the capsule wall envelope maintains a complete spherical and closed structure, avoiding deformation, rupture and failure of the phase change microcapsules during the coating, drying, winding and other manufacturing processes, and then causing the overall failure of the lithium battery.
[0110] In this embodiment, the capsule wall coating of the microcapsule is formed by a mixture of melamine formaldehyde resin with a softening (glass transition) temperature greater than 160°C and a conductive modifier (conductive graphite); when the external temperature of the coating is lower than 160°C, its surface is hard, its compressive strength is high, and it can withstand a large internal and external pressure difference. By matching the softening temperature with the withstand rupture strength, the phase change microcapsules can adapt to changes in temperature and pressure (including single changes or simultaneous changes) over a wide range during the entire preparation process and normal use. Before reaching the set safety critical temperature or critical rupture strength, they can remain solid as a whole and their appearance is intact, sealed, and not ruptured, thereby preventing premature failure of the lithium battery.
[0111] In this embodiment, a safety slurry for the safety coating is prepared, wherein the weight ratio of each substance can be specifically selected within the range of safety particles: phase change microcapsules: conductive agent: binder = (50-90): (5-20): (0.5-10): (4.5-20). Specifically, the ratio adopted in this embodiment is safety particles: phase change microcapsules: conductive agent: binder = 75:10:5:10.
[0112] The safety particulate matter is a lithium metal phosphate salt or a modified material thereof, including one or more of lithium iron phosphate or a modified material thereof, lithium iron manganese phosphate or a modified material thereof, and lithium vanadium phosphate or a modified material thereof; wherein the lithium iron phosphate has a particle size D50 of 0.2-2.0 μm. Specifically, the safety particulate matter in this embodiment is lithium iron phosphate, with a particle size D50 of 1.2 μm.
[0113] The conductive agent is one or more of conductive carbon black, acetylene black, conductive graphite, carbon nanotubes, or graphene. The binder is a water-based polymer or its salt with a decomposition temperature greater than 300°C, including one or more of polyacrylic acid (PAA) or its salt, modified acrylic acid, modified polyacrylonitrile (PAN), and sodium alginate. Specifically, in this embodiment, the conductive agent is conductive carbon black and conductive graphite in a 1:1 weight ratio; the binder is modified acrylic acid and sodium alginate in an 8:1 mixing ratio.
[0114] The positive electrode current collector is a metal aluminum foil or aluminum mesh with a thickness of 8-20μm; the safety coating has a thickness of 0.5-5μm after drying, and the thickness of the positive electrode active layer after drying is 59-115μm; the total thickness of the electrode sheet after the safety coating and the positive electrode active layer are compacted and dried is 60-120μm. Specifically, in this embodiment, the positive electrode current collector is a smooth metal aluminum foil with a thickness of 13μm; the safety coating has a thickness of 3μm after drying, and the thickness of the positive electrode active layer after drying is 80μm; the total thickness of the safety coating and the positive electrode active layer applied on one side after compaction and drying is 83μm, and the thickness of the electrode sheet after drying after the single-sided coating is 96μm. Of course, these parameters can also be selected according to specific needs.
[0115] Referring to Figure 2, the high-safety ternary lithium battery using the aforementioned composite positive electrode provided in this embodiment includes a shell 4, a diaphragm 5, a negative electrode current collector 6, an electrolyte and the high-safety lithium battery composite positive electrode. A plurality of phase change microcapsules 8 are evenly distributed in the safety coating 2 of the high-safety lithium battery composite positive electrode; on the two side surfaces of the positive electrode current collector of the composite positive electrode, a safety coating 2 and a positive electrode active layer 3 are symmetrically stacked and bonded in sequence, and a plurality of phase change microcapsules 8 are evenly distributed in each full coating 2, which can release insulating organic matter when the set safety temperature (such as 160°C) or the maximum pressure value (internal and external rupture pressure difference ≥2.5MPa) inside the lithium battery is reached, forming two independent insulating layers, blocking the internal electrochemical reaction of the lithium battery from both sides, thereby improving reliability and reaction speed.
[0116] A method for preparing the aforementioned high-safety lithium battery, wherein the composite positive electrode is prepared by the following steps:
[0117] (1) Prepare the positive electrode current collector 1 (smooth aluminum foil with a thickness of 13 μm), the safety slurry of the safety coating 2, and the active slurry of the positive electrode active layer 3 respectively;
[0118] (2) The safety slurry of the safety coating 2 is applied to one side surface of the current collector by one of the methods of comma scraper, spin coating, doctor blade, gravure or micro-gravure printing, and is coated, tensioned, wound and compacted under the conditions of drying at a temperature below 160° C. and a pressure of less than 2.5 MPa. During this process, the phase change microcapsules are always kept in a solid and sealed state to protect the capsule core material from leakage, thereby obtaining a positive electrode current collector 1 provided with a safety coating 2; the safety coating 2 has a single-side thickness of 3 μm after drying; specifically, the coating method used for applying the safety coating 2 in this embodiment is comma scraper coating, and the single-side thickness of the safety coating 2 after drying is 3 μm;
[0119] (3) Under an environment with an ambient humidity of less than 30%, the active slurry of the positive electrode active layer 3 is applied to the outer surface of the safety coating 2 by a comma blade coating method, a roller coating transfer method, or a slit extrusion method, and compacted under conditions of drying at a temperature below 160°C and a pressure of less than 2.5 MPa to obtain the positive electrode active layer 3; the total thickness of the electrode after drying and compacting is 59-115 μm, and during this process, the phase change microcapsules are always kept in a solid and sealed state, protecting the capsule core material from leakage, thereby obtaining a lithium battery composite positive electrode; specifically, the coating method used for coating the positive electrode active layer 3 in this embodiment is a comma blade coating method, and the total thickness of the coating of the positive electrode active layer 3 after drying and compacting is 83 μm;
[0120] (4) Repeat steps (2)-(3) to prepare a safety coating 2 and a positive electrode active layer 3 symmetrical to step (2) on the other side surface of the positive electrode current collector 1; after the safety coating 2 and the positive electrode active layer 3 on both sides are compacted and dried as a whole (compacted under conditions of drying below 160°C and pressure <2.5MPa), the total thickness of the electrode sheet after single-side coating is 60-120μm; wherein the thickness of the safety coating 2 is 0.5-5μm, and the thickness of the positive electrode active layer 3 is 59-115μm; a lithium battery composite positive electrode with a safety coating 2 and a positive electrode active layer 3 on both sides is prepared, and the phase change microcapsules are always kept in a solid and sealed state during the whole process to protect the capsule core material from leakage; specifically, in this embodiment, after the safety coating 2 and the positive electrode active layer 3 on both sides are coated, the total thickness of the electrode sheet is 179μm, wherein the thickness of the safety coating 2 on both sides is 3μm, the thickness of the positive electrode active layer 3 is 80μm, and the thickness of the aluminum foil is 13μm.
[0121] More specifically, the preparation of the safety slurry for the safety coating 2 in step (1) comprises the following steps:
[0122] (11) Prepare safety particles, phase change microcapsules 8, conductive agent, and binder respectively, and weigh each component according to a set ratio; wherein the preparation of phase change microcapsules refers to the aforementioned steps (111)-(113).
[0123] (12) Stirring and mixing: conductive carbon black, carbon nanotubes or graphene, graphite, safety particles, phase change microcapsules 8, and a binder are added to the solvent in sequence, and a high-speed vacuum disperser is used first, followed by a sand mill for preliminary dispersion; then, an ultrasonic treatment device is used to disperse the components again in an ultrasonic resonance manner, so that the components are evenly dispersed, thereby obtaining a safety slurry for preparing a safety coating.
[0124] The safety mechanism design of the phase change microcapsule in this embodiment is a passive strain mechanism. When the internal temperature of the lithium battery of this embodiment is lower than the set safety temperature of 160°C, the phase change microcapsule 8 maintains a solid shape. The safety coating can improve the electrical and thermal conductivity of the composite positive electrode through the cooperation of its porous structure with the binder, conductive agent, safety particles and phase change microcapsule 8. When the lithium battery has an internal short circuit or other circumstances that cause its internal temperature to reach or exceed the set safety temperature of 160°C and continue, the phase change material (insulating organic material paraffin) in the phase change microcapsule 8 in the safety coating 2 quickly changes from solid to liquid after being heated, and rapidly expands in volume. The internal pressure is increased, and the microcapsules are eventually broken and flowed out from the inside, and diffused rapidly, which quickly increases the internal resistance of the lithium battery, cuts off the internal electrochemical reaction, prevents the reaction from continuing, and inhibits side reactions, gas generation and thermal runaway diffusion, thereby controlling the internal temperature and volume of the battery to a safe state. The technical solution of the present application can, on the one hand, ensure that the lithium battery automatically terminates the electrochemical reaction under conditions such as disasters (internal short circuit or strong external extrusion and deformation), and on the other hand, does not affect the comprehensive performance of the lithium battery during the manufacturing process and under normal use, thereby resolving the technical contradiction between improving battery safety and ensuring the normal manufacturing and normal use of the battery.
[0125] In this embodiment, the set safety temperature is 160°C. In other embodiments, it can also be set to other required temperatures such as 110-150°C, and the rupture trigger temperature of the phase change microcapsule or one of the internal and external rupture pressure differences can be adjusted accordingly. The phase change microcapsule 8 is a spherical microcapsule with a capsule wall membrane and a capsule core, and an overall particle size of D50 = 2μm. The capsule thickness of the capsule wall membrane is 1.3-1.50μm. The internal and external safety critical pressure difference (i.e., the capsule rupture pressure difference) ΔP ≥ 2.5MPa, and ΔP can be specifically selected between 2.5-12.5MPa as needed. The phase change temperature of the phase change material matches the rupture strength of the membrane, which can simultaneously meet the preparation process of lithium batteries of known types and systems, and ensure that the phase change microcapsules do not rupture or fail during the entire preparation process.
[0126] The high-safety lithium battery and its composite positive electrode provided in the embodiments of the present application introduce phase change microcapsules with specific structures, components, and physical and chemical properties, and enable them to maintain their morphological integrity and sealed capsule wall membrane during the entire battery manufacturing process and normal use of the battery. Passive strain is triggered only when the battery is about to experience thermal runaway. It can specifically prevent internal short circuits, thermal runaway, and volume expansion, and rupture and release of insulating organic matter due to temperature rise or external pressure rising to a set value, thereby promptly stopping the electrochemical reaction inside the battery, so as to quickly, reliably, and effectively solve problems such as chain reactions and thermal runaway, and can meet the safety and high performance requirements of products such as lithium cobalt oxide and ternary lithium batteries.
[0127] The high-safety lithium battery composite positive electrode and lithium battery preparation method provided in this embodiment starts with improving the positive electrode side of the battery. By setting a safety coating on the positive electrode side, and setting phase change microcapsules that are conductive under normal conditions and shatter and insulate before thermal runaway in the safety coating, the internal electrochemical reaction is prevented when thermal runaway is about to occur, thereby avoiding its ultimate occurrence of thermal runaway. At the same time, by synchronously improving the lithium battery positive electrode structure, materials and preparation process, the mechanical strength, adhesion, thermal stability, and surface smoothness of the positive electrode sheet are improved, the internal resistance of the battery is reduced, and its overall thickness is uniform, so that it can inhibit the occurrence of side reactions under normal conditions and inhibit the growth of lithium dendrites on the negative electrode side. When the set temperature is reached, a phase change occurs to inhibit the spread of thermal runaway, thereby effectively and reliably solving the thermal runaway problem of lithium-ion batteries caused by various factors, improving the safety and stability of lithium-ion batteries, avoiding crises such as lithium battery explosion, and achieving rapid and effective control of crises; and without reducing the overall energy density, consistency or other charge and discharge performance of the battery, and extending the battery life.
[0128] Example 2
[0129] The phase change microcapsules, high-safety lithium batteries, and preparation methods thereof provided in this embodiment are further improvements based on Example 1, so that the internal and external safety critical pressure difference ΔP is not less than 3 MPa, and ΔP can be specifically selected between 2.5-10.5 MPa as needed.
[0130] The embodiment of the present application provides a highly safe lithium cobalt oxide (LCO) lithium power battery, which uses lithium cobalt oxide as the main positive electrode active material, artificial graphite as the negative electrode material, LiPF6 as the electrolyte, and a ceramic diaphragm (12 micron thick PE base film + 4 micron thick ceramic layer) to form a soft-pack lithium-ion battery with a capacity of about 5Ah.
[0131] The high-safety lithium battery composite positive electrode provided in this embodiment includes a positive electrode collector 1, a safety coating 2, and a positive electrode active layer 3; wherein the substrate of the positive electrode collector 1 is an aluminum foil (glossy) with a thickness of 15 μm; on both sides of the positive electrode collector 1, there are provided a safety coating 2 and a positive electrode active layer 3 stacked and bonded in sequence, and the safety coating 2 is arranged between the positive electrode collector 1 and the positive electrode active layer 3, and the three together form a composite positive electrode with a stacked structure.
[0132] The safety coating 2 in this embodiment is a porous, strongly adhesive, lubricating, elastic layer made of safety particles, phase-change microcapsules 8, a conductive agent, and a binder in a set ratio, and has a thickness of 2 μm after drying. The safety coating is prepared from its active slurry.
[0133] The active slurry of the safety coating 2 is prepared from the following components in the following mass ratio: safety particles: phase change microcapsules: conductive agent: binder = 90:15:5:4.5;
[0134] The phase change microcapsule 8 is formed by a capsule wall coating formed by melamine formaldehyde resin (softening temperature of 150-160°) and a modified conductive agent, which covers the insulating organic phase change material paraffin in the capsule core; the capsule wall coating is specifically a mixture of liquid methyl etherified melamine formaldehyde resin and solid conductive agent conductive graphite particles, the mass ratio (dry weight) of the two is 10:2, and the particles of the solid conductive agent conductive graphite are in the range of D50 = 0.75-1μm. By adjusting its particle size and mass ratio, the thickness and rupture pressure difference of the capsule wall coating after the melamine formaldehyde resin is cured can be appropriately reduced, which is adapted to the passive strain volume expansion ratio of the capsule core, so that the microcapsules are broken at the set temperature, their internal chemical reactions are prevented, and the thermal runaway diffusion is inhibited. In this embodiment, the mass ratio of liquid melamine resin to solid conductive agent conductive graphite particles is selected to be 10:2, and the particle size of the conductive graphite particles is D50 = 2.2 μm; the prepared phase change microcapsules have a particle size D50 = 2.2 μm, and the average thickness of the capsule wall membrane is 1-1.25 μm. When the volume expansion rate of the internal capsule core material reaches or exceeds 4% after the phase change (or the external pressure reaches the pressure limit value of the capsule wall membrane, and the internal and external rupture pressure difference is ≥3 MPa), rupture occurs, allowing the liquid capsule core material after the internal phase change to flow out quickly, rapidly increase the internal resistance of the lithium battery, and until the internal electrochemical reaction is cut off, avoiding catastrophic consequences.
[0135] In this embodiment, specifically, a solution of formaldehyde and melamine in a molar ratio of 8:1 is evenly mixed, the pH is adjusted to about 9, and the mixture is stirred and reacted at 75°C for 4 hours. The hexahydroxymethylmelamine crystals precipitated at the bottom are obtained and dried with filter paper; the hexahydroxymethylmelamine crystals are slowly added to methanol (the molar ratio of hexahydroxymethylmelamine to methanol is 1:15), and the pH is adjusted to 1.5-2.0 with sulfuric acid. The temperature is controlled at 45°C and stirred and kept warm for 6 hours to obtain a methylated melamine formaldehyde resin solution. After the reaction is completed, the temperature is restored to room temperature and the pH is adjusted to 8.0-8.5 with lithium carbonate; the conductive graphite with a D50 range of 0.75-1 μm is mixed with the prepolymer solution, and the ratio of the mass of the conductive graphite to the mass of the prepolymer solid is 2:10, and dispersed at 4000 rpm for 30 minutes to obtain an organic film-forming resin solution mixed with a modifier; the solution is evenly sprayed onto 70# paraffin wax powder, vacuum dried, rinsed with deionized water 3 times, and then infrared dried at 50°C for 4 hours to obtain phase change microcapsule particles synthesized by the spraying process, and then particles with a particle size of D50 = 2.2 μm are selected.
[0136] The phase change microcapsules synthesized in this embodiment have a capsule wall coating of methylated melamine formaldehyde resin, which has higher strength than unmethylated melamine formaldehyde resin. By controlling the mass ratio of resin solid to conductive graphite to 10:2, it is ensured that the capsule wall coating has sufficient compressive strength (when the conductive graphite added to the resin increases in the ratio range of 10:2-20, it has little effect on the compressive strength of the capsule wall coating, but the internal pressure resistance of the capsule core expansion decreases with the increase in the proportion of conductive graphite); by controlling the flow rate of the conductive mixed liquid during spraying, the thickness of the coating is ensured to be within 1-1.25μm, able to withstand internal and external pressure differences of 3MPa or more; the capsule core liquefies at around 65°C. When the external temperature rises to 150°C, the capsule core temperature will be slightly lower than the external temperature due to factors such as heat transfer efficiency. The volume expansion rate of the capsule core material at 150°C is about 13.8%, so it can reach a sufficient expansion rate (>3%) at 150°C, bursting the connection interface between the resin and the conductive graphite at the capsule wall membrane, thereby causing the microcapsule to rupture and release the insulating organic matter in the capsule core into the battery, which automatically terminates the chemical reaction.
[0137] The active material in this embodiment is granular lithium manganese iron phosphate; the conductive agent is conductive carbon black; and the binder is a water-based polymer PAA with a decomposition temperature greater than 300° C. The D50 of the granular lithium manganese iron phosphate is 0.5 μm.
[0138] The preparation method for the safety slurry of the safety coating 2 specifically comprises the following steps: lithium iron manganese phosphate, phase change microcapsules, and conductive carbon black are weighed in a mass ratio of 90:15:5, added to a glue solution containing 5% polyacrylic acid (PAA) solids by weight, and the solid content is controlled to 50%. After stirring and mixing, the active slurry is obtained. The stirring and mixing steps include sequentially adding the conductive carbon black, safety particles, phase change microcapsules, and binder to the PAA solvent, performing preliminary dispersion using a high-speed vacuum disperser and then a sand mill. Ultrasonic processing equipment is then used to further disperse the components using ultrasonic resonance to achieve uniform dispersion, thereby producing the safety slurry for the safety coating.
[0139] The active material in the positive electrode active layer 3 of this embodiment is lithium cobalt oxide, and the positive electrode active layer 3 is prepared from its active slurry. The active slurry is made of the following components in a mass ratio: 95% lithium cobalt oxide, 3.5% polyvinylidene fluoride (PVDF) as a binder, and 1.5% conductive carbon black as a conductive agent. The conductive carbon black is in granular form with a microscopic particle size of 20-60 nm.
[0140] The preparation method of active slurry is:
[0141] (1) Lithium cobalt oxide, polyvinylidene fluoride, and conductive carbon black were weighed in a mass ratio of 95:3.5:1.5;
[0142] (2) uniformly mixing the binder polyvinylidene fluoride and the NMP solvent to obtain a positive electrode glue;
[0143] (3) After the active material of the positive electrode active layer, polyvinylidene fluoride and conductive carbon black are evenly mixed, the positive electrode glue is added, stirred and mixed evenly, and the solid content is adjusted to 60% to obtain the active slurry of the positive electrode active layer; the stirring and mixing operation is performed by first using a high-speed vacuum disperser and then a sand mill for preliminary dispersion; then an ultrasonic treatment device is used to disperse again in an ultrasonic resonance manner so that the components therein are evenly dispersed.
[0144] A method for preparing the aforementioned high-safety lithium battery, wherein the composite positive electrode comprises the following steps:
[0145] (1) preparing the positive electrode current collector (aluminum foil), the safety slurry of the safety coating, and the active slurry of the positive electrode active layer respectively;
[0146] (2) The safety slurry of the safety coating is applied to one side of the current collector by a comma blade, spin coating, doctor blading, gravure or micro-gravure printing, and dried to obtain a positive electrode current collector provided with a safety coating; the thickness of the safety coating on one side after drying is 2.5 μm; In this embodiment, the safety slurry of the safety coating is evenly and continuously applied to the aluminum foil using a micro-gravure coater, and the single-side coating thickness is controlled to be 2.5 μm, and then dried. This process allows the phase change microcapsules 8 to maintain a spherical solid structure and a sealed capsule wall membrane, thereby obtaining a composite aluminum foil containing a safety coating;
[0147] (3) In an environment with an ambient humidity of less than 30%, the active slurry of the positive electrode active layer is applied to the outer surface of the safety coating by a comma scraper method, a roller coating transfer method, or a slit extrusion method, and then dried and compacted to obtain a positive electrode active layer; the thickness of a single side after drying and compacting is 60 μm; This embodiment adopts a coating method using a comma scraper to uniformly and continuously apply the active slurry of the positive electrode active layer to the upper layer of the safety coating, and controls the overall thickness of the electrode piece after single-sided coating to be 110-120 μm, compacted, and dried. This process allows the phase change microcapsules 8 to maintain a spherical solid complete structure and a sealed capsule wall membrane, thereby obtaining a composite positive electrode electrode piece with a safety coating and a positive electrode active layer on one side;
[0148] (4) Furthermore, when preparing a composite positive electrode with a safety coating and a positive electrode active layer on both sides of the aluminum foil, repeat steps (2)-(3) to prepare a safety coating and a positive electrode active layer symmetrical to step (2) on the other side surface of the positive electrode current collector 1; the safety coating 2 and the positive electrode active layer 3 on both sides are compacted and dried to a total thickness of 61.5 μm on one side; wherein the thickness of the safety coating is 2.5 μm, and the thickness of the positive electrode active layer is 59 μm; in each step, the phase change microcapsule 8 maintains a spherical solid complete structure and a sealed capsule wall membrane, thereby preparing a lithium battery composite positive electrode with a safety coating 2 and a positive electrode active layer 3 on both sides.
[0149] The drying temperature in the above steps is lower than 110° C., and the pressure during coating, winding and compacting is less than 3 MPa.
[0150] The phase change microcapsules, safety particles, porous structure, binder and conductive agent of the safety coating 2 in this embodiment cooperate with each other to improve the bonding strength between the layers of the composite positive electrode and reduce the surface resistance of the joint; the strong bonding, lubrication and elasticity characteristics it possesses improve the flexibility and mechanical strength of the composite positive electrode as a whole, so that the composite positive electrode can avoid the shedding of the positive electrode active material during the manufacturing and use process, and at the same time avoid the shedding of the positive electrode active material when it encounters external puncture, physical damage, internal lithium dendrites piercing the diaphragm, positive electrode active layer or positive electrode current collector; the safety coating 2 adjusts its own porous structure and elastic deformation performance through the composition, proportion and particle morphology of the safety particles and phase change microcapsules , in conjunction with the coating and compaction steps, the overall thickness uniformity and interface flatness of the positive electrode current collector and the positive electrode active layer can be adjusted, the distance of the lithium ion charge and discharge channels (i.e., the distance between the positive electrode current collector and the negative electrode current collector) can be balanced, the battery energy density and consistency can be improved, lithium ion nucleation can be avoided or reduced, and the generation and growth of lithium dendrites on the negative electrode side can be avoided or inhibited; by combining the porous structure with the binder, the conductive agent and the safety particles, the thermal stability of the composite positive electrode can be improved, the critical safety temperature of the battery thermal runaway can be increased, and the side reaction, gas generation and thermal runaway diffusion can be inhibited when the lithium battery has an internal short circuit, thereby improving the safety, consistency and stability of the lithium ion battery and extending its service life. The safety particles in this embodiment are lithium iron manganese phosphate disposed in the safety coating. Both the lithium iron manganese phosphate and the lithium cobalt oxide disposed in the positive electrode active layer participate in the lithium ion charge and discharge reaction process, but the main function of the granular lithium iron manganese phosphate as the safety particles is to improve the thermal stability of the safety coating and form a porous structure, and to cooperate with the conductive agent to improve the lubrication, electrical conductivity, thermal conductivity and other properties. This application uses two active materials with different properties to provide lithium ions for the internal chemical reaction of lithium ion batteries, which can take into account the energy density and safety of lithium ion batteries. The two positive active materials of this embodiment cooperate with each other to make the lithium ion battery have a higher energy density, which can meet the requirements of Li + The requirement for reversible insertion and extraction is that the structure is stable so that Li + The active material of the composite positive electrode is combined with a conductive agent and a binder, and has good thermal stability, so that the lithium ion battery has high safety. The lithium ion battery provided in this embodiment can achieve stable charge and discharge and has the ability to charge quickly during operation. The positive electrode material has high electrical conductivity and is easy to Li + Diffusion in the electrode material.
[0151] The coating and compaction treatment process used in this embodiment has a great influence on the resistance of the composite positive electrode plate. On the one hand, it improves the density of the particles in the electrode material layer in the plate, and on the other hand, it strengthens the interface bonding between the electrode material layer and the current collector, thereby reducing the interface resistance. In this process, in order to keep the phase change microcapsules in their solid shape, it is necessary to pre-match the capsule wall membrane and the capsule core to obtain the appropriate softening temperature value and external pressure limit value.
[0152] This embodiment solves the problem of poor interface bonding between the current collector foil and the electrode layer by providing a safety coating with specific components, structure and thickness and introducing phase change microcapsules. This causes the interface to separate quickly under the action of current shock and heat expansion during the normal charge and discharge cycle, entering a vicious cycle of "increase in interface resistance - heat expansion increases interface separation - further increase in interface resistance", and causing the internal resistance to increase rapidly. Since the expression of the capacity of the electrode layer in a lithium battery depends on the current collector to be derived, interface separation will affect the expression of the capacity, and the capacity will also decrease rapidly. This embodiment solves this problem by providing a safety coating with strong adhesion, lubrication and elasticity, as well as a compaction process, so that the lithium battery maintains its capacity during use, enhances the cycle stability of the entire battery, and extends its service life.
[0153] Example 3
[0154] The phase change microcapsules, high-safety lithium batteries and preparation methods provided in this embodiment are basically the same as those in Example 1 or 2, except that the safety particles in the safety coating are silicate ceramic powder, the proportion, composition and strength of the phase change microcapsules are different, and the active material in the positive electrode active layer is lithium cobalt oxide.
[0155] In this embodiment, the safety particles of the safety coating are silicate ceramics, whose D50 is 0.8 μm, and the mass ratio is 70; the binder is PAN, the mass ratio is 15, the mass ratio of the phase change microcapsules is 5, and the conductive agent is nickel-plated glass beads, the mass ratio is 10; the active material of the positive active layer is lithium cobalt oxide, the mass ratio is 97, the binder is polyvinylidene fluoride, the mass ratio is 2, and the conductive agent is conductive graphite, the mass ratio is 1.
[0156] In this embodiment, the active slurry for preparing the safety coating 2 is made of the following components in the following mass ratio: safety particles: phase change microcapsules, conductive agent: binder = 50:5:0.5:15.
[0157] The insulating organic matter forming the core of the phase-change microcapsule is polyethylene glycol or stearic acid, more specifically, tripalmitin; the organic film-forming resin is polystyrene modified with N-phenylmaleimide, the molar ratio of N-maleimide to styrene monomer is 3:7, and the softening temperature after modification is 159°C; the conductive modifier is nickel-plated glass microbeads with a particle size D50 of 0.5-0.9μm; the mass ratio of the film-forming mixture of the organic film-forming resin and the conductive modifier forming the coating is 10:2; the particle size D50 of the phase-change microcapsule is 2.5μm, the capsule wall coating thickness is 0.8-1.0μm, and the rupture pressure is ≥2.50MPa.
[0158] In this embodiment, THF is added as a solvent to a three-necked flask, a small amount of 4,4'-azobis(4-cyanovaleric acid) is used as an initiator (the molar ratio of initiator to reactant monomer is 1:50), and then a certain amount of N-phenylmaleimide monomer is added. Then, the three-necked flask is sealed and, under nitrogen protection and an ice-water bath, a certain amount of styrene monomer (styrene: N-phenylmaleimide = 7:3) is added to the flask using a syringe. After stirring and mixing evenly, the temperature is raised to 60°C, stirred and kept warm for 5 hours to obtain an N-phenylmaleimide-modified styrene resin. Nickel-plated glass microspheres with D50 = 0.8 μm are mixed with the prepolymer solution, the mass ratio of organic film-forming resin solids to nickel-plated glass microspheres is 10:2, and dispersed at 3000 rpm for 60 minutes to obtain an organic film-forming resin solution mixed with a modifier. Slowly add tripalmitin powder to the organic film-forming resin solution just prepared while stirring, with the core material mass: capsule wall coating material mass = 1:4. After dispersion at 3000rpm for 30min, filter and vacuum dry, rinse with chloroform three times to obtain phase change microcapsules synthesized by the dip coating process, and then screen the particles with a particle size D50 = 2.5μm.
[0159] The phase-change microcapsules synthesized using the aforementioned method feature a capsule coating composed of an N-phenylmaleimide-modified styrene resin with a glass transition temperature of 159°C and no noticeable softening below 150°C. By controlling the mass ratio of resin solids to nickel-plated glass microbeads to 10:5, the capsule coating maintains sufficient compressive strength. (Increasing the proportion of nickel-plated glass microbeads in the resin within a range of 10:1-20 has little effect on the capsule coating's compressive strength, but the capsule coating's ability to withstand internal pressure during core expansion, i.e., the strength required to trigger rupture, decreases with increasing nickel-plated glass microbead proportions.) Furthermore, by controlling the core-to-wall coating mass ratio during dip coating, the coating maintains a thickness of 0.8-1μm, capable of withstanding internal and external pressure differentials exceeding 2.5MPa. The capsule core of this embodiment undergoes phase change and liquefaction at around 66-68°C, but its volume expansion rate is less than 3% (limited by the capsule wall membrane). When the external temperature rises to 130°C, due to factors such as heat transfer efficiency, the capsule core temperature will be slightly lower than the external temperature, and the volume expansion rate of the capsule core material will rapidly rise to approximately 14% at 130°C. Therefore, a sufficient expansion rate (>4%) can be achieved at 130°C, rapidly bursting the connection interface between the resin and the nickel-plated glass beads at the capsule wall membrane, thereby causing the microcapsule to rupture and releasing the insulating organic matter in the capsule core into the battery, which automatically terminates the chemical reaction.
[0160] The safety temperature set in this embodiment is 130°C. After the internal capsule core undergoes phase change and the temperature rises to 130°C, the volume expands by more than 4%, and then ruptures. This causes the liquid capsule core after the internal phase change to flow out quickly, rapidly increasing the internal resistance of the lithium battery until the internal electrochemical reaction is cut off. The capsule core and microcapsule structure formed by the insulating organic phase change material maintains shape stability under temperature conditions below 130°C, ensuring the normal progress of the electrode coating and subsequent process of the battery cell preparation without affecting the basic performance of the electrode and battery cell. If the internal temperature of the battery exceeds 130°C, the internal capsule core will expand to more than 4% after the phase change, and then rupture. This causes the liquid capsule core after the internal phase change to flow out quickly, rapidly increasing the internal resistance of the lithium battery until the internal electrochemical reaction is cut off, avoiding catastrophic consequences. If the battery cell experiences severe thermal runaway and reaches the set safety temperature of 130°C or above in a very short time, for example, the temperature reaches 160°C, the core material has not yet been able to completely melt and burst the capsule wall membrane due to the heat transfer rate, but the capsule wall membrane resin exceeds the glass transition temperature, the capsule wall membrane softens rapidly, and loses its resistance to internal and external pressure. It can rupture under a small pressure difference (for example, 0.5MPa), releasing the core material. The core material is not only a good heat-absorbing material, but also insulating, which can sharply increase the resistance, cut off the current circuit, and completely prevent the occurrence of thermal runaway.
[0161] The steps for preparing the composite positive electrode of the high-safety lithium battery are as follows:
[0162] (1) Silicate ceramic powder, phase change microcapsules, and nickel-plated glass microbeads were weighed in a mass ratio of 50:5:0.5, and added to a glue solution with a converted PAN solid mass ratio of 20%, controlling the solid content to 30%. The solution was pre-dispersed for 30 minutes using a high-speed disperser (first stirring at a low speed, then accelerating). After the slurry was basically stirred evenly, it was vacuum dispersed at 2400RPM for 120 minutes (the vacuum degree must be greater than 0.08MPa), and then sand-milled. The slurry was sand-milled for 10 minutes at 2000 rpm to obtain a slurry. The slurry was evenly and continuously coated on a 10μm aluminum foil using a gravure coater, controlling the single-sided coating thickness to 5μm, and then dried to obtain a composite aluminum foil containing a safety coating.
[0163] (2) Lithium cobalt oxide, polyvinylidene fluoride and conductive graphite were weighed in a mass ratio of 97:2:1 and gradually added to NMP solvent, controlling the solid content at 50%. After stirring evenly, the slurry was evenly and continuously coated on the upper layer of the safety coating using a coating machine with a roller coating transfer method, controlling the coating thickness to 115-125 μm. After drying, the thickness of the positive electrode active layer was 110 μm, and a composite positive electrode sheet with a single-side coating total thickness of 115 μm was obtained.
[0164] The high-safety lithium battery and composite positive electrode provided by this embodiment improve the bonding strength of each bonding surface and the flexibility of the laminated material, and can avoid short circuits caused by the shedding of the positive electrode material during use under the conditions of normal operating temperature and internal and external pressure difference of less than 2.5MPa. When the lithium battery encounters external effects such as physical damage (including needle penetration test, mechanical impact, extrusion, deformation), if the active material on the positive electrode collector is prone to shedding (dropping), the exposed aluminum foil will come into contact with the fully charged negative electrode, which will generate the most heat and directly cause the battery to thermal runaway. The embodiment of the present application prevents the positive electrode from falling off by providing a safety coating, introducing phase change microcapsules with specific properties and dimensions, and enhancing the bonding strength and flexibility of each material; or even if a small amount of positive electrode active layer material falls off, the positive electrode collector will not be exposed, thereby enhancing the overall safety of the battery when encountering these situations.
[0165] Example 4
[0166] The phase change microcapsules, high-safety lithium batteries, composite positive electrodes or their preparation methods provided in this embodiment are basically the same as those in Examples 1-3, except that this embodiment provides an NCM811 ternary battery, the safety particles in the safety coating are hydrated alumina powder, the proportion and performance of the phase change microcapsules are different, and the active material in the positive electrode active layer is a nickel-cobalt-manganese ternary material. This embodiment takes NCM811 material as an example.
[0167] In this embodiment, the active slurry for preparing the safety coating 2 is made of components in the following mass ratio: safety particles: phase change microcapsules, conductive agent: binder = 60:20:10:20; the safety particles of the safety coating are hydrated alumina, with a mass ratio of 60, the mass ratio of the phase change microcapsules is 20, the binder is sodium alginate, with a mass ratio of 20, and the conductive agent is acetylene black, with a mass ratio of 10; the active material of the positive electrode active layer is nickel cobalt manganese, with a mass ratio of 90, the binder is polyvinylidene fluoride, with a mass ratio of 7.5, and the conductive agent is acetylene black, with a mass ratio of 2.5.
[0168] The insulating organic matter forming the core of the phase-change microcapsule is polyethylene glycol, specifically PEG-20000; the organic film-forming resin is a polystyrene resin modified with N-cyclohexyl furfuryl citral and maleic anhydride, and the molar ratio of the monomers is styrene: N-cyclohexyl furfuryl citral: maleic anhydride = 6:3.8:0.2, and the glass transition temperature after modification is 182°C; the conductive modifier is nickel-plated glass microbeads with a particle size D50 of 1.5-2μm; the mass ratio of the film-forming mixture of the organic film-forming resin and the conductive modifier forming the coating is 10:20; the particle size D50 of the phase-change microcapsule is 3μm, the thickness of the capsule wall is in the range of 0.5-0.75μm, and the difference in internal and external rupture pressure is ≥2.5MPa.
[0169] In the present embodiment, THF was added to a three-necked flask as a solvent, a small amount of t-butyl peroxybenzoate was added as an initiator (the molar ratio of the initiator to the reactant monomer was 1:40), and a certain amount of N-cyclohexyl furfuryl citric acid imide monomer and maleic anhydride were added, and then the three-necked flask was sealed. Under nitrogen protection and an ice-water bath, a certain amount of styrene monomer (styrene: N-cyclohexyl furfuryl citric acid imide: maleic anhydride = 6:3.8:0.2) was added to the flask using a syringe; after stirring and mixing, the mixture was heated to 95°C, stirred and kept warm for 8h to obtain a styrene resin prepolymer solution modified with N-cyclohexyl furfuryl citric acid imide and maleic anhydride; nickel-plated glass microbeads with D50 = 0.75 μm were added. Mixed with a modified styrene resin prepolymer solution, the mass ratio of the organic film-forming resin solids (dry matter) to the nickel-plated glass beads is 10:20, and dispersed at 3000rpm for 60min to obtain an organic film-forming resin solution mixed with a modifier; polyethylene glycol powder (PEG-20000) is slowly added to the organic film-forming resin solution just prepared while stirring, the mass of the core material (polyethylene glycol): the mass of the capsule wall coating material (organic film-forming resin solution) = 1:3.5, after dispersing at 3000rpm for 30min, filtered and vacuum dried, rinsed with chloroform 3 times, and the phase change microcapsules synthesized by the dip coating process can be obtained, and the particles with a particle size D50 = 3μm are screened.
[0170] The phase-change microcapsules synthesized using the above method have a capsule wall coating composed of a polystyrene resin modified with N-cyclohexyl furfuryl citral and maleic anhydride. This resin itself has high hardness and compressive strength, a glass transition temperature of 182°C, and no significant softening within 160°C. By controlling the mass ratio of resin solids to nickel-plated glass microbeads to 10:20, the capsule wall coating is ensured to have sufficient compressive strength (increasing the nickel-plated glass microbeads added to the resin within a ratio range of 10:1-20 has little effect on the compressive strength of the capsule wall coating, but the pressure differential tolerance range (internal and external pressure differential) during capsule core expansion decreases with increasing glass microbead proportions). This embodiment ensures a capsule coating thickness of 0.5-0.75 μm by controlling the mass ratio of capsule core to capsule wall coating during dip coating, capable of withstanding internal and external pressure differentials exceeding 2.5 MPa. The capsule core undergoes phase change and liquefaction at around 60-65°C; when the internal environment of the lithium battery rises to 120°C, the capsule core temperature will be slightly lower than the external temperature due to factors such as heat transfer efficiency. The volume expansion rate of the capsule core material at 120°C is about 11.6%, so it can reach a sufficient expansion rate (>6%) at 120°C, quickly bursting the connection interface between the resin and the nickel-plated glass beads at the capsule wall membrane, thereby causing the microcapsule to rupture and releasing the insulating organic matter in the capsule core into the battery, which automatically terminates the chemical reaction.
[0171] The safety temperature set in this embodiment can be 120°C. When the volume expansion of the internal capsule core exceeds 6% after the phase change, it will rupture, causing the liquid capsule core after the internal phase change to flow out quickly, rapidly increasing the internal resistance of the lithium battery until the internal electrochemical reaction is cut off. The capsule core and microcapsule structure formed by the insulating organic phase change material can maintain shape stability at temperatures below 120°C, ensuring the normal coating of the electrode and subsequent process of the battery cell preparation without affecting the basic performance of the electrode and battery cell. When the thermal runaway of the battery cell reaches the set safety temperature of 120°C or above, the capsule wall membrane will soften and rupture sharply, releasing the capsule core material. The capsule core material is not only a good heat-absorbing material, but also insulating, which can sharply increase the resistance, cut off the current circuit, and completely prevent the occurrence of thermal runaway.
[0172] The preparation process of the composite positive electrode sheet of the high-safety lithium battery includes the following steps:
[0173] (1) Weigh hydrated alumina powder ceramics, phase change microcapsules, and acetylene black in a mass ratio of 60:20:10, add them to a glue solution with a solid mass ratio of 4.5% of sodium alginate, control the solid content to 40%, and pre-disperse them for 30 minutes using a high-speed disperser (first stir at a low speed, then accelerate). After the slurry is basically stirred evenly, use 2400RPM vacuum dispersion for 120 minutes (the vacuum degree must be greater than 0.08MPa), and then sand grind; use 2000 rpm and sand grind for 10 minutes to obtain a slurry, use a gravure coater to evenly and continuously coat the above slurry on aluminum foil, control the single-sided coating thickness to 3μm, dry and substitute, and obtain a composite aluminum foil containing a safety coating;
[0174] (2) Lithium nickel cobalt manganese oxide, polyvinylidene fluoride and acetylene black were weighed according to the dry matter mass ratio of 90:7.5:2.5, and gradually added to the NMP solvent to control the solid content at 55%. After stirring evenly, the above slurry was evenly and continuously coated on the upper layer of the safety coating by a coating machine using an extrusion coating method, and the single-sided coating thickness was controlled to 60 μm. After drying and compacting, a composite positive electrode sheet with a total single-sided coating thickness of 60 μm was obtained.
[0175] An important internal cause of internal short circuit in lithium batteries is the growth of lithium dendrites at the negative end, which punctures the solid electrolyte interface (SEI) film and causes internal short circuit. Therefore, lithium dendrites are also one of the core issues affecting the safety and stability of lithium-ion batteries. The formation of lithium dendrites can also easily pierce the diaphragm, causing internal short circuit in the lithium-ion battery, resulting in thermal runaway of the battery and causing combustion and explosion. At present, most solutions are to improve the negative electrode material, diaphragm or electrolyte, or to make the SEI film have higher strength, so as to effectively inhibit the growth of lithium dendrites. The embodiment of the present application improves the flatness and flexibility of the positive electrode material by providing a safety coating (a porous and elastic structure formed by its safety particles and phase change microcapsules), balances the distance of the lithium ion charge and discharge channels, reduces or avoids lithium ion nucleation, and avoids or inhibits the generation and growth of lithium dendrites; at the same time, the strength and flexibility of the composite positive electrode sheet and aluminum foil are enhanced, the lithium dendrites that puncture the SEI film are inhibited from reaching the aluminum foil, and the material shedding and aluminum foil exposure caused by the lithium dendrites piercing the positive active material layer are avoided, thereby reducing the probability of thermal runaway.
[0176] Example 5
[0177] The phase change microcapsules, high-safety lithium batteries, composite positive electrodes, or preparation methods thereof provided in this embodiment are substantially the same as those in Examples 1-4, except that the safety particles of the safety coating are alumina ceramics, the proportion and performance of the phase change microcapsules are different, the conductive agent is graphene, and the binder is styrene-butadiene rubber.
[0178] The active slurry for preparing the safety coating 2 is made of the following components in the following mass ratio: safety particles: phase change microcapsules, conductive agent: binder = 80:10:8:12.
[0179] The insulating organic matter forming the core of the phase-change microcapsule is glyceryl tristearate; the organic film-forming resin is butylated melamine formaldehyde resin, and the softening temperature after modification is 160-170°C; the conductive modifier is conductive graphite with a particle size D50 of 0.5-0.75 μm; the mass ratio of the film-forming mixture of the organic film-forming resin and the conductive modifier forming the coating is 10:12; the particle size D50 of the phase-change microcapsule is 2.75 μm, the thickness of the capsule wall is 0.5-0.6 μm, and the rupture pressure is ≥6.5 MPa.
[0180] In this example, a commercially available butylated melamine formaldehyde resin with a low degree of etherification (Shanghai Nanda Resin Factory) was diluted in water to form a solution of approximately 30%. The pH was adjusted to approximately 4.5. Conductive graphite with a D50 of 0.5-0.75 μm was added to this solution, with a mass ratio of resin solids to graphite of 10:12. The solution was dispersed at 4000 rpm for 1 hour to obtain a capsule wall coating material solution in which the conductive film-forming agent and resin were uniformly mixed. Tripalmitin powder and a small amount of OP-10 were added to this solution as an emulsifier, and the solution was dispersed at 2000 rpm for 30 minutes. n-Butanol and toluene were added to this emulsion, with the molar ratio of butylated melamine formaldehyde resin, n-Butanol, and toluene being 1:4.5:0.5. The solution was stirred slowly at 200 rpm, heated to 60°C, reacted for 1 hour, then heated to a slight boil, refluxed at atmospheric pressure, and water was removed via a water separator. The mixture was then allowed to react for 6 hours. After cooling to room temperature, the mixture was filtered, rinsed with acetone three times, and dried in vacuo to obtain phase change microcapsules prepared by interfacial polymerization process, and particles with a particle size of D50 = 2.75 μm were selected.
[0181] The phase change microcapsules synthesized by the above method have a capsule wall coating of butylated melamine formaldehyde resin. By controlling the mass ratio of resin solids to graphite to 10:12, the capsule wall coating is ensured to have sufficient compressive resistance (when the conductive graphite added to the resin is gradually increased in the ratio range of 10:1-20, it has little effect on the compressive strength of the capsule wall coating, but the tolerance to the expansion of the capsule core (internal and external pressure difference) decreases with the increase in the proportion of conductive graphite). In this embodiment, by controlling the mass ratio of the capsule core to the capsule wall coating during dipping, the coating thickness is ensured to be 0.5-0.6 μm and can withstand a pressure of 6.5 MPa. The capsule core liquefies at around 71°C. When the external temperature rises to 150°C, the capsule core temperature will be slightly lower than the external temperature due to factors such as heat transfer efficiency. The volume expansion rate of the capsule core material is about 5.4% at 110°C, so it can reach a sufficient expansion rate (>5%) at 110°C, quickly bursting the connection interface between the resin and the conductive graphite at the capsule wall coating, thereby causing the microcapsule to rupture and releasing the insulating organic matter in the capsule core into the battery, which automatically terminates the chemical reaction.
[0182] The safety temperature set in this embodiment is 110°C. When the volume expansion of the internal capsule core exceeds 5% after the phase change, it will rupture, causing the liquid capsule core after the internal phase change to flow out quickly, rapidly increasing the internal resistance of the lithium battery until the internal electrochemical reaction is cut off. The capsule core and microcapsule structure formed by the insulating organic phase change material are stable at 110°C, ensuring the normal coating of the electrode and subsequent processes in the preparation of the battery cell without affecting the basic performance of the electrode and the battery cell. When the thermal runaway of the battery cell reaches the set safety temperature of 110°C or above, the capsule wall membrane will soften sharply at the controllable critical temperature of thermal runaway, releasing the capsule core material. The capsule core material is not only a good heat-absorbing material, but also insulating, which can sharply increase the resistance, cut off the current circuit, and completely prevent the occurrence of thermal runaway. The active slurry of the positive electrode active layer 3 is made of components in the following mass ratio: nickel-cobalt-aluminum high-nickel active material: graphene conductive agent: styrene-butadiene rubber binder = 98:0.5:0.5; the graphene conductive agent is 1-7 layers with a lateral size of 5-100μm. It has strong electrical and thermal conductivity and mechanical strength. Its combination with phase change microcapsules, other materials and processes can greatly improve the thermal conductivity, electrical conductivity and mechanical strength of lithium batteries, and improve the anti-puncture ability of the composite positive electrode sheet.
[0183] Among the many causes of battery thermal runaway, mechanical damage, such as needle puncture, is also an irreversible destructive behavior that causes battery damage. When a battery is punctured by a sharp external object or subjected to a large impact, it will suffer mechanical damage, breaking the internal structure and directly exposing the internal materials, which can easily cause a short circuit between the positive and negative electrodes within the battery. In particular, when a battery encounters safety issues such as needle puncture, if the positive electrode loses material or the positive electrode active material structure is unstable, the aluminum foil will come into direct contact with the fully charged negative electrode, which can easily trigger thermal runaway and lead to further safety accidents. The solution provided in this embodiment can effectively prevent this problem and overcome the battery protection and state recovery issues during short-term temperature increases and then return to normal temperature. It can also block the local electrochemical reaction through the strain response of the phase change microcapsules distributed at the puncture site without affecting the performance of other parts of the battery, avoiding the overall scrapping of the battery.
[0184] Comparative Example 1
[0185] The technical solution of Example 1 was prepared into a 5Ah lithium-ion soft-pack battery; at the same time, bare aluminum foil was used as the positive electrode current collector, and the same positive electrode ternary NCM622 system and the same negative electrode formula and process as in Example 1 were used to prepare a 5Ah lithium-ion soft-pack battery. A needle puncture test was performed at 100% SOC, and all failed, with thick smoke and fire occurring.
[0186] The battery was tested for other comprehensive electrical properties, and the use of a lithium battery with a composite positive electrode having a safety coating improved the comprehensive performance without affecting the energy density.
[0187] 18650 lithium-ion batteries were manufactured using the technical solutions of the embodiments of the present application and the technical solution of Comparative Example 1, and their performance was evaluated. The comparative data are shown in Table 1 below.
[0188] Table 1: Comparison table of test data comparing the performance of the composite cathode battery prepared using this embodiment and the battery prepared using plain foil.
[0189] The technical solutions of Example 2 of the present application and the technical solutions of Comparative Example 1 were respectively used to manufacture 18650 lithium-ion batteries, and the lithium dendrite formation thereof was tested. The test method was as follows: After the batteries prepared in Example 2 and Comparative Example 1 were cycled for 1C, the batteries were disassembled, and the lithium dendrites of the negative electrode plates were compared and observed. The comparative data are shown in Table 2.
[0190] Table 2: Comparative observation data of lithium dendrites on the negative electrode sheet after 1C cycle From the comparative data in Table 2, it can be seen that it has a good inhibitory effect on the growth of lithium dendrites.
[0191] Through actual testing, it can be known that the phase change microcapsules, high-safety lithium batteries and preparation methods provided by this application focus on the simultaneous improvement of lithium battery structure, materials and processes, and the introduction of phase change microcapsules that are passively strained based on temperature or pressure. The microcapsules can maintain the integrity and closure of the overall external structure during the entire safety coating processing, electrode processing and overall lithium battery processing and manufacturing process, as well as during normal use. The capsule core material does not flow out, and it only reacts passively when the temperature or pressure inside the battery is abnormal, thereby ensuring the normal manufacturing of lithium batteries under normal conditions, without changing the existing manufacturing process and equipment, and without changing the basic structure and operating parameters of the existing lithium batteries, and are easy to industrialize and manufacture. At the same time, the phase change microcapsules provided by this application can also be used in the manufacture of other phase change temperature control products.
[0192] It should be noted that the above embodiments of this application only list some of the technical solutions. Within the scope of the materials (components), ratios, processes and parameters described above, those skilled in the art can make specific selections as needed to achieve the technical effects described in this application. Therefore, this application will not list them one by one.
[0193] The above description is merely an exemplary embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A phase change microcapsule, characterized in that: The microcapsule is a spherical microcapsule, comprising a capsule wall membrane and a spherical capsule core completely covered by the capsule wall membrane; The capsule core is a phase-change material, which is a phase-change insulating organic matter with a phase-change temperature of 55-70°C, or a mixture of multiple insulating organic matters; The capsule wall is a conductive and thermally conductive film formed by a mixture of an organic film-forming resin and a conductive modifier; The capsule wall coating keeps the phase-change microcapsule intact and airtight when the temperature of the environment system in which it is located is not higher than the set safety critical temperature and the pressure difference between the inside and outside of the environment system in which it is located is not greater than the set safety critical pressure difference, and the phase-change insulating organic matter is coated inside the capsule wall coating; When the temperature of the environment system in which the capsule wall coating is located reaches or exceeds the set safety critical temperature, or the pressure difference between the inside and outside of the environment system reaches or exceeds one of the set safety critical pressure differences, the capsule wall coating ruptures, destroys the integrity and closed shape of the phase change microcapsule, and quickly releases the liquid phase change insulating organic matter coated inside the capsule wall coating into the environment system and diffuses it, quickly increasing the resistance of the material of the environment system in which it is located and blocking the continuation of the electrochemical reaction in the environment system.
2. The phase change microcapsule according to claim 1, characterized in that: The phase change material forming the capsule core is one of paraffin and polyethylene glycol with a phase change temperature of 55-70°C, or a composite phase change material with a phase change temperature of 55-70°C mixed with paraffin waxes with different numbers of carbon atoms and fatty acids and / or fatty alcohols, or a composite phase change material with a phase change temperature of 55-70°C mixed with polyethylene glycols with different molecular weights, and the volume expansion rate is ≥3% when the temperature rises to 110°C.
3. The phase change microcapsule according to claim 1, characterized in that: The average thickness of the capsule wall is 0.50-1.50 μm; The conductive modifier forming the capsule wall coating is one of conductive graphite and nickel-plated glass microbeads with a particle size D50 of 0.5-2.0 μm or a mixture thereof; The organic film-forming resin forming the capsule wall coating is melamine formaldehyde, polystyrene resin or a mixture thereof; The mass ratio of the organic film-forming resin to the conductive modifier in the film-forming mixture is 10:(1-20); The increase in the proportion of the conductive modifier forming the capsule wall in the film-forming mixture and the increase in particle size are negatively correlated with the conditions for achieving the rupture of the capsule wall. The increase in the proportion of the organic film-forming resin in the film-forming mixture and the increase in the glass transition temperature are positively correlated with the conditions for achieving the rupture of the capsule wall. Furthermore, the glass transition temperature of the capsule wall coating is not lower than 150° C., that is, at a temperature of 150° C. or above, the capsule wall coating changes from a glassy state to a highly elastic state.
4. The phase-change microcapsule according to any one of claims 1 to 3, characterized in that: The average particle size of the phase change microcapsules is 2-3 μm; The set safety critical temperature of the environmental system in which it is located is 110-160°C, and the set internal and external safety critical pressure difference is not less than 2.5MPa.
5. The phase change microcapsule according to claim 1, characterized in that: The capsule core is fully refined paraffin with a phase transition temperature of 55-70°C; The organic film-forming resin that forms the capsule wall coating is melamine formaldehyde resin; The preparation steps of the phase change microcapsules are as follows: evenly mixing a solution of formaldehyde and melamine in a molar ratio of 2.5:1, adjusting the pH to 8.5, and stirring the mixture at 70°C and 400 rpm for 90 minutes to obtain a melamine formaldehyde prepolymer solution; mixing a conductive graphite with a modified conductive agent D50=0.5 μm with the prepolymer solution, wherein the mass ratio of the conductive graphite to the mass of the prepolymer solid dry matter is 1:10, and dispersing the mixture at 2000 rpm for 30 minutes to obtain an organic film-forming resin solution mixed with a modifier as a capsule wall coating material solution; slowly adding the organic film-forming resin solution to an aqueous emulsion of a pre-dispersed solid fully refined paraffin powder while stirring to obtain a paraffin emulsion as a capsule core material emulsion; The mass of the core material emulsion: the mass of the wall coating material solution = 1: (2.4-2.8), add a formaldehyde aqueous solution, and make the volume ratio of formaldehyde: melamine = 2.8:1, heat to 55°C, keep warm for 1 hour, continue to heat to 85°C, keep warm for 3.5 hours, and use an in-situ polymerization process to synthesize the phase change microcapsules.
6. The phase change microcapsule according to claim 1, characterized in that: The safety critical temperature is 110-160°C.
7. The phase change microcapsule according to claim 1, characterized in that: The internal and external safety critical pressure difference refers to the internal and external pressure difference that causes the capsule to rupture, and the safety critical pressure difference is 2.5MPa.
8. The phase change microcapsule according to claim 1, characterized in that: The capsule core is an insulating organic phase change material paraffin; The capsule wall coating is a mixture of melamine formaldehyde resin, which is a liquid methyl etherified melamine formaldehyde resin, and solid conductive agent, which is conductive graphite particles; The mass ratio of the liquid methyl etherified melamine formaldehyde resin to the solid conductive agent conductive graphite particles is 10:2, and the particle size of the conductive graphite particles D50=2.2 μm; The preparation steps of the phase change microcapsule particles are as follows: uniformly mixing a solution of formaldehyde and melamine in a molar ratio of 8:1, adjusting the pH to 9, stirring and reacting at 75°C for 4 hours, obtaining hexahydroxymethylmelamine crystals precipitated at the bottom, and drying with filter paper; slowly adding the hexahydroxymethylmelamine crystals into methanol (the molar ratio of hexahydroxymethylmelamine to methanol is 1:15), adjusting the pH to 1.5-2.0 with sulfuric acid, controlling the temperature at 45°C, stirring and keeping warm for 6 hours, and obtaining a methylated melamine formaldehyde resin solution; reacting After completion, return to room temperature and adjust the pH to 8.0-8.5 with lithium carbonate; mix the conductive graphite in the range of D50=0.75-1μm with the prepolymer solution, the ratio of the mass of the conductive graphite to the mass of the prepolymer solid is 2:10, disperse at 4000rpm for 30min to obtain an organic film-forming resin solution mixed with a modifier; spray the solution evenly into 70# paraffin powder, dry it with vacuum, rinse it with deionized water 3 times, and then infrared dry it at 50°C for 4h to obtain phase change microcapsule particles synthesized by the spraying process.
9. The phase change microcapsule according to claim 1, characterized in that: The capsule core is polyethylene glycol or stearic acid or tripalmitin; The organic film-forming resin forming the capsule wall coating is polystyrene modified with N-phenylmaleimide; The preparation steps of the phase change microcapsule particles are as follows: THF is added as a solvent into a three-necked flask, a small amount of 4,4'-azobis(4-cyanovaleric acid) is added as an initiator (the molar ratio of the initiator to the reactant monomer is 1:50), and then a certain amount of N-phenylmaleimide monomer is added, and then the three-necked flask is sealed, and a certain amount of styrene monomer (styrene: N-phenylmaleimide = 7:3) is added to the flask using a syringe under nitrogen protection and an ice water bath; after stirring and mixing evenly, the temperature is raised to 60° C., and stirring is maintained and the temperature is kept for 5 hours to obtain N-phenylmaleimide-modified phenyl Ethylene resin; nickel-plated glass microbeads with D50=0.8μm are mixed with the prepolymer solution, the mass ratio of organic film-forming resin solids to nickel-plated glass microbeads is 10:2, and dispersed at 3000rpm for 60min to obtain an organic film-forming resin solution mixed with a modifier; tripalmitin powder is slowly added to the organic film-forming resin solution just prepared while stirring, the mass of core material: the mass of capsule wall coating material = 1:4, after dispersing at 3000rpm for 30min, filtered and vacuum dried, rinsed with chloroform 3 times, and phase change microcapsules synthesized by the dip coating process can be obtained.
10. The phase change microcapsule according to claim 1, characterized in that: The capsule core is PEG-20000; The organic film-forming resin forming the capsule wall coating is a polystyrene resin modified by N-cyclohexyl furancitimide and maleic anhydride; The preparation steps of the phase change microcapsule particles are as follows: THF is added as a solvent into a three-necked flask, a small amount of tert-butyl peroxybenzoate is added as an initiator (the molar ratio of the initiator to the reactant monomer is 1:40), and then a certain amount of N-cyclohexyl furan citric acid imide monomer and maleic anhydride are added, and then the three-necked flask is sealed, and a certain amount of styrene monomer (styrene: N-cyclohexyl furan citric acid imide: maleic anhydride = 6:3.8:0.2) is added to the flask using a syringe under nitrogen protection and an ice water bath; after stirring and mixing evenly, the temperature is raised to 95° C., stirring and keeping warm for 8 hours to obtain a styrene resin prepolymer solution modified with N-cyclohexyl furan citric acid imide and maleic anhydride; nickel-plated glass microbeads with D50 = 0.75 μm are mixed with the modified styrene resin prepolymer solution, and the solid content (dry matter) of the organic film-forming resin and the mass ratio of the nickel-plated glass microbeads are 1:
40. The mass ratio is 10:20, and it is dispersed at 3000rpm for 60min to obtain an organic film-forming resin solution mixed with a modifier; polyethylene glycol powder (PEG-20000) is slowly added to the organic film-forming resin solution just prepared while stirring, the mass of the core material (polyethylene glycol): the mass of the capsule wall coating material (organic film-forming resin solution) = 1:3.5, after dispersing at 3000rpm for 30min, it is filtered and vacuum dried, and rinsed with chloroform 3 times to obtain phase change microcapsules synthesized by the dip coating process.
11. The phase-change microcapsule according to claim 1, characterized in that: The capsule core is glyceryl tristearate; The organic film-forming resin that forms the capsule wall coating is butylated melamine formaldehyde resin; The preparation steps of the phase change microcapsule particles are as follows: diluting butylated melamine formaldehyde resin in water to form a 30% solution, adjusting the pH to 4.5, adding conductive graphite with D50=0.5-0.75 μm to the solution, with the mass ratio of resin solids to graphite being 10:12, dispersing at 4000 rpm for 1 hour, and obtaining a capsule wall coating material solution in which the conductive film-forming agent and the resin are uniformly mixed; adding tripalmitin powder and a small amount of OP-10 as an emulsifier to the solution. , disperse at 2000rpm for 30min; add n-butanol and toluene to the emulsion, wherein the molar ratio of butylated melamine formaldehyde resin, n-butanol and toluene is 1:4.5:0.5, maintain slow stirring at 200rpm, raise the temperature to 60°C, react for 1h, then raise the temperature to slightly boiling, reflux at normal pressure, separate water through a water separator, maintain this state for 6h; after cooling to room temperature, filter, rinse with acetone 3 times, and obtain phase change microcapsules prepared by interfacial polymerization process after vacuum drying.
12. A method for preparing the phase-change microcapsule according to any one of claims 1 to 4, characterized in that: The steps include: (111) preparing or weighing an organic film-forming resin and a conductive modifier according to the materials, proportions and particle sizes of the capsule wall coating corresponding to the set safety critical temperature and safety critical pressure difference, and mixing them uniformly to obtain a film-forming mixture for forming the capsule wall coating; (112) preparing or weighing insulating organic solid particles with a phase change temperature of 55-70° C. as capsule cores according to the phase change materials and their proportions corresponding to the set phase change temperature and the volume expansion rate at the safety critical temperature; (113) The film-forming mixture is uniformly coated on the outer surface of insulating organic solid particles by using a spraying process, a dipping process, an in-situ polymerization process or an interfacial polymerization process, and then dried. Particles with a particle size of D50 = 2-3 μm are screened at room temperature to obtain phase change microcapsules.
13. A high-safety lithium battery, characterized in that: It includes a composite positive electrode collector, on at least one side of which a safety coating and a positive electrode active layer are stacked and bonded in sequence; the safety coating, the positive electrode collector and the positive electrode active layer are mutually bonded and compacted to form a composite positive electrode with a stacked structure; wherein the safety coating is an elastic layer with a dense structure formed by tightly combining a set proportion of safety particles, the phase change microcapsules described in any one of claims 1 to 12, a conductive agent and a binder.
14. The high-safety lithium battery according to claim 13, characterized in that: The safety slurry of the safety coating is prepared, wherein the weight ratio of each substance is set as follows: safety particles: phase change microcapsules: conductive agent: binder = (50-90): (5-20): (0.5-10): (4.5-20).
15. The high-safety lithium battery according to claim 14, characterized in that: The safety slurry of the safety coating is prepared, wherein the weight ratio of each substance is set to be safety particles: phase change microcapsules: conductive agent: binder = 75:10:5:
10.
16. The high-safety lithium battery according to claim 14, characterized in that: The safety particulate matter is lithium metal phosphate or its modified material, silicate or its derivative material series, alumina ceramic or its derivative material, including: lithium iron phosphate or its modified material, lithium iron manganese phosphate or its modified material, lithium vanadium phosphate or its modified material, silicon dioxide or silicate material, aluminum silicate or its modified material, alumina ceramic or its modified material, hydrated alumina or its modified material, bauxite or its modified material, aluminum titanate ceramic or its modified material or one or more thereof; wherein the lithium iron phosphate D50 is 0.2-2.0μm, the silicate material D50 is 0.1-5μm, and the alumina material D50 is 0.2-10μm; the conductive agent is one or more of conductive carbon black, acetylene black, conductive graphite, carbon nanotubes or graphene; the binder is an aqueous polymer or its salt with a decomposition temperature greater than 300°C, including: one or more of polyacrylic acid or its salt, modified acrylic acid, modified polyacrylonitrile, and sodium alginate.
17. The high-safety lithium battery according to claim 16, characterized in that: The safety particles are lithium iron phosphate with a particle size of D50=1.2 μm; the conductive agent is conductive carbon black and conductive graphite with a weight ratio of 1:1; the binder is modified acrylic acid and sodium alginate with a mass mixing ratio of 8:1; or The safety particles are lithium iron manganese phosphate, with a particle size D50 = 0.5 μm; the conductive agent is conductive carbon black; the binder is a decomposition temperature Aqueous polymer PAA at a temperature greater than 300°C; or The safety particles are silicate ceramic powders with a particle size of D50 = 0.8 μm; the conductive agent is conductive graphite; the binder is PAN; or The safety particles are hydrated aluminum oxide powder; the conductive agent is acetylene black; the binder is sodium alginate; or The safety particles are alumina ceramics; the conductive agent is graphene; and the binder is styrene-butadiene rubber.
18. The high-safety lithium battery according to claim 13, characterized in that: The positive electrode current collector is a metal aluminum foil or aluminum mesh with a thickness of 8-20 μm; the thickness of the safety coating after drying is 0.5-5 μm, and the thickness of the positive electrode active layer after drying is 59-115 μm; the total thickness of the safety coating and the positive electrode active layer after compaction and drying is 60-120 μm.
19. The high-safety lithium battery according to claim 18, characterized in that: The positive electrode current collector is a smooth metal aluminum foil with a thickness of 13μm, the thickness of the safety coating after drying is 3μm, and the thickness of the positive electrode active layer after drying is 80μm; the total thickness of the safety coating coated on one side and the positive electrode active layer after compaction and drying is 83μm, and the thickness of the overall electrode sheet after single-sided coating is 96μm after drying.
20. The high-safety lithium battery according to claim 13, characterized in that: On both sides of the positive electrode current collector of the composite positive electrode, safety coatings and positive electrode active layers are symmetrically stacked and bonded in sequence, and a plurality of phase-change microcapsules are evenly distributed in each safety coating.
21. A method for preparing a high-safety lithium battery according to any one of claims 13 to 20, characterized in that: The composite positive electrode is prepared by the following steps: (1) preparing a positive electrode current collector, a safety slurry for a safety coating, and an active slurry for a positive electrode active layer respectively; (2) applying the safety slurry of the safety coating onto one side of the current collector by a comma scraper, spin coating, doctor blading, gravure or micro-gravure printing, and drying at a temperature below 110° C. so that the phase change microcapsules are always kept in a solid and sealed state, thereby obtaining a positive electrode current collector provided with a safety coating; the safety coating has a single-side thickness of 1.5-5 μm after drying; (3) In an environment where the ambient humidity is less than 30%, the active slurry of the positive electrode active layer is coated on the outer surface of the safety coating by a comma scraper method, a roller transfer method or a slit extrusion method, and then dried and compacted to obtain a positive electrode active layer; the overall thickness of the electrode sheet after drying and compacting at a temperature below 110° C. is 60-110 μm, so that the phase change microcapsule always remains in a solid and sealed state, thereby obtaining a lithium battery composite positive electrode.
22. The preparation method according to claim 21, characterized in that: It includes the following steps: (4) Repeat steps (2)-(3) to prepare a safety coating and a positive electrode active layer symmetrical to step (2) on the other side of the positive electrode current collector; the safety coating and the positive electrode active layer on both sides are compacted and dried to a total thickness of 60-120 μm on one side; the thickness of the safety coating is 0.5-5 μm, and the thickness of the positive electrode active layer is 59-115 μm; and a lithium battery composite positive electrode having safety coatings and positive electrode active layers on both sides is prepared.
23. The preparation method according to claim 22, characterized in that After single-sided coating, the total thickness of the electrode sheet is 60 to 120 μm; the thickness of the safety coating is 3 μm, and the thickness of the positive electrode active layer is 80 μm; a lithium battery composite positive electrode with safety coating and positive electrode active layer on both sides is prepared, and the total thickness of the electrode sheet is 179 μm; and during the whole process, the phase change microcapsules are always kept in a solid and sealed state to protect the capsule core material from leakage.
24. The preparation method according to claim 21, characterized in that: The step (1) of preparing the safety slurry for the safety coating comprises the following steps: (11) preparing safety particles, phase change microcapsules, conductive agents, and binders respectively, and weighing the components according to a set ratio; (12) Stirring and mixing: Add conductive carbon black, carbon nanotubes or graphene, graphite, safety particles, phase change microcapsules, and a binder to the solvent in sequence, and perform preliminary dispersion using a high-speed vacuum disperser and then a sand mill; then, perform secondary dispersion using an ultrasonic treatment device in an ultrasonic resonance manner so that the components are evenly dispersed, thereby obtaining a safety slurry for preparing a safety coating.
Citation Information
Patent Citations
Phase-change paraffin microcapsules for battery heat management and preparation method thereof
CN103265933A
Method for improving needling safety performance of lithium ion battery
CN105895959A
Lithium-ion battery composite membrane and preparation method thereof and lithium-ion battery
CN105932200A
Organic-microcapsule phase change material, preparation method thereof, and application of organic-microcapsule phase change material in battery thermal management system
CN113861942A
Phase change microcapsule, high-safety lithium battery composite positive electrode and preparation method of phase change microcapsule and high-safety lithium battery composite positive electrode
CN115558471A
Cited By
Battery device and electric device
CN119627298A
Battery foil, secondary battery and electric equipment
CN119812349A
High-corrosion-resistance flux-cored wire and preparation method thereof
CN120115876A
Positive electrode composite aluminum foil current collector and preparation method thereof
CN120319817A
Diaphragm and energy storage battery
CN120432802A