Method for producing a membrane-electrode assembly for an electrochemical cell

The selective oxidation of carbon-based carrier materials in fuel cells expands pores near catalysts, enhancing gas transport and cell performance, addressing the limitations of existing thermal treatments by controlling the reaction and reducing costs.

WO2024231370A1PCT designated stage expired Publication Date: 2024-11-14ROBERT BOSCH GMBH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/062513
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-07
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Current methods for producing membrane-electrode arrangements in fuel cells face challenges in optimizing the pore structure of carbon-based carrier materials, leading to limited gas transport and reduced performance, especially at high current densities, and existing thermal post-treatment processes are difficult to control and costly.

Method used

A method involving selective oxidation of carbon-based carrier materials using reactive gases like CO2, NH3, NO2, NO, or H2O to expand pores near the catalyst material, improving gas transport without excessive heat generation, allowing for controlled and cost-effective upscaling.

Benefits of technology

The method enhances the pore structure of carbon-based carrier materials, increasing the performance of fuel cells by improving gas transport and reducing platinum usage, while maintaining control over the reaction to prevent uncontrolled combustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024062513_14112024_PF_FP_ABST
    Figure EP2024062513_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing an electrochemical cell, preferably a fuel cell, in particular a PEM fuel cell, wherein in order to form an electrode of a membrane-electrode assembly, a catalyst material is deposited onto a carbon-based carrier material which has a pore structure, and the carbon-based carrier material is then subjected to a thermal aftertreatment, the carbon-based carrier material is then selectively oxidized using a reactive gas which contains at least one reactant, preferably carbon dioxide (CO2), ammonia (NH3), nitrogen dioxide (NO2), nitrogen monoxide (NO), and / or water vapor (H2O). The invention additionally relates to an electrochemical cell, preferably a fuel cell, in particular a PEM fuel cell.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Description

[0002] Method for producing a membrane-electrode assembly for an electrochemical cell

[0003] The invention relates to a method for producing a membrane electrode assembly for an electrochemical cell, preferably a fuel cell, in particular a PEM fuel cell.

[0004] State of the art

[0005] Fuel cells are electrochemical energy converters that convert the chemical energy stored in a fuel, such as hydrogen or methane, into electrical energy through an electrochemical reaction. When hydrogen is used as the energy source, the only byproduct produced during the conversion is water, which is why fuel cells are used primarily for emission-free drive systems in motor vehicles. Another area of ​​application is stationary power generation systems.

[0006] A widely used design is the polymer electrolyte membrane (PEM) fuel cell. This essentially consists of a membrane electrode assembly (MEA) in which a negative electrode, the anode, and a positive electrode, the cathode, are separated by a polymer electrolyte membrane. In combination with bipolar plates, which serve for gas supply and cooling, several membrane electrode assemblies can be connected in series to achieve the (high) voltage required for the respective end application.

[0007] The electrodes of an MEA typically consist of a porous, carbon-based support material on which nanometer-sized platinum or platinum alloy particles are deposited as a catalyst material. Since the catalyst material is a key factor in determining the performance of a fuel cell, performance can be improved by using larger amounts of platinum and / or by developing more active catalyst materials. The latter allows a reduction in the total amount of platinum required, which accounts for a significant portion of the manufacturing costs of a fuel cell.

[0008] The porous structure of the carbon-based support material of the electrode, especially the cathode, also determines performance. The respective reaction gas (hydrogen on the anode side, oxygen on the cathode side) reaches the catalyst material via the porous structure. In general, catalyst material particles located deep within the pores of the support material are better protected from adverse interactions with other electrode components and from aging. However, pores that are too deep and / or too narrow limit the transport of gas molecules to the catalyst material and thus restrict the performance of the fuel cell, especially at high current densities. Coal-based support materials with an unfavorable porous structure are also referred to as "poorly accessible carbons."Carbon-based support materials that allow the protection of the catalyst material in sufficiently large, non-transport-limiting pores are referred to as “accessible carbons”.

[0009] "Accessible carbons" can be produced synthetically through complex, multi-stage templating processes. In a subsequent step, the platinum-containing catalyst material is deposited onto this carbon. Alternatively, "poorly accessible carbons," whose pores already contain the particles of a catalyst material, can be converted into "accessible carbons" through thermal post-treatment. Thermal post-treatment requires a reactive gas that reacts with the carbon-based support material and etches it in a targeted manner, preferably in the immediate vicinity of the catalyst material particles. The previously transport-limiting pores can be expanded in this way without losing the protective effect mentioned above. Compared to templating processes, thermal post-treatment has the advantage of allowing the use of a significantly more cost-effective carbon-based support material.However, the high heat generation generated when using oxygen as the reactive gas proves to be a disadvantage. Without targeted removal of the reaction heat, the reaction accelerates, resulting in uncontrolled combustion of the carbon-based support material. Controlled reaction requires low temperatures, long reaction times, and small batch sizes, which limits the scale-up of thermal post-treatment.

[0010] The present invention is concerned with the object of providing a method for producing an electrochemical cell in which the carbon-based support material is subjected to a post-treatment to optimize the pore structure of an electrode of a membrane-electrode assembly. The method should enable controlled reaction control and be as simple and cost-effective as possible.

[0011] To achieve this objective, the method having the features of claim 1 is proposed. Advantageous developments of the invention are set forth in the subclaims. Furthermore, an electrochemical cell, preferably a fuel cell, in particular a PEM fuel cell, is specified.

[0012] Disclosure of the invention

[0013] In the proposed method for producing an electrochemical cell, preferably a fuel cell, in particular a PEM fuel cell, a catalyst material is deposited on a carbon-based support material having a porous structure to form an electrode of a membrane electrode assembly. The carbon-based support material is then subjected to a thermal post-treatment, wherein the carbon-based support material is selectively oxidized with the aid of a reactive gas containing at least one reactant, preferably carbon dioxide (CO2), ammonia (NH3), nitrogen dioxide (NO2), nitrogen monoxide (NO), and / or water vapor (H2O).

[0014] Selective oxidation is used to specifically remove carbon near the catalyst material. This means that the pores are expanded, improving gas transport to the catalyst material. The resulting optimization of the pore structure of the carbon-based support material leads to an increase in the performance of the embedded catalyst material and thus to an increase in the performance of the electrochemical cell produced using the process. Selective oxidation results in the pores near the catalyst material being expanded; in effect, a selective pore expansion occurs.

[0015] The expansion of the pores in the carbon-based support material can be demonstrated using nitrogen sorption measurements. In this case, defined amounts of nitrogen condense in the pores of the carbon-based support material. From these measurements, a pore size distribution can be determined, which shows the differential volume of pores with a certain diameter.

[0016] Current-voltage characteristics can be recorded to measure the performance of catalyst materials in fuel cells. The higher the cell potential at a defined current density, the more efficient the cell.

[0017] With the help of the proposed process, "poorly accessible coal" can be converted into "accessible coal." This means that a more cost-effective coal-based carrier material can be used. However, unlike the thermal post-treatment with oxygen described above, the proposed process does not generate heat, or only generates it to a significantly reduced extent, so that the reaction always remains controllable. In particular, self-acceleration of the reaction to the point of complete combustion of the coal-based carrier material is reliably prevented.

[0018] During thermal post-treatment with oxygen (O2), the reaction is highly exothermic because coal is burned. The reaction can be represented by the following equation:

[0019] (Eq. 1) C + O2^ CO2( H° = — 393 kj / mol)

[0020] In the case of selective oxidation using, for example, water vapor (H2O) as a reactant, the reaction is endothermic according to the following equation:

[0021] (Eq. 2) C + H20 -^ CO + H2( H° = +131 kj / mol) This applies analogously when using carbon dioxide (CO2) or ammonia (NH3) as reactant, whereby the following endothermic reactions take place:

[0022] (Eq. 3) C + C02^ 2 CO (H° = +172 kJ / mol)

[0023] If the reaction is endothermic, meaning it doesn't release heat, the thermal post-treatment process can be accelerated and / or shortened by increasing the temperature without the reaction getting out of control. In an endothermic reaction, selective oxidation is therefore easier to control. In a highly exothermic reaction, there is even a risk of the carbon-based support material burning off.

[0024] According to a preferred embodiment of the invention, the selective oxidation is therefore an endothermic reaction. Preferably, water vapor (H2O), carbon dioxide (CO2), and / or ammonia (NH3) are used as reactants, as these lead to an endothermic reaction.

[0025] According to a further preferred embodiment of the invention, the selective oxidation is a slightly exothermic reaction, where "slightly exothermic" is to be understood in contrast to the "strongly exothermic" reaction when oxygen (O2) is used as a reactant (see Equation 1 above). Although heat is also released in a slightly exothermic reaction, the amount of heat released is lower. This applies, for example, when the selective oxidation is carried out using nitrogen oxide (NO2) and / or nitrogen monoxide (NO) as a reactant.

[0026] To carry out the proposed process, nitrogen oxide (NO2) and / or nitrogen monoxide (NO) can also be used as reactants. Since the reaction is slightly exothermic, meaning only a small amount of heat is released, it remains controllable. Furthermore, further advantages can be achieved by incorporating nitrogen or nitrogen groups onto the carbon surface. The associated reactions are shown in the following equations: (Eq. 5) 280 kJ / mol)

[0027] (Eq. 6) J / mol

[0028] (Eq. 7) C + NO CO + 0.5 N2(AH° = -206 kJ / mol

[0029] (Eq. 8) C + 2 NO -> CO2 + 0.5 N2= -585 kJ / mol

[0030] It is further proposed that a gas mixture containing carbon dioxide (CO2), ammonia (NH3), nitrogen dioxide (NO2), nitrogen monoxide (NO), and / or water vapor (H2O) be used as a reactant. The aforementioned gases can therefore also be mixed, with the mixture or gas mixture containing at least two of the aforementioned gases as reactants. The mixing ratio or the respective concentration of the gases contained in the mixture then determines whether the selective reaction is endothermic or (slightly) exothermic.

[0031] In the case of an exothermic reaction, the amount of heat released during the selective oxidation is preferably controlled by the concentration of the at least one reactant in the reactive gas. This ensures that the reaction remains slightly exothermic and thus controllable. This applies both to the use of a gas mixture and to the use of a gas as a reactant. Preferably, however, the gas serving as a reactant is not present as a pure gas, but rather as a gas mixture comprising the reactant and an inert carrier gas.

[0032] Furthermore, it is proposed that a mass loss of the coal-based support material achieved via selective oxidation be controlled via the reaction temperature and / or the reaction time during the thermal aftertreatment. A higher reaction temperature with a constant reaction time leads to a greater relative mass loss, i.e., the pores are expanded more significantly. Furthermore, a defined mass loss can be achieved in a shorter time at a higher reaction temperature. This fungibility of the reaction parameters is only observed to a limited extent in the known thermal aftertreatment with oxygen, since at an excessively high reaction temperature, the self-acceleration of the reaction leads to an uncontrolled complete combustion of the coal-based support material.A reaction temperature in the range of 200 to 1000°C, preferably 300 to 700°C, and / or a reaction time between one minute and 24 hours, preferably between one hour and 24 hours, are selected. A shorter reaction time is particularly advantageous for the mass production of electrochemical cells. To shorten the reaction time, the reaction temperature should be as high as possible, which is fundamentally possible with the proposed process.

[0033] Furthermore, a carbon-based carrier material with a mass-related specific surface area between 200 and 2000 m 2 / g, preferably between 400 and 1000 m 2 / g. The mass-related specific surface area of ​​the support material allows conclusions to be drawn about the pore volume of the support material. For example, micropores with a pore size of up to 2 nm – with the same pore volume – have a larger mass-related specific surface area than mesopores with a pore size between 2 and 14 nm. Experiments with various carbon-based support materials have shown that selective oxidation leads to a slightly increased pore volume in micropores and a significantly increased pore volume in mesopores. The desired effect of pore expansion is therefore more pronounced in mesopores.

[0034] Platinum (Pt), ruthenium (Ru), rhodium (Rh), iridium (Ir), palladium (Pd), and / or an alloy thereof are preferably used as catalyst materials. Platinum is one of the most effective catalyst materials, so platinum is particularly preferred.

[0035] Furthermore, the carbon-based support material preferably contains 5 to 60 wt.% of the catalyst material, based on the total weight of the carbon-based support material, after deposition of the catalyst material and before thermal post-treatment. The presented processes produce advantageous pore expansion through selective oxidation in the vicinity of the catalyst material.

[0036] According to a further preferred embodiment of the invention, a gas mixture of water vapor (H2O) and an inert carrier gas, for example argon (Ar) and / or molecular nitrogen (N2), is used as the reactive gas. The process can thus be implemented particularly simply and cost-effectively.

[0037] Furthermore, to generate the gas mixture, the inert carrier gas is preferably passed through a water-filled humidifier. In the humidifier, the inert carrier gas absorbs water or water vapor. The gas mixture exiting the humidifier has a water vapor content corresponding to the saturation vapor pressure of the water at the humidifier temperature.

[0038] The temperature in the humidifier is preferably 10 to 100°C, more preferably 20 to 50°C. At a temperature of 10 to 100°C, the partial pressure of the water vapor in the gas stream is 1 to 100 kPa, and at a temperature of 20 to 50°C, it is 2 to 12 kPa. The reaction for the selective oxidation of the carbon-based support material can also be controlled via the partial pressure of the water vapor in the gas stream, which in turn depends on the temperature in the humidifier.

[0039] In principle, the temperature in the humidifier can exceed 100°C. In this case, the partial pressure of the water vapor can rise to over 100 kPa.

[0040] The thermal post-treatment of the coal-based support material is preferably carried out in a furnace through which the reactive gas is passed. The furnace allows for the setting of a defined reaction temperature and thus a controlled reaction process. Further reaction control is possible via the volume flow of the reactive gas, provided substoichiometric volume flows are introduced into the furnace. However, superstoichiometric volume flows are preferred to ensure homogeneous post-treatment of the coal-based support material.

[0041] Furthermore, an electrochemical cell, preferably a fuel cell, in particular a PEM fuel cell, is proposed, which has been manufactured according to a method according to the invention. The electrochemical cell is characterized by increased performance.

[0042] The invention and its advantages are explained in more detail below with reference to the accompanying drawings. These show: Fig. 1 a schematic representation of an experimental setup for the thermal post-treatment of a carbon-based carrier material,

[0043] Fig. 2 is a diagram showing the relative mass loss (%) during the thermal post-treatment as a function of the reaction temperature (°C),

[0044] Fig. 3 is a diagram showing the differential pore volume as a function of the respective pore size of a coal-based support material, (a) before thermal post-treatment and (b) after thermal post-treatment and

[0045] Fig. 4 is a diagram showing the current-voltage characteristics of a PEM fuel cell operated with hydrogen and air (21% oxygen in nitrogen) with a 5 cm 2 large active area, at 80°C, 95% relative humidity and 170 kPa a bs inlet pressure, (a) without thermal post-treatment and (b) with thermal post-treatment of the carbon-based cathode support material.

[0046] Detailed description of the drawings

[0047] Figure 1 shows an example of an experimental setup for the thermal post-treatment of a carbon-based support material 7 doped with a catalyst material. The experimental setup comprises a humidifier 2 and a furnace 5. The carbon-based support material 7 doped with the catalyst material is arranged in a quartz tube 6 of the furnace 5. For the thermal post-treatment of the carbon-based support material 7 doped with the catalyst material, a reactive gas is introduced into the furnace 5.

[0048] The reactive gas in this case is a gas mixture 4 generated in the humidifier 2. For this purpose, an inert gas 1 is introduced into the humidifier 2, which is filled with water 3. The inert gas 1 absorbs water 3 or water vapor in the humidifier 2, thus creating the gas mixture 4 serving as the reactive gas. With the aid of the gas mixture 4 introduced into the furnace 5, the carbon-based carrier material 7 is selectively oxidized. The selective oxidation can be controlled via the partial pressure of the water vapor in the gas mixture 4, the reaction temperature in the furnace 5, and the reaction duration. The partial pressure of the water vapor, in turn, depends on the temperature in the humidifier 2.

[0049] If another reactive gas is used for selective oxidation, such as carbon dioxide (CO2), the reactive gas can be introduced directly into the furnace 5. A humidifier 2 is then unnecessary.

[0050] The selective oxidation of the carbon-based support material 7 doped with the catalyst material is accompanied by a desired mass loss. Mass loss translates into a larger pore volume and thus improved gas transport capacity. The performance of the catalyst material and thus of the electrochemical cell increases accordingly. The mass loss can be controlled, among other things, by adjusting the reaction temperature. This temperature should be adjusted to avoid extreme mass losses, as these can have negative consequences.

[0051] As shown in Figure 2, the relative mass loss (%) depends on the reaction temperature (°C) and the reaction time, with measurements taken after 12 hours and after 1 hour, respectively. The higher the reaction temperature, the greater the mass loss, or the faster a given mass loss can be achieved. The relative mass loss in a non-reactive gas (here: argon) is represented by the hatched area in Figure 2.

[0052] The observed mass loss is accompanied by a widening of the pores in the carbon-based support material. This can be verified using nitrogen sorption measurements. A defined amount of nitrogen is condensed in the pores. The pore size distribution can then be determined from the measurements. As can be seen from Figure 3, the thermally post-treated carbon-based support material (curve (b)) exhibits a slightly increased pore volume in the micropore range (up to 2 nm) and a significantly increased pore volume in the mesopore range (between 2 and 14 nm) compared to the untreated starting material (curve (a)). The measurements thus demonstrate that the pores, especially the mesopores, were successfully widened.

[0053] Figure 4 also shows current-voltage characteristics that demonstrate the increased performance of an electrochemical cell manufactured using the proposed process. The higher the cell potential at a defined current density, the more efficient the cell.

[0054] In the range of low current densities (< 500 mA / cm 2 ), the achieved cell voltage (V) for the non-thermally treated starting material (curve (a)) and the thermally treated carbon-based support material (curve (b)) is practically identical. This indicates that the active catalyst material particles are located in pores of the support material in both cases and are protected from adverse interactions with other electrode components. In the range of higher current densities (> 1000 mA / cm 2), the thermally post-treated carbon-based support material achieves significantly higher cell voltages and thus a higher conversion efficiency of the hydrogen used. This can be explained by the improved gas transport capacity of the pores in the carbon-based support material, as these were expanded by the thermal post-treatment.

Claims

Claims 1 . A method for producing an electrochemical cell, preferably a fuel cell, in particular a PEM fuel cell, in which, to form an electrode of a membrane electrode assembly, a catalyst material is deposited on a carbon-based support material having a pore structure and then the carbon-based support material is subjected to a thermal aftertreatment, wherein the carbon-based support material is selectively oxidized with the aid of a reactive gas containing at least one reactant, preferably carbon dioxide (CO2), ammonia (NH3), nitrogen dioxide (NO2), nitrogen monoxide (NO) and / or water vapor (H2O).

2. Process according to claim 1, characterized in that the selective oxidation is an endothermic reaction.

3. Process according to claim 1 or 2, characterized in that water vapor (H2O), carbon dioxide (CO2) and / or ammonia (NH3) is / are used as reactant.

4. Process according to claim 1, characterized in that nitrogen dioxide (NO2) and / or nitrogen monoxide (NO) is / are used as reactant.

5. The method according to claim 1, characterized in that a gas mixture containing carbon dioxide (CO2), ammonia (NH3), nitrogen dioxide (NO2), nitrogen monoxide (NO) and / or water vapor (H2O) is used as reactant.

6. The method according to claim 4 or 5, characterized in that in the case of an exothermic reaction, the amount of heat released during the selective oxidation is controlled by the concentration of the at least one reactant in the reactive gas.

7. Process according to one of the preceding claims, characterized in that a mass loss of the carbon-based support material achieved via the selective oxidation is controlled via the reaction temperature and / or the reaction time during the thermal aftertreatment.

8. Process according to claim 1, characterized in that a reaction temperature in the range from 200 to 1000°C, preferably from 300 to 700°C, and / or a reaction time between one minute and 24 hours, preferably between 1 hour and 24 hours, is / are selected.

9. Method according to one of the preceding claims, characterized in that a carbon-based carrier material with a mass-related specific surface area between 200 and 2000 m 2 / g, preferably between 400 and 1000 m 2 / g, is used.

10. Process according to one of the preceding claims, characterized in that platinum (Pt), ruthenium (Ru), rhodium (Rh), iridium (Ir), palladium (Pd) and / or an alloy thereof is used as catalyst material.

11. Process according to one of the preceding claims, characterized in that the carbon-based support material, after deposition of the catalyst material and before thermal aftertreatment, contains 5 to 60 wt.% of the catalyst material based on the total weight of the carbon-based support material.

12. Method according to one of the preceding claims, characterized in that a gas mixture of water vapor (H2O) and an inert carrier gas, for example argon (Ar) and / or molecular nitrogen (N2), is used as the reactive gas.

13. A method according to claim 12, characterized in that to generate the gas mixture, the inert Carrier gas is passed through a humidifier filled with water, the temperature in the humidifier preferably being 10 to 100°C, further preferably 20 to 50°C.

14. A method according to any one of the preceding claims, characterized in that the thermal aftertreatment of the coal-based carrier material is carried out in a furnace through which the Reactive gas is passed.

15. Electrochemical cell, preferably fuel cell, in particular PEM fuel cell manufactured by a process according to any one of the preceding claims.

Citation Information

Patent Citations

  • Oxidative Control of Pore Structure in Carbon-Supported PGM-Based Catalysts

    US20170033368A1