Semiconductor device, and method for manufacturing semiconductor device
The semiconductor device with a vertical transistor configuration and optimized gate insulating layer structure addresses the limitations of existing devices by enhancing electrical performance, miniaturization, and integration, achieving improved breakdown voltage and on-state current for efficient and reliable semiconductor devices.
Patent Information
- Application Number
- PCT/IB2024/054222
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-02-27
- Filing Date
- 2024-05-02
- Publication Date
- 2024-11-14
AI Technical Summary
Current semiconductor devices face challenges in achieving high electrical performance, miniaturization, and low power consumption due to limitations in gate insulating layer breakdown voltage, parasitic capacitance, and on-state current, while also requiring improved manufacturing methods for higher integration and reliability.
A semiconductor device with a vertical transistor configuration, featuring a gate insulating layer with specific thickness distributions and anisotropic deposition methods, and a semiconductor layer structure that enhances contact resistance and reduces parasitic capacitance, allowing for miniaturization and high integration.
The solution provides improved electrical characteristics, increased breakdown voltage, reduced parasitic capacitance, and enhanced on-state current, enabling the development of smaller, more reliable semiconductor devices with lower power consumption and higher integration density.
Smart Images

Figure IB2024054222_14112024_PF_FP_ABST
Abstract
Description
Semiconductor device and method for manufacturing the same
[0001] 1. Field of the Invention One embodiment of the present invention relates to a semiconductor device, a memory device, a display device, and an electronic device. Another embodiment of the present invention relates to a manufacturing method of a semiconductor device.
[0002] One embodiment of the present invention is not limited to the above technical field, and examples of the technical field of one embodiment of the present invention include semiconductor devices, display devices, light-emitting devices, power storage devices, memory devices, electronic devices, lighting devices, input devices (e.g., touch sensors), input / output devices (e.g., touch panels), driving methods thereof, and manufacturing methods thereof.
[0003] In this specification and the like, a semiconductor device is a device that utilizes semiconductor characteristics, and refers to a circuit including a semiconductor element (transistor, diode, photodiode, etc.), a device having such a circuit, etc. Also, it refers to any device that can function by utilizing semiconductor characteristics. For example, an integrated circuit, a chip including an integrated circuit, and an electronic component in which a chip is housed in a package are examples of semiconductor devices. Furthermore, a memory device, a display device, a light-emitting device, a lighting device, and an electronic device may themselves be semiconductor devices and each may have a semiconductor device.
[0004] In recent years, the development of semiconductor devices has progressed, and large scale integration (LSI), central processing units (CPU), memories, etc. are mainly used in semiconductor devices. A CPU is an assembly of semiconductor elements that have semiconductor integrated circuits (at least transistors and memories) formed into chips by processing a semiconductor wafer and on which electrodes serving as connection terminals are formed.
[0005] 2. Description of the Related Art Semiconductor circuits (IC chips) such as LSIs, CPUs, and memories are mounted on circuit boards, such as printed wiring boards, and are used as components of various electronic devices.
[0006] Furthermore, a technology for constructing a transistor using a semiconductor thin film formed on a substrate having an insulating surface has attracted attention. Such transistors are widely applied to electronic devices such as integrated circuits (ICs) and display devices. While silicon-based semiconductor materials are widely known as semiconductor thin films applicable to transistors, oxide semiconductors have also attracted attention as other materials.
[0007] Furthermore, it is known that a transistor using an oxide semiconductor has an extremely small leakage current in an off state. For example, Patent Document 1 discloses a CPU with low power consumption that utilizes the property of a transistor using an oxide semiconductor having a small leakage current. Furthermore, Patent Document 2 discloses a memory device that can retain stored data for a long period of time by utilizing the property of a transistor using an oxide semiconductor having a small leakage current.
[0008] In addition, with the recent trend toward smaller and lighter electronic devices, there is an increasing demand for higher density integrated circuits. There is also a demand for improved productivity of semiconductor devices including integrated circuits. For example, Patent Document 3 and Non-Patent Document 1 disclose a technique for increasing the density of integrated circuits by stacking a first transistor using an oxide semiconductor film and a second transistor using an oxide semiconductor film to provide multiple memory cells in an overlapping manner. Patent Document 4 discloses a technique for increasing the density of integrated circuits by vertically arranging the channel of a transistor using an oxide semiconductor film.
[0009] JP 2012-257187 A JP 2011-151383 A WO 2021 / 053473 JP 2013-211537 A
[0010] M. Oota et. al, “3D-Stacked CAAC-In-Ga-Zn Oxide FETs with Gate Length of 72nm”, IEDM Tech. Dig. , 2019, pp. 50-53
[0011] An object of one embodiment of the present invention is to provide a transistor with favorable electrical characteristics. Another object of one embodiment of the present invention is to provide a transistor having a high withstand voltage of a gate insulating layer. Another object of one embodiment of the present invention is to provide a transistor with low parasitic capacitance. Another object of one embodiment of the present invention is to provide a transistor with high on-state current. Another object of one embodiment of the present invention is to provide a transistor, a semiconductor device, or a memory device that can be miniaturized or highly integrated. Another object of one embodiment of the present invention is to provide a display device with high definition or a high aperture ratio. Another object of one embodiment of the present invention is to provide a highly reliable transistor, a semiconductor device, a display device, or a memory device. Another object of one embodiment of the present invention is to provide a semiconductor device, a display device, or a memory device with low power consumption. Another object of one embodiment of the present invention is to provide a memory device with high operating speed. Another object of one embodiment of the present invention is to provide a manufacturing method of the transistor, the semiconductor device, the display device, or the memory device.
[0012] Note that the description of these problems does not preclude the existence of other problems. One embodiment of the present invention does not necessarily have to solve all of these problems. Problems other than these can be extracted from the description in the specification, drawings, and claims.
[0013] One embodiment of the present invention includes a first transistor and a first insulating layer. The first transistor includes a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer, and a gate electrode. The first conductive layer serves as one of a source electrode and a drain electrode of the first transistor, and the second conductive layer serves as the other of the source electrode and the drain electrode of the first transistor. The first conductive layer and the second conductive layer are located at different heights. The first insulating layer is provided between the first conductive layer and the second conductive layer. The gate electrode overlaps with the semiconductor layer with the gate insulating layer interposed therebetween and has a first opening reaching the first conductive layer. The second conductive layer is provided on the first insulating layer. the semiconductor layer has a first region covering an upper surface of the first conductive layer in the first opening, a second region covering a side surface of the first insulating layer in the first opening, and a third region covering an upper surface of the second conductive layer and overlapping with the gate electrode; the gate insulating layer has a fourth region facing a side wall of the first opening of the first insulating layer with the second region sandwiched therebetween, a fifth region covering an upper surface of the third region, and a sixth region covering an upper surface of the second conductive layer and positioned outward from an end of the gate electrode in a top view; and the film thickness of the fifth region is thicker than the film thickness of the fourth region, and the film thickness of the fifth region is thicker than the film thickness of the sixth region.
[0014] In the above aspect, the film thickness of the fifth region is preferably at least 2 nm thicker than the film thickness of the sixth region.
[0015] In the above aspect, the film thickness of the sixth region is preferably 1.0 nm or more and 100 nm or less.
[0016] In the above aspect, the film thickness of the fourth region is preferably 0.1 nm or more and 7.0 nm or less.
[0017] In the above embodiment, the semiconductor layer preferably has a region that covers the top surface of the second conductive layer and is covered by the sixth region.
[0018] In the above aspect, it is preferable that the second conductive layer has a second opening overlapping the first opening, the semiconductor layer has a region covering the side surface of the second conductive layer within the second opening, and the first insulating layer has a region covering the second opening with the semiconductor layer sandwiched therebetween.
[0019] Alternatively, one embodiment of the present invention includes forming a first insulating layer on a first conductive layer, forming a second conductive layer on the first insulating layer, forming a first opening that reaches the first conductive layer by removing a part of the second conductive layer and a part of the first insulating layer to expose an upper surface of the first conductive layer, forming a first semiconductor layer so as to be in contact with the upper surface of the first conductive layer, a side surface of the first insulating layer in the first opening, a side surface of the second conductive layer in the first opening, and an upper surface of the second conductive layer, respectively, and forming a second insulating layer so as to be in contact with the upper surface of the first semiconductor layer and the upper surface of the first insulating layer, and the second insulating layer is formed using a method having anisotropy in the deposition rate. the second insulating layer is formed so that a thickness of a region covering a side surface of the first opening with the first semiconductor layer sandwiched therebetween is thinner than a thickness of a region covering a top surface of the first conductive layer; a third conductive layer is formed on the second insulating layer; a first mask is formed by photolithography; dry etching is performed using the first mask; and a fourth conductive layer is formed by removing a part of the third conductive layer by dry etching; and the thickness of a portion of the second insulating layer that is not covered by the first mask is reduced by dry etching in the region covering the top surface of the first conductive layer.
[0020] In the above embodiment, the second insulating layer is preferably formed by ionization sputtering.
[0021] In the above embodiment, the second insulating layer is preferably formed by using a long throw sputtering method.
[0022] In the above aspect, the second insulating layer is preferably formed by using a plasma enhanced chemical vapor deposition method.
[0023] According to one embodiment of the present invention, a transistor with favorable electrical characteristics can be provided. According to another embodiment of the present invention, a transistor having a high withstand voltage of a gate insulating layer can be provided. According to another embodiment of the present invention, a transistor with low parasitic capacitance can be provided. According to another embodiment of the present invention, a transistor with high on-state current can be provided. According to another embodiment of the present invention, a transistor, a semiconductor device, or a memory device that can be miniaturized or highly integrated can be provided. According to another embodiment of the present invention, a display device with high definition or a high aperture ratio can be provided. According to another embodiment of the present invention, a highly reliable transistor, a semiconductor device, a display device, or a memory device can be provided. According to another embodiment of the present invention, a semiconductor device, a display device, or a memory device with low power consumption can be provided. According to another embodiment of the present invention, a memory device with high operating speed can be provided. According to another embodiment of the present invention, a manufacturing method of the above-described transistor, semiconductor device, display device, or memory device can be provided.
[0024] Note that the description of these effects does not preclude the existence of other effects. One embodiment of the present invention does not necessarily have all of these effects. Effects other than these can be extracted from the description in the specification, drawings, and claims.
[0025] FIG. 1A is a plan view showing an example of a semiconductor device. FIGS. 1B and 1C are cross-sectional views showing an example of a semiconductor device. FIG. 2A is a cross-sectional view showing an example of a semiconductor device. FIG. 2B is a plan view showing an example of a semiconductor device. FIGS. 3A and 3B are cross-sectional views showing an example of a semiconductor device. FIG. 4 is a cross-sectional view showing an example of a semiconductor device. FIGS. 5A and 5B are cross-sectional views showing an example of a method for manufacturing a semiconductor device. FIGS. 6A and 6B are cross-sectional views showing an example of a method for manufacturing a semiconductor device. FIGS. 7A and 7B are cross-sectional views showing an example of a method for manufacturing a semiconductor device. FIG. 8A is a plan view showing an example of a semiconductor device. FIGS. 8B and 8C are cross-sectional views showing an example of a semiconductor device. FIGS. 9A and 9B are cross-sectional views showing an example of a method for manufacturing a semiconductor device. FIGS. 10A to 10C are cross-sectional views showing an example of a method for manufacturing a semiconductor device. FIGS. 11A and 11B are cross-sectional views showing an example of a method for manufacturing a semiconductor device. FIGS. 12A to 12C are cross-sectional views showing an example of a method for manufacturing a semiconductor device. FIG. 13 is a cross-sectional view showing an example of a semiconductor device. 14A to 14C are cross-sectional views illustrating an example of a manufacturing method of a semiconductor device. FIGS. 15A to 15C are cross-sectional views illustrating an example of a manufacturing method of a semiconductor device. FIG. 16A is a plan view illustrating an example of a memory device. FIGS. 16B and 16C are cross-sectional views illustrating an example of a memory device. FIG. 17A is a plan view illustrating an example of a memory device. FIG. 17B is a cross-sectional view illustrating an example of a memory device. FIG. 18 is a cross-sectional view illustrating an example of a memory device. FIG. 19 is a cross-sectional view illustrating an example of a memory device. FIG. 20 is a block diagram illustrating a configuration example of a semiconductor device. FIGS. 21A to 21H are diagrams illustrating an example of a circuit configuration of a memory cell. FIGS. 22A and 22B are perspective views illustrating an example of a configuration of a semiconductor device. FIG. 23 is a block diagram illustrating a CPU. FIGS. 24A and 24B are perspective views of a semiconductor device. FIGS. 25A and 25B are perspective views of a semiconductor device. FIGS. 26A and 26B are diagrams illustrating various memory devices by layer. FIGS. 27A and 27B are perspective views of an example of a display device. FIG. 28 is a cross-sectional view of an example of a display device. Fig. 29 is a cross-sectional view showing an example of a display device. Fig. 30A to Fig. 30C are diagrams showing an example of the configuration of a display device.Figs. 31A and 31B are diagrams showing an example of an electronic component. Figs. 32A to 32C are diagrams showing an example of a mainframe computer. Fig. 32D is a diagram showing an example of space equipment. Fig. 32E is a diagram showing an example of a storage system applicable to a data center. Figs. 33A to 33F are diagrams showing an example of electronic equipment. Figs. 34A to 34G are diagrams showing an example of electronic equipment. Figs. 35A to 35F are diagrams showing an example of electronic equipment. Fig. 36 is a cross-sectional view showing an example of a display device.
[0026] The embodiments will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various changes can be made in form and detail without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0027] In the configuration of the invention described below, the same parts or parts having similar functions are denoted by the same reference numerals in different drawings, and repeated explanations thereof will be omitted. Furthermore, when referring to similar functions, the same hatching pattern may be used and no particular reference numeral may be assigned.
[0028] Furthermore, for ease of understanding, the position, size, range, etc. of each component shown in the drawings may not represent the actual position, size, range, etc. Therefore, the disclosed invention is not necessarily limited to the position, size, range, etc. disclosed in the drawings.
[0029] In this specification, the ordinal numbers "first" and "second" are used for convenience and do not limit the number of components or the order of the components (for example, the order of processes or the order of stacking). Furthermore, the ordinal numbers assigned to components in one part of this specification may not match the ordinal numbers assigned to the same components in other parts of this specification or in the claims.
[0030] A transistor is a type of semiconductor element that can amplify current or voltage, and perform a switching operation to control conduction or non-conduction. The term "transistor" as used herein includes an insulated gate field effect transistor (IGFET) and a thin film transistor (TFT).
[0031] In this specification and the like, a transistor using an oxide semiconductor or a metal oxide for a semiconductor layer and a transistor having an oxide semiconductor or a metal oxide for a channel formation region may be referred to as an OS transistor. A transistor having silicon for a channel formation region may be referred to as a Si transistor.
[0032] In this specification and the like, a transistor is an element having at least three terminals including a gate, a drain, and a source. A transistor has a region (also referred to as a channel formation region) where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode), and current can flow between the source and the drain through the channel formation region. Note that in this specification and the like, the channel formation region refers to a region through which current mainly flows.
[0033] Furthermore, the functions of "source" and "drain" may be interchangeable when transistors of different polarities are used, or when the direction of current flow changes during circuit operation, etc. For this reason, the terms "source" and "drain" may be used interchangeably in this specification.
[0034] Note that impurities in a semiconductor refer to, for example, elements other than the main components constituting the semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be considered an impurity. The presence of impurities may increase the density of defect states in the semiconductor or reduce the crystallinity, for example. When the semiconductor is an oxide semiconductor, impurities that change the characteristics of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor. Specific examples include hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, and nitrogen. Note that water may also function as an impurity. For example, the inclusion of impurities may cause oxygen deficiency (V) in the oxide semiconductor. O In some cases, a nucleus (also referred to as a nucleus) may be formed.
[0035] In this specification and the like, an oxynitride refers to a material having a composition in which oxygen is contained in a larger amount than nitrogen, and a nitride oxide refers to a material having a composition in which nitrogen is contained in a larger amount than oxygen.
[0036] To analyze the content of elements such as hydrogen, oxygen, carbon, and nitrogen contained in a film, for example, secondary ion mass spectrometry (SIMS) or X-ray photoelectron spectroscopy (XPS) can be used. XPS is suitable when the content of the target element is high (e.g., 0.5 atomic% or more, or 1 atomic% or more). On the other hand, SIMS is suitable when the content of the target element is low (e.g., 0.5 atomic% or less, or 1 atomic% or less). When comparing the content of elements, it is more preferable to perform a combined analysis using both SIMS and XPS analytical techniques.
[0037] The terms "film" and "layer" can be interchangeable depending on the circumstances. For example, the term "conductive layer" can be changed to the term "conductive film." Or, for example, the term "insulating film" can be changed to the term "insulating layer."
[0038] Furthermore, in this specification, "parallel" refers to a state in which two straight lines are arranged at an angle of -10 degrees or more and 10 degrees or less. Therefore, it also includes cases in which the angle is -5 degrees or more and 5 degrees or less. Furthermore, "substantially parallel" refers to a state in which two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. Furthermore, "perpendicular" refers to a state in which two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it also includes cases in which the angle is 85 degrees or more and 95 degrees or less. Furthermore, "substantially perpendicular" refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less.
[0039] In this specification, "electrically connected" includes connection via "something that has some kind of electrical function." Here, "something that has some kind of electrical function" is not particularly limited as long as it allows electrical signals to be transmitted and received between the connected objects. For example, "something that has some kind of electrical function" includes electrodes or wiring, as well as switching elements such as transistors, resistive elements, coils, and other elements with various functions.
[0040] In this specification and the like, unless otherwise specified, the off-state current refers to the leakage current between the source and drain when the transistor is in an off state (also referred to as a non-conducting state or a cut-off state). Unless otherwise specified, the off-state current refers to the leakage current between the source and the gate when the voltage V gs is the threshold voltage V th (For p-channel transistors, V th This refers to a state of being (higher than)
[0041] In this specification, the term "normally-on" refers to a state in which a channel exists and a current flows through a transistor even when no voltage is applied to the gate, whereas the term "normally-off" refers to a state in which no current flows through a transistor when no potential is applied to the gate or when a ground potential is applied to the gate.
[0042] In this specification, the top surface shape of a certain component refers to the contour shape of the component in a plan view. The plan view refers to a view from the normal direction of the surface on which the component is formed or the surface of a support (e.g., a substrate) on which the component is formed.
[0043] In this specification, the phrase "top surface shapes that are approximately the same" refers to at least a portion of the contours of stacked layers overlapping. For example, this includes cases where the upper and lower layers are processed using the same mask pattern or a portion of the same mask pattern. However, strictly speaking, the contours may not overlap, and the upper layer may be located inside the lower layer, or the upper layer may be located outside the lower layer. In these cases, the phrase "top surface shapes that are approximately the same" may also be used. Furthermore, when the top surface shapes are the same or approximately the same, it can also be said that the edges are aligned or approximately aligned, or that the side edges are aligned or approximately aligned.
[0044] In this specification, a tapered shape refers to a shape in which at least a portion of the side surface of a structure is inclined relative to the substrate surface or the surface to be formed. For example, it is preferable to have a region in which the angle (also called the taper angle) between the inclined side surface and the substrate surface or the surface to be formed is greater than 0 degrees and less than 90 degrees. The side surface of the structure, the substrate surface, and the surface to be formed do not necessarily need to be completely flat, and may be approximately planar with a slight curvature or approximately planar with a slight unevenness.
[0045] In this specification and the like, when it is stated that A is in contact with B, it means that at least a part of A is in contact with B. Therefore, for example, it can be rephrased as saying that A has a region in contact with B.
[0046] In this specification and the like, when it is stated that A is located on B, it means that at least a part of A is located on B. Therefore, for example, it can be rephrased as, A has a region located on B.
[0047] In this specification and the like, when it is stated that A covers B, it means that at least a part of A covers B. Therefore, for example, it can be rephrased as saying that A has a region that covers B.
[0048] In this specification and the like, when it is stated that A overlaps with B, it means that at least a part of A overlaps with B. Therefore, for example, it can be rephrased as saying that A has an overlapping region with B.
[0049] In this specification, etc., a device fabricated using a metal mask or an FMM (fine metal mask, high-resolution metal mask) may be referred to as a device with an MM (metal mask) structure. Also, in this specification, etc., a device fabricated without using a metal mask or an FMM may be referred to as a device with an MML (metal maskless) structure.
[0050] In this specification and the like, a structure in which different light-emitting layers are formed for light-emitting elements (also referred to as light-emitting devices) with different emission wavelengths is sometimes referred to as an SBS (Side By Side) structure. The SBS structure allows the materials and configuration to be optimized for each light-emitting element, increasing the degree of freedom in selecting materials and configurations and making it easier to improve brightness and reliability.
[0051] In this specification and the like, holes or electrons may be referred to as "carriers." Specifically, a hole injection layer or an electron injection layer may be referred to as a "carrier injection layer," a hole transport layer or an electron transport layer may be referred to as a "carrier transport layer," and a hole block layer or an electron block layer may be referred to as a "carrier block layer." Note that the above-mentioned carrier injection layer, carrier transport layer, and carrier block layer may not be clearly distinguishable. Furthermore, one layer may have two or three functions among the carrier injection layer, carrier transport layer, and carrier block layer.
[0052] In this specification and the like, a light-emitting element has an EL layer between a pair of electrodes. The EL layer has at least a light-emitting layer. Here, examples of layers (also referred to as functional layers) included in the EL layer include a light-emitting layer, a carrier injection layer (a hole injection layer and an electron injection layer), a carrier transport layer (a hole transport layer and an electron transport layer), and a carrier block layer (a hole block layer and an electron block layer). In this specification and the like, a light-receiving element (also referred to as a light-receiving device) has at least an active layer that functions as a photoelectric conversion layer between a pair of electrodes. In this specification and the like, one of the pair of electrodes may be referred to as a pixel electrode, and the other as a common electrode.
[0053] In this specification and the like, the sacrificial layer (which may also be referred to as a mask layer) is located above at least the light-emitting layer (more specifically, a layer that is processed into an island shape among the layers that make up the EL layer), and has the function of protecting the light-emitting layer during the manufacturing process.
[0054] In this specification, the term "island-like" refers to a state in which two or more layers made of the same material and formed in the same process are physically separated. For example, an island-like EL layer refers to a state in which the EL layer is physically separated from an adjacent EL layer.
[0055] In this specification and the like, a step disconnection refers to a phenomenon in which a layer, a film, or an electrode is separated due to the shape of the surface on which it is formed (for example, a step or the like).
[0056] In the drawings and the like relating to this specification, arrows indicating the X direction, Y direction, and Z direction may be used. In this specification and the like, the "X direction" refers to the direction along the X axis, and there may be no distinction between the forward direction and the reverse direction unless explicitly stated. The same applies to the "Y direction" and the "Z direction." The X direction, Y direction, and Z direction are directions that intersect with each other. For example, the X direction, Y direction, and Z direction are directions that are perpendicular to each other.
[0057] Embodiment 1 In this embodiment, a semiconductor device of one embodiment of the present invention will be described.
[0058] A semiconductor device of one embodiment of the present invention includes a first conductive layer, a second conductive layer, a third conductive layer, an oxide semiconductor layer, a first insulating layer, and a second insulating layer.
[0059] The first insulating layer is located over the first conductive layer, and the second conductive layer is located over the first insulating layer. The first insulating layer and the second conductive layer have openings that reach the first conductive layer. The oxide semiconductor layer is in contact with at least a top surface of the first conductive layer, a side surface of the first insulating layer, and a side surface of the second conductive layer in the openings. The second insulating layer is located over the oxide semiconductor layer in the openings. The third conductive layer overlaps with the oxide semiconductor layer in the openings, with the second insulating layer interposed therebetween. Note that the openings are also referred to as openings.
[0060] The first conductive layer functions as one of a source electrode and a drain electrode of the transistor, the second conductive layer functions as the other of the source electrode and the drain electrode of the transistor, the third conductive layer functions as a gate electrode of the transistor, and the second insulating layer functions as a gate insulating layer.
[0061] In this specification, the term "in a cross-sectional view" is used, but it can be specifically rephrased as "in a cross-sectional view from the same direction." For example, when explaining the relationship between multiple components, the relationship in a cross-sectional view from the same direction is explained. In this case, the relationship between the multiple components can be explained using one cross-sectional view.
[0062] In a transistor according to one embodiment of the present invention, a source electrode and a drain electrode are located at different heights, and a current flows in a semiconductor layer in the height direction. That is, it can be said that the channel length direction has a component in the height direction (vertical direction). Therefore, the transistor according to one embodiment of the present invention can also be called a VFET (Vertical Field Effect Transistor), a vertical transistor, a vertical channel transistor, a vertical channel transistor, or the like.
[0063] In the transistor of one embodiment of the present invention, a source electrode, a semiconductor layer, and a drain electrode can be provided so as to overlap with each other; therefore, the area occupied by the transistor can be significantly reduced compared to a so-called planar transistor in which a semiconductor layer is arranged in a planar shape.
[0064] In this specification, "edges coincide" means that, in a plan view, at least a portion of the contours of stacked layers overlap. For example, this includes cases where the upper and lower layers are processed using the same mask pattern or a portion of the same mask pattern. However, strictly speaking, the contours may not overlap, and the contour of the upper layer may be located inside the contour of the lower layer, or the contour of the upper layer may be located outside the contour of the lower layer. In these cases, the term "edges coincide" is also used.
[0065] In general, it may be difficult to clearly distinguish between an "exact match" and an "approximate match." For this reason, in this specification and elsewhere, "match" may include both an exact match and an approximate match.
[0066] <Structural Example 1 of Semiconductor Device> The structure of a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. 1A to 3B . FIG. 1A is a plan view of a semiconductor device including a transistor 200. FIG. 1B is a cross-sectional view taken along dash-dotted line A1-A2 in FIG. 1A . FIG. 1C is a cross-sectional view taken along dash-dotted line A3-A4 in FIG. 1A . FIG. 2A is an enlarged view of a region surrounded by a two-dot dashed line in FIG. 1B . FIG. 2B is a cross-sectional view in the XY plane including an insulating layer 280. Note that some elements are omitted in the plan view of FIG. 1A for clarity. Some elements may also be omitted in the subsequent plan views.
[0067] 1A to 1C, 2A, and 2B includes an insulating layer 210 over a substrate (not shown), a transistor 200 over the insulating layer 210, an insulating layer 280 over the insulating layer 210, and an insulating layer 283 over the transistor 200. The insulating layer 210, the insulating layer 280, and the insulating layer 283 function as interlayer films.
[0068] The transistor 200 includes a conductive layer 220, a conductive layer 240 over an insulating layer 280, an oxide semiconductor layer 230, an insulating layer 250 over the oxide semiconductor layer 230, and a conductive layer 260 over the insulating layer 250. The conductive layer 220 and the conductive layer 240 are located at different heights. An insulating layer 283 covers the top surface and side surfaces of the conductive layer 260. Note that although FIGS. 1B and 1C show an example in which the conductive layer 260 is formed as a two-layer stack of a conductive layer 260a and a conductive layer 260b over the conductive layer 260a, the conductive layer 260 may be formed as a single layer or as a three-layer or more layer structure.
[0069] 1B and 1C , an opening 290 is provided in the insulating layer 280 and the conductive layer 240, reaching the conductive layer 220. Here, the bottom of the opening 290 is the upper surface of the conductive layer 220, and the sidewalls of the opening 290 are the side surfaces of the insulating layer 280 and the conductive layer 240. The opening 290 includes an opening in the insulating layer 280 and an opening in the conductive layer 240. In other words, the opening in the region where the insulating layer 280 overlaps with the conductive layer 220 is one part of the opening 290, and the opening in the region where the conductive layer 240 overlaps with the conductive layer 220 is another part of the opening 290. Of the openings 290, the opening 290 provided in the insulating layer 280 is referred to as opening 290a, and the opening 290 provided in the conductive layer 240 is referred to as opening 290b.
[0070] At least some of the components of the transistor 200 are disposed inside the opening 290. Specifically, the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are disposed such that at least a portion thereof is located inside the opening 290. Within the opening 290, the oxide semiconductor layer 230 contacts the top surface of the conductive layer 220, the side surface of the insulating layer 280, and the side surface of the conductive layer 240.
[0071] Furthermore, the portions of the oxide semiconductor layer 230 and the insulating layer 250 that are disposed inside the opening 290 are provided to reflect the shape of the opening 290. Specifically, the oxide semiconductor layer 230 is provided so as to cover the bottom and sidewalls of the opening 290, and the insulating layer 250 is provided so as to cover the oxide semiconductor layer 230. Then, the conductive layer 260 is provided so as to fill the recess in the insulating layer 250 that reflects the shape of the opening 290. The oxide semiconductor layer 230 is preferably provided so as to contact the sidewall of the insulating layer 280 in the opening 290a. Furthermore, the insulating layer 250 is disposed so as to face the sidewall of the insulating layer 280 in the opening 290a, with the oxide semiconductor layer 230 sandwiched therebetween.
[0072] The width of the opening 290 is defined as width D. Width D may vary in the depth direction. For example, width D may be the width at the top end of the opening 290 in the insulating layer 280. Alternatively, width D may be the width at the bottom end. Alternatively, width D may be the width at half the depth of the opening 290 in the insulating layer 280. Alternatively, width D may be the width of the opening 290 in the conductive layer 240.
[0073] A region of the oxide semiconductor layer 230 in contact with the conductive layer 240 may function as a low-resistance region.
[0074] In the transistor 200, the oxide semiconductor layer 230 functions as a semiconductor layer, the conductive layer 260 functions as a gate electrode, the insulating layer 250 functions as a gate insulating layer, the conductive layer 220 functions as one of a source electrode and a drain electrode, and the conductive layer 240 functions as the other of the source electrode and the drain electrode.
[0075] As described above, the oxide semiconductor layer 230 is provided inside the opening 290 of the insulating layer 280. The transistor 200 has a structure in which one of the source electrode and the drain electrode (the conductive layer 220 here) is located below and the other of the source electrode and the drain electrode (the conductive layer 240 here) is located above, and thus, a current flows vertically. That is, a channel is formed along the sidewall of the opening of the insulating layer 280.
[0076] The oxide semiconductor layer 230 contacts the upper surface of the conductive layer 220 and the side surface of the conductive layer 240 inside the opening 290. The oxide semiconductor layer 230 also contacts a part of the upper surface of the conductive layer 240. In this way, the oxide semiconductor layer 230 contacts not only the side surface but also the upper surface of the conductive layer 240, so that the contact area between the oxide semiconductor layer 230 and the conductive layer 240 can be made larger compared to, for example, a case where the oxide semiconductor layer 230 contacts the side surface of the conductive layer 240 but not the upper surface. Therefore, the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced.
[0077] The conductive layer 240 has an opening 290b in a region overlapping with the conductive layer 220. Furthermore, the conductive layer 240 is preferably not provided inside the opening 290a of the insulating layer 280. That is, the conductive layer 240 preferably does not have a region in contact with the side surface of the insulating layer 280 in the opening 290a. With this structure, the opening 290b of the conductive layer 240 and the opening 290a of the insulating layer 280 can be formed simultaneously. Furthermore, by configuring the side surface of the conductive layer 240 in the opening 290b to coincide or substantially coincide with the side surface of the insulating layer 280 in the opening 290a, the film thickness distribution of the oxide semiconductor layer 230 provided inside the opening 290 can be made uniform. Furthermore, the oxide semiconductor layer 230 can be prevented from being divided by a step between the conductive layer 240 and the insulating layer 280.
[0078] The conductive layer 260 has a region located on the insulating layer 280. In Figures 1B and 1C, the conductive layer 260 has regions on the insulating layer 280 that cover the conductive layer 240, the oxide semiconductor layer 230, and the insulating layer 250, respectively.
[0079] Furthermore, it is preferable that the conductive layer 240 has a region that is not covered by the conductive layer 260. In the region that does not overlap with the conductive layer 260, the end of the conductive layer 240 is located outside the end of the conductive layer 260. In the region of the conductive layer 240 that does not overlap with the conductive layer 260, a conductive layer can be provided on top of the region, and the conductive layer and the conductive layer 240 can be electrically connected.
[0080] 1B shows a configuration in which the end of the conductive layer 240 is located outside the opening 290, further outward than the end of the conductive layer 260. With this configuration, a plug or the like can be provided on a region of the conductive layer 240 that extends outward than the conductive layer 260, and electrically connected to conductive layers such as wiring and electrodes located above the conductive layer 240 and the conductive layer 260.
[0081] 3A shows an example of a semiconductor device including an insulating layer 283 over a transistor 200, an insulating layer 285 over the insulating layer 283, a conductive layer 661 provided to penetrate the insulating layer 250, the insulating layer 283, and the insulating layer 285, and a conductive layer 662 over the conductive layer 661 and the insulating layer 285. The conductive layer 661 is preferably provided in contact with a top surface of the conductive layer 240. The conductive layer 240 is electrically connected to the conductive layer 662 through the conductive layer 661.
[0082] The insulating layer 250 is provided in contact with the top surface of the oxide semiconductor layer 230. The insulating layer 250 preferably has a region in contact with the top surface of the conductive layer 240, a region in contact with the side surface of the conductive layer 240, and a region in contact with the top surface of the insulating layer 280.
[0083] The sidewalls of the opening 290 are preferably perpendicular to the top surface of the insulating layer 210. Such a configuration enables miniaturization or high integration of the semiconductor device. In this case, the films provided inside the opening 290 are preferably formed by atomic layer deposition (ALD). The ALD method allows atoms to be deposited layer by layer, and therefore has advantages such as enabling ultrathin film formation, film formation on a structure with a high aspect ratio, film formation with fewer defects such as pinholes, film formation with excellent coverage, and film formation at low temperatures. Therefore, the film can be formed on the sidewalls of the opening 290 with good coverage. For example, the oxide semiconductor layer 230 and the conductive layer 260 can each be formed by the ALD method. Furthermore, for example, when the oxide semiconductor layer 230 and the conductive layer 260 have a stacked structure, it is preferable to form one or more of the stacked layers by the ALD method. For example, of the conductive layer 260a and the conductive layer 260b, it is preferable to form the conductive layer 260a using the ALD method. Furthermore, by embedding the conductive layer 260 in the opening 290, the cross-sectional area of the conductive layer 260 can be increased and the resistance can be reduced. Therefore, for example, by forming the conductive layer 260b using a sputtering method, a PECVD method, or the like, the conductive layer 260 can be formed so as to embed the opening 290.
[0084] Furthermore, it is preferable that the insulating layer 250 has a configuration that provides good coverage of the sidewall of the opening 290 and can prevent short circuits between the conductive layer 240 and the conductive layer 260 .
[0085] 1B and 1C , a portion of the insulating layer 250 is located outside the opening 290, i.e., on the conductive layer 240 and the insulating layer 280. In this case, the insulating layer 250 preferably covers the end of the oxide semiconductor layer 230. This can prevent the conductive layer 260 and the oxide semiconductor layer 230 from shorting out. In addition, the insulating layer 250 preferably covers the end of the conductive layer 240. This can prevent the conductive layer 260 and the conductive layer 240 from shorting out.
[0086] The insulating layer 250 functions as a gate insulating layer of the transistor 200. By thinning the gate insulating layer, it is possible to reduce the gate potential applied during operation of the transistor 200. Furthermore, it is possible to operate the transistor 200 at high speed.
[0087] On the other hand, thinning the gate insulating layer may increase leakage current in the transistor's gate insulating layer, and may also reduce the gate-drain breakdown voltage of the transistor. These concerns become more pronounced if the gate insulating layer is overetched or damaged during transistor processing.
[0088] In the insulating layer 250, a region outside the end of the conductive layer 260 is exposed to an etching atmosphere when the conductive layer 260 is formed, and there is a concern that the region may be damaged by etching. There is a concern that the withstand voltage of the insulating layer 250 may decrease due to the etching damage. In particular, when dry etching is used in the step of forming the conductive layer 260, the damage by etching may become more pronounced.
[0089] Furthermore, the insulating layer 250 is not covered by the conductive layer 260 in a region outside the end of the conductive layer 260. Therefore, over-etching in the process of forming the conductive layer 260 may result in a reduction in the film thickness of the insulating layer 250 in a region outside the end of the conductive layer 260 compared to a region overlapping with the conductive layer 260. In particular, if dry etching is used in the process of forming the conductive layer 260, the reduction in the film thickness of the insulating layer 250 due to over-etching may be more pronounced. There is a concern that the breakdown voltage may decrease in the region of the insulating layer 250 where the film thickness is reduced. Here, over-etching refers to, for example, etching of the insulating layer 250 by a dry etching process intended to etch the conductive layer 260 in a region where the insulating layer 250 is exposed after removing a portion of the conductive layer 260.
[0090] In a region where the breakdown voltage of the insulating layer 250 has decreased, there is a concern that, for example, a gate leakage current will increase due to the electric field between the conductive layer 260 and the conductive layer 240. Furthermore, if the insulating layer 250 is significantly damaged or the film thickness is significantly reduced, there is a concern that, for example, a short circuit will occur between the conductive layer 260 and the conductive layer 240.
[0091] In the transistor of one embodiment of the present invention, the thickness of a region of the insulating layer 250 between the top surface of the conductive layer 240 and the conductive layer 260 (thickness T2 described later) is preferably thicker than the thickness of a region of the insulating layer 250 facing the sidewall of the insulating layer 280 in the opening 290 a (thickness T1 described later). With this structure, even when the thickness of the insulating layer 250 is reduced by over-etching in the formation of the conductive layer 260, the thickness of a region of the insulating layer 250 that covers the top surface of the conductive layer 240 but is not covered with the conductive layer 260 (thickness T3 described later) can be thick enough to suppress gate leakage current and short circuit.
[0092] FIG. 2A shows the thicknesses of five regions of the insulating layer 250 (thicknesses T1, T2, T3, T4, and T5).
[0093] The thickness T1 is the film thickness of a region of the insulating layer 250 that faces the sidewall of the insulating layer 280 in the opening 290a. In this region, the insulating layer 250 faces the sidewall of the opening 290a with the oxide semiconductor layer 230 sandwiched therebetween.
[0094] The thickness T2 is the film thickness of the insulating layer 250 in a region sandwiched between the upper surface of the conductive layer 240 and the conductive layer 260. In this region, the insulating layer 250 covers the upper surface of the conductive layer 240 with the oxide semiconductor layer 230 interposed therebetween.
[0095] The thickness T3 is the thickness of a region of the insulating layer 250 that covers the top surface of the conductive layer 240 via the oxide semiconductor layer 230 and is not covered by the conductive layer 260. Note that in FIG. 2A , the thickness T3 is the thickness of the insulating layer 250 in a region outside the end of the conductive layer 260 and very close to the end. However, when there is a region with a different thickness (thick in the case of FIG. 2A ) as in the case of thickness T3z in FIG. 2A , for example, the region with the thinnest thickness can be used as the thickness T3. Alternatively, the average thickness of the corresponding region in cross-sectional observation may be used as the thickness T3.
[0096] Furthermore, thickness T1, thickness T2, and thickness T5 (described later) may each have a distribution of thickness within the region. In such cases, for example, the thickness of the thinnest region may be used as the thickness. Alternatively, for example, the thickness of the thickest region may be used as the thickness. Alternatively, for example, the average thickness of the region may be used as the thickness.
[0097] The thickness T4 is the film thickness of the insulating layer 250 in a region sandwiched between the upper surface of the conductive layer 220 and the conductive layer 260. In this region, the insulating layer 250 covers the upper surface of the conductive layer 220 with the oxide semiconductor layer 230 interposed therebetween.
[0098] The thickness T5 is the film thickness of a region of the insulating layer 250 that covers the upper surface of the conductive layer 240 and does not overlap with the oxide semiconductor layer 230. The thickness T5 can also be expressed as the film thickness of a region that covers the upper surface of the conductive layer 240 and is located outside the edge of the oxide semiconductor layer 230 in a top view.
[0099] For example, thickness T2 and thickness T4 are approximately the same. For example, thickness T4 is 0.8 to 1.2 times the thickness T2. Note that the portion of insulating layer 250 located at the bottom of opening 290 may not have a uniform thickness, for example, the central portion may be thicker. In such a case, thickness T4 may be the thickest portion of insulating layer 250.
[0100] Thickness T2 is thicker than thickness T1. Furthermore, since thickness T2 and thickness T4 are approximately the same, thickness T4 is thicker than thickness T1. By increasing thickness T2, the parasitic capacitance of conductive layer 240 and conductive layer 260 can be reduced. Furthermore, by increasing thickness T4, the parasitic capacitance of conductive layer 220 and conductive layer 260 can be reduced.
[0101] If the insulating layer 250 is etched due to over-etching during processing of the conductive layer 260, the thickness T3 will be thinner than the thickness T2. In such a case, in order to make the thickness T3 thick enough to prevent a short circuit between the conductive layer 260 and the conductive layer 240 or gate leakage of the insulating layer 250, the thickness T2 needs to be set in consideration of the film thickness that will be reduced by over-etching.
[0102] On the other hand, if the thickness T2 is too thick, the aspect ratio of the opening in which the conductive layer 260 is embedded increases, which may make it difficult to improve the coverage of the conductive layer 260 with respect to the insulating layer 250. Therefore, the thickness T2 may be set to, for example, 100 nm or less.
[0103] The thickness T1 is the thickness of a region of the insulating layer 250 that can function as a gate insulating layer for a channel formation region of the transistor 200. The thickness T1 is preferably 0.1 nm to 30 nm, more preferably 0.1 nm to 20 nm, even more preferably 0.1 nm to 10 nm, even more preferably 0.1 nm to 8.0 nm, and even more preferably 0.1 nm to 7.0 nm.
[0104] The thickness T3 is, for example, preferably 1.0 nm or more and 100 nm or less, preferably 2.0 nm or more and 100 nm or less, more preferably 3.0 nm or more and 100 nm or less, more preferably 4.0 nm or more and 100 nm or less, and more preferably 5.0 nm or more and 100 nm or less.
[0105] For example, the thickness T2 and the thickness T4 are each equal to or greater than the thickness T3. For example, the thickness T2 and the thickness T4 may be greater than the thickness T3 by 2 nm or more.
[0106] The thickness T5 is, for example, approximately the same as the thickness T3. The thickness T5 is, for example, preferably 1.0 nm or more and 50 nm or less, preferably 2.0 nm or more and 50 nm or less, more preferably 3.0 nm or more and 50 nm or less, more preferably 4.0 nm or more and 50 nm or less, and more preferably 5.0 nm or more and 50 nm or less.
[0107] For example, the thickness T2 and the thickness T4 are each equal to or greater than the thickness T5. For example, the thickness T2 and the thickness T4 may be 2 nm thicker than the thickness T5.
[0108] As a method for forming the insulating layer 250, for example, it is preferable to use a method in which the film formation rate is slower on a surface where the surface is perpendicular to the substrate surface than on a surface where the surface is parallel to the substrate surface. Note that such a film formation method can also be expressed as a film formation method in which the deposition rate is anisotropic.
[0109] By using such a method, the insulating layer 250 can be thinned in a region that can function as a gate insulating layer in the channel formation region of the transistor. Therefore, the driving voltage of the transistor 200 can be reduced and the operating speed can be increased. Furthermore, the insulating layer 250 can be thickened in a region that covers the top surface of the conductive layer 240. Therefore, the insulating layer 250 in the transistor 200 can be prevented from being thinned, the gate leakage current of the transistor 200 can be reduced, and a decrease in the withstand voltage of the transistor 200 can be suppressed.
[0110] The insulating layer 250 shown in FIGS. 1B, 1C, 2A, etc. can be formed by sputtering, CVD, etc.
[0111] Examples of sputtering methods that can be used include ionization sputtering and long-throw sputtering. Ionization sputtering is a method in which sputtering particles generated from a target are ionized by RF or the like, and anisotropic film formation is performed by self-bias or the like. In addition, long-throw sputtering can form anisotropic films by increasing the distance between the sputtering target and the substrate, and the distance between the sputtering target and the substrate is preferably 60 mm or more, more preferably 100 mm or more.
[0112] As the CVD method, for example, a plasma enhanced chemical vapor deposition (PECVD) method can be used. Here, it is preferable to use a PECVD method using RF. In particular, when forming an insulating layer, using RF allows for more stable plasma discharge.
[0113] 1B and 1C show a configuration in which, outside the opening 290, the end of the oxide semiconductor layer 230 is located more inward than the end of the conductive layer 240. However, the present invention is not limited to this. For example, in the X direction, the end of the oxide semiconductor layer 230 and the end of the conductive layer 240 may coincide or substantially coincide. Alternatively, the end of the oxide semiconductor layer 230 may be located more outward than the end of the conductive layer 240. For example, in FIG. 3A , in the X direction of the conductive layer 240, the end of the conductive layer 240 on the side where the conductive layer 661 is provided (the negative X direction) is located more outward than the end of the oxide semiconductor layer 230, while the end of the conductive layer 240 on the opposite side (the positive X direction) is located more outward than the end of the conductive layer 240, and the oxide semiconductor layer 230 covers the end of the conductive layer 240. By having the oxide semiconductor layer 230 cover the end portion of the conductive layer 240, the breakdown voltage between the conductive layer 240 and the conductive layer 260 can be further increased, and the leakage current of the insulating layer 250 located between the conductive layer 240 and the conductive layer 260 can be further reduced in some cases.
[0114] 3B , an end of the conductive layer 260 may be located outside an end of the oxide semiconductor layer 230 in the X direction. When the conductive layer 260 contains a light-blocking material, a current induced by light in the oxide semiconductor layer 230 is suppressed in a region covered with the conductive layer 260, which may improve the characteristics and reliability of the transistor. Furthermore, when a region functioning as a low-resistance region in the oxide semiconductor layer 230 overlaps with the conductive layer 260, the resistance is further reduced, which may further improve the on-state current of the transistor.
[0115] The sidewall of opening 290 is preferably provided so as to be perpendicular to the upper surface of insulating layer 210, for example. The angle θ formed between the side surface of insulating layer 280 in opening 290 and the upper surface of insulating layer 210 is shown in FIG. 1B . The angle θ is preferably greater than 60 degrees and less than 90 degrees, more preferably greater than 70 degrees and less than 90 degrees, and even more preferably greater than 80 degrees and less than 90 degrees. Setting angle θ to such a value allows insulating layer 250 to have anisotropy, which is preferable because it allows insulating layer 250 to be thin in the region covering the sidewall of opening 290. This is also preferable because it allows for miniaturization or high integration of semiconductor devices.
[0116] Alternatively, for example, the sidewall of the opening 290 may have an inverse tapered shape. In other words, the angle formed between the side surface of the insulating layer 280 at the opening 290 and the top surface of the insulating layer 210 may be greater than 90 degrees.
[0117] FIG. 4 shows an example in which the angle θ is less than 90 degrees.
[0118] 1B and 1C show a configuration in which the side surface of the conductive layer 240 in the opening 290b and the side surface of the insulating layer 280 in the opening 290a are aligned or approximately aligned, but the present invention is not limited to this. For example, the side surface of the conductive layer 240 in the opening 290b and the side surface of the insulating layer 280 in the opening 290a may be discontinuous. Furthermore, the inclination of the side surface of the conductive layer 240 in the opening 290b may differ from the inclination of the side surface of the insulating layer 280 in the opening 290a. In this case, for example, the angle formed between the side surface of the conductive layer 240 in the opening 290b and the top surface of the insulating layer 210 is preferably smaller than the angle formed between the side surface of the insulating layer 280 in the opening 290a and the top surface of the insulating layer 210. This configuration improves the coverage of the oxide semiconductor layer 230 on the side surface of the conductive layer 240 in the opening 290b, thereby reducing defects such as voids. In such a configuration, the thickness of the insulating layer 250 covering the side surface of the conductive layer 240 may be thicker than the thickness of the insulating layer 250 covering the side wall of the insulating layer 280 in the opening 290a.
[0119] The insulating layer 250 may be configured by laminating two or more layers. In such a case, for example, it is preferable that one or more of the multiple layers be formed with anisotropy.
[0120] The oxide semiconductor layer 230 may have a stacked structure of two or more layers. Fig. 5A shows an example in which the oxide semiconductor layer 230 has a two-layer structure of an oxide layer 230a and an oxide layer 230b over the oxide layer 230a. Fig. 5B shows an example in which the oxide semiconductor layer 230 has a three-layer structure of an oxide layer 230c, an oxide layer 230a over the oxide layer 230c, and an oxide layer 230b over the oxide layer 230a.
[0121] <Configuration Example 2 of Semiconductor Device> Another configuration example of the semiconductor device shown in FIG. 1A will be described with reference to FIGS. 6A and 6B.
[0122] 6A and 6B are cross-sectional views taken along dashed lines A1-A2 and A3-A4, respectively, shown in FIG. 1A, and differ from FIG. 1B and FIG. 1C in that insulating layer 250 is formed by laminating insulating layer 250a and insulating layer 250b on insulating layer 250a. FIG. 7A is an enlarged view of the area surrounded by the two-dot chain line in FIG. 6A.
[0123] 6A and 6B, an insulating layer 222 is provided on the insulating layer 210, and a conductive layer 220 and an insulating layer 280 are provided on the insulating layer 222. In FIG.
[0124] 6A and 6B , insulating layer 280 includes insulating layer 280a, insulating layer 280b on insulating layer 280a, and insulating layer 280c on insulating layer 280b. Insulating layer 280a includes a region in contact with the upper surface of insulating layer 222, a region in contact with the side surface of conductive layer 220, and a region in contact with the upper surface of conductive layer 220. Insulating layer 280c includes a region in contact with the lower surface of conductive layer 240.
[0125] The insulating layer 250a is preferably formed using a method with high coverage. By increasing the coverage of the insulating layer 250a, the insulating layer 250a can be suitably formed even in openings with high aspect ratios.
[0126] By increasing the coverage of the insulating layer 250a in the region that covers the sidewall of the insulating layer 280 in the opening 290a, i.e., the region that can function as a gate insulating layer in the channel formation region of the transistor, it is possible to form, for example, a thin and uniform gate insulating layer.
[0127] As a method for forming the insulating layer 250a, it is particularly preferable to use the ALD method.
[0128] A film formation method with high coverage may have low anisotropy of the deposition rate. The insulating layer 250a is formed, for example, using a film formation method with low anisotropy of the deposition rate. In the insulating layer 250a, for example, the film thickness (thickness T2a, described later) of the region sandwiched between the upper surface of the conductive layer 240 and the conductive layer 260 is approximately the same as the film thickness (thickness T1a, described later) of the region facing the sidewall of the insulating layer 280 in the opening 290a. Furthermore, the insulating layer 250a is formed using a film formation method with lower anisotropy of the deposition rate than the insulating layer 250b. The insulating layer 250a can also be expressed as being formed using a film formation method with isotropy. For example, an ALD method can be used as a film formation method with isotropy.
[0129] The insulating layer 250b is preferably formed using a method with a high anisotropy of the deposition rate. In the insulating layer 250b, the thickness (thickness T2b described later) of a region sandwiched between the upper surface of the conductive layer 240 and the conductive layer 260 is preferably thicker than the thickness (thickness T1b described later) of a region facing the sidewall of the insulating layer 280 in the opening 290a.
[0130] By combining the insulating layer 250a formed by a film formation method with high coverage and the insulating layer 250b formed by a method with high anisotropy of the deposition rate as the insulating layer 250, it is possible to make the film thickness of a region that can function as a gate insulating layer in the channel formation region of the transistor thin and uniform, and to suppress gate leakage current of the insulating layer 250 and short-circuiting between the conductive layer 240 and the conductive layer 260. Furthermore, by using the ALD method for the insulating layer 250a, it is possible to form a thin, uniform, and dense gate insulating layer.
[0131] FIG. 7A shows the film thicknesses of five regions in insulating layer 250a (thicknesses T1a, T2a, T3a, T4a, and T5a) and the film thicknesses of five regions in insulating layer 250b (thicknesses T1b, T2b, T3b, T4b, and T5b).
[0132] The thickness T1a is the thickness of a region of the insulating layer 250a that faces the sidewall of the opening 290a of the insulating layer 280. In this region, the insulating layer 250a faces the sidewall of the opening 290a with the oxide semiconductor layer 230 sandwiched therebetween.
[0133] The thickness T2a is the film thickness of the insulating layer 250a in a region sandwiched between the upper surface of the conductive layer 240 and the conductive layer 260. In this region, the insulating layer 250a covers the upper surface of the conductive layer 240 with the oxide semiconductor layer 230 interposed therebetween.
[0134] The thickness T3a is the thickness of a region of the insulating layer 250a that covers the upper surface of the conductive layer 240 via the oxide semiconductor layer 230 and is not covered by the conductive layer 260.
[0135] The thickness T4a is the thickness of the insulating layer 250a in a region sandwiched between the upper surface of the conductive layer 220 and the conductive layer 260. In this region, the insulating layer 250a covers the upper surface of the conductive layer 220 with the oxide semiconductor layer 230 interposed therebetween.
[0136] The thickness T5a is the thickness of a region of the insulating layer 250a that covers the upper surface of the conductive layer 240 and does not overlap with the oxide semiconductor layer 230.
[0137] The thickness T1b is the thickness of a region of the insulating layer 250b that faces the sidewall of the opening 290a of the insulating layer 280. In this region, the insulating layer 250b faces the sidewall of the opening 290a, with the oxide semiconductor layer 230 and the insulating layer 250a sandwiched therebetween.
[0138] The thickness T2b is the film thickness of the insulating layer 250b in a region sandwiched between the upper surface of the conductive layer 240 and the conductive layer 260. In this region, the insulating layer 250b covers the upper surface of the conductive layer 240 via the oxide semiconductor layer 230 and the insulating layer 250a.
[0139] Thickness T3b is the thickness of a region of insulating layer 250b that covers the upper surface of conductive layer 240 via oxide semiconductor layer 230 and insulating layer 250a and is not covered by conductive layer 260.
[0140] Thickness T4b is the film thickness of the insulating layer 250b in a region sandwiched between the upper surface of the conductive layer 220 and the conductive layer 260. In this region, the insulating layer 250b covers the upper surface of the conductive layer 220 via the oxide semiconductor layer 230 and the insulating layer 250a.
[0141] The thickness T5b is the thickness of a region of the insulating layer 250b that covers the upper surface of the conductive layer 240 and does not overlap with the oxide semiconductor layer 230.
[0142] The sum of the thickness T2a and the thickness T2b may be set to, for example, 100 nm or less.
[0143] 7A, the thickness T2b and the thickness T4b are, for example, approximately the same thickness. The thickness T4b is, for example, 0.8 times or more and 1.2 times or less the thickness T2b.
[0144] The thickness T2b is thicker than the thickness T1b. Furthermore, since the thickness T2b and the thickness T4b are approximately the same, the thickness T4b is thicker than the thickness T1b.
[0145] In FIG. 7A, thicknesses T2a, T3a, T4a, and T5a are, for example, approximately the same as thickness T1a, and are, for example, 0.8 to 1.2 times the thickness T1a.
[0146] The sum of the thickness T1a and the thickness T1b is preferably 0.2 nm or more and 30 nm or less, more preferably 0.2 nm or more and 20 nm or less, more preferably 0.2 nm or more and 10 nm or less, more preferably 0.2 nm or more and 8.0 nm or less, and more preferably 0.2 nm or more and 7.0 nm or less.
[0147] In FIG. 7A, the thickness T1a is, for example, 0.1 nm or more, alternatively 0.2 nm or more, alternatively 0.5 nm or more, or alternatively 1 nm or more.
[0148] 7A, the thickness T1b may be extremely thin, for example, 0.1 nm to 1 nm, or 0.1 nm to 0.5 nm, or 0.1 nm to 0.2 nm.
[0149] The sum of the thickness T3a and the thickness T3b is, for example, preferably 1.0 nm to 100 nm, more preferably 2.0 nm to 100 nm, more preferably 3.0 nm to 100 nm, more preferably 4.0 nm to 100 nm, and more preferably 5.0 nm to 100 nm.
[0150] The thicknesses T2b and T4b are each, for example, equal to or greater than the thickness T3b, and may be, for example, 2 nm or more thicker than the thickness T3b.
[0151] Furthermore, the thickness T5b is, for example, approximately the same as the thickness T3b.
[0152] Note that Figure 7A shows an example in which insulating layer 250a is a film formed by a film formation method with high coverage, and insulating layer 250b is a film formed by a method with high anisotropy of deposition rate, but as shown in Figure 7B, insulating layer 250a may be a film formed by a method with high anisotropy of deposition rate, and insulating layer 250b may be a film formed by a film formation method with high coverage.
[0153] In the configuration shown in Figure 7B, for example, the insulating layer 250b can be formed using the ALD method. At this time, the insulating layer 250a is formed on the entire surface as the formation surface. In the ALD method, the time at which film formation begins may vary depending on the material of the formation surface, etc. By forming the insulating layer 250b after the insulating layer 250a has been formed on the entire surface, for example, the insulating layer 250b can be made to have a more uniform film thickness and film quality.
[0154] 7B, the thickness T2a and the thickness T4a are, for example, approximately the same thickness. The thickness T4a is, for example, 0.8 to 1.2 times the thickness T2a.
[0155] In FIG. 7B, the thickness T2b and the thickness T4b are, for example, approximately the same as the thickness T1b, and are, for example, 0.8 to 1.2 times the thickness T1b.
[0156] In FIG. 7B, the thickness T1b is, for example, 0.1 nm or more, alternatively 0.2 nm or more, alternatively 0.5 nm or more, or alternatively 1 nm or more.
[0157] 7B, thickness T1a may be extremely thin. For example, thickness T1a may be 0.1 nm or more and 1 nm or less, or 0.1 nm or more and 0.5 nm or less, or 0.1 nm or more and 0.2 nm or less. Furthermore, as shown in FIG. 13 described later, thickness T1a may be 0 nm. That is, in the insulating layer 250, insulating layer 250b may not be provided in the region facing the sidewall of insulating layer 280 in opening 290a, and the region may be composed of only insulating layer 250a.
[0158] The thickness T3b may be set to, for example, the thickness of the thinnest region within the region.
[0159] The thickness T4a and the thickness T4b may be, for example, the thickness of the thickest region within the region.
[0160] Furthermore, thicknesses T1a, T1b, T2a, T2b, T3a, T5a, and T5b may each have a distribution of thickness within the region. In such cases, for example, the thickness of the thinnest region can be taken as the thickness. Alternatively, for example, the thickness of the thickest region can be taken as the thickness. Alternatively, for example, the average thickness of the region can be taken as the thickness.
[0161] <Configuration Example 3 of Semiconductor Device> Another configuration example of the semiconductor device will be described with reference to FIGS. 8A to 8C.
[0162] Fig. 8A is a plan view of a semiconductor device having a transistor 200. Fig. 8B is a cross-sectional view taken along dashed dotted line A1-A2 in Fig. 8A. Fig. 8C is a cross-sectional view taken along dashed dotted line A3-A4 in Fig. 8A. Fig. 9A is an enlarged view of the region surrounded by the two-dot dashed line in Fig. 8B.
[0163] The semiconductor device shown in FIGS. 8A to 8C differs from that shown in FIGS. 1A to 1C in that the insulating layer 250 is composed of an insulating layer 250c and an insulating layer 250d.
[0164] The insulating layer 250d is disposed in a region of the upper surface of the conductive layer 240 that is not covered with the oxide semiconductor layer 230. In Figures 8B and 8C, the insulating layer 250d is in contact with the upper surface and the side surface of the conductive layer 240, respectively. The insulating layer 250c is disposed on the oxide semiconductor layer 230, the insulating layer 250d, and the insulating layer 280. The insulating layer 250d is sandwiched between the conductive layer 240 and the insulating layer 250c.
[0165] The insulating layer 250d can be formed using, for example, a film that is selectively formed in a region where the surface of the conductive layer 240 is exposed. For example, when the insulating layer 250d is formed, the insulating layer 250d is not formed in a region of the conductive layer 240 that is covered with the oxide semiconductor layer 230. The conductive layer 240 preferably has a metal layer. Furthermore, when the conductive layer 240 has a stacked structure, the uppermost layer is preferably a metal layer. Furthermore, the insulating layer 250d can be formed using a film that is selectively grown on a metal.
[0166] Because the insulating layer 250d is selectively formed in a region where the surface of the conductive layer 240 is exposed, the thickness of the insulating layer 250 can be increased in a region between the conductive layer 240 and the conductive layer 260 where the oxide semiconductor layer 230 is not disposed. This reduces the leakage current of the insulating layer 250 and improves the breakdown voltage. Furthermore, even if the thickness of the insulating layer 250 is not large in the region where the oxide semiconductor layer 230 is disposed, the oxide semiconductor layer 230 is disposed between the conductive layer 240 and the conductive layer 260, thereby reducing the leakage current of the insulating layer 250 and improving the breakdown voltage.
[0167] It can be expressed that the insulating layer 250 does not overlap with the oxide semiconductor layer 230 and has a large thickness in a region overlapping with the conductive layer 240 .
[0168] The insulating layer 250c is preferably provided in contact with the top surface of the oxide semiconductor layer 230. In addition, in Figures 8B and 8C and the like, the insulating layer 250c has a region covering the top surface of the conductive layer 240 with the insulating layer 250d sandwiched therebetween, and a region covering the side surface of the conductive layer 240 with the insulating layer 250d sandwiched therebetween. The insulating layer 250c is preferably provided in contact with the insulating layer 250d. Furthermore, the insulating layer 250c preferably has a region in contact with the top surface of the insulating layer 280.
[0169] The insulating layer 250c can be formed by appropriately using an ALD method, a CVD method, an MBE method, a PLD method, a sputtering method, or the like.
[0170] By using a method with high coverage for the insulating layer 250c, a gate insulating layer with a thin and uniform film thickness can be formed.
[0171] The insulating layer 250c can be made of one or a combination of materials that can be used for the insulating layer 250.
[0172] 8B and 8C, the insulating layers 250c and 250d may be formed without using an anisotropic film formation method. Therefore, for example, in the configurations shown in FIGS. 8B and 8C, the preferable range of the angle θ may include a smaller angle. For example, in the configurations shown in FIGS. 8B and 8C, the angle θ may be 45 degrees or more and 90 degrees or less.
[0173] By setting the angle θ to a small value, for example, between 45 degrees and 60 degrees, the coverage of the oxide semiconductor layer 230, the insulating layer 250, and the like is further improved.
[0174] FIG. 9A shows the thicknesses of four regions of insulating layer 250c (thicknesses T1c, T2c, T4c, and T5c) and the thickness of one region of insulating layer 250d (thickness T5d).
[0175] The thickness T1c is the thickness of a region of the insulating layer 250c that faces the sidewall of the opening 290a of the insulating layer 280. In this region, the insulating layer 250c faces the sidewall of the opening 290a with the oxide semiconductor layer 230 sandwiched therebetween.
[0176] The thickness T2c is the thickness of the insulating layer 250c in a region sandwiched between the upper surface of the conductive layer 240 and the conductive layer 260. In this region, the insulating layer 250c covers the upper surface of the conductive layer 240 with the oxide semiconductor layer 230 interposed therebetween.
[0177] Thickness T5c is the thickness of a region of insulating layer 250c that covers the upper surface of conductive layer 240 via insulating layer 250d and is not covered by conductive layer 260.
[0178] The thickness T4c is the thickness of the insulating layer 250c in a region sandwiched between the upper surface of the conductive layer 220 and the conductive layer 260. In this region, the insulating layer 250c covers the upper surface of the conductive layer 220 with the oxide semiconductor layer 230 interposed therebetween.
[0179] The thickness T5d is the thickness of the region of the insulating layer 250d that covers the upper surface of the conductive layer 240.
[0180] For example, the thicknesses T2c and T4c are each approximately the same as the thickness T1c, for example, 0.8 to 1.2 times the thickness T1c. The thickness T5c is thinner than the thickness T1c.
[0181] The thickness T1c is preferably 0.2 nm or more and 30 nm or less, more preferably 0.2 nm or more and 20 nm or less, more preferably 0.2 nm or more and 10 nm or less, more preferably 0.2 nm or more and 8.0 nm or less, and more preferably 0.2 nm or more and 7.0 nm or less.
[0182] The sum of the thicknesses T1c and T5d is, for example, preferably 1.0 nm to 50 nm, more preferably 2.0 nm to 50 nm, more preferably 3.0 nm to 50 nm, more preferably 4.0 nm to 50 nm, and more preferably 5.0 nm to 50 nm.
[0183] Furthermore, thicknesses T1c, T2c, T4c, T5c, and T5d may each have a distribution of thickness within the region. In such cases, for example, the thickness of the thinnest region may be taken as the thickness. Alternatively, for example, the thickness of the thickest region may be taken as the thickness. Alternatively, for example, the average thickness of the region may be taken as the thickness.
[0184] 9B , an end of the oxide semiconductor layer 230 may be disposed outside an end of the conductive layer 260. By disposing the oxide semiconductor layer 230 between the end of the conductive layer 260 and the upper surface of the conductive layer 240, it may be possible to reduce leakage current in the insulating layer 250 between the conductive layer 260 and the conductive layer 240. Furthermore, the pattern width of the conductive layer 260 (here, the width in the X direction) can be reduced without considering the margin for arrangement with the pattern of the oxide semiconductor layer 230. This allows the wiring width of the conductive layer 260 that functions as the gate electrode of a transistor to be narrowed, thereby enabling, for example, further miniaturization of transistors.
[0185] The transistor 200 includes a metal oxide (also referred to as an oxide semiconductor) functioning as a semiconductor in the oxide semiconductor layer 230 including a channel formation region. That is, the transistor 200 can be said to be an OS transistor.
[0186] An OS transistor has an oxygen vacancy (V O ) and impurities, the electrical characteristics are likely to fluctuate, and reliability may be reduced. In addition, hydrogen in the vicinity of the oxygen vacancy may become a defect in which hydrogen enters the oxygen vacancy (hereinafter referred to as V O H) and generate electrons that serve as carriers. Therefore, if oxygen vacancies are present in the channel formation region of the oxide semiconductor, the OS transistor is likely to have normally-on characteristics. Therefore, it is preferable that oxygen vacancies and impurities are reduced as much as possible in the channel formation region of the oxide semiconductor. In other words, it is preferable that the carrier concentration of the channel formation region of the oxide semiconductor is reduced and the channel formation region of the oxide semiconductor is made i-type (intrinsic) or substantially i-type.
[0187] On the other hand, the source and drain regions of an OS transistor have more oxygen vacancies than the channel formation region. O The source and drain regions of an OS transistor are preferably n-type regions having a high carrier concentration and low resistance compared to a channel formation region, and the source and drain regions of the OS transistor preferably have a high carrier concentration and low resistance due to a high concentration of H or an impurity such as hydrogen, nitrogen, or a metal element.
[0188] A region of the oxide semiconductor layer 230 in contact with the insulating layer 280 and its vicinity function as a channel formation region of the transistor 200. One of a region of the oxide semiconductor layer 230 in contact with the conductive layer 220 and a region of the oxide semiconductor layer 230 in contact with the conductive layer 240 functions as a source region, and the other functions as a drain region. That is, the channel formation region is sandwiched between the source region and the drain region.
[0189] When the oxide semiconductor layer 230 and the conductive layer 220 come into contact with each other, a metal compound or oxygen vacancy is formed, and the region of the oxide semiconductor layer 230 in contact with the conductive layer 220 is reduced in resistance. This reduces the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220. Similarly, when the oxide semiconductor layer 230 and the conductive layer 240 come into contact with each other, the region of the oxide semiconductor layer 230 in contact with the conductive layer 240 is reduced in resistance. This reduces the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240.
[0190] 2B , the insulating layer 280 is in contact with the entire outer periphery of the oxide semiconductor layer 230. Therefore, the channel formation region of the transistor 200 can be formed over the entire outer periphery of the oxide semiconductor layer 230 in the opening 290 (the entire region in contact with the insulating layer 280). Note that FIG. 2B can also be considered a cross-sectional view in the XY plane including the channel formation region of the oxide semiconductor layer 230.
[0191] The channel length of the transistor 200 is the distance between the source region and the drain region. In other words, it can be said that the channel length of the transistor 200 is determined by the thickness of the insulating layer 280 on the conductive layer 220. In FIG. 1C , the channel length L of the transistor 200 is indicated by a dashed double-headed arrow. In a cross-sectional view, the channel length L is the distance between the edge of the region where the oxide semiconductor layer 230 and the conductive layer 220 contact each other and the edge of the region where the oxide semiconductor layer 230 and the conductive layer 240 contact each other. In other words, the channel length L corresponds to the length of the side surface of the insulating layer 280 on the opening 290 side in a cross-sectional view.
[0192] In conventional transistors, such as planar transistors, the channel length is limited by the exposure limit of photolithography, making further miniaturization difficult. However, in the present invention, the channel length can be set by the film thickness of the insulating layer 280. Therefore, the channel length of the transistor 200 can be made into an extremely fine structure that is equal to or less than the exposure limit of photolithography (e.g., 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less, and 0.1 nm or more, 1 nm or more, or 5 nm or more). This increases the on-state current of the transistor 200, thereby improving its frequency characteristics.
[0193] Furthermore, as described above, a channel formation region, a source region, and a drain region can be formed in the opening 290. This allows the transistor 200 to occupy a smaller area than a lateral transistor, such as a planar transistor, in which the channel formation region, the source region, and the drain region are separately provided on the XY plane. Therefore, the semiconductor device can be highly integrated. Furthermore, when the semiconductor device of one embodiment of the present invention is used in a memory device, the memory capacity per unit area can be increased.
[0194] As shown in FIG. 2B , the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are arranged concentrically. Therefore, the side surface of the conductive layer 260 located at the center faces the side surface of the oxide semiconductor layer 230 with the insulating layer 250 interposed therebetween. That is, the entire periphery of the oxide semiconductor layer 230 forms a channel formation region in a plan view. In this case, for example, the channel width of the transistor 200 is determined by the periphery length of the oxide semiconductor layer 230. That is, the channel width of the transistor 200 can be determined by the width of the opening 290 (or the diameter when the opening 290 is circular in a plan view). In FIGS. 1C and 2B , the width D of the opening 290 is indicated by a double-headed, dashed arrow. In FIG. 2B , the channel width W of the transistor 200 is indicated by a double-headed, dashed arrow. Increasing the width D of the opening 290 increases the channel width per unit area, thereby increasing the on-state current.
[0195] When the opening 290 is formed using photolithography, the width D of the opening 290 is limited by the exposure limit of photolithography. The width D of the opening 290 is set depending on the film thicknesses of the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 provided in the opening 290. The width D of the opening 290 is, for example, 5 nm or more, 10 nm or more, or 20 nm or more, and preferably 100 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, or 30 nm or less. Note that when the opening 290 has a circular shape in a plan view, the width D of the opening 290 corresponds to the diameter of the opening 290, and the channel width W can be calculated as "D × π".
[0196] The channel length L of the transistor 200 is preferably at least shorter than the channel width W of the transistor 200. The channel length L of the transistor 200 is preferably 0.1 to 0.99 times, more preferably 0.5 to 0.8 times, the channel width W of the transistor 200. With such a structure, a transistor with favorable electrical characteristics and high reliability can be realized.
[0197] Furthermore, by forming the opening 290 so as to have a circular shape in a plan view, the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are provided concentrically. This makes the distance between the conductive layer 260 and the oxide semiconductor layer 230 approximately uniform, allowing a gate electric field to be applied to the oxide semiconductor layer 230 approximately uniformly.
[0198] In this embodiment, the opening 290 has a circular shape in plan view, but the present invention is not limited to this. For example, the opening 290 may have a substantially circular shape such as an oval, a polygonal shape such as a square, or a polygonal shape such as a square with rounded corners in plan view.
[0199] <Constituent Materials of Semiconductor Device> Materials that can be used in the semiconductor device of this embodiment will be described below. Note that each layer constituting the semiconductor device of this embodiment may have a single-layer structure or a stacked-layer structure. FIGS. 1B, 1C, and 2A show an example in which the conductive layer 220, the oxide semiconductor layer 230, and the conductive layer 240 each have a single-layer structure. FIG. 2A shows an example in which the oxide semiconductor layer 230 has a single-layer structure, while FIG. 5A shows an example in which the oxide semiconductor layer 230 has a two-layer stacked structure, and FIG. 5B shows an example in which the oxide semiconductor layer 230 has a three-layer stacked structure.
[0200] [Insulating Layer] It is preferable to use an inorganic insulating film for each of the insulating layers (insulating layer 210, insulating layer 222, insulating layer 250, insulating layer 280, insulating layer 283, etc.) included in the semiconductor device. Examples of inorganic insulating films include an oxide insulating film, a nitride insulating film, an oxynitride insulating film, and a nitride oxide insulating film. Examples of oxide insulating films include a silicon oxide film, an aluminum oxide film, a magnesium oxide film, a gallium oxide film, a germanium oxide film, an yttrium oxide film, a zirconium oxide film, a lanthanum oxide film, a neodymium oxide film, a hafnium oxide film, a tantalum oxide film, a cerium oxide film, a gallium zinc oxide film, and a hafnium aluminate film. Examples of nitride insulating films include a silicon nitride film and an aluminum nitride film. Examples of oxynitride insulating films include a silicon oxynitride film, an aluminum oxynitride film, a gallium oxynitride film, an yttrium oxynitride film, and a hafnium oxynitride film. Examples of nitride oxide insulating films include a silicon nitride oxide film and an aluminum nitride oxide film. Furthermore, an organic insulating film may be used for the insulating layer of the semiconductor device.
[0201] Furthermore, a transistor using a metal oxide can have stable electrical characteristics by being surrounded by an insulating layer that has a function of suppressing the permeation of impurities and oxygen. The insulating layer that has a function of suppressing the permeation of impurities and oxygen can be, for example, a single-layer or stacked insulating layer containing one or more elements selected from boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum. Specifically, the insulating layer that has a function of suppressing the permeation of impurities and oxygen can be made of a metal oxide such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, or tantalum oxide, or a metal nitride such as aluminum nitride, silicon nitride oxide, or silicon nitride.
[0202] Specifically, it is preferable to use a barrier insulating layer against impurities such as water and hydrogen, and oxygen.
[0203] In this specification and the like, a barrier insulating layer refers to an insulating layer having barrier properties. The barrier properties refer to a property that makes it difficult for a corresponding substance to diffuse, a property that makes it difficult for a corresponding substance to permeate, a property that makes it low permeable to a corresponding substance, a function to suppress the diffusion of a corresponding substance, or a function to suppress the permeation of a corresponding substance. Note that hydrogen when described as a corresponding substance includes, for example, a hydrogen atom, a hydrogen molecule, a water molecule, and OH. − Furthermore, unless otherwise specified, impurities when described as corresponding substances refer to impurities in the channel formation region or semiconductor layer, and include, for example, hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, and nitrogen oxide molecules (N 2 O, NO, NO 2 The term "oxygen" refers to at least one of an oxygen atom, an oxygen molecule, etc., when described as a corresponding substance.
[0204] Examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen, and oxygen include metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide. Other examples include oxides containing aluminum and hafnium (hafnium aluminate). Other examples include metal nitrides such as aluminum nitride, silicon nitride oxide, and silicon nitride.
[0205] An insulating layer, such as a gate insulating layer, that is in contact with an oxide semiconductor layer or that is provided near the oxide semiconductor layer is preferably an insulating layer having a region containing oxygen that is released by heating (hereinafter, sometimes referred to as excess oxygen). For example, when an insulating layer having a region containing excess oxygen is in contact with an oxide semiconductor layer or is located near the oxide semiconductor layer, oxygen vacancies in the oxide semiconductor layer can be reduced. Examples of insulating layers that are likely to have a region containing excess oxygen include silicon oxide, silicon oxynitride, and silicon oxide having vacancies.
[0206] Furthermore, for example, as transistors become more miniaturized and highly integrated, problems such as leakage current may occur due to thinner gate insulating layers. Using a high-dielectric-constant (high-k) material for the gate insulating layer allows for lower voltage operation of the transistor while maintaining the physical film thickness. Furthermore, the equivalent oxide thickness (EOT) of the gate insulating layer can be made thinner. Furthermore, using a material with a high dielectric constant as the dielectric layer of a capacitive element allows for an element with a larger capacitance value. On the other hand, using a material with a low dielectric constant for the insulating layer functioning as an interlayer film can reduce the parasitic capacitance generated between wirings. Therefore, it is advisable to select materials according to the function of the insulating layer. Note that materials with a low dielectric constant also have high dielectric strength.
[0207] Examples of materials with a high relative dielectric constant include aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, and nitrides containing silicon and hafnium.
[0208] Examples of materials with a low dielectric constant include resins such as polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate, and acrylic resin. Other inorganic insulating materials with a low dielectric constant include silicon oxide doped with fluorine, silicon oxide doped with carbon, and silicon oxide doped with carbon and nitrogen. Another example is silicon oxide having vacancies. These silicon oxides may contain nitrogen.
[0209] Furthermore, for example, inorganic insulating materials such as silicon oxide, silicon oxynitride, and silicon nitride oxide can be applied to both layers in which a material with a high dielectric constant is preferably used, such as a gate insulating layer, and layers in which a material with a low dielectric constant is preferably used, such as an interlayer film. These materials have a relatively low dielectric constant compared to high-k materials such as hafnium oxide, and therefore may be referred to as "materials with a low dielectric constant" in this specification and the like.
[0210] Furthermore, a material capable of exhibiting ferroelectricity may be used for the insulating layer of the semiconductor device. Examples of the material capable of exhibiting ferroelectricity include hafnium oxide, zirconium oxide, and HfZrO. X (X is a real number greater than 0). Ferroelectric materials include hafnium oxide doped with element J1 (here, element J1 is one or more elements selected from zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.). The ratio of the number of hafnium atoms to the number of element J1 can be set as appropriate; for example, the ratio of the number of hafnium atoms to the number of element J1 can be set to 1:1 or close to 1:1. Ferroelectric materials include zirconium oxide doped with element J2 (here, element J2 is one or more elements selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.). Ferroelectric materials include zirconium oxide doped with element J2 (here, element J2 is one or more elements selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.). Ferroelectric materials include hafnium ... Furthermore, lead titanate (PbTiO X Piezoelectric ceramics having a perovskite structure, such as barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), and barium titanate, may also be used.
[0211] Furthermore, examples of materials that can exhibit ferroelectricity include metal nitrides containing elements M1, M2, and nitrogen. Here, element M1 is one or more elements selected from aluminum, gallium, indium, etc. Furthermore, element M2 is one or more elements selected from boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, etc. The ratio of the number of atoms of element M1 to the number of atoms of element M2 can be set as appropriate. Furthermore, metal oxides containing element M1 and nitrogen may exhibit ferroelectricity even without containing element M2. Furthermore, examples of materials that can exhibit ferroelectricity include materials in which element M3 is added to the above metal nitrides. Furthermore, element M3 is one or more elements selected from magnesium, calcium, strontium, zinc, cadmium, etc. Here, the ratio of the number of atoms of element M1 to the number of atoms of element M2 to the number of atoms of element M3 can be set as appropriate.
[0212] Furthermore, materials that can have ferroelectricity include SrTaO 2 N, BaTaO 2 Perovskite-type oxynitrides such as N, GaFeO with κ-alumina structure 3 Examples include:
[0213] Although metal oxides and metal nitrides have been described above as examples of materials that can have ferroelectricity, the materials are not limited to these. For example, metal oxynitrides in which nitrogen is added to the above-mentioned metal oxides, or metal oxynitrides in which oxygen is added to the above-mentioned metal nitrides, may also be used.
[0214] Furthermore, the material capable of exhibiting ferroelectricity may be, for example, a mixture or compound of multiple materials selected from the materials listed above. Alternatively, the insulating layer 130 may have a laminated structure of multiple materials selected from the materials listed above. However, since the crystal structure (characteristics) of the materials listed above may change depending not only on the film formation conditions but also on various processes, in this specification and the like, not only materials that exhibit ferroelectricity are referred to as ferroelectrics, but also as materials capable of exhibiting ferroelectricity.
[0215] Metal oxides containing either or both of hafnium and zirconium can have ferroelectricity even in thin films of a few nanometers. Furthermore, metal oxides containing either or both of hafnium and zirconium can have ferroelectricity even in very small areas. Therefore, by using metal oxides containing either or both of hafnium and zirconium, miniaturization of semiconductor devices can be achieved.
[0216] In this specification, a layer of a material that can have ferroelectricity may be referred to as a ferroelectric layer. Also, in this specification, a device having such a ferroelectric layer, metal oxide film, or metal nitride film may be referred to as a ferroelectric device.
[0217] Ferroelectricity is believed to be manifested by the displacement of oxygen or nitrogen in crystals contained in the ferroelectric layer due to an external electric field. Furthermore, the manifestation of ferroelectricity is presumed to depend on the crystal structure of the crystals contained in the ferroelectric layer. Therefore, for the insulating layer to exhibit ferroelectricity, the insulating layer 130 must contain crystals. In particular, it is preferable for the insulating layer to contain crystals having an orthorhombic crystal structure, as this will result in the manifestation of ferroelectricity. The crystal structure of the crystals contained in the insulating layer may be one or more selected from the group consisting of cubic, tetragonal, orthorhombic, monoclinic, and hexagonal. The insulating layer may also have an amorphous structure. In this case, the insulating layer may have a composite structure having an amorphous structure and a crystalline structure.
[0218] The insulating layer 250 functions as a gate insulating layer of the transistor 200. For the insulating layer 250, a material with a high dielectric constant is preferably used.
[0219] The insulating layer 250 preferably has a function of capturing and fixing hydrogen. This can reduce the hydrogen concentration in the oxide semiconductor layer 230 (particularly, the hydrogen concentration in the channel formation region of the transistor). O By reducing H, the channel forming region can be made i-type or substantially i-type.
[0220] Examples of materials for insulating layers capable of capturing or adhering hydrogen include metal oxides such as oxides containing hafnium, oxides containing aluminum, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing magnesium. These metal oxides may further contain zirconium, such as oxides containing hafnium and zirconium. Metal oxides with amorphous structures have dangling bonds in some oxygen atoms, which enhance their ability to capture or adsorb hydrogen. Therefore, these metal oxides preferably have an amorphous structure. For example, an amorphous structure may be achieved by including silicon in these oxides. For example, it is preferable to use an oxide containing hafnium and silicon (hafnium silicate). Metal oxides may have crystalline regions and / or grain boundaries in some regions.
[0221] The ability to capture or fix a corresponding substance can also be said to have the property of making it difficult for the corresponding substance to diffuse. Therefore, the ability to capture or fix a corresponding substance can be rephrased as barrier properties.
[0222] When the insulating layer 250 has a stacked structure, it is preferable to use a layer having a function of capturing and fixing hydrogen as one of the layers (hereinafter referred to as a first insulating layer of the insulating layer 250). Furthermore, by using a layer having a function of capturing and fixing hydrogen as a layer in contact with the oxide semiconductor layer 230 when the insulating layer 250 has a stacked structure of two layers, or as a layer close to the oxide semiconductor layer 230 when the insulating layer 250 has a stacked structure of three or more layers, hydrogen contained in the oxide semiconductor layer 230 can be more effectively captured or fixed. Therefore, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced.
[0223] Furthermore, the insulating layer 250 preferably includes a barrier insulating layer against hydrogen as a second insulating layer in addition to the first insulating layer. Examples of materials for the barrier insulating layer against hydrogen include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide.
[0224] The insulating layer 250 may be made of, for example, hafnium silicate as the first insulating layer. The first insulating layer of the insulating layer 250 preferably has an amorphous structure. The amorphous structure can suppress the formation of grain boundaries. Suppressing the formation of grain boundaries can improve the flatness of the insulating layer. This makes the film thickness distribution of the insulating layer uniform, reducing areas with extremely thin film thickness, thereby improving the breakdown voltage of the insulating layer. Furthermore, the film thickness distribution of the film provided on the insulating layer can be made uniform.
[0225] Furthermore, by suppressing the formation of grain boundaries in the insulating layer, it is possible to reduce leakage current caused by defect levels in the grain boundaries, and thus the insulating layer can function as an insulating film with low leakage current.
[0226] Furthermore, since hafnium oxide is a material with a high dielectric constant, hafnium silicate can also be a material with a high dielectric constant depending on the silicon content. Therefore, when the insulating layer 250a is used as a gate insulating layer, it is possible to reduce the gate potential applied during transistor operation while maintaining the physical film thickness of the gate insulating layer. Furthermore, it is possible to reduce the equivalent oxide thickness (EOT) of the gate insulating layer.
[0227] From the above, it is preferable to use an oxide containing one or both of aluminum and hafnium as the first insulating layer of the insulating layer 250, it is more preferable to use an oxide having an amorphous structure and containing one or both of aluminum and hafnium, and it is even more preferable to use aluminum oxide having an amorphous structure.
[0228] Furthermore, by using a barrier insulating layer against hydrogen as the second insulating layer of the insulating layer 250, it is possible to suppress diffusion of impurities contained in the conductive layer 260 into the oxide semiconductor layer 230. Silicon nitride has a high barrier property against hydrogen and is therefore suitable for the insulating layer 250b. Here, the second insulating layer is preferably an upper layer of the first insulating layer.
[0229] With such a structure, a semiconductor device having good electrical characteristics, high reliability, little variation in the electrical characteristics of the transistors, and a large on-state current can be provided.
[0230] Additionally, insulating layer 250 may comprise an insulating layer of a thermally stable structure, such as silicon oxide or silicon oxynitride.
[0231] The insulating layer 250 preferably includes a layer capable of supplying oxygen to the oxide semiconductor layer 230. An oxide can be used as the layer capable of supplying oxygen. When the insulating layer 250 includes silicon oxide or silicon oxynitride, oxygen can be suitably supplied from the insulating layer 250 to the oxide semiconductor layer 230.
[0232] Furthermore, the insulating layer 250 may have an insulating layer having a thermally stable structure between a pair of insulating layers having the functions of capturing and fixing hydrogen.
[0233] The insulating layer 250 preferably has a barrier insulating layer against oxygen, which can suppress oxidation of the conductive layer 240, the conductive layer 260, and the like. When the insulating layer 250 has a stacked structure, it is preferable that the layer in contact with the conductive layer 240 and the layer in contact with the conductive layer 260 each be a barrier insulating layer against oxygen.
[0234] The layer of the insulating layer 250 that is in contact with the conductive layer 240 is preferably less permeable to oxygen than at least the insulating layer 280. The layer has a barrier property against oxygen, which can prevent the side surfaces of the conductive layer 240 from being oxidized and an oxide film from being formed on the side surfaces. This can prevent a decrease in the on-state current or the field-effect mobility of the transistor 200.
[0235] For example, by using a barrier insulating layer against hydrogen and oxygen as the second insulating layer, it is possible to suppress oxidation of the conductive layer 260. Furthermore, it is possible to suppress the oxygen contained in the oxide semiconductor layer 230 from diffusing into the conductive layer 260 and the formation of oxygen vacancies in the oxide semiconductor layer 230.
[0236] Examples of the barrier insulating layer against oxygen include oxides containing hafnium, oxides containing aluminum, oxides containing aluminum and hafnium (hafnium aluminate), magnesium oxide, gallium oxide, gallium zinc oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide. Examples of oxides containing one or both of aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate).
[0237] Hafnium and silicon oxides (hafnium silicates) function as a barrier insulating layer against oxygen, and as mentioned above, they are also excellent insulating layers that can easily achieve an amorphous structure and have the ability to capture or fix hydrogen.
[0238] Furthermore, silicon nitride is an excellent insulating layer that not only functions as a barrier insulating layer against oxygen but also has high barrier properties against hydrogen, as described above.
[0239] The insulating layer 250 preferably has a two-layer structure in which a first insulating layer having a function of capturing or fixing hydrogen and a second insulating layer having a barrier property against hydrogen and oxygen are stacked in this order from the oxide semiconductor layer 230 side.
[0240] For example, the first insulating layer can be made of an oxide containing one or both of aluminum and hafnium, and the second insulating layer can be made of silicon nitride.
[0241] Here, when the insulating layer 250 has a two-layer structure, the first insulating layer can be applied as the insulating layer 250a shown in Figures 6A and 6B, and the second insulating layer can be applied as the insulating layer 250b.
[0242] Alternatively, when the thickness T1b of the insulating layer 250b is extremely thin, the insulating layer 250a may have a laminated structure of a first insulating layer and a second insulating layer.
[0243] Furthermore, the insulating layer 250c shown in FIGS. 8B and 8C can have the two-layer laminated structure described above.
[0244] The insulating layer 250 preferably has a three-layer structure in which, from the oxide semiconductor layer 230 side, a third insulating layer made of a material with a relatively low dielectric constant, a first insulating layer having a function of capturing or fixing hydrogen, and a second insulating layer having barrier properties against hydrogen and oxygen are stacked in this order. The material of the third insulating layer with a relatively low dielectric constant refers to, for example, a material with a lower dielectric constant than any one or more of the other layers in the stacked structure. Here, silicon oxide or silicon oxynitride can be used as the third insulating layer. The third insulating layer is a layer in contact with the oxide semiconductor layer 230. Using an oxide for the third insulating layer can supply oxygen to the oxide semiconductor layer 230. Furthermore, providing the second insulating layer can suppress diffusion of oxygen contained in the third insulating layer into the conductive layer 260, thereby suppressing oxidation of the conductive layer 260. Furthermore, a decrease in the amount of oxygen supplied from the third insulating layer to the oxide semiconductor layer 230 can be suppressed.
[0245] As an example, silicon oxide or silicon oxynitride can be used as the third insulating layer, an oxide containing one or both of aluminum and hafnium can be used as the first insulating layer, and silicon nitride can be used as the second insulating layer.
[0246] 6A and 6B, the insulating layer 250a may have a two-layer laminate structure of a third insulating layer and a first insulating layer, and the insulating layer 250b may have a second insulating layer. Alternatively, the insulating layer 250a may have a third insulating layer, and the insulating layer 250b may have a two-layer laminate structure of a first insulating layer and a second insulating layer.
[0247] Alternatively, when the thickness T1b of the insulating layer 250b is extremely thin, the insulating layer 250a may have a laminated structure of a third insulating layer, a first insulating layer, and a second insulating layer.
[0248] Furthermore, the insulating layer 250c shown in FIGS. 8B and 8C can have the above-described three-layer laminated structure.
[0249] The insulating layer 250 preferably has a four-layer structure in which, from the oxide semiconductor layer 230 side, a fourth insulating layer having a barrier property against oxygen, a third insulating layer made of a material with a relatively low dielectric constant, a first insulating layer having a function of capturing or fixing hydrogen, and a second insulating layer having a barrier property against hydrogen and oxygen are stacked in this order. The first to third insulating layers can have the same structure as the layers used in the above-described three-layer structure. The fourth insulating layer is in contact with the oxide semiconductor layer 230. The fourth insulating layer has a barrier property against oxygen, which can prevent oxygen from being released from the oxide semiconductor layer 230. For example, aluminum oxide may be used as the fourth insulating layer. Aluminum oxide has a function of capturing or fixing hydrogen, and is therefore suitable as the fourth insulating layer in contact with the oxide semiconductor layer 230.
[0250] As an example, aluminum oxide can be used as the fourth insulating layer, silicon oxide or silicon oxynitride can be used as the third insulating layer, an oxide containing one or both of aluminum and hafnium can be used as the first insulating layer, and silicon nitride can be used as the second insulating layer.
[0251] Here, when the insulating layer 250 has the four-layer structure described above, the insulating layer 250a shown in Figures 6A and 6B can be a three-layer laminated structure of a fourth insulating layer, a third insulating layer, and a first insulating layer, and the insulating layer 250b can be a second insulating layer. Alternatively, the insulating layer 250a can be a two-layer laminated structure of a fourth insulating layer and a third insulating layer, and the insulating layer 250b can be a two-layer laminated structure of a first insulating layer and a second insulating layer. Alternatively, the insulating layer 250a can be a fourth insulating layer, and the insulating layer 250b can be a three-layer laminated structure of a third insulating layer, a first insulating layer, and a second insulating layer.
[0252] Alternatively, when the thickness T1b of the insulating layer 250b is extremely thin, the insulating layer 250a may have a four-layer laminate structure of a fourth insulating layer, a third insulating layer, a first insulating layer, and a second insulating layer.
[0253] Furthermore, the insulating layer 250c shown in FIGS. 8B and 8C can have the four-layer laminate structure described above.
[0254] The insulating layer 250d can be made of one or more materials selected from the above-described materials applicable to the insulating layer 250. The insulating layer 250d can preferably be formed using a method for selectively growing the insulating layer 250 on a metal.
[0255] In particular, the thickness of the insulating layer 250 in a region overlapping with the channel formation region of the oxide semiconductor layer 230 is preferably 0.1 nm to 30 nm, more preferably 0.1 nm to 20 nm, still more preferably 0.1 nm to 10 nm, still more preferably 0.1 nm to 8.0 nm, and still more preferably 0.5 nm to 7.0 nm.
[0256] In order to miniaturize transistors, it is preferable that the thickness of each layer constituting the insulating layer 250 is thin. For example, the thickness of each layer constituting the insulating layer 250 is 0.1 nm to 10 nm, or 0.1 nm to 5 nm, or 0.5 nm to 5 nm, or 1 nm to less than 5 nm, or 1 nm to 3 nm. Note that it is sufficient that each layer constituting the insulating layer 250 has a region with the above-mentioned thickness in at least a portion thereof.
[0257] Typically, the thicknesses of the fourth insulating layer, the third insulating layer, the first insulating layer, and the second insulating layer are 1 nm, 2 nm, 2 nm, and 1 nm, respectively. With such a structure, the transistor can have good electrical characteristics even when miniaturized or highly integrated.
[0258] Since the insulating layer 210 functions as an interlayer film, it is preferable that the insulating layer 210 has a low dielectric constant. By using a material with a low dielectric constant for the interlayer film, the parasitic capacitance generated between wirings can be reduced. Silicon oxide and silicon oxynitride are both thermally stable, and therefore are suitable for the insulating layer 210.
[0259] The concentration of impurities such as water and hydrogen in the insulating layer 210 is preferably reduced, which can prevent impurities such as water and hydrogen from entering the channel formation region of the oxide semiconductor layer 230.
[0260] A barrier insulating layer against hydrogen is preferably used as the insulating layer 210. When the insulating layer 210 provided on the outer side of the oxide semiconductor layer 230 has a barrier property against hydrogen, diffusion of hydrogen into the oxide semiconductor layer 230 can be suppressed.
[0261] Examples of materials for the barrier insulating layer against hydrogen include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide.
[0262] For example, it is preferable to use a silicon nitride film as the insulating layer 210 .
[0263] An insulating layer having a function of capturing or fixing hydrogen is preferably used for the insulating layer 222. In this way, hydrogen in the oxide semiconductor layer 230 can be diffused to the insulating layer 222 through the conductive layer 220 and the hydrogen can be captured or fixed. Therefore, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced.
[0264] For example, it is preferable to use a silicon nitride film as the insulating layer 210 and an oxide film containing hafnium and silicon (hafnium silicate film) as the insulating layer 222 .
[0265] A barrier insulating layer against hydrogen is preferably used for the insulating layer 283. This can suppress diffusion of hydrogen from above the insulating layer 283 to the oxide semiconductor layer 230. A silicon nitride film and a silicon nitride oxide film each have characteristics of releasing little impurities (for example, water and hydrogen) from themselves and being less permeable to oxygen and hydrogen, and therefore can be suitably used for the insulating layer 283.
[0266] It is particularly preferable to use silicon nitride formed by a sputtering method as the insulating layer 283. The sputtering method does not require the use of molecules containing hydrogen in the deposition gas, and therefore can reduce the hydrogen concentration in the insulating layer 283. Furthermore, by forming the insulating layer 283 by a sputtering method, silicon nitride with high density can be formed.
[0267] Alternatively, an insulating layer having a function of capturing or fixing hydrogen may be used as the insulating layer 283. With such a structure, diffusion of hydrogen from above the insulating layer 283 to the oxide semiconductor layer 230 can be suppressed, and further, hydrogen contained in the oxide semiconductor layer 230 can be captured or fixed. Therefore, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced. Hafnium silicate or the like can be used as the insulating layer 283.
[0268] Alternatively, the insulating layer 283 may have a stacked structure of an insulating layer having a function of capturing or fixing hydrogen and a barrier insulating layer against hydrogen. For example, the insulating layer 283 may be a stacked film of aluminum oxide and silicon nitride over the aluminum oxide.
[0269] The insulating layer 280 preferably includes the aforementioned barrier insulating layer against hydrogen. The insulating layer 280 is provided so as to surround the oxide semiconductor layer 230. When the insulating layer 280 provided on the outer side of the oxide semiconductor layer 230 has a barrier property against hydrogen, it is possible to suppress diffusion of hydrogen into the oxide semiconductor layer 230. For example, the insulating layer 280 preferably includes a silicon nitride film.
[0270] Silicon nitride also has a barrier property against oxygen. Therefore, by using silicon nitride for the insulating layer 280, oxygen can be prevented from being extracted from the oxide semiconductor layer 230, and excessive oxygen vacancies can be prevented from being formed in the oxide semiconductor layer 230.
[0271] Furthermore, the use of silicon nitride for the insulating layer 280 can prevent excess oxygen from being supplied to the oxide semiconductor layer 230. Thus, excess oxygen can be prevented from being contained in the channel formation region of the oxide semiconductor layer 230, thereby improving the reliability of the transistor 200.
[0272] The insulating layer 280 preferably includes the above-described insulating oxide insulating film, the oxynitride insulating film, or the insulating layer having a region containing excess oxygen.
[0273] For example, an insulating layer having a region containing excess oxygen can be formed by sputtering in an oxygen-containing atmosphere. Furthermore, by using a sputtering method in which hydrogen-containing molecules are not used in the deposition gas, the hydrogen concentration in the insulating layer 280 can be reduced. By depositing at least some of the layers constituting the insulating layer 280 in this manner, oxygen can be supplied from the insulating layer 280 to the channel formation region of the oxide semiconductor layer 230, thereby reducing oxygen vacancies and VoH.
[0274] The concentration of impurities such as water and hydrogen in the insulating layer 280 is preferably reduced, which can prevent impurities such as water and hydrogen from entering the channel formation region of the oxide semiconductor layer 230.
[0275] Note that the thickness of the insulating layer 280 on the conductive layer 220 corresponds to the channel length of the transistor 200 , and therefore the thickness of the insulating layer 280 is set appropriately in accordance with the design value of the channel length of the transistor 200 .
[0276] 6A and 6B includes an insulating layer 280a, an insulating layer 280b on the insulating layer 280a, and an insulating layer 280c on the insulating layer 280b.
[0277] The insulating layer 280b is a layer in contact with a channel formation region of the oxide semiconductor layer 230. When an insulating layer containing oxygen is used as the insulating layer 280b, oxygen can be supplied to the oxide semiconductor layer 230.
[0278] The insulating layer 280b preferably has a region with a higher oxygen content than at least one of the insulating layer 280a and the insulating layer 280c. In particular, the insulating layer 280b preferably has a region with a higher oxygen content than each of the insulating layer 280a and the insulating layer 280c. Increasing the oxygen content of the insulating layer 280b makes it easier to form an i-type region in the oxide semiconductor layer 230 near the insulating layer 280b.
[0279] It is more preferable to use a film that releases oxygen by heating for the insulating layer 280b. When the insulating layer 280b releases oxygen due to heat applied during the manufacturing process of the transistor 200, oxygen can be supplied to the oxide semiconductor layer 230. When oxygen is supplied from the insulating layer 280b to the oxide semiconductor layer 230, particularly to the channel formation region of the oxide semiconductor layer 230, oxygen vacancies and V in the oxide semiconductor layer 230 can be reduced. O H can be reduced, and a highly reliable transistor can be obtained that exhibits favorable electrical characteristics.
[0280] To improve the electrical characteristics and reliability of an OS transistor, it is important to sufficiently reduce the hydrogen concentration in the oxide semiconductor and then optimize the amount of oxygen supplied to the oxide semiconductor.
[0281] As an example, the amount of oxygen molecules released from the insulating layer 280b is 1.0×10 14 molecules / cm 2 That's it, 1.0 x 10 15 molecules / cm 2 The amount of released oxygen molecules can be measured by thermal desorption spectroscopy.
[0282] In particular, when the channel length of the transistor 200 is small, oxygen vacancies in the channel formation region and V O The influence of H on the electrical characteristics and reliability is particularly large. Therefore, by sufficiently reducing the hydrogen concentration in the oxide semiconductor layer 230 and then optimizing the amount of oxygen supplied to the oxide semiconductor layer 230, a transistor with a short channel length, favorable electrical characteristics, and high reliability can be realized.
[0283] The insulating layer 280b is preferably formed by a deposition method such as a sputtering method or a PECVD method. In particular, when a sputtering method is used, hydrogen gas is not used as a deposition gas, and therefore a film with an extremely low hydrogen content can be obtained. Therefore, supply of hydrogen to the oxide semiconductor layer 230 can be suppressed, and the electrical characteristics of the transistor 200 can be stabilized.
[0284] To increase the amount of oxygen supplied to the oxide semiconductor layer 230, for example, heat treatment in an oxygen-containing atmosphere or plasma treatment in an oxygen-containing atmosphere may be performed after the insulating layer 280b is formed. Alternatively, oxygen may be supplied by forming an oxide film on the top surface of the insulating layer 280b by a sputtering method in an oxygen atmosphere. The oxide film may then be removed. By performing such treatment, oxygen can be supplied to the insulating layer 280b, and the amount of oxygen supplied to the oxide semiconductor layer 230 can be increased.
[0285] Furthermore, the region of the oxide semiconductor layer 230 in contact with the insulating layer 280a and the region of the oxide semiconductor layer 230 in contact with the insulating layer 280c receives a smaller amount of oxygen than the region of the oxide semiconductor layer 230 in contact with the insulating layer 280b. Therefore, the region of the oxide semiconductor layer 230 in contact with the insulating layer 280a and the region of the oxide semiconductor layer 230 in contact with the insulating layer 280c may have a lower resistance. In other words, by adjusting the thickness of the insulating layer 280a, the range of the region that functions as one of the source region and the drain region can be controlled. Similarly, by adjusting the thickness of the insulating layer 280c, the range of the region that functions as the other of the source region and the drain region can be controlled. In this way, the thicknesses of the insulating layers 280a and 280c can be appropriately set according to the characteristics desired for the transistor.
[0286] Furthermore, it is preferable to use a material with a low relative dielectric constant for the insulating layer 280b, which can reduce the parasitic capacitance that occurs between wirings. For example, silicon oxide or silicon oxynitride can be used for the insulating layer 280b.
[0287] It is preferable that the insulating layer 280a and the insulating layer 280c each be a barrier insulating layer against oxygen. By providing the insulating layer 280a between the insulating layer 280b and the conductive layer 220, it is possible to prevent the conductive layer 220 from being oxidized and the resistance of the conductive layer 220 from increasing. Furthermore, by providing the insulating layer 280c between the insulating layer 280b and the conductive layer 240, it is possible to prevent the conductive layer 240 from being oxidized and the resistance of the conductive layer 240 from increasing.
[0288] Alternatively, the insulating layer 280a may be an insulating layer having a function of capturing or fixing hydrogen. Such a structure can suppress diffusion of hydrogen from below the insulating layer 280a into the oxide semiconductor layer 230 and further allow hydrogen contained in the oxide semiconductor layer 230 to be captured or fixed. This reduces the hydrogen concentration in the oxide semiconductor layer 230. The insulating layer 280a may be made of magnesium oxide, aluminum oxide, hafnium oxide, or an oxide containing hafnium and silicon. Alternatively, the insulating layer 280a may be made of, for example, a stacked film of aluminum oxide and silicon nitride on the aluminum oxide. Similarly, the insulating layer 280c may be made of an insulating layer having a function of capturing or fixing hydrogen.
[0289] For example, the insulating layers 280a and 280c can be formed using silicon nitride, and the insulating layer 280b can be formed using silicon oxide.
[0290] [Conductive Layer] The conductive layers (conductive layer 220, conductive layer 240, conductive layer 260, etc.) of the semiconductor device preferably contain a metal element selected from tungsten, copper, aluminum, chromium, silver, gold, platinum, zinc, tantalum, nickel, titanium, iron, cobalt, molybdenum, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing the above-mentioned metal element as a component, or an alloy combining the above-mentioned metal elements. As the alloy containing the above-mentioned metal element as a component, a nitride of the alloy or an oxide of the alloy may be used. For example, tantalum nitride, titanium nitride, ruthenium nitride, nitride containing molybdenum, nitride containing tungsten, titanium, and aluminum, nitride containing tantalum and aluminum, ruthenium oxide, oxide containing strontium and ruthenium, oxide containing lanthanum and nickel, etc. are preferably used. Furthermore, semiconductors with high electrical conductivity, such as polycrystalline silicon containing impurity elements such as phosphorus, and silicides such as nickel silicide may also be used.
[0291] Nitrogen-containing conductive materials, such as nitrides containing tantalum, nitrides containing titanium, nitrides containing molybdenum, nitrides containing tungsten, nitrides containing ruthenium, nitrides containing tantalum and aluminum, or nitrides containing titanium and aluminum; oxygen-containing conductive materials, such as ruthenium oxide, oxides containing strontium and ruthenium, or oxides containing lanthanum and nickel; and materials containing metal elements, such as titanium, tantalum, or ruthenium, are preferred because they are conductive materials that are resistant to oxidation, have a function of suppressing oxygen diffusion, or maintain conductivity even after absorbing oxygen. Examples of oxygen-containing conductive materials include indium oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide (also referred to as ITO), indium tin oxide containing titanium oxide, indium tin oxide with added silicon (also referred to as ITSO), indium zinc oxide (also referred to as IZO®), and indium zinc oxide containing tungsten oxide. In this specification and the like, a conductive film formed using a conductive material containing oxygen may be referred to as an oxide conductive film.
[0292] Conductive materials based on tungsten, copper, or aluminum are preferred because they have high conductivity.
[0293] Furthermore, a plurality of conductive layers formed from the above materials may be stacked. For example, a stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing oxygen. A stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing nitrogen. A stacked structure may be formed by combining the above-described material containing a metal element, a conductive material containing oxygen, and a conductive material containing nitrogen.
[0294] When a metal oxide is used for the channel formation region of a transistor, the conductive layer that functions as a gate electrode preferably has a stacked structure that combines a material containing the metal element and a conductive material containing oxygen. In this case, the conductive material containing oxygen is preferably provided on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen desorbed from the conductive material is easily supplied to the channel formation region.
[0295] The conductive layer 260 can be made of the above-mentioned metal elements, alloys containing the above-mentioned metal elements, or alloys combining the above-mentioned metal elements. For example, it is preferable to use a highly conductive material such as tungsten. Furthermore, it is preferable to use a conductive material that is resistant to oxidation or a conductive material that has the function of suppressing oxygen diffusion as the conductive layer 260. As described above, examples of such conductive materials include conductive materials containing nitrogen and conductive materials containing oxygen. This can suppress a decrease in the conductivity of the conductive layer 260.
[0296] The conductive layer 260 is preferably made of a conductive material containing oxygen and a metal element contained in the metal oxide in which the channel is formed. Alternatively, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide to which silicon is added may be used. Nitrogen-containing indium gallium zinc oxide may also be used. Using such a material may allow hydrogen contained in the metal oxide in which the channel is formed to be captured. Alternatively, hydrogen introduced from an outer insulating layer or the like may be captured.
[0297] The conductive layer 260 may have a thickness of, for example, 3 nm or more and 500 nm or less. The thickness of the conductive layer 260 may be, for example, equal to or greater than the thickness of the insulating layer 250. By making the conductive layer 260 thicker, the resistance of the conductive layer 260 can be reduced.
[0298] Alternatively, the conductive layer 260 may have a two-layer structure including a conductive layer 260a and a conductive layer 260b on the conductive layer 260a.
[0299] By using a conductive material having a function of suppressing oxygen diffusion as the conductive layer 260a, for example, release of oxygen from the oxide semiconductor layer 230 can be suppressed, and formation of oxygen vacancies in the oxide semiconductor layer 230 can be suppressed.
[0300] Furthermore, by using a conductive material that is resistant to oxidation as the conductive layer 260a, it is possible to prevent the conductive layer 260a from being oxidized and its conductivity from being reduced due to, for example, the release of oxygen from the oxide semiconductor layer 230 or the release of oxygen from the insulating layer 250.
[0301] The material used for the conductive layer 260b preferably has higher conductivity than the material used for the conductive layer 260a, for example. In addition, by making the conductive layer 260b thicker, the current flowing through the conductive layer 260b can be further increased.
[0302] By using a film formation method with high coverage for the conductive layer 260 a, the conductive layer 260 a can be suitably formed along the sidewall of the opening 290 .
[0303] The conductive layer 260a can be, for example, a conductive material containing nitrogen, a conductive material containing oxygen, etc. Alternatively, the conductive layer 260a can be, for example, a conductive material containing oxygen and a metal element contained in a metal oxide in which a channel is formed.
[0304] For example, a conductive material containing the above-mentioned metal element and nitrogen can be used as the conductive layer 260a, such as tantalum nitride, titanium nitride, ruthenium nitride, nitrides containing molybdenum, nitrides containing tungsten, titanium, and aluminum, nitrides containing tantalum and aluminum, etc.
[0305] Furthermore, the conductive layer 260a can be made of a conductive material containing the aforementioned metal element and oxygen, such as ruthenium oxide, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel.
[0306] Alternatively, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide doped with silicon may be used. Alternatively, indium gallium zinc oxide containing nitrogen may be used.
[0307] Furthermore, as the conductive layer 260a, materials containing titanium, tantalum, ruthenium, and one or more selected from these metal elements are preferred because they are conductive materials that are resistant to oxidation, conductive materials that have the function of suppressing oxygen diffusion, or materials that maintain conductivity even when absorbing oxygen.
[0308] The conductive layer 260b may be made of, for example, the above-mentioned metal elements, alloys containing the above-mentioned metal elements, or alloys combining the above-mentioned metal elements. For example, tungsten may be used.
[0309] The conductive layer 260a may further have a stacked structure. The conductive layer 260b may further have a stacked structure. When the conductive layer 260a has a stacked structure, for example, a plurality of materials that can be used for the conductive layer 260a may be stacked. Alternatively, a plurality of materials selected from the materials that can be used for the conductive layer of one embodiment of the present invention may be stacked. When the conductive layer 260b has a stacked structure, for example, a plurality of materials that can be used for the conductive layer 260b may be stacked. Alternatively, a plurality of materials selected from the materials that can be used for the conductive layer of one embodiment of the present invention may be stacked.
[0310] The conductive layer 220 and the conductive layer 240 are conductive layers in contact with the oxide semiconductor layer 230, and therefore, it is preferable to use a conductive material that is resistant to oxidation, a conductive material that maintains low electrical resistance even when oxidized, an oxide conductive material, or a conductive material that has a function of suppressing oxygen diffusion, for each of them. Examples of such conductive materials include a conductive material containing nitrogen and a conductive material containing oxygen. This can suppress a decrease in the conductivity of the conductive layer 220 and the conductive layer 240.
[0311] By using a conductive material containing oxygen for the conductive layer 220 or the conductive layer 240, the conductive layer 220 or the conductive layer 240 can maintain its conductivity even if it absorbs oxygen. In addition, even when an insulating layer containing oxygen, such as hafnium oxide, is used as the insulating layer 210, the conductive layer 220 is preferable because it can maintain its conductivity. For example, ITO, ITSO, IZO (registered trademark), or the like is preferably used for each of the conductive layer 220 and the conductive layer 240.
[0312] When the conductive layer 220 has a three-layer structure of a first conductive layer, a second conductive layer, and a third conductive layer formed in this order on the insulating layer 210, it is preferable to use, for example, a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion as the first conductive layer, a material with high conductivity as the second conductive layer, and a conductive material containing oxygen as the third conductive layer. Specifically, it is preferable to use, for example, titanium nitride as the first conductive layer, tungsten as the second conductive layer, and ITO or ITSO as the third conductive layer. In this case, titanium nitride is in contact with the insulating layer 210, and ITO or ITSO is in contact with the oxide semiconductor layer 230. With this structure, the conductive layer 220 can maintain conductivity even when in contact with the oxide semiconductor layer 230. Furthermore, when an oxide insulating layer is used for the insulating layer 210, the insulating layer 210 can prevent the conductive layer 220 from being excessively oxidized. Furthermore, when tungsten, which has high conductivity, is used for the second conductive layer, the conductivity of the conductive layer 220 can be increased.
[0313] 1B and 1C show a configuration in which the upper surface of the conductive layer 220 is flat, but the present invention is not limited to this. For example, a recess that overlaps with the opening 290 may be formed in the upper surface of the conductive layer 220. By forming at least a portion of the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 so as to fill the recess, it becomes easier to apply the gate electric field of the conductive layer 260 up to the vicinity of the conductive layer 220 of the oxide semiconductor layer 230.
[0314] Furthermore, when the conductive layer 240 has a two-layer stacked structure, for example, it is preferable to use a material with higher conductivity for the lower layer than the upper layer and a conductive material containing oxygen for the upper layer. Specifically, for example, it is preferable to use ruthenium, tungsten, titanium nitride, or tantalum nitride for the lower layer and ITO or ITSO for the upper layer. In this case, ITO or ITSO is in contact with the oxide semiconductor layer 230. With such a structure, the conductive layer 240 can maintain conductivity even when in contact with the oxide semiconductor layer 230. Furthermore, by using a material with higher conductivity than the upper layer for the lower layer, the conductivity of the conductive layer 240 can be increased.
[0315] [Oxide Semiconductor Layer 230] As described above, the oxide semiconductor layer 230 has a channel formation region. The channel formation region is i-type (intrinsic) or substantially i-type. The oxide semiconductor layer 230 further has a source region and a drain region. The source region and the drain region are n-type regions (low-resistance regions) with higher carrier concentrations than the channel formation region.
[0316] The crystallinity of a semiconductor material used for the oxide semiconductor layer 230 is not particularly limited, and any of an amorphous semiconductor, a single crystal semiconductor, and a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part) may be used. Use of a single crystal semiconductor or a crystalline semiconductor is preferable because deterioration of transistor characteristics can be suppressed.
[0317] The band gap of a metal oxide functioning as a semiconductor is preferably 2.0 eV or more, more preferably 2.5 eV or more. By using a metal oxide with a wide band gap, the off-state current of a transistor can be reduced. Because the off-state current of an OS transistor is low, the power consumption of a semiconductor device can be sufficiently reduced. Furthermore, because the frequency characteristics of an OS transistor are high, the semiconductor device can operate at high speed.
[0318] Examples of metal oxides that can be used for the oxide semiconductor layer 230 include indium oxide, gallium oxide, and zinc oxide. The metal oxide preferably contains at least indium (In) or zinc (Zn). The metal oxide preferably contains two or three elements selected from indium, element M, and zinc. Note that element M is a metal element or a metalloid element having a high bond energy with oxygen, for example, a metal element or a metalloid element having a bond energy with oxygen higher than that of indium. Specific examples of element M include aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony. The element M contained in the metal oxide is preferably one or more of the above elements, more preferably one or more selected from aluminum, gallium, tin, and yttrium, and even more preferably gallium. In this specification and the like, metal elements and metalloid elements may be collectively referred to as "metal elements," and the "metal elements" described in this specification and the like may include metalloid elements.
[0319] The oxide semiconductor layer 230 may be formed of, for example, indium oxide (In oxide), indium zinc oxide (In—Zn oxide, also referred to as IZO (registered trademark)), indium tin oxide (In—Sn oxide), indium titanium oxide (In—Ti oxide), indium gallium oxide (In—Ga oxide), indium gallium aluminum oxide (In—Ga—Al oxide), indium gallium tin oxide (In—Ga—Sn oxide, also referred to as IGTO), gallium zinc oxide (Ga—Zn oxide, also referred to as GZO), aluminum zinc oxide (Al—Zn oxide, also referred to as AZO), Examples of usable oxides include indium aluminum zinc oxide (In-Al-Zn oxide, also referred to as IAZO), indium tin zinc oxide (In-Sn-Zn oxide, also referred to as ITZO (registered trademark)), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium zinc oxide (In-Ga-Zn oxide, also referred to as IGZO), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide, also referred to as IGZTO), and indium gallium aluminum zinc oxide (In-Ga-Al-Zn oxide, also referred to as IGAZO, IGZAO, or IAGZO). Alternatively, silicon-containing indium tin oxide, gallium tin oxide (Ga-Sn oxide), aluminum tin oxide (Al-Sn oxide), and the like can be used. Alternatively, the above oxides having an amorphous structure can be used. For example, indium oxide having an amorphous structure, indium tin oxide having an amorphous structure, or the like can be used.
[0320] By increasing the ratio of the number of indium atoms to the total number of atoms of all metal elements contained in the metal oxide, the field-effect mobility of the transistor can be increased, and a transistor with a large on-state current can be realized.
[0321] Note that the metal oxide may contain one or more metal elements with a larger periodic number instead of or in addition to indium. The greater the overlap of the orbitals of the metal elements, the greater the carrier conduction in the metal oxide. Therefore, including a metal element with a larger periodic number may improve the field-effect mobility of a transistor. Examples of metal elements with a larger periodic number include metal elements belonging to the fifth period and the sixth period. Specific examples of such metal elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium. Note that lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium are called light rare earth elements.
[0322] The metal oxide may also contain one or more nonmetallic elements. The presence of a nonmetallic element in the metal oxide may increase the carrier concentration or narrow the band gap, thereby increasing the field-effect mobility of the transistor. Examples of nonmetallic elements include carbon, nitrogen, phosphorus, sulfur, selenium, fluorine, chlorine, bromine, and hydrogen.
[0323] Furthermore, by increasing the ratio of the number of zinc atoms to the sum of the numbers of atoms of all metal elements contained in the metal oxide, the metal oxide can be made highly crystalline, and the diffusion of impurities in the metal oxide can be suppressed, thereby suppressing fluctuations in the electrical characteristics of the transistor and improving its reliability.
[0324] Furthermore, by increasing the ratio of the number of atoms of element M to the sum of the number of atoms of all metal elements contained in the metal oxide, a metal oxide with a wide band gap can be obtained. Furthermore, the formation of oxygen vacancies in the metal oxide can be suppressed. Therefore, carrier generation due to oxygen vacancies can be suppressed, resulting in a transistor with a low off-state current. Furthermore, a shift in the threshold voltage of the transistor can be suppressed. Furthermore, fluctuations in the electrical characteristics of the transistor can be suppressed, resulting in improved reliability.
[0325] The electrical characteristics and reliability of a transistor vary depending on the composition of the metal oxide used in the oxide semiconductor layer 230. Therefore, by varying the composition of the metal oxide depending on the electrical characteristics and reliability required of the transistor, a semiconductor device with both excellent electrical characteristics and high reliability can be provided.
[0326] When the metal oxide is an In-M-Zn oxide, the atomic ratio of In in the In-M-Zn oxide is preferably equal to or greater than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxides include In:M:Zn=1:1:0.5, In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=1:1:2, In:M:Zn=2:1:3, In:M:Zn=3:1:1, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:3, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, and compositions close to these. Note that the term "nearby composition" includes a range of ±30% of the desired atomic ratio. By increasing the atomic ratio of indium in the metal oxide, the on-state current, field-effect mobility, and the like of the transistor can be increased.
[0327] Furthermore, the atomic ratio of In in the In-M-Zn oxide may be less than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxide include In:M:Zn=1:3:2, In:M:Zn=1:3:3, In:M:Zn=1:3:4, and compositions close to these. By increasing the proportion of M atoms in the metal oxide, the generation of oxygen vacancies can be suppressed.
[0328] When the element M contains a plurality of metal elements, the total proportion of the number of atoms of the metal elements can be used as the proportion of the number of atoms of the element M.
[0329] In this specification and the like, the ratio of the number of indium atoms to the sum of the numbers of atoms of all contained metal elements may be referred to as the indium content. The same applies to other metal elements.
[0330] Furthermore, when the metal oxide is an In-Zn oxide, the atomic ratio of the metal elements in the In-Zn oxide may be, for example, In:Zn = 1:1, In:Zn = 2:1, In:Zn = 4:1, or a composition in the vicinity thereof. The In-Zn oxide may also contain a trace amount of element M. For example, when Sn is contained as element M, the atomic ratio of the metal elements in the metal oxide may be, for example, In:Sn:Zn = 2:0.1:1, In:Sn:Zn = 4:0.1:1, or a composition in the vicinity thereof.
[0331] For example, energy dispersive X-ray spectrometry (EDX), X-ray photoelectron spectrometry (XPS), inductively coupled plasma mass spectrometry (ICP-MS), or inductively coupled plasma atomic emission spectrometry (ICP-AES) can be used to analyze the composition of the metal oxide used in the oxide semiconductor layer 230. Alternatively, a combination of these techniques may be used for the analysis. For elements with low content, the actual content may differ from the content obtained by analysis due to the influence of analytical accuracy. For example, when the content of element M is low, the content of element M obtained by analysis may be lower than the actual content.
[0332] The sputtering method or the ALD method can be suitably used for forming the metal oxide. When forming the metal oxide by the sputtering method, the composition of the metal oxide after film formation may differ from the composition of the target. In particular, the zinc content in the metal oxide after film formation may decrease to about 50% compared to the target. In addition, the metal oxide film may be formed by a chemical vapor deposition (CVD) method, a molecular beam epitaxy (MBE) method, a pulsed laser deposition (PLD) method, or the like.
[0333] The oxide semiconductor layer 230 may have a stacked structure including two or more metal oxide layers. The two or more metal oxide layers included in the oxide semiconductor layer 230 may have the same or approximately the same composition. By using a stacked structure of metal oxide layers having the same composition, for example, the same sputtering target can be used for formation, thereby reducing manufacturing costs.
[0334] The two or more metal oxide layers included in the oxide semiconductor layer 230 may have different compositions.
[0335] The oxide semiconductor layer 230 may have, for example, a two-layer structure. Fig. 5A shows an example in which the oxide semiconductor layer 230 has a two-layer structure of an oxide layer 230a and an oxide layer 230b on the oxide layer 230a in the structure shown in Fig. 2A.
[0336] For example, the oxide layer 230a is preferably made of a material having higher conductivity than the oxide layer 230b. By using a material having high conductivity for the oxide layer 230a in contact with the source electrode and the drain electrode (the conductive layer 220 and the conductive layer 240), the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced, and a transistor with high on-state current can be obtained.
[0337] Here, if a material with high conductivity is used for the oxide layer 230b provided on the conductive layer 260 side functioning as the gate electrode, the threshold voltage of the transistor 200 may shift, and the drain current (hereinafter also referred to as cutoff current) that flows when the gate voltage is 0 V may become large. Specifically, when the transistor 200 is an n-channel transistor, the threshold voltage may become low. Therefore, it is preferable to use a material with lower conductivity than the oxide layer 230a for the oxide layer 230b. As a result, when the transistor 200 is an n-channel transistor, the threshold voltage can be increased, and the transistor can have a small cutoff current. Note that a small cutoff current may be referred to as a normally-off transistor.
[0338] As described above, by using a material having higher conductivity than that of the oxide layer 230b for the oxide semiconductor layer 230 having a stacked structure, a normally-off transistor with a large on-state current can be obtained. Therefore, a semiconductor device with both low power consumption and high performance can be provided.
[0339] The carrier concentration of the oxide layer 230a is preferably higher than that of the oxide layer 230b. Increasing the carrier concentration of the oxide layer 230a increases the conductivity, and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced, resulting in a transistor with a large on-state current. In addition, decreasing the carrier concentration of the oxide layer 230b decreases the conductivity, resulting in a normally-off transistor.
[0340] Note that the oxide semiconductor layer 230 is not limited to the above-described structure, and the oxide layer 230a may be made of a material having lower conductivity than the oxide layer 230b. The carrier concentration of the oxide layer 230a may be lower than the carrier concentration of the oxide layer 230b.
[0341] The band gap of the first metal oxide used in the oxide layer 230 a is preferably different from the band gap of the second metal oxide used in the oxide layer 230 b. For example, the difference between the band gaps of the first metal oxide and the second metal oxide is preferably 0.1 eV or more, more preferably 0.2 eV or more, and even more preferably 0.3 eV or more.
[0342] The band gap of the first metal oxide used for the oxide layer 230a is preferably smaller than the band gap of the second metal oxide used for the oxide layer 230b. This can reduce the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240, thereby enabling a transistor with large on-state current. Furthermore, when the transistor 200 is an n-channel transistor, the threshold voltage can be increased, enabling the transistor to be a normally-off transistor. Furthermore, the large band gap of the second metal oxide can suppress generation and induction of carriers in the oxide layer 230b and at the interface between the oxide layer 230b and the insulating layer 250. This can improve the reliability of the transistor.
[0343] For example, it is preferable that the content of element M in the first metal oxide is lower than the content of element M in the second metal oxide. More specifically, it is preferable that the oxide layer 230a uses a metal oxide having a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition thereabout, and the oxide layer 230b uses a metal oxide having a composition of In:M:Zn=1:3:2 [atomic ratio] or a composition thereabout. In this case, it is particularly preferable to use one or more of gallium, aluminum, and tin as the element M.
[0344] Note that the oxide semiconductor layer 230 is not limited to the above-described structure, and the band gap of the first metal oxide may be larger than the band gap of the second metal oxide.
[0345] Furthermore, the content of element M in the first metal oxide is preferably lower than the content of element M in the second metal oxide. The first metal oxide may contain a trace amount of element M or may not contain element M. For example, it is preferable that the first metal oxide used in the oxide layer 230a be an In-Zn oxide and the second metal oxide used in the oxide layer 230b be an In-M-Zn oxide. Specifically, the first metal oxide can be an In-Zn oxide and the second metal oxide can be an In-Ga-Zn oxide.
[0346] For example, the oxide layer 230 a is preferably made of a metal oxide having an atomic ratio of In:Zn=1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Zn=2:1 or a composition thereof, a metal oxide having an atomic ratio of In:Sn:Zn=2:0.1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Zn=4:1 or a composition thereof, a metal oxide having an atomic ratio of In:Sn:Zn=4:0.1:1 or a composition thereof, or an indium oxide. The oxide layer 230 b is preferably made of a metal oxide having an atomic ratio of In:Ga:Zn=1:1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Ga:Zn=1:3:2 or a composition thereof, or a metal oxide having an atomic ratio of In:Ga:Zn=1:3:4 or a composition thereof. This allows the on-state current of the transistor 200 to be increased, and the transistor structure to have high reliability and little variation can be obtained.
[0347] Note that the oxide semiconductor layer 230 is not limited to the above-described structure, and the content of the element M in the first metal oxide may be higher than the content of the element M in the second metal oxide.
[0348] The oxide semiconductor layer 230 preferably includes a crystalline metal oxide layer. Examples of the structure of a crystalline metal oxide include a c-axis aligned crystal (CAAC) structure, a polycrystalline structure, and a nanocrystalline (nc) structure. By using a crystalline metal oxide layer for the oxide semiconductor layer 230, the density of defect states in the oxide semiconductor layer 230 can be reduced, and a highly reliable semiconductor device can be realized.
[0349] The higher the crystallinity of the metal oxide layer used for the oxide semiconductor layer 230, the more the density of defect states in the oxide semiconductor layer 230 can be reduced. On the other hand, by using a metal oxide layer with low crystallinity, a transistor capable of passing a large current can be realized.
[0350] When a metal oxide layer is formed by a sputtering method, the higher the substrate temperature (stage temperature) during formation, the higher the crystallinity of the formed metal oxide layer.Furthermore, the higher the ratio of the flow rate of oxygen gas to the total film formation gas used during formation (hereinafter also referred to as the oxygen flow rate ratio), the higher the crystallinity of the formed metal oxide layer.
[0351] The crystallinity of the oxide semiconductor layer 230 can be analyzed by, for example, X-ray diffraction (XRD), a transmission electron microscope (TEM), or electron diffraction (ED). Alternatively, the analysis may be performed by combining a plurality of these techniques.
[0352] The oxide semiconductor layer 230 may have a stacked structure of two or more metal oxide layers with different crystallinity. For example, the oxide semiconductor layer 230 may have a stacked structure of a first metal oxide layer and a second metal oxide layer provided on the first metal oxide layer, and the second metal oxide layer may have a region with higher crystallinity than the first metal oxide layer. Alternatively, the second metal oxide layer may have a region with lower crystallinity than the first metal oxide layer. In this case, the first metal oxide layer and the second metal oxide layer may have different compositions or may have the same or approximately the same composition.
[0353] For example, it is preferable to use a metal oxide having an In:M:Zn=1:3:2 (atomic ratio) or a metal oxide having an In:M:Zn=1:3:4 ... Alternatively, for example, a stacked structure of any one selected from indium oxide, indium gallium oxide, and IGZO and any one selected from IAZO, IAGZO, and ITZO (registered trademark) may be used.
[0354] As shown in FIG. 5B, the oxide semiconductor layer 230 may also have a three-layer structure including an oxide layer 230c, an oxide layer 230a on the oxide layer 230c, and an oxide layer 230b on the oxide layer 230a.
[0355] The oxide layer 230a and the oxide layer 230b can have the same structure as that of the oxide layer 230b.
[0356] For example, the oxide layer 230 a is preferably made of a metal oxide having an atomic ratio of In:Zn=1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Zn=2:1 or a composition thereof, a metal oxide having an atomic ratio of In:Sn:Zn=2:0.1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Zn=4:1 or a composition thereof, a metal oxide having an atomic ratio of In:Sn:Zn=4:0.1:1 or a composition thereof, or an indium oxide. Furthermore, the oxide layers 230 b and 230 c are preferably made of a metal oxide having an atomic ratio of In:Ga:Zn=1:1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Ga:Zn=1:3:2 or a composition thereof, or a metal oxide having an atomic ratio of In:Ga:Zn=1:3:4 or a composition thereof, respectively.
[0357] The oxide layers 230b and 230c preferably have a band gap larger than that of the oxide layer 230a. As a result, the oxide layer 230a is sandwiched between the oxide layers 230b and 230c, which have larger band gaps, and the oxide layer 230a functions primarily as a current path (channel). By sandwiching the oxide layer 230a between the oxide layers 230b and 230c, trap levels at and near the interface of the oxide layer 230a can be reduced. This allows for a buried channel transistor in which the channel is spaced away from the insulating layer interface, thereby increasing field-effect mobility. Furthermore, the influence of interface states that may form on the back channel side can be reduced, suppressing photodegradation (e.g., photodegradation due to negative bias current) of the transistor and improving transistor reliability.
[0358] The thickness of the oxide semiconductor layer 230 is preferably 3 nm to 200 nm, more preferably 3 nm to 100 nm, further preferably 5 nm to 100 nm, further preferably 10 nm to 100 nm, further preferably 10 nm to 70 nm, further preferably 15 nm to 70 nm, further preferably 15 nm to 50 nm, and further preferably 20 nm to 50 nm. In a transistor used in a smaller semiconductor device, the thickness of the oxide semiconductor layer 230 is preferably 1 nm to 3 nm, or 5 nm, and is preferably 20 nm to 15 nm, 12 nm to 10 nm.
[0359] Hydrogen contained in the oxide semiconductor reacts with oxygen that bonds to metal atoms to form water, and oxygen vacancies (V O In addition, defects in which hydrogen enters oxygen vacancies (hereinafter referred to as V O Hydrogen atoms (H) may function as donors and generate electrons as carriers. Furthermore, some of the hydrogen atoms may bond with oxygen atoms that are bonded to metal atoms to generate electrons as carriers. Therefore, a transistor using an oxide semiconductor containing a large amount of hydrogen is likely to have normally-on characteristics (i.e., a negative threshold voltage). Furthermore, hydrogen atoms in an oxide semiconductor are easily mobile due to stresses such as heat and an electric field. Therefore, if an oxide semiconductor contains a large amount of hydrogen, the reliability of the transistor may be reduced.
[0360] V in the oxide semiconductor layer 230 O It is preferable to reduce H as much as possible to make the oxide semiconductor layer 230 highly intrinsic or substantially highly intrinsic. O To obtain an oxide semiconductor in which H is sufficiently reduced, it is important to remove impurities such as water and hydrogen from the oxide semiconductor (sometimes referred to as dehydration or dehydrogenation treatment) and to supply oxygen to the oxide semiconductor to repair oxygen vacancies. OStable electrical characteristics can be obtained by using an oxide semiconductor in which impurities such as H are sufficiently reduced for a channel formation region of a transistor. Note that supplying oxygen to an oxide semiconductor to repair oxygen vacancies is sometimes referred to as oxygen-adding treatment.
[0361] The carrier concentration of the oxide semiconductor in the region functioning as a channel formation region is 1×10 18 cm −3 Preferably, it is 1×10 or less. 17 cm −3 More preferably, it is less than 1×10 16 cm −3 More preferably, it is less than 1×10 13 cm −3 More preferably, it is less than 1×10 12 cm −3 The lower limit of the carrier concentration of the oxide semiconductor in the region functioning as a channel formation region is not particularly limited, but is preferably, for example, 1×10 −9 cm −3 It can be said that:
[0362] Here, the influence of each impurity in a metal oxide (oxide semiconductor) will be described.
[0363] When an oxide semiconductor contains silicon or carbon, which is one of the Group 14 elements, defect levels are formed in the oxide semiconductor. Therefore, the carbon concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than or equal to 3×10, more preferably 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3 Less than or equal to 3×10, more preferably 18 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3The silicon concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than or equal to 3×10, more preferably 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3 Less than or equal to 3×10, more preferably 18 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 The following applies.
[0364] Furthermore, when nitrogen is contained in an oxide semiconductor, electrons serving as carriers are generated, the carrier concentration increases, and the semiconductor is likely to become n-type. As a result, a transistor using an oxide semiconductor containing nitrogen as a semiconductor tends to have normally-on characteristics. Alternatively, when nitrogen is contained in an oxide semiconductor, trap states may be formed. As a result, the electrical characteristics of the transistor may become unstable. Therefore, the nitrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3 Less than or equal to 5 × 10, more preferably 18 atoms / cm 3 Less than 1×10, more preferably 1×10 18 atoms / cm 3 or less, more preferably 5 × 10 17 atoms / cm 3 The following applies.
[0365] Furthermore, hydrogen contained in an oxide semiconductor reacts with oxygen bonded to a metal atom to form water, which may form an oxygen vacancy. Hydrogen entering the oxygen vacancy may generate electrons as carriers. Furthermore, some of the hydrogen may bond with oxygen bonded to a metal atom to generate electrons as carriers. Therefore, a transistor using an oxide semiconductor containing hydrogen is likely to have normally-on characteristics. Therefore, it is preferable to reduce hydrogen as much as possible in the channel formation region of the oxide semiconductor. Specifically, the hydrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Less than 5×10 19 atoms / cm 3 less than 1×10 19 atoms / cm 3 less than 5×10 18 atoms / cm 3 less than 1×10 18 atoms / cm 3 Less than.
[0366] Furthermore, when an oxide semiconductor contains an alkali metal or an alkaline earth metal, defect levels may be formed and carriers may be generated. Therefore, a transistor using an oxide semiconductor containing an alkali metal or an alkaline earth metal is likely to have normally-on characteristics. Therefore, when the concentration of the alkali metal or the alkaline earth metal in the channel formation region of the oxide semiconductor obtained by SIMS is set to 1×10 18 atoms / cm 3 Below 2 × 10, preferably 16 atoms / cm 3 Do the following:
[0367] When an oxide semiconductor with sufficiently reduced impurities is used for a channel formation region of a transistor, stable electrical characteristics can be obtained.
[0368] Note that the semiconductor device of this embodiment may also be applied to a transistor using another semiconductor material in the channel formation region. Examples of such another semiconductor material include semiconductors made of simple elements or compound semiconductors. Examples of semiconductors made of simple elements include silicon and germanium. Examples of compound semiconductors include gallium arsenide and silicon germanium. Other examples of compound semiconductors include organic semiconductors and nitride semiconductors. Note that the aforementioned oxide semiconductor is also a type of compound semiconductor. Note that these semiconductor materials may contain impurities as dopants.
[0369] Silicon that can be used as a semiconductor material for a transistor includes single crystal silicon, polycrystalline silicon, microcrystalline silicon, and amorphous silicon. An example of polycrystalline silicon is low temperature polysilicon (LTPS).
[0370] The semiconductor layer of a transistor may include a layered material that functions as a semiconductor. A layered material is a general term for a group of materials that have a layered crystal structure. A layered crystal structure is a structure in which layers formed by covalent or ionic bonds are stacked via bonds weaker than covalent or ionic bonds, such as van der Waals forces. A layered material has high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, a transistor with a large on-state current can be provided.
[0371] Examples of the layered material include graphene, silicene, and chalcogenides. Chalcogenides are compounds containing chalcogen (an element belonging to Group 16). Examples of chalcogenides include transition metal chalcogenides and Group 13 chalcogenides. Specific examples of transition metal chalcogenides that can be used as semiconductor layers of transistors include molybdenum sulfide (typically MoS 2 ), molybdenum selenide (typically MoSe 2 ), molybdenum telluride (typically MoTe2 ), tungsten sulfide (typically WS 2 ), tungsten selenide (typically WSe 2 ), tungsten tellurium (typically WTe 2 ), hafnium sulfide (typically HfS 2 ), hafnium selenide (typically HfSe 2 ), zirconium sulfide (typically ZrS 2 ), zirconium selenide (typically ZrSe 2 ) etc.
[0372] [Substrate] Substrates on which transistors are formed can be, for example, insulating substrates, semiconductor substrates, or conductive substrates. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconia substrates (e.g., yttria-stabilized zirconia substrates), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon or germanium, or compound semiconductor substrates made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, and gallium oxide. Examples of semiconductor substrates include those having an insulating region within the semiconductor substrate, such as an SOI (Silicon-On-Insulator) substrate. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Other examples include substrates having a metal nitride or a metal oxide. Examples of other substrates include a substrate having a conductor or semiconductor provided on an insulating substrate, a substrate having a conductor or insulator provided on a semiconductor substrate, and a substrate having a semiconductor or insulator provided on a conductive substrate. Alternatively, a substrate provided with elements may be used, such as a capacitor element, a resistor element, a switch element, a light-emitting element, a memory element, and the like.
[0373] 1A to 1C and the like will be described with reference to Fig. 10A to Fig. 11B. Note that the description of the materials and forming methods of each element that are the same as those described above may be omitted.
[0374] Thin films (insulating films, semiconductor films, conductive films, etc.) constituting a semiconductor device can be formed by a sputtering method, a CVD method, a vacuum evaporation method, a PLD method, an ALD method, or the like.
[0375] Sputtering methods include RF sputtering, which uses a high-frequency power source as the sputtering power source; DC sputtering, which uses a direct current power source; and pulsed DC sputtering, which changes the voltage applied to the electrode in a pulsed manner. RF-superimposed DC sputtering, which superimposes RF and DC, is also available. RF sputtering is preferred for film formation using insulating targets. DC sputtering is primarily used when forming films using conductive targets. DC sputtering can also form insulating films by reactive sputtering, in addition to forming conductive films. Pulsed DC sputtering is primarily used when depositing films of compounds such as oxides, nitrides, and carbides using reactive sputtering. RF-superimposed DC sputtering allows for control of ion energy and target potential during film formation. Therefore, compared to RF sputtering, damage caused by film formation is reduced. Furthermore, high-quality films can be obtained.
[0376] Examples of sputtering methods that can be used include ionization sputtering and long-throw sputtering. Ionization sputtering is a method in which sputtering particles generated from a target are ionized by RF or the like, and anisotropic film formation is achieved by self-bias or the like. In addition, long-throw sputtering can form anisotropic films by increasing the distance between the sputtering target and the substrate.
[0377] CVD methods can be classified into PECVD, thermal CVD (TCVD) using heat, photo CVD (Photo CVD) using light, etc. They can also be further classified into metal CVD (MCVD) and metal organic CVD (MOCVD) depending on the source gas used.
[0378] The plasma CVD method can produce high-quality films at relatively low temperatures. Furthermore, the thermal CVD method is a film formation method that can minimize plasma damage to the workpiece because it does not use plasma. For example, wiring, electrodes, elements (transistors, capacitors, etc.) included in a semiconductor device may become charged up by receiving electric charge from the plasma. In this case, the accumulated electric charge may destroy the wiring, electrodes, elements, etc. included in the semiconductor device. On the other hand, the thermal CVD method, which does not use plasma, does not cause such plasma damage, and therefore can increase the yield of semiconductor devices. Furthermore, the thermal CVD method does not cause plasma damage during film formation, so films with fewer defects can be obtained.
[0379] As the ALD method, a thermal ALD method in which a precursor and a reactant are reacted using only thermal energy, a PEALD (Plasma Enhanced ALD) method in which a plasma-excited reactant is used, or the like can be used.
[0380] Furthermore, the ALD method can deposit atoms layer by layer, which has the advantages of enabling ultrathin film formation, film formation on structures with high aspect ratios, film formation with fewer defects such as pinholes, film formation with excellent coverage, and film formation at low temperatures. The PEALD (Plasma Enhanced ALD) method may be preferable because it utilizes plasma, allowing film formation at lower temperatures. Note that some precursors used in the ALD method contain impurities such as carbon. Therefore, films formed by the ALD method may contain more impurities such as carbon than films formed by other film formation methods. The amount of impurities can be quantified using X-ray photoelectron spectroscopy (XPS).
[0381] Unlike film formation methods in which particles emitted from a target or the like are deposited, CVD and ALD are film formation methods in which a film is formed by a reaction on the surface of a workpiece. Therefore, they are film formation methods that are less affected by the shape of the workpiece and have good step coverage. In particular, ALD has excellent step coverage and excellent thickness uniformity, making it suitable for coating the surface of an opening with a high aspect ratio. However, because ALD has a relatively slow film formation rate, it may be preferable to use it in combination with other film formation methods, such as CVD, which have a faster film formation rate.
[0382] The CVD method and the ALD method can control the composition of the resulting film by adjusting the flow rate ratio of the source gases. For example, the CVD method and the ALD method can form a film of any composition by adjusting the flow rate ratio of the source gases. Furthermore, for example, the CVD method and the ALD method can form a film whose composition changes continuously by changing the flow rate ratio of the source gases while forming the film. When forming a film while changing the flow rate ratio of the source gases, the time required for film formation can be shortened compared to when forming a film using multiple film formation chambers because no time is required for transportation and pressure adjustment. Therefore, the productivity of semiconductor devices can be improved in some cases.
[0383] Furthermore, the CVD method allows deposition of a film with any composition by adjusting the flow rate ratio of the source gases. For example, the CVD method allows deposition of a film with a continuously changing composition by changing the flow rate ratio of the source gases during deposition. When deposition is performed while changing the flow rate ratio of the source gases, the time required for deposition can be shortened compared to deposition using multiple deposition chambers because no time is required for transport or pressure adjustment. Therefore, the productivity of semiconductor devices can be improved in some cases.
[0384] Furthermore, in the ALD method, a film of any composition can be formed by simultaneously introducing multiple different precursors, or by controlling the number of cycles of each precursor when multiple different precursors are introduced.
[0385] Furthermore, thin films (insulating films, semiconductor films, conductive films, etc.) constituting the semiconductor device can be formed by a wet film formation method such as spin coating, dip coating, spray coating, inkjet printing, dispensing, screen printing, offset printing, doctor knife method, slit coating, roll coating, curtain coating, or knife coating.
[0386] Furthermore, when processing a thin film that constitutes a semiconductor device, a photolithography method or the like can be used. Alternatively, the thin film may be processed by a nanoimprint method, a sandblasting method, a lift-off method, or the like. Furthermore, an island-shaped thin film may be directly formed by a film formation method using a shielding mask such as a metal mask.
[0387] There are two typical photolithography methods: one is to form a resist mask on the thin film to be processed, process the thin film by etching or the like, and then remove the resist mask; the other is to form a photosensitive thin film, and then process the thin film into the desired shape by exposure and development.
[0388] In photolithography, the light used for exposure may be, for example, i-line (wavelength 365 nm), g-line (wavelength 436 nm), h-line (wavelength 405 nm), or a mixture of these. Other light sources that can be used include ultraviolet light, KrF laser light, ArF laser light, etc. Exposure may also be performed by immersion exposure technology. Extreme ultraviolet (EUV) light or X-rays may also be used as the light used for exposure. An electron beam may also be used instead of the light used for exposure. Extreme ultraviolet light, X-rays, or an electron beam are preferred because they enable extremely fine processing. When exposure is performed by scanning a beam such as an electron beam, a photomask is not required.
[0389] For etching the thin film, dry etching, wet etching, sandblasting, or the like can be used.
[0390] First, the conductive layer 220 is formed on the insulating layer 210 , the insulating layer 280 is formed on the conductive layer 220 , and the conductive layer 240 is formed on the insulating layer 280 .
[0391] Note that after the insulating layer 280 is formed, it is preferable to perform planarization treatment (also referred to as CMP treatment) using a chemical mechanical polishing (CMP) method to planarize the top surface of the insulating layer 280. By performing the planarization treatment on the insulating layer 280, the surface on which the conductive layer 240, which functions as a wiring, is formed can be flattened, and discontinuity of the conductive layer 240 can be suppressed. Note that the planarization treatment is not necessarily performed, and in that case, manufacturing costs can be reduced.
[0392] Subsequently, openings 290 are formed in the conductive layer 240 and the insulating layer 280 at positions where they overlap the conductive layer 220 .
[0393] Because the opening 290 has a large aspect ratio, it is preferable to process a portion of the conductive layer 240 and a portion of the insulating layer 280 using anisotropic etching. In particular, processing by dry etching is preferable because it is suitable for fine processing. Different conditions may be used for each layer. Note that, depending on the processing conditions for the conductive layer 240 and the insulating layer 280, the slope of the side surface of the conductive layer 240 and the slope of the side surface of the insulating layer 280 at the opening 290 may differ from each other.
[0394] Subsequently, heat treatment may be performed at a temperature of, for example, 250° C. to 650° C., preferably 300° C. to 500° C., and more preferably 320° C. to 450° C.
[0395] The heat treatment is performed in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more. For example, when the heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas concentration is preferably about 20%. The heat treatment may be performed under reduced pressure. Alternatively, after the heat treatment in the nitrogen gas or inert gas atmosphere, the heat treatment may be performed in an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more to compensate for the desorbed oxygen. By performing the above heat treatment, impurities such as water contained in the insulating layer 280 and the like can be reduced before the formation of the oxide semiconductor layer 230.
[0396] Furthermore, the gas used in the heat treatment is preferably highly purified. For example, the amount of moisture contained in the gas used in the heat treatment is preferably 1 ppb or less, more preferably 0.1 ppb or less, and even more preferably 0.05 ppb or less. By performing the heat treatment using a highly purified gas, it is possible to prevent moisture and the like from being taken into the insulating layer 280 and the like as much as possible.
[0397] Next, the conductive layer 240 is processed into an island shape ( FIG. 10A ). The process of processing the conductive layer 240 into an island shape and the process of forming an opening 290 in the conductive layer 240 can be performed independently, and the order of these processes does not matter. Alternatively, the island shape and the formation of the opening may be performed simultaneously by performing exposure using a mask for processing the conductive layer 240 into a square island shape and exposure using a mask for forming a circular opening, followed by etching. Exposure using a multi-tone mask (typically a half-tone mask or gray-tone mask) may also be used. The conductive layer 240 and the insulating layer 280 may be opened using the same mask or different masks.
[0398] Next, an oxide semiconductor layer 230 is formed so as to cover the opening 290. Next, an insulating layer 250 is formed on the oxide semiconductor layer 230 ( FIG. 10B ). The oxide semiconductor layer 230 is formed in contact with the upper surface of the conductive layer 220, the side surface of the insulating layer 280, and the upper surface and side surface of the conductive layer 240. The insulating layer 250 is formed in contact with the oxide semiconductor layer 230.
[0399] The oxide semiconductor layer 230 can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, or an ALD method.
[0400] The oxide semiconductor layer 230 is preferably formed as a film with as uniform a thickness as possible in the opening 290 along the top surface of the conductive layer 220, the side surface of the insulating layer 280, and the side surface of the conductive layer 240. By forming the oxide semiconductor layer 230 using the ALD method, a thin film can be formed with good controllability. Therefore, the oxide semiconductor layer 230 is preferably formed using the ALD method.
[0401] Furthermore, when the oxide semiconductor layer 230 has high crystallinity, diffusion of impurities in the oxide semiconductor layer 230 is suppressed, which makes it difficult for the electrical characteristics of the transistor to fluctuate and improves reliability. Forming the oxide semiconductor layer 230 by a sputtering method is preferable because it makes it easier to form a layer with high crystallinity than forming the oxide semiconductor layer 230 by an ALD method.
[0402] When the oxide semiconductor layer 230 is formed by a sputtering method, oxygen or a mixed gas of oxygen and a noble gas is used as a sputtering gas. By increasing the proportion of oxygen contained in the sputtering gas, the amount of excess oxygen in the oxide film to be formed can be increased. When the oxide film is formed by a sputtering method, an In-M-Zn oxide target or the like can be used.
[0403] When the oxide semiconductor layer 230 is formed by a sputtering method, an oxygen-excess oxide semiconductor is formed when the percentage of oxygen contained in the sputtering gas is set to more than 30% and less than or equal to 100%, preferably 70% to 100%. A transistor using an oxygen-excess oxide semiconductor for a channel formation region can have relatively high reliability. However, one embodiment of the present invention is not limited thereto. An oxygen-deficient oxide semiconductor is formed when the percentage of oxygen contained in the sputtering gas is set to 1% to 30%, preferably 5% to 20%. A transistor using an oxygen-deficient oxide semiconductor for a channel formation region can have relatively high field-effect mobility. Furthermore, the crystallinity of the oxide semiconductor layer can be improved by performing film formation while heating the substrate.
[0404] Next, heat treatment is preferably performed. The heat treatment is preferably performed within a temperature range in which the oxide semiconductor layer 230 does not become polycrystallized. The temperature of the heat treatment is preferably from 100° C. to 650° C., more preferably from 250° C. to 600° C., and further preferably from 350° C. to 550° C. For details of the heat treatment, refer to the above description.
[0405] The gas used in the heat treatment is preferably highly purified. When the heat treatment is performed using a highly purified gas, moisture and the like can be prevented from being introduced into the oxide semiconductor layer 230 as much as possible.
[0406] In this embodiment, the heat treatment is performed at 450° C. for 1 hour with a flow rate ratio of nitrogen gas to oxygen gas of 4:1. By such heat treatment using oxygen gas, impurities such as carbon, water, and hydrogen in the oxide semiconductor layer 230 can be reduced. Reducing the impurities in the film in this manner improves the crystallinity of the oxide semiconductor layer 230, resulting in a denser and more compact structure. This increases the crystalline regions in the oxide semiconductor layer 230, reducing in-plane variations in the crystalline regions in the oxide semiconductor layer 230. Therefore, in-plane variations in the electrical characteristics of the transistor can be reduced.
[0407] In the case where the insulating layer 280 contains oxygen, oxygen is preferably supplied from the insulating layer 280 to a channel formation region of the oxide semiconductor layer 230 by heat treatment. This can reduce oxygen vacancies and VoH.
[0408] The insulating layer 250 is preferably formed using a method that has anisotropy in the deposition rate, such as sputtering or CVD.
[0409] As the sputtering method, for example, an ionization sputtering method, a long throw sputtering method, or the like can be used.
[0410] As the CVD method, for example, a PECVD method can be used, and in this case, a PECVD method using RF is preferably used.
[0411] 6A to 7B , when the insulating layer 250 is composed of an insulating layer 250 a and an insulating layer 250 b on the insulating layer 250 a, it is preferable to use a method with a high anisotropy of the deposition rate for one of the insulating layers 250 a and 250 b. On the other hand, it is preferable to use a method with a relatively low anisotropy of the deposition rate for the other insulating layer. For example, it is preferable to use an ALD method as a method with a relatively low anisotropy of the deposition rate.
[0412] Subsequently, a conductive layer 260af is formed on the insulating layer 250, and a conductive layer 260bf is formed by stacking on the conductive layer 260af.
[0413] The conductive layer 260af is formed in contact with the insulating layer 250 provided in the opening 290 with a large aspect ratio. Therefore, the conductive layer 260af is preferably formed by a film formation method with good coverage, and more preferably by a CVD method, an ALD method, or the like.
[0414] Furthermore, by using, for example, a sputtering method or a CVD method to form the conductive layer 260bf, a thick film can be suitably formed at a high film formation rate, and the efficiency of the manufacturing process can be improved.
[0415] Subsequently, a mask 278 is formed over the conductive layer 260bf (FIG. 10C). A resist mask can be used as the mask 278. Alternatively, the mask 278 may have a structure in which a spin-on-carbon (SOC) film, a spin-on-glass (SOG) film, and a resist mask are stacked in this order over the conductive layer 260bf.
[0416] Subsequently, a mask 278 is used to remove a portion of the conductive layer 260bf to form the conductive layer 260b.
[0417] Next, a portion of the conductive layer 260af is removed to form a conductive layer 260a (FIG. 11A). Here, the conductive layer 260af is partially removed using the conductive layer 260b as a mask. Here, the mask 278 may remain when the conductive layer 260a is formed. If the mask 278 remains, the conductive layer 260af is partially removed using the mask 278 and the conductive layer 260b as masks. If the mask 278 remains, for example, the mask 278 is removed after the conductive layer 260a is formed.
[0418] For example, dry etching is used to process the conductive layer 260b and the conductive layer 260a. In the dry etching process, after removing a portion of the conductive layer 260af to process the conductive layer 260a, the surface of the insulating layer 250 is exposed in the region not covered by the conductive layer 260a. At this time, over-etching reduces the film thickness of the region of the insulating layer 250 where the surface is exposed. By using a film with an anisotropic deposition rate as the insulating layer 250, the film thickness in the region where over-etching occurs can be increased. Therefore, even if the film thickness of the insulating layer 250 is reduced by over-etching, it is possible to ensure a thickness sufficient to suppress gate leakage current and short circuits.
[0419] Subsequently, an insulating layer 283 is formed on the insulating layer 250 and the conductive layer 260 (FIG. 11B).
[0420] Through the above steps, a semiconductor device of one embodiment of the present invention can be manufactured.
[0421] <Second Example of Manufacturing Method of Semiconductor Device> A modified example of the method for manufacturing the insulating layer 250 will be described with reference to FIGS.
[0422] 10A, a conductive layer 220, an insulating layer 280, and a conductive layer 240 are formed on an insulating layer 210. Then, an oxide semiconductor layer 230 is formed to cover the opening 290.
[0423] Subsequently, an insulating layer 250a is formed on the oxide semiconductor layer 230, the conductive layer 240, and the insulating layer 280 (FIG. 12A). The insulating layer 250a is formed using a method in which the deposition rate is anisotropic.
[0424] Next, the insulating layer 250a is removed by a desired thickness from the surface, thereby removing the region of the insulating layer 250a that covers the sidewall of the insulating layer 280 at the opening 290a. This exposes the surface of the oxide semiconductor layer 230 in the region that covers the sidewall of the insulating layer 280 at the opening 290a ( FIG. 12B ). Wet etching is preferably used as the etching method for the insulating layer 250a. Compared to dry etching, wet etching can significantly reduce damage to the exposed oxide semiconductor layer 230 caused by etching. Examples of chemicals that can be used for wet etching include hydrofluoric acid, a mixed solution containing hydrofluoric acid, and a solution containing phosphoric acid.
[0425] Next, an insulating layer 250b is formed over the insulating layer 250a and over the exposed region of the oxide semiconductor layer 230 (FIG. 12C). By using an ALD method to form the insulating layer 250b, a dense gate insulating layer with a uniform thickness can be formed so as to overlap with the channel formation region of the oxide semiconductor layer 230.
[0426] The insulating layer 250a is formed by an etching technique that utilizes anisotropic deposition rates. Such an anisotropic technique can make it difficult to control the thickness of the sidewalls, for example. By using the structure shown in FIG. 12C, the thickness of the gate insulating layer in the region overlapping the channel formation region is determined solely by the thickness of the insulating layer 250b, further enhancing the controllability of the thickness.
[0427] Subsequently, a conductive layer 260 and an insulating layer 283 are formed, and the semiconductor device shown in FIG. 13 can be manufactured.
[0428] <Example 3 of Manufacturing Method of Semiconductor Device> Next, a method for manufacturing the semiconductor shown in FIGS. 8A to 8C will be described with reference to FIGS. 14A to 15C.
[0429] 10A, a conductive layer 220, an insulating layer 280, and a conductive layer 240 are formed on an insulating layer 210. Then, an oxide semiconductor layer 230 is formed to cover the opening 290 (FIG. 14A).
[0430] The conductive layer 240 preferably includes a metal layer. When the conductive layer 240 has a stacked structure, the top layer is preferably a metal layer. Here, for example, ITO or ITSO is used as the lower layer, and ruthenium or tungsten is used as the upper layer. The upper surface of the upper layer of the conductive layer 240 is in contact with the oxide semiconductor layer 230. If a metal that is easily oxidized, such as aluminum, is used as the upper layer of the conductive layer 240, an insulating oxide (e.g., aluminum oxide) may be formed between the conductive layer 240 and the oxide semiconductor layer 230, preventing electrical conduction therebetween. Therefore, the upper layer of the conductive layer 240 is preferably made of a conductive material that is resistant to oxidation, a conductive material that maintains low electrical resistance even when oxidized, or a conductive oxide material. When a metal is used as the upper layer of the conductive layer 240, titanium, ruthenium, tungsten, or the like can be used. These materials are preferred because they are conductive materials that are resistant to oxidation or that maintain electrical conductivity even when oxidized.
[0431] Next, an insulating layer 250d is selectively formed on the exposed surface region of the conductive layer 240 ( FIG. 14B ). When vapor deposition is used to form the insulating layer 250d, for example, by using a material that grows selectively on metal during the growth process, for example, at the beginning of the growth process, the insulating layer 250d can be selectively formed on the metal layer that is the uppermost layer of the conductive layer 240. Here, the insulating layer 250d is preferably formed on the upper surface of the conductive layer 240. Alternatively, the insulating layer 250d may be formed on the side surface of the conductive layer 240. Note that the insulating layer 250d may not be formed on the side surface of the conductive layer 240, or may be thinner than the thickness of the film formed on the upper surface.
[0432] Next, the insulating layer 250c is formed on the oxide semiconductor layer 230, the insulating layer 250d, and the insulating layer 280 (FIG. 14C).
[0433] The insulating layer 250c can be formed by appropriately using an ALD method, a CVD method, an MBE method, a PLD method, a sputtering method, or the like.
[0434] Next, a conductive layer 260af and a conductive layer 260bf are formed on the insulating layer 250c (FIG. 15A).
[0435] Next, a mask is used to form conductive layers 260b and 260a (FIG. 15B). Here, after the conductive layer 260a is processed, the surface of the insulating layer 250 is exposed in areas not covered by the conductive layer 260a. At this time, over-etching reduces the film thickness of the exposed surface area of the insulating layer 250. Because the insulating layer 250d is provided on the conductive layer 240, even if the film thickness of the insulating layer 250c is reduced by over-etching, the insulating layer 250d can remain on the conductive layer 240 with a thickness sufficient to suppress gate leakage current and short circuits.
[0436] 15C , under the etching conditions for processing the conductive layer 260 a, the insulating layer 250 c may disappear in the region not covered by the conductive layer 260 a. Even in such a case, by providing the insulating layer 250 d, it is possible to leave the insulating layer 250 d on the conductive layer 240 with a thickness sufficient to suppress the gate leakage current and the short circuit.
[0437] Subsequently, an insulating layer 283 is formed over the insulating layer 250 and the conductive layer 260, whereby the semiconductor device of one embodiment of the present invention can be manufactured.
[0438] This embodiment mode can be combined with other embodiment modes as appropriate. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be combined as appropriate.
[0439] 16 to 19. The memory device of one embodiment of the present invention includes a memory cell. The memory cell includes a transistor and a capacitor.
[0440] 16A to 16C , the structure of a memory device including a transistor and a capacitor will be described. Fig. 16A is a plan view of a memory device including a transistor 200 and a capacitor 100. Fig. 16B is a cross-sectional view taken along dashed line A1-A2 in Fig. 16A . Fig. 16C is a cross-sectional view taken along dashed line A3-A4 in Fig. 16A .
[0441] 16A to 16C includes an insulating layer 140 over a substrate (not shown), a conductive layer 110 over the insulating layer 140, a memory cell 150 over the conductive layer 110, an insulating layer 180 over the conductive layer 110, an insulating layer 280, and an insulating layer 283 over the memory cell 150. The insulating layer 140, the insulating layer 180, the insulating layer 280, and the insulating layer 283 function as interlayer films. The conductive layer 110 functions as a wiring.
[0442] The memory cell 150 includes a capacitor 100 over a conductive layer 110 and a transistor 200 over the capacitor 100 .
[0443] The capacitor 100 includes a conductive layer 115 on the conductive layer 110, an insulating layer 130 on the conductive layer 115, and a conductive layer 120 on the insulating layer 130. The conductive layer 120 functions as one of a pair of electrodes (sometimes referred to as an upper electrode), the conductive layer 115 functions as the other of the pair of electrodes (sometimes referred to as a lower electrode), and the insulating layer 130 functions as a dielectric. In other words, the capacitor 100 constitutes a metal-insulator-metal (MIM) capacitor.
[0444] As shown in FIGS. 16B and 16C , an opening 190 is provided in the insulating layer 180, reaching the conductive layer 110. At least a portion of the conductive layer 115 is disposed in the opening 190. The conductive layer 115 has a region in contact with the upper surface of the conductive layer 110 in the opening 190, a region in contact with the side surface of the insulating layer 180 in the opening 190, and a region in contact with at least a portion of the upper surface of the insulating layer 180. The insulating layer 130 is disposed so that at least a portion of it is located in the opening 190. The conductive layer 120 is disposed so that at least a portion of it is located in the opening 190. As shown in FIGS. 16B and 16C , the conductive layer 120 is preferably disposed so as to fill the opening 190. The films disposed inside the openings 190 are preferably formed using an ALD method. This improves the coverage of the films. For example, the conductive layer 115, the insulating layer 130, and the conductive layer 120 are preferably formed by an ALD method.
[0445] The capacitor 100 has a configuration in which the upper electrode and the lower electrode face each other across a dielectric not only on the bottom surface but also on the side surfaces of the opening 190, allowing for a larger capacitance per unit area. Therefore, the deeper the opening 190, the larger the capacitance of the capacitor 100 can be. Increasing the capacitance per unit area of the capacitor 100 in this way can stabilize the read operation of the memory device. Furthermore, this can promote miniaturization or high integration of memory devices.
[0446] 16B and 16C show an example in which the sidewall of the opening 190 is perpendicular to the top surface of the conductive layer 110. In this case, the opening 190 has a cylindrical shape. With such a configuration, miniaturization or high integration of the memory device can be achieved.
[0447] A conductive layer 115 and an insulating layer 130 are stacked along the sidewall of the opening 190 and the upper surface of the conductive layer 110. A conductive layer 120 is provided on the insulating layer 130 so as to fill the opening 190. The capacitor element 100 having such a configuration may be called a trench capacitor or a trench capacitor.
[0448] An insulating layer 280 is disposed on the capacitor element 100. That is, the insulating layer 280 is disposed on the conductive layer 115, the insulating layer 130, and the conductive layer 120. In other words, the conductive layer 120 is disposed below the insulating layer 280.
[0449] The transistor 200 includes a conductive layer 120 (corresponding to the conductive layer 220 in FIG. 1B , etc.), a conductive layer 240 over an insulating layer 280, an oxide semiconductor layer 230, an insulating layer 250 over the oxide semiconductor layer 230, and a conductive layer 260 over the insulating layer 250. The oxide semiconductor layer 230 functions as a semiconductor layer, the conductive layer 260 functions as a gate electrode, the insulating layer 250 functions as a gate insulating layer, the conductive layer 120 functions as one of a source electrode and a drain electrode, and the conductive layer 240 functions as the other of the source electrode and drain electrode.
[0450] The detailed description of the transistor 200 is omitted here because the description in Embodiment 1 (FIGS. 1 and 2, etc.) can be referred to. The transistor included in the memory cell 150 is not limited to the transistor 200 shown in FIGS. 1 and 2, etc., and any of the transistors exemplified in Embodiment 1 can be applied.
[0451] As shown in FIGS. 16A to 16C , the transistor 200 is provided so as to overlap with the capacitor 100. Furthermore, an opening 290 in which part of the structure of the transistor 200 is provided overlaps with an opening 190 in which part of the structure of the capacitor 100 is provided. In particular, the conductive layer 120 functions as one of the source electrode and drain electrode of the transistor 200 and as the upper electrode of the capacitor 100. Therefore, the transistor 200 and the capacitor 100 share part of their structures. With this structure, the transistor 200 and the capacitor 100 can be provided without significantly increasing the occupied area in a plan view. This reduces the occupied area of the memory cell 150, thereby enabling the memory cells 150 to be arranged at a high density and increasing the storage capacity of the memory device. In other words, the memory device can be highly integrated.
[0452] Furthermore, by providing the transistor 200 above the capacitor 100, the transistor 200 is not affected by heat treatment during manufacturing of the capacitor 100. Therefore, in the transistor 200, deterioration of electrical characteristics such as a change in threshold voltage and an increase in parasitic resistance, as well as an increase in variation in electrical characteristics due to the deterioration of the electrical characteristics, can be suppressed.
[0453] 21A shows a circuit diagram of the memory device described in this embodiment. As shown in FIG. 21A, the configurations shown in FIGS. 16A to 16C function as memory cells. A memory cell 951 includes a transistor M1 and a capacitor CA. Here, the transistor M1 corresponds to the transistor 200, and the capacitor CA corresponds to the capacitor 100.
[0454] One of the source and drain of the transistor M1 is connected to one of a pair of electrodes of the capacitor CA. The other of the source and drain of the transistor M1 is connected to a wiring BIL. The gate of the transistor M1 is connected to a wiring WOL. The other of the pair of electrodes of the capacitor CA is connected to a wiring CAL.
[0455] Here, the wiring BIL corresponds to the conductive layer 240, the wiring WOL corresponds to the conductive layer 260, and the wiring CAL corresponds to the conductive layer 110. As shown in FIGS. 16A to 16C , it is preferable that the conductive layer 260 is provided extending in the X direction, and the conductive layer 240 is provided extending in the Y direction. With this configuration, the wiring BIL and the wiring WOL are provided so as to intersect with each other. Also, in FIG. 16A , the wiring CAL (conductive layer 110) is provided in a planar shape, but the present invention is not limited to this. For example, the wiring CAL may be provided parallel to the wiring WOL (conductive layer 260) or parallel to the wiring BIL (conductive layer 240).
[0456] The memory cells will be described in detail in a later embodiment.
[0457] [Capacitor 100] The capacitor 100 includes a conductive layer 115, an insulating layer 130, and a conductive layer 120. The conductive layer 110 is provided below the conductive layer 115. The conductive layer 115 has a region in contact with the conductive layer 110.
[0458] The conductive layer 110 is provided over the insulating layer 140. The conductive layer 110 functions as a wiring CAL and can be provided in a planar shape, for example. The conductive layer 110 can be formed as a single layer or a stacked layer using the conductive material described in the section [Conductive Layer] of Embodiment 1. For example, a conductive material with high conductivity, such as tungsten, can be used as the conductive layer 110. By using such a conductive material with high conductivity, the conductivity of the conductive layer 110 can be improved, allowing the conductive layer 110 to function sufficiently as a wiring CAL.
[0459] The conductive layer 115 is preferably made of a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion, and is used in a single layer or a stacked layer. For example, titanium nitride or indium tin oxide with added silicon may be used. Alternatively, for example, a structure in which titanium nitride is stacked on tungsten may be used. Alternatively, for example, a structure in which tungsten is stacked on a first titanium nitride and a second titanium nitride is stacked on the tungsten may be used. With such a structure, when an oxide is used for the insulating layer 130, the insulating layer 130 can suppress oxidation of the conductive layer 110. Furthermore, when an oxide is used for the insulating layer 180, the insulating layer 180 can suppress oxidation of the conductive layer 110.
[0460] The insulating layer 130 is provided on the conductive layer 115. The insulating layer 130 is provided so as to contact the upper surface and side surfaces of the conductive layer 115. In other words, the insulating layer 130 is preferably structured to cover the side edges of the conductive layer 115. This can prevent the conductive layer 115 and the conductive layer 120 from shorting out.
[0461] Alternatively, a structure may be used in which the side edges of the insulating layer 130 coincide with the side edges of the conductive layer 115. With such a structure, the insulating layer 130 and the conductive layer 115 can be formed using the same mask, which can simplify the manufacturing process of the memory device.
[0462] It is preferable to use a material with a high relative dielectric constant (high-k) for the insulating layer 130. By using a high-k material for the insulating layer 130, the insulating layer 130 can be made thick enough to suppress leakage current, and the capacitance of the capacitive element 100 can be sufficiently ensured.
[0463] Furthermore, the insulating layer 130 is preferably formed by stacking insulating layers made of a high-k material, and preferably by using a stack structure of a high-dielectric-constant (high-k) material and a material with a higher dielectric strength than the high-k material. For example, the insulating layer 130 can be formed by stacking zirconium oxide, aluminum oxide, and zirconium oxide in this order. Alternatively, the insulating layer 130 can be formed by stacking zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide in this order. Alternatively, the insulating layer 130 can be formed by stacking hafnium zirconium oxide, aluminum oxide, hafnium zirconium oxide, and aluminum oxide in this order. By stacking insulating layers with a relatively high dielectric strength, such as aluminum oxide, the dielectric strength is improved, and electrostatic breakdown of the capacitor element 100 can be suppressed.
[0464] Furthermore, a material that can have ferroelectricity may be used as the insulating layer 130. For details of the material that can have ferroelectricity, the description in the first embodiment can also be referred to.
[0465] Metal oxides containing one or both of hafnium and zirconium can have ferroelectricity even when the thickness is as thin as a few nanometers, and are therefore preferable as the insulating layer 130. The film thickness of the insulating layer 130 is preferably 100 nm or less, more preferably 50 nm or less, even more preferably 20 nm or less, and even more preferably 10 nm or less (typically, 2 nm to 9 nm). Furthermore, for example, the film thickness is preferably 8 nm to 12 nm. By using a ferroelectric layer that can be thinned, the capacitor element 100 can be combined with a semiconductor element such as a miniaturized transistor to form a semiconductor device.
[0466] Furthermore, a metal oxide containing one or both of hafnium and zirconium can have ferroelectricity even in a small area, and is therefore preferable as the insulating layer 130. For example, when the area (occupied area) of the ferroelectric layer in a plan view is 100 μm 2 Below, 10μm 2 Below, 1μm 2 or less than 0.1 μm 2 Even if the thickness is less than 10,000 nm, the film can still have ferroelectricity. 2 or less than 1000 nm 2 Even if the thickness is less than 100 Å, the ferroelectric layer may have ferroelectricity. By using a ferroelectric layer with a small area, the area occupied by the capacitor element 100 can be reduced.
[0467] A ferroelectric material is an insulator that generates polarization internally when an external electric field is applied, and the polarization remains even when the electric field is removed. Therefore, a nonvolatile memory element can be formed using a capacitor element (hereinafter sometimes referred to as a ferroelectric capacitor) that uses this material as a dielectric. A nonvolatile memory element using a ferroelectric capacitor is sometimes called a Ferroelectric Random Access Memory (FeRAM), a ferroelectric memory, or the like. For example, a ferroelectric memory includes a transistor and a ferroelectric capacitor, and one of the source and drain of the transistor is electrically connected to one terminal of the ferroelectric capacitor. Therefore, when a ferroelectric capacitor is used as the capacitor element 100, the memory device described in this embodiment functions as a ferroelectric memory.
[0468] The conductive layer 120 is provided in contact with a portion of the upper surface of the insulating layer 130. The side edges of the conductive layer 120 are preferably located more inward than the side edges of the conductive layer 115 in both the X and Y directions. Note that in a structure in which the insulating layer 130 covers the side edges of the conductive layer 115, the side edges of the conductive layer 120 may be located more outward than the side edges of the conductive layer 115.
[0469] The conductive layer 120 can be formed as a single layer or a stacked layer using the conductive material described in the section [Conductive Layer] of Embodiment 1. It is preferable to use a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion for the conductive layer 120. For example, titanium nitride or tantalum nitride can be used. Alternatively, for example, a structure in which tantalum nitride is stacked on titanium nitride may be used. In this case, titanium nitride is in contact with the insulating layer 130, and tantalum nitride is in contact with the oxide semiconductor layer 230. With such a structure, excessive oxidation of the conductive layer 120 by the oxide semiconductor layer 230 can be suppressed. Furthermore, when an oxide is used for the insulating layer 130, excessive oxidation of the conductive layer 120 by the insulating layer 130 can be suppressed. Alternatively, for example, the conductive layer 120 may have a structure in which tungsten is stacked on titanium nitride.
[0470] Furthermore, since the conductive layer 120 has a region in contact with the oxide semiconductor layer 230, it is preferable to use a conductive material containing oxygen. By using a conductive material containing oxygen for the conductive layer 120, the conductive layer 120 can maintain its conductivity even when it absorbs oxygen. Furthermore, even when an insulating layer containing oxygen, such as zirconium oxide, is used for the insulating layer 130, the conductive layer 120 is preferably able to maintain its conductivity. For example, ITO, ITSO, IZO (registered trademark), or the like can be used as a single layer or a stacked layer.
[0471] Since the insulating layer 180 functions as an interlayer film, it preferably has a low dielectric constant. By using a material with a low dielectric constant as the interlayer film, the parasitic capacitance generated between wirings can be reduced. As the insulating layer 180, an insulating layer containing a material with a low dielectric constant can be used in a single layer or a stacked layer. Silicon oxide and silicon oxynitride are preferable because they are thermally stable.
[0472] 16B and 16C, the insulating layer 180 is shown as a single layer, but the present invention is not limited to this. The insulating layer 180 may have a stacked structure of two layers, or a stacked structure of three or more layers.
[0473] <Configuration Example 2 of Memory Device> The memory cell 150 including the transistor 200 and the capacitor 100 described in this embodiment can be used as a memory cell of a memory device. The transistor 200 is a transistor in which a channel is formed in a semiconductor layer including an oxide semiconductor. The transistor 200 has a low off-state current; therefore, by using the transistor 200 in a memory device, stored data can be retained for a long period of time. That is, a refresh operation is not required or the frequency of the refresh operation is extremely low; therefore, the power consumption of the memory device can be sufficiently reduced. Furthermore, the high frequency characteristics of the transistor 200 enable high-speed reading and writing of data from and to the memory device.
[0474] A memory cell array can be configured by arranging the memory cells 150 in a three-dimensional matrix.
[0475] 17A is a plan view of a memory device, showing an example in which 2×2 memory cells (memory cells 150a to 150d) are arranged in the X and Y directions.
[0476] 17B is a cross-sectional view taken along dashed line A3-A4 in FIG. 17A. In FIG. 17A and FIG. 17B, two memory cells (memory cell 150a and memory cell 150b in FIG. 17B) are connected to a common wiring (conductive layer 246).
[0477] Here, each of the memory cells 150a and 150b shown in FIGS. 17A and 17B has the same configuration as the memory cell 150. The memory cell 150a includes a capacitor 100a and a transistor 200a, and the memory cell 150b includes a capacitor 100b and a transistor 200b. The memory cells 150c and 150d shown in FIG. 17A also have the same configuration as the memory cell 150. Therefore, in the memory device shown in FIGS. 17A and 17B, structures having the same functions as the structures constituting the memory device shown in FIG. 10 are denoted by the same reference numerals. For details of the memory cells 150a to 150d, the description of the memory cell 150 in <Configuration Example 1 of Memory Device> can be referred to.
[0478] 17A and 17B , a conductive layer 260 functioning as a wiring WOL is provided in each of the memory cells 150a and 150b. As shown in FIG. 17A , one conductive layer 260 is provided in common to the memory cells 150a and 150c, and another conductive layer 260 is provided in common to the memory cells 150b and 150d. One conductive layer 240 functioning as part of the wiring BIL is provided in common to the memory cells 150a and 150b. That is, the conductive layer 240 is in contact with the oxide semiconductor layer 230 of the memory cell 150a and the oxide semiconductor layer 230 of the memory cell 150b. The other conductive layer 240 is provided in common to the memory cells 150c and 150d.
[0479] 17A and 17B includes conductive layers 245 and 246 that are electrically connected to the memory cell 150a and the memory cell 150b and function as plugs (which can also be referred to as connection electrodes). The conductive layer 245 is disposed in openings formed in the insulating layer 140, the insulating layer 180, the insulating layer 130, and the insulating layer 280, and is in contact with the bottom surface of the conductive layer 240. The conductive layer 246 is disposed in openings formed in the insulating layer 285, the insulating layer 283, and the insulating layer 250, and is in contact with the top surface of the conductive layer 240. Note that the conductive layers 245 and 246 can be formed using a conductive material that can be used for the conductive layer 240, or the like.
[0480] The insulating layer 285 preferably has a low relative dielectric constant because it functions as an interlayer film. By using a material with a low relative dielectric constant as the interlayer film, parasitic capacitance occurring between wirings can be reduced.
[0481] The concentration of impurities such as water and hydrogen in the insulating layer 285 is preferably reduced. This can prevent impurities such as water and hydrogen from entering a channel formation region of the oxide semiconductor layer 230.
[0482] The conductive layers 245 and 246 function as plugs or wirings for electrically connecting circuit elements, wirings, electrodes, or terminals, such as switches, transistors, capacitors, inductors, resistors, and diodes, to the memory cells 150a and 150b. For example, the conductive layer 245 can be electrically connected to a sense amplifier (not shown) provided below the memory device shown in FIG. 17B, and the conductive layer 246 can be electrically connected to a similar memory device (not shown) provided above the memory device shown in FIG. 17B. In this case, the conductive layers 245 and 246 function as part of the wiring BIL. In this way, by providing a memory device above or below the memory device shown in FIG. 17B, the memory capacity per unit area can be increased.
[0483] The memory cell 150a and the memory cell 150b are symmetrical with respect to the perpendicular bisector of the dashed-dotted line A3-A4. Therefore, the transistor 200a and the transistor 200b are also arranged symmetrically with the conductive layer 245 and the conductive layer 246 sandwiched therebetween. The conductive layer 240 functions as the other of the source and drain electrodes of the transistor 200a and the other of the source and drain electrodes of the transistor 200b. The transistor 200a and the transistor 200b share the conductive layer 245 and the conductive layer 246, which function as plugs. By configuring the connections between the two transistors and the plugs as described above, a memory device that can be miniaturized or highly integrated can be provided.
[0484] Note that the conductive layer 110 functioning as the wiring CAL may be provided in each of the memory cells 150 a and 150 b, or may be provided in common to the memory cells 150 a and 150 b. However, as shown in FIG. 17B , the conductive layer 110 is provided apart from the conductive layer 245 to prevent a short circuit between the conductive layer 110 and the conductive layer 245.
[0485] 18 shows an example in which the four memory cells shown in FIG. 17A are stacked in n layers (n is an integer of 3 or more) in the Z direction. FIG. 18 is a cross-sectional view taken along dashed line A3-A4 shown in FIG. 17A.
[0486] The memory device shown in FIG. 18 has n memory layers 160. Specifically, memory layer 160[2] is provided on memory layer 160[1], and (n-2) memory layers are further provided on memory layer 160[2], with memory layer 160[n] provided at the top. The number of memory cells included in one memory layer 160 is not particularly limited, and two or more memory cells may be included. The memory cells included in the n memory layers 160 are electrically connected to a sense amplifier (not shown) provided below the n memory layers 160 by conductive layers 245, 246, 247, 248, etc.
[0487] 18, by stacking a plurality of memory cells, it is possible to integrate and arrange the cells without increasing the area occupied by the memory cell array, that is, it is possible to configure a 3D memory cell array.
[0488] FIG. 19 shows an example of a cross-sectional configuration of a memory device in which a layer having memory cells is stacked over a layer in which a driver circuit including a sense amplifier is provided.
[0489] In FIG. 19, the memory cell 150 (the transistor 200 and the capacitor 100 ) is provided above the transistor 300 .
[0490] The transistor 300 is one of the transistors included in the sense amplifier.
[0491] For the memory cell 150 shown in FIG. 19, the description of the memory cell 150 in <Configuration example 1 of memory device> can be referred to.
[0492] 19, by configuring the sense amplifier so that it overlaps with the memory cell 150, the bit line can be shortened. This reduces the bit line capacitance and the memory cell storage capacitance. This allows the memory device to be driven at high speed.
[0493] 19 can correspond to the semiconductor device 900 described in Embodiment 3. Specifically, the transistor 300 corresponds to a transistor included in a sense amplifier 927 in the semiconductor device 900. The memory cell 150 corresponds to a memory cell 950.
[0494] The transistor 300 is provided over a substrate 311 and includes a conductive layer 316 functioning as a gate, an insulating layer 315 functioning as a gate insulating layer, a semiconductor region 313 formed of part of the substrate 311, and a low-resistance region 314 a and a low-resistance region 314 b functioning as a source region or a drain region. The transistor 300 may be either a p-channel type or an n-channel type.
[0495] Here, in the transistor 300 shown in FIG. 19 , a semiconductor region 313 (a part of a substrate 311) where a channel is formed has a convex shape. A conductive layer 316 is provided to cover the side and top surfaces of the semiconductor region 313 with an insulating layer 315 interposed therebetween. Note that the conductive layer 316 may be made of a material that adjusts the work function. Such a transistor 300 is also called a FIN-type transistor because it utilizes the convex portion of the semiconductor substrate. Note that an insulating layer that is in contact with the top of the convex portion and functions as a mask for forming the convex portion may be provided. Although the case where the convex portion is formed by processing a part of the semiconductor substrate has been described here, a semiconductor film having a convex shape may also be formed by processing an SOI substrate.
[0496] Note that the transistor 300 illustrated in FIG. 19 is just an example, and the structure is not limited thereto. An appropriate transistor can be used depending on the circuit configuration or driving method.
[0497] Between each structure, a wiring layer provided with an interlayer film, wiring, plugs, etc. may be provided. Furthermore, multiple wiring layers may be provided depending on the design. Here, for a conductive layer functioning as a plug or wiring, multiple structures may be collectively assigned the same reference numeral. Furthermore, in this specification and the like, the wiring and the plug electrically connected to the wiring may be integrated. That is, there are cases where a part of the conductive layer functions as the wiring, and cases where a part of the conductive layer functions as the plug.
[0498] For example, an insulating layer 320, an insulating layer 322, an insulating layer 324, and an insulating layer 326 are stacked in this order as an interlayer film over the transistor 300. A conductive layer 328 is embedded in the insulating layer 320 and the insulating layer 322, and a conductive layer 330 is embedded in the insulating layer 324 and the insulating layer 326. The conductive layer 328 and the conductive layer 330 function as plugs or wirings.
[0499] The insulating layer serving as an interlayer film may also function as a planarizing film that covers the underlying unevenness. For example, the top surface of the insulating layer 322 may be planarized by a planarization process using a CMP method or the like to improve the planarity.
[0500] A wiring layer may be provided over the insulating layer 326 and the conductive layer 330. For example, in FIG. 19 , an insulating layer 350, an insulating layer 352, and an insulating layer 354 are stacked in this order. A conductive layer 356 is formed in the insulating layer 350, the insulating layer 352, and the insulating layer 354. The conductive layer 356 functions as a plug or a wiring.
[0501] The insulating layer 352, the insulating layer 354, and the like, which function as interlayer films, can be formed using the above-described insulating layer that can be used in a semiconductor device or a memory device.
[0502] For conductive layers functioning as plugs or wirings, such as the conductive layer 328, the conductive layer 330, and the conductive layer 356, a conductive material applicable to the conductive layer 240 can be used. A high-melting-point material that has both heat resistance and conductivity, such as tungsten or molybdenum, is preferably used, and tungsten is preferably used. Alternatively, a low-resistance conductive material, such as aluminum or copper, is preferably used. The use of a low-resistance conductive material can reduce wiring resistance.
[0503] The conductive layer 240 of the transistor 200 is electrically connected to the low-resistance region 314b functioning as a source region or a drain region of the transistor 300 through the conductive layer 643, the conductive layer 642, the conductive layer 644, the conductive layer 645, the conductive layer 646, the conductive layer 356, the conductive layer 330, and the conductive layer 328.
[0504] The conductive layer 643 is buried in the insulating layer 280. The conductive layer 642 is provided over the insulating layer 130 and buried in the insulating layer 641. The conductive layer 642 can be manufactured using the same material and in the same process as the conductive layer 120. The conductive layer 644 is buried in the insulating layer 180 and the insulating layer 130. The conductive layer 645 is buried in the insulating layer 647. The conductive layer 645 can be manufactured using the same material and in the same process as the conductive layer 110. The conductive layer 646 is buried in the insulating layer 648. The insulating layer 648 electrically insulates the transistor 300 from the conductive layer 110.
[0505] As described above, the memory device of this embodiment has a transistor with reduced parasitic capacitance, and therefore the operating speed can be increased. In addition, the memory device of this embodiment has a capacitor and a transistor stacked on top of each other, and therefore the area occupied by the memory cell in a plan view can be reduced, and a memory device with high integration can be realized.
[0506] This embodiment mode can be combined with other embodiment modes as appropriate.
[0507] Embodiment 3 In this embodiment, a semiconductor device 900 according to one embodiment of the present invention will be described. The semiconductor device 900 can function as a memory device.
[0508] Fig. 20 is a block diagram showing a configuration example of a semiconductor device 900. The semiconductor device 900 shown in Fig. 20 has a driver circuit 910 and a memory array 920. The memory array 920 has one or more memory cells 950. Fig. 20 shows an example in which the memory array 920 has a plurality of memory cells 950 arranged in a matrix.
[0509] The memory cell 950 can be any of the memory devices described in Embodiment 2 (such as the memory cell 150 ).
[0510] The driver circuit 910 includes a PSW 931 (power switch), a PSW 932, and a peripheral circuit 915. The peripheral circuit 915 includes a peripheral circuit 911, a control circuit 912, and a voltage generating circuit 928.
[0511] In the semiconductor device 900, each circuit, signal, and voltage can be appropriately selected or omitted as needed. Alternatively, other circuits or signals may be added. The signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are input signals from the outside, and the signal RDA is an output signal to the outside. The signal CLK is a clock signal.
[0512] Furthermore, signals BW, CE, and GW are control signals. Signal CE is a chip enable signal, signal GW is a global write enable signal, and signal BW is a byte write enable signal. Signal ADDR is an address signal. Signal WDA is write data, and signal RDA is read data. Signals PON1 and PON2 are power gating control signals. Note that signals PON1 and PON2 may be generated by the control circuit 912.
[0513] The control circuit 912 is a logic circuit having a function of controlling the overall operation of the semiconductor device 900. For example, the control circuit 912 performs a logical operation on the signals CE, GW, and BW to determine the operation mode (e.g., write operation, read operation) of the semiconductor device 900. Alternatively, the control circuit 912 generates a control signal for the peripheral circuit 911 so that this operation mode is executed.
[0514] The voltage generating circuit 928 has a function of generating a negative voltage. The signal WAKE has a function of controlling the input of the signal CLK to the voltage generating circuit 928. For example, when an H-level signal is given as the signal WAKE, the signal CLK is input to the voltage generating circuit 928, and the voltage generating circuit 928 generates a negative voltage.
[0515] The peripheral circuit 911 is a circuit for writing and reading data to and from the memory cells 950. The peripheral circuit 911 includes a row decoder 941, a column decoder 942, a row driver 923, a column driver 924, an input circuit 925, an output circuit 926, and a sense amplifier 927.
[0516] The row decoder 941 and the column decoder 942 have the function of decoding the signal ADDR. The row decoder 941 is a circuit for specifying a row to be accessed, and the column decoder 942 is a circuit for specifying a column to be accessed. The row driver 923 has the function of selecting the row specified by the row decoder 941. The column driver 924 has the function of writing data to the memory cells 950, reading data from the memory cells 950, and retaining the read data.
[0517] The input circuit 925 has a function of holding a signal WDA. The data held by the input circuit 925 is output to the column driver 924. The output data of the input circuit 925 is data (Din) to be written to the memory cell 950. The data (Dout) read from the memory cell 950 by the column driver 924 is output to the output circuit 926. The output circuit 926 has a function of holding Dout. In addition, the output circuit 926 has a function of outputting Dout to the outside of the semiconductor device 900. The data output from the output circuit 926 is a signal RDA.
[0518] The PSW 931 is a V DD The PSW 932 has the function of controlling the supply of V to the row driver 923. HM Here, the high power supply voltage of the semiconductor device 900 is V DD and the low power supply voltage is GND (ground potential). HM is the high power supply voltage used to drive the word line high, and V DDThe signal PON1 controls the on / off of the PSW 931, and the signal PON2 controls the on / off of the PSW 932. In FIG. 20, in the peripheral circuit 915, V DD Although the number of power domains to which power is supplied is set to one, it is also possible to set it to a plurality of power domains. In this case, a power switch may be provided for each power domain.
[0519] 21A to 21H, examples of memory cell configurations that can be applied to the memory cell 950 will be described.
[0520] In the following description, when two components are said to be connected, this includes being electrically connected via a circuit element (such as a transistor, a switch, a diode, or a resistor). Electrical connection means that a current can flow between the two components. Note that when two components are connected via a switch or a transistor, this is also included in the term "electrical connection," because a current can flow when these are in the on state.
[0521] 21A shows an example of a circuit configuration of a DRAM memory cell. In this specification and the like, a DRAM using an OS transistor is referred to as a DOSRAM (Dynamic Oxide Semiconductor Random Access Memory). The memory cell 951 includes a transistor M1 and a capacitor CA.
[0522] The transistor M1 may have a front gate (sometimes simply referred to as a gate) and a back gate. In this case, the back gate may be connected to a wiring to which a constant potential or a signal is applied, or the front gate and the back gate may be connected to each other.
[0523] A first terminal of the transistor M1 is connected to a first terminal of the capacitance element CA, a second terminal of the transistor M1 is connected to the wiring BIL, and a gate of the transistor M1 is connected to the wiring WOL. The second terminal of the capacitance element CA is connected to the wiring CAL.
[0524] The wiring BIL functions as a bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitance element CA. When writing and reading data, it is preferable to apply a low-level potential (sometimes referred to as a reference potential) to the wiring CAL.
[0525] Data is written and read by applying a high-level potential to the wiring WOL, turning on the transistor M1, and bringing the wiring BIL and the first terminal of the capacitor CA into a conductive state (a state in which current can flow).
[0526] Furthermore, the memory cell that can be used as the memory cell 950 is not limited to the memory cell 951, and the circuit configuration can be changed. For example, the memory cell 952 shown in FIG. 21B may be used. The memory cell 952 is an example in which the capacitor CA and the wiring CAL are not included. The first terminal of the transistor M1 is in an electrically floating state.
[0527] In the memory cell 952, the potential written through the transistor M1 is held in a capacitance (also referred to as a parasitic capacitance) between the first terminal and the gate, which is indicated by a dashed line. With this configuration, the configuration of the memory cell can be significantly simplified.
[0528] Note that an OS transistor is preferably used as the transistor M1. An OS transistor has a characteristic of extremely low off-state current. By using an OS transistor as the transistor M1, the leakage current of the transistor M1 can be significantly reduced. That is, written data can be held by the transistor M1 for a long time, so that the frequency of refreshing the memory cell can be reduced. Alternatively, the refresh operation of the memory cell can be eliminated. Furthermore, because the leakage current is extremely low, multilevel data or analog data can be held in the memory cell 951 and the memory cell 952.
[0529] 21C shows an example circuit configuration of a gain cell type memory cell having two transistors and one capacitor. The memory cell 953 includes a transistor M2, a transistor M3, and a capacitor CB. In this specification and the like, a storage device having a gain cell type memory cell using an OS transistor as the transistor M2 is referred to as a nonvolatile oxide semiconductor RAM (NOSRAM).
[0530] The first terminal of transistor M2 is connected to the first terminal of capacitance element CB, the second terminal of transistor M2 is connected to wiring WBL, and the gate of transistor M2 is connected to wiring WOL. The second terminal of capacitance element CB is connected to wiring CAL. The first terminal of transistor M3 is connected to wiring RBL, the second terminal of transistor M3 is connected to wiring SL, and the gate of transistor M3 is connected to the first terminal of capacitance element CB.
[0531] The wiring WBL functions as a write bit line, the wiring RBL functions as a read bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitance element CB. When writing data, while retaining data, and when reading data, it is preferable to apply a low-level potential (sometimes referred to as a reference potential) to the wiring CAL.
[0532] Data is written by applying a high-level potential to the wiring WOL, turning on the transistor M2, and establishing electrical continuity between the wiring WBL and the first terminal of the capacitor CB. Specifically, when the transistor M2 is on, a potential corresponding to the information to be recorded is applied to the wiring WBL, and the potential is written to the first terminal of the capacitor CB and the gate of the transistor M3. Then, a low-level potential is applied to the wiring WOL, turning off the transistor M2, thereby maintaining the potential of the first terminal of the capacitor CB and the potential of the gate of the transistor M3.
[0533] Data is read by applying a predetermined potential to the wiring SL. The current flowing between the source and drain of the transistor M3 and the potential of the first terminal of the transistor M3 are determined by the potential of the gate of the transistor M3 and the potential of the second terminal of the transistor M3. Therefore, the potential held in the first terminal of the capacitor CB (or the gate of the transistor M3) can be read by reading the potential of the wiring RBL connected to the first terminal of the transistor M3. In other words, information written in this memory cell can be read from the potential held in the first terminal of the capacitor CB (or the gate of the transistor M3).
[0534] Alternatively, for example, the wiring WBL and the wiring RBL may be combined into a single wiring BIL. An example circuit configuration of such a memory cell is shown in FIG. 21D. The memory cell 954 is configured such that the wiring WBL and the wiring RBL of the memory cell 953 are combined into a single wiring BIL, and the second terminal of the transistor M2 and the first terminal of the transistor M3 are connected to the wiring BIL. In other words, the memory cell 954 is configured to operate as a write bit line and a read bit line using a single wiring BIL.
[0535] 21E is an example in which the capacitor element CB and the wiring CAL in the memory cell 953 are omitted. Also, the memory cell 956 in Fig. 21F is an example in which the capacitor element CB and the wiring CAL in the memory cell 954 are omitted. With such a configuration, the integration degree of the memory cells can be increased.
[0536] Note that at least the transistor M2 is preferably an OS transistor, and in particular, the transistors M2 and M3 are preferably OS transistors.
[0537] Since the OS transistor has an extremely low off-state current, written data can be held by the transistor M2 for a long time, which reduces the frequency of refreshing the memory cell. Alternatively, the refresh operation of the memory cell can be eliminated. Furthermore, since the leakage current is extremely low, multilevel data or analog data can be held in the memory cell 953, the memory cell 954, the memory cell 955, and the memory cell 956.
[0538] The memory cell 953, the memory cell 954, the memory cell 955, and the memory cell 956, each of which uses an OS transistor as the transistor M2, are one embodiment of an NOSRAM.
[0539] Note that a Si transistor may be used as the transistor M3. The Si transistor can increase the field effect mobility and can also be used as a p-channel transistor, thereby increasing the degree of freedom in circuit design.
[0540] When an OS transistor is used as the transistor M3, the memory cell can be configured as a unipolar circuit.
[0541] 21G shows a three-transistor, one-capacitor gain cell type memory cell 957. The memory cell 957 has transistors M4 to M6 and a capacitor CC.
[0542] The first terminal of transistor M4 is connected to the first terminal of capacitor CC, the second terminal of transistor M4 is connected to wiring BIL, and the gate of transistor M4 is connected to wiring WOL. The second terminal of capacitor CC is connected to the first terminal of transistor M5 and wiring GNDL. The second terminal of transistor M5 is connected to the first terminal of transistor M6, and the gate of transistor M5 is connected to the first terminal of capacitor CC. The second terminal of transistor M6 is connected to wiring BIL, and the gate of transistor M6 is connected to wiring RWL.
[0543] The wiring BIL functions as a bit line, the wiring WOL functions as a write word line, and the wiring RWL functions as a read word line. The wiring GNDL is a wiring that applies a low-level potential.
[0544] Data is written by applying a high-level potential to the wiring WOL, turning on the transistor M4, and establishing electrical continuity between the wiring BIL and the first terminal of the capacitor CC. Specifically, when the transistor M4 is on, a potential corresponding to the information to be recorded is applied to the wiring BIL, and the potential is written to the first terminal of the capacitor CC and the gate of the transistor M5. Then, a low-level potential is applied to the wiring WOL, turning off the transistor M4, thereby maintaining the potential of the first terminal of the capacitor CC and the potential of the gate of the transistor M5.
[0545] Data is read by precharging the wiring BIL to a predetermined potential, then electrically floating the wiring BIL, and applying a high-level potential to the wiring RWL. Because the wiring RWL is at a high-level potential, the transistor M6 is turned on, and the wiring BIL and the second terminal of the transistor M5 are electrically connected. At this time, the potential of the wiring BIL is applied to the second terminal of the transistor M5. The potential of the second terminal of the transistor M5 and the potential of the wiring BIL change depending on the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5). By reading the potential of the wiring BIL, the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5) can be read. In other words, information written in this memory cell can be read from the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5).
[0546] Note that at least the transistor M4 is preferably an OS transistor.
[0547] Note that Si transistors may be used as the transistors M5 and M6. As described above, Si transistors may have higher field-effect mobility than OS transistors depending on the crystalline state of silicon used in the semiconductor layer.
[0548] When OS transistors are used as the transistors M5 and M6, the memory cell can be configured as a unipolar circuit.
[0549] 21H shows an example of an SRAM (Static Random Access Memory) using an OS transistor. In this specification and the like, an SRAM using an OS transistor is referred to as an OS-SRAM (Oxide Semiconductor-SRAM). Note that a memory cell 958 shown in FIG. 21H is a memory cell of an SRAM capable of backing up data.
[0550] The memory cell 958 includes transistors M7 to M10, transistors MS1 to MS4, and capacitors CD1 and CD2. Note that the transistors MS1 and MS2 are p-channel transistors, and the transistors MS3 and MS4 are n-channel transistors.
[0551] A first terminal of transistor M7 is connected to wiring BIL, and a second terminal of transistor M7 is connected to a first terminal of transistor MS1, a first terminal of transistor MS3, the gate of transistor MS2, the gate of transistor MS4, and a first terminal of transistor M10. The gate of transistor M7 is connected to wiring WOL. A first terminal of transistor M8 is connected to wiring BILB, and a second terminal of transistor M8 is connected to a first terminal of transistor MS2, the first terminal of transistor MS4, the gate of transistor MS1, the gate of transistor MS3, and a first terminal of transistor M9. The gate of transistor M8 is connected to wiring WOL.
[0552] A second terminal of the transistor MS1 is connected to the wiring VDL. A second terminal of the transistor MS2 is connected to the wiring VDL. A second terminal of the transistor MS3 is connected to the wiring GNDL. A second terminal of the transistor MS4 is connected to the wiring GNDL.
[0553] A second terminal of the transistor M9 is connected to a first terminal of the capacitor CD1, and a gate of the transistor M9 is connected to the wiring BRL. A second terminal of the transistor M10 is connected to a first terminal of the capacitor CD2, and a gate of the transistor M10 is connected to the wiring BRL.
[0554] A second terminal of the capacitance element CD1 is connected to the wiring GNDL, and a second terminal of the capacitance element CD2 is connected to the wiring GNDL.
[0555] The wirings BIL and BILB function as bit lines, the wiring WOL functions as a word line, and the wiring BRL is a wiring that controls the on / off states of the transistors M9 and M10.
[0556] The wiring VDL is a wiring that applies a high-level potential, and the wiring GNDL is a wiring that applies a low-level potential.
[0557] Data is written by applying a high-level potential to the wiring WOL and a high-level potential to the wiring BRL. Specifically, when the transistor M10 is on, a potential corresponding to information to be written is applied to the wiring BIL, and the potential is written to the second terminal of the transistor M10.
[0558] Since the memory cell 958 includes an inverter loop formed by the transistors MS1 and MS2, an inverted signal of the data signal corresponding to the potential is input to the second terminal of the transistor M8. Because the transistor M8 is on, the potential applied to the wiring BIL, i.e., the inverted signal of the signal input to the wiring BIL, is output to the wiring BILB. Because the transistors M9 and M10 are on, the potentials of the second terminals of the transistors M7 and M8 are held in the first terminals of the capacitors CD2 and CD1, respectively. After that, a low-level potential is applied to the wiring WOL and a low-level potential is applied to the wiring BRL to turn off the transistors M7 to M10, thereby holding the potentials of the first terminals of the capacitors CD1 and CD2.
[0559] Data is read by precharging the wirings BIL and BILB to a predetermined potential in advance, and then applying a high-level potential to the wiring WOL and a high-level potential to the wiring BRL. The potential of the first terminal of the capacitor CD1 is refreshed by the inverter loop of the memory cell 958 and output to the wiring BILB. The potential of the first terminal of the capacitor CD2 is refreshed by the inverter loop of the memory cell 958 and output to the wiring BIL. The potentials of the wirings BIL and BILB change from the precharged potentials to the potentials of the first terminal of the capacitor CD2 and the first terminal of the capacitor CD1, respectively. Therefore, the potential held in the memory cell can be read from the potential of the wiring BIL or BILB.
[0560] Note that OS transistors are preferably used as the transistors M7 to M10. This allows written data to be held by the transistors M7 to M10 for a long time, which reduces the frequency of refreshing the memory cells. Alternatively, refreshing the memory cells can be eliminated.
[0561] Note that Si transistors may be used as the transistors MS1 to MS4.
[0562] The driver circuit 910 and memory array 920 of the semiconductor device 900 may be provided on the same plane. Alternatively, as shown in FIG. 22A, the driver circuit 910 and memory array 920 may be provided overlapping each other. By providing the driver circuit 910 and memory array 920 overlapping each other, the signal propagation distance can be shortened. Alternatively, as shown in FIG. 22B, the memory array 920 may be provided in multiple layers on the driver circuit 910.
[0563] Next, an example of a processing unit that can include a semiconductor device such as the memory device will be described.
[0564] 23 shows a block diagram of the arithmetic device 960. The arithmetic device 960 shown in FIG. 23 can be applied to, for example, a CPU (Central Processing Unit). The arithmetic device 960 can also be applied to processors such as a GPU (Graphics Processing Unit), a TPU (Tensor Processing Unit), or an NPU (Neural Processing Unit) that have a large number (several tens to several hundreds) of processor cores capable of parallel processing more than a CPU.
[0565] The arithmetic device 960 shown in FIG. 23 has an ALU 991 (ALU: Arithmetic logic unit, arithmetic circuit), an ALU controller 992, an instruction decoder 993, an interrupt controller 994, a timing controller 995, a register 996, a register controller 997, a bus interface 998, a cache 999, and a cache interface 989 on a substrate 990. The substrate 990 may be a semiconductor substrate, an SOI substrate, a glass substrate, or the like. It may also have a rewritable ROM and a ROM interface. The cache 999 and the cache interface 989 may also be provided on separate chips.
[0566] The cache 999 is connected to a main memory provided on a separate chip via a cache interface 989. The cache interface 989 has a function of supplying part of the data held in the main memory to the cache 999. The cache interface 989 also has a function of outputting part of the data held in the cache 999 to the ALU 991, register 996, etc. via the bus interface 998.
[0567] As will be described later, a memory array 920 can be provided stacked on the arithmetic unit 960. The memory array 920 can be used as a cache. In this case, the cache interface 989 may have a function of supplying data held in the memory array 920 to the cache 999. In this case, it is preferable that a drive circuit 910 be included as part of the cache interface 989.
[0568] It is also possible to use only the memory array 920 as a cache without providing the cache 999 .
[0569] The arithmetic device 960 shown in FIG. 23 is merely an example of a simplified configuration, and actual arithmetic devices 960 have a wide variety of configurations depending on their applications. For example, it is preferable to use a configuration including the arithmetic device 960 shown in FIG. 23 as one core, and to include multiple such cores, each of which operates in parallel, in a so-called multi-core configuration. The greater the number of cores, the higher the computational performance. The greater the number of cores, for example, two, preferably four, more preferably eight, even more preferably twelve, and even more preferably sixteen or more. Furthermore, when extremely high computational performance is required, such as for server applications, a multi-core configuration having 16 or more, preferably 32 or more, and even more preferably 64 or more cores is preferable. Furthermore, the number of bits that the arithmetic device 960 can handle via its internal computation circuit, data bus, etc. can be, for example, 8 bits, 16 bits, 32 bits, 64 bits, etc.
[0570] An instruction input to the arithmetic unit 960 via the bus interface 998 is input to the instruction decoder 993, decoded, and then input to the ALU controller 992, interrupt controller 994, register controller 997, and timing controller 995.
[0571] The ALU controller 992, interrupt controller 994, register controller 997, and timing controller 995 perform various controls based on the decoded instructions. Specifically, the ALU controller 992 generates signals for controlling the operation of the ALU 991. Furthermore, the interrupt controller 994 determines and processes interrupt requests from external input / output devices, peripheral circuits, etc. based on their priority, mask status, etc. while the arithmetic unit 960 is executing a program. The register controller 997 generates addresses for registers 996 and reads and writes data from and to the registers 996 depending on the state of the arithmetic unit 960.
[0572] Furthermore, the timing controller 995 generates signals that control the timing of the operations of the ALU 991, the ALU controller 992, the instruction decoder 993, the interrupt controller 994, and the register controller 997. For example, the timing controller 995 includes an internal clock generation unit that generates an internal clock signal based on a reference clock signal, and supplies the internal clock signal to the various circuits described above.
[0573] 23, the register controller 997 selects the holding operation of the register 996 in accordance with an instruction from the ALU 991. That is, it selects whether the memory cells of the register 996 will hold data using flip-flops or using capacitance elements. If holding data using flip-flops is selected, a power supply voltage is supplied to the memory cells in the register 996. If holding data using capacitance elements is selected, the data is rewritten to the capacitance elements, and the supply of power supply voltage to the memory cells in the register 996 can be stopped.
[0574] The memory array 920 and the arithmetic unit 960 can be provided overlapping each other. Perspective views of a semiconductor device 970A are shown in Figures 24A and 24B. The semiconductor device 970A has a layer 930 on which memory arrays are provided above the arithmetic unit 960. The layer 930 is provided with memory arrays 920L1, 920L2, and 920L3. The arithmetic unit 960 and each memory array have overlapping regions. To make the configuration of the semiconductor device 970A easier to understand, the arithmetic unit 960 and the layer 930 are shown separately in Figure 24B.
[0575] By stacking the layer 930 having the memory array and the arithmetic unit 960, the connection distance between them can be shortened, thereby increasing the communication speed between them. In addition, the short connection distance reduces power consumption.
[0576] As a method for stacking the layer 930 having a memory array and the arithmetic device 960, a method (also called monolithic stacking) in which the layer 930 having a memory array is stacked directly on the arithmetic device 960 may be used, or a method in which the arithmetic device 960 and the layer 930 are formed on different substrates, the two substrates are bonded together, and the two substrates are electrically connected using a through-via or a conductive film bonding technique (such as Cu-Cu bonding) may be used. The former method does not require consideration of misalignment during bonding, and therefore can not only reduce the chip size but also reduce the manufacturing cost.
[0577] Here, the arithmetic unit 960 does not have a cache 999, and the memory arrays 920L1, 920L2, and 920L3 provided in the layer 930 can each be used as a cache. In this case, for example, the memory array 920L1 can be used as an L1 cache (also referred to as a level 1 cache), the memory array 920L2 can be used as an L2 cache (also referred to as a level 2 cache), and the memory array 920L3 can be used as an L3 cache (also referred to as a level 3 cache). Of the three memory arrays, the memory array 920L3 has the largest capacity and the lowest access frequency. Furthermore, the memory array 920L1 has the smallest capacity and the highest access frequency.
[0578] When the cache 999 provided in the arithmetic unit 960 is used as an L1 cache, each memory array provided in the layer 930 can be used as a lower-level cache or a main memory. The main memory has a larger capacity than the cache and is accessed less frequently.
[0579] 24B, a driving circuit 910L1, a driving circuit 910L2, and a driving circuit 910L3 are provided. The driving circuit 910L1 is connected to the memory array 920L1 via a connection electrode 940L1. Similarly, the driving circuit 910L2 is connected to the memory array 920L2 via a connection electrode 940L2, and the driving circuit 910L3 is connected to the memory array 920L3 via a connection electrode 940L3.
[0580] Although the number of memory arrays functioning as caches is three in this example, the number may be one or two, or four or more.
[0581] When the memory array 920L1 is used as a cache, the drive circuit 910L1 may function as part of the cache interface 989, or may be configured so that the drive circuit 910L1 is connected to the cache interface 989. Similarly, the drive circuits 910L2 and 910L3 may also function as part of the cache interface 989, or may be configured so that they are connected thereto.
[0582] Whether the memory array 920 is made to function as a cache or as a main memory is determined by a control circuit 912 included in each drive circuit 910. The control circuit 912 can cause some of the memory cells 950 included in the semiconductor device 900 to function as RAM based on a signal supplied from the arithmetic device 960.
[0583] The semiconductor device 900 can cause some of the memory cells 950 to function as a cache and the other memory cells to function as a main memory. That is, the semiconductor device 900 can function as both a cache and a main memory. The semiconductor device 900 according to one embodiment of the present invention can function as, for example, a universal memory.
[0584] Furthermore, a layer 930 having one memory array 920 may be provided over the arithmetic device 960. Figure 25A shows a perspective view of a semiconductor device 970B.
[0585] In the semiconductor device 970B, one memory array 920 can be divided into multiple areas, each of which can be used for a different function. Fig. 25A shows an example in which area L1 is used as an L1 cache, area L2 is used as an L2 cache, and area L3 is used as an L3 cache.
[0586] Furthermore, in the semiconductor device 970B, the capacity of each of the areas L1 to L3 can be changed depending on the situation. For example, if it is desired to increase the capacity of the L1 cache, this can be achieved by increasing the area of the area L1. This configuration can improve the efficiency of calculation processing and increase the processing speed.
[0587] Also, multiple memory arrays may be stacked. Figure 25B shows a perspective view of a semiconductor device 970C.
[0588] The semiconductor device 970C includes a layer 930L1 having a memory array 920L1, a layer 930L2 having a memory array 920L2 on top of that, and a layer 930L3 having a memory array 920L3 on top of that. The memory array 920L1, which is physically closest to the arithmetic unit 960, can be used as a higher-level cache, and the memory array 920L3, which is farthest, can be used as a lower-level cache or main memory. This configuration allows the capacity of each memory array to be increased, thereby further improving processing power.
[0589] This embodiment mode can be combined with other embodiment modes as appropriate.
[0590] Embodiment 4 In this embodiment, an application example of a memory device according to one embodiment of the present invention will be described.
[0591] Generally, various memory devices are used in semiconductor devices such as computers depending on the application. FIG. 26A shows various memory devices used in semiconductor devices by layer. The higher the layer, the faster the operating speed of the memory device is required, while the lower the layer, the larger the memory capacity and recording density are required. In FIG. 26A , from the top layer, there are memories embedded as registers in a processing unit such as a CPU, an L1 cache, an L2 cache, an L3 cache, a main memory, and storage. Note that while an example having up to an L3 cache is shown here, lower-level caches may also be included.
[0592] The memory embedded as a register in a processing unit such as a CPU is used for temporary storage of calculation results, and is therefore frequently accessed by the processing unit. Therefore, a higher operating speed is required than a larger memory capacity. Registers also have the function of storing setting information for the processing unit.
[0593] A cache has the function of duplicating and storing a portion of the data stored in main memory. By duplicating frequently used data and storing it in the cache, the access speed to the data can be increased. The storage capacity required for a cache is smaller than that of main memory, but it is required to operate at a faster speed than main memory. In addition, data rewritten in the cache is duplicated and supplied to the main memory.
[0594] The main memory has a function of holding programs, data, etc. read from storage.
[0595] Storage has the function of storing data that requires long-term storage, various programs used by processing units, etc. Therefore, storage requires a large memory capacity and high recording density rather than an operating speed. For example, high-capacity, non-volatile storage devices such as 3D NAND can be used.
[0596] A storage device (OS memory) using an oxide semiconductor according to one embodiment of the present invention has high operating speed and can retain data for a long period of time. Therefore, as shown in FIG. 26A , the storage device according to one embodiment of the present invention can be suitably used in both a tier where a cache is located and a tier where a main memory is located. The storage device according to one embodiment of the present invention can also be applied to a tier where a storage is located.
[0597] FIG. 26B also shows an example in which an SRAM is used as part of a cache and an OS memory of one embodiment of the present invention is used as the other part of the cache.
[0598] The lowest level cache can be called a last level cache (LLC). While an LLC does not require faster operation speed than higher level caches, it is desirable for the LLC to have a large storage capacity. The OS memory of one embodiment of the present invention has a high operation speed and can retain data for a long period of time, and therefore can be suitably used for an LLC. The OS memory of one embodiment of the present invention can also be applied to a final level cache (FLC).
[0599] For example, as shown in Fig. 26B, a configuration can be adopted in which SRAM is used for the higher-level caches (L1 cache, L2 cache, etc.) and the OS memory according to one aspect of the present invention is used for the LLC. Also, as shown in Fig. 26B, not only the OS memory but also DRAM can be applied to the main memory.
[0600] This embodiment mode can be combined with other embodiment modes as appropriate.
[0601] Embodiment 5 In this embodiment, a display device according to one embodiment of the present invention will be described.
[0602] The semiconductor device of one embodiment of the present invention can be used for a display device or a module including the display device. Examples of the module including the display device include a module in which a connector such as a flexible printed circuit (hereinafter referred to as FPC) or a tape carrier package (TCP) is attached to the display device, and a module in which an integrated circuit (IC) is mounted by a chip-on-glass (COG) method, a chip-on-film (COF) method, or the like.
[0603] The display device of this embodiment may also have a function as a touch panel. For example, various detection elements (also referred to as sensor elements) that can detect the proximity or contact of a detection target such as a finger can be applied to the display device.
[0604] Examples of sensor types include a capacitance type, a resistive film type, a surface acoustic wave type, an infrared type, an optical type, and a pressure-sensitive type.
[0605] The capacitance type includes, for example, a surface capacitance type and a projected capacitance type. The projected capacitance type includes, for example, a self-capacitance type and a mutual capacitance type. The mutual capacitance type is preferable because it enables simultaneous multi-point detection.
[0606] Examples of touch panels include out-cell, on-cell, and in-cell types. Note that an in-cell touch panel is a type in which electrodes constituting a detection element are provided on one or both of a substrate supporting a display element and an opposing substrate.
[0607] 27A shows a perspective view of the display module 170. The display module 170 includes a display device 600A and an FPC 298. Note that the display device included in the display module 170 is not limited to the display device 600A, and may be a display device 600B described later.
[0608] The display module 170 includes a substrate 291 and a substrate 299. The display module 170 includes a display portion 297. The display portion 297 is a region that displays an image in the display module 170, and is a region where light from each pixel provided in a pixel portion 294 (described later) can be viewed.
[0609] 27B is a perspective view schematically illustrating the configuration on the substrate 291 side. A circuit portion 292, a pixel circuit portion 293 on the circuit portion 292, and a pixel portion 294 on the pixel circuit portion 293 are stacked on the substrate 291. A terminal portion 295 for connecting to an FPC 298 is provided in a portion of the substrate 291 that does not overlap with the pixel portion 294. The terminal portion 295 and the circuit portion 292 are electrically connected by a wiring portion 296 composed of a plurality of wirings.
[0610] The semiconductor device of one embodiment of the present invention can be applied to one or both of the circuit portion 292 and the pixel circuit portion 293 .
[0611] The pixel section 294 has a plurality of periodically arranged pixels 294a. An enlarged view of one pixel 294a is shown on the right side of Fig. 27B. Fig. 27B shows an example in which one pixel 294a has a sub-pixel 130R that emits red light, a sub-pixel 130G that emits green light, and a sub-pixel 130B that emits blue light.
[0612] Each subpixel has a display element. Various elements can be used as the display element, including, for example, a liquid crystal element and a light-emitting element. Other examples include shutter-type or optical interference-type MEMS (Micro Electro Mechanical Systems) elements, display elements using microcapsules, electrophoresis, electrowetting, or electronic liquid powder (registered trademark) methods, etc. Furthermore, a QLED (Quantum-dot LED) using a light source and color conversion technology using quantum dot materials may also be used.
[0613] Examples of the light-emitting element include self-luminous light-emitting elements such as LEDs (Light Emitting Diodes), OLEDs (Organic LEDs), semiconductor lasers, etc. Examples of the LED that can be used include mini LEDs and micro LEDs.
[0614] The pixel arrangement in the display device of this embodiment is not particularly limited, and various methods can be applied. Examples of pixel arrangements include a stripe arrangement, an S-stripe arrangement, a matrix arrangement, a delta arrangement, a Bayer arrangement, and a pentile arrangement. Figure 27B shows an example in which a stripe arrangement is applied to the pixel arrangement.
[0615] The pixel circuit section 293 has a plurality of pixel circuits 293a arranged periodically.
[0616] One pixel circuit 293a is a circuit that controls the driving of multiple elements included in one pixel 294a. One pixel circuit 293a can be configured to have three circuits that control the light emission of one light-emitting element. For example, the pixel circuit 293a can be configured to have at least one selection transistor, one current control transistor (drive transistor), and a capacitor for each light-emitting element. In this case, a gate signal is input to the gate of the selection transistor, and a source signal is input to the source. This realizes an active matrix display device.
[0617] The circuit portion 292 includes a circuit for driving each pixel circuit 293a of the pixel circuit portion 293. For example, it is preferable that the circuit portion 292 includes one or both of a gate line driver circuit and a source line driver circuit. In addition, the circuit portion 292 may include at least one of an arithmetic circuit, a memory circuit, a power supply circuit, and the like.
[0618] The FPC 298 functions as wiring for supplying a video signal, a power supply potential, or the like from the outside to the circuit portion 292. An IC may be mounted on the FPC 298.
[0619] The display module 170 can be configured such that one or both of the pixel circuit portion 293 and the circuit portion 292 are provided overlapping below the pixel portion 294, thereby making it possible to extremely increase the aperture ratio (effective display area ratio) of the display portion 297. In addition, the pixels 294a can be arranged at extremely high density, making it possible to extremely increase the resolution of the display portion 297.
[0620] Because such a display module 170 has extremely high resolution, it can be suitably used in VR devices such as HMDs or eyeglass-type AR devices. For example, even in a configuration in which the display unit of the display module 170 is viewed through lenses, the display module 170 has an extremely high-resolution display unit 297, so even when the display unit is enlarged with lenses, the pixels are not visible, allowing for a highly immersive display. Furthermore, the display module 170 is not limited to this, and can be suitably used in electronic devices with relatively small displays. For example, it can be suitably used in the display unit of a wearable electronic device such as a wristwatch.
[0621] 28 shows a cross-sectional view of a display device 600A. The display device 600A is an example of a display device to which an MML (metal maskless) structure is applied. In other words, the display device 600A has light-emitting elements fabricated without using a fine metal mask.
[0622] The island-shaped light-emitting layers in the light-emitting elements of a display device employing the MML structure are formed by depositing a light-emitting layer on one surface and then processing it using photolithography. This allows for the realization of high-definition display devices or display devices with a high aperture ratio, which have been difficult to achieve until now. Furthermore, since the light-emitting layers can be created separately for each color, a display device with extremely vivid images, high contrast, and high display quality can be realized. For example, if a display device is composed of three types of light-emitting elements, namely, light-emitting elements that emit blue light, light-emitting elements that emit green light, and light-emitting elements that emit red light, the deposition of the light-emitting layers and the processing by photolithography can be repeated three times to form the three types of island-shaped light-emitting layers.
[0623] Because devices with an MML structure can be manufactured without using a metal mask, they can exceed the upper limit of resolution imposed by the alignment accuracy of the metal mask. Furthermore, when devices are manufactured without using a metal mask, the equipment required for manufacturing the metal mask and the metal mask cleaning process are unnecessary. Furthermore, since photolithography processing can be performed using the same or similar equipment as that used to manufacture transistors, there is no need to introduce special equipment to manufacture devices with an MML structure. As such, the MML structure allows for low manufacturing costs, making it suitable for mass production of devices.
[0624] In a display device to which the MML structure is applied, there is no need to artificially increase the resolution by applying a special pixel arrangement such as a pentile arrangement, and therefore it is possible to realize a display device with high resolution (for example, 500 ppi or more, 1000 ppi or more, 2000 ppi or more, 3000 ppi or more, or 5000 ppi or more) using a so-called stripe arrangement in which R, G, and B sub-pixels are each arranged in one direction.
[0625] Furthermore, by providing a sacrificial layer on the light-emitting layer, damage to the light-emitting layer during the manufacturing process of the display device can be reduced, and the reliability of the light-emitting element can be improved. Note that the sacrificial layer may remain in the completed display device or may be removed during the manufacturing process. For example, the sacrificial layer 618a shown in FIG. 28, FIG. 29 (described later), and FIG. 36 (described later) is a part of the sacrificial layer provided on the light-emitting layer.
[0626] Furthermore, by employing a film formation step using an area mask and a processing step using a resist mask, a light-emitting element can be manufactured through a relatively simple process.
[0627] A display device 600A illustrated in Figure 28 is a cross-sectional schematic diagram of a display device (semiconductor device) of one embodiment of the present invention. The display device 600A has a structure in which a pixel circuit, a driver circuit, and the like are provided over a substrate 410. Note that in the display device 600A illustrated in Figure 28, in addition to element layers 620, 630, and 660, a wiring layer 670 is also illustrated. The wiring layer 670 is a layer in which wirings are provided.
[0628] A pixel circuit of the display device is preferably provided in the element layer 630. A driver circuit of the display device (either a gate driver or a source driver, or both) is preferably provided in the element layer 620. The element layer 620 may also be provided with one or more types of circuits such as an arithmetic circuit and a memory circuit.
[0629] The element layer 620 includes, for example, a substrate 410 over which a transistor 400d is formed. A wiring layer 670 is provided above the transistor 400d. The wiring layer 670 includes a wiring that electrically connects the transistor 400d to a conductive layer or a transistor (the conductive layer 514 in FIG. 28 ) provided in the element layer 630. An element layer 630 and an element layer 660 are provided above the wiring layer 670. The element layer 630 includes, for example, a transistor MTCK. The element layer 660 includes a light-emitting element 650 (a light-emitting element 650R, a light-emitting element 650G, and a light-emitting element 650B in FIG. 28 ).
[0630] The transistor 400d is an example of a transistor included in the element layer 620. The transistor MTCK is an example of a transistor included in the element layer 630. The light-emitting elements (light-emitting element 650R, light-emitting element 650G, and light-emitting element 650B) are an example of light-emitting elements included in the element layer 660.
[0631] 28 illustrates an example in which the transistor 200 described in the above embodiment is used as the transistor MTCK.
[0632] The substrate 410 can be, for example, a semiconductor substrate (e.g., a single-crystal substrate made of silicon or germanium). Other than a semiconductor substrate, the substrate 410 can be, for example, an SOI (Silicon On Insulator) substrate, a glass substrate, a quartz substrate, a plastic substrate, a sapphire glass substrate, a metal substrate, a stainless steel substrate, a substrate having stainless steel foil, a tungsten substrate, a substrate having tungsten foil, a flexible substrate, a lamination film, paper containing a fibrous material, or a base film. In this embodiment, the substrate 410 will be described as a semiconductor substrate made of silicon. Therefore, the transistor included in the element layer 620 can be a Si transistor.
[0633] The transistor 400d includes an element isolation layer 412, a conductive layer 416, an insulating layer 415, an insulating layer 417, a semiconductor region 413 formed of a part of the substrate 410, and low-resistance regions 414a and 414b that function as source and drain regions. Therefore, the transistor 400d is a Si transistor. Note that although FIG. 28 illustrates a structure in which one of the source and drain of the transistor 400d is electrically connected to the conductive layer 514 provided in the element layer 630 through the conductive layer 428, the conductive layer 430, and the conductive layer 456, the electrical connection structure of the display device of one embodiment of the present invention is not limited thereto.
[0634] The transistor 400d can be a Fin type by, for example, covering the top surface and the side surfaces in the channel width direction of the semiconductor region 413 with a conductive layer 416 via an insulating layer 415 that functions as a gate insulating layer. By making the transistor 400d a Fin type, the effective channel width can be increased, and the on-state characteristics of the transistor 400d can be improved. Furthermore, the contribution of the electric field of the gate electrode can be increased, and the off-state characteristics of the transistor 400d can be improved. The transistor 400d may be a planar type instead of a Fin type.
[0635] Note that the transistor 400d may be either a p-channel transistor or an n-channel transistor. Alternatively, a plurality of transistors 400d may be provided, and both p-channel and n-channel transistors may be used.
[0636] The region in the semiconductor region 413 where the channel is formed, the region nearby, and the low-resistance region 414a and low-resistance region 414b that will become the source region or drain region preferably contain a silicon-based semiconductor, specifically, single-crystal silicon. Alternatively, each of the above-mentioned regions may be formed using, for example, germanium, silicon germanium, gallium arsenide, aluminum gallium arsenide, or gallium nitride. Alternatively, a configuration using silicon in which the effective mass is controlled by applying stress to the crystal lattice and changing the lattice spacing may be used. Alternatively, the transistor 400d may be, for example, a high electron mobility transistor (HEMT) using gallium arsenide and aluminum gallium arsenide.
[0637] The conductive layer 416 functioning as a gate electrode can be made of a semiconductor material such as silicon containing an element that imparts n-type conductivity, such as arsenic or phosphorus, or an element that imparts p-type conductivity, such as boron or aluminum. Alternatively, the conductive layer 416 can be made of a conductive material such as a metal material, an alloy material, or a metal oxide material.
[0638] Since the work function is determined by the material of the conductive layer, the threshold voltage of the transistor can be adjusted by selecting the material of the conductive layer. Specifically, it is preferable to use one or both of titanium nitride and tantalum nitride for the conductive layer. Furthermore, in order to achieve both conductivity and embeddability, it is preferable to use one or both of tungsten and aluminum as a stacked layer for the conductive layer, and tungsten is particularly preferable in terms of heat resistance.
[0639] The element isolation layer 412 is provided to isolate a plurality of transistors formed on the substrate 410. The element isolation layer can be formed using, for example, a local oxidation of silicon (LOCOS) method, a shallow trench isolation (STI) method, or a mesa isolation method.
[0640] Over a transistor 400d shown in FIG. 28, an insulating layer 420 and an insulating layer 422 are stacked in this order from the substrate 410 side.
[0641] The insulating layer 420 and the insulating layer 422 can be formed using, for example, one or more selected from silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, aluminum oxynitride, aluminum nitride oxide, and aluminum nitride.
[0642] The insulating layer 422 may function as a planarizing film that planarizes steps caused by the insulating layer 420 and the transistor 400d covered with the insulating layer 422. For example, the top surface of the insulating layer 422 may be planarized by planarization treatment using a CMP method or the like to improve the planarity.
[0643] A conductive layer 428 is buried in the insulating layer 420 and the insulating layer 422 and connected to the transistor MTCK and the like provided above the insulating layer 422. Note that the conductive layer 428 functions as a plug or a wiring.
[0644] In the display device 600A, a wiring layer 670 is provided over the transistor 400d. The wiring layer 670 includes, for example, an insulating layer 424, an insulating layer 426, a conductive layer 430, an insulating layer 450, an insulating layer 452, an insulating layer 454, and a conductive layer 456.
[0645] An insulating layer 424 and an insulating layer 426 are stacked in this order over the insulating layer 422 and the conductive layer 428. An opening is formed in the insulating layer 424 and the insulating layer 426 in a region overlapping with the conductive layer 428. A conductive layer 430 is embedded in the opening.
[0646] An insulating layer 450, an insulating layer 452, and an insulating layer 454 are stacked in this order over the insulating layer 426 and the conductive layer 430. In addition, openings are formed in the insulating layer 450, the insulating layer 452, and the insulating layer 454 in regions overlapping with the conductive layer 430. A conductive layer 456 is embedded in the openings.
[0647] The conductive layer 430 and the conductive layer 456 function as a plug or a wiring connected to the transistor 400d.
[0648] Note that, for example, the insulating layers 424 and 450 are preferably insulating layers having a barrier property against one or more selected from hydrogen, oxygen, and water, similar to the insulating layer 592 described later. Furthermore, the insulating layers 426, 452, and 454 are preferably insulating layers having a relatively low relative dielectric constant in order to reduce parasitic capacitance between wirings, similar to the insulating layer 594 described later. Furthermore, the insulating layers 426, 452, and 454 function as interlayer insulating films and planarizing films.
[0649] The conductive layer 456 preferably includes a conductive layer having a barrier property against one or more selected from hydrogen, oxygen, and water.
[0650] For example, tantalum nitride may be used as the insulating layer having a barrier property against hydrogen. Furthermore, by stacking tantalum nitride and tungsten, which has high conductivity, it is possible to suppress diffusion of hydrogen from the transistor 400d while maintaining the conductivity of the wiring. In this case, it is preferable that the tantalum nitride layer having a barrier property against hydrogen be in contact with the insulating layer 450 having a barrier property against hydrogen.
[0651] An insulating layer 513 is provided above the insulating layer 454 and the conductive layer 456. An insulating layer IS1 is provided over the insulating layer 513. A conductive layer functioning as a plug or a wiring is embedded in the insulating layer IS1 and the insulating layer 513. This allows the transistor 400d to be electrically connected to the conductive layer 514 provided in the element layer 630. Alternatively, one of the source or drain of the transistor MTCK may be electrically connected to one of the source or drain of the transistor 400d.
[0652] A transistor MTCK and an insulating layer IS2 are provided on the insulating layer IS1. A semiconductor layer of the transistor MTCK, an insulating layer functioning as a gate insulating layer, a conductive layer functioning as a gate electrode, etc. are arranged in an opening in the insulating layer IS2. An insulating layer IS3, an insulating layer 574, and an insulating layer 581 are stacked in this order on the transistor MTCK. A conductive layer MPG functioning as a plug or wiring is buried in the insulating layer IS3, the insulating layer 574, and the insulating layer 581.
[0653] The insulating layer 574 preferably has a function of suppressing diffusion of impurities such as water and hydrogen (e.g., hydrogen atoms and / or hydrogen molecules). That is, the insulating layer 574 preferably functions as a barrier insulating film that suppresses the impurities from entering the transistor MTCK. The insulating layer 574 also preferably has a function of suppressing diffusion of oxygen (e.g., oxygen atoms and / or oxygen molecules). For example, the insulating layer 574 preferably has lower oxygen permeability than the insulating layers IS2 and IS3.
[0654] Therefore, the insulating layer 574 preferably functions as a barrier insulating film that suppresses diffusion of impurities such as water and hydrogen. Therefore, the insulating layer 574 does not diffuse hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, or nitrogen oxide molecules (for example, N 2 O, NO, and NO 2It is preferable to use an insulating material that has a function of suppressing the diffusion of impurities such as copper atoms and copper atoms (i.e., the impurities are less likely to permeate through the insulating material). Alternatively, it is preferable to use an insulating material that has a function of suppressing the diffusion of oxygen (e.g., oxygen atoms and / or oxygen molecules) (i.e., the oxygen is less likely to permeate through the insulating material).
[0655] For the insulating layer having a function of suppressing the permeation of impurities such as water and hydrogen and oxygen, any of the materials that can be used for the insulating layer having a function of suppressing the permeation of impurities and oxygen, which are exemplified in Embodiment 1, can be used.
[0656] In particular, it is preferable to use aluminum oxide or silicon nitride for the insulating layer 574. This can prevent impurities such as water and hydrogen from diffusing from above the insulating layer 574 to the transistor MTCK. Alternatively, it can prevent oxygen contained in the insulating layer IS3 or the like from diffusing above the insulating layer 574.
[0657] The insulating layer 581 is a film that functions as an interlayer film, and preferably has a lower dielectric constant than the insulating layer 574. By using a material with a low dielectric constant as the interlayer film, the parasit...
Claims
A first transistor and a first insulating layer, the first transistor has a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer, and a gate electrode; the first conductive layer is one of a source electrode and a drain electrode of the first transistor, and the second conductive layer is the other of the source electrode and the drain electrode of the first transistor; the first conductive layer and the second conductive layer are located at different heights; the first insulating layer is provided between the first conductive layer and the second conductive layer and has a first opening reaching the first conductive layer; the second conductive layer is provided on the first insulating layer; the gate electrode overlaps with the semiconductor layer with the gate insulating layer interposed therebetween; the semiconductor layer has a first region covering an upper surface of the first conductive layer in the first opening, a second region covering a side surface of the first insulating layer in the first opening, and a third region covering an upper surface of the second conductive layer and overlapping the gate electrode; the gate insulating layer has a fourth region provided facing a side wall of the first opening of the first insulating layer with the second region therebetween, a fifth region covering an upper surface of the third region, and a sixth region covering an upper surface of the second conductive layer and positioned outside an end of the gate electrode in a top view; The film thickness of the fifth region is greater than the film thickness of the fourth region, A semiconductor device, wherein the fifth region is thicker than the sixth region. In claim 1, A semiconductor device, wherein the fifth region has a thickness that is at least 2 nm thicker than the sixth region. In claim 1 or 2, A semiconductor device, wherein the sixth region has a thickness of 1.0 nm or more and 100 nm or less. In claim 1, A semiconductor device, wherein the fourth region has a thickness of 0.1 nm or more and 7.0 nm or less. In claim 1, The semiconductor layer covers an upper surface of the second conductive layer and has a region covered by the sixth region. In claim 1, the second conductive layer has a second opening overlapping the first opening; the semiconductor layer has a region covering a side surface of the second conductive layer in the second opening, The first insulating layer has a region that covers the second opening with the semiconductor layer sandwiched therebetween. forming a first insulating layer on the first conductive layer; forming a second conductive layer on the first insulating layer; forming a first opening reaching the first conductive layer by removing a portion of the second conductive layer and a portion of the first insulating layer to expose an upper surface of the first conductive layer; forming a first semiconductor layer so as to be in contact with an upper surface of the first conductive layer, a side surface of the first insulating layer within the first opening, a side surface of the second conductive layer within the first opening, and an upper surface of the second conductive layer; forming a second insulating layer in contact with an upper surface of the first semiconductor layer and an upper surface of the first insulating layer; The second insulating layer is formed using a method having anisotropic deposition rate; the second insulating layer is formed such that a thickness of a region covering a side surface of the first opening with the first semiconductor layer therebetween is thinner than a thickness of a region covering an upper surface of the first conductive layer; forming a third conductive layer on the second insulating layer; forming a first mask using a photolithography method; performing dry etching using the first mask; forming a fourth conductive layer by removing a portion of the third conductive layer by the dry etching; a first mask that is formed on the second insulating layer and that is formed on the first conductive layer; a first insulating layer that is formed on the first conductive layer and that is not covered with the first mask; In claim 7, The method for manufacturing a semiconductor device, wherein the second insulating layer is formed by ionization sputtering. In claim 7, The method for manufacturing a semiconductor device, wherein the second insulating layer is formed by a long throw sputtering method. In claim 7, The method for manufacturing a semiconductor device, wherein the second insulating layer is formed by using a plasma enhanced chemical vapor deposition method.
Citation Information
Patent Citations
Thin-film transistor of semiconductor memory device and its manufacture
JP1994053440A
Semiconductor device, and manufacturing method for the same
JP2016149552A
Semiconductor device
JP2017168764A
Cited By
Semiconductor device and method for manufacturing semiconductor device
WO2026167508A1