Method for preparation of hard carbon

The synthesis of hard carbon electrodes through pyrolysis and KOH activation of bagasse, combined with graphene oxide coating, addresses structural limitations, enhancing their electrochemical performance and efficiency for energy storage systems.

WO2024231941A1PCT designated stage expired Publication Date: 2024-11-14GODI INDIA PVT LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/IN2024/050317
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-03-26
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Conventional methods for synthesizing hard carbon electrodes face challenges such as low packing density, irreversible capacity, and rate capability limitations, particularly due to high oxygen content and disordered structures, which affect their performance in energy storage systems like sodium-ion and lithium-ion batteries and capacitors.

Method used

A method involving the pyrolysis of bagasse at 1000 °C, followed by chemical activation with KOH and subsequent graphene oxide coating, to enhance the electrochemical properties and structural integrity of hard carbon, improving its charge storage capacity and retention.

Benefits of technology

The method results in hard carbon electrodes with increased Initial Coulombic efficiency, reduced irreversible capacity loss, and enhanced rate capability, suitable for high-performance energy storage applications, including Li-ion and Na-ion batteries and capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IN2024050317_14112024_PF_FP_ABST
    Figure IN2024050317_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparation of hard carbon for an energy storage device The method comprises burning dry bagasse in air to obtain a first carbonaceous material (C1). The first carbonaceous material (C1) is chemically activated with a Potassium Hydroxide (KOH) solution at a first pre-defined temperature for a first pre-defined time period, to obtain a chemically activated first carbonaceous material. The chemically activated first carbonaceous material is washed using Deionized (DI) water, to obtain a second carbonaceous material (C2). A heat treatment is performed on the second carbonaceous material (C2) in an inert atmosphere at a second pre-defined temperature for a second pre-defined time period, to obtain hard carbon. The hard carbon can be used for fabrication of an anode of an energy storage device.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR PREPARATION OF HARD CARBON

[0002] FIELD OF INVENTION

[0003] The present invention relates to preparation of a material for fabrication of electrodes of a cell, and specifically relates to preparation of hard carbon for synthesis of electrodes.

[0004] BACKGROUND

[0005] With rise in awareness for use of renewable energy sources and rise in number of portable electronic devices, high performance clean energy storage systems are in great demand. Energy storage systems, for example Sodium-ion batteries, Lithium-ion batteries, Sodium- ion capacitors, and Lithium-ion capacitors have drawn remarkable attention due to their high energy density and long cycling lifespan. Hard Carbon (HC), also known as non- graphitizable carbon, has become a leading candidate as anode material due to its well- reported reversible capacity of around 300 mA h / g on pyrolyzed glucose. For better performance of energy storage systems, HC is one of the most promising carbonaceous material used in electronic devices. HC can be used as a potential anode material due to its higher capacity, longer life, higher rate performance, and improved safety. Asymmetric hybrid super-capacitors and metal-ion capacitors seek use of HC-based anode material for obtaining higher energy than conventional capacitors. Sodium-ion batteries widely use HC as anode material due to large ionic radius of Na+of 1.06 A. The large ionic radius of Na+restricts usage of graphite as negative electrode. Further, HC suffers from some drawbacks, such as low packing density, large irreversible capacity, low-rate capability and large Capacitance-Voltage (CV) hysteresis.

[0006] To overcome the drawbacks of HC and improve the electrochemical performance through structural and physical modifications, different precursors of HC such as eggshell membrane, rice husk, glucose derived, template based, doped and co-doped HC have been utilised. In use of the above-mentioned precursors, HC structure reveals presence of graphite-like micro crystallites and amorphous regions with simultaneous presence of layer stacking and numerous active sites, such as edges, defects, and functional groups. Further, HC cannot be fully graphitized even at very high temperatures because of the high oxygen content and disordered structure of the precursors. Therefore, there is a need for a method of synthesis of HC from a HC precursor having high oxygen content, which overcomes the above-mentioned shortcomings of conventional methods of synthesis of HC. An alkali-based energy storage system, such as sodium storage mechanism utilising HC was tested and experimental evidence has demonstrated for study of characteristic of HC. The experimental evidence has demonstrated two voltage regions, for example sloping region (above 0.1 V) and plateau region (below 0.1 V). Sloping region and plateau region are ranges of voltage levels where Na-ions are inserted into graphene layers and Na filling into nanopores take place. HC precursor material and synthesis process parameters, particularly pyrolyzation temperature have crucial roles in determining the electrochemical properties of HC. Experimental observations demonstrate that HC pyrolyzed at less than 1000 °C have copious micropores and don’t display any plateau capacity. The plateau capacity is inversely proportional to the micropore volume and directly proportional to the graphitization degree, which in turn is dependent on the pyrolyzation temperature. Conventional electrodes developed using HC have displayed low charge storing capacity and an Initial Coulombic efficiency (ICE) due to large consumption of Na-ions in first irreversible cycle. To overcome such challenges, pyrolyzation at a high temperature greater than 1400 °C, is performed to enhance the graphitic interlayer spacing that in turn provides accommodation of the NaC.v compounds. However, it is difficult to maintain high temperature and impacts industrial applicability of HC in electrodes of energy storage devices.

[0007] Further, the plateau region involves intercalation reaction and provides slow rate capability. Therefore, HC with balanced sloping region (above 0.1 V) and plateau region (below 0.1 V) can be beneficial for high-rate Li-ion battery or Na-ion battery. Additionally, HC with less or minimal plateau region (below 0.1 V) can be beneficial for Li-ion capacitor or Na- ion capacitors.

[0008] Thus, there is a need for a cost-effective and industrially feasible method for improving electrochemical performance of energy storing systems.

[0009] OBJECTS OF THE INVENTION

[0010] A general objective of the present invention is to prepare Hard Carbon (HC) from an environment friendly material.

[0011] Another objective of the present invention is to fabricate an electrode using HC for use in an energy storage system. Another objective of the present invention to increase Initial Coulombic efficiency (ICE) of the electrode.

[0012] Another objective of the present invention is to develop a commercially feasible process for synthesis of the HC.

[0013] Still another objective of the present invention to prepare the HC that exhibits less loss and high retention of irreversible capacity for Li-ion battery or Na-ion battery.

[0014] Yet another objective of the present invention to prepare graphene coated HC for fabrication of high-rate Li-ion capacitor or Na-ion capacitor.

[0015] SUMMARY OF THE INVENTION

[0016] The summary is provided to introduce aspects related to a method for preparation of hard carbon. Other aspects and advantages of the invention will become apparent from the following description, taken in conjunction with the accompanying drawings, illustrating by way of example the principles of the invention.

[0017] In one embodiment, a method for preparation of hard carbon for an energy storage device may comprise burning dry bagasse in air to obtain a first carbonaceous material (Cl). The first carbonaceous material (Cl) may be chemically activated with the first carbonaceous material (Cl) with a Potassium Hydroxide (KOH) solution at a first pre-defined temperature for a first pre-defined time period, to obtain a chemically activated first carbonaceous material. The chemically activated first carbonaceous material may be washed chemically using Deionized (DI) water, to obtain a second carbonaceous material (C2). The second carbonaceous material (C2) may be heat treated in an inert atmosphere at a second predefined temperature for a second pre-defined time period, to obtain hard carbon.

[0018] In one aspect, dry bagasse may be obtained by heating raw bagasse, at a temperature ranging from 100 °C to 110 °C for a time-period ranging from 40 to 48 hours. In one aspect, ash mixed with the first carbonaceous material (Cl) during the burning of the dry bagasse may be removed from the first carbonaceous material (Cl) through centrifugation.

[0019] In one aspect, the KOH solution may have a molar concentration of KOH ranging from 5-6 M. The first carbonaceous material (Cl) may be chemically activated with the KOH solution at a molar ratio of 1 :4.

[0020] In one aspect, the first pre-defined temperature may range from 120°C to 130°C and the first pre-defined time period may range from 18-24 hours.

[0021] In one aspect, the second pre-defined temperature may be 1000°C, the second pre-defined time period may be 2 hours, and the inert atmosphere may be nitrogen (N2).

[0022] In one aspect, after performing the heat treatment, the second carbonaceous material (C2) may be kept at an intermediate temperature ranging from 320°C to 350°C for removal of one or more of moisture and organic volatiles from the second carbonaceous material (C2).

[0023] In one aspect, the hard carbon is utilized for fabrication of an anode of Li-ion battery or Na- ion battery. The anode is prepared using a water-based slurry including the hard carbon, a conductive additive, cellulose based binder, and butadiene-based binder additive. The water-based slurry may be coated on a current collector to obtain an electrode.

[0024] In one aspect, the hard carbon may be washed using vacuum pump distillation for maintaining pH of about 7.

[0025] In one aspect, the hard carbon may be kept in the oven at a temperature ranging from 100°C to 110°C overnight.

[0026] In one aspect the HC synthesized at 1000 °C was mixed with urea and Graphene Oxide (GO) dispersed in DI water to obtain a mixed dispersion. A ratio of GO to urea can be in the range of 1:3 to 1:5. The mixed dispersion is dried under vacuum and calcinated at a temperature range of 350-800 °C in an inert atmosphere to obtain reduced Graphene Oxide coated Hard Carbon ( rGHC). In another aspect, rGHC may be utilized to fabricate anode of Li-ion capacitor or Na-ion capacitor. The anode may be prepared using a water-based slurry including rGHC, a conductive additive, cellulose based binder, and butadiene-based binder additive. The water-based slurry may be coated on a current collector to obtain an electrode.

[0027] Other aspects and advantages of the invention will become apparent from the following description, taken in conjunction with the accompanying drawings, illustrating by way of example the principles of the invention.

[0028] BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings constitute a part of the description and are used to provide further understanding of the present invention. Such accompanying drawings illustrate the embodiments of the present invention which are used to describe the principles of the present invention. The embodiments are illustrated by way of example and not by way of limitation in the figures of the accompanying drawings in which like references indicate similar elements. It should be noted that references to “an” or “one” embodiment in this invention are not necessarily to the same embodiment, and they mean at least one. In the drawings:

[0030] Fig. 1 illustrates a method for preparation of hard carbon and reduced Graphene Oxide coated Hard Carbon (rGHC), in accordance with an embodiment of the present invention;

[0031] Fig. 2 illustrates a method for fabrication of an anode of Li-ion battery or Na-ion battery, in accordance with an embodiment of the present invention;

[0032] Fig. 3 illustrates a method for fabrication of an anode of Li-ion capacitor or Na-ion capacitor, in accordance with an embodiment of the present invention;

[0033] Fig. 4 illustrates a plot of impedance spectra of a hard carbon anode of a Li-ion battery, in accordance with an embodiment of the present invention;

[0034] Fig. 5 illustrates a plot of cyclic voltammetry of the hard carbon anode of the Li-ion battery, in accordance with an embodiment of the present invention; Fig. 6 illustrates voltage vs. specific capacity plots for various charge-discharge cycles of the hard carbon anode of the Li-ion battery, in accordance with an embodiment of the present invention;

[0035] Fig. 7 illustrates rate capability curves of the hard carbon anode at different current density of a Li-half cell, in accordance with an embodiment of the present invention;

[0036] Fig. 8 illustrates a plot of impedance spectra of a hard carbon anode of a Na-ion battery, in accordance with an embodiment of the present invention;

[0037] Fig. 9 illustrates a plot of cyclic voltammetry of the hard carbon anode of the Na-ion battery , in accordance with an embodiment of the present invention;

[0038] Fig. 10 illustrates voltage vs. specific capacity plots for various charge-discharge cycles the hard carbon anode of the Na-ion battery, in accordance with an embodiment of the present invention;

[0039] Fig. 11 illustrates rate capability curves of the hard carbon anode at different current density in a Na-half cell, in accordance with an embodiment of the present invention;

[0040] Fig. 12 illustrates voltage vs. specific capacity plots for rGHC anode of the Na-ion capacitor, in accordance with an embodiment of the present invention;

[0041] Fig. 13 (a) illustrates a comparative plot of impedance spectra of rGHC and hard carbon anode of Na-ion capacitor, in accordance with an embodiment of the present invention; and

[0042] Fig. 13 (b) illustrates an enlarged portion of the comparative plot of impedance spectra of rGHC and the hard carbon anode against Na / Na+, in accordance with an embodiment of the present invention.

[0043] DETAILED DESCRIPTION OF THE INVENTION

[0044] The detailed description set forth below in connection with the appended drawings is intended as a description of various embodiments of the present invention and is not intended to represent the only embodiments in which the present invention may be practiced. Each embodiment described in this disclosure is provided merely as an example or illustration of the present invention, and should not necessarily be construed as preferred or advantageous over other embodiments. The detailed description includes specific details for the purpose of providing a thorough understanding of the present invention. However, it will be apparent to those skilled in the art that the present invention may be practiced without these specific details.

[0045] Fig. 1 illustrates a method 100 for preparation of hard carbon reduced Graphene Oxide coated Hard Carbon (rGHC), in accordance with an embodiment of the present invention. The hard carbon may be prepared through treatment of bagasse i.e. biowaste of sugarcane. Bagasse is used as a source for preparation of the hard carbon as bagasse is a rich source of cellulose, hemicellulose, and lignin with an almost balance ratio of 1:1 of cellulose and hemicellulose / lignin. The method may comprise drying the bagasse in presence of sunlight. Thereafter, the bagasse may be cleaned in a mixture of water and ethanol. Upon cleaning, the bagasse may be oven dried to completely eliminate moisture and obtain dry bagasse. The dry bagasse may be burnt in air, at step 102. Upon burning the dry bagasse, a first carbonaceous material (Cl) with ash content may be obtained as a residue. The ash content may be removed from the first carbonaceous material (Cl) through centrifugation, at step 104. The centrifugation may be performed on the first carbonaceous material (Cl) for a prolonged time, using distilled water. The first carbonaceous material (Cl) may be washed with ethanol. The first carbonaceous material (Cl) may be oven dried for a pre-defined time period at a pre-defined temperature. The first carbonaceous material (Cl) may be chemically activated with a Potassium Hydroxide (KOH) solution at a first pre-defined temperature for a first pre-defined time period, to obtain a chemically activated first carbonaceous material, at step 106. In an implementation, the first pre-defined temperature may range from 120 °C to 130 °C and the first pre-defined time period may range from 18 to 24 hours.

[0046] The chemically activated first carbonaceous material may be washed using Deionized (DI) water, to obtain a second carbonaceous material (C2), at step 108. Post washing, the second carbonaceous material (C2) may be subjected to centrifugation. Subsequently, the second carbonaceous material (C2) may be pyrolyzed i.e. high temperature heat treatment of the second carbonaceous material (C2) may be performed in an inert atmosphere. The pyrolyzation may be performed at a second pre-defined temperature for a second pre- defined time period, for removal of any remove any moisture or organic volatiles. In an implementation, the second pre-defined temperature may range from 950 to 1050 °C, preferably 1000°C, and the second pre-defined time period may be 2 hours. After pyrolyzation of the second carbonaceous material (C2), hard carbon may be obtained, at step 110. The pyrolyzation performed at temperature 1000 °C may increase micropores in the hard carbon. The hard carbon may be treated with (5%) graphene oxide dispersed in water and urea to obtain a mixed dispersion, at step 112. The ratio of graphene oxide to urea may range from 1:3 to 1:5. The mixed dispersion may be dried under vacuum at a temperature ranging from 75 °C to 85 °C for 16 hours. Drying of the mixed dispersion may result in formation of dried powder. The dried powder may be calcinated at a temperature ranging from 350 °C to 800 °C for 2 hours, at step 114. As a result, edges of the hard carbon may be blocked by trapping the existing functional groups. Usage of urea for reduction of graphene oxide and source of nitrogen. The graphene coating may enhance the capacitive contribution in the material. Volume of the micropores may increase charge storing performance by increasing insertion-adsorption and intercalation mechanism for storage of sodium ions or lithium ions in hard carbon, in Sodium-ion battery and Lithium-ion battery.

[0047] In one test implementation, 200 gm of raw bagasse may be chopped into pieces of length ranging from 8 to 10 cm. Pieces of the raw bagasse may be sun dried for 40 to 50 hours approximately. The pieces of bagasse may be cleaned properly in water and ethanol. After cleaning, the pieces of bagasse may be oven dried at a temperature ranging from 100 to 110 °C for a time period ranging from 40 to 48 hours, for complete drying of the pieces of bagasse. The bagasse may be burnt in air to obtain a first carbonaceous material (Cl) with ash content. Ash may be removed from the first carbonaceous material (Cl) by washing using distilled water. Thereafter, the first carbonaceous material (Cl) may be subject to centrifugation. Subsequent to centrifugation, ethanol may be used for washing of the first carbonaceous material (Cl). Thereafter, the first carbonaceous material (Cl) may be kept in an oven for complete drying at a temperature ranging from 100 to 110 °C for a time period ranging from 18 to 24 hours . Upon drying, the first carbonaceous material (Cl) with a yield of 8-10% carbon may be obtained.

[0048] The first carbonaceous material (Cl) may be chemically activated with 6M KOH solution of 100 ml having a molar ratio of 1:4 of carbon to KOH solution. The KOH solution may be kept in an autoclave for occurrence of hydrothermal reaction for a time period of 18 to 24 hours at a temperature ranging from 120 to 130°C, to obtain the second carbonaceous material (C2). The second carbonaceous material (C2) may be washed repeatedly with DI water and may then be subjected to centrifugation followed by pyrolyzation. The pyrolyzation may be carried out at 1000 °C for 2 hours in pure N2 atmosphere. The second carbonaceous material (C2) may be kept at an intermediate temperature ranging from 320 to 350 °C for half an hour to remove any moisture or organic volatiles such as lattice entrapped K+, K2CO3, and residual by-products. A ramp rate may be maintained at 4.5-5 °C / minute, for pyrolyzation. After recovering the second carbonaceous material (C2), final washing may be done by a vacuum pump distillation to maintain a pH level of the second carbonaceous material (C2) at ~7. The neutral pH may be maintained after thorough and repeated washing using DI water and finally by reagent grade pure isopropanol. After final washing of the second carbonaceous material (C2), wet carbon may be dried in an oven at a temperature ranging from 100 to 110 °C overnight, to obtain hard carbon. The hard carbon, obtained through above-mentioned process, may contain 75 to 80% of the first carbonaceous material (Cl).

[0049] In one implementation, the hard carbon obtained from method 100 may be utilized for fabrication of an anode of an energy storage device. Fig. 2 illustrates a method 200 for fabrication of the anode of Li-ion battery or Na-ion battery, in accordance with an embodiment of the present invention. The method 200 may comprise preparation of a waterbased slurry, by mixing an anode active material in water, at step 202. The anode active material may be the hard carbon obtained through the above described step 110 of method 100. The anode active material may be mixed homogeneously with a conductive additive, a cellulose based binder, and a butadiene-based binder additive. In one implementation, the conductive additive may be carbon super P (C65), the cellulose based binder may be Na- carboxymethyl cellulose (CMC), and butadiene -based binder additive may be styrene butadiene rubber dispersion (SBR). In one implementation, C65, CMC, and SBR may be mixed in a weight ratio of 85-90:2-5:3-5:4-5.

[0050] At step 204, the water-based slurry may be coated on a current collector. The current collector may be made of a copper (Cu) foil in case of Li-ion battery and aluminium (Al) foil in case of Na-ion battery. In one implementation, the Cu / Al foil may be uniformly coated with the water-based slurry using a doctor blade. The water-based slurry may then be dried overnight at a temperature ranging from 100 to 110 degree Celsius, for complete elimination of water. As a result, the anode (negative electrode) may be obtained. The negative electrode may be calendered to obtain a uniform electrode.

[0051] In one implementation, the rGHC obtained from step 114 of method 100 may be utilized for fabrication of an anode of Li-ion capacitor or Na-ion capacitor. Fig. 3 illustrates a method 300 for fabrication of the anode of Li-ion capacitor or Na-ion capacitor, in accordance with an embodiment of the present invention. The method 300 may comprise preparation of a water-based slurry, by mixing an anode active material in water, at step 302. The anode active material may be rGHC obtained through the above -described step 114 of the method 100. The anode active material may be mixed homogeneously with a conductive additive, a cellulose based binder, and a butadiene-based binder additive. In one implementation, the conductive additive may be carbon super P (C65), the cellulose-based binder may be Na- CMC, and butadiene -based binder additive may be SBR. In one implementation, C65, CMC, and SBR may be mixed in a weight ratio of 85-90:2-5:3-5:4-5.

[0052] At step 304, the water-based slurry may be coated over a current collector. The current collector may be made of a copper (Cu) foil in case of Li-ion capacitor and aluminium foil (Al) in case of Na-ion capacitor. In one implementation, the Cu / Al foil may be uniformly coated with the water-based slurry using a doctor blade. The anode slurry may then be dried overnight at a temperature ranging from 100 to 110 degree Celsius, for complete elimination of water. As a result, the anode (negative electrode) may be obtained. The negative electrode may be calendered to obtain a uniform electrode.

[0053] In one implementation, the negative electrode made of hard carbon may be fabricated for a coin cell arrangement of CR 2032 type. The negative electrode for the coin cell may be obtained by electrode punching. The negative electrodes for the coin cell may be dried for 24 hours. In one arrangement, a coin cell of 16mm diameter may be developed. The coin cell may utilise Sodium (Na) metal as cathode. The coin cell may utilise sodium perchlorate- based salt dissolved in a mixture of propylene carbonate and fluoroethylene carbonate solvent as an electrolyte.

[0054] Electrochemical tests were conducted on the coin cell obtained though above-mentioned process, and Cyclic Voltammetry (CV) and Galvanostatic Charge-Discharge (GCD) profiles of the coin cell were obtained. Fig. 4 illustrates a plot of impedance spectra of a hard carbon anode of against Li / Li+, in accordance with an embodiment of the present invention. A Nyquist plot for a cell utilising hard carbon negative electrode and Li-half cell was drawn by Electrochemical Impedance Spectroscopy (EIS). EIS was performed to estimate the solution resistance of the hard carbon. It was observed that low value of solution resistance of around 200 is obtained for the hard carbonaceous material with Mitsubishi electrolyte (composition 1-1.2 M LiPFe+EC+EMC+DMC+FEC). The low value of solution resistance arose due to generation of porosity in the hard carbon electrode synthesized by KOH treatment.

[0055] Fig. 5 illustrates a plot of cyclic voltammetry of the hard carbon anode of the Li / Li+,, in accordance with an embodiment of the present invention. A plot of current density and potential (V) of Li / Li-i- was recorded for a cell utilising hard carbon negative electrode and Li-half cell. A first charging cycle (depicted by curve (i)) and a second charging cycle (depicted by curve (ii)) were plotted. It was observed that anodic reaction indicated at positive current density axis showed a broad peak at around 0.1 V and cathodic reaction indicated at negative current density axis depicted a very sharp peak at around 0.01 V. A prominent peak at around 0.7 V was observed in first charging cycle, as illustrated by curve

[0056] (i). The first charging cycle indicates proper formation of Solid Electrolyte Interphase (SEI) layer due to the KOH treatment. An overlapping of the first charging cycle and the second charging cycle reveals reversibility of the lithiation and de-lithiation process throughout, in the hard carbon anode.

[0057] Fig. 6 illustrates voltage vs. specific capacity plots for various charge-discharge cycles of the hard carbon anode of the high-rate Li-ion battery, in accordance with an embodiment of the present invention. Curve (i) depicts discharge cycle of the hard carbon anode. Curves

[0058] (ii) and (iii) depict a first discharging cycle of the anode and a second discharging cycle of the hard carbon anode, respectively. During charging of the high-rate Li-ion battery from about 0V to 2V, a reversible capacity of around 252 mA h / g was obtained at a potential of 2V, as illustrated by curve (i). During the first discharging cycle, there was irreversible reaction and SEI formation on surface of the hard carbon anode, with irreversible capacity of around 400 mA h / g. During second discharging cycle (iii), there was reversible reaction. It was observed that there was an irreversible loss of around 37% of capacity with a retention of around 63% of capacity after SEI formation of the Li-ion capacitor. It was further obtained that a sloping capacity between 1 V to OV of around 252 mA h / g and a plateau capacity at OV of around 400 mA h / g are obtained. The sloping capacity and the plateau capacity imply availability of both power density and energy density. During the second discharging cycle, there was reversible reaction, implying that there was mostly surface adsorption (sloping capacity) rather pore filling phenomena. After 80 cycles, the capacity of around 21.2% of the initial capacity was remained.

[0059] Fig. 7 illustrates rate capability curves of the hard carbon anode at different current densities of a Li-half cell, in accordance with an embodiment of the present invention. It was observed that the hard carbon anode exhibits a discharge capacity retention of around 57% after 20 cycles at 10 fold increase of current density of 0.1 A / g. It was further observed that the hard carbon anode exhibits a discharge capacity retention of 21% at 100-fold increase at current density of 1 A / g after 80 cycles.

[0060] Fig. 8 illustrates a plot of impedance spectra of a hard carbon anode of a Na-ion battery, in accordance with an embodiment of the present invention. A Nyquist plot for a cell utilising hard carbon negative electrode and Na-half cell was drawn by Electrochemical Impedance Spectroscopy (EIS). EIS was performed to estimate the solution resistance of the hard carbon. It was observed that value of solution resistance of around 600 is obtained for the hard carbonaceous material with the Mitsubishi electrolyte. The value of solution resistance arose due to generation of porosity in the hard carbon electrode synthesized by KOH treatment.

[0061] Fig. 9 illustrates a plot of cyclic voltammetry of the hard carbon anode of the Na-ion battery, in accordance with an embodiment of the present invention. A plot of current density and potential (V) of Na / Na+ was recorded for a cell utilising hard carbon negative electrode and Na-half cell. A first charging cycle (depicted by curve (i)) and a second charging cycle (depicted by curve (ii)) was plotted. It was observed that anodic reaction indicated at positive current density axis showed a broad peak at around 0.3 V, indicating prominent desodiation from graphitic layers. It was further observed that, cathodic reaction indicated at negative current density axis depicts a very sharp peak at around 0.1 V, indicating distinct sodiation. A prominent peak at around 0.8 V was observed in the first charging cycle, as illustrated by curve (i). The first charging cycle indicates proper formation of SEI layer due to the KOH treatment. An overlapping of the first charging cycle and the second charging cycle reveals reversibility of the sodiation and de-sodiation process throughout, in the hard carbon anode.

[0062] A charge-discharge profile of the half-cell at coin cell level was performed. It was observed that during the pre-sodiation process, the discharge capacity of 305 mA h / g is obtained. It was further observed that, the SEI layer is formed after the pre-sodiation process and the first chare-discharge cycle at a current density of 0.01 A / g exhibits a reversible capacity of around 230 mA h / g. Thus, the retention of the capacity of 75% was achieved after the pre- sodiation process. After 70 charge-discharge cycles, the capacity of 52 mA h / g was remained, which is around 22.4% of the initial capacity.

[0063] Fig. 10 illustrates voltage vs. specific capacity plots for various charge-discharge cycles of the hard carbon anode of the Na-ion battery, in accordance with an embodiment of the present invention. Curve (i) depicts a first charging cycle of the hard carbon anode. Curves (ii) and (iii) depicts a first discharging cycle and a second discharging cycle of the hard carbon anode, respectively. During charging of the Na-ion capacitor from about 0V to 2V after pre-sodiation, a reversible capacity of around 230 mA h / g was obtained at a potential of 2V, at current rate of 10 mA / g, as illustrated by curve (i). During the first discharging cycle, there was irreversible reaction and SEI formation on surface of the hard carbon anode, with irreversible discharge capacity of around 305 mA h / g. It was further obtained that a sloping capacity between 1.25 V to 0V of around 200 mA h / g, and a plateau capacity at 0V of around300 mA h / g are obtained.

[0064] The 1:1 portion of sloping capacity and the plateau capacity imply the balanced energy and power density. During the second discharging cycle, there was reversible reaction, implying that there was mostly surface adsorption (sloping capacity) rather pore filling phenomena. It was observed that there was a retention of around 75% capacity after SEI formation of the Na-ion capacitor. After 70 cycles, the capacity of around 52 mA h / g was obtained, which is around 22.4% of the initial capacity.

[0065] Fig. 11 illustrates rate capability curves of the hard carbon anode at different current densities of a Na-half cell, in accordance with an embodiment of the present invention. It was observed that the hard carbon anode exhibits a reversible discharge capacity retention of around 52% after 20 cycles at 10 fold increase of current density of 0.1 A / g. A discharge capacity retention of 22.4% at 60-fold increase was observed at current density of 0.6 A / g after 70 cycles.

[0066] Fig. 12 illustrates voltage vs. specific capacity plots for various charge-discharge cycles of the hard carbon anode of the Na-ion capacitor, in accordance with an embodiment of the present invention. Curve (i) and (iii) depict the charging cycles of the rGHC anode. Curves (ii) and (iv) depict the discharging cycles and a second discharging cycle of the hard carbon anode, respectively. It was observed that the plateau part is almost eliminated, and this electrode may be used for Na-ion capacitor.

[0067] Fig. 13 (a) illustrates a plot of impedance spectra of a hard carbon anode of a Na-ion capacitor, in accordance with an embodiment of the present invention. A Nyquist plot for a cell utilising hard carbon negative electrode and Na-half cell was drawn by Electrochemical Impedance Spectroscopy (EIS). The enlarged part of the Nyquist plot in the frequency range of 0-600 Hz is presented in Fig. 13(b). It was observed that the solution resistance of rGHC (illustrated by pattern (i)) is reduced as compared to the hard carbon (illustrated by pattern (ii)).

[0068] The above-described method enables preparation of hard carbon from biowaste sugarcane bagasse and allows use of the hard carbon as an anode in high power alkali -ion batteries. Usage of the hard carbon obtained from the biowaste sugarcane bagasse exhibits high electrochemical performance. The hard carbon is synthesized at an industrial viable pyrolyzation temperature of 1000 °C. It was observed that a reversible capacity with a significant low potential (< 0.01 V) capacity with possible low loss of the initial irreversible capacity is obtained. It was further observed that a balanced capacity from both the sloping and plateau region in first discharge cycle was obtained due to optimized chemical treatment, calcination temperature and time. Thus, a 230 mAh.g1reversible capacity at 10 mA.g1current density with a retention of around 75% capacity from the SEI formation was obtained in a Na-ion capacitor and a retention of around 63% capacity from the SEI formation was obtained in a Li-ion capacitor system.

[0069] The terms “or” and “and / or” as used herein are to be interpreted as inclusive or meaning any one or any combination. Therefore, “A, B or C” or “A, B and / or C” mean “any of the following: A; B; C; A and B; A and C; B and C; A, B and C.” An exception to this definition will occur only when a combination of elements, functions, steps or acts are in some way inherently mutually exclusive.

[0070] Any combination of the above features and functionalities may be used in accordance with one or more embodiments. In the foregoing specification, embodiments have been described with reference to numerous specific details that may vary from implementation to implementation. The specification and drawings are, accordingly, to be regarded in an illustrative rather than a restrictive sense. The sole and exclusive indicator of the scope of the invention, and what is intended by the applicants to be the scope of the invention, is the literal and equivalent scope of the set as claimed in claims that issue from this application, in the specific form in which such claims issue, including any subsequent correction.

[0071] It should also be noted that in some alternative implementations, the functions noted in the blocks described in methods (flow charts) described in the description may occur out of the order noted in the drawings. Two blocks shown in succession may in fact be executed substantially concurrently or the blocks may sometimes be executed in the reverse order, depending upon the functionality involved. Alternate implementations are included within the scope of the example embodiments in which functions may be executed out of order from that shown or discussed, including substantially concurrently or in reverse order, depending on the functionality involved.

Claims

CLAIMS:

1. A method for preparation of hard carbon for an energy storage device, the method comprising: burning dry bagasse in air to obtain a first carbonaceous material (Cl); chemically activating the first carbonaceous material (Cl) with a Potassium Hydroxide (KOH) solution at a first pre-defined temperature for a first pre-defined time period, to obtain a chemically activated first carbonaceous material; washing the chemically activated first carbonaceous material using Deionized (DI) water, to obtain a second carbonaceous material (C2); and performing heat treatment of the second carbonaceous material (C2) in an inert atmosphere at a second pre-defined temperature for a second pre-defined time, to obtain hard carbon.

2. The method as claimed in claim 1 , wherein the dry bagasse is obtained by heating raw bagasse, at a temperature ranging from 100 °C to 110 °C for a time-period ranging from 40 to 48 hours.

3. The method as claimed in claim 1, wherein ash mixed with the first carbonaceous material (Cl), during the burning of the dry bagasse, is removed from the first carbonaceous material (Cl) through centrifugation.

4. The method as claimed in claim 1, wherein the KOH solution has a molar concentration of KOH ranging from 5-6 M, and wherein the first carbonaceous material (Cl) is chemically activated with the KOH solution at a molar ratio of 1:4.

5. The method as claimed in claim 1, wherein the first pre-defined temperature ranges from 120°C to 130°C and the first pre-defined time period ranges from 18-24 hours.

6. The method as claimed in claim 1, wherein the second pre -defined temperature is 1000°C, the second pre-defined time period is 2 hours, and the inert atmosphere is nitrogen (N2).

7. The method as claimed in claim 1, wherein, after performing the heat treatment, the second carbonaceous material (C2) is kept at an intermediate temperature ranging from 320°C to 350°C for removal of one or more of moisture and organic volatiles from the second carbonaceous material (C2).

8. The method as claimed in claim 1, wherein the hard carbon is utilized for fabrication of an anode of Li-ion battery or Na-ion battery by: preparing a water-based slurry using the hard carbon, a conductive additive, cellulose based binder, and butadiene-based binder additive; and coating the water-based slurry on a current collector to obtain an electrode.

9. The method as claimed in claim 1, wherein the hard carbon is washed using vacuum pump distillation for maintaining pH of about 7.

10. The method as claimed in claim 9, wherein the hard carbon is kept in the oven at a temperature ranging from 100°C to 110°C overnight.

11. The method as claimed in claim 10, wherein the hard carbon is mixed with Graphene Oxide (GO) dispersed in DI water and urea to obtain a mixed dispersion, and wherein the mixed dispersion is dried in vacuum and calcinated at a temperature ranging from 350 °C to 800 °C in an inert atmosphere to obtain reduced Graphene Oxide coated Hard Carbon (rGHC).

12. The method as claimed in claim 11, wherein a ratio of GO to urea ranges from 1:3 to13. The method as claimed in claim 11, wherein rGHC is utilized for fabrication of an anode of a Li-ion capacitor or a Na-ion capacitor: preparing a water-based slurry using rGHC, a conductive additive, cellulose based binder, and butadiene-based binder additive; and coating the water-based slurry on a current collector to obtain an electrode.

Citation Information

Patent Citations

  • Preparation method and application of fuel cell anode catalyst containing activated graphite

    CN115986145A