Semiconductor device and method for manufacturing semiconductor device
The introduction of a titanium-containing capping layer between the noble metal layer and the dielectric layer in semiconductor devices prevents oxygen diffusion, addressing interface defects and maintaining dielectric properties, thus improving the semiconductor device's performance by ensuring a uniform dielectric constant and enhanced adhesion.
Patent Information
- Application Number
- PCT/KR2024/006251
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-14
AI Technical Summary
The diffusion of oxygen from the dielectric layer into the lower electrode in semiconductor devices leads to interface defects, reducing the dielectric constant and adhesion between the dielectric layer and the electrode, thereby deteriorating the capacitor's characteristics.
A capping layer containing titanium, such as a titanium metal, nitride, oxide, or oxynitride layer, is formed between the noble metal-containing layer and the dielectric layer to prevent oxygen diffusion, using techniques like spraying titanium precursors and exposing them to hydrogen plasma to enhance adhesion and maintain dielectric properties.
This approach effectively suppresses defects at the interface, maintains a uniform dielectric constant, and improves the bonding strength of the dielectric layer, enhancing the overall performance of the semiconductor device.
Smart Images

Figure KR2024006251_14112024_PF_FP_ABST
Abstract
Description
Semiconductor devices and methods for manufacturing semiconductor devices
[0001] The present invention relates to a semiconductor device and a method for manufacturing a semiconductor device, and more particularly, to a semiconductor device capable of improving characteristics and a method for manufacturing a semiconductor device.
[0002] The capacitor includes a lower electrode formed on a substrate, a dielectric layer formed on the lower electrode, and an upper electrode formed on the dielectric layer. The lower electrode is formed of ruthenium (Ru), and the dielectric layer is formed by depositing ZrO2 or HfO2, an oxide having a high dielectric constant, on the lower electrode.
[0003] However, when a dielectric layer is formed on the lower electrode, the oxygen contained in the dielectric layer diffuses or migrates toward the lower electrode. This causes an interface defect as the oxygen concentration at the interface between the dielectric layer and the lower electrode increases. As a result, the dielectric properties of the dielectric layer deteriorate. That is, the dielectric constant of the dielectric layer decreases or becomes non-uniform. In addition, the adhesive strength between the dielectric layer and the lower electrode deteriorates. And due to this deterioration in the dielectric properties and adhesive strength of the dielectric layer, the characteristics of the capacitor deteriorate.
[0004] (Prior art literature)
[0005] (Patent Document 1) Korean Registered Patent KR 10-0881728
[0006] The present invention provides a semiconductor device and a method for manufacturing a semiconductor device that can suppress or prevent the occurrence of defects between an electrode and a dielectric layer.
[0007] The present invention provides a semiconductor device and a method for manufacturing the semiconductor device that can improve the dielectric properties of a dielectric layer and improve the adhesive strength between an electrode and a dielectric layer.
[0008] A semiconductor device according to an embodiment of the present invention may include an electrode formed on a substrate and including a noble metal-containing layer; a dielectric layer formed on one surface of the noble metal-containing layer; and a capping layer formed between the noble metal-containing layer and the dielectric layer and containing titanium (Ti).
[0009] The capping layer may be formed of at least one of a titanium metal layer, a titanium oxide layer, a titanium nitride layer, and a titanium oxynitride layer.
[0010] The thickness of the capping layer may be 10Å or less.
[0011] The above precious metal-containing layer may contain at least one of ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Y), and molybdenum (Mo).
[0012] The above precious metal-containing layer may be a precious metal layer or precious metal oxide layer containing at least one of ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Y), and molybdenum (Mo).
[0013] The above precious metal-containing layer includes a first precious metal-containing layer and a second precious metal-containing layer formed on the first precious metal-containing layer, and one of the first and second precious metal-containing layers may be a precious metal layer, and the other may be a precious metal oxide layer.
[0014] The above electrode may include a titanium nitride layer formed on the other surface of the precious metal-containing layer.
[0015]
[0016] A method for manufacturing a semiconductor device according to an embodiment of the present invention may include a step of forming an electrode including a precious metal-containing layer by spraying a precursor containing a precious metal onto a substrate; a step of forming a capping layer on the electrode by spraying a precursor containing titanium (Ti) toward the electrode; and a step of forming a dielectric layer on the capping layer.
[0017] The step of forming the capping layer may include a step of exposing a titanium-containing layer formed by spraying a precursor containing titanium (Ti) to hydrogen plasma.
[0018] It may include a step of injecting a reactant gas containing at least one of oxygen and nitrogen toward a titanium-containing layer formed by injecting a precursor containing the titanium (Ti).
[0019] The step of injecting the above reactant gas may include a step of generating plasma using the above reactant gas.
[0020] In the step of spraying a precursor containing the above precious metal, a precursor containing at least one of ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Y), and molybdenum (Mo) can be sprayed.
[0021] The step of forming the electrode may include a step of generating hydrogen plasma after spraying a precursor containing the precious metal.
[0022] The step of forming the electrode may include a step of generating oxygen plasma after spraying a precursor containing the precious metal.
[0023] The step of forming the electrode may include a step of forming a titanium nitride layer on the substrate before forming a precious metal-containing layer on the substrate.
[0024] According to embodiments of the present invention, the occurrence of defects at the interface between an electrode and a dielectric layer can be suppressed or prevented. As a result, a decrease in the dielectric constant of the dielectric layer can be suppressed or prevented, and the dielectric constant of the dielectric layer can be made uniform. In addition, the bonding strength of the dielectric layer can be improved.
[0025] FIG. 1 is a conceptual diagram illustrating a semiconductor device according to a first embodiment of the present invention.
[0026] Figures 2 (a) to (d) are process diagrams sequentially showing a method for manufacturing a semiconductor device according to the first embodiment of the present invention.
[0027] FIG. 3 is a conceptual diagram illustrating a semiconductor device according to a modified example of the first embodiment of the present invention.
[0028] Figure 4 is a conceptual diagram illustrating a semiconductor device according to a second embodiment of the present invention.
[0029] Hereinafter, embodiments of the present invention will be described in more detail with reference to the attached drawings. However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms. These embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention. To illustrate the embodiments of the present invention, the drawings may be exaggerated, and like reference numerals in the drawings represent like components.
[0030]
[0031] FIG. 1 is a conceptual diagram illustrating a semiconductor device according to a first embodiment of the present invention.
[0032] A semiconductor device may be a device including an electrode containing a precious metal and a dielectric layer formed on the electrode. More specifically, the semiconductor device may be a capacitor.
[0033] Referring to FIG. 1, the capacitor may include a substrate (S), a lower electrode (100) formed on the substrate (S), a dielectric layer (300) formed on the lower electrode (100), a capping layer (200) formed between the lower electrode (100) and the dielectric layer (300), and an upper electrode (400) formed on the dielectric layer (300).
[0034] The substrate (S) may be a wafer or glass. If the substrate (S) is a wafer, the substrate (S) may be any one of a Si wafer, a GaAs wafer, and a SiGe wafer. Of course, various types of wafers may be used as the substrate (S) in addition to the types of wafers described above.
[0035] The dielectric layer (300) is formed on the lower electrode (100) and may be formed of an oxide layer having a high dielectric constant. As a more specific example, the dielectric layer (300) may be formed of at least one of ZrO2, HfO2, Al2O3, TiO2, and TaO2.
[0036] At least one of the lower electrode (100) and the upper electrode (400) may be formed to contain a precious metal. In other words, at least one of the lower electrode (100) and the upper electrode (400) may be formed to contain a precious metal layer. As a more specific example, at least one of the lower electrode (100) and the upper electrode (400) may be formed to contain ruthenium (Ru), which is a precious metal. That is, at least one of the lower electrode (100) and the upper electrode (400) may be formed to contain a ruthenium-containing layer.
[0037] Of course, the precious metal contained in at least one of the lower electrode (100) and the upper electrode (400) is not limited to the above-described ruthenium (Ru), and various precious metal materials may be applied. That is, at least one of the lower electrode (100) and the upper electrode (400) may be formed to contain at least one of ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Y), and molybdenum (Mo).
[0038] Hereinafter, among the lower electrode (100) and the upper electrode (400), an example in which the lower electrode (100) is formed to contain a precious metal will be described. In addition, ruthenium (Ru) will be described as an example of the precious metal.
[0039] The dielectric layer (300) is formed as an oxide layer as described above, and may be formed of, for example, any one of ZrO2, HfO2, Al2O3, TiO2, and TaO2. In addition, the dielectric layer (300) is formed by being deposited on a lower electrode (100) containing a noble metal, for example, ruthenium. However, when the dielectric layer (300) is formed on the lower electrode (100), oxygen contained in the dielectric layer (300) may diffuse or move toward the lower electrode (100). As a result, an interface defect may occur as the oxygen concentration at the interface between the dielectric layer (300) and the lower electrode (100) increases. Accordingly, the dielectric properties of the dielectric layer (300) deteriorate. That is, there is a problem that the dielectric constant of the dielectric layer (300) decreases or the dielectric constant becomes non-uniform in the thickness direction of the dielectric layer (300). Additionally, the adhesive strength between the dielectric layer (300) and the lower electrode (100) may be reduced. In addition, the characteristics of the capacitor may be reduced due to the reduction in the dielectric properties and adhesive strength of the dielectric layer (300).
[0040] Therefore, in the embodiment, in order to suppress or prevent the dielectric properties of the dielectric layer (300) from deteriorating or the adhesive strength of the dielectric layer (300) from decreasing, a capping layer (200) containing titanium (Ti) is formed between the lower electrode (100) containing a precious metal and the dielectric layer (300). The capping layer (200) may be formed of at least one of a titanium (Ti) metal layer, a titanium nitride (TiN) layer, a titanium oxide (TiO) layer, and a titanium oxynitride (TiON) layer.
[0041]
[0042] Figures 2 (a) to (d) are process diagrams sequentially showing a method for manufacturing a semiconductor device according to the first embodiment of the present invention.
[0043] Hereinafter, a method for manufacturing a semiconductor device according to a first embodiment of the present invention will be described with reference to (a) to (d) of FIG. 2.
[0044]
[0045] Referring to (a) to (d) of FIG. 2, the manufacturing steps of a semiconductor device may include a step (a) of forming a lower electrode (100) on a substrate (S), a step (b) of forming a capping layer (200) on the lower electrode (100), a step (c) of forming a dielectric layer (300) on the capping layer (200), and a step (d) of forming an upper electrode (400) on the dielectric layer (300).
[0046] The lower electrode (100) may be formed of a layer containing a precious metal. For a more specific example, the lower electrode (100) may be formed of a layer containing the precious metal ruthenium (Ru) (ruthenium-containing layer). Here, the ruthenium-containing layer may be a ruthenium (Ru) metal layer or a ruthenium oxide (RuO2) layer. In other words, the lower electrode (100) may include a ruthenium metal layer or a ruthenium oxide layer.
[0047] Hereinafter, an example in which the lower electrode (100) is formed as a ruthenium-containing layer and the ruthenium-containing layer is a ruthenium metal layer will be described. That is, in explaining a method for manufacturing a semiconductor device, an example in which the lower electrode (100) is formed as a ruthenium metal layer will be described. In addition, for convenience of explanation, the lower electrode (100) formed as a ruthenium-containing layer will be simply referred to as a 'ruthenium-containing layer'. In addition, in explaining the ruthenium-containing layer, it will be described by referring to it as '100', which is the same drawing reference number as the lower electrode (100).
[0048] The step of forming a ruthenium-containing layer (100) (step of forming a lower electrode) may include a step of depositing a ruthenium-containing layer (100) by spraying a ruthenium-containing precursor toward a substrate (S) (ruthenium-containing precursor spraying step), and a step of exposing the ruthenium-containing layer (100) to hydrogen plasma (hydrogen plasma exposure step).
[0049] In addition, the 'ruthenium-containing precursor injection step - hydrogen plasma exposure step' is one cycle (hereinafter, ruthenium-containing layer formation cycle (CY) Ru )) can be done. That is, the step of forming the ruthenium-containing layer (100) is a ruthenium-containing layer forming cycle (CY Ru ) and the ruthenium-containing layer formation cycle (CY) Ru ) may include a step of spraying a ruthenium-containing precursor and a step of exposing the ruthenium-containing layer (100) to hydrogen plasma.
[0050] In addition, the step of forming a ruthenium-containing layer (100) may further include at least one of a step of injecting a purge gas between the ruthenium-containing precursor injection step and the hydrogen plasma exposure step (first purge step) and a step of injecting a purge gas after the hydrogen plasma exposure step (second purge step). Here, argon (Ar) gas may be used as the purge gas. In this case, 'ruthenium-containing precursor injection step - first purge step - hydrogen plasma exposure step - second purge step' is referred to as one cycle (ruthenium-containing layer forming cycle (CY) Ru )) can be done. That is, the step of forming the ruthenium-containing layer (100) is a ruthenium-containing layer forming cycle (CY Ru ) and the ruthenium-containing layer formation cycle (CY) Ru ) may include a ruthenium-containing precursor injection step, a first purge step, a hydrogen plasma exposure step, and a second purge step. At this time, the ruthenium-containing layer formation cycle (CY Ru ) at least one of the first and second fuzzy steps may be omitted.
[0051] And, the ruthenium-containing layer formation cycle (CY) as described above Ru ) can be performed multiple times. That is, the step of forming a ruthenium-containing layer (100) may be performed multiple times by forming a ruthenium-containing layer by forming multiple cycles (CY). Ru ) may be included.
[0052] Below is the ruthenium-containing layer formation cycle (CY Ru) will be described in more detail. In the step of spraying a ruthenium-containing precursor, a precursor containing or including ruthenium is sprayed toward the substrate (S). That is, the ruthenium-containing precursor is sprayed into the interior of the chamber in which the substrate (S) is loaded. Here, as the precursor raw material containing ruthenium (Ru), for example, ethylcyclopentadienyl ruthenium ((EtCp)2Ru)(Bis(ethylcyclopentadienyl)ruthenium) can be used. Of course, the precursor raw material containing ruthenium (Ru) is not limited to the above-described materials, and various precursor raw materials containing ruthenium (Ru) can be used.
[0053] When a precursor containing ruthenium (Ru) is sprayed toward a substrate (S), the precursor is deposited or adsorbed on one surface of the substrate (S) to deposit a layer containing ruthenium. That is, a ruthenium metal layer is deposited.
[0054] When the precursor injection step is completed, a purge gas is injected into the chamber where the substrate (S) is loaded to perform a primary purge. At this time, the purge gas can be, for example, argon (Ar) gas.
[0055] When the first purge is completed, the ruthenium-containing layer (100) is exposed to hydrogen plasma. That is, hydrogen plasma is generated inside the chamber in which the substrate (S) on which the ruthenium-containing layer (100) is formed is loaded, thereby exposing the ruthenium-containing layer (100) to the hydrogen plasma. To this end, RF (Radio Frequency) power is applied to at least one of the susceptor on which the substrate (S) is mounted inside the chamber and the injection unit that injects gas into the inside of the chamber. In addition, a gas containing hydrogen (H2) is used as the gas for generating the plasma. More specifically, the gas for generating the plasma may be hydrogen (H2) gas. As described above, when RF power is applied and the gas containing hydrogen (H2) is injected, a plasma containing hydrogen (H2), i.e., hydrogen plasma, can be generated inside the chamber. Accordingly, the substrate (S) on which the ruthenium-containing layer (100) is formed is exposed to the hydrogen plasma.
[0056] The hydrogen plasma exposure step is a step of generating hydrogen plasma as described above to expose the ruthenium-containing layer (100) to hydrogen plasma. Accordingly, the hydrogen plasma exposure step may be referred to as a hydrogen plasma generation step.
[0057] The ruthenium-containing precursor may contain impurities. For example, the ruthenium-containing precursor may contain, in addition to ruthenium (Ru), at least one ligand selected from carbon (C) and oxygen (O). Accordingly, the ruthenium-containing layer (100) deposited by spraying the ruthenium-containing precursor may contain or include at least one ligand selected from carbon (C) and oxygen (O), and such ligand is an impurity that increases the resistivity of the ruthenium-containing layer (100). Therefore, it is desirable to remove impurities included in the ruthenium-containing layer (100).
[0058] Therefore, in the embodiment, after a ruthenium-containing precursor is sprayed to deposit a ruthenium-containing layer (100), the ruthenium-containing layer (100) is exposed to hydrogen plasma to remove impurities. When the ruthenium-containing layer (100) is exposed to hydrogen plasma, impurities included in the ruthenium-containing layer (100) react with hydrogen. Accordingly, at least one impurity among C (carbon) and O (oxygen) included in the ruthenium-containing layer (100) reacts with hydrogen to become a gas and escapes from the ruthenium-containing layer (100). Accordingly, the content of at least one impurity among C (carbon) and O (oxygen) included in the ruthenium-containing layer (100) decreases. As a result, the resistivity of the ruthenium-containing layer (100) can be reduced.
[0059] Afterwards, a second purge is performed by injecting purge gas into the chamber in which the substrate (S) is loaded. At this time, the purge gas can be the same gas as the gas used in the first purge, and for example, argon (Ar) gas can be used.
[0060] A process including a ruthenium-containing precursor injection step, a first purge step, a hydrogen plasma exposure step, and a second purge step as described above is referred to as one ruthenium-containing layer formation cycle (CY). Ru ) can be used. That is, a cycle (CY) for forming a ruthenium-containing layer (100) Ru ) may include 'ruthenium-containing precursor injection step - first purge step - hydrogen plasma exposure step - second purge step'. And, the ruthenium-containing layer formation cycle (CY Ru ) can be performed multiple times in succession to form a ruthenium-containing layer (100) having a target thickness as shown in (a) of Fig. 2. That is, a ruthenium metal layer is formed on the substrate (S). In other words, a lower electrode (100) made of a ruthenium metal layer is formed on the substrate (S).
[0061] Next, a capping layer (200) is formed on the ruthenium-containing layer (100). The capping layer (200) may be formed as a layer containing titanium (Ti), and the titanium-containing layer may be formed of any one of a titanium metal layer, a titanium oxide (TiO) layer, a titanium nitride (TiN) layer, and a titanium oxynitride (TiON). Hereinafter, an example in which the capping layer (200) is formed as a titanium metal layer will be described.
[0062] The step of forming the capping layer (200) may include a step of depositing the capping layer (200) by spraying a titanium-containing precursor toward the ruthenium-containing layer (100) (titanium-containing precursor spraying step), and a step of exposing the capping layer (200) to hydrogen plasma (hydrogen plasma exposure step).
[0063]
[0064] In addition, the 'titanium-containing precursor injection step - hydrogen plasma exposure step' is one cycle (hereinafter referred to as a capping layer formation cycle (CY) C )) can be done. That is, the step of forming the capping layer (200) is a capping layer forming cycle (CY C ) and includes the capping layer formation cycle (CY C ) may include a step of spraying a titanium-containing precursor and a step of exposing the capping layer (200) to hydrogen plasma.
[0065] And, the step of forming a capping layer (200) may further include at least one of a step of injecting a purge gas between the titanium-containing precursor injection step and the hydrogen plasma exposure step (first purge step) and a step of injecting a purge gas after the hydrogen plasma exposure step (second purge step). In this case, 'titanium-containing precursor injection step - first purge step - hydrogen plasma exposure step - second purge step' is referred to as one cycle (capping layer formation cycle (CY) C )) can be done. That is, the step of forming the capping layer (200) is a capping layer forming cycle (CYC ) and includes the capping layer formation cycle (CY C ) may include a titanium-containing precursor injection step, a first purge step, a hydrogen plasma exposure step, and a second purge step. At this time, a capping layer formation cycle (CY C ) at least one of the first and second fuzzy steps may be omitted.
[0066] And, the capping layer formation cycle (CY) as described above C ) can be performed multiple times. That is, the step of forming the capping layer (200) may be performed multiple times by performing multiple capping layer forming cycles (CY C ) may be included.
[0067] Below is the capping layer formation cycle (CY C ) will be described in more detail. In the step of spraying a titanium-containing precursor, a precursor containing or including titanium (Ti) is sprayed toward the substrate (S). That is, the precursor containing titanium is sprayed into the interior of the chamber in which the substrate (S) is loaded. Here, the precursor raw material containing titanium is, for example, TDMAT (Tetrakis(dimethylamino)titanium: C8H 24 N4Ti) can be used. Of course, the precursor raw material containing titanium is not limited to the materials described above, and various precursor raw materials containing titanium can be used.
[0068] When a precursor containing titanium is sprayed toward a substrate (S), the precursor is deposited or adsorbed on one surface of the substrate (S) as shown in (b) of Fig. 2, thereby depositing a layer containing titanium. That is, a titanium metal layer is deposited. In other words, a capping layer (200) made of a titanium metal layer is formed.
[0069] After the step of spraying the titanium-containing precursor is completed, the capping layer (200) is exposed to hydrogen plasma. The hydrogen plasma is used to form a ruthenium-containing layer in a cycle (CY Ru) is generated in the same way as described in , so its description is omitted.
[0070] The titanium-containing precursor may contain impurities, and the impurities may be, for example, ligands of either carbon (C) or oxygen (O). Accordingly, the capping layer (200) formed by spraying the titanium-containing precursor may contain or be comprised of impurities, and these impurities may deteriorate the performance of the semiconductor device. Therefore, it is desirable to remove impurities contained in the capping layer (200).
[0071] Accordingly, in the embodiment, after depositing a capping layer (200) by spraying a titanium-containing precursor, the capping layer (200) is exposed to hydrogen plasma to remove impurities. When the capping layer (200) is exposed to hydrogen plasma, the impurities contained in the capping layer (200) react with hydrogen. For example, at least one impurity among C (carbon) and O (oxygen) contained in the capping layer (200) reacts with hydrogen to become a gas and escape from the capping layer (200). Accordingly, the content of impurities in the capping layer (200) is reduced.
[0072] Afterwards, a second purge is performed by spraying purge gas, for example, argon (Ar) gas, into the chamber in which the substrate (S) is loaded.
[0073] A process including a titanium-containing precursor injection step, a first purge step, a hydrogen plasma exposure step, and a second purge step as described above is referred to as one capping layer formation cycle (CY). C ) can be used. That is, the cycle (CY) for forming the capping layer (200) C ) may include 'titanium-containing precursor injection step - first purge step - hydrogen plasma exposure step - second purge step'. And, the capping layer formation cycle (CY C) can be performed multiple times in succession to form a capping layer (200) having a target thickness as shown in (b) of Fig. 2. At this time, it is preferable that the capping layer (200) be formed to a thickness of 10 Å or less, more preferably 1 Å or more and 10 Å or less.
[0074] Meanwhile, if the thickness of the capping layer (200) exceeds 10Å, there is a problem that the overall thickness of the capacitor becomes thick. That is, it is desirable for a capacitor to be thin but have a high capacity, but if the thickness of the capacitor exceeds 10Å, there is a problem that the overall thickness of the capacitor becomes thick. On the other hand, if the thickness of the capping layer (200) is less than 1Å, it may not be possible to suppress or prevent oxygen contained in the dielectric layer (300) using the capping layer (200) from moving toward the capping layer (200) or the lower electrode (100). As a result, the permittivity of the dielectric layer (300) may decrease, or the permittivity of the dielectric layer (300) may not be uniform in the thickness direction.
[0075] Thereafter, a dielectric layer (300) is formed on the capping layer (200) as shown in (c) of FIG. 2. As a more specific example, zirconia (ZrO2) is deposited on the capping layer (200) to form the dielectric layer (300). When forming the dielectric layer (300), it is formed on the capping layer (200) as described above. That is, before forming the dielectric layer (300), a capping layer (200) containing titanium is formed on the ruthenium-containing layer (100), and the dielectric layer (300) is formed on the capping layer (200). As a result, it is possible to suppress or prevent oxygen contained in the dielectric layer (300) from diffusing or moving toward the capping layer (200) or the ruthenium-containing layer (100). In other words, the capping layer (200) containing titanium can suppress or prevent oxygen contained in the dielectric layer (300) from diffusing or moving toward the capping layer (200) or the ruthenium-containing layer (100).
[0076] Accordingly, it is possible to suppress or prevent the occurrence of defects due to oxygen at the interface between the dielectric layer (300) and the lower electrode (100). Accordingly, it is possible to suppress or prevent the dielectric constant of the dielectric layer (300) from decreasing, and it is possible to suppress or prevent the dielectric constant of the dielectric layer (300) from becoming non-uniform in the thickness direction. That is, the dielectric layer (300) can have a high dielectric constant and a uniform dielectric constant in the thickness direction. In addition, the adhesive strength between the dielectric layer (300) and the lower electrode (100) can be improved. Accordingly, it is possible to suppress or prevent the deterioration of the characteristics of the capacitor due to the deterioration of the dielectric characteristics and adhesive strength of the dielectric layer (300). That is, in a capacitor including a lower electrode (100) formed using a noble metal, the characteristics of the capacitor can be improved.
[0077] Next, as shown in (d) of Fig. 2, an upper electrode (400) is formed on the dielectric layer (300). At this time, the upper electrode (400) may be formed of various conductive materials. In addition, the upper electrode (400) may be formed to contain a noble metal, similar to the lower electrode (100), and may be formed to contain, for example, ruthenium. In this way, when the upper electrode (400) is formed to contain a noble metal, a capping layer (200) containing titanium may be formed between the upper electrode (400) and the dielectric layer (300).
[0078]
[0079] In the first embodiment described above, it was described that the ruthenium-containing layer (100) was formed as a ruthenium metal layer. However, the present invention is not limited thereto, and the ruthenium-containing layer (100) may be formed as a ruthenium oxide (RuO2) layer.
[0080] Hereinafter, a method for forming a ruthenium oxide (RuO2) layer will be described. The method for forming a ruthenium oxide (RuO2) layer is similar to the method for forming a ruthenium metal layer, except that oxygen plasma is generated. Therefore, in describing the method for forming a ruthenium oxide (RuO2) layer, any overlapping content with the previously described method for forming a ruthenium metal layer will be omitted or briefly explained.
[0081] The step of forming a ruthenium oxide layer (step of forming a lower electrode) may include a step of depositing a ruthenium metal layer by spraying a ruthenium-containing precursor toward the substrate (S) (ruthenium-containing precursor spraying step), and a step of exposing the ruthenium metal layer to oxygen plasma to oxidize the ruthenium metal layer (oxygen plasma exposure step). In addition, the 'ruthenium-containing precursor spraying step - oxygen plasma exposure step' is referred to as one cycle (hereinafter, ruthenium-containing layer forming cycle (CY) Ru )) can be used.
[0082] And, the step of forming a ruthenium oxide layer may further include at least one of a step of injecting a purge gas between the ruthenium-containing precursor injection step and the oxygen plasma exposure step (first purge step) and a step of injecting a purge gas after the oxygen plasma exposure step (second purge step). In this case, 'ruthenium-containing precursor injection step - first purge step - oxygen plasma exposure step - second purge step' is referred to as one cycle (ruthenium-containing layer formation cycle (CY) Ru )) can be used. At this time, the ruthenium-containing layer formation cycle (CY) Ru ) at least one of the first and second fuzzy steps may be omitted.
[0083] And, the ruthenium-containing layer formation cycle (CY) as described above Ru ) can be performed multiple times. That is, the step of forming a ruthenium-containing layer (100) may be performed multiple times by forming a ruthenium-containing layer by forming multiple cycles (CY).Ru ) may be included.
[0084]
[0085] In the first embodiment described above, it has been described that the capping layer (200) is formed of a titanium metal layer. However, the present invention is not limited thereto, and the capping layer (200) may be formed of at least one of a titanium oxide layer, a titanium nitride layer, and a titanium oxynitride layer.
[0086] Hereinafter, a method for forming a capping layer (200) made of a titanium oxide layer will be described. The step of forming the titanium oxide layer (the step of forming the lower electrode (100)) may include a step of depositing a titanium metal layer by spraying a titanium-containing precursor toward the substrate (S) (titanium-containing precursor spraying step) and a step of forming a titanium oxide layer by spraying a reactant gas containing oxygen toward the titanium metal layer (reactant gas spraying step). In addition, the 'titanium-containing precursor spraying step - reactant gas spraying step' is referred to as one cycle (hereinafter, a capping layer forming cycle (CY) C )) can be used. In addition, in the step of injecting a reactant gas containing oxygen, it may be more preferable to generate plasma (i.e., oxygen plasma) using oxygen.
[0087] And, the step of forming a titanium oxide layer may further include at least one of a step of injecting a purge gas between the titanium-containing precursor injection step and the reactant gas injection step (first purge step) and a step of injecting a purge gas after the reactant gas injection step (second purge step). In this case, 'titanium-containing precursor injection step - first purge step - reactant gas injection step - second purge step' is referred to as one cycle (capping layer formation cycle (CY) C )) can be used. At this time, the capping layer formation cycle (CY) C ) at least one of the first and second fuzzy steps may be omitted.
[0088] In addition, the capping layer formation cycle (CY) as described above C ) can be performed multiple times. That is, the step of forming the capping layer (200) may be performed multiple times by performing multiple capping layer forming cycles (CY C ) may be included.
[0089]
[0090] As described above, the capping layer (200) can be formed as a titanium nitride layer. The method for forming the titanium nitride layer is similar to the method for forming the titanium oxide layer, except that the type of reactant gas is different. That is, a reactant gas containing nitrogen is injected when forming the titanium nitride layer.
[0091] Additionally, the capping layer (200) may be formed as a titanium oxynitride layer. The method for forming the titanium oxynitride layer is similar to the method for forming a titanium oxide layer or the method for forming a titanium nitride layer, and in the reactant gas injection step, a reactant gas containing nitrogen and a reactant gas containing oxygen are injected.
[0092]
[0093] FIG. 3 is a conceptual diagram illustrating a semiconductor device according to a modified example of the first embodiment of the present invention.
[0094] In the first embodiment, it was described that the lower electrode (100) is formed of a single ruthenium-containing layer (100). That is, it was described that the lower electrode (100) is formed of a ruthenium metal layer or a ruthenium oxide layer.
[0095] However, the lower electrode (100) is not limited thereto, and may be formed in a structure in which a ruthenium metal layer and a ruthenium oxide layer are laminated. That is, referring to FIG. 3, the lower electrode (100) may include a first ruthenium-containing layer (110) and a second ruthenium-containing layer (120) formed on the first ruthenium-containing layer (110). In addition, a capping layer (200) is formed on the second ruthenium-containing layer (120).
[0096] The first ruthenium-containing layer (110) may be a ruthenium oxide layer, and the second ruthenium-containing layer (120) may be a ruthenium metal layer. Of course, the present invention is not limited thereto, and the first ruthenium-containing layer (110) may be a ruthenium metal layer, and the second ruthenium-containing layer (120) may be a ruthenium oxide layer.
[0097]
[0098] Figure 4 is a conceptual diagram illustrating a semiconductor device according to a second embodiment of the present invention.
[0099] In the first embodiment, it was described that the lower electrode (100) includes only the ruthenium-containing layer (100). However, the present invention is not limited thereto, and the lower electrode (100) may further include a titanium nitride layer (130) formed on the lower side of the ruthenium-containing layer (110). That is, the lower electrode according to the second embodiment may include a titanium nitride layer (130) formed on the substrate (S) and a ruthenium-containing layer (110) formed on the titanium nitride layer (130). In addition, a capping layer (200) is formed on the ruthenium-containing layer (110).
[0100] The ruthenium-containing layer (110) may be a ruthenium metal layer or a ruthenium oxide layer. In addition, the method for forming the titanium nitride layer (130) may be the same as the method for forming the capping layer (200) made of the titanium nitride layer. Therefore, a description of the method for forming the titanium nitride layer (130) constituting the lower electrode (100) is omitted.
[0101]
[0102] In the above, it has been described that the lower electrode (100) is formed to contain a precious metal, and a capping layer (200) containing titanium is formed between the lower electrode (100) and the dielectric layer (300). However, the present invention is not limited thereto, and the upper electrode (400) may be formed to contain a precious metal, and a capping layer (200) containing titanium may be formed between the upper electrode (400) and the dielectric layer (300). Of course, the lower electrode (100) and the upper electrode (400) may each be formed to contain a precious metal, and a capping layer (200) containing titanium may be formed between the lower electrode (100) and the dielectric layer (300) and between the upper electrode (400) and the dielectric layer (300).
[0103] In addition, the precious metal contained in at least one of the lower electrode (100) and the upper electrode (400) is not limited to ruthenium (Ru), and various precious metals may be applied. That is, at least one of the lower electrode (100) and the upper electrode (400) may be formed to contain at least one of ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Y), and molybdenum (Mo).
[0104]
[0105] In this way, in the embodiments, a capping layer (200) containing titanium is formed between an electrode containing a precious metal and a dielectric layer (300). As a result, the occurrence of defects at the interface between the electrode and the dielectric layer (300) can be suppressed or prevented. As a result, a decrease in the dielectric constant of the dielectric layer (300) can be suppressed or prevented, and the dielectric constant of the dielectric layer (300) can be made uniform. In addition, the bonding strength of the dielectric layer (300) can be improved. Accordingly, a decrease in the dielectric properties and adhesive strength of the dielectric layer (300) can be suppressed or prevented from causing a decrease in the characteristics of the capacitor. That is, in a semiconductor device including a lower electrode (100) formed using a precious metal, the characteristics of the semiconductor device can be improved.
[0106] According to embodiments of the present invention, the occurrence of defects at the interface between an electrode and a dielectric layer can be suppressed or prevented. As a result, a decrease in the dielectric constant of the dielectric layer can be suppressed or prevented, and the dielectric constant of the dielectric layer can be made uniform. In addition, the bonding strength of the dielectric layer can be improved.
Claims
1. An electrode formed on a substrate and including a precious metal-containing layer; A dielectric layer formed on one surface of the noble metal-containing layer; and A semiconductor device comprising a capping layer formed between the noble metal-containing layer and the dielectric layer and containing titanium (Ti).
2. In claim 1, A semiconductor device wherein the capping layer is formed of at least one of a titanium metal layer, a titanium oxide layer, a titanium nitride layer, and a titanium oxynitride layer.
3. In claim 1, A semiconductor device wherein the thickness of the capping layer is 10Å or less.
4. In claim 1, A semiconductor device in which the above precious metal-containing layer contains at least one of ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Y), and molybdenum (Mo).
5. In claim 4, A semiconductor device in which the above precious metal-containing layer is a precious metal layer or precious metal oxide layer containing at least one of ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Y), and molybdenum (Mo).
6. In claim 4, The above precious metal-containing layer includes a first precious metal-containing layer and a second precious metal-containing layer formed on the first precious metal-containing layer, A semiconductor device wherein one of the first and second noble metal-containing layers is a noble metal layer and the other is a noble metal oxide layer.
7. In claim 1, The above electrode is a semiconductor device including a titanium nitride layer formed on the other surface of the precious metal-containing layer.
8. A step of forming an electrode including a precious metal-containing layer by spraying a precursor containing a precious metal on a substrate; A step of forming a capping layer on the electrode by spraying a precursor containing titanium (Ti) toward the electrode; A method for manufacturing a semiconductor device, comprising: forming a dielectric layer on the capping layer.
9. In claim 8, The step of forming the capping layer is: A method for manufacturing a semiconductor device, comprising a step of exposing a titanium-containing layer formed by spraying a precursor containing the titanium (Ti) to hydrogen plasma.
10. In claim 8, A method for manufacturing a semiconductor device, comprising the step of injecting a reactant gas containing at least one of oxygen and nitrogen toward a titanium-containing layer formed by injecting a precursor containing the titanium (Ti).
11. In claim 10, A method for manufacturing a semiconductor device, wherein the step of injecting the reactant gas includes a step of generating plasma using the reactant gas.
12. In claim 8, A method for manufacturing a semiconductor device, wherein in the step of spraying a precursor containing the above precious metal, a precursor containing at least one of ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Y) and molybdenum (Mo) is sprayed.
13. In claim 8, The step of forming the above electrode is: A method for manufacturing a semiconductor device, comprising a step of generating hydrogen plasma after spraying a precursor containing the above-mentioned precious metal.
14. In claim 8, The step of forming the above electrode is: A method for manufacturing a semiconductor device, comprising a step of generating oxygen plasma after spraying a precursor containing the above-mentioned precious metal.
15. In claim 8, The step of forming the above electrode is: A method for manufacturing a semiconductor device, comprising the step of forming a titanium nitride layer on the substrate before forming a precious metal-containing layer on the substrate.
Citation Information
Patent Citations
Semiconductor device with ruthenium electrode and method for fabricating the same
KR100881728B1
A semiconductor device including metal interconnections and method for fabricating the same
KR102154112B1
Electric leakage detection type processed
KR102586054B1
Semiconductor device having a capping layer including cobalt and method of fabricating the same
US20060145269A1
KR20220074676A