Eco-friendly soil conditioner and method for manufacturing same
The combination of hydroxyethyl cellulose and glycerin with porous inorganic materials and crosslinking agents in a thermoplastic resin addresses the limitations of existing soil conditioners by enhancing water retention and bio-carbon content, providing an eco-friendly solution for desertification and reducing global warming.
Patent Information
- Application Number
- PCT/KR2024/006313
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-14
AI Technical Summary
Existing soil conditioners, such as hygroscopic polymers and inorganic salts, fail to effectively improve water retention and bio-carbon content in sandy soils, leading to desertification and environmental pollution, while posing health risks and contributing to greenhouse gases.
A thermoplastic resin composed of 65% to 80% hydroxyethyl cellulose and 20% to 35% glycerin, combined with porous inorganic materials and crosslinking agents, is used to create an eco-friendly soil conditioner that enhances water retention and bio-carbon content, reducing global warming.
The eco-friendly soil conditioner improves drought tolerance, increases bio-carbon content, and is biodegradable, offering excellent processability and durability, thus addressing desertification and environmental concerns.
Smart Images

Figure KR2024006313_14112024_PF_FP_ABST
Abstract
Description
Eco-friendly soil conditioner and its manufacturing method
[0001] The present invention relates to a soil conditioner and a method for producing the same, and more particularly, to an eco-friendly soil conditioner and a method for producing the same, which can increase the moisture retention capacity of the soil when mixed into natural or artificial soil, and can increase the bio-carbon content while being biodegradable, thereby reducing global warming.
[0002] Soil conditioners generally refer to substances used to improve soil physical, chemical and / or biological properties of disturbed soils that affect plant growth / crop quality and safety due to natural / human influences.
[0003] Impaired soils include sandy soil, clay soil, structural obstacle soil, acid soil, saline soil, alkaline soil, and contaminated soil. These impaired soils are mainly those with insufficient vegetation, poor structure, hindered plant root growth, low fertility, or lack of nutrients (imbalance, acidification, salinity, excessive or insufficient soil moisture, toxic substances, etc.).
[0004] Sandy soils, in particular, are primarily found in arid regions and where desertification is progressing. In arid regions, soil erosion by wind or heavy rainfall can lower the survival rate of afforestation trees. Furthermore, sandy soils, due to their inherent inability to retain water, are often washed away with the water flow. This prevents the roots of plants like trees and grasses from utilizing both water and nutrients, making forests and grasslands difficult to form.
[0005] In such arid regions, attempts have been made to improve soil moisture by adding hygroscopic polymers such as polyacrylic acid (ASAP; acrylic sodium salt polymer) or polyacrylamide to prevent desertification (Patent Document 0001, Patent Document 0002). However, organic materials, including fertilizers, have difficulty maintaining or improving soil moisture. In particular, polyacrylamide is classified as a Class 2 carcinogen, posing a health hazard. Furthermore, petroleum-based acrylics are a major greenhouse gas emitter and should no longer be used to prevent environmental pollution.
[0006] Meanwhile, inorganic salts, such as magnesium chloride (MgCl2), can help retain moisture in the soil. However, they are easily dissolved by rain, especially in sandy soils, and are easily removed from the soil. They then flow into rivers and other aquatic ecosystems, negatively impacting river ecosystems and other aquatic ecosystems due to elevated salt concentrations. Furthermore, excessive use of inorganic salts can lead to environmental problems such as soil acidification and plant death.
[0007] In addition, hygroscopic polymers require a long time to decompose in the soil, and hygroscopic polymers and / or their decomposition products in the soil may act as toxic components in the soil ecosystem, causing environmental pollution problems.
[0008] Therefore, in order to improve the soil of arid regions to prevent desertification, a soil conditioner is required that maintains / improves soil moisture while preventing the runoff of fertilizer components in the soil and enhancing the fertilizer effect to improve the survival rate / production of crops during afforestation, pasture formation, or agricultural activities in arid regions without using inorganic salts or polymers that cause soil toxicity as the main ingredient.
[0009] [Prior Art Literature]
[0010] [Patent Document]
[0011] (Patent Document 1) Korean Patent No. 10-1264829 (Published: January 23, 2013)
[0012] (Patent Document 2) Korean Patent No. 10-2479792 (Published: April 20, 2022)
[0013] The main purpose of the present invention is to solve the above-described problems, and to provide an eco-friendly soil conditioner and a method for producing the same, which can increase the moisture retention capacity of soil and increase the bio-carbon content while being biodegradable, thereby reducing global warming.
[0014] In order to achieve the above purpose, one embodiment of the present invention provides an eco-friendly soil conditioner characterized by including a thermoplastic resin containing 65 to 80 wt% of hydroxyethyl cellulose and 20 to 35 wt% of glycerin.
[0015] In a preferred embodiment of the present invention, the eco-friendly soil improver may be characterized by further comprising 5 to 60 parts by weight of a porous inorganic material relative to 100 parts by weight of a thermoplastic resin, or further comprising 5 to 40 parts by weight of a crosslinking agent relative to 100 parts by weight of a thermoplastic resin.
[0016] In a preferred embodiment of the present invention, the porous inorganic material may be characterized by being at least one selected from the group consisting of perlite, vermiculite, bentonite, and zeolite.
[0017] In a preferred embodiment of the present invention, the crosslinking agent may be characterized by being at least one selected from the group consisting of citric acid, polyethylene glycol, and hexanediol.
[0018] In a preferred embodiment of the present invention, the hydroxyethyl cellulose may be characterized in that the viscosity of an aqueous solution dissolved in water at 2 wt% is 10 cps to 250,000 cps when measured using a Brookfield viscometer at 20°C.
[0019] Another embodiment of the present invention provides a method for producing an eco-friendly soil conditioner, comprising the steps of: (a) mixing 65 to 80 wt% of hydroxyethyl cellulose with 20 to 35 wt% of glycerin to obtain a mixture; (b) kneading and plasticizing the obtained mixture to obtain a thermoplastic resin; and (c) granulating the obtained thermoplastic resin.
[0020] In another preferred embodiment of the present invention, the method for producing the eco-friendly soil conditioner may be characterized in that a porous inorganic material and / or a crosslinking agent are further added and mixed in step (a) or step (c), and the content of the porous inorganic material is 5 to 60 parts by weight relative to 100 parts by weight of the mixture in step (a) or 100 parts by weight of the thermoplastic resin in step (c), and the content of the crosslinking agent is 5 to 40 parts by weight relative to 100 parts by weight of the mixture in step (a) or 100 parts by weight of the thermoplastic resin in step (c).
[0021] In another preferred embodiment of the present invention, the porous inorganic material may be characterized by being at least one selected from the group consisting of perlite, vermiculite, bentonite, and zeolite.
[0022] In another preferred embodiment of the present invention, the crosslinking agent may be characterized by being at least one selected from the group consisting of citric acid, polyethylene glycol, and hexanediol.
[0023] In another preferred embodiment of the present invention, the hydroxyethyl cellulose may be characterized in that the viscosity of an aqueous solution dissolved in water at 2 wt% is 10 cps to 250,000 cps when measured using a Brookfield viscometer at 20°C.
[0024] In another preferred embodiment of the present invention, the mixing in step (b) may be performed at 50°C to 90°C and at 300 rpm or more.
[0025] In another preferred embodiment of the present invention, the granulation in step (c) may be characterized by pressurizing and molding into a granular or pellet-shaped granular state.
[0026] The eco-friendly soil conditioner according to the present invention can improve drought and dry growing environments of crops by increasing the moisture retention capacity of the soil, and at the same time, can increase the bio-carbon content as a biodegradable raw material, thereby reducing global warming.
[0027] In addition, the eco-friendly soil conditioner according to the present invention has excellent moldability and processability, and is easy to control particle size, so that large-capacity spraying or machine spraying is possible, thereby simplifying the soil conditioner spreading work, shortening the working time and saving the spraying cost, and is efficient in that it has excellent absorbency and durability, so that it can maintain constant performance for a long period of time.
[0028] Figures 1 (a) and (b) are photographic images of soil improvers manufactured in Experimental Examples 1-3 and 1-4 of the present invention, taken with a digital camera.
[0029] Figure 2 is a photographic image of a soil improver manufactured in Experimental Example 2-3 of the present invention, taken with a digital camera.
[0030] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the experimental examples described in detail below together with the accompanying drawings. However, the present invention is not limited to the experimental examples disclosed below, but may be implemented in various different forms. These experimental examples are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined solely by the scope of the claims.
[0031] In describing the present invention, if it is determined that a detailed description of a related known technology may unnecessarily obscure the gist of the present invention, the detailed description is omitted.
[0032] In the specification, when "includes," "has," "consists of," and "consists of" are used, other parts may be added unless "only" is used. When a component is expressed in the singular, it includes the plural unless otherwise explicitly stated.
[0033] The characteristics of each of the various experimental examples of the present invention can be partially or wholly combined or combined with each other, and various technical linkages and operations are possible, and each experimental example can be performed independently of each other or can be performed together in a related relationship.
[0034] The present invention relates to an eco-friendly soil conditioner, characterized in that it comprises a thermoplastic resin containing 65 to 80 wt% of hydroxyethyl cellulose and 20 to 35 wt% of glycerin.
[0035] In general, cellulose derivatives have water retention, salt tolerance, pH stability, and are biodegradable, and have been developed into various soil conditioners recently. However, they are difficult to mix with inorganic materials, crosslinkers, and additives due to the strong hydrogen bonds that cause thermal decomposition below the melting point, and they have a high molecular structure that is difficult to mold and process, so they have not been able to perform their role as sufficient soil conditioners.
[0036] Accordingly, in the present invention, a thermoplastic resin obtained by adding a specific amount of glycerin to hydroxyethyl cellulose having a specific viscosity among cellulose derivatives is used, and by further mixing a porous inorganic material and / or a crosslinking agent therein to granulate the resin, the molding processability is excellent and the mechanical properties are improved, so that the moisture retention capacity in the soil can be stably increased, and not only is soil granulation, pH control, nutrient supply, and incorporation of microorganisms possible, but also biodegradation can increase the bio-carbon content, and since the particle size of the product is easy to control, it is advantageous for large-scale spraying using machines such as drones and tractors, and an eco-friendly soil conditioner capable of biodegradation can be provided by utilizing plant and natural materials.
[0037] To avoid duplication, the description of each component above is provided in the manufacturing method of the eco-friendly soil conditioner described below.
[0038] From another aspect, the present invention relates to a method for producing an eco-friendly soil conditioner, characterized by comprising the steps of: (a) mixing 65 to 80 wt% of hydroxyethyl cellulose with 20 to 35 wt% of glycerin to obtain a mixture; (b) kneading and plasticizing the obtained mixture to obtain a thermoplastic resin; and (c) granulating the obtained thermoplastic resin.
[0039] The method for manufacturing an eco-friendly soil improver according to the present invention first adds glycerin to hydroxyethyl cellulose to obtain a mixture [step (a)].
[0040] The above hydroxyethyl cellulose (HEC) is a water-soluble polymer component in the form of a white or light yellowish white powder. It has the best salt resistance and pH stability among cellulose derivatives, and is recognized as a raw material that can be used in various products in various industries due to its colloidal properties, water retention properties, and temperature resistance.
[0041] In the present invention, the hydroxyethyl cellulose may be a base resin having a viscosity of 10 cps or more, preferably 10 cps to 250,000 cps, and more preferably 100 cps to 250,000 cps. In this case, the viscosity of the hydroxyethyl cellulose is the viscosity of an aqueous solution (hydroxyethyl cellulose: 2 wt%) of hydroxyethyl cellulose dissolved in water, measured using a Brookfield viscometer at 20°C.
[0042] If the viscosity of the hydroxyethyl cellulose is less than 10 cps, the amount of glycerin mixed therein, which will be described later, increases, causing stickiness after extrusion and problems with formability when manufacturing thermoplastic resin chips.
[0043] In addition, the hydroxyethyl cellulose may be mixed in an amount of 65 wt% to 80 wt% based on the total weight of hydroxyethyl cellulose and glycerin. If the content of the hydroxyethyl cellulose is less than 65 wt%, excessive glycerin may be contained, resulting in stickiness and difficulty in the granulation process, and the mixture may be formed in the form of lumps that are difficult to feed into a device such as an extruder after plasticization. If it exceeds 80 wt%, the plasticization by glycerin may not proceed sufficiently, resulting in a problem in that it is impossible to manufacture a thermoplastic resin.
[0044] The above hydroxyethyl cellulose can be used as a commercial product or manufactured and used, and any manufacturing method known in the art can be applied without limitation as a manufacturing method for the hydroxyethyl cellulose. Preferably, the hydroxyethyl cellulose can be manufactured by reacting cellulose with an alkalizing agent to obtain alkalized cellulose, and then subjecting the obtained alkalized cellulose to an etherification reaction.
[0045] Meanwhile, glycerin can be obtained as a byproduct when manufacturing soap or fatty acids from natural resins. Recently, however, glycerin has been synthesized by treating propylene with chlorine to produce epichlorohydrin, which is then hydrolyzed. It is used in a variety of fields, including rubber, toothpaste, cosmetics, chemicals, paints, cellophane, printing ink, and confectionery.
[0046] In the present invention, the glycerin is mixed into hydroxyethyl cellulose to prevent strong hydrogen bonding due to hydroxyethyl cellulose hydroxyl groups and to widen the distance between cellulose polymer chains, thereby creating an environment in which microbrown motion easily occurs. The glycerin may be added in an amount of 20 wt% to 35 wt% based on the total weight of hydroxyethyl cellulose and glycerin.
[0047] If the glycerin content is less than 20 wt% based on the total weight of hydroxyethyl cellulose and glycerin, the effect of interfering with the strong hydrogen bonding due to the hydroxyl group of hydroxyethyl cellulose and widening the distance between cellulose polymer chains to create an environment in which microBrownian motion easily occurs is insufficient, so that the glass transition temperature cannot be lowered and flexibility cannot be provided to the resin. If it exceeds 35 wt%, excessive glycerin may be eluted, causing stickiness, and problems such as difficulty in granulation of pellets may occur.
[0048] Thereafter, a mixture of hydroxyethyl cellulose and glycerin can be plasticized by kneading to obtain a thermoplastic resin [step (b)].
[0049] The mixing of the above mixture can be performed at 50°C to 90°C and 300 rpm or more, preferably 70°C to 90°C and 300 rpm to 600 rpm, so that the plasticization of hydroxyethyl cellulose can easily proceed, and the mixing time can be appropriately adjusted depending on the content of the mixture or the degree of plasticization, and can be preferably performed for 30 to 60 minutes.
[0050] When mixing is performed under the above conditions, the glass transition temperature and melting point of hydroxyethyl cellulose can be lowered to facilitate micro-Brownian motion of hydroxyethyl cellulose, thereby improving the plasticization efficiency of hydroxyethyl cellulose even with a small amount of glycerin.
[0051] The above mixing may be performed in any manner, but may be performed alone using a mixer, or together with the extrusion described below using an extruder. The mixer is not particularly limited, and any mixer commonly used in the art may be used without limitation. Examples of such mixers include high-speed stirrers, mixers, and blenders.
[0052] Additionally, additives may be further added and mixed as needed before and / or after the mixing (plasticizing) step.
[0053] The above additive may preferably be at least one selected from the group consisting of an antioxidant, a lubricant, a biodegradation accelerator, and a strength reinforcing agent, and the present invention does not place any particular limitation on the selection of the above additive as it is a component commonly used in the field.
[0054] Specifically, among the above additives, the antioxidant plays a role in preventing decomposition due to heat during thermoplasticization and molding of hydroxyethyl cellulose, and may be a common antioxidant that can be used in the relevant field. For example, it may be in the form of a single or mixed compound such as tetrakismethylene (3,5-di-t-butyl-4-hydroxyhydrocinnamate) methane, tris (2,4-di-t-butylphenyl) phosphate, etc.
[0055] In addition, the lubricant is intended to improve the lubricating properties of the thermoplastic resin, and any common lubricant usable in the field can be used without limitation, and in terms of compatibility with and lubricity of the thermoplastic resin of the present invention, it may preferably be at least one selected from the group consisting of sorbitol, magnesium stearate, calcium stearate, ethylene glycol, glycerol monostearate, and lecithin.
[0056] In addition, the biodegradation accelerator and strength reinforcing agent may be used without limitation as long as they are conventional biodegradation accelerators and strength reinforcing agents that can promote biodegradation of thermoplastic resins or reinforce the strength of the resin, and the biodegradation accelerator may be a fatty oil of soybean oil, castor oil, linseed oil, sunflower oil, coconut oil, fatty acids of caproic acid, capric acid, lauric acid, oleic acid, olenic acid, linoleic acid, fatty acid esters such as ethyl oleate, ethyl linoleate, and isooctylate, alone or in combination of two or more, and the strength reinforcing agent may be glass fiber, carbon fiber, etc.
[0057] Such additives may be selected without limitation in a content commonly used within a range that does not impair the desired physical properties of the thermoplastic resin of the present invention, but preferably, each additive may be independently 0.01 to 10 parts by weight per 100 parts by weight of the thermoplastic resin of the present invention.
[0058] As described above, the thermoplastic resin that has been mixed (plasticized) can be obtained in a form that is easy to manufacture by further including an extrusion step and a cutting step of extruding and cutting.
[0059] The above extrusion step can be performed through an extruder, and the extruder is not particularly limited, and any extruder commonly used in the art can be used without limitation. For example, a single-screw extruder equipped with one screw or a multi-screw extruder equipped with multiple screws can be used. Considering uniform mixing of materials, ease of processing, and economy, it may be preferable to use a twin-screw extruder with two screws.
[0060] At this time, the temperature of the extruder may be 70°C to 200°C, preferably 130°C to 180°C, so that extrusion can be efficiently performed without decomposition of the thermoplastic resin, and the screw rotation speed of the extruder may be 20 rpm to 300 rpm, preferably 20 rpm to 200 rpm. Such extrusion conditions have the advantage of allowing sufficient extrusion while ensuring excellent process efficiency due to an appropriate throughput per unit time, and not causing problems such as thermal decomposition of the resin component.
[0061] The extruded extrudate can be cut into a form that is easy to handle and easy to manufacture into a molded product using a pelletizer or the like, and preferably can be in the form of granules or pellets.
[0062] In addition, in the step of obtaining a thermoplastic resin according to the present invention, it is also effective to further include a cooling step of cooling through a cooling water tank between the extrusion and cutting steps, and after the cutting step, it is preferable to perform a drying step of drying at 50°C to 80°C for 4 to 8 hours.
[0063] The thermoplastic resin obtained in this manner may have, for example, a tensile strength of 4.5 MPa to 6.5 MPa as measured by ASTM D638, an elongation of 20 mm to 45 mm, excellent mechanical properties and molding processability, and biodegradability.
[0064] Thereafter, the obtained thermoplastic resin is granulated to manufacture a soil improver [step (c)].
[0065] The above granulation can be obtained in a form that is easy to manufacture by including an extrusion step and a cutting step of extruding and cutting the above-described mixture.
[0066] The above extrusion step can be performed through an extruder, and the extruder is not particularly limited, and any extruder commonly used in the art can be used without limitation. For example, a single-screw extruder equipped with one screw or a multi-screw extruder equipped with multiple screws can be used. Considering uniform mixing of materials, ease of processing, and economy, it may be preferable to use a twin-screw extruder with two screws.
[0067] At this time, the temperature of the extruder may be 70 ℃ to 200 ℃, preferably 130 ℃ to 180 ℃, so that extrusion is efficiently performed without decomposition of the soil conditioner, and the screw rotation speed of the extruder may be 20 rpm to 300 rpm, preferably 20 rpm to 200 rpm. Such extrusion conditions have the advantage of enabling sufficient extrusion while ensuring excellent process efficiency due to an appropriate throughput per unit time, and not causing problems such as thermal decomposition of the resin component.
[0068] The extruded extrudate can be cut into a form that is easy to handle and easy to manufacture into a molded product using a pelletizer or the like, and preferably can be in the form of granules or pellets.
[0069] In addition, in the manufacture of a soil conditioner according to the present invention, it is also effective to further include a cooling step through cold air drying between the extrusion and cutting steps, and after the cutting step, it is preferable to perform a drying step of drying at 50°C to 80°C for 4 to 8 hours.
[0070] The soil conditioner manufactured in this manner may have an average diameter of 1 mm to 7 mm, and specifically, an average diameter of 2 mm to 5 mm. A soil conditioner having an average diameter within the above range is easy to spread on soil, and has the advantage of increasing the amount of water absorbed due to its large surface area per unit weight when absorbing water.
[0071] Meanwhile, the method for manufacturing an eco-friendly soil conditioner according to the present invention can manufacture an eco-friendly soil conditioner by further mixing a porous inorganic material and / or a crosslinking agent into a thermoplastic resin in which the mixture of hydroxyethyl cellulose and glycerin in step (a) or the mixture of ethyl cellulose and glycerin in step (c) is plasticized.
[0072] At this time, the porous inorganic material plays a role in helping absorb and release moisture, and may be included in an amount of 5 to 60 parts by weight, preferably 10 to 50 parts by weight, relative to 100 parts by weight of the mixture of step (a) or the thermoplastic resin of step (c). If it is included in an amount of less than 5 parts by weight relative to 100 parts by weight of the mixture of step (a) or the thermoplastic resin of step (c), the movement path of moisture may be blocked, which may cause problems in absorption and release of moisture, and if it is included in an amount exceeding 60 parts by weight, the sustainability of moisture release may be reduced, and also, due to the addition of an excessive amount of porous inorganic material, problems in formability after extrusion may occur.
[0073] The above porous inorganic material can be applied without limitation as long as it is an inorganic material having porosity, and specifically, it can be at least one selected from the group consisting of perlite, vermiculite, bentonite, and zeolite, and more specifically, it can be perlite.
[0074] In addition, the crosslinking agent is mixed into the mixture of step (a) or the thermoplastic resin of step (c) to lower the extrusion temperature, thereby increasing flowability, minimizing deterioration of physical properties even when moisture is absorbed, and increasing moisture absorption capacity. The crosslinking agent may be mixed in an amount of 5 to 40 parts by weight, preferably 10 to 40 parts by weight, based on 100 parts by weight of the mixture of step (a) or the thermoplastic resin of step (c). If the crosslinking agent is included in an amount of less than 5 parts by weight, a problem may arise in that the moisture absorption amount and absorption speed may be reduced, and if it is included in an amount of more than 40 parts by weight, a problem may arise in that strands cannot be manufactured during extrusion due to an excess of the crosslinking agent.
[0075] The above crosslinking agent may be applied without limitation as long as it is a crosslinking agent capable of crosslinking a thermoplastic resin, and specifically may be at least one selected from the group consisting of citric acid, polyethylene glycol, and hexanediol, and more specifically may be citric acid. Since the citric acid is a natural substance, it is non-toxic and has the advantage of being more advantageous for biodegradation.
[0076] The soil conditioner according to the present invention manufactured in this manner is biodegradable and has excellent moldability and mechanical properties, so that it stably increases the moisture retention capacity of the soil, while at the same time enabling soil agglomeration, pH control, nutrient supply, and incorporation of microorganisms, thereby creating optimal vegetation conditions. In addition, it can increase the bio-carbon content while being biodegraded.
[0077] In describing the soil improver of the present invention and its manufacturing method, it is stated that other conditions or equipment, etc. that are not explicitly described can be appropriately selected within the range commonly practiced in the art and are not particularly limited.
[0078] Hereinafter, the present invention will be described in more detail through specific experimental examples. The following experimental examples are merely illustrative examples intended to aid understanding of the present invention and are not intended to limit the scope of the present invention.
[0079] <Experimental Example 1-1>
[0080] 23 g of glycerin was added to 77 g of hydroxyethyl cellulose (Lotte Fine Chemical, HEC B100K) having a viscosity of 100,000 cps, and plasticized by high-speed mixing at 300 rpm for 30 minutes. Then, a thermoplastic resin was obtained by extruding at an average temperature of 150°C using a twin-screw extruder having a screw speed of 30 rpm [the speed of the main motor was 200 to 250 rpm]. Perlite was added to the thermoplastic resin obtained above in the amount shown in Table 1, and then mixed for 20 minutes. Then, a twin-screw extruder with a screw speed of 30 rpm [the speed of the main motor was 200 rpm to 250 rpm] was used to extrude at an average temperature of 150°C, thereby producing a soil conditioner in the shape of a strand (3 mm × 3 mm).
[0081] <Experimental Examples 1-2 to 1-14>
[0082] A soil conditioner was manufactured in the same manner as Experimental Example 1-1, but the conditions in Table 1 below were changed to manufacture a soil conditioner in the form of a strand.
[0083] <Experimental Example 1-15>
[0084] A mixture was obtained by mixing 26 g of glycerin with 74 g of hydroxyethyl cellulose (Lotte Fine Chemical, HEC H200K) having a viscosity of 200,000 cps, and 10 g of perlite was added to the mixture, followed by plasticization by high-speed mixing at 300 rpm for 30 minutes. After plasticization, a soil conditioner in the shape of strands (3 mm × 3 mm) was manufactured by extruding the mixture using a twin-screw extruder with a screw speed of 30 rpm [the speed of the main motor was 200 rpm to 250 rpm] at an average temperature of the extruder of 150°C.
[0085] Experimental Example 1-16
[0086] A soil conditioner was manufactured in the same manner as Experimental Example 1-15, but the conditions in Table 1 below were changed to manufacture a soil conditioner in the form of a strand.
[0087] <Experimental Examples 1-17 to 1-27>
[0088] A soil conditioner was manufactured in the same manner as Experimental Example 1-1, but the conditions in Table 1 below were changed to manufacture a soil conditioner in the form of a strand.
[0089] Experimental Example 1-28
[0090] 10 g of perlite was added to 100 g of hydroxyethyl cellulose (Lotte Fine Chemical, HEC B100K) having a viscosity of 100,000 cps, and then mixed for 20 minutes. Then, the mixture was extruded at an average temperature of 150°C using a twin-screw extruder with a screw speed of 30 rpm [the speed of the main motor was 200 to 250 rpm] to produce a soil conditioner in the shape of a strand (3 mm × 3 mm).
[0091] [Measurement of Formability, Water Absorption, and Water Release of Soil Improvers]
[0092] The properties of the soil improvers manufactured in Experimental Examples 1-1 to 1-28 were measured using the following methods, and the results are shown in Table 1 below.
[0093] measurement method
[0094] (1) Formability Measurement: The flowability of the extrudate was visually evaluated immediately after extrusion. If extrusion was easy and the extrudate was in good condition, it was recorded as “good.” If extrusion was not successful, it was recorded as “poor” in Table 1.
[0095] (2) Measurement of moisture absorption: 100 g of the soil conditioner specimen manufactured in the experimental example was placed in a plastic container, 1,500 ml of water was mixed, and after 60 minutes, the moisture absorption amount absorbed by the soil conditioner was calculated using Equation 1 and shown in Table 1.
[0096] Moisture absorption (g) = Weight of soil conditioner after absorption (g) - [Weight of soil conditioner before absorption (g) + Weight of plastic container (g)].....(1)
[0097] (3) Measurement of moisture release: After moisture absorption, the soil conditioner was left at a temperature of 20℃ and a humidity of 60% for 180 hours (7 days), and the moisture release was measured with a scale every 12 hours, and then calculated using Equation 2 and shown in Table 1.
[0098] Moisture release rate (g / h) = [Weight of soil conditioner after absorption (g) - Weight of soil conditioner after moisture release (g)] / 144 (h).....(2)
[0099] [Table 1]
[0100]
[0101] As shown in Table 1, the soil conditioners of Experimental Examples 1-1 to 1-19 showed good formability and sufficient water absorption and water release per hour, whereas when the hydroxyethyl cellulose content was outside of 65% to 80%, the formability of the soil conditioners showed poor. In addition, when PEG was applied as a plasticizer, the formability was good, but the water absorption and water release per hour were poor, and when hydroxypropyl methylcellulose (HPMC), methylcellulose (MC), and hydroxyethyl methylcellulose (HEMC) were applied, the formability showed poor.
[0102] <Experimental Example 2-1>
[0103] A mixture was obtained by adding 23 g of glycerin to 77 g of hydroxyethyl cellulose (Lotte Fine Chemical, HEC B100K) having a viscosity of 100,000 cps, and 5 g of citric acid as a cross-linking agent was added to the obtained mixture, and the mixture was plasticized by high-speed mixing at 300 rpm for 30 minutes, and then extruded at an average temperature of 130°C, which is an extruder, using a twin-screw extruder having a screw speed of 30 rpm [the speed of the main motor was 200 rpm to 250 rpm] to produce a soil conditioner in the shape of a strand (3 mm × 3 mm).
[0104] <Experimental Examples 2-2 to 2-14>
[0105] A soil conditioner was manufactured in the same manner as Experimental Example 2-1, but the conditions in Table 2 below were changed to manufacture a soil conditioner in the form of a strand.
[0106] Experimental Example 2-15
[0107] A mixture was obtained by mixing 26 g of glycerin with 74 g of hydroxyethyl cellulose (Lotte Fine Chemical, HEC H200K) having a viscosity of 200,000 cps, and the mixture was plasticized by high-speed mixing at 300 rpm for 30 minutes, and then extruded at an average temperature of 150°C, which is an extruder, using a twin-screw extruder having a screw speed of 30 rpm [the speed of the main motor was 200 rpm to 250 rpm], to obtain a thermoplastic resin. Citric acid, a crosslinking agent, was added to the thermoplastic resin obtained above in the amount shown in Table 2, and then mixed for 20 minutes. Then, a twin-screw extruder with a screw speed of 30 rpm [the speed of the main motor was 200 rpm to 250 rpm] was used to extrude at an average temperature of 130°C, thereby producing a soil conditioner in the shape of a strand (3 mm × 3 mm).
[0108] <Experimental Examples 2-16 and 2-17>
[0109] A soil conditioner was manufactured in the same manner as Experimental Example 2-15, but the conditions in Table 2 below were changed to manufacture a soil conditioner in the form of a strand.
[0110] <Experimental Examples 2-18 to 2-27>
[0111] A soil conditioner was manufactured in the same manner as Experimental Example 2-1, but the conditions in Table 2 below were changed to manufacture a soil conditioner in the form of a strand.
[0112] <Experimental Example 2-28>
[0113] To 100 g of hydroxyethyl cellulose (Lotte Fine Chemical, HEC B100K) having a viscosity of 100,000 cps, 25 g of citric acid was added, and then mixed for 20 minutes. Then, the mixture was extruded at an average temperature of 130°C using a twin-screw extruder with a screw speed of 30 rpm [the speed of the main motor was 200 to 250 rpm] to produce a soil conditioner in the shape of a strand (3 mm × 3 mm).
[0114] [Measurement of Formability, Water Absorption, and Water Release of Soil Improvers]
[0115] The properties of the soil improvers manufactured in Experimental Examples 2-1 to 2-28 were measured using the following methods, and the results are shown in Table 2 below.
[0116] measurement method
[0117] (1) Formability Measurement: The flowability of the extrudate was visually evaluated immediately after extrusion. If extrusion was easy and the extrudate was in good condition, it was recorded as “good.” If extrusion was not possible, it was recorded as “bad” in Table 2.
[0118] (2) Measurement of moisture absorption: 100 g of the soil conditioner specimen manufactured in the experimental example was placed in a plastic container and mixed with 1,500 ml of water. After 60 minutes, the moisture absorption amount absorbed by the soil conditioner was calculated using Equation 3 and shown in Table 2.
[0119] Moisture absorption (g) = Weight of soil conditioner after absorption (g) - [Weight of soil conditioner before absorption (g) + Weight of plastic container (g)].....(3)
[0120] (3) Measurement of moisture release: After moisture absorption, the soil conditioner was left for 180 hours (7 days) under conditions of temperature 20℃ and humidity 60%, and the moisture release was measured with a scale every 12 hours, and then calculated using Equation 4 and shown in Table 2.
[0121] Moisture release rate (g / h) = [Weight of soil conditioner after absorption (g) - Weight of soil conditioner after moisture release (g)] / 144 (h)....(4)
[0122] [Table 2]
[0123]
[0124] As shown in Table 2, the soil conditioners of Experimental Examples 2-1 to 2-20 showed good formability and sufficient water absorption and water release per hour, whereas when the hydroxyethyl cellulose content was outside of 65 wt% to 80 wt%, the formability was poor. In addition, when polyethylene glycol was applied as a plasticizer, the formability was good, but the water absorption and water release per hour were poor, and when hydroxypropyl methylcellulose (HPMC), methylcellulose (MC), and hydroxyethyl methylcellulose (HEMC) were applied, the formability was poor.
[0125] Therefore, it was confirmed that the soil conditioner according to the present invention can increase the moisture retention capacity of soil and increase the bio-carbon content while being biodegraded, thereby reducing global warming.
[0126] As described above, although the present invention has been described through limited experimental examples and drawings, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical idea of the present invention and the equivalent scope of the patent claims to be described below by a person having ordinary skill in the art to which the present invention pertains.
Claims
1. An eco-friendly soil conditioner comprising a thermoplastic resin containing 65 to 80 wt% of hydroxyethyl cellulose and 20 to 35 wt% of glycerin.
2. In paragraph 1, The above-mentioned eco-friendly soil improver is characterized in that it further comprises 5 to 60 parts by weight of a porous inorganic material relative to 100 parts by weight of a thermoplastic resin, or 5 to 40 parts by weight of a crosslinking agent relative to 100 parts by weight of a thermoplastic resin.
3. In paragraph 2, An eco-friendly soil conditioner characterized in that the above porous inorganic material is at least one selected from the group consisting of perlite, vermiculite, bentonite, and zeolite.
4. In paragraph 2, An eco-friendly soil improver characterized in that the crosslinking agent is at least one selected from the group consisting of citric acid, polyethylene glycol, and hexanediol.
5. In paragraph 1, The above hydroxyethyl cellulose is an eco-friendly soil conditioner characterized in that the viscosity of an aqueous solution dissolved in water at 2 wt% is 10 cps to 250,000 cps when measured using a Brookfield viscometer at 20°C. 6.(a) A step of obtaining a mixture by mixing 20 to 35 wt% of glycerin with 65 to 80 wt% of hydroxyethyl cellulose; (b) a step of kneading and plasticizing the obtained mixture to obtain a thermoplastic resin; and (c) A method for producing an eco-friendly soil improver, characterized by including a step of granulating the obtained thermoplastic resin.
7. In paragraph 6, The method for manufacturing the above-mentioned eco-friendly soil conditioner is characterized in that the porous inorganic material and / or crosslinking agent are further added and mixed in step (a) or step (c), and the content of the porous inorganic material is 5 to 60 parts by weight relative to 100 parts by weight of the mixture in step (a) or 100 parts by weight of the thermoplastic resin in step (c), and the content of the crosslinking agent is 5 to 40 parts by weight relative to 100 parts by weight of the mixture in step (a) or 100 parts by weight of the thermoplastic resin in step (c).
8. In paragraph 7, A method for manufacturing an eco-friendly soil conditioner, characterized in that the porous inorganic material is at least one selected from the group consisting of perlite, vermiculite, bentonite, and zeolite.
9. In paragraph 7, A method for manufacturing an eco-friendly soil conditioner, characterized in that the cross-linking agent is at least one selected from the group consisting of citric acid, polyethylene glycol, and hexanediol.
10. In paragraph 6, A method for manufacturing an eco-friendly soil conditioner, characterized in that the above hydroxyethyl cellulose has a viscosity of 10 cps to 250,000 cps when an aqueous solution dissolved in water at 2 wt% is measured using a Brookfield viscometer at 20°C.
11. In paragraph 6, A method for manufacturing an eco-friendly soil improver, characterized in that the mixing in the above step (b) is performed at 50°C to 90°C and 300 rpm or more.
12. In paragraph 6, A method for manufacturing an eco-friendly soil conditioner, characterized in that the granulation in the above step (c) is pressure-molded into a granular or pellet-shaped granular state.
Citation Information
Patent Citations
Soil conditioner incliding functional ingredient for management of water and nutrients
KR101264829B1
Soil moisture retention agent comprising nanocomposite hydrogel and method of managing soil using the same
KR102479792B1
Use of agglomerated hydroxyethylcellulose in pharmaceutical, personal care and household care applications
KR1020150010981A
Wrist Cushion Notebook Cooling Pad
KR1020210037828A
Light emitting device and display device having the same
KR1020240166258A