Spinning disk centripetal coater

The roll-to-roll vacuum coating system with a centripetal spinning disk coater addresses the overheating issue in lithium deposition by using a centripetal spinning disk to apply molten lithium, ensuring uniform and efficient coating without overheating the substrate.

WO2024233688A1PCT designated stage expired Publication Date: 2024-11-14APPLIED MATERIALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/028408
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Current deposition techniques for thin lithium coatings on battery anodes, such as thermal evaporation, often cause substrates like copper or graphite to overheat due to thermal radiation and high latent heat of vaporization, leading to non-uniform coatings and potential damage.

Method used

A roll-to-roll vacuum coating system incorporating a centripetal spinning disk coater that rotates at an angular velocity, feeding molten lithium or other metals onto its surface, allowing for a second layer deposition with controlled fluid droplet size and distribution, reducing thermal load on the substrate.

Benefits of technology

This method enables uniform deposition of thicker lithium layers with reduced substrate temperature, preventing overheating and enhancing processing efficiency while maintaining coating quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024028408_14112024_PF_FP_ABST
    Figure US2024028408_14112024_PF_FP_ABST
Patent Text Reader

Abstract

In one aspect, a roll-to-roll vacuum coating system is provided and includes a substrate, an evaporation assembly, and a centripetal coater assembly. The centripetal coater assembly includes one or more centripetal coaters configured to rotate along a center axis at an angular velocity. The one or more centripetal coaters include a diameter, an upper surface, and a fluid feed line having a fluid feed rate at which a fluid (e.g., molten metal) is deposited on the upper surface.
Need to check novelty before this filing date? Find Prior Art

Description

SPINNING DISK CENTRIPETAL COATERBACKGROUNDField

[0001] The present disclosure generally relates to a roll-to-roll vacuum coating system with a centripetal coating assembly for a deposition process. More particularly, the present disclosure generally relates to a centripetal coating assembly design and methods, which provide a uniform deposition layer.Description of the Related Art

[0002] For making anodes for batteries, such as lithium ion batteries, the deposition of thin coatings of lithium is required. However, suitable anode substrates (e.g., copper, graphite, silicon, or combination thereof) may overheat from current techniques used for deposition of these thin coatings. Such techniques include sputtering, thermal evaporation, and plating. Thermal evaporation for such coating thicknesses can very easily overheat the substrate from thermal radiation coming off of the evaporator as well as from the latent heat of vaporization (e.g., 145.92 kJ / mol for lithium, compared to a latent heat of fusion of only 3 kJ / mol).

[0003] Thus, there is a need for methods and systems for reducing the thermal load on substrates during deposition processes.SUMMARY

[0004] In one aspect, a roll-to-roll vacuum coating system is provided. The roll-to-roll vacuum coating system includes a substrate, an evaporation assembly, and a centripetal coater assembly. The centripetal coater assembly includes one or more centripetal coaters configured to rotate along a center axis at an angular velocity. The one or more centripetal coaters include adiameter, an upper surface, and a fluid feed line having a fluid feed rate at which a fluid is deposited on the upper surface. The fluid includes a molten metal.

[0005] In another aspect, a method for depositing material on a substrate in a rol l-to-roll vacuum system is provided. The method includes depositing a first layer on a substrate via an evaporation assembly and depositing a second layer over the first layer via a centripetal spinning disk coater where the depositing a second layer includes rotating a disk while feeding a molten fluid to an upper surface of the disk.

[0006] In yet another aspect, a method for depositing material on a substrate in a roll-to-roll vacuum system is provided. The method includes depositing a first layer on a substrate via an evaporation assembly, flowing molten lithium over an upper surface of a centripetal spinning disk through a fluid feed line; rotating the centripetal spinning disk at an angular velocity, and depositing a second layer over the first layer via the centripetal spinning disk, the second layer having a thickness greater than a thickness of the first layer.BRIEF DESCRIPTION OF THE DRAWINGS

[0007] So that the manner in which the above-recited features of the present disclosure can be understood in detail, a more particular description of the implementations, briefly summarized above, may be had by reference to implementations, some of which are illustrated in the appended drawings. It is to be noted, however, that the appended drawings illustrate only typical implementations of this disclosure and are therefore not to be considered limiting of its scope, for the disclosure may admit to other equally effective implementations.

[0008] FIG. 1 illustrates a schematic side view of an evaporation system having an evaporation assembly and a centripetal coater assembly according to one or more embodiments.

[0009] FIG. 2A illustrates a schematic top view of a centripetal coater according to one or more embodiments.

[0010] FIG. 2B illustrates a schematic top view of a centripetal coater assembly according to one or more embodiments.

[0011] FIG. 3 illustrates a top view of atomized fluid droplets according to one or more embodiments.

[0012] FIG. 4 illustrates a schematic block diagram view of a method of processing substrates according to one or more embodiments.

[0013] FIG. 5 illustrates a schematic block diagram view of a method of processing substrates according to one or more embodiments.

[0014] To facilitate understanding, identical reference numerals have been used, where possible, to designate identical elements that are common to the figures. It is contemplated that elements and features of one implementation may be beneficially incorporated in other implementations without further recitation.DETAILED DESCRIPTION

[0015] Reference will now be made in detail to the various implementations of the present disclosure, one or more examples of which are illustrated in the figures. Within the following description of the drawings, the same reference numbers refer to the same components. Generally, only the differences with respect to individual implementations are described. Each example is provided by way of explanation of the present disclosure and is not meant as a limitation of the present disclosure. Further, features illustrated or described as part of one implementation can be used on or in conjunction with other implementations to yield yet a further implementation. It is intended that the description includes such modifications and variations.

[0016] Many of the details, dimensions, angles and other features shown in the Figures are merely illustrative of particular implementations. Accordingly, other implementations can have other details, components, dimensions, angles and features without departing from the spirit or scope of the present disclosure.In addition, further implementations of the disclosure can be practiced without several of the details described below.

[0017] FIG. 1 illustrates a schematic side view of an evaporation system having one or more evaporation assemblies 140a-140b and one or more centripetal coater assemblies 150 according to one or more embodiments. The evaporation system 100 can be a roll-to-roll system adapted for depositing coatings on web materials, for example, for depositing metal containing film stacks according to the implementations described herein. In one example, the evaporation system 100 can be used for depositing metals or metal alloys. For example, the evaporation system 100 and evaporation assemblies 140 can be used for depositing elemental metals, metal alloys, and / or other elements. Examples of metal elements, metal alloys, and other elements can be or include alkali metals (e.g., lithium or sodium), alkaline earth metals (e.g., magnesium or beryllium), selenium, zinc, cadmium, aluminum, gallium, indium, thallium, tin, lead, antimony, bismuth, and tellurium, silver, alloys thereof, or any combination thereof. These metals or metal alloys can be used for manufacturing energy storage devices, and particularly for film stacks for lithium-containing anode structures. The evaporation system 100 includes a chamber body 102 that defines a common processing environment 104 in which some or all of the processing actions for depositing coatings on web materials can be performed. In one example, the common processing environment 104 is operable as a vacuum environment. In another example, the common processing environment 104 is operable as an inert gas environment. In some examples, the common processing environment 104 can be maintained at a process pressure of about 1 x 10’3mbar or less, for example, about 1 x 10’4mbar or less.

[0018] The evaporation system 100 is constituted as a roll-to-roll system including an unwinding reel 106 for supplying a continuous flexible substrate 108 or web, a coating drum 110 over which the continuous flexible substrate 108 is processed, and a winding reel 112 for collecting the continuous flexible substrate 108 after processing. The coating drum 110 includes a depositionsurface 111 over which the continuous flexible substrate 108 travels while material is deposited onto the continuous flexible substrate 108. The evaporation system 100 can further include one or more auxiliary transfer reels 114, 116 positioned between the unwinding reel 106, the coating drum 110, and the winding reel 112. According to one aspect, at least one of the one or more auxiliary transfer reels 114, 116, the unwinding reel 106, the coating drum 110, and the winding reel 112, can be driven and rotated by a motor. In one example, the motor is a stepper motor. Although the unwinding reel 106, the coating drum 110, and the winding reel 112 are shown as positioned in the common processing environment 104, it should be understood that the unwinding reel 106 and the winding reel 112 can be positioned in separate chambers or modules, for example, at least one of the unwinding reel 106 can be positioned in an unwinding module, the coating drum 110 can be positioned in a processing module, and the winding reel 112 can be positioned in an unwinding module.

[0019] The unwinding reel 106, the coating drum 110, and the winding reel 112 can be individually temperature controlled. For example, the unwinding reel 106, the coating drum 110, and the winding reel 112 can be individually heated using an internal heat source positioned within each reel or an external heat source.

[0020] In one implementation, which can be combined with other implementations, the one or more evaporation assemblies 140, for example, thermal evaporators, can be removably coupled with an evaporation shield (not shown). In another implementation, which can be combined with other implementations, the one or more evaporation assemblies 140 can be spaced apart from the coating drum 110. The one or more thermal evaporation assemblies 140 and the one or more centripetal coater assemblies 150 are positioned to deliver evaporated material onto the continuous flexible substrate 108 as the continuous flexible substrate 108 travels over the deposition surface 111 of the coating drum 110.

[0021] A deposition volume 120 is defined in between the one or more thermal evaporation assemblies 140, the one or more centripetal coater assemblies 150, and the deposition surface 111 of the coating drum 110. In some implementations, the deposition volume 120 provides an isolated processing within the common processing environment 104 of the chamber body 102. The deposition volume 120 can be minimized and defined to conform to a web, for example, the continuous flexible substrate 108 that is wound on a cylindrical cooling drum, for example, the coating drum 110, a planar cooling plate, or in a free span orientation.

[0022] In one or more embodiments a separation partition (not shown) is situated between the one or more evaporation assemblies 140 and the one or more centripetal coater assemblies 150, such that the deposition volume 120 is split into two separate volumes. In one or more embodiments, the separation partition (not shown) does not fully split the deposition volume 120 into two separate volumes.

[0023] The one or more evaporation assemblies 140 and the one or more centripetal coater assemblies 150 are positioned to perform one or more processing operations to the continuous flexible substrate 108 or web of material. In one example, as depicted in FIG. 1 , the one or more thermal evaporation assemblies 140 and the one or more centripetal coaters 150 are radially disposed about the coating drum 110. In addition, arrangements other than radial are contemplated. In one implementation which can be combined with other implementations, the one or more thermal evaporation assemblies 140 and the one or more centripetal coater assemblies 150 include a lithium (Li) source. Further, the one or more thermal evaporation assemblies 140 and the one or more centripetal coater assemblies 150 can also include a source of an alloy of two or more metals. The material to be deposited can be evaporated, for example, by thermal evaporation techniques.

[0024] In operation, the one or more thermal evaporation assemblies 140 emit a plume of evaporated material 122, which is drawn to the continuous flexible substrate 108 where a thin film (e.g. less than or about 1 pm thick, suchas a thickness in the range of about 100 nm to about 500 nm thick) of deposited material is formed on the continuous flexible substrate 108.

[0025] In addition, although two thermal evaporation assemblies 140a-140b are shown in FIG. 1 , it should be understood that any number of evaporation assemblies 140 can be used. In addition, although one centripetal coater assembly 150 is shown in FIG. 1 , it should be understood that any number of centripetal coater assemblies 150 can be used. In addition, the evaporation system 100 can further include one or more additional deposition sources. For example, the one or more deposition sources as described herein include an electron beam source and additional sources, which can be selected from the group of CVD sources, PECVD sources, and various PVD sources. Exemplary PVD sources include sputtering sources, electron beam evaporation sources, and thermal evaporation sources. In addition, these additional deposition sources can be positioned radially relative to the deposition surface 111 of the coating drum 110.

[0026] In one implementation of the present disclosure which can be combined with other implementations, the evaporation system 100 is configured to process both sides of the continuous flexible substrate 108. For example, additional evaporation assemblies similar to the one or more thermal evaporation assemblies 140 and additional centripetal coater assemblies, such as centripetal coater assembly 150 can be positioned to process the opposing side of the continuous flexible substrate 108. Although the evaporation system 100 is configured to process the continuous flexible substrate 108, which is horizontally oriented, the evaporation system 100 can be configured to process substrates positioned in different orientations, for example, the continuous flexible substrate 108 can be vertically oriented. In one implementation of the present disclosure which can be combined with other implementations, the continuous flexible substrate 108 is a flexible conductive substrate. In one implementation of the present disclosure which can be combined with other implementations, the continuous flexible substrate 108 includes a conductive substrate with one or more layers formed thereon. In one implementation ofthe present disclosure which can be combined with other implementations, the conductive substrate is a copper substrate.

[0027] The evaporation system 100 further includes a gas panel 160. The gas panel 160 uses one or more conduits (not shown) to deliver processing gases to the evaporation system 100. The gas panel 160 can include mass flow controllers and shut-off valves, to control gas pressure and flow rate for each individual gas supplied to the evaporation system 100. Examples of gases that can be delivered by the gas panel 160 include, but are not limited to, inert gases for pressure control (e.g., argon), etching chemistries including but not limited to diketones used for in-situ cleaning of the evaporation system 100, and deposition chemistries including but not limited to 1 , 1 ,1 ,2- Tetrafluoroethane or other hydrofluorocarbons and trimethylaluminum, titanium tetrachloride, or other metal organic precursors used for in-situ tens of nanometer thick reactive lithium mixed conductor surface modification.

[0028] The evaporation system 100 further includes a system controller 170 operable to control various aspects of the evaporation system 100. The system controller 170 facilitates the control and automation of the evaporation system 100 and can include a central processing unit (CPU), memory, and support circuits (or I / O). Software instructions and data can be coded and stored within the memory for instructing the CPU. The system controller 170 can communicate with one or more of the components of evaporation system 100 via, for example, a system bus. A program (or computer instructions) readable by the system controller 170 determines which tasks are performable on a substrate. In some aspects, the program is software readable by the system controller 170, which can include code for monitoring chamber conditions, including independent temperature control of the one or more evaporation assemblies 140 and the one or more centripetal coating assemblies 150. Although only a single system controller, the system controller 170 is shown, it should be appreciated that multiple system controllers can be used with the aspects described herein.

[0029] FIG. 2A illustrates a schematic top view of a centripetal coater assembly 150a according to one or more embodiments. The centripetal coater assembly 150a can be used in place of the centripetal coater assembly 150 depicted in FIG. 1.

[0030] The centripetal coater assembly 150a includes a centripetal coater 152, a fluid feed line 202, and a rotation 204. The centripetal coater 152 includes an upper surface 206. Although a single centripetal coater 152 is shown in FIG. 2A, it is contemplated that two or more centripetal coaters 152 may be utilized, as shown in FIG. 2B. The centripetal coater 152 is configured to rotate with rotation 204 while the fluid feed line 202 releases one or more fluids (e.g., molten lithium) onto the upper surface 206 of the centripetal coater 152. Exemplary fluid can be or include molten metals, molten elements, and / or molten compounds, such as lithium, aluminum, zinc, sodium, magnesium, silver, indium, alloys thereof, dopants thereof, or any combination there. In some examples, the fluid can be or include molten metals, molten elements, and / or molten compounds with a melting point of less than 1 ,000 degrees Celsius. As the centripetal coater 152 rotates with rotation 204, atomized fluid (e.g., atomized molten lithium) is released from the upper surface 206 of the centripetal coater 152 along deposition paths 208a-208c onto a first surface 210 of the substrate 108 in order to deposit a deposition layer (not shown). In one or more embodiments, the deposition layer (not shown) may be greater than about 1 pm, such as from about 1 pm to about 3 pm, from about 4 pm to about 6 pm, from about 7 pm to about 10 pm, or from about 10 pm to about 20 pm.

[0031] In one or more embodiments, the fluid feed line 202 is movably situated, such that a location of the fluid feed line 202 over the upper surface 206 of the centripetal coater 152 may be changed before and / or during operation. If the fluid feed line 202 is situated too close to an edge of the upper surface 206 of the centripetal coater 152, then globs of fluid (see the description of FIG. 3 below) may be released from the upper surface 206 of the centripetal coater 152 resulting in an uneven deposition layer (not shown) on the firstsurface 210 of the substrate 108. Smaller, atomized fluid droplets are desirable for a more uniform deposition layer (not shown) on the first surface 210 of the substrate 108 (e.g., less than 20 pm fluid droplets, such as from about 10 pm to about 20 pm, or such as less than 10 pm).

[0032] Fluid droplet size, d, is a product of the feed rate, Q, of the fluid feed line 202, the surface tension, t, of the fluid, the angular velocity, w, of the rotation 204, and density, p, of the fluid, and the outside radius of the centripetal coater 152, R, where d is proportional to Qt / Rwp.

[0033] In order to control fluid droplet size, a number of factors may be involved including, but no limited to the diameter of the centripetal coater 152, the feed rate of the fluid feed line 202, and the angular velocity of the rotation 204. Thus, it is contemplated that the diameter of the centripetal coater may be changed or adjusted in order to obtain desired fluid droplet size (e.g., less than 20 pm fluid droplets, such as from about 10 pm to about 15 pm, such as less than 10 pm). For example, the diameter of the centripetal coater may be from about 15 mm to about 300 mm, such as from about 50 mm to about 200 mm, such as from about 200 mm to about 300 mm. The feed rate of the fluid feed line 202 and the speed of the rotation 204 may be adjusted before and / or during operation. The feed rate of the fluid feed line 202 may be designed to match the amount of fluid (e.g., molten lithium) consumed by the fluid released from the upper surface 206 of the centripetal coater 152. In one or more embodiments, fluid released form the upper surface 206 of the centripetal coater 152 which is not incident on the first surface 210 of the substrate 108 is collected and returned to the fluid feed line 202.

[0034] In one or more embodiments, the system controller 170 is coupled to the fluid feed line 202 and controls the feed rate of the fluid feed line 202 before and / or during operation. The system controller may also be configured to control the angular velocity of the rotation 204 before and / or during operation. In one or more embodiments, the rotation 204 is as high as 10,000 rotations per minute (rpm), such as from about 5,000 rpm to about 10,000 rpm, such as from about 7,000 rpm to about 10,000 rpm. In one or more embodiments, thesystem controller 170 is configured to control a motor (not shown), where the motor is configured to rotate the centripetal coater 152 at rotation 204. The motor may be any suitable motor, such as an electric motor. In one or more embodiments, the motor is located in atmosphere and a vacuum to atmosphere rotary feedthrough is utilized to bring the rotary motion into the vacuum. All components of the motor, such as pulleys and / or drive belts may be poor conductors of heat such that the motor does not overheat.

[0035] FIG. 2B illustrates a schematic top view of a centripetal coater assembly 150b according to one or more embodiments. The centripetal coater assembly 150b can be used in place of the centripetal coater assembly 150 depicted in FIG. 1.

[0036] The centripetal coater assembly 150b includes one or more centripetal coaters 152a-152d, one or more fluid feed lines 202a-202d, and one or more rotations 204a-204d, respectively. The one or more centripetal coaters 152 include one or more upper surfaces 206a-206d, respectively. Although four centripetal coaters 152 are shown in FIG. 2A, it is contemplated that any number of centripetal coaters 152 may be utilized. The one or more centripetal coaters 152 are configured to rotate with rotation 204 while the one or more fluid feeds line 202 release one or more fluids (e.g., molten lithium) onto the one or more upper surfaces 206 of the one or more centripetal coaters 152. Exemplary fluid can be or include molten metals, molten elements, and / or molten compounds, such as lithium, aluminum, zinc, sodium, magnesium, silver, indium, alloys thereof, dopants thereof, or any combination there. In some examples, the fluid can be or include molten metals, molten elements, and / or molten compounds with a melting point of less than 1 ,000 degrees Celsius. As the one or more centripetal coaters 152 rotate with one or more rotations 204, respectively, atomized fluid (e.g., atomized molten lithium) is released from the one or more upper surfaces 206 of the centripetal coater 152 along deposition paths (not shown) onto the first surface 210 of the substrate 108 in order to deposit a deposition layer (not shown). In one or more embodiments, the deposition layer (not shown) may be greater than or about 1pm, such as from about 1 pm to about 3 pm, from about 4 pm to about 6 pm, from about 7 pm to about 10 pm, or from about 10 pm to about 20 pm.

[0037] As shown in FIG. 2B, the rotations 204a and 204c are clockwise and the rotations 204b and 204d are counterclockwise, such that the rotations 204 alternate direction in order to achieve a uniform deposition. It is contemplated that the directions of the rotations 204 may be changed before and / or during operation in order to achieve a desired deposition pattern.

[0038] In one or more embodiments, the one or more fluid feed lines 202 are movably situated, such that a location of the one or more fluid feed lines 202 over the one or more respective upper surfaces 206 of the one or more respective centripetal coaters 152 may be changed before and / or during operation. If the one or more fluid feed lines 202 are situated too close to an edge of the one or more respective upper surfaces 206 of the one or more respective centripetal coaters 152, then globs of fluid (see the description of FIG. 3 below) may be released from the one or more upper surfaces 206 of the one or more respective centripetal coaters 152 resulting in an uneven deposition layer (not shown) on the first surface 210 of the substrate 108. Smaller, atomized fluid droplets are desirable for a more uniform deposition layer (not shown) on the first surface 210 of the substrate 108.

[0039] For coating with two or more centripetal coaters 152, the uniformity of the deposited layer is proportional to 1 / Rtotai, or 1 / Ri + I / R2+ ... + 1 / Rfinai (see FIG. 2B). The density of the fluid droplets at each point on the first surface 210 of the substrate 108 are inversely proportional to the respective radius (e.g., R1 or R2). The uniformity profile of the deposited layer (not shown) on the first surface 210 of the substrate 108 is shown in FIG. 2B. As shown, the deposition rate of the inner two centripetal coaters 152b and 152c is faster than the deposition rate of the outer two centripetal coaters 152a and 152d due to a larger exposed area of the first surface 210 of the substrate 108 in contact with the released fluid from the upper surfaces 206b and 206c. As shown, inner deposition layers 214 are thicker than outer deposition layers 212. In order to achieve a more uniform coating, a blocking shield 214 may be situated betweenthe two inner centripetal coaters 152b and 152c in order to lower the exposed area of the first surface 210 of the substrate 108 in contact with the released fluid from the upper surfaces 206b and 206c. In one or more embodiments, the blocking shield 214 may contain or include one or more metals or metal alloys (e.g., stainless steel, tungsten, tantalum, or other refractory metals).

[0040] In order to control fluid droplet size, a number of factors may be involved including, but no limited to the diameters of the one or more centripetal coaters 152, the respective feed rates of the one or more fluid feed lines 202, and the angular velocities of the one or more respective rotations 204. Thus, it is contemplated that the diameters of the one or more centripetal coaters may be changed or adjusted in order to obtain desired fluid droplet size (e.g., about 10 pm to about 15 pm). In one or more embodiments, the diameters of the one or more centripetal coaters 152 may be the same. In another embodiment, the diameters of the one or more centripetal coaters 152 may be different. The respective feed rates of the one or more fluid feed lines 202 and the angular velocities of the rotations 204 may be adjusted before and / or during operation. The respective feed rates of the one or more fluid feed lines 202 may be designed to match the amount of fluid (e.g., molten lithium) consumed by the fluid released from the one or more upper surfaces 206 of the one or more centripetal coaters 152. In one or more embodiments, fluid released from the one or more upper surfaces 206 of the one or more centripetal coaters 152 which is not incident on the first surface 210 of the substrate 108 is collected in a catch basin (not shown), flown into a collection reservoir (not shown), and returned to the respective one or more fluid feed lines 202.

[0041] In one or more embodiments, the system controller 170 is coupled to the one or more fluid feed lines 202 and controls the respective feed rates of the one or more fluid feed lines 202 before and / or during operation. In one or more embodiments, the respective fluid feed rates of the one or more fluid feed lines 202 may be the same. In other embodiments, the respective fluid feed rates of the one or more fluid feed lines 202 may be different. The system controller may also be configured to control the angular velocity of the rotations204 before and / or during operation. In one or more embodiments, the rotations 204 are as high as 10,000 rotations per minute (rpm), such as from about 5,000 rpm to about 10,000 rpm, such as from about 7,000 rpm to about 10,000 rpm. In one or more embodiments, the system controller 170 is configured to control one or more motors (not shown), where the one or more motors are configured to rotate the one or more centripetal coaters 152 at rotations 204. The motor may be any suitable motor, such as an electric motor. In one or more embodiments, the motor is located in atmosphere and a vacuum to atmosphere rotary feedthrough is utilized to bring the rotary motion into the vacuum. All components of the motor, such as pulleys and / or drive belts may be poor conductors of heat such that the motor does not overheat. In one or more embodiments, a single motor is utilized in conjunction with gears (not shown) in order to obtain a singular angular velocity from the rotations 204 in order to obtain a uniform coating. In one or more embodiments, two or more motors, such as four motors, are utilized with synchronous motor control in order to obtain a singular angular velocity from the rotations 204 in order to obtain a uniform coating. It is contemplated that the respective angular velocities of the rotations 204 may be different in order to achieve desired deposition patterns.

[0042] FIG. 3 illustrates a top view of atomized fluid droplets 304 according to one or more embodiments. Ligaments 302 extend beyond the plane of the upper surface 206 (not shown) of the centripetal coater 152 (not shown) as the centripetal coater 152 rotates with rotation 204 (not shown). Atomized fluid droplets 304 of a desired size (e.g., about 10 pm) are released from ligaments 302 and contact and coat the first surface 210 of the substrate 208 (not shown). Undesirable globs 306 may form in a number of situations, which will result in a non-uniform deposition pattern (e.g., location of fluid feed lines 202 are not in desirable locations and / or angular velocity of the centripetal coater 152 is too slow (and the molten material does not atomize) or too fast (and the droplets are too small).

[0043] FIG. 4 illustrates a schematic block diagram view of a method 400 of processing substrates according to one or more embodiments. Operation 402includes depositing a first layer on a substrate via an evaporation assembly. Operation 404 includes depositing a second layer over the first layer via a centripetal spinning disk coater. Depositing the second layer over the first layer includes rotating the centripetal spinning disk coater while feeding one or more molten fluids (e.g., molten lithium) to an upper surface of the centripetal spinning disk coater. Exemplary fluid can be or include molten metals, molten elements, and / or molten compounds, such as lithium, aluminum, zinc, sodium, magnesium, silver, indium, alloys thereof, dopants thereof, or any combination there. In some examples, the fluid can be or include molten metals, molten elements, and / or molten compounds with a melting point of less than 1 ,000 degrees Celsius.

[0044] FIG. 5 illustrates a schematic block diagram view of a method 500 of processing substrates according to one or more embodiments. Operation 502 includes depositing a first layer on a substrate via an evaporation assembly. Operation 504 includes flowing a molten lithium over an upper surface of a centripetal spinning disk. Operation 506 includes rotating the centripetal spinning disk at an angular velocity. Operation 508 includes depositing a second layer over the first layer via the centripetal spinning disk. The second layer may be thicker than the first layer.

[0045] Implementations can include one or more of the following potential advantages. The use of thermal evaporators for an initial pre-l ith iation allow for the centripetal coater assembly to wet out on the substrate and not bead up. Such beading would cause a non-uniform coating. Furthermore, the use of a centripetal coater for the thicker (e.g., greater than 1 pm thick, such as in the range of about 1 pm to about 10 pm thick) film rather than thermal evaporation allows for a much lower temperature for the substrate to the lower latent heat of fusion compared to the higher latent heat of vaporization (e.g., for lithium the latent heat of fusion is 3 kJ / mol and the latent heat of vaporization is 145.92 kJ / mol). These advantages may lead to a more uniform coating as well as the ability to process the substrate more quickly without overheating the substrate.

[0046] Implementations and all of the functional operations described in this specification can be implemented in digital electronic circuitry, or in computer software, firmware, or hardware, including the structural means disclosed in this specification and structural equivalents thereof, or in combinations of them. Implementations described herein can be implemented as one or more non- transitory computer program products, e.g., one or more computer programs tangibly embodied in a machine readable storage device, for execution by, or to control the operation of, data processing apparatus, e.g., a programmable processor, a computer, or multiple processors or computers.

[0047] The processes and logic flows described in this specification can be performed by one or more programmable processors executing one or more computer programs to perform functions by operating on input data and generating output. The processes and logic flows can also be performed by, and apparatus can also be implemented as, special purpose logic circuitry, e.g., an FPGA (field programmable gate array) or an ASIC (application specific integrated circuit).

[0048] The term "data processing apparatus" encompasses all apparatus, devices, and machines for processing data, including by way of example a programmable processor, a computer, or multiple processors or computers. The apparatus can include, in addition to hardware, code that creates an execution environment for the computer program in question, e.g., code that constitutes processor firmware, a protocol stack, a database management system, an operating system, or a combination of one or more of them. Processors suitable for the execution of a computer program include, by way of example, both general and special purpose microprocessors, and any one or more processors of any kind of digital computer.

[0049] Computer readable media suitable for storing computer program instructions and data include all forms of nonvolatile memory, media and memory devices, including by way of example semiconductor memory devices, e.g., EPROM, EEPROM, and flash memory devices; magnetic disks, e.g., internal hard disks or removable disks; magneto optical disks; and CD ROMand DVD-ROM disks. The processor and the memory can be supplemented by, or incorporated in, special purpose logic circuitry.

[0050] When introducing elements of the present disclosure or exemplary aspects or implementation(s) thereof, the articles “a,” “an,” “the” and “said” are intended to mean that there are one or more of the elements.

[0051] The terms “comprising,” “including” and “having” are intended to be inclusive and mean that there may be additional elements other than the listed elements.

[0052] While the foregoing is directed to implementations of the present disclosure, other and further implementations of the disclosure may be devised without departing from the basic scope thereof, and the scope thereof is determined by the claims that follow.

Claims

ClaimsWhat is claimed is:1 . A roll-to-roll vacuum coating system, comprising: a substrate; an evaporation assembly; and a centripetal coater assembly, the centripetal coater assembly including one or more centripetal coaters configured to rotate along a center axis at an angular velocity, the one or more centripetal coaters comprising: a diameter; an upper surface; and a fluid feed line having a fluid feed rate at which a fluid is deposited on the upper surface, the fluid comprising a molten metal.

2. The roll-to-roll vacuum coating system of claim 1 , further comprising one or more blocking shields disposed between the one or more centripetal coaters.

3. The roll-to-roll vacuum coating system of claim 1 , wherein the one or more centripetal coaters contains four centripetal coaters.

4. The roll-to-roll vacuum coating system of claim 1 , wherein the fluid feed line is stationary with respect to the center axis of the centripetal coater.

5. The roll-to-roll vacuum coating system of claim 1 , wherein the fluid feed line is movable with respect to the upper surface.

6. The roll-to-roll vacuum coating system of claim 1 , wherein each of the one or more centripetal coaters independently has a diameter in a range from about 15 mm to about 250 mm.

7. The roll-to-roll vacuum coating system of claim 1 , wherein the angular velocity of the one or more centripetal coaters is in a range from about 90 rpm to about 6,000 rpm.

8. The roll-to-roll vacuum coating system of claim 1 , wherein the fluid feed rate is equal to the volume of the fluid escaping the upper surface of the centripetal coater in a set amount of time.

9. The roll-to-roll vacuum coating system of claim 1 , wherein the fluid is molten lithium, molten sodium, molten aluminum, molten magnesium, molten indium, molten silver, molten alloys thereof, or any combination thereof.

10. A method for depositing material on a substrate in a roll-to-roll vacuum system, comprising: depositing a first layer on a substrate via an evaporation assembly; and depositing a second layer over the first layer via a centripetal spinning disk coater, the depositing a second layer including rotating a disk while feeding a molten fluid to an upper surface of the disk.11 . The method of claim 10, wherein each of the first layer and the second layer independently comprises lithium.

12. The method of claim 10, wherein the first layer has a thickness of less than or equal to 1 pm.

13. The method of claim 10, wherein the second layer has a thickness of greater than or equal to 1 pm.

14. The method of claim 10, wherein the second layer has a uniform deposition of less than or equal to 5%.

15. A method for depositing material on a substrate in a roll-to-roll vacuum system, comprising: depositing a first layer on a substrate via an evaporation assembly; flowing molten lithium over an upper surface of a centripetal spinning disk through a fluid feed line; rotating the centripetal spinning disk at an angular velocity; and depositing a second layer over the first layer via the centripetal spinning disk, the second layer having a thickness greater than a thickness of the first layer.

16. The method of claim 15, wherein the first layer has a thickness of less than or equal to 1 pm.

17. The method of claim 15, wherein the second layer has a thickness of greater than or equal to 1 pm.

18. The method of claim 15, wherein the second layer has a uniform deposition of less than or equal to 5%.

19. The method of claim 15, wherein the first layer has a thickness in a range from about 100 nm to about 500 nm.

20. The method of claim 15, wherein the second layer has a thickness in a range from about 1 pm to about 10 pm.

Citation Information

Patent Citations

  • Metal vapor deposition apparatus

    JP2003239066A

  • Vacuum coating installation and method of producing a coating layer on a substrate

    US20090191327A1

  • Method of making inorganic or inorganic / organic hybrid barrier films

    US20110081502A1

  • Evaporation unit and vacuum coating apparatus

    US20140030435A1

  • Method and apparatus for magnetron sputtering

    WO2016164276A1