Preparation method for composite electrode material and use thereof

By using carbon nanotube templates to prepare LiFePO4/α-Fe2O3 composite materials in lithium-ion batteries, the problems of poor hydrophilicity and low lithium ion diffusion rate in Li-ion batteries are solved, and efficient lithium ion extraction and recovery of Li-ion , improves the production efficiency and current density of the battery.

WO2024234146A1PCT designated stage expired Publication Date: 2024-11-21GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/093901
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In existing lithium-ion batteries, LiFePO4 has poor hydrophilicity and low lithium ion diffusion rate in electrochemical lithium-enhancing working electrodes, resulting in low production efficiency and low current density, making it difficult to efficiently extract lithium under low lithium concentration and low temperature conditions.

Method used

Carbon nanotubes are used as templates, and LiFePO4/α-Fe2O3 composite materials are prepared by sonication, stirring and adsorption and spray drying + laser sintering to increase the hydrophilicity and pore structure of the electrodes, and improve the diffusion rate and current density of lithium ion.

Benefits of technology

The hydrophilicity and adsorption capacity of the electrode are significantly improved, the current density is increased, the lithium extraction rate and the recovery efficiency of lithium ions are improved, and the preparation process consumes less energy, has small grains, and a stable structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023093901_21112024_PF_FP_ABST
    Figure CN2023093901_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure belongs to the technical field of lithium extraction from a salt lake. Disclosed are a preparation method for a composite electrode material by means of electrochemical lithium extraction and the use thereof. The preparation method comprises: mixing carbon nanotubes, sulfuric acid and nitric acid, subjecting same to ultrasonic treatment to obtain pretreated carbon nanotubes, dissolving a trivalent iron salt into a solvent, adding a precipitant and the pretreated carbon nanotubes and stirring same for adsorption, so as to obtain a carbon nanotube precursor, dispersing the carbon nanotube precursor and lithium iron phosphate into the solvent, spraying the obtained suspension by means of a nozzle of a spray dryer, and in addition, arranging a laser beam at the nozzle, and sintering fog drops formed by means of spraying, so as to obtain an LiFePO4 / α-Fe2O3 composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Preparation method and application of composite electrode materials Technical Field

[0001] The present invention belongs to the technical field of lithium extraction from salt lakes, and particularly relates to a preparation method and application of a composite electrode material. Background Art

[0002] Electrochemical lithium extraction is the process of using lithium-ion battery cathode materials to produce Li + The principle of transfer between the solid electrode and the liquid electrolyte is realized. The active materials of the working electrode in the electrochemical lithium extraction system proposed by researchers are mainly olivine structure LiFePO4, spinel structure LiMn2O4, spinel structure LiNi 0.5 Mn 1.5 O4 and layered LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 four categories. LiFePO4 has a typical olivine structure, which can realize the insertion and extraction of lithium ions. LiFePO4 has been widely studied and applied as a positive electrode material in lithium-ion batteries. LiFePO4 has good stability in aqueous solution as a working electrode for electrochemical lithium extraction. For FePO4 formed after delithiation, even in brine with an ultra-high Mg / Li ratio, as long as the battery voltage is properly controlled, lithium ions can be selectively separated from a variety of impurity ions. However, strong covalent oxygen bonds will lead to a low lithium ion diffusion rate, and the hydrophilicity of lithium iron phosphate electrodes is poor, resulting in low current density and low production efficiency during the production process.

[0003] Summary of the Invention

[0004] The present disclosure aims to at least solve the technical problems existing in the above-mentioned prior art. To this end, the present disclosure proposes a preparation method and application of a composite electrode material, which can improve the hydrophilicity and adsorption capacity of the electrochemical lithium extraction electrode material, increase the current density, and thus increase the lithium extraction rate.

[0005] According to one aspect of the present disclosure, a method for preparing an electrochemical lithium extraction composite electrode material is proposed, comprising the following steps:

[0006] S1: mixing carbon nanotubes, sulfuric acid and nitric acid, performing ultrasonic treatment, solid-liquid separation and washing to obtain pretreated carbon nanotubes;

[0007] S2: dissolving a trivalent iron salt in a first solvent, adding a precipitant and mixing, then adding the pretreated carbon nanotubes and stirring and adsorbing them, performing solid-liquid separation, and washing the obtained solid to obtain a carbon nanotube precursor;

[0008] S3: dispersing the carbon nanotube precursor and lithium iron phosphate in a second solvent to obtain a suspension;

[0009] S4: spraying the suspension through a nozzle of a spray dryer, and setting a laser beam at the nozzle to sinter the droplets formed by the spray, thereby obtaining a LiFePO4 / α-Fe2O3 composite material.

[0010] In some embodiments of the present disclosure, the content of α-Fe2O3 in the LiFePO4 / α-Fe2O3 composite material is 1 wt%-2.5 wt% of the content of LiFePO4.

[0011] In some embodiments of the present disclosure, in step S1, the carbon nanotubes are multi-walled carbon nanotubes with a tube diameter of 50-150 nm.

[0012] In some embodiments of the present disclosure, in step S1, the concentration of the sulfuric acid is 1-5 mol / L, the concentration of the nitric acid is 1-6 mol / L, and the solid-liquid ratio of the carbon nanotubes, sulfuric acid and nitric acid is 1 g: (50-200) mL: (50-200) mL.

[0013] In some embodiments of the present disclosure, in step S2, the trivalent iron salt is at least one of ferric nitrate or ferric chloride.

[0014] In some embodiments of the present disclosure, in step S2, the solid-liquid ratio of the trivalent iron salt to the first solvent is (0.01-1) mol:1L.

[0015] In some embodiments of the present disclosure, in step S2, the first solvent is a mixed solution of water and ethanol in a volume ratio of (1-3):1. The addition of ethanol can disrupt the hydrogen bonding between water molecules or the cohesive force between molecules, thereby reducing the surface tension between the particle surface and the solvent, enhancing the wettability between the particles and the solvent, and ethanol helps the solution penetrate into the carbon nanotubes, thereby promoting ion transport in the carbon nanotubes.

[0016] In some embodiments of the present disclosure, in step S2, the temperature of the stirring adsorption is 35-55° C., and the time is 4-10 h.

[0017] In some embodiments of the present disclosure, in step S2, a drying operation is further included after the washing, and the drying temperature is 70-90° C. and the drying time is 4-8 hours.

[0018] In some embodiments of the present disclosure, in step S2, the solvent used for washing is ethanol.

[0019] In some embodiments of the present disclosure, in step S2, the precipitant is ammonia water or sodium hydroxide. Using ammonia water as a precipitant can form a weak alkaline environment to produce iron hydroxide precipitation, and the reaction formula is as follows: 3NH3·H2O+FeCl3=Fe(OH)3+3NH4Cl.

[0020] In some embodiments of the present disclosure, in step S3, the mass ratio of the carbon nanotube precursor to lithium iron phosphate is (1-1.5):5.

[0021] In some embodiments of the present disclosure, in step S3, the particle size D50 of the lithium iron phosphate is 200-800 nm.

[0022] In some embodiments of the present disclosure, in step S3, the liquid-to-solid ratio of the second solvent to lithium iron phosphate is (1-2) ml:1 g.

[0023] In some embodiments of the present disclosure, in step S3, the second solvent is at least one of water or ethanol.

[0024] In some embodiments of the present disclosure, in step S4, the power of the laser beam is 4-10 kW, and the droplets are heated to 600-800° C. within 0.1-1.5 s.

[0025] In some embodiments of the present disclosure, in step S4, the temperature of the nozzle is 110-180°C.

[0026] In some embodiments of the present disclosure, in step S4, the spot area of ​​the laser beam is 1.2-1.7 times the area of ​​the nozzle spray outlet.

[0027] The present disclosure also provides the use of the LiFePO4 / α-Fe2O3 composite material produced by the preparation method described above in lithium extraction from salt lakes. Specifically, a LiFePO4 / α-Fe2O3 composite electrode is prepared by adding the LiFePO4 / α-Fe2O3 composite material, a conductive agent, and a hydrophilic binder to N-methylpyrrolidone, stirring to form a slurry, coating the resulting slurry on a mesh-shaped conductive current collector, and drying to obtain the LiFePO4 / α-Fe2O3 composite electrode.

[0028] In some embodiments of the present disclosure, the conductive agent is one of carbon black, carbon fiber or graphene.

[0029] In some embodiments of the present disclosure, the hydrophilic binder is one of sodium carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyvinyl alcohol (PVA), acrylonitrile multipolymer (LA132), polybutyl acrylate (PBA) or polyacrylonitrile (PA).

[0030] According to the embodiments of the present disclosure, there are at least the following beneficial effects:

[0031] 1. Carbon nanotubes react in a mixture of sulfuric acid and nitric acid to load carboxyl groups on the surface of carbon nanotubes to obtain carboxylated carbon nanotubes. After adding a precipitant, Fe 3+ It reacts with a precipitant to generate Fe(OH)3, which undergoes an acid-alcohol dehydration reaction with the carboxyl groups on the surface of the carbon nanotubes, thereby loading a layer of oxide precursor coating on the surface of the carbon nanotubes, which is connected by chemical bonds and is not easily detached. The carbon nanotubes loaded with Fe(OH)3 are mixed with lithium iron phosphate and sintered. The carbon nanotubes act as a template and are gradually removed during the sintering process with the release of CO2, creating pores between the lithium iron phosphate particles, thus forming porous lithium iron phosphate. In addition, the Fe(OH)3 loaded on the carbon nanotubes will form corresponding α-Fe2O3 embedded in the pores of the lithium iron phosphate. The mesoporous structure of lithium iron phosphate helps increase the contact area between the electrode and the solution, providing a good channel for the diffusion and mass transfer of the solution within the electrode, improving the permeability of the electrode, effectively improving the mass transfer of the solution within the electrode, and facilitating the diffusion of lithium ions in the electrode.

[0032] 2. The ɑ-Fe2O3 nanonetwork formed in the pores of lithium iron phosphate materials using carbon nanotubes as templates has super hydrophilicity, which can improve the wettability of the microporous surface of lithium iron phosphate, thereby further improving the hydrophilicity of the electrode material and increasing the current density, thereby increasing the rate of lithium extraction from brine under low temperature and low lithium concentration conditions.

[0033] 3. This method uses spray drying + laser sintering, which consumes less energy and has an extremely short sintering time. Laser sintering not only ensures that the carbon nanotubes are removed smoothly, but also avoids oxidation of lithium iron phosphate due to the extremely short sintering time. The prepared LiFePO4 / α-Fe2O3 composite material has fine grains and a stable structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The present disclosure is further described below with reference to the accompanying drawings and embodiments, wherein:

[0035] FIG1 is a graph showing the variation of current density over electrolysis time for the embodiments and comparative examples;

[0036] FIG2 shows the cycling performance of the electrode prepared in Example 1. DETAILED DESCRIPTION

[0037] The following will clearly and completely describe the concept and technical effects of the present disclosure in conjunction with embodiments to fully understand the purpose, features and effects of the present disclosure.

[0038] Example 1

[0039] This embodiment prepares a LiFePO4 / α-Fe2O3 composite electrode material and its electrode, and the specific process is as follows:

[0040] (1) Pretreatment of carbon nanotubes: CNTs, 2.5 mol / L sulfuric acid, and 3 mol / L dilute nitric acid were stirred in a container at a ratio of 1 g:100 mL:100 mL, stirred at 400 rpm, ultrasonically treated for 1 h, filtered under reduced pressure, and washed with deionized water until the pH value was neutral. The product was vacuum dried at 100°C to obtain pretreated CNTs; the CNTs were multi-walled CNTs with a diameter of 100 nm.

[0041] (2) Fe(NO3)3 was dissolved in a water-ethanol mixture with a volume ratio of 2:1 at a solid-liquid ratio of 0.05 mol:1 L, and then ammonia water was added and stirred evenly. Then, pretreated carbon nanotubes were added and stirred and adsorbed in a 45°C water bath for 5 hours. After the adsorption was completed, the carbon nanotubes obtained were filtered and washed with anhydrous ethanol, and dried in an oven at 80°C for 6 hours to obtain a carbon nanotube precursor.

[0042] (3) The carbon nanotube precursor and lithium iron phosphate (particle size D50 is 650 nm) are dispersed in anhydrous ethanol at a mass ratio of 1.25:5 and ultrasonically dispersed. The liquid-solid ratio of anhydrous ethanol to lithium iron phosphate is 1.4 mL:1 g to obtain a suspension.

[0043] (4) The suspension is sprayed out at high pressure through the nozzle of a spray dryer. At the same time, a 7kW laser beam is set at the nozzle. The nozzle temperature is 140°C, the angle between the laser beam and the nozzle is 60°, and the laser spot area is 1.4 times the nozzle spray outlet area. It is heated to 700°C within 1 second. After laser rapid sintering, the LiFePO4 / α-Fe2O3 composite electrode material can be obtained.

[0044] (5) The above-mentioned composite electrode material, carbon fiber and sodium carboxymethyl cellulose are added to N-methyl pyrrolidone in a mass ratio of 88:2:10 and stirred evenly to form a slurry. The slurry is evenly coated on a titanium mesh, first dried at 70°C for 4 hours, and then dried at 100°C for 8 hours to prepare a LiFePO4 / α-Fe2O3 composite electrode for electrochemical lithium extraction.

[0045] The α-Fe2O3 content in the composite electrode material obtained in this example is 1.72 wt% of the LiFePO4 content.

[0046] Example 2

[0047] This embodiment prepares a LiFePO4 / α-Fe2O3 composite electrode material and its electrode, and the specific process is as follows:

[0048] (1) Pretreatment of carbon nanotubes: CNTs, 1 mol / L sulfuric acid, and 1 mol / L dilute nitric acid were stirred in a container at a ratio of 1 g:50 mL:50 mL, stirred at 400 rpm, ultrasonically treated for 1 h, filtered under reduced pressure, and washed with deionized water until the pH value was neutral. The product was vacuum dried at 100°C to obtain pretreated CNTs; the CNTs were multi-walled CNTs with a diameter of 50 nm.

[0049] (2) Fe(NO3)3 was dissolved in a water-ethanol mixture with a volume ratio of 3:1 at a solid-liquid ratio of 0.01 mol:1 L, and then ammonia water was added and stirred evenly. Then, the pretreated carbon nanotubes were added and stirred and adsorbed in a 55°C water bath for 8 hours. After the adsorption was completed, the carbon nanotubes obtained were filtered and washed with anhydrous ethanol, and dried in an oven at 80°C for 4 hours to obtain a carbon nanotube precursor.

[0050] (3) The carbon nanotube precursor and lithium iron phosphate were dispersed in a solvent at a mass ratio of 1:5 and ultrasonically dispersed, and the liquid-solid ratio of anhydrous ethanol to lithium iron phosphate was 1.4 mL:1 g to obtain a suspension.

[0051] (4) The suspension is sprayed out at high pressure through the nozzle of a spray dryer. At the same time, a 10kW laser beam is set at the nozzle. The nozzle temperature is 170°C, the angle between the laser beam and the nozzle is 70°, and the laser spot area is 1.5 times the nozzle spray outlet area. It is heated to 800°C within 1.5 seconds. After laser rapid sintering, the LiFePO4 / α-Fe2O3 composite electrode material can be obtained.

[0052] (5) The above composite electrode material, graphene, and sodium carboxymethyl cellulose are added to N-methyl pyrrolidone in a mass ratio of 88:2:10 and stirred evenly to form a slurry. The slurry is evenly coated on a titanium mesh, first dried at 70°C for 4 hours, and then dried at 100°C for 8 hours to prepare a LiFePO4 / α-Fe2O3 composite electrode for electrochemical lithium extraction.

[0053] The α-Fe2O3 content in the composite electrode material obtained in this example is 1.11 wt% of the LiFePO4 content.

[0054] Example 3

[0055] This embodiment prepares a LiFePO4 / α-Fe2O3 composite electrode material and its electrode, and the specific process is as follows:

[0056] (1) Pretreatment of carbon nanotubes: CNTs, 5 mol / L sulfuric acid, and 6 mol / L dilute nitric acid were stirred in a container at a ratio of 1 g: 200 mL: 200 mL, stirred at 400 rpm, ultrasonically treated for 1 h, filtered under reduced pressure, and washed with deionized water until the pH value was neutral. The product was vacuum dried at 100°C to obtain pretreated CNTs; the CNTs were multi-walled CNTs with a diameter of 150 nm.

[0057] (2) Fe(NO3)3 was dissolved in a water-ethanol mixture with a volume ratio of 1:1 at a solid-liquid ratio of 1 mol:1 L, and then ammonia water was added and stirred evenly. Then, the pretreated carbon nanotubes were added and stirred in a 35°C water bath for 2 hours of adsorption. After the adsorption was completed, the carbon nanotubes obtained were filtered and washed with anhydrous ethanol, and dried in an oven at 80°C for 8 hours to obtain a carbon nanotube precursor.

[0058] (3) The carbon nanotube precursor and lithium iron phosphate were dispersed in a solvent at a mass ratio of 1.5:5 and ultrasonically dispersed, and the liquid-solid ratio of anhydrous ethanol to lithium iron phosphate was 1.4 mL:1 g to obtain a suspension.

[0059] (4) The suspension is sprayed out at high pressure through the nozzle of a spray dryer, and a 4kW laser beam is set at the nozzle. The nozzle temperature is 110°C, the angle between the laser beam and the nozzle is 50°, and the laser spot area is 1.3 times the nozzle spray outlet area. It is heated to 600°C within 0.1s. After laser rapid sintering, the LiFePO4 / α-Fe2O3 composite electrode material can be obtained.

[0060] (5) The above composite electrode material, carbon black and sodium carboxymethyl cellulose were added to N-methyl pyrrolidone in a mass ratio of 88:2:10 and stirred evenly to form a slurry. The slurry was evenly coated on a titanium mesh, first dried at 70°C for 4 hours, and then dried at 100°C for 8 hours to prepare a LiFePO4 / α-Fe2O3 composite electrode for electrochemical lithium extraction.

[0061] The α-Fe2O3 content in the composite electrode material obtained in this example is 2.47 wt% of the LiFePO4 content.

[0062] Comparative Example

[0063] This comparative example prepared an electrode. The difference from Example 1 is that the electrode material used is ordinary lithium iron phosphate. The specific process is as follows:

[0064] The untreated lithium iron phosphate active positive electrode material was directly added to N-methylpyrrolidone with carbon fiber and sodium carboxymethyl cellulose in a mass ratio of 88:2:10 and stirred evenly to form a slurry. The slurry was evenly coated on a titanium mesh, first dried at 70°C for 4 hours and then dried at 100°C for 8 hours to prepare a lithium iron phosphate electrode for electrochemical lithium extraction.

[0065] Performance testing

[0066] Lithium extraction test 1: The prepared lithium iron phosphate electrode was used as the anode and nickel foam was used as the cathode. They were placed in a 20g / L NaCl solution and a 1V voltage was applied across the electrodes until the current density was lower than 0.5A / m 2 , which can be made into delithiated Li 1-x FePO4 electrode. An anion membrane was used to separate the electrolysis apparatus into a cathode chamber and an anode chamber. The prepared lithium iron phosphate electrode and the delithiated lithium iron phosphate electrode were placed in the anode and cathode chambers, respectively. 15 L of brine to be treated, the composition of which is shown in Table 1, was injected into the cathode chamber. 2 L of a 5 g / L NaCl solution was injected into the anode as a supporting electrolyte. A voltage of 0.4 V was applied to the anode and cathode, and electrolysis was performed at 20°C for 4 hours. The compositions of the brine and the lithium-rich anode solution after lithium extraction are shown in Table 2. Figure 1 shows the change in current density with electrolysis time.

[0067] Table 1

[0068] Table 2

[0069] As can be seen from Table 2 and Figure 1, after electrochemical lithium extraction using the electrode prepared in Example 1, the lithium concentration in the brine decreased from 0.49 g / L to 0.05 g / L, and the lithium recovery rate reached 90%. The lithium concentration in the anode lithium-rich solution increased to 3.90 g / L, and its magnesium-lithium ratio decreased from 93 in the brine to 0.22. After the electrolysis, the adsorption capacity of the electrode was 38.59 mg (Li) / g (LiFePO4), and the average current density during the above process was 58.14 A / m 2 The average current density of electrolysis using Example 2 and Example 3 was 55.5A / m 2 and 53.29A / m 2 , the electrode adsorption capacity is 35.54mg(Li) / g(LiFePO4) and 34.04mg(Li) / g(LiFePO4) respectively. From the concentration of brine and the magnesium-lithium ratio after electrochemical lithium extraction in the comparative example, it can be found that the lithium concentration in the brine is reduced from 0.49g / L to 0.16g / L, the electrode adsorption capacity is 15.1mg(Li) / g(LiFePO4), and its average current density is 22.35A / m 2, which is lower than the current density of the same brine treated in the embodiment.

[0070] Lithium Extraction Test 2: The electrolysis apparatus was separated into a cathode and an anode compartment using an anionic membrane. The lithium iron phosphate electrode and the delithiated lithium iron phosphate electrode prepared in Example 1 were placed in the anode and cathode compartments, respectively. 10 L of brine to be treated was injected into the cathode compartment, and 2 L of a 5 g / L NaCl solution was injected into the anode as the supporting electrolyte. A voltage of 0.6 V was applied to the anode and cathode. After 5 hours of electrolysis at 10°C, the compositions of the brine and the lithium-rich anode solution before and after lithium extraction are shown in Table 3.

[0071] Table 3

[0072] As can be seen from Table 3, the lithium concentration in the brine decreased from 1.75g / L to 0.18g / L, and the lithium recovery rate was as high as 92%. The lithium concentration in the lithium-rich solution of the anode increased to 6.88g / L, and its magnesium-lithium ratio decreased from 70 in the brine to 0.18 in the lithium-rich solution. After the electrolysis was completed, the adsorption capacity of the electrode was 35.9mg(Li) / g(LiFePO4), and the average current density during the above process was 46.85A / m 2 .

[0073] Lithium Extraction Test 3: The electrolysis apparatus was separated into a cathode and an anode compartment using an anionic membrane. The lithium iron phosphate electrode and the delithiated lithium iron phosphate electrode prepared in Example 1 were placed in the anode and cathode compartments, respectively. 30 L of brine to be treated was injected into the cathode compartment, and 2 L of a 5 g / L NaCl solution was injected into the anode as a supporting electrolyte. A voltage of 0.8 V was applied to the anode and cathode. After 6 hours of electrolysis at 5°C, the compositions of the brine and the lithium-rich anode solution before and after lithium extraction are shown in Table 4.

[0074] Table 4

[0075] As can be seen from Table 4, the lithium concentration in the brine decreased from 0.24g / L to 0.05g / L. At a lower temperature and in a lower lithium-containing brine, the lithium recovery rate can reach 80%. The adsorption capacity of the electrode after the electrolysis is 28.3mg(Li) / g(LiFePO4). The average current density during the above process is 40.8A / m 2 .

[0076] Electrode cycle performance test: After the above-mentioned lithium extraction test of the electrode of Example 1 is completed, the cathode and anode are swapped, 15L of NaCl solution with a concentration of 5g / L is injected into the anode as the supporting electrolyte, and 30L of the above-mentioned fresh brine is injected into the cathode. A voltage of 0.4V is applied to the anode and anode, and electrolysis is carried out at 20°C. After each electrolysis cycle, the cathode and anode are swapped, and the lithium-containing anode liquid of the previous cycle continues to be used as the anode liquid of the next cycle. The cathode liquid is replaced with 30L of fresh brine each time, and lithium extraction is carried out under the same conditions. The cycle performance of the electrode and the effect of lithium enrichment are examined. The results are shown in Figure 2. As can be seen from Figure 2, the lithium iron phosphate electrode prepared in Example 1 has excellent cycle performance, and the degree of lithium enrichment is high during the cycle process.

Claims

1. A method for preparing a composite electrode material, characterized in that: The following steps are involved: S1: mixing carbon nanotubes, sulfuric acid and nitric acid, subjecting the mixture to ultrasonic treatment, solid-liquid separation and water washing to obtain pretreated carbon nanotubes; S2: dissolving the trivalent iron salt in the first solvent, adding a precipitant and mixing, then adding the pretreated carbon nanotubes to perform stirring adsorption, solid-liquid separation, and washing the obtained solid to obtain a carbon nanotube precursor; S3: dispersing the carbon nanotube precursor and lithium iron phosphate in a second solvent to obtain a suspension; S4: spraying the suspension through a nozzle of a spray dryer, and setting a laser beam at the nozzle to sinter the droplets formed by the spray, so as to obtain a LiFePO4 / α-Fe2O3 composite material.

2. The preparation method according to claim 1, characterized in that: The content of α-Fe2O3 in the composite material is 1wt%-2.5wt% of the content of LiFePO4.

3. The preparation method according to claim 1, characterized in that: In step S1, the carbon nanotubes are multi-walled carbon nanotubes with a tube diameter of 50-150 nm.

4. The preparation method according to claim 1, characterized in that: In step S1, the concentration of the sulfuric acid is 1-5 mol / L, the concentration of the nitric acid is 1-6 mol / L, and the solid-liquid ratio of the carbon nanotubes, sulfuric acid and nitric acid is 1 g: (50-200) mL: (50-200) mL.

5. The preparation method according to claim 1, characterized in that: In step S2, the trivalent iron salt is at least one of ferric nitrate or ferric chloride.

6. The preparation method according to claim 1, characterized in that: In step S2, the solid-liquid ratio of the trivalent iron salt to the first solvent is (0.01-1) mol:1L.

7. The preparation method according to claim 1, characterized in that: In step S2, the first solvent is a mixed solution of water and ethanol in a volume ratio of (1-3):

1.

8. The preparation method according to claim 1, characterized in that: In step S2, the temperature of the stirring adsorption is 35-55°C and the time is 4-10 hours.

9. The preparation method according to claim 1, characterized in that: In step S2, a drying operation is further included after the washing, the drying temperature is 70-90° C., and the drying time is 4-8 hours.

10. The preparation method according to claim 1, characterized in that: In step S2, the solvent used for washing is ethanol.

11. The preparation method according to claim 1, characterized in that: In step S2, the precipitant is urea.

12. The preparation method according to claim 1, characterized in that: In step S3, the mass ratio of the carbon nanotube precursor to lithium iron phosphate is (1-1.5):

5.

13. The preparation method according to claim 1, characterized in that: In step S3, the particle size D50 of the lithium iron phosphate is 200-800 nm.

14. The preparation method according to claim 1, characterized in that: In step S3, the liquid-to-solid ratio of the second solvent to lithium iron phosphate is (1-2) ml:1 g.

15. The preparation method according to claim 1, characterized in that: In step S3, the second solvent is at least one of water or ethanol.

16. The preparation method according to claim 1, characterized in that: In step S4, the power of the laser beam is 4-10 kW, and the droplets are heated to 600-800° C. within 0.1-1.5 s.

17. The preparation method according to claim 1, characterized in that: In step S4, the temperature of the nozzle is 110-180°C.

18. The preparation method according to claim 1, characterized in that: In step S4, the spot area of ​​the laser beam is 1.2-1.7 times the area of ​​the nozzle spray outlet.

19. Use of the LiFePO4 / α-Fe2O3 composite material obtained by the preparation method according to any one of claims 1 to 18 in extracting lithium from salt lakes.

Citation Information

Patent Citations

  • Preparing method of highly conductive lithium iron phosphate anode material of lithium ionic cell

    CN101335347A

  • Method for preparing lithium iron phosphate / nanometer carbon composite anode material

    CN101533904A

  • Nanoscale lithium iron phosphate compound and preparation method thereof

    CN101630730A

  • Lithium iron phosphate-carbon nanotube composite material, preparation method, and application thereof

    CN102427130A

  • High power iron phosphate ion battery material and preparation method thereof

    CN102760880A