Positive electrode material, preparation method therefor, secondary battery, and electrical apparatus

By covering the surface of the high-nickel positive electrode material with a cladding layer containing lithium solid solution and boron elements, the problem of battery safety performance degradation when the specific capacity is improved is solved, and higher battery safety and cycling performance are achieved.

WO2024234494A1PCT designated stage expired Publication Date: 2024-11-21TIANJIN B&M SCI & TECH LTD

Patent Information

Application Number
PCT/CN2023/114657
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2023-08-24
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

While increasing the specific capacity of high nickel positive electrode materials, the battery safety performance becomes worse, especially when the nickel content is greater than 80%, alkaline compounds are easily generated on the surface of the material, resulting in a decrease in battery inflation and processing performance.

Method used

The positive electrode material adopting a clad structure, including a lithium nickel oxide matrix, a first cladding layer of lithium-containing solid solution and a second cladding layer of boron element, reduces the formation of surface alkaline compounds, reduces the amount of residual alkali, and improves the battery. Safety performance.

Benefits of technology

It effectively reduces the formation of alkaline compounds on the surface of the positive electrode material, improves the safety and circulation performance of the battery, reduces the water absorption during the preparation process, and optimizes the processing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023114657_21112024_PF_FP_ABST
    Figure CN2023114657_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A positive electrode material, a preparation method therefor, a secondary battery, and an electrical apparatus. The positive electrode material comprises: a base, a first coating layer covering at least part of the surface of the base, and a second coating layer covering at least part of the surface of the first coating layer; the material of the base comprises a lithium nickel oxide, and within the lithium nickel oxide, the molar ratio of elemental nickel to the totality of the remaining elements other than elemental lithium and elemental oxygen is 83%-100%; the material of the first coating layer comprises a lithium-containing solid solution; and the material of the second coating layer comprises elemental boron. Coating the surface of the base with the first coating layer replaces a traditional water washing process, reducing side reactions between positive electrode material lithium residue and water, reducing the amount of residual alkali contained in the positive electrode material, decreasing the amount of gas generated, and improving the safety performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode material and preparation method thereof, secondary battery and electric device

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 12, 2023, with application number 2023105333715 and invention name “Positive electrode material and preparation method thereof, secondary battery and electrical device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present invention relates to the technical field of lithium-ion batteries, and in particular to a positive electrode material and a preparation method thereof, a secondary battery and an electrical device. Background Art

[0003] With the rapid development of new energy vehicles, people's demand for high energy density of power batteries is increasing day by day, so improving the energy density of lithium-ion power batteries has become the focus of the whole society. + Developing cathode materials with high specific capacity is the key to achieving high energy density performance of electric vehicle batteries.

[0004] High-nickel cathode materials are considered candidate cathode materials for power batteries due to their advantages such as low cost, high specific capacity, and long cycle life. However, research has found that as the nickel content in high-nickel cathode materials increases, the specific capacity of the material significantly increases, but the battery's safety performance deteriorates.

[0005] Summary of the Invention

[0006] Based on this, it is necessary to provide a positive electrode material and a preparation method thereof, a secondary battery and an electrical device, so that the material specific capacity can be improved while the battery has higher safety.

[0007] A first aspect of the present invention provides a positive electrode material, comprising:

[0008] A substrate, wherein the material of the substrate comprises lithium nickel oxide, wherein the molar proportion of nickel in the total elements other than lithium and oxygen is 83% to 100%;

[0009] The first coating layer is coated on at least a portion of the surface of the substrate, wherein the material of the first coating layer includes a lithium-containing solid solution, and the chemical formula of the lithium-containing solid solution is Li a M″ n b O c , wherein the M″ element includes one or more of Co, Mn, Y, S, Ta, Ti, Zr, Nb, W and P, n is the valence of the M″ element, a+nb=2c; and

[0010] The second coating layer is coated on at least a portion of the surface of the first coating layer, and the material of the second coating layer includes boron element.

[0011] In some embodiments, the chemical formula of the lithium nickel oxide is Li w Ni x M y M z 'O2, wherein the M element includes one or more of Co, Mn and Al, the M' element is a doping element including one or more of Al, Ti, Zr, Mg, W, Mo, Y, Ta, Nb, Sb and Sr, 0.95≤w≤1.05, 0.83≤x≤1.0, 0≤z<0.1, x+y+z=1.

[0012] In some embodiments, the material of the second coating layer includes one or more lithium borate compounds;

[0013] Optionally, the material of the second coating layer includes lithium borate.

[0014] In some embodiments, the cathode material has at least one of the following characteristics:

[0015] (1) The material of the matrix is ​​a single crystal primary particle; the average particle size of the matrix material is 2 μm-5 μm; the average particle size of the positive electrode material is 2.5 μm-6 μm;

[0016] (2) The material of the matrix is ​​agglomerate; the average particle size of the matrix material is 10 μm-12 μm; the average particle size of the positive electrode material is 10.5 μm-12.5 μm;

[0017] (3) The thickness of the first coating layer is 5 nm to 20 nm;

[0018] (4) The thickness of the second coating layer is 2nm-5nm;

[0019] (5) The mass ratio of the first coating layer to the substrate is (1-15):100;

[0020] (6) The ratio of the mass of the second coating layer to the total mass of the substrate and the first coating layer is (0.02-0.5):1.

[0021] The second aspect of the present invention provides a method for preparing the positive electrode material of the first aspect of the present application, comprising the following steps:

[0022] Mixing a nickel-containing precursor and a lithium source, and performing a first sintering process to prepare the substrate;

[0023] The substrate and the M″-containing compound are mixed and subjected to a second sintering process to prepare the first coating layer on at least a portion of the outer surface of the substrate to obtain an intermediate;

[0024] The intermediate is mixed with a boron source, water is sprayed into the mixture during the mixing process, and a third sintering treatment is performed to prepare the second coating layer on at least a portion of the outer surface of the first coating layer to obtain the positive electrode material.

[0025] In some embodiments, the first sintering process includes at least one of the following conditions:

[0026] (1) The chemical formula of the nickel-containing precursor is Ni d M 1-d (OH)2, wherein the M element includes one or more of Co, Mn and Al, 0.9≤d≤1.0;

[0027] (2) The lithium source includes one or more of lithium carbonate, lithium hydroxide, lithium phosphate, lithium nitrate, lithium acetate and lithium oxalate;

[0028] (3) The molar ratio of the lithium element contained in the lithium source to the nickel-containing precursor is (1.02-1.06):1;

[0029] (4) During the first sintering treatment, a compound containing a doping element M′ is also added;

[0030] Optionally, the compound containing the doping element M' includes one or more of an oxide, oxalate, carbonate, hydroxide and metal organic compound containing the element M', and the doping element M' includes one or more of Al, Ti, Zr, Mg, W, Mo, Y, Ta, Nb, Sb and Sr; further optionally, the compound containing the doping element M' includes an oxide containing the element M';

[0031] Optionally, the mass ratio of the compound containing the doping element M′ to the nickel-containing precursor is (0.05-0.5):100;

[0032] (5) The temperature of the first sintering is 700°C-900°C, the sintering time is 10h-20h, and the heating rate is 2°C / min-5°C / min.

[0033] In some embodiments, the second sintering process includes at least one of the following conditions:

[0034] (1) The M″-containing compound includes one or more of oxides, oxalates, carbonates, hydroxides and metal organic compounds containing the M″ element;

[0035] (2) The mass ratio of the M″-containing compound to the matrix is ​​(0.5-5):100;

[0036] (3) The temperature of the second sintering is 600°C-800°C, the sintering time is 6h-12h, and the heating rate is 2°C / min-5°C / min.

[0037] In some embodiments, the third sintering process includes at least one of the following conditions:

[0038] (1) The boron source includes one or more of boron hydroxide and boron oxide;

[0039] (2) The mass ratio of the boron source to the intermediate is (0.05-0.3):100;

[0040] (3) The mass ratio of the water to the intermediate is (1-2):100;

[0041] (4) The temperature of the third sintering is 250°C-450°C, the sintering time is 6h-10h, and the heating rate is 1°C / min-3°C / min.

[0042] A third aspect of the present invention provides a secondary battery, comprising a positive electrode plate, wherein the positive electrode plate comprises a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector;

[0043] Wherein, the positive electrode active material layer comprises the positive electrode material of the first aspect of the present application; or

[0044] The positive electrode active material layer includes a positive electrode material prepared by the preparation method according to the second aspect of the present application.

[0045] A fourth aspect of the present invention provides an electrical device comprising the secondary battery according to the third aspect of the present application.

[0046] The above-mentioned positive electrode material and its preparation method, secondary battery and electrical device, wherein the positive electrode material includes a substrate, a first coating layer coated on the surface of the substrate and a second coating layer coated on the surface of the first coating layer; on the one hand, the present invention reduces the generation of alkaline compounds (such as Li2CO3 and LiOH) on the surface of the positive electrode material by coating the first coating layer and the second coating layer on the surface of the substrate, reduces the amount of residual alkali on the surface of the positive electrode material, thereby reducing the amount of gas generated due to the side reaction between the residual alkali and the electrolyte, and improving the battery safety performance; on the other hand, the present invention develops a process to replace traditional water washing to reduce the residual alkali content on the surface, which can reduce the proton exchange reaction between the residual lithium on the surface of the positive electrode material and water during the water washing process, stabilize the surface structure of the positive electrode material, and improve the electrochemical capacity and cycle performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] FIG1 is a scanning electron microscope image of the positive electrode material prepared in Example 1;

[0048] FIG2 is a scanning electron microscope image of the positive electrode material prepared in Example 5;

[0049] FIG3 is a scanning electron microscope image of the positive electrode material prepared in Comparative Example 1;

[0050] FIG4 is a schematic diagram of the initial charge and discharge test results of Example 1 and Comparative Examples 1-4;

[0051] FIG5 is a schematic diagram of the cycle test results of Example 1 and Comparative Examples 1-4. DETAILED DESCRIPTION

[0052] To facilitate understanding of the present invention, the present invention will be described more fully below with reference to the accompanying drawings. Preferred embodiments of the present invention are shown in the accompanying drawings. However, the present invention may be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the present disclosure.

[0053] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0054] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0055] In the present invention, when referring to numerical ranges, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Furthermore, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.

[0056] Only certain numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.

[0057] The temperature parameters in the present invention, unless otherwise specified, allow for either constant temperature treatment or treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range controlled by the instrument.

[0058] In the description of the invention, “plurality” means at least two, for example, two, three, etc., unless otherwise clearly and specifically defined.

[0059] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution. Unless otherwise specified, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.

[0060] Unless otherwise specified, all steps of the present invention may be performed sequentially or randomly, but are preferably performed sequentially.

[0061] High nickel positive electrode materials are considered to be candidate positive electrode materials for power batteries due to their advantages such as low cost, high specific capacity and long cycle life. However, as the nickel content in high nickel positive electrode materials increases, the specific capacity of the material is significantly improved, while the safety performance of the battery deteriorates. The present technicians have found through research that as the nickel content in high nickel positive electrode materials increases, especially when the nickel content is greater than 80%, due to the residual lithium on the surface of the high nickel positive electrode material, the material is more sensitive to H2O and CO2 in the air, and it is easy to generate alkaline compounds (such as Li2CO3 and LiOH) on the surface of the material, and the amount of residual alkali on the surface of the material increases. The residual alkali easily reacts with the electrolyte at high temperature to generate gas, causing battery flatulence, thereby deteriorating the safety performance of the battery. In addition, the increase in the amount of residual alkali on the surface of the material will also cause water absorption during the processing of the homogenate during the battery preparation process, and the processing performance will deteriorate.

[0062] The first aspect of the present application provides a positive electrode material, comprising a substrate, a first coating layer coated on at least a portion of the surface of the substrate, and a second coating layer coated on at least a portion of the surface of the first coating layer; the material of the substrate comprises lithium nickel oxide, in which the molar proportion of nickel in the total elements other than lithium and oxygen is 83%-100%; the material of the first coating layer comprises a lithium-containing solid solution, the chemical formula of the lithium-containing solid solution is Li a M″ n b O c , wherein the M″ element includes one or more of Co, Mn, Y, S, Ta, Ti, Zr, Nb, W and P, n is the valence state of the M″ element, a+nb=2c; the material of the second coating layer includes boron element.

[0063] It should be noted that the material of the matrix can be single crystal primary particles or agglomerates. Agglomerates refer to a collection of single crystal primary particles connected to each other at edges or corners.

[0064] Lithium nickel oxide refers to an oxide containing lithium and nickel elements. The lithium nickel oxide may be doped with other metal elements or may not be doped with other metal elements, which can be determined according to needs.

[0065] The first coating layer may cover the entire surface of the substrate or only a portion of the substrate; preferably, the first coating layer covers the entire surface of the substrate. The second coating layer may cover the entire surface of the first coating layer or only a portion of the substrate; preferably, the second coating layer covers the entire surface of the first coating layer. Of course, it is understood that if the first coating layer does not cover the entire surface of the substrate, the second coating layer may also be directly coated on the surface of the substrate.

[0066] The matrix can be entirely composed of lithium nickel oxide, or a mixture of lithium nickel oxide and other materials that can be used as positive electrode materials. The first coating layer can be entirely composed of a lithium-containing solid solution, or a mixture of a lithium-containing solid solution and other materials; preferably, the first coating layer is entirely composed of a lithium-containing solid solution.

[0067] The molar proportion of nickel in the total elements other than lithium and oxygen refers to the ratio of the molar amount of nickel to the total molar amount of all elements other than lithium and oxygen in lithium nickel oxide.

[0068] It can be understood that the positive electrode material mentioned above includes a substrate, a first coating layer coated on the surface of the substrate, and a second coating layer coated on the surface of the first coating layer; in the first aspect of the present invention, by coating the surface of the substrate with the first coating layer and the second coating layer, the generation of alkaline compounds (such as Li2CO3 and LiOH) on the surface of the positive electrode material is reduced, and the amount of residual alkali on the surface of the positive electrode material is reduced, thereby reducing the amount of gas generated by the side reaction between the residual alkali and the electrolyte, and improving the safety performance of the battery; on the other hand, the present invention has developed a process to replace the traditional water washing to reduce the residual alkali content on the surface, which can reduce the proton exchange reaction between the residual lithium of the positive electrode material and water during the water washing process, stabilize the surface structure of the positive electrode material, and improve the electrochemical capacity and cycle performance of the material. At the same time, since the amount of residual alkali contained in the positive electrode material is reduced, water absorption during the preparation of the positive electrode slurry can be reduced or avoided, and the processing performance is optimized.

[0069] The M" element added when preparing the first coating layer can consume the lithium on the surface of the substrate at high temperature to generate a lithium-containing solid solution Li with good conductivity. a M″ n b O cCoating and modifying the substrate surface allows the first coating layer to more tightly adhere to the substrate, promoting the intercalation and deintercalation of lithium ions during charge and discharge. Deionized water is added during the preparation of the second coating layer to increase the wettability of the particle surface, allowing boron to better penetrate the surface of the first coating layer during sintering, forming a lithium borate compound. This reduces the specific surface area of ​​the positive electrode material, inhibits the overflow of transition metal ions, and improves the structural and thermal stability of the positive electrode material.

[0070] In addition, by coating the surface of the substrate with a first coating layer instead of the traditional water washing process, the obtained positive electrode material is more stable, thereby improving the battery capacity and cycle performance.

[0071] In some embodiments, the chemical formula of lithium nickel oxide is Li w Ni x M y M z 'O2, wherein the M element includes one or more of Co, Mn, and Al, and the M' element is a doping element including one or more of Al, Ti, Zr, Mg, W, Mo, Y, Ta, Nb, Sb, and Sr, 0.95≤w≤1.05, 0.83≤x≤1.0, 0≤z<0.1, and x+y+z=1. By doping the lithium nickel oxide with the M' element, the crystal structure of the matrix can be stabilized, phase change can be suppressed, and the stability of the positive electrode material can be improved.

[0072] As a possible embodiment, the material of the second coating layer includes one or more lithium borate compounds; when preparing the second coating layer, the boron element in the boron source and the lithium element remaining on the surface of the first coating layer generate a lithium borate compound. As the second coating layer, the boron element can better melt and penetrate into the surface of the first coating layer, thereby reducing the specific surface area of ​​the positive electrode material.

[0073] It should be noted that lithium borate compounds refer to a series of compounds formed by lithium borate doped with other elements or not doped with other elements.

[0074] Optionally, the material of the second coating layer includes lithium borate.

[0075] In some possible embodiments, the substrate material is a single crystal. When the substrate material is a single crystal, the battery produces relatively less gas after fabrication, resulting in higher safety. The average particle size of the substrate material is 2μm-5μm; for example, it can be, but is not limited to, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, or a range between any two of the above values. When the average particle size of the single crystal substrate material is within the above range, the kinetics of the positive electrode material is relatively good, and the capacity and rate capability can be excellent. When the average particle size of the substrate material is higher than the above range, the lithium ion diffusion path increases, affecting lithium ion transport. When the average particle size of the substrate material is lower than the above range, the difficulty of the positive electrode material preparation process increases. The average particle size of the positive electrode material is 2.5μm-6μm; for example, it can be, but is not limited to, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, or a range between any two of the above values.

[0076] In some possible embodiments, the material of the matrix is ​​an agglomerate; when the material of the matrix is ​​an agglomerate, the positive electrode material may have a higher compaction density and capacity. The average particle size of the matrix material is 10μm-12μm; for example, it can be but not limited to 10μm, 10.5μm, 11μm, 11.5μm, 12μm, or a range between any two of the above values. When the average particle size of the matrix material of the agglomerate is within the above range, the positive electrode material particle strength is better; when the average particle size of the matrix material is lower than the above range, the positive electrode material compaction density may decrease; when the average particle size of the matrix material is higher than the above range, the positive electrode material particles are prone to cracking. The average particle size of the positive electrode material is 10.5μm-12.5μm; for example, it can be but not limited to 10.5μm, 11μm, 11.5μm, 12μm, 12.5μm, or a range between any two of the above values.

[0077] In some embodiments, the thickness of the first coating layer is 5 nm to 20 nm; for example, it can be, but is not limited to, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, or a range between any two of the above values. When the thickness of the first coating layer is within the above range, the amount of residual alkali on the surface of the positive electrode material particles can be reduced, and the lithium-containing solid solution formed can promote the deintercalation of lithium ions during the charge and discharge process, thereby improving the electrochemical performance of the positive electrode material. When the thickness of the first coating layer is greater than the above range, the deintercalation of lithium ions during the charge and discharge process may be affected.

[0078] In some embodiments, the thickness of the second coating layer is 2 nm to 5 nm; for example, it can be, but is not limited to, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, or a range between any two of the foregoing values. When the thickness of the second coating layer is within the foregoing range, the specific surface area of ​​the positive electrode material can be reduced, the overflow of transition metal ions can be suppressed, and the positive electrode material can have higher structural stability and thermal stability.

[0079] In some embodiments, the mass ratio of the first coating layer to the substrate is (1-15):100; for example, it can be, but is not limited to, 1:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100, 11:100, 12:100, 13:100, 14:100, 15:100, or a range between any two of the above ratios. When the mass ratio of the first coating layer to the substrate is within the above range, the amount of residual alkali on the surface of the positive electrode material particles can be reduced, the subsequent electrode sheet processing process of the positive electrode material can be optimized, and the electrochemical performance of the positive electrode material can be improved.

[0080] In some embodiments, the ratio of the mass of the second coating layer to the total mass of the substrate and the first coating layer is (0.02-0.5):100; for example, it can be, but is not limited to, 0.02:100, 0.05:100, 0.1:100, 0.15:100, 0.2:100, 0.25:100, 0.3:100, 0.35:100, 0.4:100, 0.45:100, 0.5:100, or a range between any two of the above ratios. When the ratio of the mass of the second coating layer to the total mass of the substrate and the first coating layer is within the above range, the structural stability and thermal stability of the positive electrode material can be improved, thereby improving the electrochemical performance of the positive electrode material.

[0081] The second aspect of the present invention provides a method for preparing the positive electrode material of the first aspect, comprising the following steps:

[0082] Mixing a nickel-containing precursor and a lithium source, and performing a first sintering process to prepare a substrate;

[0083] The substrate and the M″-containing compound are mixed and subjected to a second sintering process to prepare a first coating layer on at least a portion of the outer surface of the substrate to obtain an intermediate;

[0084] The intermediate is mixed with a boron source, water is sprayed into the mixture during the mixing process, and a third sintering treatment is performed to prepare a second coating layer on at least a portion of the outer surface of the first coating layer to obtain a positive electrode material.

[0085] The nickel-containing precursor can be a single crystal or an agglomerate; when the nickel-containing precursor is a single crystal, the material of the prepared substrate is a single crystal; when the nickel-containing precursor is an agglomerate, the material of the prepared substrate is an agglomerate.

[0086] Adding water when preparing the second coating layer can increase the wettability of the intermediate surface, allowing the boron element to better melt and penetrate into the surface of the first coating layer during the sintering process, reducing the specific surface area of ​​the prepared positive electrode material, inhibiting the overflow of transition metal ions, and making the positive electrode material have better structural stability and thermal stability.

[0087] When preparing the positive electrode material, by coating the outer surface of the substrate with a first coating layer instead of the traditional water washing process, the side reaction between residual lithium and water in the positive electrode material can be reduced, the generation of alkaline compounds in the positive electrode material can be reduced, and the amount of residual alkali contained in the positive electrode material can be reduced, thereby reducing the amount of gas generated by the side reaction between the residual alkali and the electrolyte, and improving the battery safety performance.

[0088] In some embodiments, the chemical formula of the nickel-containing precursor is Ni d M 1-d (OH)2, wherein the M element includes one or more of Co, Mn and Al, and 0.9≤d≤1.0.

[0089] As a possible embodiment, the lithium source includes one or more of lithium carbonate, lithium hydroxide, lithium phosphate, lithium nitrate, lithium acetate and lithium oxalate.

[0090] In some possible embodiments, the molar ratio of the lithium element contained in the lithium source to the nickel-containing precursor is (1.02-1.06):1; for example, it can be, but is not limited to, 1.02:1, 1.025:1, 1.03:1, 1.035:1, 1.04:1, 1.045:1, 1.05:1, 1.055:1, 1.06:1, or a range between any two of the above ratios. When the molar ratio of the lithium element contained in the lithium source to the nickel-containing precursor is within the above range, the matrix particles have good crystallinity and the prepared positive electrode material has excellent electrochemical performance.

[0091] In some embodiments, during the first sintering treatment, a compound containing the doping element M′ is also added; optionally, the compound containing the doping element M′ includes one or more of oxides, oxalates, carbonates, hydroxides and metal organics containing the M′ element, and the doping element M′ includes one or more of Al, Ti, Zr, Mg, W, Mo, Y, Ta, Nb, Sb and Sr; further optionally, the compound containing the doping element M′ includes an oxide containing the M′ element.

[0092] Optionally, the mass ratio of the compound containing the doping element M' to the nickel-containing precursor is (0.05-0.5):100; for example, it can be, but is not limited to, 0.05:100, 0.1:100, 0.15:100, 0.2:100, 0.25:100, 0.3:100, 0.35:100, 0.4:100, 0.45:100, 0.5:100, or a range between any two of the above ratios. When the mass ratio of the M'-containing compound to the nickel-containing precursor is within the above range, the structural phase transition of the matrix can be suppressed and the structural stability of the matrix can be improved. The doping element M' includes one or more of Al, Ti, Zr, Mg, W, Mo, Y, Ta, Nb, Sb, and Sr.

[0093] In some embodiments, the sintering temperature of the first sintering treatment is 700°C-900°C; for example, it can be but not limited to 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, or a range between any two of the above values. The sintering time of the first sintering treatment is 10 hours-20 hours; for example, it can be but not limited to 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, or a range between any two of the above values. The heating rate of the first sintering treatment is 2°C / min-5°C / min; for example, it can be but not limited to 2°C / min, 2.3°C / min, 2.5°C / min, 2.7°C / min, 3°C / min, 3.3°C / min, 3.5°C / min, 3.8°C / min, 4°C / min, 4.3°C / min, 4.5°C / min, 4.8°C / min, 5°C / min or a range between any two of the above values.

[0094] It should be noted that the heating rate of the first sintering process refers to the rate at which the nickel-containing precursor, the lithium source and the M′-containing compound are heated from their own temperatures at the beginning of the first sintering process to the sintering temperature.

[0095] In some embodiments, the M"-containing compound includes one or more of an oxide, an oxalate, a carbonate, a hydroxide, and a metal organic compound containing an M" element.

[0096] In some embodiments, the mass ratio of the M″-containing compound to the matrix is ​​(0.5-5):100; for example, it can be but is not limited to 0.5:100, 1:100, 1.5:100, 2:100, 2.5:100, 3:100, 3.5:100, 4:100, 4.5:100, 5:100 or a range between any two of the above ratios. When the mass ratio of the matrix to the M″-containing compound is within the above range, the amount of residual alkali on the surface of the matrix can be significantly reduced, thereby improving the stability of the positive electrode material and improving the electrochemical properties of the positive electrode material.

[0097] In some embodiments, the sintering temperature of the second sintering treatment is 600°C-800°C; for example, it can be, but is not limited to, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, or a range between any two of the above values. The sintering time of the second sintering treatment is 6 hours-12 hours; for example, it can be, but is not limited to, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, or a range between any two of the above values. The heating rate of the second sintering treatment is 2°C / min-5°C / min; for example, it can be but not limited to 2°C / min, 2.3°C / min, 2.5°C / min, 2.7°C / min, 3°C / min, 3.3°C / min, 3.5°C / min, 3.8°C / min, 4°C / min, 4.3°C / min, 4.5°C / min, 4.8°C / min, 5°C / min or a range between any two of the above values.

[0098] It should be noted that the heating rate of the second sintering treatment refers to the rate at which the substrate and the M″-containing compound are heated from their own temperatures at the beginning of the second sintering treatment to the sintering temperature.

[0099] As a possible embodiment, the boron source includes one or more of boron hydroxide and boron oxide.

[0100] In some embodiments, the mass ratio of the boron source to the intermediate is (0.05-0.3):100; for example, it can be, but is not limited to, 0.05:100, 0.1:100, 0.15:100, 0.2:100, 0.25:100, 0.3:100, or any range between any two of the above ratios. When the mass ratio of the boron source to the intermediate is within the above range, the structural stability of the positive electrode material can be enhanced, thereby improving its electrochemical performance.

[0101] In some possible embodiments, the mass ratio of water to intermediate is (1-2):100; for example, it can be, but is not limited to, 1:100, 1.1:100, 1.2:100, 1.3:100, 1.4:100, 1.5:100, 1.6:100, 1.7:100, 1.8:100, 1.9:100, 2:100, or any range between any two of the above ratios. When the mass ratio of water to intermediate is within the above range, the intermediate particles can have better wettability, thereby better utilizing the boron. It is understood that the water can be deionized water, pure water, ultrapure water, etc.

[0102] In some embodiments, the sintering temperature of the third sintering process is 250°C-450°C; for example, it can be, but is not limited to, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, or a range between any two of the foregoing values. The sintering time of the third sintering process is 6 hours-10 hours; for example, it can be, but is not limited to, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, or a range between any two of the foregoing values. The heating rate of the third sintering treatment is 1°C / min-3°C / min; for example, it can be but not limited to 1°C / min, 1.1°C / min, 1.2°C / min, 1.3°C / min, 1.4°C / min, 1.5°C / min, 1.6°C / min, 1.7°C / min, 1.8°C / min, 1.9°C / min, 2°C / min, 2.1°C / min, 2.2°C / min, 2.3°C / min, 2.4°C / min, 2.5°C / min, 2.6°C / min, 2.7°C / min, 2.8°C / min, 2.9°C / min, 3°C / min or a range between any two of the above values.

[0103] It should be noted that the heating rate of the third sintering process refers to the rate at which the intermediate and the boron source are heated from their own temperatures at the beginning of the third sintering process to the sintering temperature.

[0104] In some embodiments, the method for preparing the positive electrode material according to the first aspect of the present invention comprises the following steps:

[0105] The nickel-containing precursor, lithium source and compound containing doping element M' are mixed and evenly mixed, and then the first sintering treatment is performed at 700-900 ° C. The sintering time is 10-20 hours and the heating rate is 2 ° C / min-5 ° C / min. The chemical formula of the nickel-containing precursor is Ni d M 1-d(OH)2, wherein the M element includes one or more of Co, Mn and Al, 0.9≤d≤1.0; the lithium source includes one or more of lithium carbonate, lithium hydroxide, lithium phosphate, lithium nitrate, lithium acetate and lithium oxalate; the compound containing the doping element M' includes one or more of oxides, oxalates, carbonates, hydroxides and metal organics containing the M' element; the molar ratio of the lithium element contained in the lithium source to the nickel-containing precursor is (1.02-1.06):1; the mass ratio of the compound containing the doping element M' to the nickel-containing precursor is (0-0.5):100, which can be optionally (0.05-0.5):100; the M' element includes one or more of Al, Ti, Zr, Mg, W, Mo, Y, Ta, Nb, Sb and Sr;

[0106] The substrate and the M″-containing compound are uniformly mixed, and a second sintering treatment is performed at 600° C.-800° C. for 6-12 hours at a heating rate of 2° C. / min-5° C. / min; a first coating layer is formed on at least a portion of the surface of the substrate to obtain an intermediate; wherein the M″-containing compound comprises one or more of oxides, oxalates, carbonates, hydroxides, and metal organics containing the M″ element; the M″ element comprises one or more of Co, Mn, Y, S, Ta, Ti, Zr, Nb, W, and P; and the mass ratio of the M″-containing compound to the substrate is (0.5-5):100;

[0107] The intermediate is mixed with a boron source, water is sprayed into the mixture during the mixing process, the mixture is evenly mixed, and a third sintering treatment is performed at 250°C-450°C, the sintering time is 6-10 hours, and the heating rate is 1°C / min-3°C / min. A second coating layer is prepared on at least a portion of the surface of the first coating layer to obtain a positive electrode material; wherein the boron source includes one or more of boron hydroxide and boron oxide; the mass ratio of the boron source to the intermediate is (0.05-0.3):100; and the mass ratio of water to the intermediate is (1-2):100.

[0108] A third aspect of the present invention provides a positive electrode sheet comprising a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector; wherein the positive electrode active material layer comprises the positive electrode material of the first aspect of the present invention; or the positive electrode active material layer comprises the positive electrode material prepared using the preparation method of the second aspect of the present invention. The positive electrode sheet comprising the positive electrode material of the present invention has a high energy density.

[0109] A third aspect of the present invention provides a secondary battery comprising a positive electrode plate, the positive electrode plate comprising a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector; wherein the positive electrode active material layer comprises the positive electrode material of the first aspect of the present invention; or the positive electrode active material layer comprises the positive electrode material prepared using the preparation method of the second aspect of the present invention. The positive electrode plate comprising the positive electrode material of the present invention has a high energy density, and the secondary battery has improved capacity while also having excellent safety and cycling performance.

[0110] A fourth aspect of the present invention provides an electrical device comprising the secondary battery according to the third aspect of the present invention.

[0111] The technical solution of the present invention is described in detail below with reference to specific embodiments.

[0112] 1. Preparation of positive electrode materials

[0113] Example 1

[0114] Weigh Ni 0.93 Co 0.05 Mn 0.02 (OH)2 (as nickel-containing precursor), LiOH (as lithium source), Al2O3 and SrO (as compound containing doping element M') are mixed evenly, placed in oxygen atmosphere, sintered at 800℃ for 12h, and crushed to obtain matrix LiNi 0.925 Co 0.05 Mn 0.019 Al 0.005 Sr 0.001 O2; wherein the molar ratio of the lithium element contained in the lithium source to the nickel-containing precursor is 1.035:1, the mass ratio of SrO and the nickel-containing precursor is 0.1:100, and the mass percentage of Al2O3 to the mass of the nickel-containing precursor is 0.3%;

[0115] The substrate and Co(OH)2 (as an M″-containing compound) are uniformly mixed, and the mixture is then placed in a box furnace and sintered at 700°C for 8 hours. A first coating layer is coated on the outer surface of the substrate, and the intermediate is obtained after pulverization. The thickness of the first coating layer is 10-12 nm, the mass ratio of the M″-containing compound to the substrate is 2.5:100, and the mass ratio of the first coating layer to the substrate is 2.67:100.

[0116] The intermediate was mixed with H3BO3 (as a boron source), deionized water was sprayed into the mixing process, and after being mixed evenly, the mixture was placed in a box furnace and sintered at 300°C for 8 hours. The second coating layer was coated on the outer surface of the first coating layer. After sintering, the material was sieved through a 325-mesh sieve to obtain a positive electrode material with an average particle size of 3 μm.

[0117] Example 2-10

[0118] The preparation methods of the positive electrode materials in Examples 2-10 are basically similar to the preparation method of the positive electrode material in Example 1, except that at least one of the type of lithium source, the type and / or amount of the nickel-containing precursor, the type and / or amount of the M′-containing compound, the temperature and / or time of the first sintering treatment, the type and / or amount of the M″-containing compound, the temperature and / or time of the second sintering treatment, the type and / or amount of the boron source, the amount of deionized water, the temperature and time of the third sintering treatment, and the type and / or average particle size of the substrate is different.

[0119] The process parameters in Example 2-10 are detailed in Table 1; the product parameters of the positive electrode material prepared in Example 2-10 are detailed in Table 2.

[0120] Comparative Example 1

[0121] The difference between Comparative Example 1 and Example 1 is that only a substrate was prepared, and no coating layer was prepared on the substrate. See Table 1 for details.

[0122] Comparative Example 2

[0123] The difference between Comparative Example 2 and Example 1 is that the first coating layer is not prepared, and only the residual lithium on the outer surface of the substrate is removed by water washing. The other processes are the same. The specific process of the water washing process is as follows:

[0124] The matrix was weighed and placed in deionized water with a mass ratio of matrix to deionized water of 7:3. The mixture was stirred at 180 rpm for 3 min, filtered, and dried at a temperature of 150°C for 4 h. Details are shown in Table 1.

[0125] Comparative Example 3

[0126] The difference between Comparative Example 3 and Example 1 is that the second coating layer is not prepared, and the other aspects are the same. For details, see Table 1.

[0127] Comparative Example 4

[0128] The difference between Comparative Example 4 and Example 1 is that deionized water was not sprayed when preparing the second coating layer. Other details are the same. See Table 1 for details.

[0129] Comparative Example 5

[0130] The difference between Comparative Example 5 and Example 5 is that only a substrate was prepared, and no coating layer was prepared on the substrate. See Table 1 for details.

[0131] Table 1. Process parameters

[0132] In Table 1, n1 represents the molar ratio of the lithium element contained in the lithium source to the nickel-containing precursor; n2 represents the mass ratio of the compound 1 containing the doping element M′ and the nickel-containing precursor; n3 represents the mass ratio of the compound 2 containing the doping element M′ and the nickel-containing precursor; T1 represents the first sintering treatment temperature; t1 represents the first sintering treatment time; n4 represents the mass ratio of the M″-containing compound to the matrix; T2 represents the second sintering treatment temperature; t2 represents the second sintering treatment time; n5 represents the mass ratio of the boron source to the intermediate; n6 represents the mass ratio of deionized water to the intermediate; T3 represents the third sintering treatment temperature; and t3 represents the third sintering treatment time.

[0133] Table 2

[0134] Among them, D1 represents the average particle size of the substrate, D2 represents the thickness of the first coating layer, D3 represents the thickness of the second coating layer, and D4 represents the average particle size of the positive electrode material; n7 represents the mass ratio of the first coating layer to the substrate, and n8 represents the ratio of the mass of the second coating layer to the total mass of the substrate and the first coating layer.

[0135] The positive electrode materials prepared in Example 1, Example 5 and Comparative Example 1 were scanned using an electron scanning electron microscope, and the results are shown in Figures 1, 2 and 3, respectively.

[0136] As can be seen from FIG1 , the surface of the positive electrode material prepared in Example 1 has a coating layer, and the substrate used is a single crystal.

[0137] As shown in FIG2 , the surface of the positive electrode material prepared in Example 5 has a dense and uniform coating layer, and the matrix used is an agglomerate.

[0138] As shown in FIG3 , the surface of the material prepared in Comparative Example 1 is smooth, indicating that the surface of the substrate in Comparative Example 1 is not coated.

[0139] 2. Cathode Material Performance Test

[0140] Weigh 5.000 ± 0.050 g of cathode material powder and place it in 45 g of deionized water. Stir thoroughly for 10 minutes and filter through filter paper to obtain a clear aqueous solution containing dissolved LiOH and Li2CO3. Titrate the solution using 0.1 M HCl on a potentiometric titrator. Determine the amount of HCl consumed based on the indicator or potential change, and record the corresponding volume. Calculate the LiOH and Li2CO3 contents based on the volume of HCl consumed. The results are shown in Table 3.

[0141] Table 3

[0142] From the comparison of the results of Examples 1-3 and Comparative Example 1, and the comparison of Example 5 and Comparative Example 5, it can be seen that compared with the uncoated material, the content of LiOH and Li2CO3 remaining on the surface of the positive electrode material after coating of the present invention is significantly reduced; from the comparison of the results of Examples 1-3 and Comparative Example 2, it can be seen that compared with the amount of LiOH and Li2CO3 remaining on the surface of the positive electrode material prepared after treatment with the traditional water washing process, the amount of LiOH and Li2CO3 remaining on the surface of the positive electrode material after coating of the present invention is reduced, indicating that the coating process of the present invention can significantly reduce the residual alkali content on the surface of the positive electrode material.

[0143] 3. Battery Preparation and Performance Testing

[0144] The positive electrode materials prepared in Examples 1-5, Examples 8-10 and Comparative Examples 1-5 were prepared into button batteries. The specific preparation method is as follows:

[0145] The positive electrode material, conductive agent SP, and binder PVDF were weighed in a 90:5:5 mass ratio and added to an NMP solution. Stirring was carried out under argon for 4 hours to prepare a slurry of high-nickel positive electrode material for button cells. The slurry was coated onto smooth copper foil, dried, and then cut to form a positive electrode sheet. The positive electrode sheet was then assembled with a lithium metal sheet (negative electrode), a separator, and an electrolyte to form a propylene carbonate button cell. The separator was a 14μm-thick polypropylene separator, and the electrolyte contained LiPF6 at a 1M concentration.

[0146] The button cells prepared above were subjected to the initial charge-discharge test. The single crystal test protocol was as follows: constant current charging at 0.1C to 4.30V, constant voltage charging to 50uA, and then discharging at 0.1C to 2.8V for a complete charge-discharge cycle. The aggregate test protocol was as follows: constant current charging at 0.1C to 4.25V, constant voltage charging to 50uA, and then discharging at 0.1C to 2.5V for a complete charge-discharge cycle at room temperature. The results are shown in Table 4.

[0147] The button cell prepared above was subjected to a cycle test, specifically, after 50 cycles at 45°C and a 0.5C charge / discharge rate, its cycle capacity retention was measured. The results are shown in Table 4.

[0148] The initial charge and discharge test results of the button-type batteries in Example 1 and Comparative Examples 1-4 are shown in FIG4 , and the cycle test results of the button-type batteries in Example 1 and Comparative Examples 1-4 are shown in FIG5 .

[0149] Table 4

[0150] From the above results, it can be seen that the positive electrode material prepared by the coating process of the present invention has higher first-cycle charge and discharge efficiency and cycle capacity retention rate, indicating that the positive electrode material of the present invention has higher capacity and better cycle performance.

[0151] The difference between Examples 1-3 and Comparative Example 1 is that two layers of coating were performed; the difference between Examples 1-3 and Comparative Example 2 is that a double layer of coating was performed on the outside of the substrate, and the traditional water washing process was not used; the difference between Example 1 and Comparative Example 3 is that a double layer of coating was performed in Example 1, while only a single layer of coating was performed in Comparative Example 3; the difference between Example 5 and Comparative Example 5 is that a double layer of coating was performed. Comparison of the results of the above groups of Examples and Comparative Examples shows that compared with no coating on the substrate surface, only a single layer of coating, or using a traditional water washing process instead to prepare the first coating layer, the positive electrode material prepared using the coating process of the present invention has higher first-cycle charge-discharge efficiency and cycle capacity retention, indicating that the positive electrode material of the present invention has higher capacity and better cycle performance.

[0152] The difference between Example 1, Examples 8-10 and Comparative Example 4 is that the amount of deionized water added when preparing the second coating layer is different; comparing the results of each group of examples and comparative examples, it can be seen that when deionized water is added during the preparation of the second coating layer, and the amount of deionized water added is within 1-2wt%, the cycle capacity retention rate and the first-week charge and discharge efficiency of the secondary battery can be improved; however, when the amount of deionized water added is greater than 2wt%, the first-week charge and discharge efficiency and the cycle capacity retention rate of the secondary battery are both reduced; technicians analyzed that the reason may be due to: excessive moisture on the surface of the intermediate particles, increased material viscosity, poor mixing uniformity, affecting subsequent lithium ion intercalation and deintercalation, and causing the electrochemical performance of the secondary battery to deteriorate. Therefore, when preparing the second coating layer, when the ratio of the amount of deionized water added to the total mass of the substrate and the first coating layer is (1-2): 100, it helps to improve the structural stability and thermal stability of the positive electrode material, thereby improving the cycle performance of the secondary battery.

[0153] The first-cycle charge-discharge efficiency and cycle capacity retention rate of Example 5 are lower than those of the other examples, mainly because: compared with the single crystal, the charge-discharge voltage of the electrical performance test of the agglomerate is lower.

[0154] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0155] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.

Claims

1. A positive electrode material, characterized in that: include: A substrate, wherein the material of the substrate comprises lithium nickel oxide, in which the molar proportion of nickel element in the total elements other than lithium element and oxygen element is 83%-100%; A first coating layer is coated on at least a portion of the surface of the substrate, wherein the material of the first coating layer includes a lithium-containing solid solution, wherein the chemical formula of the lithium-containing solid solution is Li a M″ n b O c , wherein the M″ element includes one or more of Co, Mn, Y, S, Ta, Ti, Zr, Nb, W and P, n is the valence state of the M″ element, and a+nb=2c; as well as The second coating layer is coated on at least a portion of the surface of the first coating layer, and the material of the second coating layer includes boron element.

2. The positive electrode material according to claim 1, characterized in that The chemical formula of the lithium nickel oxide is Li w Ni x M y M z 'O2, wherein the M element includes one or more of Co, Mn and Al, the M' element is a doping element including one or more of Al, Ti, Zr, Mg, W, Mo, Y, Ta, Nb, Sb and Sr, 0.95≤w≤1.05, 0.83≤x≤1.0, 0≤z<0.1, x+y+z=1.

3. The positive electrode material according to claim 1 or 2, characterized in that The material of the second coating layer includes one or more lithium borate compounds; Optionally, the material of the second coating layer includes lithium borate.

4. The positive electrode material according to any one of claims 1 to 3, characterized in that The positive electrode material has at least one of the following characteristics: (1) The material of the matrix is ​​a single crystal primary particle; the average particle size of the matrix material is 2 μm-5 μm; the average particle size of the positive electrode material is 2.5 μm-6 μm; (2) The material of the matrix is ​​agglomerate; the average particle size of the matrix material is 10 μm-12 μm; the average particle size of the positive electrode material is 10.5 μm-12.5 μm; (3) The thickness of the first coating layer is 5nm-20nm; (4) The thickness of the second coating layer is 2nm-5nm; (5) The mass ratio of the first coating layer to the substrate is (1-15):100; (6) The ratio of the mass of the second coating layer to the total mass of the substrate and the first coating layer is (0.02-0.5):

100.

5. A method for preparing a positive electrode material according to any one of claims 1 to 4, characterized in that: The steps include: Mixing a nickel-containing precursor and a lithium source, and performing a first sintering treatment to prepare the substrate; The substrate and the M″-containing compound are mixed and subjected to a second sintering treatment to prepare the first coating layer on at least a portion of the outer surface of the substrate to obtain an intermediate; The intermediate is mixed with a boron source, water is sprayed into the mixture during the mixing process, and a third sintering treatment is performed to prepare the second coating layer on at least a portion of the outer surface of the first coating layer to obtain the positive electrode material.

6. The method for preparing the positive electrode material according to claim 5, characterized in that: The first sintering process includes at least one of the following conditions: (1) The chemical formula of the nickel-containing precursor is Ni d M 1-d (OH)2, wherein the M element includes one or more of Co, Mn and Al, 0.9≤d≤1.0; (2) The lithium source includes one or more of lithium carbonate, lithium hydroxide, lithium phosphate, lithium nitrate, lithium acetate and lithium oxalate; (3) The molar ratio of the lithium element contained in the lithium source to the nickel-containing precursor is (1.02-1.06):1; (4) during the first sintering treatment, a compound containing a doping element M′ is also added; Optionally, the compound containing the doping element M' includes one or more of an oxide, oxalate, carbonate, hydroxide and metal organic matter containing the M' element, and the doping element M' includes one or more of Al, Ti, Zr, Mg, W, Mo, Y, Ta, Nb, Sb and Sr; further optionally, the compound containing the doping element M' includes an oxide containing the M' element; Optionally, the mass ratio of the compound containing the doping element M′ to the nickel-containing precursor is (0.05-0.5):100; (5) The temperature of the first sintering is 700°C-900°C, the sintering time is 10h-20h, and the heating rate is 2°C / min-5°C / min.

7. The method for preparing the positive electrode material according to claim 5, characterized in that: The second sintering process includes at least one of the following conditions: (1) The M″-containing compound includes one or more of oxides, oxalates, carbonates, hydroxides and metal organic compounds containing the M″ element; (2) The mass ratio of the M″-containing compound to the matrix is ​​(0.5-5):100; (3) The second sintering temperature is 600°C-800°C, the sintering time is 6h-12h, and the heating rate is 2℃ / min-5℃ / min.

8. The method for preparing a positive electrode material according to any one of claims 5 to 7, characterized in that: The third sintering process includes at least one of the following conditions: (1) The boron source includes one or more of boron hydroxide and boron oxide; (2) The mass ratio of the boron source to the intermediate is (0.05-0.3):100; (3) The mass ratio of the water to the intermediate is (1-2):100; (4) The temperature of the third sintering is 250°C-450°C, the sintering time is 6h-10h, and the heating rate is 1°C / min-3°C / min.

9. A secondary battery, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector; Wherein, the positive electrode active material layer comprises the positive electrode material according to any one of claims 1 to 4; or The positive electrode active material layer comprises a positive electrode material prepared by the preparation method according to any one of claims 5 to 8.

10. An electrical device, characterized in that: Comprising the secondary battery as claimed in claim 9.

Citation Information

Patent Citations

  • High-nickel positive electrode material, preparation method thereof and lithium ion secondary battery

    CN112382741A

  • High-nickel positive electrode material, lithium ion battery and preparation methods of high-nickel positive electrode material and lithium ion battery

    CN114079043A

  • Multi-element coated and modified single-crystal lithium nickel cobalt manganate positive electrode material, preparation method thereof and lithium ion battery

    CN115863602A

  • Positive electrode material and preparation method thereof, secondary battery and electric device

    CN116632190A

  • Positive electrode active material for non-aqueous electrolyte secondary battery and method of manufacturing the same

    JP2019192512A

Cited By

  • Positive electrode active material and preparation method thereof, positive plate and battery

    CN121172089A

  • High-nickel positive electrode material for lithium ion battery as well as preparation method and application of high-nickel positive electrode material

    CN121641927A