Sodium layered metal oxide and preparation method therefor, secondary battery and electric device
By doping specific elements in sodium layered metal oxides and forming double-site doping, the problem of structural instability is solved, and the cycle performance and service life are significantly improved.
Patent Information
- Application Number
- PCT/CN2023/115723
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2023-08-30
- Publication Date
- 2024-11-21
AI Technical Summary
The structure of sodium layered metal oxides is unstable during the cycle charging and discharge process and is prone to phase change, affecting their cycle life.
By doping the A elements of Group IIA, Group V and Group IIIB elements in the sodium layered metal oxide, and the C elements of the third to fifth cycles, the two-site doping is formed to improve its structural stability. sex.
It significantly improves the circulation performance and service life of sodium layered metal oxides, reduces the risk of layer slippage and phase transition, and improves the stability and energy density of the cathode material.
Smart Images

Figure CN2023115723_21112024_PF_FP_ABST
Abstract
Description
Sodium layered metal oxide, preparation method thereof, secondary battery and electrical device
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 15, 2023, with application number 202310541146.6 and invention name “Sodium layered metal oxide and preparation method thereof, secondary battery and electrical device”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application belongs to the field of battery material technology, and specifically relates to a sodium layered metal oxide and a preparation method thereof, a secondary battery and an electrical device. Background Art
[0003] Sodium-ion batteries (SIBs) have the advantages of abundant sodium reserves, low cost, and unique battery safety characteristics, making them a key candidate for large-scale energy storage systems. Sodium layered metal oxides, represented by NaMO₂, where M is a transition metal, have high specific capacity, high compaction density, and a tunable voltage range, making them suitable as cathode materials for SIBs.
[0004] However, sodium layered metal oxides have the defect of structural instability. During the cyclic charge and discharge process of sodium-ion batteries, sodium layered metal oxides as positive electrode materials are prone to phase change, which affects their cycle life.
[0005] Summary of the Invention
[0006] In view of the above problems, the present application provides a sodium layered metal oxide and a preparation method thereof, a secondary battery and an electrical device, aiming to solve the technical problem of unstable structure of sodium layered metal oxide.
[0007] In the first aspect, the present invention provides a sodium layered metal oxide, the chemical formula of which is: Na 1-x A x C y M 1-y O2; among them,
[0008] M contains transition metal elements;
[0009] A comprises at least one of a Group IIA element, a Group V metal element, a Group VIA metal element, and a Group IIIB element, and the ionic radius of A is greater than the ionic radius of M;
[0010] C comprises at least one of the third period metal elements, the fourth period metal elements and the fifth period metal elements, and the valence of C is less than or equal to the valence of M;
[0011] x=0.001~0.150, y=0.001~0.500.
[0012] By incorporating unique element A and element C species into the sodium layered metal oxide, due to the characteristics that the ionic radius of A is larger than that of the transition metal M and the valence is greater than that of the sodium ion, the strong Coulomb interaction between the high-valent element A and the oxygen atom can make the sodium layered metal oxide less likely to undergo layer slip and phase change when in the desodiumated state, thereby playing a role in supporting the layered structure, and the element C with a lower valence than the transition metal M can well balance the valence state and reduce the increase in lattice stress caused by local valence changes; therefore, the sodium layered metal oxide incorporating element A and element C species provided in the embodiment of the present application has good stability and can improve its cycle performance and service life.
[0013] In one embodiment, A is a doping element for the sodium site, and C is a doping element for M.
[0014] A doping is performed through the sodium site and C doping is performed through the M site to form a stable dual-site doped sodium layered metal oxide.
[0015] In some embodiments, the valence of A is +2 to +4.
[0016] After the sodium layered metal oxide is doped with A with a valence of +2 to +4, the strong Coulomb interaction between the doping element A and the oxygen atom relative to the sodium ion with a valence of +1 makes it less likely for layer slip to occur in the desodiumated state, playing a good structural column role, thereby improving the crystal structure stability of the sodium layered metal oxide.
[0017] In some embodiments, the Group IIA element in A includes at least one of calcium, strontium, and barium, the Group V metal element includes at least one of antimony and bismuth, the Group VIA metal element includes tellurium, and the Group IIIB element includes at least one of yttrium, cerium, and lanthanum; or, A contains calcium.
[0018] The ionic radii of calcium, strontium, barium, antimony, bismuth, yttrium, cerium, lanthanum, and tellurium are similar to or slightly larger than those of sodium ions, and their valences are higher than those of sodium ions. Therefore, these doping elements can be incorporated into the sodium sites of sodium layered metal oxides. The strong Coulombic interaction between these elements and oxygen atoms can effectively suppress interlayer slip in the sodium layered metal oxides. Calcium not only effectively incorporates into the sodium sites but also stabilizes the crystal structure of the sodium layered metal oxides.
[0019] In some embodiments, the third period metal element in C includes at least one of magnesium and aluminum, the fourth period metal element includes at least one of zinc, gallium, and germanium, and the fifth period metal element includes zirconium; or, C contains aluminum.
[0020] The ionic radii of zirconium, magnesium, aluminum, zinc, gallium, and germanium are similar to or smaller than those of transition metal M, and their valences are less than or equal to those of transition metal M. Therefore, they can be easily doped into transition metal M sites while also balancing valence states, reducing the risk of increased lattice stress caused by large local valence variations. Aluminum, on the other hand, not only does well in doping transition metal M sites, but also better balances valence states.
[0021] In some embodiments, M includes at least two of nickel, manganese, copper, and iron; or, M includes nickel, iron, and manganese.
[0022] The sodium layered metal oxides formed by multiple transition metals such as nickel, manganese, copper, and iron not only prevent the migration of transition metal ions in the transition metal layer, but also combine with the carbon doping element at the sodium site to better suppress phase transitions and improve the electrochemical stability of the desodiumated state. Nickel, iron, and manganese together form the transition metal elements at the M site. The sodium layered metal oxides formed by these three transition metals not only have high specific capacity, but are also easy to dope with the carbon doping element.
[0023] In one embodiment, the molar ratio of nickel, iron and manganese in M is (0.2-0.4):(0.2-0.4):(0.2-0.6).
[0024] The sodium layered metal oxide formed by the three transition metals of nickel, iron and manganese under the above molar ratio conditions has high specific capacity and good stability.
[0025] In one embodiment, x=0.01-0.02, y=0.01-0.02.
[0026] Doping modification of the doping element A and the doping element C under the above-mentioned parameter mass conditions can greatly improve the stability of the sodium layered metal oxide, while having little effect on the energy density of the sodium layered metal oxide.
[0027] In one embodiment, the sodium layered metal oxide has an O3 type crystal structure.
[0028] Sodium layered metal oxides with an O3-type crystal structure have high specific capacity and can be used as positive electrode materials for sodium-ion batteries.
[0029] In some embodiments, the sodium layered metal oxide has the formula Na 0.98 Ca 0.02 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 O2.
[0030] The sodium layered metal oxide of the above chemical formula not only has good structural stability, but also has high specific capacity and high energy density, and has better comprehensive performance when used as a positive electrode active material.
[0031] In a second aspect, the present invention provides a method for preparing the sodium layered metal oxide, comprising the following steps:
[0032] The mixture containing the transition metal M source and the doping element C source is subjected to a first grinding process, and then subjected to a first calcination process to obtain an intermediate product;
[0033] The intermediate product is mixed with a sodium source and a doping element A source, subjected to a second grinding process, and then subjected to a second calcination process to obtain a sodium layered metal oxide.
[0034] In the preparation process of sodium layered metal oxides, the transition metal M site is first doped with C, and then the sodium site is doped with A. In this way, sodium layered metal oxides doped with both the sodium site and the transition metal M site can be obtained. This preparation method is not only simple in process, but also easy to achieve doping. The obtained sodium layered metal oxide has good stability.
[0035] In some embodiments, the steps of preparing a mixture containing a transition metal M source and a doping element C source include:
[0036] Separately preparing an aqueous solution of a transition metal M source and an aqueous solution of a doping element C source;
[0037] Adding a complexing agent to an aqueous solution of a transition metal M source and an aqueous solution of a doping element C source to carry out complexing reactions, respectively obtaining a first gel-like substance and a second gel-like substance;
[0038] The first gel-like substance and the second gel-like substance are mixed and dried to obtain a mixture.
[0039] By adopting the sol-gel method, the transition metal M source and the doping element C source can be mixed evenly, thereby achieving better uniform doping.
[0040] In some embodiments, one or more of the following (1) to (3) are satisfied:
[0041] (1) the complexing agent comprises at least one of citric acid, oxalic acid, glutamic acid, polypropylene glycol, polyvinylidene fluoride and polyacrylamide;
[0042] (2) The temperature of the complexation reaction is 40-100°C;
[0043] (3) The pH value of the complexation reaction is 7-11.
[0044] The types of complexing agents and complexing reaction conditions can enable the transition metal M source and the doping element C source to generate gel-like substances respectively.
[0045] In some embodiments, the first calcination treatment comprises: calcining at 800-950° C. for 6-10 hours, then cooling to 200-600° C. for 3-6 hours; and / or,
[0046] The second calcination treatment includes: calcining at 800-950° C. for 6-10 hours, then cooling to 200-600° C. and calcining for 3-6 hours.
[0047] The first calcination treatment condition can achieve C element doping at the M site, while the second calcination treatment condition can achieve A doping at the Na site.
[0048] In some embodiments, one or more of the following (1) to (4) are satisfied:
[0049] (1) The source of transition metal M includes at least one of a soluble halide salt, acetate, carbonate, nitrate, sulfate, hydroxide, and oxide of M;
[0050] (2) the doping element C source includes at least one of a soluble halide salt, acetate, carbonate, nitrate, sulfate, hydroxide, and oxide of C;
[0051] (3) the source of the doping element A includes at least one of a soluble halide salt, acetate, carbonate, nitrate, sulfate, hydroxide, and oxide of A;
[0052] (4) The sodium source includes at least one of sodium halide, sodium acetate, sodium carbonate, sodium nitrate, sodium sulfate, sodium hydroxide and sodium oxide.
[0053] The material type of the above-mentioned transition metal M source can provide M element for the preparation of sodium layered metal oxide, the material type of the doping element C source can provide C element for the preparation of sodium layered metal oxide, the material type of the doping element A source can provide A element for the preparation of sodium layered metal oxide, and sodium salt can provide sodium element for the preparation of sodium layered metal oxide.
[0054] In a third aspect, an embodiment of the present application provides a secondary battery, wherein the positive electrode sheet of the secondary battery contains the sodium layered metal oxide provided in the first aspect of the embodiment of the present application and / or the sodium layered metal oxide prepared by the preparation method provided in the second aspect of the embodiment of the present application.
[0055] By using the sodium layered metal oxide provided in the first aspect of the embodiment of the present application and / or the sodium layered metal oxide prepared by the preparation method provided in the second aspect of the embodiment of the present application as the positive electrode active material in the positive electrode sheet of the secondary battery, based on the unique structural stability of the sodium layered metal oxide, the material particles on the surface of the positive electrode active material layer are not easy to break or fall off, so that there are fewer side reactions on the surface of the positive electrode active material layer, thereby reducing the capacity attenuation phenomenon and improving the cycle performance and service life.
[0056] In a fourth aspect, an embodiment of the present application provides an electrical device, comprising the secondary battery provided in the third aspect of the embodiment of the present application.
[0057] By adopting the secondary battery provided in the third aspect of the embodiment of the present application, the electrical device can work for a longer period of time.
[0058] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0060] FIG1 is a schematic diagram of a sodium layered metal oxide before and after doping according to an embodiment of the present application;
[0061] FIG2 is a schematic flow chart of a method for preparing sodium layered metal oxide according to an embodiment of the present application;
[0062] FIG3 is a schematic structural diagram of an embodiment of a secondary battery of the present application;
[0063] FIG4 is an exploded schematic diagram of the secondary battery shown in FIG3 ;
[0064] FIG5 is a schematic structural diagram of an embodiment of a battery module according to the present application;
[0065] FIG6 is a schematic structural diagram of an embodiment of a battery pack according to the present application;
[0066] FIG7 is a schematic diagram of the exploded structure of the battery pack shown in FIG6 ;
[0067] FIG8 is a schematic diagram of an embodiment of an electrical device including a battery according to an embodiment of the present application as a power source;
[0068] FIG9 is an example of the present application Na 0.98 Ca 0.02 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 XRD curve of O2;
[0069] Figure 10 is a comparative example of NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 XRD curve of O2;
[0070] Figure 11 is a comparative example of the present invention. 0.98 Ca 0.02 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 XRD curve of O2;
[0071] Figure 12 is a comparative example of NaNi 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 XRD curve of O2.
[0072] Explanation of reference numerals: 10 - battery cell; 11 - housing; 12 - top cover assembly; 13 - electrode assembly; 20 - battery module; 30 - battery pack; 31 - upper case; 32 - lower case. DETAILED DESCRIPTION
[0073] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.
[0074] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0075] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0076] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0077] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0078] In the description of the embodiments of this application, the term "plurality" refers to two or more (including two). Similarly, "multiple groups" refers to two or more (including two groups), and "multiple sheets" refers to two or more (including two sheets). "At least one" refers to more than one (including one, two, three, etc.).
[0079] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.
[0080] In the description of the embodiments of the present application, unless otherwise expressly specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; internal connections between two components or interactions between two components. Those skilled in the art can understand the specific meanings of the above terms in the embodiments of the present application based on specific circumstances.
[0081] With the increasing depletion of traditional energy resources, the development of new energy storage devices is gaining increasing attention. Secondary batteries, in particular, have attracted significant attention due to their high energy density, high theoretical capacity, excellent cycle stability, and environmentally friendly properties. Secondary batteries are not only used in energy storage power systems such as hydropower, thermal power, wind power, and solar power plants, but are also widely used in electric vehicles such as electric bicycles, electric motorcycles, and electric vehicles, as well as in military equipment and aerospace. As the application areas of secondary batteries as power batteries continue to expand, their market demand is also growing, and the requirements for battery performance, such as cycle performance, are becoming increasingly stringent.
[0082] Lithium-ion batteries, a type of secondary battery, boast high energy density, long lifespan, and energy conservation and environmental friendliness. However, due to global lithium resource limitations and rising costs, their application in large-scale energy storage presents challenges. Sodium-ion batteries, with their advantages such as abundant sodium reserves, low cost, and unique battery safety characteristics, have become a key candidate for large-scale energy storage systems. Therefore, the development of resource-free, low-cost sodium-ion batteries holds great potential in the energy storage field.
[0083] Sodium layered metal oxides have the characteristics of high specific capacity, high compaction density, and adjustable voltage range, making them suitable as cathode materials for sodium-ion batteries. However, the structure of sodium layered metal oxides is unstable, and sodium layered metal oxides used as cathode materials in sodium-ion batteries are prone to phase transitions during the cyclic charge and discharge process.
[0084] During the charge and discharge process of currently commonly used sodium layered metal oxides, the release of sodium ions during the charge process weakens the interlayer interaction and increases the interlayer spacing. As the interlayer spacing increases, the phase stability decreases, making layer slip more likely to occur under thermodynamic drive. At the end of discharge, the phase transition can occur again, leading to stress accumulation and particle fragmentation in the sodium layered metal oxide particles, thereby reducing structural stability. Furthermore, the rupture of sodium layered metal oxide particles creates new surfaces, which may undergo side reactions such as surface oxygen loss phase transition, solvent molecule oxidation, and transition metal dissolution, leading to rapid battery capacity decay.
[0085] In order to solve the problem of unstable structure of sodium layered metal oxides, relevant technologies have modified sodium layered metal oxides, such as coating or doping modification. Surface coating modification is difficult to fundamentally improve the phase change of the internal structure of sodium layered metal oxides, and has little effect on inhibiting layer slip. Doping modification tends to ignore the sodium ion ion radius parameter. The ion radius of the doping elements generally used is close to that of transition metals, which makes it easy to form doping at the transition metal site. Excessive doping of inactive elements at the transition metal site can easily reduce the overall capacity. In addition, if low-valence doping elements are doped at the sodium site, it is still easy to produce phase change problems in the de-sodium state, resulting in insufficient stability.
[0086] Based on the above considerations, in order to solve the problem of structural instability of sodium layered metal oxides, the present invention combines theoretical calculations with experiments to research and design a new type of doped sodium layered metal oxide. By dual-site doping of the sodium site and transition metal M site of the sodium layered metal oxide, the sodium layered metal oxide has better stability, thereby significantly improving its cycle performance and service life. The following technical solution is proposed.
[0087] Sodium layered metal oxides
[0088] In the first aspect, the present invention provides a sodium layered metal oxide. As an embodiment of the present invention, the chemical formula of the sodium layered metal oxide in the present invention is: Na 1-x A x C y M 1-y O2.
[0089] Na 1-x A x C y M 1-y In O2, M includes a transition metal element; A includes at least one of Group IIA elements, Group V metal elements, Group VIA metal elements and Group IIIB elements, and the ionic radius of A is larger than the ionic radius of M; C includes at least one of Period III metal elements, Period IV metal elements and Period V metal elements, and the valence of C is less than or equal to the valence of M; x = 0.001 ~ 0.150, y = 0.001 ~ 0.500.
[0090] It should be noted that the elements of A, C, and M are different. For example, if an element appears in the A position, then C and M do not contain the element in the A position. The chemical elements in the embodiments of the present application are divided according to the periodic table of elements known in the art, that is, a list of chemical elements sorted from small to large according to the charge number of the element's nucleus. The periodic table has 7 periods and 16 groups. Each horizontal row is called a period, and each vertical row is called a group (Group VIII contains three vertical columns).
[0091] By adding unique A element species and C element species to the sodium layered metal oxide, the sodium layered metal oxide has good stability, which can improve its cycle performance and service life.
[0092] Chemical formula Na 1-x A x C y M 1-y In O2, A and C are doping elements, where A is the doping element for the sodium site and C is the doping element for M.
[0093] Doping refers to the modification of a material with a doping element, by replacing the position of the doping site with the doping element, generally changing the lattice constant of the material or the valence state of the elements in the material to improve the material performance; in the embodiment of the present application, the modification is performed by replacing the sodium site and the transition metal M site with the doping element.
[0094] The doping element A can satisfy the following requirements: (1) the ionic radius is larger than the ionic radius of the transition metal M; and (2) the valence of the doping element A after doping is larger than the valence of the sodium ion (i.e., +1). After such a doping element A is doped into the sodium site of the sodium layered metal oxide, there is a strong Coulomb interaction between the high-valence doping element A and the oxygen atoms. When the sodium layered metal oxide is in a desodiumized state, the strong Coulomb interaction between the doping element A and the oxygen atoms can inhibit the interlayer slip of the sodium layered metal oxide, making it less likely to undergo phase transition, thereby supporting the layered structure.
[0095] The doping element C can satisfy the following requirement: the valence of the doping element C after doping is less than or equal to the valence of the transition metal M. Because the valence of the doping element A after doping is greater than the valence of the sodium ion, the low-valence doping element C at the transition metal M site can effectively balance the valence state and reduce the lattice stress change caused by the valence change after A doping.
[0096] Therefore, the sodium layered metal oxide in the embodiment of the present application is doped with element A at the sodium site and element C at the transition metal M site. The dual-site doped sodium layered metal oxide has good stability and thus has good cycle performance and service life.
[0097] In some embodiments, the valence of the doping element A after doping is +2 to +4. For example, it can be +2, +3, or +4. As shown in FIG1 , by doping the sodium layered metal oxide with the doping element A having a valence of +2 to +4, the doping element A has a stronger Coulomb interaction with oxygen atoms than the sodium ion with a valence of +1. Therefore, when the sodium layered metal oxide is in the desodiumated state, layer slip is less likely to occur, and the doping element A acts as a good structural pillar, thereby improving the crystal structure stability of the sodium layered metal oxide.
[0098] In some embodiments, among the doping elements A, the IIA group elements include at least one of calcium, strontium, and barium, the V group metal elements include at least one of antimony and bismuth, the VIA group metal elements include tellurium, and the IIIB group elements include at least one of yttrium, cerium, and lanthanum.
[0099] It should be noted that the metal elements in this application refer to elements with metallic properties, including metalloids between metals and non-metals such as tellurium.
[0100] Specifically, the doping element A includes at least one of calcium (Ca), strontium (Sr), barium (Ba), antimony (Sb), bismuth (Bi), yttrium (Y), cerium (Ce), lanthanum (La), and tellurium (Te). Calcium, strontium, and barium can be doped with a valence of +2, antimony, bismuth, yttrium, and lanthanum can be doped with a valence of +3, and cerium and tellurium can be doped with a valence of +4. The ionic radius of calcium, strontium, barium, antimony, bismuth, yttrium, cerium, lanthanum, and tellurium is close to that of sodium ions, and their valence is higher than that of sodium ions. Therefore, these doping elements can be easily doped into the sodium sites of the sodium layered metal oxide. At the same time, the strong Coulomb interaction between these elements and oxygen atoms can suppress interlayer slip of the sodium layered metal oxide.
[0101] In some embodiments, the doping element A must include calcium. The ionic radius of calcium is closer to that of sodium, making it easier to dope at sodium sites. Furthermore, calcium doping can reduce the risk of additional structural distortion caused by doping, thereby improving structural stability. Therefore, calcium not only effectively dopes at sodium sites but also further stabilizes the crystal structure of the sodium layered metal oxide.
[0102] In some embodiments, the third period metal element of the doping element C includes at least one of magnesium and aluminum, the fourth period metal element includes at least one of zinc, gallium, and germanium, and the fifth period metal element includes zirconium.
[0103] Specifically, the doping element C includes at least one of zirconium (Zr), magnesium (Mg), aluminum (Al), zinc (Zn), gallium (Ga), and germanium (Ge). The ionic radius of zirconium, magnesium, aluminum, zinc, gallium, and germanium is close to or smaller than the ionic radius of the transition metal M, and their valence is less than or equal to that of the transition metal M. For example, when the transition metal M is trivalent iron or tetravalent manganese, the doping element can be selected from magnesium, aluminum, zinc, etc. The above-mentioned doping element C not only allows for easier doping into the transition metal M site, but also balances the valence state, reducing changes in lattice stress caused by large local valence state changes.
[0104] In some embodiments, the doping element C must contain aluminum. Aluminum can not only be well doped into the transition metal M site, but also better balance the valence state.
[0105] In some embodiments, M includes at least two of nickel (Ni), manganese (Mn), copper (Cu), and iron (Fe). It should be noted that when M includes multiple elements, the valence of the doping element C after doping is less than or equal to the valence of the transition metal M, which means that it is less than or equal to the valence of at least one transition metal in the transition metal M. The sodium layered metal oxide formed by multiple transition metals among nickel, manganese, copper, and iron not only makes it difficult for the transition metal ions of the transition metal layer to migrate, but also combines with the C doping element at the sodium site to better suppress phase transition and improve the electrochemical stability of the desodiumized state.
[0106] In some embodiments, M contains nickel, iron, and manganese. Nickel, iron, and manganese form transition metal elements at the M site. The sodium layered metal oxide formed by the three transition metals of nickel, iron, and manganese not only has a high specific capacity, but also is easy to dope with the doping element C.
[0107] In one embodiment, the molar ratio of nickel, iron, and manganese in M is (0.2-0.4):(0.2-0.4):(0.2-0.6). For example, the molar ratio of nickel, iron, and manganese is 0.2:0.2:0.6, or the molar ratio of nickel, iron, and manganese is 0.25:0.25:0.5, or the molar ratio of nickel, iron, and manganese is 0.3:0.3:0.4, or the molar amounts of nickel, iron, and manganese are the same. The sodium layered metal oxide formed by the three transition metals of nickel, iron, and manganese under the above molar ratio conditions has high specific capacity and good stability.
[0108] As an embodiment of the present application, the chemical formula Na 1-x A x C y M 1-yIn O2, x is the doping amount of the doping element A, y is the doping amount of the doping element C, x=0.001-0.150, y=0.001-0.400. In examples, x can be a typical but non-limiting value such as 0.001, 0.005, 0.010, 0.015, 0.020, 0.030, 0.050, 0.080, 0.100, 0.120, 0.150, etc., and x can be a typical but non-limiting value such as 0.001, 0.005, 0.010, 0.015, 0.020, 0.030, 0.050, 0.080, 0.100, 0.120, 0.150, 0.200, 0.250, 0.350, 0.380, 0.400, etc. At the same time, the values of x and y must maintain the system's electrical neutrality. For example, assuming the valence of dopant element A is a, the valence of dopant element C is b, and the valence of transition metal M is c, then (1-x) + ax + by + c(1-y) = 4. When dopant element A is added, the valence of transition metal M changes to maintain valence equilibrium.
[0109] Furthermore, x = 0.01 to 0.02, y = 0.01 to 0.02. Doping modification of the doping element A and the doping element C under the above-mentioned parameter mass conditions can greatly improve the stability of the sodium layered metal oxide while having little effect on the energy density of the sodium layered metal oxide.
[0110] In one embodiment, the sodium layered metal oxide has an O3 type crystal structure.
[0111] Sodium layered metal oxides can have a variety of different structures, including O3, P3, O'3, and P2 phases. O and P represent the octahedral and prismatic coordination structures of sodium ions, respectively. O3-type sodium layered metal oxides have high specific capacity and are well-suited for use as cathode materials in sodium-ion batteries.
[0112] In some embodiments, the chemical formula of the sodium layered metal oxide is Na 0.98 Ca 0.02 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 O2. When calcium is doped, the valence balance is maintained by the transition metal Mn valence change, that is, the 0.02 valence state increased by sodium doping calcium is reduced by 0.02 valence state through partial manganese valence change. Specifically, Na 0.98 Ca 0.02 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3In O₂, Na is +1, Ca is +2, Ni is +2, Fe is +3, and Al is +3. Approximately 0.02 mol of Mn atoms become +3, leaving approximately 0.31 mol of atoms at +4. O is -2, ultimately maintaining the system's electrical neutrality. The sodium layered metal oxides of the above chemical formula not only possess excellent structural stability but also high specific capacity and energy density, offering superior overall performance as positive electrode active materials.
[0113] Preparation method of sodium layered metal oxide
[0114] In the second aspect, the present invention provides a method for preparing a sodium layered metal oxide, namely, a sodium layered metal oxide having a general chemical formula of 1-x A x C y M 1-y Preparation method of sodium layered metal oxide of O2. As shown in Figure 2, the preparation method of sodium layered metal oxide includes the following steps:
[0115] S01: performing a first grinding process on a mixture containing a transition metal M source and a doping element C source, and then performing a first calcination process to obtain an intermediate product;
[0116] S02: The intermediate product is mixed with a sodium source and a doping element A source to perform a second grinding process, and then a second calcination process is performed to obtain a sodium layered metal oxide.
[0117] In the preparation process of the sodium layered metal oxide in the embodiment of the present application, the transition metal M site is first doped with C, and then the sodium site is doped with A, so that a sodium layered metal oxide doped with both the sodium site and the transition metal M site can be obtained. Since the preparation method of the sodium layered metal oxide in the embodiment of the present application is to prepare a sodium layered metal oxide with the general chemical formula Na 1-x A x C y M 1-y The sodium layered metal oxide material of O2 is ground and calcined to form a transition metal M site and a sodium site, respectively. The preparation method of the embodiment of the present application is not only easy to achieve doping, but also simple in process, and the obtained sodium layered metal oxide has good stability.
[0118] Step S01:
[0119] A transition metal source (M) can be understood as a soluble compound that can provide a source of the doping element (M). Specifically, the transition metal source (M) includes at least one of a soluble halide, acetate, carbonate, nitrate, sulfate, hydroxide, and oxide of M. For example, using iron as the transition metal (M), the iron source can include iron halides, iron acetate, iron carbonate, iron nitrate, iron sulfate, and the like. Similarly, other transition metals can be prepared by analogy. Soluble compounds corresponding to M can be formulated into solutions. The aforementioned transition metal source (M) materials are well suited to provide the M element for the preparation of sodium layered metal oxides.
[0120] A doping element C source can be understood as a compound that can provide a source of the doping element C. Specifically, the doping element C source includes at least one of soluble halides, acetates, carbonates, nitrates, sulfates, hydroxides, and oxides of C. For example, using zinc as the doping element C, the zinc source can include zinc halides, zinc acetate, zinc carbonate, zinc nitrate, zinc sulfate, and the like. The same applies to other doping elements C. Soluble compounds corresponding to C can be prepared into solutions. The aforementioned doping element C source materials are well suited to provide C for the preparation of sodium layered metal oxides.
[0121] In some embodiments, the steps of preparing the mixture containing the transition metal M source and the doping element C source include:
[0122] S011: preparing a solution of a transition metal M source and a solution of a doping element C source respectively;
[0123] S012: adding a complexing agent to the solution of the transition metal M source and the solution of the doping element C source respectively to carry out a complexing reaction to obtain a first gel-like substance and a second gel-like substance respectively;
[0124] S013: Mixing and drying the first gel-like substance and the second gel-like substance to obtain a mixture.
[0125] In the embodiment of the present application, a sol-gel method is adopted to prepare the transition metal M source and the doping element C source into solutions respectively, and respectively complex them with a complexing agent to form a gel-like substance. In this way, the mixing of the gel-state M source and C source can better achieve uniform doping.
[0126] In step S011, a solution of a transition metal M source can be prepared by dissolving the transition metal M source in water at a certain ratio, wherein the M concentration is 0.2 to 0.8 mol / L. A solution of a doping element C source can be prepared by dissolving the doping element C source in water at a certain ratio, wherein the C concentration is 0.2 to 2 mol / L.
[0127] In step S012: a complexing agent is added to the solution of the transition metal M source, the reaction temperature and pH value are controlled, and the reaction system obtains a first gel-like substance through a complex reaction; a complexing agent is added to the solution of the doping element C source, the reaction temperature and pH value are controlled, and the reaction system obtains a second gel-like substance through a complex reaction.
[0128] In some embodiments, the complexing agent is an organic complexing agent, including at least one of citric acid, oxalic acid, glutamic acid, polypropylene alcohol, polyvinylidene fluoride and polyacrylamide; the complexing agent can be added by mixing a complexing agent solution with a solution of a transition metal M source or a solution of a doping element C source.
[0129] In some embodiments, the conditions for the complexation reaction include: a temperature of 40 to 100° C., which may be, but not limited to, typical but non-limiting temperatures such as 45° C., 50° C., 60° C., 70° C., and 80° C.; a pH value of 7 to 11, which may be, but not limited to, typical but non-limiting pH values such as pH = 7.0, 7.5, 8, 9, 10, and 11.
[0130] By selecting the complexing agent and complexing reaction conditions described above, a gentle complexing reaction can be performed, resulting in the transition metal M source and the doping element C source forming a first gel-like substance and a second gel-like substance, respectively. The first and second gel-like substances are then mixed and dried to form a mixture, which facilitates subsequent doping processes.
[0131] In step S013, drying is primarily performed to remove the solvent from the gel-like material. The drying temperature can be between 100°C and 120°C. Drying under these conditions minimizes the impact on the quality and stability of the mixture. After drying, the mixture undergoes a first grinding step and a first calcination step, yielding an intermediate product, which can be understood as a transition metal hydroxide modified by a doping with a transition metal layer.
[0132] In some embodiments, the first grinding may be a ball milling process.
[0133] In some embodiments, the first calcination treatment includes two calcination stages: (1) first calcination at 800-950°C for 6-10 hours; in exemplary embodiments, the temperature may be, but is not limited to, 800°C, 850°C, 900°C, 920°C, 940°C, and other typical but non-limiting temperatures, and the time may be, but is not limited to, 6 hours, 8 hours, 9 hours, 10 hours, and other typical but non-limiting times. (2) then cooling to 200-600°C and calcining for 3-6 hours; in exemplary embodiments, the temperature may be, but is not limited to, 200°C, 250°C, 300°C, 400°C, 500°C, and other typical but non-limiting temperatures, and the time may be, but is not limited to, 3 hours, 4 hours, 5 hours, 6 hours, and other typical but non-limiting times. The above-mentioned first calcination treatment conditions of first high-temperature long-term calcination and then cooling for a short-term calcination can well achieve C element doping at the M site.
[0134] Step S02:
[0135] The intermediate product obtained in step S01 is mixed with a sodium source and a doping element A source, subjected to a second grinding process, and then subjected to a second calcination process to obtain a target product: sodium layered metal oxide.
[0136] In the step of mixing the intermediate product with the sodium source and the doping element A source, the sodium source and the doping element A source can be prepared separately as solutions, and then a complexing agent is added to carry out a complexation reaction to form a gel-like substance. The gel-like substance of the sodium source and the doping element A source is dried and then mixed with the intermediate product. This sol-gel method can achieve more uniform doping.
[0137] The source of doping element A can be understood as a soluble compound that can provide a source of doping element A. Specifically, the source of doping element A includes at least one of soluble halides, acetates, carbonates, nitrates, sulfates, hydroxides, and oxides of A. Taking calcium as the doping element A as an example, the calcium source can be calcium halide, calcium acetate, calcium nitrate, etc., and the same applies to other doping elements. The soluble compounds corresponding to A can be prepared into a solution. The material types of the above-mentioned doping element A sources can well provide element A for the preparation of sodium layered metal oxides. The sodium source includes at least one of sodium halide, sodium acetate, sodium carbonate, sodium nitrate, sodium sulfate, sodium hydroxide, and sodium oxide. The material types of the above-mentioned sodium source can well provide sodium for the preparation of sodium layered metal oxides.
[0138] In some embodiments, the second milling may be a ball milling process.
[0139] In some embodiments, the second calcination treatment includes two calcination stages: (1) first calcination at 800-950°C for 6-10 hours; in exemplary embodiments, the temperature may be, but is not limited to, 800°C, 850°C, 900°C, 920°C, 940°C, and other typical but non-limiting temperatures, and the time may be, but is not limited to, 6 hours, 8 hours, 9 hours, 10 hours, and other typical but non-limiting times. (2) then cooling to 200-600°C and calcining for 3-6 hours; in exemplary embodiments, the temperature may be, but is not limited to, 200°C, 250°C, 300°C, 400°C, 500°C, and other typical but non-limiting temperatures, and the time may be, but is not limited to, 3 hours, 4 hours, 5 hours, 6 hours, and other typical but non-limiting times. The first calcination treatment conditions of first high-temperature long-term calcination and then cooling for a short-term calcination can well achieve the doping of A element at the sodium site.
[0140] secondary batteries
[0141] In a third aspect, an embodiment of the present application provides a secondary battery, wherein the positive electrode of the secondary battery contains the sodium layered metal oxide provided in the first aspect of the embodiment of the present application and / or the sodium layered metal oxide prepared by the preparation method provided in the second aspect of the embodiment of the present application.
[0142] By using the general formula of Na in the positive electrode of the secondary battery 1-x A x C y M 1-y O2's sodium layered metal oxide is used as the positive electrode active material. Based on the unique structural stability of sodium layered metal oxide, the material particles on the surface of the positive electrode active material layer are not easy to break or fall off. In this way, there are fewer side reactions on the surface of the positive electrode active material layer, thereby reducing capacity attenuation and improving cycle performance and service life.
[0143] In one embodiment, the positive electrode sheet of the secondary battery provided in the embodiment of the present application includes: (1) a current collector; and (2) a positive electrode active material layer, wherein the positive electrode active material layer is combined with the current collector. The positive electrode active material layer contains a positive electrode active material, and the positive electrode active material is the sodium layered metal oxide provided in the first aspect of the embodiment of the present application and / or the sodium layered metal oxide prepared by the preparation method provided in the second aspect of the embodiment of the present application.
[0144] In the embodiments of this application, the positive electrode active material layer refers to the active layer contained in the positive electrode sheet, which at least contains a layer structure of positive electrode material and is combined with the current collector. By using the sodium layered metal oxide provided by the first aspect of the embodiments of this application and / or the sodium layered metal oxide prepared by the preparation method provided by the second aspect as the positive electrode active material in the positive electrode sheet, the unique structural stability of the sodium layered metal oxide makes the material particles on the surface of the positive electrode active material layer less likely to break or fall off. In this way, the side reactions on the surface of the positive electrode active material layer are reduced, thereby reducing capacity fading and improving cycle performance and service life.
[0145] In one embodiment, the positive electrode active material layer may be combined with at least one surface of the current collector.
[0146] In some embodiments, the current collector of the positive electrode sheet is also called the positive electrode current collector, and a metal foil or a composite current collector may be used. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0147] In some embodiments, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0148] In some embodiments, the positive electrode active material layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0149] In the exemplary embodiment, the secondary battery of the present application includes a positive electrode sheet, a separator and a negative electrode sheet. That is, the positive electrode sheet contained in the secondary battery contains the general formula of the above embodiment of the present application, Na 1-x A x C y M 1-y Thus, the secondary battery of the embodiment of the present application has good cycle stability, low capacity decay during the cycle, and significantly improved cycle performance.
[0150] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are inserted and removed from the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.
[0151] In some embodiments, the electrolyte acts as a conductive medium between the positive and negative electrodes. The present invention does not specifically limit the type of electrolyte, and the electrolyte may be selected based on the needs. For example, the electrolyte may be liquid, gel, or solid.
[0152] In some embodiments, the secondary battery of the present application may include any one of a battery cell, a battery module, and a battery pack.
[0153] A battery cell is a battery cell comprising a battery housing and a cell encapsulated within the housing. The shape of a battery cell is not particularly limited and can be cylindrical, square, or any other shape. A square-shaped battery cell 10 is shown in FIG3 .
[0154] In some embodiments, as shown in Figure 4, the outer packaging of the battery cell 10 may include a shell 11 and a top cover assembly 12. The shell 11 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 11 has an opening connected to the receiving cavity, and the top cover assembly 12 is used to cover the opening to close the receiving cavity. The positive electrode, diaphragm and negative electrode sheet contained in the secondary battery of the embodiment of the present application can be formed into an electrode assembly 13 through a winding process and / or a lamination process. The electrode assembly 13 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 13. The number of electrode assemblies 13 contained in the battery cell 10 can be one or more, which can be adjusted according to actual needs.
[0155] The preparation method of the battery cell 10 is well known. In some embodiments, the positive electrode, separator, negative electrode sheet, and electrolyte can be assembled to form the battery cell 10. As an example, the positive electrode, separator, and negative electrode sheet can be wound or laminated to form the electrode assembly 13. The electrode assembly 13 is placed in an outer package, dried, and then injected with electrolyte. The battery cell 10 is then vacuum packaged, allowed to stand, formed, and shaped.
[0156] A battery module is assembled from the battery cells 10 , that is, it may contain a plurality of battery cells 10 , and the specific number can be adjusted according to the application and capacity of the battery module.
[0157] In some embodiments, FIG5 is a schematic diagram of an exemplary battery module 20. As shown in FIG5 , in the battery module 20, multiple battery cells 10 may be arranged sequentially along the length of the battery module 20. Of course, they may also be arranged in any other manner. Furthermore, the multiple battery cells 10 may be secured by fasteners. Optionally, the battery module 20 may further include a housing having a storage space, wherein the multiple battery cells 10 are accommodated in the storage space.
[0158] A battery pack is assembled from the battery cells 10 described above, and may contain multiple battery cells 10, wherein multiple battery cells 10 may be assembled into the battery module 20 described above. The specific number of battery cells 10 or battery modules 20 contained in a battery pack may be adjusted according to the application and capacity of the battery pack.
[0159] In the embodiment, Figures 6 and 7 are schematic diagrams of an exemplary battery pack 30. The battery pack 30 may include a battery box and multiple battery modules 20 disposed within the battery box. The battery box includes an upper box body 31 and a lower box body 32. The upper box body 31 covers the lower box body 32 and forms an enclosed space for accommodating the battery modules 20. The multiple battery modules 20 may be arranged in any manner within the battery box.
[0160] Electrical devices
[0161] Fourthly, embodiments of the present application further provide an electrical device comprising the secondary battery of the aforementioned embodiments. The secondary battery can serve as both a power source and an energy storage unit for the electrical device. Consequently, the electrical device of the embodiments of the present application has a long standby or battery life.
[0162] Electrical devices may include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc. These electrical devices may use secondary batteries, battery modules, or battery packs based on their usage requirements.
[0163] Figure 8 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.
[0164] As another example, the electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a secondary battery as a power source.
[0165] Example
[0166] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0167] 1. Sodium layered metal oxide and its preparation method embodiment
[0168] Example A1
[0169] A sodium layered metal oxide with the chemical formula: Na 0.98 Ca 0.02 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 O2. The preparation method of sodium layered metal oxide comprises the following steps:
[0170] S11: Preparation of intermediate products:
[0171] Solution Preparation: Dissolve nickel nitrate, iron nitrate, and manganese nitrate in water according to the chemical formula molar ratio to obtain a transition metal salt solution with a total transition metal M concentration of approximately 0.5 mol / L. Dissolve aluminum nitrate in water to obtain an aluminum salt solution with a concentration of 2 mol / L. Dissolve citric acid in water to obtain a complexing agent solution with a concentration of 0.5 mol / L.
[0172] The transition metal salt solution and the complexing agent solution are mixed, and the temperature is controlled at 50° C. and the pH is controlled at 8, until a first gel-like substance is obtained; the aluminum salt solution and the complexing agent solution are mixed, and the temperature is controlled at 50° C. and the pH is controlled at 8, until a second gel-like substance is obtained.
[0173] The first gel-like substance and the second gel-like substance are mixed, dried at 110°C for 10 minutes, and then ball-milled for 30 minutes. After ball-milling, the mixture is calcined at 800°C for 6 hours and then at 250°C for 3 hours to obtain an intermediate product (i.e., a transition metal hydroxide doped with a transition metal layer).
[0174] S12: The intermediate product was mixed with sodium nitrate and calcium nitrate according to the chemical formula and ball-milled for a second time for 30 minutes. After ball-milling, the intermediate product was calcined at 800°C for 6 hours and then at 250°C for 3 hours to obtain the sodium layered metal oxide of the above chemical formula. Figure 9 shows the XRD pattern of the characterization.
[0175] Example A2
[0176] A sodium layered metal oxide with the chemical formula: Na 0.98 Bi0.02 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different.
[0177] Example A3
[0178] A sodium layered metal oxide with the chemical formula: Na 0.98 Ca 0.02 Ni 1 / 3 Fe 0.31 Mg 0.02 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different.
[0179] Example A4
[0180] A sodium layered metal oxide with the chemical formula: Na 0.98 Ca 0.02 Ni 1 / 3 Fe 0.31 W 0.02 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different.
[0181] Example A5
[0182] A sodium layered metal oxide with the chemical formula: Na 0.98 Ca 0.03 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different.
[0183] Example A6
[0184] A sodium layered metal oxide with the chemical formula: Na 0.98 Ca 0.04 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different.
[0185] Comparative Example A1
[0186] A sodium layered metal oxide with the chemical formula: NaNi1 / 3 Fe 1 / 3 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different. Figure 10 is the XRD pattern of the characterization.
[0187] Comparative Example A2
[0188] A sodium layered metal oxide with the chemical formula: Na 0.98 Ca 0.02 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different. Figure 11 is the XRD pattern of the characterization.
[0189] Comparative Example A3
[0190] A sodium layered metal oxide with the chemical formula: NaNi 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different. Figure 12 is the XRD pattern of the characterization.
[0191] Comparative Example A4
[0192] A sodium layered metal oxide with the chemical formula: Na 0.98 Li 0.02 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different.
[0193] Comparative Example A5
[0194] A sodium layered metal oxide with the chemical formula: Na 0.8 Ca 0.2 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 The preparation method of sodium layered metal oxide is basically the same as that of Example 1 except that the corresponding raw materials and amounts are different.
[0195] 2. Secondary Battery Cell Example
[0196] Example B1 to Example B6 and Comparative Examples B1 to Comparative Examples B5;
[0197] The present embodiments B1 to B6 and comparative examples B1 to B5 respectively provide a secondary battery cell, each of which includes a battery cell formed by a positive electrode sheet, a separator, and a negative electrode sheet, and also includes an electrolyte. The positive electrode active material in the positive electrode sheets of embodiments B1 to B6 and comparative examples B1 to B5 corresponds to the sodium layered metal oxide provided in embodiments A1 to A6 and comparative examples A1 to A5, respectively. For example, the sodium layered metal oxide in the above embodiment A1 serves as the positive electrode active material in the battery cell of the secondary battery embodiment B1, the sodium layered metal oxide in embodiment A2 serves as the positive electrode active material in the battery cell of the secondary battery embodiment B2, and so on. The sodium layered metal oxide in comparative example A5 serves as the positive electrode active material in the battery cell of the secondary battery comparative example B5.
[0198] The positive electrode sheet was prepared as follows:
[0199] Using methyl pyrrolidone (NMP) as a solvent, sodium layered metal oxide, conductive agent (carbon nanotubes), and binder (PVDF) were mixed in a mass ratio of 8:1:1 to prepare a positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil for double-sided coating, with the surface density of each single side being 0.25 mg / mm 2 After sufficient vacuum drying, cold pressing and slitting, the positive electrode sheet is obtained.
[0200] Negative electrode: Metallic sodium serves as the counter electrode, i.e. the negative electrode.
[0201] Electrolyte: Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed at a volume ratio of 1:1 at room temperature, and NaPF6 was added to the mixed solution to obtain a solution with a concentration of 1 mol / L as the electrolyte.
[0202] Secondary battery assembly: In a low-humidity constant temperature room, in an argon atmosphere glove box, the positive and negative electrode sheets prepared as above are stacked in the order of "positive electrode-separator-negative electrode", filled with electrolyte, and assembled into button batteries.
[0203] Performance Testing
[0204] (1) Material characterization
[0205] By comparing and analyzing the sodium layered metal oxide XRD curve of Example A1 (Figure 9), the sodium layered metal oxide XRD curve of Comparative Example A1 (Figure 10), the sodium layered metal oxide XRD curve of Comparative Example A2 (Figure 11), and the sodium layered metal oxide XRD curve of Comparative Example A3 (Figure 12), it can be seen that Example A1 of the present application achieves doping of calcium and aluminum.
[0206] (2) Battery charge and discharge test
[0207] The secondary battery cells of the above Examples B1-B6 and Comparative Examples B1-B5 were tested respectively.
[0208] The charge and discharge test conditions were: test temperature 45°C, charge and discharge rate 0.1C, charge and discharge cut-off voltage 2.0-4.2V (vs. Na+ / Na), and 300 cycles. The test results are shown in Table 1.
[0209] Table 1
[0210] From the test results in Table 1, we can see that:
[0211] Compared to the comparative examples in which the sodium layered metal oxide is undoped or doped at one position, the embodiments of the present application can effectively improve the cycle performance of the secondary battery by co-doping the sodium position and the transition metal M position, and a small amount of doping has little effect on the first charge capacity. Through Example B1, Example B5, Example B6 and Comparative Example B5, it can be found that when Ca is excessively doped to 2%, the cycle performance and capacity of the secondary battery are significantly affected, and when the Ca doping concentration is adjusted from 4% to 2%, the corresponding secondary battery capacity is improved, and the corresponding cycle capacity retention rate is also improved, indicating that a Ca doping concentration of 2% is more effective.
[0212] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A sodium layered metal oxide, characterized in that The chemical formula of the sodium layered metal oxide is: 1-x A x C y M 1-y O2; among them, M contains transition metal elements; A comprises at least one of a Group IIA element, a Group V metal element, a Group VIA metal element, and a Group IIIB element, and the ionic radius of A is greater than the ionic radius of M; C includes at least one of the third period metal elements, the fourth period metal elements and the fifth period metal elements, and the valence of C is less than or equal to the valence of M; x=0.001~0.150, y=0.001~0.
500.
2. The sodium layered metal oxide according to claim 1, characterized in that The A is a doping element for the sodium site, and the C is a doping element for the M.
3. The sodium layered metal oxide according to claim 1 or 2, characterized in that The valence of A is +2 to +4.
4. The sodium layered metal oxide according to any one of claims 1 to 3, characterized in that The IIA group element in A includes at least one of calcium, strontium and barium, the V group metal element includes at least one of antimony and bismuth, the VIA group metal element includes tellurium, and the IIIB group element includes at least one of yttrium, cerium and lanthanum; or, The A contains calcium element.
5. The sodium layered metal oxide according to any one of claims 1 to 4, characterized in that The third period metal element in C includes at least one of magnesium and aluminum, the fourth period metal element includes at least one of zinc, gallium and germanium, and the fifth period metal element includes zirconium; or, The C contains aluminum element.
6. The sodium layered metal oxide according to any one of claims 1 to 5, characterized in that The M includes at least two of nickel, manganese, copper and iron; or, The M includes nickel, iron and manganese.
7. The sodium layered metal oxide according to claim 6, characterized in that The molar ratio of nickel, iron and manganese in the M is (0.2-0.4): (0.2-0.4): (0.2-0.6).
8. The sodium layered metal oxide according to any one of claims 1 to 7, characterized in that x=0.01~0.02, y=0.01~0.
02.
9. The sodium layered metal oxide according to any one of claims 1 to 8, characterized in that The sodium layered metal oxide has an O3 type crystal structure.
10. The sodium layered metal oxide according to any one of claims 1 to 9, characterized in that The chemical formula of the sodium layered metal oxide is Na 0.98 Ca 0.02 Ni 1 / 3 Fe 0.31 Al 0.02 Mn 1 / 3 O2.
11. A method for preparing a sodium layered metal oxide according to any one of claims 1 to 10, characterized in that: The following steps are involved: The mixed material containing the transition metal M source and the doping element C source is subjected to a first grinding process, and then subjected to a first calcination process to obtain an intermediate product; The intermediate product is mixed with a sodium source and a doping element A source to perform a second grinding process, and then a second calcination process is performed to obtain the sodium layered metal oxide.
12. The preparation method according to claim 11, characterized in that: The steps of preparing the mixture containing the transition metal M source and the doping element C source include: Separately preparing an aqueous solution of the transition metal M source and an aqueous solution of the doping element C source; Adding a complexing agent to the aqueous solution of the transition metal M source and the aqueous solution of the doping element C source to carry out a complexing reaction, thereby obtaining a first gel-like substance and a second gel-like substance respectively; The first gel-like substance and the second gel-like substance are mixed and dried to obtain the mixture.
13. The preparation method according to claim 12, characterized in that: Satisfy one or more of the following (1) to (3): (1) The complexing agent includes at least one of citric acid, oxalic acid, glutamic acid, polypropylene alcohol, polyvinylidene fluoride and polyacrylamide; (2) The temperature of the complexation reaction is 40 to 100° C.; (3) The pH value of the complex reaction is 7-11.
14. The preparation method according to any one of claims 11 to 13, characterized in that: The first calcination treatment comprises: calcining at 800-950° C. for 6-10 hours, then cooling to 200-600° C. for calcining for 3-6 hours; and / or, The second calcination treatment includes: calcining at 800-950° C. for 6-10 hours, and then cooling to 200-600° C. for calcining for 3-6 hours.
15. The preparation method according to any one of claims 11 to 14, characterized in that: Satisfy one or more of the following (1) to (4): (1) The transition metal M source includes at least one of a soluble halide, acetate, carbonate, nitrate, sulfate, hydroxide and oxide of M; (2) the doping element C source includes at least one of soluble halogen salts, acetates, carbonates, nitrates, sulfates, hydroxides and oxides of C; (3) the doping element A source includes at least one of a soluble halide, acetate, carbonate, nitrate, sulfate, hydroxide and oxide of A; (4) The sodium source includes at least one of sodium halide, sodium acetate, sodium carbonate, sodium nitrate, sodium sulfate, sodium hydroxide and sodium oxide.
16. A secondary battery, characterized in that: The positive electrode sheet of the secondary battery contains the sodium layered metal oxide according to any one of claims 1 to 10 and / or the sodium layered metal oxide prepared by the preparation method according to any one of claims 11 to 15.
17. An electrical device, characterized in that: Includes the secondary battery as claimed in claim 16.
Citation Information
Patent Citations
Sodium layered metal oxides and their preparation methods, secondary batteries and electrical devices
CN116314728B
Positive electrode active material, preparation method thereof and sodium ion battery
CN111554919A
Layered oxide positive electrode, preparation method and application thereof and sodium-ion battery containing layered oxide positive electrode
CN111564605A
High-entropy doped manganese-based layered oxide, preparation method thereof, sodium ion battery positive electrode material and battery
CN116062807A
Sodium layered metal oxide and preparation method thereof, secondary battery and electric device
CN116314728A
Cited By
High-entropy doped manganese / iron-based layered material, preparation method thereof, pole piece and battery
CN120048897A