Battery separator and preparation method therefor, and secondary battery and electric device
By setting up a conductive coating on the lithium battery separator, the short circuit risk caused by lithium dendrites piercing the separator is solved, the time of short circuit occurs is extended, the risk of accidents is reduced, and the warning time is provided.
Patent Information
- Application Number
- PCT/CN2023/140735
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2023-12-21
- Publication Date
- 2024-11-21
AI Technical Summary
During multiple charge and discharge cycles of lithium batteries, the growth of lithium dendrites due to the uneven deposition of lithium ions increases the risk of the diaphragm being pierced, which in turn causes catastrophic accidents such as battery short circuit, ignition, gas production explosions, etc.
The conductive coating is provided on the surface of the separator side of the lithium battery. The conductivity of the coating is 102-106S/m. It contains conductive materials such as carbon nanotubes and insulating materials such as aluminum oxide to form a partial conductive separator. When lithium dendrites penetrate, it penetrates the membrane. The insulation side is intercepted by the conductive coating, forming a low-current micro-short circuit, extending the time when the short circuit occurs.
It effectively reduces the risk of short circuit after lithium dendrites pierce the diaphragm, provides a longer time for the battery management system to warn in time, and reduces the damage and losses caused by serious accidents.
Smart Images

Figure CN2023140735_21112024_PF_FP_ABST
Abstract
Description
Battery separator and preparation method thereof, secondary battery and electric device
[0001] Citation of Related Applications
[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on May 16, 2023, with application number 202310551408.7 and invention name “Battery separator and preparation method thereof, secondary battery and electrical device”, the entire contents of which are incorporated by reference in this application. Technical Field
[0003] The present application relates to the field of batteries, and in particular to a battery separator and a preparation method thereof, a secondary battery and an electrical device. Background Art
[0004] With the continuous development of the lithium battery industry, the demand for higher energy density has brought challenges to battery safety, and the use of thinner separators increases the risk of separator puncture. Among them, lithium dendrites are one of the problems encountered during the use of lithium batteries. During the battery's multiple charge and discharge cycles, due to the uneven deposition of lithium ions, lithium dendrites will continue to grow on the lithium metal surface. A large number of dendrites exerts great stress on the separator, causing it to be punctured, leading to catastrophic accidents such as battery short circuits, fires, and gas explosions.
[0005] Summary of the Invention
[0006] The main purpose of this application is to propose a battery separator and its preparation method, a secondary battery and an electrical device, aiming to provide a way to alleviate the risk of battery short circuit caused by lithium dendrites piercing the separator.
[0007] In a first aspect, the present application provides a battery separator, comprising:
[0008] basement membrane; and
[0009] The coating layer is arranged on the surface of the side of the base film facing the cathode of the battery, and the material of the coating layer includes a conductive material and an insulating material.
[0010] In the technical solution of the embodiment of the present application, a conductive material and an insulating material with a conductivity of 10 is provided on the surface of the base film facing the cathode of the battery. 2 ~10 6S / m conductive coating, thus, one side of the base film of the battery separator is insulating, while the coating side is conductive, so that the battery separator can be called a "partially conductive separator". When this battery separator is used in a lithium battery, when the lithium dendrites grow to completely penetrate the side of the base film where no coating is set (i.e., the insulating side), the lithium dendrites will be intercepted by the conductive coating and will not directly contact the cathode. At the same time, a low-current micro-short circuit is formed by the conductive coating, thereby extending the time from the short circuit to the occurrence of a serious accident.
[0011] In some embodiments, the electrical conductivity of the coating is 10 2 ~10 6 S / m. By controlling the conductivity of the coating at 10 2 ~10 6 Within the S / m range, the obtained battery separator has a significant effect on alleviating battery short circuit conditions.
[0012] In some embodiments, the conductive material includes at least one of carbon nanotubes, graphene, graphene oxide, carbon black, polystyrene sulfonate, polyaniline, nickel, copper, and platinum. Selecting at least one of the above substances as the conductive material has good electrical conductivity.
[0013] In some embodiments, the insulating material includes at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate, and magnesium fluoride. Selecting at least one of the above substances as the insulating material is low-cost, readily available, and allows for easy control of the electrical conductivity of the coating.
[0014] In some embodiments, the conductive material is in granular form, and the Dv50 of the conductive material is 0.1 to 10 μm. Selecting a granular conductive material with a Dv50 of 0.1 to 10 μm is advantageous for regulating the thickness of the coating and its apparent properties.
[0015] In some embodiments, the conductive material is in granular form, and the Dv50 of the conductive material is 0.1 to 10 μm. By selecting a granular conductive material with a Dv50 of 1 to 3 μm, the conductive material is more easily dispersed in the slurry used to prepare the coating, and the surface of the subsequent coating is smoother and more uniform.
[0016] In some embodiments, the insulating material is in granular form, and the Dv50 of the insulating material is 0.1 to 10 μm. Selecting a granular insulating material with a Dv50 of 0.1 to 10 μm is advantageous for regulating the thickness of the coating and its apparent properties.
[0017] In some embodiments, the insulating material is in granular form, and the Dv50 of the insulating material is 0.1 to 10 μm. By selecting a granular insulating material with a Dv50 of 1 to 3 μm, the insulating material is more easily dispersed in the slurry used to prepare the coating, and the surface of the subsequent coating is smoother and more uniform.
[0018] In some embodiments, the mass fraction of the conductive material in the coating is 30-90%. By controlling the mass fraction of the conductive material to 30-90%, the conductivity of the coating can be adjusted to match the requirements of batteries of various structures and capacities.
[0019] In some embodiments, the mass ratio of the conductive material to the insulating material is 30 to 90: 1 to 64. By controlling the addition ratio of the conductive material to the insulating material, the conductivity of the coating can be regulated.
[0020] In some embodiments, the coating material further comprises a binder. The addition of the binder allows the coating to better adhere to the base film, thereby improving the structural stability of the battery separator.
[0021] In some embodiments, the binder includes at least one of polyacrylate, acrylic acid, carboxymethyl cellulose, and polyvinylidene fluoride. Selecting at least one of the above substances as the binder can provide a stronger bond with the base film.
[0022] In some embodiments, the mass ratio of the binder to the conductive material is 5 to 10:30 to 90. By controlling the addition ratio of the binder, it is advantageous to obtain a coating with suitable conductivity and good bonding with the base film.
[0023] In some embodiments, the coating material further comprises a dispersant. The addition of the dispersant helps to adjust the dispersion of the solid matter in the coating, thereby obtaining a more uniform coating with better apparent quality.
[0024] In some embodiments, the dispersant includes at least one of polyethylene glycol and polyacrylamide. Selecting at least one of the above substances as the dispersant has a good dispersion effect on solid matter.
[0025] In some embodiments, the mass ratio of the dispersant to the conductive material is 1 to 5:30 to 90. By controlling the addition ratio of the dispersant, the dispersibility of the solid material can be greatly improved, thereby facilitating the reduction of the difficulty of coating processing and preparation.
[0026] In some embodiments, the base film material includes at least one of polyolefins, polyethers, polyetheretherketones, polyimides, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymers, and copolymers containing C-H bonds. Using at least one of the above-mentioned materials as the base film material can result in a battery separator having superior overall performance.
[0027] In a second aspect, the present application provides a method for preparing a battery separator, comprising the following steps:
[0028] Mixing conductive material, insulating material, binder and solvent to prepare coating slurry;
[0029] applying the coating slurry onto a base film;
[0030] curing the coating slurry on the base film to form a coating to prepare a battery separator;
[0031] Wherein, the coating slurry includes conductive material and insulating material.
[0032] In the technical solution of the embodiment of the present application, a coating slurry containing a conductive material and an insulating material is coated on the surface of one side of the base film, and a conductive coating is formed on the base film by curing. When the prepared battery separator is used in a lithium battery, when the lithium dendrites grow to completely penetrate the side of the base film where no coating is set, the lithium dendrites will be intercepted by the conductive coating and will not directly contact the cathode. At the same time, a low-current micro-short circuit is formed by the conductive coating, thereby prolonging the time from the short circuit to the occurrence of a serious accident.
[0033] In some embodiments, the solvent includes at least one of acetone, deionized water, methyl ethyl ketone, and 3-pentanone. Selecting at least one of the above-mentioned substances as the solvent facilitates the dispersion of the conductive material, insulating material, and the like, thereby obtaining a slurry having an appropriate viscosity and uniform dispersion of solid matter.
[0034] In some embodiments, the solvent includes acetone. When acetone is selected as the solvent, the solid matter is more fully dispersed, and the coating slurry obtained is more evenly applied on the base film, which is conducive to obtaining a more uniform coating.
[0035] In some embodiments, the solid content of the coating slurry is 40-45%. By controlling the solid content of the coating slurry within the range of 40-45%, the coating slurry has an appropriate viscosity, good coating performance, and fast curing speed.
[0036] In some embodiments, the step of curing the coating slurry on the base film to form a coating comprises:
[0037] The base film coated with the coating slurry is placed at a temperature of 40 to 45° C. and dried for 25 to 30 seconds.
[0038] The coating slurry is cured and formed into a coating on the base film by drying at 40-45° C. for 20-25 seconds. The formed coating has good surface quality, good bonding with the base film, and fast curing rate.
[0039] In a third aspect, the present application provides a secondary battery, which includes the battery separator in the above embodiment or the battery separator prepared in the above embodiment.
[0040] In a fourth aspect, the present application provides an electrical device, which includes the secondary battery in the above embodiment. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without paying any creative work.
[0042] FIG1 is a schematic structural diagram of a battery separator in some embodiments of the present application.
[0043] Description of Figure Numbers:
[0044] The realization of the objectives, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0045] Below, the battery separator and its preparation method, secondary battery and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0046] The "ranges" disclosed herein are defined in terms of lower and upper limits, where a given range is defined by selecting a lower limit and an upper limit, and the selected lower and upper limits define the boundaries of the particular range. Ranges defined in this manner can be inclusive or exclusive of the end values and can be combined arbitrarily, i.e., any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60 to 120 and 80 to 110 are listed for a particular parameter, it is understood that ranges of 60 to 110 and 80 to 120 are also contemplated. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, the following ranges are all contemplated: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5. In this application, unless otherwise indicated, the numerical range "a to b" is a shorthand representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0047] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0048] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0049] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0050] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0051] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0052] Currently, market developments indicate that power batteries are becoming increasingly widely used. They are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric vehicles, as well as in military equipment and aerospace. As power battery applications continue to expand, market demand is also growing.
[0053] Currently, market developments indicate that power batteries are becoming increasingly widely used. They are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric vehicles, as well as in military equipment and aerospace. As power battery applications continue to expand, market demand is also growing.
[0054] In the actual use of secondary batteries, lithium dendrites are one of their main problems. During the battery's multiple charge and discharge cycles, due to the uneven deposition of lithium ions, lithium dendrites will continue to grow on the lithium metal surface. A large number of dendrites exert great stress on the diaphragm, causing the diaphragm to be punctured, leading to catastrophic accidents such as battery short circuits, fires, and gas explosions. After research, the inventors found that the current use of functional coatings to inhibit the growth of lithium dendrites can only delay the penetration of lithium dendrites and cannot alleviate the short circuit caused by lithium dendrites puncturing the diaphragm. The subsequent short circuit can still lead to serious failures and accidents.
[0055] Based on the above problems, the inventors have conducted in-depth research and proposed a new type of battery separator that can reduce the short circuit distance and control failure. Specifically, the present application provides a battery separator, as shown in Figure 1, which includes a base film 10 and a coating 20. The coating 20 is provided on the side of the base film 10 facing the cathode of the battery. The conductivity of the coating 20 is 10 2 ~10 6 S / m, the material of the coating 20 includes conductive materials and insulating materials.
[0056] In the technical solution of the embodiment of the present application, a conductive material and an insulating material with a conductivity of 10 are provided on the surface of the base film 10 facing the battery cathode. 2 ~10 6S / m coating 20, thus, one side of the base film 10 of the battery separator is insulated (the resistance of the insulating side is greater than 9990 megohms measured by an insulation resistance meter), and the side of the coating 20 is conductive, so that the battery separator can be called a "partially conductive separator". When this battery separator is used in a lithium battery, when the lithium dendrites grow to completely penetrate the side of the base film 10 where the coating 20 is not set (i.e., the insulating side), the lithium dendrites will be intercepted by the set coating 20 and will not directly contact the cathode. At the same time, a low-current micro-short circuit is formed by the coating 20, thereby extending the time from the short circuit to the occurrence of a serious accident. Therefore, although it may eventually cause battery failure, it can provide a longer time for the battery management system to provide timely warnings, which is conducive to minimizing the damage and losses caused by serious accidents.
[0057] In some embodiments of the present application, the conductive material includes at least one of carbon nanotubes, graphene, graphene oxide, carbon black, polystyrene sulfonate, polyaniline, nickel, copper, and platinum. The conductive material may be any one of these substances or a combination of any two or more thereof. Selecting at least one of these substances as the conductive material offers the advantage of excellent electrical conductivity, making it easier to control the conductivity of the coating 20 when combined with an insulating material.
[0058] In some embodiments of the present application, the insulating material includes at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate, and magnesium fluoride. The insulating material may be any one of the above substances or a combination of any two or more thereof. Selecting at least one of the above substances as the insulating material is low-cost, readily available, and, when combined with a conductive material, facilitates control of the electrical conductivity of the coating 20.
[0059] In some embodiments of the present application, the conductive material is in a granular form, and the Dv50 of the conductive material is 0.1 to 10 μm. A Dv50 of 0.1 to 10 μm means that 50% of the particle volume distribution corresponds to a particle size of 0.1 to 10 μm. Therefore, selecting a granular conductive material with a Dv50 of 0.1 to 10 μm facilitates controlling the thickness of the coating 20, resulting in a coating 20 with a thickness of 1 to 10 μm, and also helps improve the apparent properties of the coating 20.
[0060] In some embodiments of the present application, the conductive material is in a granular form, and the Dv50 of the conductive material is 0.1 to 10 μm. By selecting a granular conductive material with a Dv50 of 0.1 to 10 μm, the conductive material is more easily dispersed in the slurry used to prepare the coating 20, and the surface of the subsequently prepared coating 20 is smoother and more uniform.
[0061] In some embodiments of the present application, the insulating material is in a granular form, and the Dv50 of the insulating material is 0.1 to 10 μm. Selecting a granular insulating material with a Dv50 of 0.1 to 10 μm facilitates controlling the thickness of the coating 20, resulting in a coating 20 with a thickness of 1 to 10 μm, and also helps improve the surface properties of the coating 20.
[0062] In some embodiments of the present application, the insulating material is in a granular form, and the Dv50 of the insulating material is 0.1 to 10 μm. By selecting a granular insulating material with a Dv50 of 0.1 to 10 μm, the insulating material is more easily dispersed in the slurry used to prepare the coating 20, and the surface of the subsequently prepared coating 20 is smoother and more uniform.
[0063] In some embodiments of the present application, the mass fraction of the conductive material in the coating 20 is 30-90%. By controlling the mass fraction of the conductive material to 30-90%, the conductivity of the coating 20 can be adjusted to match the requirements of batteries of various structures and capacities. At the same time, since the coating 20 is generally obtained by curing a slurry, controlling the mass fraction of the conductive material also helps to control the dispersion performance of the conductive material in the slurry and the coating performance of the slurry.
[0064] In some embodiments of the present application, the mass ratio of the conductive material to the insulating material is 30 to 90:1 to 64. Controlling the amount of insulating material added facilitates regulating the conductivity of the coating 20; similarly, it also helps regulate the dispersion of the conductive material in the slurry and the coating properties of the slurry.
[0065] In some embodiments of the present application, the coating 20 also includes a binder. By adding the binder, the coating 20 is better bonded to the base film 10, thereby improving the structural stability of the battery separator and ensuring the performance of the battery.
[0066] In some specific embodiments of the present application, the binder includes at least one of polyacrylate, acrylic acid, carboxymethyl cellulose, and polyvinylidene fluoride. It can be any one of these substances or a combination of any two or more thereof. Using at least one of these substances as the binder can strengthen the bond between the conductive material, the insulating material, and the base film 10, improve the bonding strength between the coating 20 and the base film 10, and further enhance the structural stability of the battery separator.
[0067] In some embodiments of the present application, the mass ratio of the binder to the conductive material is 5-10:30-90. By controlling the binder addition ratio, a coating 20 having excellent bonding with the base film 10 is obtained, and the conductive material and the insulating material are mixed and dispersed more evenly with the binder, which helps to ensure the conductivity of the coating 20.
[0068] In some embodiments of the present application, the material of the coating 20 further includes a dispersant. By adding the dispersant, the dispersion of the solid matter in the slurry used to prepare the coating 20 can be regulated, thereby helping to reduce the difficulty of slurry processing and improve the coating performance of the slurry. Furthermore, the dispersion of the solid matter in the coating 20 can be adjusted, resulting in a more uniform coating 20 with better apparent quality and more controllable electrical conductivity.
[0069] In some specific embodiments of the present application, the dispersant includes at least one of polyethylene glycol and polyacrylamide, which can be either one of the above substances or a combination of the two substances. Selecting at least one of the above substances as the dispersant has a good dispersion effect on conductive materials, insulating materials, and adhesives.
[0070] In some embodiments of the present application, the mass ratio of the dispersant to the conductive material is 1-5:30-90. By controlling the addition ratio of the dispersant, the dispersibility of the solid material in the slurry used to prepare the coating 20 can be greatly improved, thereby helping to reduce the processing difficulty of the slurry, improve the coating performance of the slurry, and reduce the process difficulty of preparing the coating 20.
[0071] In some embodiments of the present application, the material of the base film 10 includes at least one of polyolefins, polyethers, polyetheretherketones, polyimides, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymers, and copolymers containing C-H bonds. Using at least one of the above-mentioned materials as the material for the base film 10 results in a battery separator having superior overall performance. By using at least one of the above-mentioned materials as the material for the base film 10, the resulting battery separator has superior overall performance and good heat resistance. It should be noted that, the “selection of any one of the above-mentioned substances” mentioned here means selecting polyolefin film, polyether film, polyetheretherketone film, polyimide film, polytetrafluoroethylene film, polyvinyl fluoride film, polyvinylidene fluoride film, polyvinylidene chloride film, polyethylene-propylene copolymer film or copolymer film containing CF bond as the base film 10; the “combination of any two or more of the above-mentioned substances can also be selected” means selecting a film made of a mixture formed by any two or more of the above-mentioned substances, or a composite film synthesized by combining any two or more of the films selected from polyolefin film, polyether film, polyetheretherketone film, polyimide film, polytetrafluoroethylene film, polyvinyl fluoride film, polyvinylidene fluoride film, polyvinylidene chloride film, polyethylene-propylene copolymer film and copolymer film containing CF bond as the base film 10. In the subsequent specific embodiments of the present application, the base film 10 will be described in detail by taking any one of polyolefin film, polyether film, polyetheretherketone film, polyimide film, polytetrafluoroethylene film, polyvinyl fluoride film, polyvinylidene fluoride film, polyvinylidene chloride film, polyethylene-propylene copolymer film, and copolymer film containing CF bonds as an example.
[0072] In a second aspect, the present application provides a method for preparing a battery separator, comprising the following steps:
[0073] Mixing conductive material, insulating material, binder and solvent to prepare coating slurry;
[0074] Applying the coating slurry onto the base film 10;
[0075] The coating slurry is cured on the base film 10 to form a coating 20 to prepare a battery separator;
[0076] The coating slurry includes conductive material and insulating material.
[0077] In the technical solution of the embodiment of the present application, a coating slurry containing a conductive material and an insulating material is coated on one side of the base film 10, and a coating slurry is cured on the base film 10 to form a layer of coating 20. The electrical conductivity of the coating 20 is 10 2 ~10 6S / m, thus, one side of the base film 10 of the battery separator is insulated, while the one side of the coating 20 is conductive, so that the battery separator can be called a "partially conductive separator". When this battery separator is used in a lithium battery, when the lithium dendrites grow to completely penetrate the side of the base film 10 where the coating 20 is not set, the lithium dendrites will be intercepted by the set coating 20 and will not directly contact the cathode. At the same time, a low-current micro-short circuit is formed by the coating 20, thereby extending the time from the short circuit to the occurrence of a serious accident. Therefore, although it may still eventually cause battery failure, it can provide a longer time for the battery management system to provide timely warnings, which is conducive to minimizing the damage and losses caused by serious accidents.
[0078] It is understandable that a dispersant can also be added to the coating slurry to improve the dispersion performance of the solid matter in the slurry and make the slurry coating more uniform. Correspondingly, in the step of preparing the coating slurry, the conductive material, insulating material, binder, dispersant and solvent can be mixed.
[0079] Furthermore, in some specific embodiments of the present application, the steps for preparing the coating slurry may be referred to as follows:
[0080] mixing a binder with an insulating material to obtain a first mixture;
[0081] dispersing the conductive material in a solvent to obtain a second mixed material;
[0082] The first mixed material and the second mixed material are mixed to prepare a coating slurry.
[0083] The conductive material can be dispersed in the solvent by ultrasonic treatment to achieve more uniform and rapid dispersion. Furthermore, the first and second mixed materials can be mixed under heating and stirring conditions to accelerate rapid and uniform dispersion. For example, stirring can be performed at a temperature of 55 to 65° C. for 20 to 30 hours.
[0084] In some embodiments of the present application, the solvent includes at least one of acetone, deionized water, methyl ethyl ketone, and 3-pentanone. Selecting at least one of the above-mentioned substances as the solvent facilitates the full dispersion of the conductive material, insulating material, and binder, thereby obtaining a slurry with suitable viscosity and uniform dispersion of solid materials.
[0085] In some specific embodiments of the present application, the solvent includes acetone. When acetone is selected as the solvent, the solid matter is more fully dispersed, and the coating slurry obtained is more evenly coated on the base film 10, which is conducive to obtaining a more uniform coating 20.
[0086] In some embodiments of the present application, the solid content of the coating slurry is 40-45%. By controlling the solid content of the coating slurry within the range of 40-45%, the coating slurry has an appropriate viscosity, good coating performance, and a fast curing speed, which also helps to reduce the difficulty of preparing the coating slurry.
[0087] In some embodiments of the present application, the step of curing the coating slurry on the base film 10 to form the coating 20 includes:
[0088] The base film 10 coated with the coating slurry is placed at a temperature of 40 to 45° C. and dried for 25 to 30 seconds.
[0089] The coating slurry is cured on the base film 10 to form a coating 20 by drying at 40-45°C for 20-25s. The solvent in the coating slurry is basically completely evaporated, and the formed coating 20 has good surface quality, good bonding with the base film 10, and a fast curing rate.
[0090] In a third aspect, the present application provides a secondary battery, which includes the battery separator in the above embodiment or the battery separator prepared in the above embodiment.
[0091] A secondary battery includes a battery separator as described in the above embodiment, as well as a positive electrode sheet, a negative electrode sheet, and an electrolyte. A secondary battery can be a single battery cell. For example, a lithium-ion battery cell primarily relies on the movement of lithium ions between the positive and negative electrode sheets to function. In cylindrical battery cells, a three-layer thin film structure is wound into a cylindrical electrode assembly, while in rectangular battery cells, the thin film structure is wound or stacked into a roughly rectangular electrode assembly.
[0092] In a typical battery cell structure, the battery cell includes a casing, an electrode assembly, and an electrolyte. The electrode assembly is housed in the battery cell casing and includes a positive electrode sheet, a negative electrode sheet, and a separator. The casing includes an outer shell and end caps. The outer shell includes a housing formed by multiple walls and an opening. The end caps are arranged at the opening to seal the housing. In addition to the electrode assembly, the housing cavity also contains electrolyte. The positive and negative electrode sheets in the electrode assembly include tabs. To ensure that high currents can pass without melting, the positive electrode tabs are multiple and stacked together, and the negative electrode tabs are multiple and stacked together. The tabs are electrically connected to electrode terminals located outside the battery cell via connecting members. The electrode terminals generally include positive and negative electrode terminals. For rectangular battery cells, the electrode terminals are generally located on the end caps. Multiple battery cells are connected in series and / or in parallel via the electrode terminals for various applications.
[0093] A battery composed of cells assembled in a wound manner is called a wound battery. Wound batteries are also called cells, and those in the battery industry call them roll cores. Compared to flat-plate batteries, wound batteries are made by winding plates only about 1mm thick at high pressure. Through special processing methods, the battery has many unique features: super high-rate discharge capability, with a maximum discharge rate of 18C to 30C; excellent high and low temperature performance, capable of operating at -55°C to 150°C; stable high output voltage and higher energy density; sturdy structure with excellent seismic resistance; no free electrolyte (such as colloidal acid), allowing it to be placed in any direction for operation; fast charging, with a charge of over 95% in 40 minutes (1C charging); extremely long life, with a designed float charge life of over 8 years; and extremely high resistance to low-current deep discharge.
[0094] The electrolyte used in the present application may be an electrolyte known in the prior art, including an organic solvent, a lithium salt, and an additive; the isolation membrane used in the present application may be an isolation membrane known in the prior art.
[0095] The secondary battery proposed in this application has all the beneficial effects of the above-mentioned battery separators, which will not be described in detail here.
[0096] Secondary batteries can be formed into battery modules. A battery module is a system that electrically connects a number of secondary batteries and houses them in a frame to protect them from external impact, heat, and vibration. A common battery module typically consists of two end plates, with multiple battery cells (secondary batteries) arranged between them. The end plate with the module's output terminal is called the output terminal plate, while the end plate without the module's output terminal is called the non-output terminal plate.
[0097] Secondary batteries can also be battery packs. In some battery production and processing technologies, multiple battery cells are first integrated into battery modules, and then the battery modules are encapsulated in a battery box to form a battery pack. A battery pack can encapsulate multiple battery modules in one row, or multiple rows of multiple battery modules. The arrangement of multiple rows of multiple battery modules can be double rows and multiple columns, multiple rows and double columns, or multiple rows and multiple columns. Taking a battery pack encapsulating double rows and multiple columns of battery modules as an example, the first end plate of each column is generally the head output extreme plate, the two adjacent end plates between the two rows of battery modules are the middle non-output extreme plates, and the last end plate of each column is the tail non-output extreme plate. The head output extreme plate and one of the middle non-output extreme plates belong to the first row of battery modules, and one of the middle non-output extreme plates and the tail output extreme plate belong to the second row of battery modules.
[0098] In a fourth aspect, the present application provides an electrical device, which includes the secondary battery in the above embodiment.
[0099] The electrical devices proposed in this application include but are not limited to: mobile phones, portable devices, laptops, electric vehicles, electric cars, electric vehicles, ships, spacecraft, electric toys and electric tools, etc. For example, spacecraft include airplanes, rockets, space shuttles and spacecraft, etc. Electric toys include fixed or mobile electric toys, such as game consoles, electric vehicle toys, electric ship toys and electric airplane toys, etc. Electric tools include metal cutting power tools, grinding power tools, assembly power tools and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers.
[0100] The electrical device proposed in this application has all the beneficial effects of the above-mentioned battery separator, which will not be described in detail here.
[0101] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0102] Example 1
[0103] The battery separator includes a polypropylene base film (thickness 4 μm, surface density 3 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 1 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon nanotubes with an average length of 3μm and a conductivity of 207S / m), insulating material particles (silicon dioxide, Dv50 is 5μm) and a binder (polyvinylidene fluoride), and the mass ratio of the conductive material particles, the insulating material particles and the binder is 30:2:3.
[0104] Example 2
[0105] The battery separator includes a polypropylene base film (thickness 6 μm, surface density 4 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 2 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (graphene, Dv50 is 10μm), insulating material particles (aluminum oxide, Dv50 is 0.1μm) and binder (polyacrylate), and the mass ratio of conductive material particles, insulating material particles and binder is 40:1:5.
[0106] Example 3
[0107] The battery separator includes a polypropylene base film (thickness 8 μm, surface density 5 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 4 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (graphene oxide, Dv50 is 8μm), insulating material particles (zinc oxide, Dv50 is 1μm) and binder (acrylic acid), and the mass ratio of conductive material particles, insulating material particles and binder is 50:5:8.
[0108] Example 4
[0109] The battery separator includes a polypropylene base film (thickness 10 μm, surface density 6 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 4 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon nanotubes with an average length of 3μm), insulating material particles (silicon dioxide, Dv50 is 5μm), a binder (polyvinylidene fluoride) and a dispersant (polyethylene glycol), and the mass ratio of the conductive material particles, the insulating material particles, the binder and the dispersant is 30:2:3:2.
[0110] Example 5
[0111] The battery separator includes a polypropylene base film (thickness 12 μm, surface density 7 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 5 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon black, Dv50 is 6μm), insulating material particles (cerium oxide, Dv50 is 3μm), binder (polyacrylate, acrylic acid and carboxymethyl cellulose, mass ratio is 1:1:1) and dispersant (polyethylene glycol), and the mass ratio of conductive material particles, insulating material particles, binder and dispersant is 60:10:8:4.
[0112] Example 6
[0113] The battery separator includes a polypropylene base film (thickness 14 μm, surface density 8 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 6 μm and an electrical conductivity of 10 2 ~10 6S / m, the coating materials include conductive material particles (nickel, Dv50 is 0.1-10μm), insulating material particles (zirconium titanate, Dv50 is 10μm), binder (polyacrylate) and dispersant (polyethylene glycol), and the mass ratio of conductive material particles, insulating material particles, binder and dispersant is 70:30:7:3.
[0114] Example 7
[0115] The battery separator includes a polypropylene base film (thickness 5 μm, surface density 9 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 7 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (copper, Dv50 is 0.1-10μm), insulating material particles (titanium oxide, Dv50 is 6μm), binder (acrylic acid) and dispersant (polyacrylamide), and the mass ratio of conductive material particles, insulating material particles, binder and dispersant is 80:50:9:4.
[0116] Example 8
[0117] The battery separator includes a polypropylene base film (thickness 7 μm, surface density 10 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 8 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon nanotubes with an average length of 1 μm, polystyrene sulfonate with a Dv50 of 3 μm, and a mass ratio of 1:1), insulating material particles (silicon dioxide with a Dv50 of 5 μm, nickel oxide with a Dv50 of 8 μm, and a mass ratio of 1:1), a binder (carboxymethyl cellulose) and a dispersant (polyacrylamide). The mass ratio of the conductive material particles, the insulating material particles, the binder and the dispersant is 90:64:10:5.
[0118] Example 9
[0119] The battery separator includes a polypropylene base film (thickness 9 μm, surface density 5 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 9 μm and an electrical conductivity of 10 2 ~10 6S / m, the coating materials include conductive material particles (polyaniline with a Dv50 of 0.1 to 10 μm, carbon black with a Dv50 of 0.1 to 10 μm, platinum with a Dv50 of 0.1 to 10 μm, and a mass ratio of 10:10:1), insulating material particles (calcium oxide with a Dv50 of 0.1 to 10 μm, zirconium oxide with a Dv50 of 4 μm, barium titanate with a Dv50 of 0.1 to 10 μm, and magnesium fluoride with a Dv50 of 0.1 to 10 μm, and a mass ratio of 1:1:1:1), a binder (carboxymethyl cellulose and polyacrylate, and a mass ratio of 1:1) and a dispersant (polyethylene glycol), and the mass ratio of the conductive material particles, the insulating material particles, the binder and the dispersant is 40:20:5:1.
[0120] Example 10
[0121] The battery separator includes a polypropylene base film (thickness 8 μm, surface density 8 g / m 2 ) and a coating provided on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 10 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon nanotubes with an average length of 3μm), insulating material particles (boehmite with a Dv50 of 0.1 to 10μm, tin dioxide with a Dv50 of 9μm, with a mass ratio of 3:1), a binder (polyvinylidene fluoride and acrylic acid, with a mass ratio of 2:1) and a dispersant (polyethylene glycol and polyacrylamide, with a mass ratio of 1:1). The mass ratio of the conductive material particles, the insulating material particles, the binder and the dispersant is 30:10:10:5.
[0122] Example 11
[0123] The structure and constituent materials of the battery separator are as described in Example 1. The preparation method of the battery separator includes:
[0124] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;
[0125] (2) adding the conductive material particles into acetone and dispersing them under ultrasonic conditions to obtain a second mixture;
[0126] (3) adding the first mixture to the second mixture and stirring at 60° C. for 24 h to prepare a coating slurry;
[0127] (4) The coating slurry was coated on a polypropylene base film, and then dried at 42°C for 26 seconds to prepare a battery separator.
[0128] Example 12
[0129] The structure and constituent materials of the battery separator are as described in Example 1. The preparation method of the battery separator includes:
[0130] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;
[0131] (2) adding the conductive material particles into deionized water and dispersing them under ultrasonic conditions to obtain a second mixture;
[0132] (3) adding the first mixture to the second mixture and stirring at 55° C. for 30 h to prepare a coating slurry;
[0133] (4) The coating slurry was coated on a polypropylene base film, and then dried at 40°C for 30 seconds to prepare a battery separator.
[0134] Example 13
[0135] The structure and constituent materials of the battery separator are as described in Example 1. The preparation method of the battery separator includes:
[0136] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;
[0137] (2) adding the conductive material particles to methyl ethyl ketone and dispersing the mixture under ultrasonic conditions to obtain a second mixture;
[0138] (3) adding the first mixture to the second mixture and stirring at 65° C. for 20 h to prepare a coating slurry;
[0139] (4) The coating slurry was coated on a polypropylene base film, and then dried at 45°C for 25 seconds to prepare a battery separator.
[0140] Example 14
[0141] The structure and constituent materials of the battery separator are as described in Example 1. The preparation method of the battery separator includes:
[0142] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;
[0143] (2) adding the conductive material particles to 3-pentanone and dispersing the mixture under ultrasonic conditions to obtain a second mixture;
[0144] (3) adding the first mixture to the second mixture and stirring at 65° C. for 20 h to prepare a coating slurry;
[0145] (4) The coating slurry was coated on a polypropylene base film, and then dried at 45°C for 25 seconds to prepare a battery separator.
[0146] Example 15
[0147] The structure and constituent materials of the battery separator are as described in Example 3. The preparation method of the battery separator includes:
[0148] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;
[0149] (2) adding the conductive material particles into acetone and dispersing them under ultrasonic conditions to obtain a second mixture;
[0150] (3) adding the first mixture to the second mixture and stirring at 60° C. for 24 h to prepare a coating slurry;
[0151] (4) The coating slurry was coated on a polypropylene base film, and then dried at 42°C for 27 seconds to prepare a battery separator.
[0152] Comparative Example 1
[0153] With a thickness of 4μm and a surface density of 3g / m 2 Polypropylene film is used as battery separator.
[0154] Comparative Example 2
[0155] The battery separator includes a polypropylene base film layer (thickness 4 μm, surface density 3 g / m 2 ), conductive coating (the conductive material in the coating is carbon nanotubes with an average length of 3 μm) and insulating coating (the insulating material in the coating is silicon dioxide with a Dv50 of 5 μm).
[0156] The battery separators prepared in each embodiment and the battery separators provided in the comparative examples were subjected to relevant performance tests. The test methods and results are as follows:
[0157] (1) Production of coin batteries:
[0158] Preparation of NMC(LiNi 0.5 Mn 0.2 Co 0.3 O2): Carbon: PVDF cathode slurry with a ratio of 8:1:1 was coated on aluminum foil. The electrode thickness after drying and cold pressing was 80 μm.
[0159] Assemble coin cells using a 1.0 M LiPF in DMC solution as the electrolyte, lithium metal as the anode, an 18 mm diameter cathode and a 20 mm diameter anode, and the battery separators prepared in the example and the comparative example, respectively;
[0160] (2) Example Battery separator ability test for intercepting lithium dendrites and generating controllable circuits:
[0161] At 1.2C (2mA / cm 2) charge and discharge rate to charge the prepared coin battery, and record the short circuit of the battery. The results are shown in Table 1.
[0162] (3) Short circuit test of lithium dendrites in comparative battery separator:
[0163] At 1.2C (2mA / cm 2 ) charge and discharge rate to charge the prepared coin battery, and record the short circuit of the battery. The results are shown in Table 1.
[0164] Table 1 Short-circuit test results of lithium dendrites on battery separators of Examples and Comparative Examples
[0165] According to the comparative test results in Table 1, the battery separator prepared in the embodiment began to alleviate the short circuit of the battery separator at least around the 60th cycle, which was manifested as an increase in the charging capacity required to reach the cut-off voltage. For example, the battery assembled with the battery separator prepared in Example 1 increased from (148mAh / g) in the 57th cycle to (165mAh / g) in the 60th cycle, and finally to (480mAh / g) in the 76th cycle. The battery separator prepared in the comparative example short-circuited around the 49th cycle, as shown by a rapid drop in voltage, a rapid rise in current, and obvious self-discharge inside the surface battery. It can be seen that compared to the situation in which a battery short circuit occurred after the battery separator was punctured by lithium dendrites in the comparative example, the battery separator provided with a conductive coating prepared in the embodiment of the present application showed a relief of the battery short circuit after the lithium dendrites punctured the battery separator, thereby providing a certain amount of early warning and post-processing time for the operator, reducing the possibility of a major accident.
[0166] The above are only preferred embodiments of the present application and are not intended to limit the scope of the present application. Those skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present application shall be included within the scope of the present application.
Claims
1. A battery separator, characterized in that: The battery separator comprises: basement membrane; and The coating is arranged on the surface of the side of the base film facing the cathode of the battery, and the material of the coating includes a conductive material and an insulating material.
2. The battery separator according to claim 1, characterized in that The conductivity of the coating is 10 2 ~10 6 S / m.
3. The battery separator according to claim 1, characterized in that The conductive material includes at least one of carbon nanotubes, graphene, graphene oxide, carbon black, polystyrene sulfonate, polyaniline, nickel, copper, and platinum.
4. The battery separator according to claim 1, characterized in that The insulating material includes at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate, and magnesium fluoride.
5. The battery separator according to claim 1, characterized in that The conductive material is in granular form, and the Dv50 of the conductive material is 0.1 to 10 μm; and / or, The insulating material is in granular form, and the Dv50 of the insulating material is 0.1-10 μm.
6. The battery separator according to claim 1, characterized in that The conductive material is in granular form, and the Dv50 of the conductive material is 1 to 3 μm; and / or, The insulating material is in a granular form, and the Dv50 of the insulating material is 1 to 3 μm.
7. The battery separator according to claim 1, characterized in that The mass fraction of the conductive material in the coating is 30-90%.
8. The battery separator according to claim 1, characterized in that The mass ratio of the conductive material to the insulating material is 30-90:1-64.
9. The battery separator according to claim 1, characterized in that The material of the coating layer also includes a binder.
10. The battery separator according to claim 9, characterized in that The binder comprises at least one of polyacrylate, acrylic acid, carboxymethyl cellulose and polyvinylidene fluoride; and / or, The mass ratio of the binder to the conductive material is 5-10:30-90.
11. The battery separator according to claim 1, characterized in that The coating material also includes a dispersant.
12. The battery separator according to claim 11, characterized in that The dispersant comprises at least one of polyethylene glycol and polyacrylamide; and / or, The mass ratio of the dispersant to the conductive material is 1-5:30-90.
13. The battery separator according to claim 1, characterized in that The material of the base film includes at least one of polyolefin, polyether, polyetheretherketone, polyimide, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymer, and copolymer containing CF bond.
14. A method for preparing a battery separator according to any one of claims 1 to 13, characterized in that: The following steps are involved: Mixing conductive material, insulating material, binder and solvent to prepare coating slurry; applying the coating slurry onto a base film; The coating slurry is cured on the base film to form a coating to prepare a battery separator.
15. The method for preparing a battery separator according to claim 14, characterized in that: The solvent includes at least one of acetone, deionized water, methyl ethyl ketone, and 3-pentanone.
16. The method for preparing a battery separator according to claim 14, characterized in that: The solvent includes acetone.
17. The method for preparing a battery separator according to claim 14, characterized in that: The solid content of the coating slurry is 40-45%.
18. The method for preparing a battery separator according to claim 14, characterized in that: The step of curing the coating slurry on the base film to form a coating comprises: The base film coated with the coating slurry is placed at a temperature of 40 to 45° C. and dried for 25 to 30 seconds.
19. A secondary battery, characterized in that: The secondary battery comprises the battery separator according to any one of claims 1 to 13 or a battery separator prepared by the method for preparing a battery separator according to any one of claims 14 to 18.
20. An electrical device, characterized in that: The electric device comprises the secondary battery as claimed in claim 19.
Citation Information
Patent Citations
Battery diaphragm and preparation method thereof, secondary battery and electric device
CN119009367A
Separator for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
CN102498590A
Lithium ion battery safe in case of internal micro-short-circuit failure
CN108428924A
Functional diaphragm, preparation method of functional diaphragm and lithium metal battery
CN112436233A
Diaphragm and lithium ion battery
CN212517438U
Cited By
Lithium ion battery and preparation method thereof
CN119764530A