Method for loosening pretreatment of spent wool textiles

WO2024234737A1PCT designated stage expired Publication Date: 2024-11-21GUANGDONG UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/074613
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-01-30
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

During the physical recycling process, the fiber length obtained by mechanical impact of textiles is shorter, and the fiber main body is easily damaged. How to minimize the damage of fibers in mechanical loosening is the most urgent problem that needs to be solved.

Method used

By uniformly spraying oil agent on the surface of waste wool textiles and pretreating them in a sealed environment, the amount of oil agent is 10% to 25% of the textile mass, the temperature is 0℃ to 20℃, and the moisture rebate is 30% to 90%. To reduce the friction between fibers, make the yarn soft, improve the elongation and strength of the yarn, and reduce fiber damage.

Benefits of technology

After pretreatment, mechanical loosening is performed. The obtained wool fiber has higher fiber length, fineness and strength of fracture. The fiber main body is protected, reducing the damage to the fiber during mechanical loosening and improving the durability of the regenerated fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024074613_21112024_PF_FP_ABST
    Figure CN2024074613_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A method for the loosening pretreatment of spent wool textiles. The method comprises the following steps: uniformly spraying an oil agent onto the surface of a spent wool textile, and sealing; the amount of oil agent used being 10%-25% of the mass of the spent wool textile. The method for the loosening pretreatment of spent wool textiles involves spraying a certain amount of oil agent onto a spent wool textile, then combining a specific temperature and moisture regain rate to perform pretreatment and improve the breaking elongation of the yarn, reducing the strength of the yarn; following this pretreatment, performing physical mechanical loosening of the spent wool textile, which compared to direct mechanical loosening results in a wool fiber having higher fiber length, fineness, and breaking strength, thereby protecting the wool fibers, and reducing damage to the fibers during mechanical loosening.
Need to check novelty before this filing date? Find Prior Art

Description

Opening pretreatment method for waste wool textiles

[0001] The present invention claims priority to Chinese patent application No. 2023105437610, filed with the Patent Office of China on May 15, 2023, entitled “Method for Pretreatment of Waste Wool Textiles”, the entire contents of which are incorporated herein by reference. Technical Field

[0002] The present invention belongs to the technical field of wool processing, and more specifically, the present invention relates to a method for pretreating and opening waste wool textiles, and a method for opening waste wool textiles. Background Art

[0003] Wool, a biocompatible natural fiber, has garnered widespread attention in textile technology due to its unique structure, high moisture regain, excellent elasticity, and superior compatibility. Over 2.5 million tons of wool waste is produced annually worldwide, including used wool clothing and low-quality wool from textile processing. Recycling textile waste can promote sustainable development of the textile industry and reduce environmental pollution.

[0004] Physical recycling (also known as mechanical opening and recycling) is a common method for recycling and reusing waste textiles. This involves using mechanical equipment to disassemble and shred waste textiles into fibers, which are then reused in textile weaving processes. The mechanical opening process involves stretching and tearing the textile, essentially breaking it apart, similar to a stretching process.

[0005] In the relevant research on wool fabric opening experiment, Wang Hong et al. compared the performance of wool fibers before and after mechanical opening. The results showed that the length of wool fibers after opening was between 15-20 mm, and the length loss was 75% compared with the original fiber, and the strength loss was between 20%-30%. The fiber scale layer was combed off, and the main body was damaged and cracked (Wang Hong, Ding Xuemei, Wu Xiongying. Damage test analysis of recycled wool fibers [J]. Wool Textile Technology, 2013, 41(03): 1-5.). Ma Jingxuan et al. compared the wool fibers after opening with the original wool fibers. The fiber strength loss was 18% and the length loss was 43%, which increased the fiber short-hair rate. The durability of the spun recycled wool / polyester blended fabric was low (Ma Jingxuan, Wang Xiaoning, Liao Qing. Research on the durability of recycled wool blended fabrics [J]. Journal of Beijing Institute of Fashion Technology (Natural Science Edition), 2019, 39(02): 23-29.).

[0006] Therefore, in the physical recycling process, the fibers obtained after mechanical impact of textiles are short in length and the fiber body is easily damaged. How to minimize the damage to the fibers during mechanical opening is the most urgent problem that needs to be solved in the mechanical opening recycling method.

[0007] Summary of the Invention

[0008] Based on this, the object of the present invention is to provide a loosening pretreatment method and an opening method for waste wool textiles.

[0009] The first aspect of the present invention provides a method for pre-treating loosening of waste wool textiles, comprising the following steps: evenly spraying an oil agent on the surface of the waste wool textiles and then sealing; the amount of the oil agent used is 10% to 25% of the mass of the waste wool textiles.

[0010] The second aspect of the present invention provides a method for loosening waste wool textiles, comprising the following steps: S.1 pretreatment: after evenly spraying an oil agent on the surface of the waste wool textile, sealing it for 20 to 30 hours; the amount of the oil agent used is 10% to 25% of the mass of the waste wool textile, the sealing temperature is 0°C to 20°C, and the moisture regain in the sealed environment is 30% to 90%.

[0011] S2. Opening.

[0012] In the opening pretreatment method for waste wool textiles of the present invention, a certain amount of oil is sprayed on the waste wool textiles, and then pretreated in combination with a specific temperature and regain, the breaking elongation of the yarn is improved and the yarn strength is reduced. After this pretreatment, the waste wool textiles are physically and mechanically opened. Compared with direct mechanical opening, the obtained wool fibers have higher fiber length, fineness and breaking strength, the wool fiber body is protected, and the damage to the fibers during mechanical opening is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] FIG1 shows the tensile properties of wool yarn at different oil ratios in Test Example 1 of the present invention.

[0014] FIG2 shows the tensile properties of wool yarn under different temperatures in Test Example 3 of the present invention.

[0015] FIG3 shows the tensile properties of wool yarn at different moisture regains in Test Example 4 of the present invention.

[0016] FIG4 is an electron microscope image of the fiber sample No. 0 in Test Example 6 of the present invention at a magnification of 1000 times.

[0017] FIG5 is an electron microscope image of fiber sample No. 1 in Test Example 6 of the present invention at 1000 times magnification.

[0018] FIG6 is an electron microscope image of fiber sample No. 2 in Test Example 6 of the present invention at a magnification of 1000 times. DETAILED DESCRIPTION

[0019] To facilitate understanding of the present invention, the present invention will be described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the present disclosure more thorough and comprehensive.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art to which this invention pertains. The terms used in this specification are for the purpose of describing specific embodiments only and are not intended to limit the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0021] In some embodiments of the present invention, a method for loosening and pretreating waste wool textiles is disclosed, comprising the following steps: evenly spraying an oil agent on the surface of the waste wool textile and then placing the textile in a sealed environment; the amount of the oil agent used is 10% to 25% of the mass of the waste wool textile.

[0022] The inventors of the present invention have discovered that pre-treating waste wool textiles with a certain amount of oil effectively reduces interfiber friction, softens the yarn, increases its elongation at break, and reduces yarn strength. This pre-treatment, followed by mechanical opening of the waste wool textile, reduces fiber damage during the opening process. Specifically, the wool fibers obtained from mechanical opening after pre-treatment have a significantly lower short-hair ratio, higher fiber length, fineness, and breaking strength than those obtained from direct mechanical opening. The main body of the wool fibers is protected, reducing fiber damage during mechanical opening. The amount of oil used must be within an appropriate range. Excessive oil application can lead to accumulation on the fiber surface, forming a rough, uneven film. This increases the interfiber friction coefficient and can easily cause sticking between the oil and metal impurities on the fiber surface, hindering mechanical opening of the textile. Therefore, the amount of oil used is 10% to 25% of the mass of the waste wool textile.

[0023] In some embodiments, the amount of the oil agent used is 15% to 25% of the mass of the waste wool textiles.

[0024] In some embodiments, the amount of the oil agent used is 19% to 21% of the mass of the waste wool textiles.

[0025] In some embodiments, the sealing conditions include: temperature 0°C to 20°C, and moisture regain 30% to 90%.

[0026] The ambient temperature and moisture regain during pretreatment also have a significant impact on the quality of subsequent mechanical opening of wool. When the pretreatment temperature is between 0°C and 20°C, the moisture and oil in the yarn can fully react, making the wool yarn relatively soft and having a higher elongation at break. After being treated at 40°C for about 24 hours, the moisture in the wool yarn evaporates, causing the oil to accumulate on the fiber surface into an uneven film layer, resulting in severe cracking, and the fiber surface becomes rough. The friction between fibers increases, reducing the strength and elongation of the yarn. At high temperatures of 50°C to 60°C, the moisture in the yarn decreases, the chain segment movement of the wool keratin macromolecules is strengthened, the intermolecular interaction is weakened, the intermolecular crosslinking disintegrates, the fiber has a higher flexibility, and is prone to yarn deformation. Therefore, the preferred pretreatment temperature is 0°C to 20°C, the optimal pretreatment temperature is 0-10°C, and the treatment time is 20-30 hours. When the moisture regain in the yarn is low (less than 30%), the lubricating effect of water between the fibers in the yarn is reduced, which is the main reason for the low elongation at break of the yarn. The elongation at break of the yarn will gradually increase with the increase of the moisture regain. This is because the water has a plasticizing effect in the yarn, which improves the mechanical properties of the yarn and makes the wool yarn softer and more elastic. When the moisture regain reaches 90%, the yarn reaches the highest elongation at break of 35.2%. The breaking strength first decreases with the increase of the moisture regain, reaching the lowest at a moisture regain of 30%. After that, the breaking strength remains basically unchanged as the moisture regain increases. In summary, when pre-treating wool fabrics before opening, the moisture regain can be 30% to 90%.

[0027] In some embodiments, the temperature is 0°C to 10°C.

[0028] In some embodiments, the moisture regain is 80% to 90%.

[0029] In some embodiments, the sealing treatment time is 20 hours to 30 hours, and in some more preferred embodiments, the sealing treatment time is 22 hours to 26 hours.

[0030] In some embodiments, the oil agent is deionized water, a hair oil agent, and an antistatic agent in a mass ratio of 11-13:0.8-1.2:0.2-0.4.

[0031] In some embodiments, the mass ratio of the deionized water, the hair oil agent and the antistatic agent is 12:1:0.3.

[0032] In other embodiments of the present invention, a method for opening waste wool textiles is also disclosed, which includes the following steps: before opening, the waste wool textiles are first subjected to the above-mentioned pretreatment.

[0033] The opening may be mechanical opening, for example, opening by an opening machine.

[0034] The waste wool textiles described in the present invention can be wool textiles with a mass content of wool raw materials greater than 10%, greater than 20%, greater than 30%, greater than 40%, greater than 50%, greater than 60%, greater than 70%, greater than 80%, greater than 90%, or even 100%. Wool textiles are finished products prepared from fabrics (wool fabrics) woven mainly with wool as raw material. The wool fabrics can be woven fabrics or knitted fabrics. Wool textiles can be tops, trousers, jackets, overcoats, and can also be various products with wool as the main raw material, such as woolen cloth, wool yarn, blankets, and felt.

[0035] In the following examples, waste wool textile yarn and fabric were provided by Shenzhen Jinrongda Knitting Garment Co., Ltd. The wool yarn used in the tensile test was 21 tex, 100% pure wool yarn, with a wool fiber length of 58 mm and a fineness of 19.5 microns. The additives used were FX-K902N wool oil and FX-AS30N antistatic agent, provided by Beijing Fangxing Auxiliary Agent Co., Ltd. The specifications of the waste wool textile fabric are as follows:

[0036] Organization structure: plain weft; yarn linear density (tex): 21; fabric transverse density (turns / 5cm): 55; fabric longitudinal density (turns / 5cm): 44; fabric thickness (mm): 0.48; square meter weight (g / m2): 182.

[0037] In the following examples, the tensile properties of wool yarns were tested with reference to the standard GB / T 3916-2013 "Test method for breaking strength and elongation of single yarn". The tensile test was carried out using a universal tensile testing machine, with the clamping distance set to 250 mm and the tensile speed set to 500 mm / min. The tensile test can obtain a graph showing the relationship between the breaking strength and elongation of wool yarns under different pretreatment conditions. The tensile properties of wool fibers after opening were tested using the standard GB / T 4711-1984 "Test method for breaking strength and elongation of single wool fibers", with a clamping distance of 20 mm, a tensile speed of 20 mm / min, and a pre-tension of 9 millinewtons / tex. The fiber fineness test after mechanical opening was carried out using the standard GB / T 10685-2007 "Test method for diameter of wool fibers, projection microscope method", with a magnification of 500 times. The indicators that can be obtained include the average fiber fineness and the coefficient of variation. The fiber length test of mechanically loosened wool uses the GB / T 19722-2005 "Scoured Sheep Wool" standard and the plot method. The available indicators include average fiber length, coefficient of variation, fiber short hair rate, and fiber length loss rate. The fiber length loss rate is calculated as follows:

[0038] Where: S is the fiber length loss rate, %; A is the fiber length before opening, mm; B is the fiber length after opening, mm.

[0039] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0040] Example 1 Opening pretreatment method for waste wool textiles

[0041] The method for pretreating the loosening of waste wool textiles of this embodiment comprises the following steps:

[0042] (1) Prepare the oil in a laboratory at room temperature of 20°C and relative humidity of 65%. Take 36g of room temperature (20°C) deionized water, 3g of crude oil, and 0.9g of antistatic agent (deionized water: crude oil: antistatic agent = 12:1:0.3) and put them into a 100ml conical flask. Use a magnetic stirrer (RCT basic model) to stir at 20°C for 20 to 30 minutes until the aqueous solution becomes clear and transparent. The prepared oil should be used on the same day.

[0043] (2) After evenly spraying 20% ​​of the mass of the waste wool textiles on the surface of the waste wool textiles, seal them at 0°C and 90% moisture regain for 24 hours.

[0044] Example 2 Opening pretreatment method for waste wool textiles

[0045] The method for pretreating the loosening of waste wool textiles of this embodiment comprises the following steps:

[0046] (1) The preparation method of the oil is the same as that of Example 1;

[0047] (2) After evenly spraying 15% of the mass of the waste wool textiles on the surface of the waste wool textiles, seal them at 10°C and 80% moisture regain for 24 hours.

[0048] Example 3: Opening pretreatment method for waste wool textiles

[0049] The method for pretreating the loosening of waste wool textiles of this embodiment comprises the following steps:

[0050] (1) The preparation method of the oil is the same as that of Example 1;

[0051] (2) After evenly spraying 25% of the mass of the waste wool textiles on the surface of the waste wool textiles, seal them at 20°C and 60% moisture regain for 24 hours.

[0052] Experimental Example 1 Effects of different oil ratios on the tensile properties of waste wool yarn

[0053] The prepared oil agent (same as in Example 1) was evenly sprayed on the surface of the waste wool yarn at a mass ratio of 0%, 5%, 10%, 15%, 20% and 25% of the waste wool yarn, and then placed in a constant temperature and humidity chamber (20°C, RH65%) and sealed for 24 hours, and then the tensile properties were tested in the laboratory.

[0054] The results, shown in Figure 1, show that, with constant temperature and humidity, the elongation at break of wool yarn increases with increasing oil content from 0% to 20%, with a more pronounced increase from 5% to 20%. However, as the oil content increases from 20% to 25%, the elongation at break decreases. The breaking strength of wool yarn decreases below 15% and remains unchanged above 15%.

[0055] The results of this test show that applying a certain amount of oil to waste wool yarn can effectively reduce interfiber friction, soften the yarn, significantly improve its elongation at break, and reduce the loss of yarn breaking strength to a certain extent. However, when the amount of oil is too high, it tends to accumulate on the fiber surface, forming a rough, uneven film on the fiber surface, which increases the interfiber friction coefficient. Furthermore, excessive oil application in waste textiles can easily lead to sticky interactions between the oil and metal impurities on the fiber surface, hindering the mechanical opening of the textile.

[0056] After tensile test experimental analysis, when the oil agent accounts for 10% to 25%, the yarn has higher breaking elongation and strength, which will help reduce fiber damage during the opening process. When the oil agent accounts for 20%, the yarn breaking elongation reaches the maximum.

[0057] Experimental Example 2 Effects of different oils on the tensile properties of waste wool yarn

[0058] The oils prepared in Table 1 were evenly sprayed on the surface of the waste wool yarn at a mass ratio of 20% of the waste wool yarn, and then sealed and stored in a constant temperature and humidity chamber (0°C, RH 90%) for 24 hours before tensile performance testing was performed in the laboratory.

[0059] Table 1

[0060] The results are shown in Table 1. As can be seen from Table 1, the yarn breaking strength, yarn breaking elongation, and average length of the regenerated fiber obtained after opening of the 0# sample pretreated with the oil of the present invention (i.e., ionized water: and wool oil: antistatic agent = 12:1:0.3) are significantly better than those of the 1# sample pretreated with a different oil ratio (ionized water: and wool oil: antistatic agent = 14:0.3:0.1) and the 2# sample pretreated with atomized silicone oil (Zhangjiagang Saier Fine Chemical Co., Ltd.). Among them, the 2# sample pretreated with atomized silicone oil had a reduced yarn breaking elongation and still had large static electricity during the opening and combing process, resulting in severe fiber entanglement with the roller and being unable to be processed, resulting in the inability to produce recycled fiber for the regenerated fiber average length test.

[0061] Experimental Example 3 Effect of different temperatures on the tensile properties of waste wool yarn

[0062] Long-term high-temperature treatment of wool yarn will reduce the toughness of the yarn and easily cause the yarn to break. Therefore, the pretreatment temperature of the yarn should not be too high. The waste wool yarn after applying 20% ​​oil agent is placed in a constant temperature and humidity box with a humidity of 90% and different temperatures (0℃, 20℃, 30℃, 40℃, 50℃ and 60℃) for 24 hours, and then the tensile properties of the yarn are tested.

[0063] The results are shown in Figure 2. As can be seen from Figure 2, the elongation at break shows an overall downward trend from 0°C to 60°C, with a particularly significant decrease from 20°C to 40°C and a more gradual decline from 40°C to 60°C. The breaking strength of the yarn also shows an overall downward trend. Both the elongation and breaking strength of the yarn decrease significantly from 20°C to 40°C. This is likely due to the fact that at 20°C, the moisture and oil in the yarn fully react, making the wool yarn softer and exhibiting a higher elongation at break. However, after treatment at 40°C for 24 hours, the moisture in the yarn evaporates, causing the oil to accumulate on the fiber surface, forming an uneven film. This leads to severe cracking, roughening the fiber surface, and increasing interfiber friction, resulting in reduced yarn strength and elongation. At elevated temperatures of 50°C to 60°C, the moisture content in the yarn decreases, enhancing the segmental motion of the wool keratin macromolecules and weakening the intermolecular interactions, leading to the disintegration of intermolecular crosslinks. This results in increased fiber flexibility and facilitates yarn deformation.

[0064] The breaking elongation and breaking strength of yarn decrease with increasing temperature. Therefore, when pretreating waste wool fabrics before opening, the pretreatment temperature is 0℃~20℃, and the optimal pretreatment temperature is 0~10℃.

[0065] Experimental Example 4 Effects of different moisture regains on the tensile properties of waste wool yarn

[0066] The moisture regain test refers to the standard GB / T 6500-2008 "Plush fiber moisture regain test method oven method", and the oven used is the DHG-9145A electric blast drying oven. The moisture regain of the waste wool yarn after applying the oil is regulated. The moisture regain can be controlled by changing the relative humidity of the constant temperature and humidity chamber and spraying water. Two samples are prepared for each experiment, one for the determination of the moisture regain and the other for the yarn tensile test. The moisture regain setting is controlled at eight points of 0%, 15%, 30%, 45%, 60%, 70%, 80%, and 90% for the tensile test (20% oil, temperature 0°C).

[0067] The results are shown in Figure 3. The yarn's elongation at break shows a significant upward trend from 0% to 30% moisture regain, remains essentially unchanged from 30% to 45%, and then shows a significant upward trend above 45%. The yarn's breaking tenacity shows a significant downward trend from 0% to 30%, then increases slightly from 30% to 65%, and remains virtually unchanged above 65%.

[0068] When the moisture regain in the yarn is low, the lubricating effect of water between the fibers in the yarn is reduced, which is the main reason for the low elongation at break of the yarn. The elongation at break of the yarn will gradually increase with the increase of moisture regain. This is because the water in the yarn has a plasticizing effect, which improves the mechanical properties of the yarn and makes the wool yarn softer and more elastic. When the moisture regain reaches 90%, the yarn elongation reaches the highest yarn elongation of 35.2%. The breaking strength first decreases with the increase of moisture regain, reaching the lowest at 30%. After that, the breaking strength remains basically unchanged as the moisture regain increases. In summary, when pre-treating waste wool fabrics before opening, the moisture regain can be 30% to 90%.

[0069] Based on the results of Experiments 1 to 3, the optimal pretreatment conditions for waste wool yarn before mechanical opening are: an oil content of 15% to 25%, an ambient temperature of 0°C to 10°C, and a moisture regain of 80% to 90% for 24 hours. Under this pretreatment, the wool yarn exhibits higher elongation and breaking strength.

[0070] Experimental Example 5 Effect of pretreatment on the mechanical properties of wool fibers after opening

[0071] After pretreatment of the waste wool fabric using the method described in Example 1 (oiling agent 20%, temperature 0°C, moisture regain 90%, and storage for 24 hours), the wool fiber obtained by mechanical opening was designated as Sample 1. The wool fiber obtained by mechanical opening of the wool fabric without pretreatment was designated as Sample 2. A certain amount of wool fiber was extracted from the fabric as raw wool fiber, designated as Sample 0, with care taken to avoid damaging the fibers during the removal process. The fiber length, fineness, and tensile properties of the three samples were tested respectively. The test results of the three wool fiber sample parameters are shown in Table 2.

[0072] Table 2

[0073] Note: Sample No. 0 is raw wool fiber; Sample No. 1 is wool fiber obtained by pretreatment and opening according to the present invention; Sample No. 2 is wool fiber obtained without pretreatment and opening.

[0074] From the results in Table 2, it can be seen that the fiber fineness, breaking strength and elongation of sample No. 2 are all higher than those of sample No. 0, which may be caused by mechanical impact during the opening process. The breaking strength and elongation of sample No. 1 are higher than those of sample No. 2, which may be related to the residual oil on the fiber surface. The fiber fineness of sample No. 1 is lower than that of sample No. 2. This is because the mechanical impact makes the fiber flat, and the effect of the oil reduces the damage to the fiber during the opening. The wool fiber obtained by opening without pretreatment has a fiber length of 25.4mm, while the wool fiber obtained by opening after pretreatment has a length of 28.3mm, and the average length of the regenerated fiber has increased by about 3mm. The fiber length loss rate is the main factor reflecting the fiber damage before and after fiber opening. The fiber length loss rate of sample No. 1 is 51.2%, and the fiber length loss rate of sample No. 2 is 56.2%. The length loss rate of the regenerated fiber obtained by opening the fabric pretreated by the present invention is reduced by 5.0%, which proves that pretreatment before mechanical opening can effectively protect the waste wool fabric from fiber length damage during opening.

[0075] Compared with sample No. 2, the fiber length loss rate of sample No. 1 was reduced by 5.0%, the short hair rate of the fiber was reduced by 15.6%, the breaking strength was increased by 3%, and the breaking elongation was increased by 10%. It can be seen that the overall performance of the wool fiber obtained by pretreatment is higher than that of the wool fiber obtained by direct opening.

[0076] In summary, the results of this test example show that mechanically opening the wool fabric pretreated by the pretreatment method of the present invention can obtain wool fibers with higher fiber length, fineness and breaking strength than wool fibers obtained by direct opening, and can effectively reduce the short-hair rate of the wool fibers.

[0077] Experimental Example 6 Effect of pretreatment on the surface structure of wool fibers after opening

[0078] In order to explore the effect of pretreatment conditions on fiber damage during mechanical opening of waste wool, an EVO18 large-cavity scanning electron microscope was used to conduct electron microscopy experiments on the three fiber samples No. 0, No. 1, and No. 2 in Experimental Example 5. The electron micrographs of different fiber samples are shown in Figure 4.

[0079] Figures 4, 5, and 6 are electron microscope images of fiber samples No. 0, 1, and 2 at 1000 times magnification, respectively. As can be seen from Figure 4, the wool fiber obtained after direct opening (Figure 6) is severely damaged, with obvious scratches on the surface, the fiber becomes flat, and the scale structure is also damaged. The wool fiber obtained after pretreatment opening (Figure 5) has a protected scale structure and no scratches on the surface, which proves that the pretreatment effectively reduces the damage to the fiber during the opening process. Compared with fiber sample No. 0 (Figure 4), there are flaky or granular substances on the surface of fiber No. 1 (Figure 5), which may be part of the oil remaining on the fiber surface after the water evaporates.

[0080] The results of this test example show that the pretreatment method of the present invention is performed on waste wool before opening, so that the main body of the wool fiber is protected after mechanical opening, and the damage to the fiber during mechanical opening is reduced.

[0081] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0082] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.

Claims

1. A method for pretreating waste wool textiles, characterized in that: The following steps are involved: After spraying oil evenly on the surface of waste wool textiles, the product is sealed; the amount of the oil is 10% to 25% of the mass of the waste wool textiles, the sealing temperature is 0°C to 20°C, the regain is 30% to 90%, and the sealing time is 20 hours to 30 hours.

2. The method for pre-treating the waste wool textiles according to claim 1, characterized in that: The usage of the oil agent is 15% to 25% of the mass of the waste wool textiles.

3. The method for pretreating the loosening of waste wool textiles according to claim 2, characterized in that: The usage of the oil agent is 19% to 21% of the mass of the waste wool textiles.

4. The method for pretreating the loosening of waste wool textiles according to claim 1, characterized in that: The temperature is 0°C to 10°C.

5. The method for pre-treating the loosening of waste wool textiles according to claim 1, characterized in that: The moisture regain is 80% to 90%.

6. The method for pre-treating the waste wool textiles according to any one of claims 1 to 5, characterized in that: The oil agent is deionized water, a hair oil agent and an antistatic agent in a mass ratio of 11-13:0.8-1.2:0.2-0.

4.

7. The method for pre-treating the loosening of waste wool textiles according to claim 6, characterized in that: The mass ratio of the deionized water, the hair oil agent and the antistatic agent is 12:1:0.

3.

8. The method for pre-treating the waste wool textiles according to any one of claims 1 to 5, characterized in that: The sealing time is 22 hours to 26 hours.

9. A method for opening waste wool textiles, characterized in that: The following steps are involved: S.1 Pretreatment: comprising the following steps: after uniformly spraying the oil agent on the surface of the waste wool textile, sealing for 20 to 30 hours; the amount of the oil agent is 10% to 25% of the mass of the waste wool textile, the sealing temperature is 0°C to 20°C, and the moisture regain is 30% to 90%; S2. Loosen.

Citation Information

Patent Citations

  • Textile made of high count and high alpine animal fiber blended yarns

    CN102704105A

  • Pure wool open-end spinning process

    CN103320924A

  • Textile pretreatment method for reducing yarn extraction force in waste fabrics

    CN104294609A

  • Oiling agent for producing regenerated fibers from waste textiles

    CN113802375A

  • Opening pretreatment method of waste wool textile

    CN116556042A