Mos2-pd hydrogen-sensitive material and preparation method therefor
By electrochemically depositing Pd nanoparticles on MoS2 films, the problem of easy shedding of palladium film hydrogen-sensitive materials during hydrogen absorption and release is solved, the stability and sensitivity of the hydrogen sensor are improved, and efficient hydrogen monitoring is achieved.
Patent Information
- Application Number
- PCT/CN2024/080705
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-03-08
- Publication Date
- 2024-11-21
AI Technical Summary
The existing palladium membrane hydrogen-sensitive materials are prone to cracking and falling off after hydrogen absorption and release cycles, resulting in a degradation in the performance of hydrogen sensors and a short service life, making it difficult to work stably in a flammable and explosive environment.
The MoS2 film was grown by chemical vapor deposition method, and Pd nanoparticles were deposited on its surface by electrochemical deposition method to enhance the force between Pd and MoS2 films, and overcome the problem of easy shedding of Pd nanoparticles during hydrogen absorption and hydrogen release. .
It improves the structural stability and sensitivity of the fiber grating hydrogen sensor, extends the life of the sensor, achieves fast and continuous hydrogen monitoring, and has environmentally friendly and low cost.
Smart Images

Figure CN2024080705_21112024_PF_FP_ABST
Abstract
Description
A MoS2-Pd hydrogen-sensitive material and preparation method thereof
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310542209X filed in China on May 15, 2023, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present disclosure belongs to the technical field of hydrogen sensors, and particularly relates to a MoS2-Pd hydrogen-sensitive material and a preparation method thereof. Background Art
[0004] In recent years, fossil fuels have been depleted, and their combustion has led to serious environmental pollution. Hydrogen, with its widespread distribution, clean and renewable nature, high energy density, and wide application, is considered an ideal alternative to fossil fuels. However, hydrogen is a colorless, odorless, flammable gas with a low ignition energy. It is highly explosive when exposed to open flames or electrical currents. Furthermore, hydrogen is prone to leakage during production, storage, and transportation, posing a serious safety hazard. Therefore, timely, accurate, and sensitive detection of hydrogen is of paramount importance.
[0005] Fiber Bragg grating (FBG) hydrogen sensors offer advantages such as small size, long life, intrinsic safety, resistance to electromagnetic interference, and high sensitivity. They are suitable for use in flammable and explosive environments and have become a research hotspot for hydrogen detection technology. The precious metal palladium (Pd) exhibits specific selectivity and reversible adsorption for hydrogen, making it a widely used hydrogen-sensitive material in fiber Bragg grating (FBG) hydrogen sensors. However, after hydrogen absorption, Pd forms Pd hydrides in both α and β phases. These α and β phases exhibit significant differences in lattice expansion coefficients, leading to cracking and shedding of the Pd film hydrogen-sensitive material commonly used in fiber Bragg grating (FBG) sensors after repeated cycles of hydrogen absorption and release, reducing sensor performance and service life. Therefore, the development of new hydrogen-sensitive materials is needed to overcome the hydrogen embrittlement and shedding problem of Pd films and improve the performance of hydrogen sensors.
[0006] Summary of the Invention
[0007] The present disclosure aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the present disclosure provides a MoS2-Pd hydrogen-sensitive material and a preparation method thereof.
[0008] The present disclosure provides a method for preparing a MoS2-Pd hydrogen-sensitive material, comprising the following steps:
[0009] S1, growing a MoS2 thin film on a substrate by chemical vapor deposition to obtain a substrate loaded with the MoS2 thin film;
[0010] S2, preparing a conductive substrate;
[0011] S3, transferring the MoS2 thin film on the substrate to the conductive substrate to obtain a conductive substrate loaded with the MoS2 thin film;
[0012] S4, preparing a palladium chloride hydrochloric acid solution as an electroplating solution;
[0013] S5, immersing the conductive substrate loaded with the MoS2 thin film in the electroplating solution, performing electrochemical deposition under constant potential, and then immersing in deionized water to remove residual electroplating solution, thereby preparing the MoS2-Pd hydrogen-sensitive material;
[0014] Wherein, in the step S2, the method for preparing the conductive substrate is: evaporating a metal film on the surface of a SiO2 / Si substrate to obtain the conductive substrate; the evaporation area of the metal film accounts for 30% to 50% of the surface area of the SiO2 / Si substrate; the metal film is a Cr / Au metal film or a Ti / Au metal film; in the Cr / Au metal film, the thickness ratio of the Cr metal film to the Au metal film is 1:10; and the thickness of the Cr metal film is 6 to 10 nm; the thickness of the Au metal film is 60 to 100 nm; in the Ti / Au metal film, the thickness ratio of the Ti metal film to the Au metal film is 1:10; and the thickness of the Ti metal film is 6 to 10 nm; the thickness of the Au metal film is 60 to 100 nm;
[0015] In step S5, the constant potential is -0.20 V vs SCE, and the electrochemical deposition time is 5 to 30 seconds.
[0016] In the embodiment of the present disclosure, Pd nanoparticles are deposited on the MoS2 film by electrochemical deposition. Since the MoS2 film has a large specific surface area and various types of defects on the surface, including point defects (vacancies and substitutions), dislocations and grain boundaries, Pd nanoparticles can be used as the catalyst. 2+ The deposition active sites make the Pd in the plating solution 2+ They can be firmly deposited on the active sites of the MoS2 surface and reduced to Pd nanoparticles under constant potential. The strong interaction between the Pd nanoparticles and the MoS2 film overcomes the problem of Pd nanoparticles easily falling off during hydrogen absorption and release. Furthermore, electrochemical deposition of Pd nanoparticles is simpler, and the entire preparation process is green, pollution-free, non-destructive, and low-cost.
[0017] In some embodiments of the present disclosure, in step S1, the method for growing a MoS2 thin film on a substrate is: using MoO3 and sulfur powder as reaction raw materials, growing the MoS2 thin film on the substrate by chemical vapor deposition to obtain the substrate loaded with the MoS2 thin film; the molar ratio of the MoO3 to the sulfur powder is 1:2.5 to 1:3; the temperature of the chemical vapor deposition is 820 to 850°C, and the time is 10 to 15 minutes; the substrate is any one of mica, silicon wafer or sapphire.
[0018] In some embodiments of the present disclosure, in step S3, the method of transferring the MoS2 thin film is: using PMMA as a medium to transfer the MoS2 thin film on the substrate to the conductive substrate by wet etching.
[0019] In some embodiments of the present disclosure, in step S4, the method for preparing the palladium chloride hydrochloric acid solution is: dissolving palladium chloride and concentrated hydrochloric acid in deionized water, and mixing them evenly to obtain the palladium chloride hydrochloric acid solution; the molar concentration ratio of the palladium chloride to the concentrated hydrochloric acid is 0.03:1 to 0.04:1.
[0020] On the other hand, the embodiments of the present disclosure further provide a MoS2-Pd hydrogen-sensitive material, which is prepared by the preparation method described in any embodiment of the first aspect of the present disclosure.
[0021] The characteristics and advantages described above for the preparation method of MoS2-Pd hydrogen-sensitive material are also applicable to MoS2-Pd hydrogen-sensitive material and will not be repeated here.
[0022] On the other hand, the embodiments of the present disclosure further propose the application of the above-mentioned MoS2-Pd hydrogen-sensitive material in a fiber Bragg grating hydrogen sensor. The MoS2-Pd hydrogen-sensitive material is used as a hydrogen-sensitive material in a fiber Bragg grating hydrogen sensor and exhibits good sensitivity and stability.
[0023] The present disclosure also provides a method for preparing the above-mentioned fiber Bragg grating hydrogen sensor, comprising the following steps:
[0024] 1) etching the optical fiber cladding on the surface of the fiber Bragg grating using 40 wt % hydrofluoric acid to obtain a pretreated optical fiber;
[0025] 2) spin-coating a drop of PMMA on the surface of the MoS2-Pd hydrogen-sensitive material and heating the PMMA to solidify it to form a PMMA film; then immersing the material in a 5wt% NaOH solution, and using the etching effect of NaOH on the SiO2 / Si substrate to separate the PMMA film with the MoS2-Pd hydrogen-sensitive material adhered to it from the SiO2 / Si substrate, thereby obtaining a PMMA film loaded with the MoS2-Pd hydrogen-sensitive material, wherein the MoS2-Pd hydrogen-sensitive material is prepared by the preparation method described in any embodiment of the first aspect of the present disclosure;
[0026] 3) The PMMA film loaded with the MoS2-Pd hydrogen-sensitive material is attached to the pretreated optical fiber, and after natural drying, the film is processed and packaged to obtain the fiber Bragg grating hydrogen sensor.
[0027] In the preparation method of the fiber Bragg grating hydrogen sensor of the embodiment of the present disclosure, MoS2-Pd is used as the hydrogen-sensitive material, and is transferred to the processed optical fiber by wet etching using PMMA as a medium. The entire process causes almost no damage to the optical fiber, thereby ensuring that the prepared fiber Bragg grating hydrogen sensor has a long life and good stability.
[0028] In some embodiments of the present disclosure, in step 2), the spin coating speed is 2000-3000 rpm, and the spin coating time is 45-60 s; the etching temperature is 50-70° C., and the etching time is 15-20 min.
[0029] The present disclosure has the following advantages and beneficial effects:
[0030] (1) In the embodiment of the present disclosure, metal Pd nanoparticles are deposited on the MoS2 film. Since the interaction between the Pd nanoparticles and the MoS2 film is strong, the problem of Pd easily falling off during the hydrogen absorption and release process can be overcome. In addition, the MoS2 film has a strong bonding force with the fiber Bragg grating, which can improve the structural stability of the fiber Bragg grating hydrogen sensor.
[0031] (2) In the embodiments of the present disclosure, an electrochemical deposition method is used to firmly deposit Pd nanoparticles on the surface of the MoS2 film. Compared with the metal evaporation method and chemical reduction method commonly used in the existing technology, the electrochemical deposition operation is simpler, non-destructive and low-cost.
[0032] (3) In the embodiments of the present disclosure, the size of the Pd nanoparticles in the MoS2-Pd hydrogen-sensitive material can be controlled by regulating the time of electrochemical deposition, so as to meet the actual needs of the fiber Bragg grating hydrogen sensor under different working conditions.
[0033] (4) The fiber Bragg grating hydrogen sensor in the embodiment of the present disclosure has a long life and good stability, and can monitor hydrogen quickly and continuously, showing good sensitivity and responsiveness. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] FIG1 is a schematic diagram of a device for preparing MoS2-Pd hydrogen-sensitive material by electrochemical deposition according to an embodiment of the present disclosure;
[0035] Among them, 1-conductive substrate loaded with MoS2 thin film, 2-working electrode, 3-saturated calomel electrode, 4-platinum counter electrode, 5-palladium chloride hydrochloric acid electroplating solution.
[0036] FIG2 is a cyclic voltammetry curve of a conductive substrate loaded with MoS2 thin film to be deposited in a palladium chloride hydrochloric acid electroplating solution.
[0037] FIG3 is a structural diagram of the MoS2-Pd hydrogen-sensitive material in an embodiment of the present disclosure;
[0038] Among them, 6-MoS2 thin film, 7-Pd nanoparticles, 8-PMMA film, 9-Au metal film, 10-Cr metal film, 11-SiO2, 12-Si.
[0039] FIG4 is a schematic diagram of the atomic structure of the MoS2-Pd hydrogen-sensitive material in an embodiment of the present disclosure.
[0040] FIG5 a is an atomic force microscope image of the MoS2-Pd hydrogen-sensitive material prepared in Example 1 of the present disclosure.
[0041] FIG5 b is an atomic force microscope image of the MoS 2 -Pd hydrogen-sensitive material prepared in Example 2 of the present disclosure.
[0042] FIG5c is an atomic force microscope image of the MoS2-Pd hydrogen-sensitive material prepared in Example 3 of the present disclosure.
[0043] FIG5 d is an atomic force microscope image of the MoS2-Pd hydrogen-sensitive material prepared in Example 4 of the present disclosure.
[0044] FIG6 is a graph showing the relationship between the diameter of Pd nanoparticles and the deposition time in Examples 1-4 of the present disclosure.
[0045] FIG7 is an atomic force microscope image of the MoS2-Pd hydrogen-sensitive material prepared in Comparative Example 2.
[0046] FIG8 is a response curve diagram of the fiber Bragg grating hydrogen sensor prepared in Experimental Example 1 of the present disclosure to 1% concentration of hydrogen.
[0047] FIG9 is a response curve diagram of the fiber Bragg grating hydrogen sensor prepared in Experimental Example 2 of the present disclosure to 1% concentration of hydrogen. DETAILED DESCRIPTION
[0048] To make the purpose, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions of the embodiments of the present disclosure are clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of them. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0049] Unless otherwise defined, technical or scientific terms used in the embodiments of the present disclosure should have the same general meanings as those generally understood by persons having ordinary skills in the field to which the present disclosure belongs.
[0050] In this article, the term "and / or" is merely a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone.
[0051] As used herein, the terms "about" and "approximately" refer to + / - 10% of the recited value.
[0052] Where values are described herein as ranges, it should be understood that such disclosure includes disclosure of all possible sub-ranges within that range, as well as specific values falling within that range, regardless of whether a specific value or sub-range is explicitly stated.
[0053] On the one hand, an embodiment of the present disclosure provides a method for preparing a MoS2-Pd hydrogen-sensitive material, comprising steps S1 to S5.
[0054] S1, growing a MoS2 thin film on a substrate to obtain a substrate loaded with the MoS2 thin film.
[0055] S2, preparing a conductive substrate.
[0056] S3, transferring the MoS2 thin film on the substrate to a conductive substrate to obtain a conductive substrate loaded with the MoS2 thin film.
[0057] S4, prepare palladium chloride hydrochloric acid solution as electroplating solution.
[0058] S5, immersing the conductive substrate loaded with the MoS2 thin film in an electroplating solution, performing electrochemical deposition under a constant potential, and then immersing it in deionized water to remove the residual electroplating solution to prepare a MoS2-Pd hydrogen-sensitive material.
[0059] In the embodiment of the present disclosure, Pd nanoparticles are loaded on the MoS2 film by electrochemical deposition. On the one hand, the MoS2 film has a large specific surface area and various types of defects on the surface, including point defects (vacancies and substitutions), dislocations and grain boundaries, which can serve as Pd nanoparticles. 2+ The deposition active sites make Pd2+ It can be firmly deposited at the active sites on the MoS2 surface and reduced to Pd nanoparticles. The Pd nanoparticles are firmly loaded on the MoS2 film, which enhances the interaction force between the Pd nanoparticles and the MoS2 film, thereby overcoming the problem that the Pd nanoparticles are easy to fall off during the hydrogen absorption and release process. On the other hand, by depositing Pd nanoparticles by electrochemical deposition, the metal Pd precursor salt can be reduced to metal Pd nanoparticles without the need for any additional reducing agent and a high-temperature environment. Compared with the metal evaporation method and chemical reduction method commonly used in existing technologies, the electrochemical deposition method is simpler to operate, the preparation process is environmentally friendly, non-toxic, non-destructive, and has lower cost.
[0060] In some specific embodiments, in step S1, the method for growing a MoS2 thin film on a substrate is: using MoO3 and sulfur powder as reaction raw materials, first placing MoO3 on a substrate and placing it in a tube furnace, then placing a quartz boat filled with sulfur powder in the tube furnace, so that the distance between the two is 15 to 20 cm; then growing a MoS2 thin film on the substrate by chemical vapor deposition to obtain a substrate loaded with a MoS2 thin film.
[0061] In some embodiments, the molar ratio of MoO3 to sulfur powder is 1:2.5 to 1:3, non-limiting examples include 1:2.5, 1:2.7, 1:2.8, 1:3, etc.
[0062] In some embodiments, the temperature of chemical vapor deposition is 820-850° C., non-limiting examples include 820° C., 830° C., 840° C., 850° C., etc. In some embodiments, the temperature is 850° C.
[0063] In some embodiments, the time is 10 to 15 minutes, non-limiting examples include 10 minutes, 12 minutes, 15 minutes, etc. In some embodiments, the time is 15 minutes.
[0064] In some embodiments, the substrate is any one of mica, silicon wafer, or sapphire, and in some embodiments, is mica.
[0065] In some specific embodiments, in step S2, the method for preparing the conductive substrate is: first, PMMA (polymethyl methacrylate) is coated on a partial area of the surface of the SiO2 / Si substrate, and heated at 100°C for 5 to 10 minutes to solidify the PMMA to form a PMMA film; then a metal film is evaporated on the entire surface of the substrate, and then it is immersed in acetone at 65°C. The metal film coated on the PMMA film will fall off as the PMMA film dissolves, so that the metal film is retained only on the residual area of the surface of the SiO2 / Si substrate, thereby obtaining a conductive substrate.
[0066] In some embodiments, the evaporated area of the metal film occupies 30% to 50% of the surface area of the SiO 2 / Si substrate.
[0067] In some embodiments, the metal film is a Cr / Au metal film or a Ti / Au metal film, and in some embodiments, a Cr / Au metal film.
[0068] In some embodiments, in the Cr / Au metal film, the thickness ratio of the Cr metal film to the Au metal film is 1:10; the thickness of the Cr metal film is 6 to 10 nm, including non-limiting examples such as 6 nm, 8 nm, and 10 nm. In some embodiments, it is 10 nm; the thickness of the Au metal film is 60 to 100 nm, including non-limiting examples such as 60 nm, 70 nm, 80 nm, and 100 nm. In some embodiments, it is 100 nm.
[0069] In the Ti / Au metal film, the thickness ratio of the Ti metal film to the Au metal film is 1:10; the thickness of the Ti metal film is 6 to 10 nm, including non-limiting examples such as 6 nm, 8 nm, and 10 nm. In some embodiments, it is 10 nm. The thickness of the Au metal film is 60 to 100 nm, including non-limiting examples such as 60 nm, 70 nm, 80 nm, and 100 nm. In some embodiments, it is 100 nm.
[0070] In some specific embodiments, in step S3, the method of transferring the MoS2 thin film is: spin-coating a drop of PMMA on the surface of the substrate loaded with the MoS2 thin film obtained in step S1, and heating it at 100°C for 5 to 10 minutes to solidify the PMMA to form a PMMA film; then immersing it in deionized water, and using the surface tension of water to separate the PMMA film with the MoS2 thin film from the substrate; then sticking the PMMA film with the MoS2 thin film to the conductive substrate obtained in step S2, and drying it so that the PMMA film with the MoS2 thin film is tightly fitted to the conductive substrate; finally, immersing it in a hot acetone solution at 65°C for 15 to 20 minutes to dissolve and fall off the PMMA film on the surface of the MoS2 thin film, and then washing it with deionized water and isopropyl alcohol in sequence, and blowing it dry with nitrogen to obtain a conductive substrate with a surface loaded with MoS2 thin film.
[0071] In some embodiments, the spin coating speed is 2000-3000 rpm, non-limiting examples include 2000 rpm, 2500 rpm, 2800 rpm, 3000 rpm, etc.; the spin coating time is 45-60 s, non-limiting examples include 45 s, 50 s, 55 s, 60 s, etc.
[0072] In some specific embodiments, in step S4, the method for preparing the palladium chloride hydrochloric acid solution is: dissolving palladium chloride and concentrated hydrochloric acid in deionized water, and mixing them uniformly to obtain the palladium chloride hydrochloric acid solution.
[0073] In some embodiments, the molar concentration ratio of palladium chloride to concentrated hydrochloric acid is 0.03:1 to 0.04:1, non-limiting examples include 0.03:1, 0.035:1, 0.04:1, etc.
[0074] In some specific embodiments, in step S5, the constant potential is -0.20 V vs SCE, and the electrochemical deposition time is 5 to 30 s, non-limiting examples include: 5 s, 10 s, 18 s, 20 s, 25 s, 30 s, etc.; in some embodiments, it is 10 to 15 s, non-limiting examples include: 10 s, 12 s, 15 s, etc.
[0075] In the embodiment of the present disclosure, Pd nanoparticles are deposited on the MoS2 film by an electrochemical deposition method, and the size of the Pd nanoparticles can be controlled by regulating the deposition time so that it can meet the actual needs of the fiber Bragg grating hydrogen sensor under different working conditions. This method is more flexible and simple, has a wider range of applications, and is more adaptable.
[0076] In the preparation method of the MoS2-Pd hydrogen-sensitive material in the embodiment of the present disclosure, step S5 is to connect a traditional three-electrode system with an electrochemical workstation CHI660E for electrochemical deposition (as shown in Figure 1). Specifically, a saturated calomel electrode (SCE) is used as a reference electrode, a platinum sheet is used as a counter electrode, and a conductive clamp is used to clamp the conductive substrate with the surface-loaded MoS2 film obtained in step (3) as a working electrode; the electroplating solution uses a prepared palladium chloride hydrochloric acid solution, and it is necessary to pay attention to keeping a distance of 3 mm between the solution interface and the clamp to prevent the electroplating solution from dipping into the clamp.
[0077] The deposition mode adopts constant potential deposition, and the appropriate deposition potential is selected according to the potential corresponding to the position of the Pd reduction peak in the cyclic voltammetry test curve. Specifically: the cyclic voltammetry test is performed at a scan rate of 10mV / s, and the scan range is 0.30~-0.45V vs SCE. As shown in Figure 2, after three cyclic scans, the cyclic voltammetry curve tends to be stable, and the potential corresponding to the position of the Pd reduction peak in the curve is approximately -0.10~-0.20V vs SCE. The inventors found that selecting a relatively negative potential can increase the nucleation density of Pd. Therefore, the embodiment of the present disclosure limits the deposition potential of Pd to -0.20V vs SCE.
[0078] In step (5), the electrochemical reduction process is involved in loading Pd nanoparticles on the conductive substrate with the MoS2 thin film on the surface by electrochemical deposition:
[0079] By applying less than Pd 2+(0.915V vs SHE) the deposition potential of the reduction potential (-0.20V vs SCE), resulting in the Pd in the plating solution 2+ It receives electrons and is reduced to Pd nanoparticles.
[0080] As one of the most representative emerging two-dimensional layered materials, MoS2 is another semiconductor material that has attracted much attention after graphene, and has excellent physical and chemical properties. The MoS2 film prepared in the embodiment of the present disclosure has a large specific surface area, and various types of defects exist on its surface, including point defects (vacancies and substitutions), dislocations and grain boundaries, which can act as a Pd in the plating solution. 2+ At the same time, since the electron distribution near the defect shows obvious localization characteristics, there is a high density of electrons gathered near the vacancy, which makes Pd 2+ Pd nanoparticles can be preferentially reduced at defect sites, nucleating and growing to form Pd nanoparticles. This increases the interaction between the Pd nanoparticles and the MoS2 film, overcoming the problem of Pd nanoparticles easily falling off during hydrogen absorption and release. Furthermore, compared to metallic Pd films, Pd nanoparticles have a larger specific surface area. When used in hydrogen sensors, hydrogen can adsorb onto the surface of the Pd nanoparticles from all directions and then diffuse into the interior, increasing the contact area between gas molecules and Pd and shortening the hydrogen adsorption-permeation-diffusion time, thereby improving the response speed of the hydrogen sensor.
[0081] Another aspect of the present disclosure is a MoS2-Pd hydrogen-sensitive material prepared by the above-described preparation method. Its macroscopic structure and atomic structure are shown in Figures 3 and 4, respectively. In the MoS2-Pd hydrogen-sensitive material of the present disclosure, the interaction between the metallic Pd nanoparticles and the MoS2 film is stronger, overcoming the problem of Pd easily falling off during hydrogen absorption and release.
[0082] On the other hand, the embodiments of the present disclosure further propose the application of the above-mentioned MoS2-Pd hydrogen-sensitive material in a fiber Bragg grating hydrogen sensor. The MoS2-Pd hydrogen-sensitive material is used as a hydrogen-sensitive material in a fiber Bragg grating hydrogen sensor and exhibits good sensitivity and responsiveness.
[0083] The present disclosure also provides a method for preparing the above-mentioned fiber Bragg grating hydrogen sensor, comprising the following steps:
[0084] 1) etching the optical fiber cladding on the surface of the fiber Bragg grating using 40 wt % hydrofluoric acid to obtain a pretreated optical fiber;
[0085] 2) Spin-coating a drop of PMMA on the surface of the MoS2-Pd hydrogen-sensitive material and heating it at 100°C for 5-10 minutes to solidify the PMMA to form a PMMA film; then immersing the material in a 5wt% NaOH solution, and using the etching effect of NaOH on the SiO2 / Si substrate to separate the PMMA film with the MoS2-Pd hydrogen-sensitive material from the SiO2 / Si substrate, thereby obtaining a PMMA film loaded with the MoS2-Pd hydrogen-sensitive material;
[0086] 3) affixing a PMMA film loaded with MoS2-Pd hydrogen-sensitive material to the pretreated optical fiber, drying the film naturally, and then processing and packaging the film to obtain the fiber Bragg grating hydrogen sensor.
[0087] In the preparation method of the fiber Bragg grating hydrogen sensor in the embodiment of the present disclosure, MoS2-Pd is used as the hydrogen-sensitive material, and is transferred to the processed optical fiber by wet etching using PMMA as a medium. The entire process causes almost no damage to the optical fiber, thereby ensuring that the prepared fiber Bragg grating hydrogen sensor has a long life, good stability, and can quickly and continuously monitor hydrogen.
[0088] In some specific embodiments, in step 2), the spin coating speed is 2000-3000 rpm, non-limiting examples include: 2000 rpm, 2500 rpm, 2800 rpm, 3000 rpm, etc.; the spin coating time is 45-60 s, non-limiting examples include: 45 s, 50 s, 55 s, 60 s, etc.
[0089] In some specific embodiments, in step 2), the etching temperature is 50-70°C, non-limiting examples include: 50°C, 75°C, 50°C, 70°C, etc.; the etching time is 15-20 minutes, non-limiting examples include: 15 minutes, 18 minutes, 20 minutes, etc.
[0090] The present invention is further described in detail below with reference to specific examples. The following examples utilize conventional instruments and equipment in the art. Experimental methods not specifically specified in the examples are based on conventional methods and conditions well known in the art, or methods and conditions recommended by the manufacturer. Unless otherwise noted, the various raw materials used in the following examples are conventional commercially available products or can be prepared by known methods.
[0091] Example 1
[0092] This embodiment provides a method for preparing a MoS2-Pd hydrogen-sensitive material, comprising the following steps:
[0093] S1, preparation of MoS2 thin film on substrate
[0094] 2.7 g of MoO3 was placed on a mica substrate and placed in a tube furnace. A quartz boat containing 1.5 g of sulfur powder was then placed in the tube furnace with a distance of 20 cm between the two. The tube furnace was then heated to 850°C and kept warm for 15 minutes to allow the MoO3 to react with sulfur vapor to form MoS2, which was then deposited on the mica substrate, obtaining a mica substrate loaded with MoS2 thin film.
[0095] S2, preparation of conductive substrate
[0096] PMMA (polymethyl methacrylate) is coated on half of the surface of a SiO2 / Si substrate and heated at 100°C for 10 minutes to solidify the PMMA to form a PMMA film. A Cr / Au (10nm / 100nm) metal film is then thermally evaporated on the entire surface of the substrate. The substrate is then immersed in acetone at 65°C. The Cr / Au metal film on the PMMA film will fall off as the PMMA film dissolves, leaving only half of the surface of the SiO2 / Si substrate coated with the Cr / Au metal film, thus obtaining a conductive substrate.
[0097] Transfer of S3, MoS2 thin films
[0098] A drop of PMMA is spin-coated on the surface of the mica substrate loaded with the MoS2 thin film obtained in step S1, and heated at 100°C for 10 minutes to solidify the PMMA to form a PMMA film; then immersed in deionized water, and the PMMA film with the MoS2 thin film is separated from the mica substrate by the surface tension of water; then the PMMA film with the MoS2 thin film is attached to the conductive substrate obtained in step S2 and dried. After the water between the two evaporates, the PMMA film with the MoS2 thin film is tightly attached to the conductive substrate due to the van der Waals force between molecules; finally, it is immersed in a hot acetone solution at 65°C for 15 minutes to dissolve the PMMA film on the surface of the MoS2 thin film and fall off, and then washed with deionized water and isopropyl alcohol in sequence, and blown dry with nitrogen to obtain a conductive substrate with a surface loaded with MoS2 thin film;
[0099] S4, prepare the plating solution
[0100] 0.53 g of palladium chloride and 3.1 mL of 36% concentrated hydrochloric acid were dissolved in 1000 mL of deionized water and mixed well to obtain a palladium chloride hydrochloric acid solution, which was used as an electroplating solution for preparing metal Pd nanoparticles by electrochemical deposition;
[0101] S5, Controllable Deposition of Pd Nanoparticles on MoS2 Thin Films by Electrochemical Deposition
[0102] The conductive substrate with the surface-loaded MoS2 film obtained in step S3 was immersed in an electroplating solution and electrochemically deposited at a constant potential of -0.20 V vs SCE. After deposition for 5 seconds, the substrate was immersed in deionized water to remove the residual electroplating solution, thereby obtaining a MoS2-Pd hydrogen-sensitive material.
[0103] As shown in FIG5a, it is an atomic force microscope image of the MoS2-Pd hydrogen-sensitive material prepared in this embodiment. It can be seen from the figure that the diameter of the Pd nanoparticles deposited on the MoS2 film in this embodiment is about 2 nm.
[0104] Example 2
[0105] The preparation process of the MoS2-Pd hydrogen-sensitive material in this embodiment is similar to the preparation process of the MoS2-Pd hydrogen-sensitive material in Example 1, with the only difference being that in this embodiment, the deposition time in step S5 is 10 s.
[0106] As shown in FIG5 b , it is an atomic force microscope image of the MoS 2 -Pd hydrogen-sensitive material prepared in this embodiment. As can be seen from the image, the diameter of the Pd nanoparticles deposited on the MoS 2 film in this embodiment is about 9 nm.
[0107] Example 3
[0108] The preparation process of the MoS2-Pd hydrogen-sensitive material in this embodiment is similar to the preparation process of the MoS2-Pd hydrogen-sensitive material in Example 1, with the only difference being that in this embodiment, the deposition time in step S5 is 15 s.
[0109] As shown in FIG5c, it is an atomic force microscope image of the MoS2-Pd hydrogen-sensitive material prepared in this embodiment. It can be seen from the figure that the diameter of the Pd nanoparticles deposited on the MoS2 film in this embodiment is about 16 nm.
[0110] Example 4
[0111] The preparation process of the MoS2-Pd hydrogen-sensitive material in this embodiment is similar to the preparation process of the MoS2-Pd hydrogen-sensitive material in Example 1, with the only difference being that in this embodiment, the deposition time in step S5 is 30 s.
[0112] As shown in FIG5d, it is an atomic force microscope image of the MoS2-Pd hydrogen-sensitive material prepared in this embodiment. It can be seen from the figure that the diameter of the Pd nanoparticles deposited on the MoS2 film in this embodiment is about 36 nm.
[0113] Figure 6 is a relationship diagram between the diameter size of Pd nanoparticles in the MoS2-Pd hydrogen-sensitive material obtained in Examples 1-4 of the present disclosure and the deposition time. It can be seen from the figure that the diameter size of the Pd nanoparticles is approximately linearly related to the deposition time. Therefore, the size of the Pd nanoparticles in the MoS2-Pd hydrogen-sensitive material can be flexibly controlled by adjusting the deposition time to meet the actual needs of the hydrogen sensor under different working conditions.
[0114] Comparative Example 1
[0115] The preparation process of the MoS2-Pd hydrogen-sensitive material in this comparative example is similar to the preparation process of the MoS2-Pd hydrogen-sensitive material in Example 4, except that: the preparation method of this comparative example does not include step S4, and in step S5 of this comparative example, a Pd metal film of about 36 nm is sputtered on the MoS2 film by magnetron sputtering.
[0116] Comparative Example 2
[0117] The preparation process of the MoS2-Pd hydrogen-sensitive material in this comparative example is similar to that of the MoS2-Pd hydrogen-sensitive material in Example 4, except that in this comparative example, in step S5, electrochemical deposition is performed at a constant potential of -0.10 V vs SCE.
[0118] As shown in FIG7 , it is an atomic force microscope image of the MoS2-Pd hydrogen-sensitive material prepared in this comparative example. It can be seen from the figure that in the MoS2-Pd hydrogen-sensitive material prepared in this comparative example, the diameter of the Pd nanoparticles deposited on the MoS2 film is about 10 nm.
[0119] By comparing Example 4 with Comparative Example 2, it can be seen that the same electrochemical deposition method is used with a deposition time of 30s. However, the results show that in Example 4, electrochemical deposition is performed at a constant potential of -0.20V vs SCE, and the diameter of the Pd nanoparticles in the MoS2-Pd hydrogen-sensitive material obtained is about 36nm, with a high nucleation density; while in Comparative Example 2, electrochemical deposition is performed at a constant potential of -0.10V vs SCE, and the diameter of the Pd nanoparticles in the MoS2-Pd hydrogen-sensitive material obtained is only about 10nm, with a low nucleation density. This further illustrates that the use of electrochemical deposition at a constant potential of -0.20V vs SCE in the disclosed embodiments can increase the nucleation density of Pd nanoparticles.
[0120] Experimental Example 1
[0121] In this experimental example, the MoS2-Pd hydrogen-sensitive material prepared in Example 4 was selected as the hydrogen-sensitive material of the fiber Bragg grating hydrogen sensor to prepare the fiber Bragg grating hydrogen sensor.
[0122] The preparation method of the fiber Bragg grating hydrogen sensor comprises the following steps:
[0123] 1) etching the optical fiber cladding on the surface of the fiber Bragg grating using 40 wt % hydrofluoric acid to obtain a pretreated optical fiber;
[0124] 2) Spin-coating a drop of PMMA on the surface of the MoS2-Pd hydrogen-sensitive material at a rotation speed of 3000 rpm for 60 seconds, and heating at 100°C for 5-10 minutes to solidify the PMMA to form a PMMA film; then immersing the material in a 5 wt% NaOH solution at 50°C to separate the PMMA film with the MoS2-Pd hydrogen-sensitive material from the SiO2 / Si substrate by etching the SiO2 / Si substrate with NaOH. After etching for 15 minutes, a PMMA film loaded with the MoS2-Pd hydrogen-sensitive material is obtained;
[0125] 3) a PMMA film loaded with MoS2-Pd hydrogen-sensitive material is attached to the pretreated optical fiber and allowed to dry naturally. The PMMA film on the surface of the MoS2-Pd hydrogen-sensitive material is directly used as a protective layer without being removed. Finally, the PMMA film is processed and packaged to obtain a fiber Bragg grating hydrogen sensor.
[0126] A hydrogen detection experiment was conducted on the fiber Bragg grating hydrogen sensor prepared above: the prepared fiber Bragg grating hydrogen sensor was placed in a gas chamber, and hydrogen with a concentration of 1% was introduced to detect the real-time cyclic response of the fiber Bragg grating hydrogen sensor to 1% hydrogen concentration. The test results are shown in Figure 8.
[0127] As shown in Figure 8, when the hydrogen concentration increases from 0 to 1%, the wavelength shifts significantly, reaching 105 pm. The sensor sensitivity is 105 pm / %, indicating high sensitivity. The sensor's response and recovery times are 25 and 40 seconds, respectively, with minimal wavelength fluctuation and excellent sensor stability. Compared to similar Pd-based fiber Bragg grating hydrogen sensors, the sensor's performance is superior.
[0128] The above test results show that the fiber Bragg grating hydrogen sensor based on MoS2-Pd hydrogen-sensitive material in the embodiment of the present disclosure can monitor hydrogen quickly and continuously, and exhibits good sensitivity, responsiveness and stability.
[0129] Experimental Example 2
[0130] In this experimental example, the MoS2-Pd hydrogen-sensitive material prepared in Comparative Example 1 was used as the hydrogen-sensitive material of the fiber Bragg grating hydrogen sensor to prepare the fiber Bragg grating hydrogen sensor. The preparation method of the fiber Bragg grating hydrogen sensor was the same as that in Experimental Example 1.
[0131] A hydrogen detection experiment was conducted on the fiber Bragg grating hydrogen sensor prepared in this experimental example: the prepared fiber Bragg grating hydrogen sensor was placed in a gas chamber, and hydrogen with a concentration of 1% was introduced to detect the real-time cyclic response of the above fiber Bragg grating hydrogen sensor to 1% hydrogen concentration. The test results are shown in Figure 9.
[0132] As can be seen from Figure 9, when the hydrogen concentration first increases from 0 to 1%, the wavelength drift is 80 pm, the sensor sensitivity is 80 pm / %, and the sensor response time and recovery time are 80 s and 110 s, respectively. In the next two experiments, the wavelength drift is 45 pm, the sensor sensitivity is 45 pm / %, and the sensor response time and recovery time are 100 s and 140 s, respectively. The wavelength fluctuation is large, and the sensor performance is degraded.
[0133] From the above results, it can be seen that compared with the electrochemical deposition method to deposit Pd nanoparticles on MoS2 thin film, the sputtering of Pd metal film on MoS2 thin film by magnetron sputtering is more likely to cause partial phase change of Pd metal film during the reaction with hydrogen, because the binding force between Pd metal film and MoS2 is weaker than that between Pd nanoparticles and MoS2, and the Pd metal film becomes brittle and falls off, which in turn leads to a decrease in the sensitivity of the fiber Bragg grating hydrogen sensor, and the performance will decay after multiple tests; and compared with Pd nanoparticles, the Pd metal film has a smaller specific surface area, which reduces the contact area between hydrogen molecules and Pd, resulting in a longer hydrogen adsorption-permeation-diffusion time, so the prepared fiber Bragg grating hydrogen sensor has a longer response time and recovery time; in addition, compared with the electrochemical deposition method, magnetron sputtering is not a non-destructive process, which leads to a decrease in the quality of the prepared MoS2-Pd hydrogen-sensitive material.
[0134] In the present disclosure, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.
[0135] Although the embodiments of the present disclosure have been shown and described above, it is understood that the above embodiments are illustrative and are not to be construed as limitations on the present disclosure. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present disclosure.
Claims
1. A method for preparing a MoS2-Pd hydrogen-sensitive material, characterized in that: The steps include: S1, growing a MoS2 thin film on a substrate by chemical vapor deposition to obtain a substrate loaded with the MoS2 thin film; S2, preparing a conductive substrate; S3, transferring the MoS2 thin film on the substrate to the conductive substrate to obtain a conductive substrate loaded with the MoS2 thin film; S4, preparing palladium chloride hydrochloric acid solution as an electroplating solution; S5, immersing the conductive substrate loaded with the MoS2 thin film into the electroplating solution, performing electrochemical deposition under constant potential, and then immersing in deionized water to remove residual electroplating solution to obtain the MoS2-Pd hydrogen-sensitive material; Wherein, in the step S2, the method for preparing the conductive substrate is: evaporating a metal film on the surface of a SiO2 / Si substrate to obtain the conductive substrate; the evaporation area of the metal film accounts for 30% to 50% of the surface area of the SiO2 / Si substrate; the metal film is a Cr / Au metal film or a Ti / Au metal film; in the Cr / Au metal film, the thickness ratio of the Cr metal film to the Au metal film is 1:10; and the thickness of the Cr metal film is 6 to 10 nm; the thickness of the Au metal film is 60 to 100 nm; in the Ti / Au metal film, the thickness ratio of the Ti metal film to the Au metal film is 1:10; and the thickness of the Ti metal film is 6 to 10 nm; the thickness of the Au metal film is 60 to 100 nm; In the step S5, the constant potential is -0.20 V vs SCE, and the electrochemical deposition time is 5 to 30 seconds.
2. The method for preparing the MoS2-Pd hydrogen-sensitive material according to claim 1, characterized in that: In the step S1, the method for growing the MoS2 thin film on the substrate is: using MoO3 and sulfur powder as reaction raw materials, growing the MoS2 thin film on the substrate by chemical vapor deposition to obtain the substrate loaded with the MoS2 thin film; the molar ratio of the MoO3 to the sulfur powder is 1:2.5 to 1:3; the temperature of the chemical vapor deposition is 820 to 850°C, and the time is 10 to 15 minutes; the substrate is any one of mica, silicon wafer or sapphire.
3. The method for preparing the MoS2-Pd hydrogen-sensitive material according to claim 1 or 2, characterized in that: In the step S3, the method of transferring the MoS2 film is: using PMMA as a medium to transfer the MoS2 film on the substrate to the conductive substrate by wet etching.
4. The method for preparing the MoS2-Pd hydrogen-sensitive material according to any one of claims 1 to 3, characterized in that: In step S4, the method for preparing the palladium chloride hydrochloric acid solution is: dissolving palladium chloride and concentrated hydrochloric acid in deionized water, and mixing them evenly to obtain the palladium chloride hydrochloric acid solution; the molar concentration ratio of the palladium chloride to the concentrated hydrochloric acid is 0.03:1 to 0.04:
1.
5. A MoS2-Pd hydrogen-sensitive material, characterized in that: The MoS2-Pd hydrogen-sensitive material is prepared by the preparation method described in any one of claims 1 to 4.
6. The use of the MoS2-Pd hydrogen sensitive material according to claim 5 in a fiber Bragg grating hydrogen sensor, characterized in that: The MoS2-Pd hydrogen-sensitive material is used as a hydrogen-sensitive material in a fiber Bragg grating hydrogen sensor.
7. A method for preparing a fiber Bragg grating hydrogen sensor, characterized in that: The steps include: 1) using 40 wt % hydrofluoric acid to etch the optical fiber cladding on the surface of the optical fiber Bragg grating to obtain a pretreated optical fiber; 2) Spin coating a drop of PMMA on the surface of the MoS2-Pd hydrogen-sensitive material, and heating the PMMA to solidify it to form a PMMA film; and then immersing it in a 5wt% NaOH solution, and using the etching effect of NaOH on the SiO2 / Si substrate to separate the PMMA film adhered with the MoS2-Pd hydrogen-sensitive material from the SiO2 / Si substrate, to obtain a PMMA film loaded with the MoS2-Pd hydrogen-sensitive material, wherein the MoS2-Pd hydrogen-sensitive material is prepared by the preparation method described in any one of claims 1 to 4; 3) The PMMA film loaded with the MoS2-Pd hydrogen-sensitive material is attached to the pretreated optical fiber, and after natural drying, the film is processed and packaged to obtain the fiber Bragg grating hydrogen sensor.
8. The method for preparing a fiber Bragg grating hydrogen sensor according to claim 7, characterized in that: In step 2), the rotation speed of the spin coating is 2000-3000 rpm, and the spin coating time is 45-60 s; the etching temperature is 50-70° C., and the etching time is 15-20 min.
Citation Information
Patent Citations
Method for preparing two-dimensional transition metal sulfide through directional transfer CVD method
CN110676218A
Controllable preparation method of palladium-based hydrogen sensitive material
CN115418621A
MoS2-Pd hydrogen sensitive material and preparation method thereof
CN116288234A
Cutter for metal wastes
KR1020220101463A