Low-oxygen-vacancy and high-performance lithium manganate positive electrode material and preparation method therefor

By optimizing the heat treatment process and doping technology of lithium manganate, the performance problems caused by oxygen vacancy in the lithium manganate positive electrode material are solved, and the circulation and storage performance of the battery is significantly improved, which is suitable for the power terminal field.

WO2024234880A1PCT designated stage expired Publication Date: 2024-11-21HUNAN SHANSHAN ENERGY TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/086989
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-04-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The presence of oxygen vacancy in the lithium manganate positive electrode material leads to a decline in battery performance. The existing technology is difficult to effectively reduce the proportion of oxygen vacancy, affecting the high-temperature performance and service life of the battery.

Method used

By controlling the heat treatment process of the material and adding an appropriate amount of metal compound doping, the high-temperature calcination parameters and secondary sintering temperature of lithium manganese oxide are optimized to form a tight network structure, reducing the dissolution of oxygen vacancies and manganese ions, and improving electrochemical performance.

Benefits of technology

It significantly reduces the amount of oxygen vacancy and Mn dissolution in lithium manganate crystals, improves the circulation and storage performance of the battery, and makes the product suitable for power terminal fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024086989_21112024_PF_FP_ABST
    Figure CN2024086989_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A low-oxygen-vacancy and high-performance lithium manganate positive electrode material. The oxygen vacancy amount thereof is in the range of 10-10,000 ppm after the lithium manganate positive electrode material is characterized by means of an electron paramagnetic resonance spectrum. A preparation method for the positive electrode material comprises the following steps: mixing an Li source compound, an Mn source compound and a compound containing a fluxing agent element, and performing primary calcination in an air atmosphere; and mixing the primary calcination product with a monovalent metal ion compound, performing secondary calcination in an air atmosphere at a temperature lower than that of the primary calcination, and cooling and crushing same to obtain the product. The oxygen vacancy amount of the obtained high-performance lithium manganate positive electrode material is reduced to 1080 ppm, and the Mn dissolution amount is reduced to 23 ppm, such that the high-temperature cycle performance and storage performance are greatly improved, and the product can be well used in the power terminal field of passenger vehicles, electric bicycles, electric tools, etc.
Need to check novelty before this filing date? Find Prior Art

Description

A high-performance lithium manganate cathode material with low oxygen vacancies and its preparation method Technical Field

[0001] The present invention belongs to the field of lithium-ion battery positive electrode materials, and in particular relates to a high-performance lithium manganate positive electrode material with low oxygen vacancies and a preparation method thereof. Background Art

[0002] Lithium manganese oxide (LiMn2O4) is a commonly used positive electrode material. It is widely used in lithium-ion batteries due to its low price, easy synthesis, and good low-temperature performance. The crystal structure of lithium manganese oxide belongs to the cubic system with the space group Fd3m. Conventional synthesis processes in the industry generally have crystal structure defects, such as the sintering process reaction rate is too fast or the resulting oxygen penetration is insufficient, and oxygen vacancies caused by the lack of internal oxygen atoms. This structural defect can weaken the bond energy between metal atoms and oxygen atoms, prompting the dissolution of trivalent manganese elements from the spinel structure, resulting in a disproportionation effect that leads to the dissolution of manganese, consumption of positive electrode active materials, and thus reducing the performance and service life of the battery. Therefore, oxygen vacancies in lithium manganese oxide crystals are an important influencing factor leading to its performance degradation. Process optimization measures are needed to reduce the proportion of oxygen vacancies so that it has high performance and can be successfully applied in the power field.

[0003] Patent document CN108091858A discloses a lithium-rich cathode material of Li-O doped lithium manganate and its preparation method, wherein the lithium-rich cathode material is modified by doping elemental lithium compounds, wherein the Li-doped elemental lithium compound is doped with N, P at the Li position and / or the O-doped elemental lithium compound is doped with F, Cl at the O position, so as to form a strong covalent bond or reduce part of the Mn 4+ , achieving the goal of reducing the charge compensation of oxygen atoms during the charge and discharge process and reducing the occurrence of oxygen vacancies. However, this patent reduces the oxygen vacancies generated by layered lithium manganese oxide with the molecular formula Li2MnO3 during the charge and discharge process, which is different from the present invention's solution to the oxygen vacancies in the crystal structure itself, and the preparation process is complex.

[0004] Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology, reduce the oxygen vacancy ratio of existing lithium manganese oxide positive electrode materials, and provide a high-performance lithium manganese oxide positive electrode material with low oxygen vacancies and a preparation method thereof.

[0006] To reduce the impact of oxygen vacancies in lithium manganese oxide crystals on battery performance, optimization can be achieved by controlling the material's heat treatment process and adding appropriate additives. For example, using appropriate high-temperature calcination parameters and adding metal compound doping methods can effectively reduce the proportion of oxygen vacancies in lithium manganese oxide crystals and the amount of Mn dissolution, thereby improving its electrochemical performance.

[0007] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0008] A high-performance lithium manganate cathode material with low oxygen vacancies. After being characterized by electron paramagnetic resonance spectroscopy, the high-performance lithium manganate cathode material has an oxygen vacancy content of 10-10000 ppm, indicating that the number of vacancies per 1000 oxygen atoms is 0.01-10.

[0009] The amount of oxygen vacancies can be characterized using EPR (Electron Paramagnetic Resonance Spectroscopy). In lithium manganate crystals, oxygen deficiency leads to hole formation and changes in the redox state of manganese ions, resulting in the generation of unpaired electrons. EPR technology can detect the characteristic spectral lines of these unpaired electrons, and the internal standard method can be used to quantitatively detect the presence and content of oxygen vacancies. Oxygen vacancies can also cause a small plateau at the end of the discharge curve during electrical performance testing. During product characterization, the proportion of the capacity below 3.5V on the first discharge curve to the total discharge capacity is used to determine the presence of oxygen vacancies.

[0010] The above-mentioned high-performance lithium manganate positive electrode material, preferably, the molecular formula of the high-performance lithium manganate positive electrode material is Li 1+x (M1) y (M2) z Mn 2-x-y-z O4, wherein 0<x<0.15, 0<y<0.15, 0<z<0.15, M1 is at least one of the monovalent metal elements K, Na, and Li, and M2 is at least one of B, Nb, Mo, and V.

[0011] Preferably, the Mn dissolution amount of the high-performance lithium manganate positive electrode material is ≤100 ppm.

[0012] Preferably, the tap density of the high-performance lithium manganate positive electrode material is ≥1.6 g / cm 3 , with a specific surface area of ​​0.15-1.20m 2 / g, particle size D50 is 10-20μm, and span value is 0.5-1.20.

[0013] Based on a general inventive concept, the present invention also provides a method for preparing the above-mentioned high-performance lithium manganese oxide positive electrode material with low oxygen vacancies, comprising the following steps:

[0014] (1) uniformly mixing a Li source compound, a Mn source compound, and a compound containing a flux element according to a stoichiometric ratio to obtain a primary mixture;

[0015] (2) calcining the primary mixture in an air atmosphere, cooling, and crushing to obtain a calcined product;

[0016] (3) mixing the calcined product with a monovalent metal ion compound to obtain a secondary mixture;

[0017] (4) The secondary mixture is subjected to secondary calcination in an air atmosphere at a temperature lower than that of the primary calcination, cooled, and crushed to obtain the secondary calcination product, which is the high-performance lithium manganate positive electrode material.

[0018] The high-performance lithium manganate of the present invention is doped with a fluxing material during the first sintering. By introducing a fluxing agent element (M2 element) doping, the interior and surface grain boundaries of the lithium manganate particles are molten, and the atoms in the crystal are imprisoned to form a tight network structure, thereby effectively reducing the formation of oxygen vacancies; the secondary sintering is doped by adding a monovalent metal cation compound to reduce the dissolution of manganese formed by the trivalent manganese disproportionation reaction. The secondary sintering temperature is controlled to be relatively low to form an annealing stage, which is conducive to repairing internal lattice defects during the sintering process, reducing the amount of oxygen vacancies, and obtaining the final high-performance lithium manganate positive electrode material. The molecular formula of the high-performance lithium manganate positive electrode material can be characterized as Li 1+x (M1) y (M2) z Mn 2-x-y-z O4, wherein 0<x<0.15, 0<y<0.15, 0<z<0.15; M1 is at least one of the monovalent metal elements K, Na, and Li, and M2 is at least one of B, Nb, Mo, and V.

[0019] In the above preparation method, preferably, in step (1), the Li source compound is at least one of LiCO3, LiOH, and LiCl; and the Mn source compound is at least one of MnO2, Mn2O3, Mn3O4, MnCO3, and Mn5O8.

[0020] Preferably, in step (1), the compound containing the flux element is at least one of an oxide, hydroxide, phosphate, carbonate, oxyhydroxyl and alkali containing the flux element, and the flux element is at least one of B, Nb, Mo and V.

[0021] Preferably, in step (2), the temperature of the primary calcination is 750-1100°C, the heating rate is 1-5°C / min, and the calcination time is 2-20h; the ventilation volume of the air atmosphere is 0.1-3m 3 / h; the particle size D50 of the calcined product after crushing is 10-20μm.

[0022] Preferably, in step (3), the monovalent metal ion compound is at least one of an oxide, hydroxide, phosphate, carbonate, oxyhydroxyl and alkali containing a monovalent metal element, and the monovalent metal element is at least one of Li, Na and K.

[0023] Preferably, in step (4), the temperature of the secondary calcination is 500-750°C, and the time is 2-15h; and the ventilation volume of the air atmosphere is 0.1-3m 3 / h; the particle size D50 of the calcined product after crushing is 10-20μm.

[0024] Compared with the prior art, the advantages of the present invention are:

[0025] (1) The present invention incorporates a flux element (M2 element) compound during the first sintering. Under the action of the flux element, lithium and the flux element penetrate into the interior of the manganese source matrix particles and form lithium manganate particles around the manganese source particle matrix under the action of high temperature. The flux element has a low melting point and adhesion, so that the interior and surface grain boundaries of the lithium manganate particles are molten, and the atoms in the crystal are confined to form a tight network structure, thereby effectively reducing the formation of oxygen vacancies. During the secondary sintering, a monovalent metal ion compound (M1 element) is incorporated at a relatively low temperature to balance the comprehensive valence of Mn, and the oxygen vacancies in the manganese source matrix are repaired at low temperature, and its circulation and storage performance are significantly improved. The flux element and the monovalent metal cation compound are compounded after two sinterings, and it is easy to enrich and fix the micropowder particles or fine particles on the surface of the large particles, so that the particle size concentration is high and the specific surface area is reduced, so that the direct contact between the positive electrode material and the electrolyte is reduced, which is beneficial to the material structure stability during the long cycle process.

[0026] (2) Through the preparation method of the present invention, the oxygen vacancy content in the high-performance lithium manganate positive electrode material obtained is reduced from 38140 ppm to 1080 ppm, and the Mn dissolution amount is reduced from about 203 ppm to 23 ppm. Therefore, the high-temperature cycle and storage performance are greatly improved, making the product better applicable to power terminal fields such as passenger cars, electric bicycles, and electric tools. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0028] FIG1 is an XRD spectrum of the high-performance lithium manganate synthesized in Example 1;

[0029] FIG2 is a SEM image of the high-performance lithium manganate synthesized in Example 1;

[0030] FIG3 is a particle size distribution diagram of the high-performance lithium manganate synthesized in Example 1;

[0031] FIG4 is a room temperature (25° C.) cyclic decay curve of the high-performance lithium manganese oxide synthesized in Example 1;

[0032] FIG5 is a high temperature (45° C.) cycle decay curve of the high performance lithium manganese oxide synthesized in Example 1;

[0033] FIG6 is a SEM image of the high-performance lithium manganate synthesized in Example 2;

[0034] FIG7 is a SEM image of the high-performance lithium manganate synthesized in Example 3;

[0035] FIG8 is a SEM image of the high-performance lithium manganate synthesized in Example 4. DETAILED DESCRIPTION

[0036] To facilitate understanding of the present invention, the present invention will be described in more comprehensive and detailed form below in conjunction with the accompanying drawings and preferred embodiments. However, the protection scope of the present invention is not limited to the following specific embodiments.

[0037] Unless otherwise defined, all technical terms used hereinafter have the same meanings as those generally understood by those skilled in the art. The technical terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0039] Example 1:

[0040] A high-performance lithium manganese oxide cathode material with low oxygen vacancies, the molecular formula is Li 1.075 Na 0.008 Mn 1.912 B 0.005 O4.

[0041] The preparation method of the modified lithium manganate positive electrode material of this embodiment includes the following steps:

[0042] (1) Press Li 1.075 Mn 1.912 B 0.005The stoichiometric ratio was designed and calculated. 10 kg of manganese source raw material Mn3O4, 2.679 kg of lithium carbonate, and 20.8 g of a compound containing a flux element H3BO3 were added to a high-speed mixer and mixed at 500 rpm for 5 minutes and then at 1500 rpm for 20 minutes. After the mixing was completed, no white spots were observed visually to obtain a mixture.

[0043] (2) Using a box-type atmosphere furnace, the mixture obtained in step (1) is loaded into a sagger, the loading amount is 50% of the sagger capacity, and placed in a sintering device, and the air atmosphere is ventilated at a ventilation volume of 1m 3 / h / kg mixture (for every sintering of 1kg of mixture, the ventilation volume is 1m 3 / h) setting, raise the temperature to 850℃ at a rate of 2.5℃ / min, keep the temperature constant for 10h, then cool naturally to room temperature and take out of the oven;

[0044] (3) Rolling the mixture sintered in step (2), crushing it with a jet mill, sieving it through a 300-mesh sieve, removing the oversize matter, and obtaining a powder with a particle size not exceeding 12 μm, thereby obtaining a sintered product;

[0045] (4) Take 10 kg of the calcined product, weigh 28.5 g of the monovalent metal ion compound Na2CO3, and put it into a high-speed mixer of a mixing equipment. First, mix it at a low speed of 400 rpm for 5 minutes, and then mix it at 1500 rpm for 15 minutes to obtain a mixture;

[0046] (5) The mixture obtained in step (4) was calcined at 700° C. for 5 h, cooled to room temperature, crushed, and sieved through 300 mesh to obtain a final sample, i.e., the final lithium manganate product. The sample was tested for XRD to obtain the compound phase. The XRD spectrum is shown in Figure 1.

[0047] As shown in FIG1 , the product obtained in this example is free of impurities and has excellent crystallinity after XRD detection.

[0048] The final sample prepared in this example was scanned using an electron microscope (SEM). The results are shown in Figure 2. The primary particles are uniform, with no fine powder particles attached to the surface, and the tap density is 2.2 g / cm 3 , the tap density is high, the internal structure of the material is dense; the specific surface area is 0.21m 2 / g, particle size D50 = 12 μm, span [(D90-D10) / D50] value is 0.96.

[0049] The modified lithium manganese oxide product synthesized in this embodiment was used as the positive electrode and assembled into a CR2032 button cell, and its initial charge and discharge capacity was evaluated. The positive electrode was mixed according to the mass ratio of modified lithium manganese oxide: SP (conductive carbon black): PVDF (binder) = 92.5:0.5:0.25, and then evenly coated on aluminum foil. After drying, rolling, and cutting, the positive electrode sheet was made. The negative electrode sheet used a metal lithium sheet. The assembly and sealing were carried out in a glove box. After static activation for 10 hours, the battery was tested on a Xinwei 5V, 5mA test cabinet with a voltage range of 3.0-4.3V and a charge and discharge of 0.1C. The test results are shown in Figure 3. The initial discharge capacity reached 107.5mAh / g, the initial efficiency reached 98%, the initial discharge capacity below 3.5V accounted for 0.21% of the discharge capacity, the 1C / 0.1C ratio reached 98%, and the rate performance was excellent. The prepared button cells were simultaneously characterized for Mn dissolution. After 10 hours of static activation, they were charged and discharged for a week and then fully charged. The cells were disassembled, the positive electrode plates were placed in a 5 mL plastic bottle, 4 mL of electrolyte was added, and the bottle was placed in a 60°C oven for 2 weeks. The electrolyte was then withdrawn with a syringe, filtered, acid-treated, and diluted. The Mn content was then measured by ICP to obtain the Mn dissolution level. The Mn dissolution level in this example was 23 ppm, as measured by the above method.

[0050] The high-performance lithium manganese oxide synthesized in this example was used as the positive electrode and assembled into a 053048A soft-pack battery. The positive electrode was prepared according to the ratio of modified lithium manganese oxide: SP (conductive carbon black): PVDF (binder) = 93.5:3.25:3.25, and the negative electrode was prepared according to the ratio of FSN-1 (Shanghai Shanshan artificial graphite): SP (conductive carbon black): CMC: SBR = 94.8:1.5:1.7:2.0. The positive electrode slurry was then evenly coated on aluminum foil, and the negative electrode slurry was evenly coated on copper foil. After sheeting, assembly, liquid injection and formation, the battery was tested using a Xinwei test cabinet with a voltage test range of 3.0-4.2V. The cycle performance was tested at room temperature of 25°C and high temperature of 45°C. Figure 4 shows the charge and discharge cycle decay curve at room temperature of 25°C. The capacity retention rate reached 86.2% after 1000 cycles. Figure 5 shows the charge and discharge cycle curve at high temperature of 45°C, and the capacity retention rate reaches 73% after 800 cycles.

[0051] The modified lithium manganate synthesized in this example was characterized by oxygen vacancies using EPR, and the oxygen vacancies were 1080 ppm.

[0052] Example 2:

[0053] The present invention provides a high-performance lithium manganate cathode material with low oxygen vacancies, characterized by the molecular formula Li 1.065 Li 0.009 Mn 1.925 Mo 0.001 O4.

[0054] The preparation method of the modified lithium manganate positive electrode material of this embodiment includes the following steps:

[0055] Press Li 1.065 Mn 1.925 Mo 0.001 After designing the ratio and calculating, 10 kg of manganese source raw material Mn3O4, 2.636 kg of battery-grade lithium carbonate, and 9.6 g of MoO3, a compound containing a flux element, were weighed and added to a high-speed mixer in a mixing equipment. Parameters such as mixing and sintering temperature were the same as those in Example 1. After obtaining a calcined product, 14.4 g of a monovalent metal ion compound LiOH was added per 10 kg of the calcined product. After thorough mixing, the product was added to a high-speed mixer in a mixing equipment. Parameters such as mixing and sintering temperature were the same as those in Example 1. This yielded the final sample, i.e., a high-performance lithium manganate positive electrode material.

[0056] The relevant properties of the modified lithium manganate positive electrode material of this embodiment were tested in the same manner as in Example 1. The oxygen vacancy content of the final product was 1530 ppm as characterized by EPR. The final sample prepared in this embodiment was scanned using an electron microscope (SEM). The results are shown in Figure 6. The primary particles are uniform, with no fine powder particles attached to the surface. The tap density of the material is 2.2 g / cm 3 ;Specific surface area is 0.50m 2 / g, particle size D50 = 11.3μm, span [(D90-D10) / D50] value is 0.92. The prepared button battery, under the voltage range of 3.0-4.3V and charge and discharge 0.1C, tested the first capacity and first discharge capacity to reach 112.5mAh / g, the first efficiency reached 97%, and the capacity below 3.5V in the first discharge capacity accounted for 0.36% of the discharge capacity. The Mn dissolution characterization dissolution amount was 42ppm. The prepared soft pack battery, tested under the voltage test range of 3.0-4.2V, had a 1C / 0.1C ratio of 99%, a capacity retention rate of 84% after 1000 cycles at room temperature, and a capacity retention rate of 76% after 800 cycles at high temperature of 45°C.

[0057] Example 3:

[0058] The present invention provides a high-performance lithium manganate cathode material with low oxygen vacancies, characterized by the molecular formula Li 1.045 Na 0.007 Mn 1.942 Nb 0.006 O4.

[0059] The preparation method of the modified lithium manganate positive electrode material of this embodiment includes the following steps:

[0060] Press Li 1.045 Mn 1.942 Nb 0.006After designing the ratio and calculating, 10 kg of manganese source raw material MnO2, 2.20 kg of battery-grade lithium carbonate, and 45 g of the compound containing flux element Nb2O5 were weighed and added to a high-speed mixer in the mixing equipment. The mixing and sintering temperature and other parameters were consistent with those in Example 1. After obtaining the calcined product, 16 g of the monovalent metal ion compound Na2CO3 was added per 10 kg of the calcined product. After thorough mixing, the product was added to the high-speed mixer in the mixing equipment. The mixing and sintering temperature and other parameters were consistent with those in Example 1. The final sample was obtained, namely, a high-performance lithium manganate positive electrode material.

[0061] The relevant properties of the modified lithium manganate positive electrode material of this embodiment were tested in the same manner as in Example 1. The oxygen vacancy content of the final product was 2340 ppm as characterized by EPR. The final sample prepared in this embodiment was scanned using an electron microscope scanner. The results are shown in Figure 7. The primary particles are uniform and the material tap density is 2.1 g / cm 3 ;Specific surface area is 0.68m 2 / g, particle size D50 = 17μm, span [(D90-D10) / D50] value is 1.05; the prepared button battery, under the voltage range of 3.0-4.3V and charge and discharge at 0.1C, tested the first capacity and first discharge capacity to reach 116.3mAh / g, the first efficiency reached 95%, and the first discharge capacity below 3.5V accounted for 0.64% of the discharge capacity. The Mn dissolution test showed a dissolution amount of 51ppm. The prepared soft-pack battery, tested under the voltage test range of 3.0-4.2V, achieved a 1C / 0.1C ratio of 99%, a capacity retention rate of 82% after 1000 cycles at room temperature, and a capacity retention rate of 75% after 800 cycles at a high temperature of 45°C.

[0062] Example 4:

[0063] The present invention provides a high-performance lithium manganate cathode material with low oxygen vacancies, characterized by the molecular formula Li 1.055 K 0.008 Mn 1.932 V 0.005 O4.

[0064] The preparation method of the modified lithium manganate positive electrode material of this embodiment includes the following steps:

[0065] Press Li 1.055 Mn 1.932 V 0.005After designing the ratio and calculating, 10 kg of manganese source raw material Mn3O4, 2.602 kg of battery-grade lithium carbonate, and 30.20 g of the compound V2O5 containing a flux element were weighed and added to a high-speed mixer in the mixing equipment. The mixing and sintering temperature and other parameters were the same as in Example 1. After obtaining the calcined product, 29.81 g of the monovalent metal ion compound KOH was added per 10 kg of the calcined product. After thorough mixing, the product was added to the high-speed mixer in the mixing equipment. The mixing and sintering temperature and other parameters were the same as in Example 1. The final sample was obtained, namely, a high-performance lithium manganate positive electrode material.

[0066] The modified lithium manganate cathode material of this example was tested using the same method as in Example 1. The final product showed an oxygen vacancy content of 3500 ppm as determined by EPR. The final sample prepared in this example was scanned using an electron microscope (SEM). The results, as shown in Figure 8, show uniform primary particles and a tap density of 2.1 g / cm. 3 Specific surface area is 0.32m 2 / g, particle size D50 = 13.3μm, span [(D90-D10) / D50] value is 0.95; the prepared button battery, under the voltage range of 3.0-4.3V and charge and discharge at 0.1C, tested the first discharge capacity to reach 117.8mAh / g, the first efficiency reached 97.5%, and the capacity below 3.5V in the first discharge accounted for 0.47% of the discharge capacity. The Mn dissolution test showed a dissolution amount of 62ppm. The prepared soft-pack battery, tested under the voltage test range of 3.0-4.2V, achieved a 1C / 0.1C ratio of 99%, a capacity retention rate of 83% after 1000 cycles at room temperature, and a capacity retention rate of 74% after 800 cycles at a high temperature of 45°C.

[0067] Comparative Example 1:

[0068] The preparation method of the modified lithium manganate positive electrode material in this comparative example is different from that in Example 1, except that H3BO3 is not added in step (1).

[0069] The same evaluation method as in Example 1 was used. The oxygen vacancy content of the final product of Example 1 was 14500 ppm as characterized by EPR. The tap density of the material was 2.1 g / cm 3 Specific surface area is 0.65m 2 / g, particle size D50 = 14μm, span [(D90-D10) / D50] value of 1.15; the prepared button cell, tested in the voltage range of 3.0-4.3V and charge and discharge at 0.1C, achieved an initial discharge capacity of 102.6mAh / g, an initial efficiency of 93%, an initial discharge capacity below 3.5V as a proportion of the discharge capacity of 1.05%, and a 1C / 0.1C ratio of 92%. Mn dissolution was 155ppm.

[0070] Assembled into 053048A soft-pack batteries, they were tested within a voltage range of 3.0-4.2V, and their cycling performance was tested at both room temperature (25°C) and high temperature (45°C). The charge-discharge cycle decay curve at room temperature (25°C) showed a capacity retention rate of 70% after 1000 cycles and 65% after 800 cycles.

[0071] Comparative Example 2:

[0072] The preparation method of the modified lithium manganate positive electrode material in this comparative example is different from that in Example 1 except for step (4). The specific operation of step (4) is as follows: 10 kg of the calcined product is put into a high-speed mixer of a mixing equipment without adding Na2CO3, first mixed at a low speed of 400 rpm for 5 minutes, and then mixed at 1500 rpm for 15 minutes to obtain the material to be sintered twice.

[0073] Using the same evaluation method as Example 1, the EPR characterization of the oxygen vacancy content of the final product of Comparative Example 2 was 28260 ppm. The tap density of the material was 1.9 g / cm 3 Specific surface area is 0.58m 2 / g, particle size D50 = 11μm, span [(D90-D10) / D50] value is 1.20; the prepared button battery was tested in the voltage range of 3.0-4.3V and charge and discharge at 0.1C, with an initial discharge capacity of 106.0mAh / g, an initial efficiency of 93.3%, and the capacity below the initial discharge of 3.5V accounted for 1.33% of the discharge capacity. The Mn dissolution test showed that the dissolution amount was 125ppm. The prepared 053048A soft-pack battery was tested in the voltage test range of 3.0-4.2V, with a 1C / 0.1C ratio of 92%, a capacity retention rate of 73% for 1000 weeks at room temperature, and a capacity retention rate of 60% for 800 weeks at high temperature of 45°C.

[0074] Comparative Example 3:

[0075] The preparation method of the modified lithium manganate positive electrode material in this comparative example is the same as the method for preparing the calcined product in Example 1, that is, the methods of steps (1) and (4) are different. The difference is that H3BO3 is not added in step (1); and Na2CO3 is not added in step (4).

[0076] Using the same evaluation method as Example 1, the EPR characterization of the oxygen vacancy content of the final product of Comparative Example 3 was 38140 ppm. The tap density of the material was 1.9 g / cm 3 Specific surface area is 0.70m 2 / g, particle size D50 = 11μm, span [(D90-D10) / D50] value is 1.27; the prepared button battery was tested in the voltage range of 3.0-4.3V and charge and discharge at 0.1C, and the first discharge capacity reached 105.2mAh / g, the first efficiency reached 91%, the capacity below the first discharge 3.5V accounted for 1.78% of the discharge capacity, and the Mn dissolution test showed that the dissolution amount was 203ppm. The prepared 053048A type soft-pack battery was tested in the voltage test range of 3.0-4.2V, the 1C / 0.1C ratio reached 95%, the capacity retention rate at room temperature for 1000 weeks was 60%, and the capacity retention rate at high temperature of 45℃ for 800 weeks was 53%.

Claims

1. A high-performance lithium manganese oxide positive electrode material with low oxygen vacancies, characterized in that: The high-performance lithium manganate positive electrode material is characterized by electron paramagnetic resonance spectroscopy, and its oxygen vacancy content is 10-10000 ppm.

2. The high performance lithium manganate positive electrode material according to claim 1, characterized in that: The molecular formula of the high-performance lithium manganese oxide positive electrode material is Li 1+x (M1) y (M2) z Mn 2-x-y-z O4, wherein 0<x<0.15, 0<y<0.15, 0<z<0.15, M1 is at least one of the monovalent metal elements K, Na, Li, and M2 is at least one of the flux elements B, Nb, Mo, V.

3. The high performance lithium manganate positive electrode material according to claim 1, characterized in that: The Mn dissolution amount of the high-performance lithium manganate positive electrode material is ≤100ppm.

4. The high-performance lithium manganate positive electrode material according to any one of claims 1 to 3, characterized in that The tap density of the high-performance lithium manganate positive electrode material is ≥1.6 g / cm 3 , with a specific surface area of ​​0.15-1.20m 2 / g, particle size D50 is 10-20μm, and span value is 0.50-1.

20.

5. A method for preparing a high-performance lithium manganate positive electrode material with low oxygen vacancies as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: (1) mixing a Li source compound, a Mn source compound, and a compound containing a flux element uniformly according to a stoichiometric ratio to obtain a primary mixture; (2) calcining the primary mixture in an air atmosphere, cooling, and crushing to obtain a calcined product; (3) mixing the primary calcined product with a monovalent metal ion compound to obtain a secondary mixed material; (4) The secondary mixture is subjected to secondary calcination in an air atmosphere at a temperature lower than that of the primary calcination, cooled, and crushed to obtain the secondary calcination product, which is the high-performance lithium manganate positive electrode material.

6. The preparation method according to claim 5, characterized in that: In step (1), the Li source compound is at least one of LiCO3, LiOH, and LiCl, and the Mn source compound is at least one of MnO2, Mn2O3, Mn3O4, MnCO3, and Mn5O8.

7. The preparation method according to claim 5, characterized in that: In step (1), the compound containing the flux element is at least one of an oxide, a hydroxide, a phosphate, a carbonate, a hydroxy oxide, and an alkali containing the flux element, and the flux element is at least one of B, Nb, Mo, and V.

8. The preparation method according to claim 5, characterized in that: In step (2), the primary calcination temperature is 750-1100°C, the heating rate is 1-5°C / min, and the calcination time is 2-20h; for each calcination of 1kg of the primary mixture, the ventilation volume of the air atmosphere is 0.1-3m 3 / h; the particle size D50 of the calcined product after crushing is 10-20μm.

9. The preparation method according to claim 5, characterized in that: In step (3), the monovalent metal ion compound is at least one of an oxide, a hydroxide, a phosphate, a carbonate, a hydroxy oxide, and an alkali containing a monovalent metal element, and the monovalent metal element is at least one of Li, Na, and K.

10. The preparation method according to any one of claims 5 to 9, characterized in that: In step (4), the temperature of the secondary calcination is 500-750°C, and the time is 2-15 hours; and the ventilation volume of the air atmosphere is 0.1-3m 3 / h; the particle size D50 of the pulverized di-calcined product is 10-20μm.

Citation Information

Patent Citations

  • Li-O site lithium manganate doped lithium-enriched positive electrode material and preparation method thereof

    CN108091858A

  • Preparation method of power type lithium manganate

    CN110980811A

  • Composite positive electrode material and preparation method and application thereof

    CN115863592A

  • Low-oxygen-vacancy high-performance lithium manganate positive electrode material and preparation method thereof

    CN116581283A

  • Spinel-Type Lithium-Manganese-Containing Complex Oxide

    US20190051900A1