Solar cell and preparation method therefor

By using an amorphous doped interface layer in silicon heterojunction solar cells, the series resistance is reduced, the filling factor and conversion efficiency are improved, and the battery efficiency is solved in the existing technology caused by the nanocrystalline interface layer.

WO2024234954A1PCT designated stage expired Publication Date: 2024-11-21TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/089570
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-04-24
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In the existing silicon heterojunction solar cells, the N-type interface layer and the P-type interface layer are nanocrystal interface layers, resulting in a large series resistance, making it difficult to improve the filling factor, thus limiting the conversion efficiency of the solar cell.

Method used

The solar cell design adopts a laminated structure, wherein at least one of the N-type interface layer and the P-type interface layer is an amorphous doped interface layer. By improving the contact between the nanocrystal doped layer and the transparent conductive film layer, the series resistance is reduced and the filling is improved. Factors to improve the conversion efficiency of the battery.

Benefits of technology

It significantly reduces the series resistance of solar cells, significantly improves the filling factor and conversion efficiency, and achieves higher battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024089570_21112024_PF_FP_ABST
    Figure CN2024089570_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a solar cell and a preparation method therefor. The solar cell comprises first metal gate line electrodes (100), a first transparent conductive film layer (200), an N-type interfacial layer (300), an N-type nanocrystalline doped layer (400), a first passivation layer (500), a monocrystalline silicon substrate (600), a second passivation layer (700), a P-type nanocrystalline doped layer (800), a P-type interfacial layer (900), a second transparent conductive film layer (1000), and second metal gate line electrodes (1100), wherein said layers and electrodes are stacked. At least one of the N-type interfacial layer (300) and the P-type interfacial layer (900) is an amorphous doped interfacial layer. Therefore, the present invention can increase the area of contact between nanocrystalline doped layers and transparent conductive film layers, can reduce the series resistance of the solar cell, and can increase a fill factor, thereby improving the conversion efficiency of the cell.
Need to check novelty before this filing date? Find Prior Art

Description

Solar cell and preparation method thereof

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 17, 2023, with application number 2023105590112 and invention name “Solar Cell and Its Preparation Method”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present invention belongs to the field of silicon heterojunction solar cells, and in particular relates to a solar cell and a preparation method thereof. Background Art

[0003] Energy has always been an important material basis for human survival and development. As an emerging low-carbon energy source, the photovoltaic industry has been continuously expanding. In order to pursue higher photoelectric conversion efficiency, solar cells are updated and iterated very quickly. Among them, HJT solar cells (Silicon Heterojunction solar cells, silicon heterojunction solar cells, referred to as heterojunction solar cells) have the advantages of structural symmetry, low-temperature preparation process, high open circuit voltage, good temperature characteristics, and thin silicon wafers. They are one of the new generation of crystalline silicon solar cell products. As we all know, improving efficiency and reducing costs have always been the eternal goal of the solar cell industry. Efficiency can be improved by improving the conversion efficiency of cells or increasing the power generation power of components. However, existing solar cells have the problem of low efficiency.

[0004] Therefore, it is necessary to improve solar cells.

[0005] Summary of the Invention

[0006] The present invention is based on the findings and recognition of the following facts and problems by the inventors.

[0007] The formula for calculating solar cell efficiency is: Solar cell efficiency = (open circuit voltage * short circuit current * fill factor) / (cell area * light amplitude) * 100%. The conversion efficiency of the solar cell is proportional to the fill factor (FF). The larger the fill factor (FF), the higher the conversion efficiency of the solar cell.

[0008] Among the internal factors that influence the output characteristics of solar cells, series and parallel resistance have the greatest impact on the fill factor (FF). Specifically, the smaller the series resistance, the larger the parallel resistance, and the higher the fill factor. Improving the FF can generally be achieved by improving material properties and the contact between materials. Heterojunction solar cells include N-type and P-type interface layers. In existing designs, these layers are nanocrystalline, resulting in a high series resistance (Rs) for the cell, making it difficult to further increase the fill factor (FF), a major obstacle to improving cell efficiency.

[0009] To address the above-mentioned technical issues, the present invention provides a solar cell comprising a stacked structure comprising: a first metal grid electrode, a first transparent conductive film layer, an N-type interface layer, an N-type nanocrystal doped layer, a first passivation layer, a single-crystal silicon substrate, a second passivation layer, a P-type nanocrystal doped layer, a P-type interface layer, a second transparent conductive film layer, and a second metal grid electrode; at least one of the N-type interface layer and the P-type interface layer is an amorphous doped interface layer. As a result, the present invention improves contact between the nanocrystal doped layer and the transparent conductive film layer, reduces the series resistance of the solar cell, increases the fill factor, and thereby improves the conversion efficiency of the cell.

[0010] According to an embodiment of the present invention, when one of the N-type interface layer and the P-type interface layer is an amorphous doped interface layer, the other is a nanocrystalline interface layer.

[0011] According to an embodiment of the present invention, the doping concentration of the N-type interface layer is greater than the doping concentration of the N-type nanocrystal doping layer, thereby further improving the fill factor of the battery and thus improving the conversion efficiency of the battery.

[0012] According to an embodiment of the present invention, the doping concentration of the P-type interface layer is greater than the doping concentration of the P-type nanocrystal doping layer, thereby further improving the fill factor of the battery and thus improving the conversion efficiency of the battery.

[0013] According to an embodiment of the present invention, the thickness of the N-type interface layer is 1 to 2 nm, and the thickness of the P-type interface layer is 1 to 2 nm.

[0014] According to an embodiment of the present invention, the solar cell meets at least one of the following conditions: the thickness of the single crystal silicon substrate is 50 to 300 μm; the single crystal silicon substrate is an N-type single crystal silicon wafer or a P-type single crystal silicon wafer; the thickness of the first passivation layer and the second passivation layer are independently selected from 5 to 10 nm; the first passivation layer and the second passivation layer are independently selected from any one of an intrinsic amorphous silicon layer, an intrinsic amorphous silicon oxide layer, and an intrinsic amorphous silicon carbon layer; the N-type nanocrystal doped layer is an N-type nanocrystal silicon oxide layer; the thickness of the N-type nanocrystal doped layer is 20 to 30 nm; The P-type nanocrystal doped layer is a P-type nanocrystalline silicon layer; the thickness of the P-type nanocrystal doped layer is 30 to 40 nm; the thickness of the first transparent conductive film layer and the second transparent conductive film layer are independently selected from 70 to 100 nm; the material forming the first transparent conductive film layer and the material forming the second transparent conductive film layer are independently selected from any one of indium oxide doped with tin, indium oxide doped with tungsten, indium oxide doped with cesium, and zinc oxide doped with aluminum; the first metal grid line electrode and the second metal grid line electrode are independently selected from any one of a silver electrode, a silver-clad copper electrode, and an electroplated copper electrode.

[0015] The present invention also provides a method for preparing the aforementioned solar cell, the method comprising: forming a first passivation layer and a second passivation layer on opposite sides of a single-crystal silicon substrate, respectively; forming an N-type nanocrystal doped layer on a side of the first passivation layer away from the single-crystal silicon substrate; forming a P-type nanocrystal doped layer on a side of the second passivation layer away from the single-crystal silicon substrate; forming an N-type interface layer on a side of the N-type nanocrystal doped layer away from the first passivation layer; forming a P-type interface layer on a side of the P-type nanocrystal doped layer away from the second passivation layer, at least one of the N-type interface layer and the P-type interface layer being an amorphous doped interface layer; forming a first transparent conductive film layer on a side of the N-type interface layer away from the N-type nanocrystal doped layer; forming a second transparent conductive film layer on a side of the P-type interface layer away from the P-type nanocrystal doped layer; forming a first metal gate electrode on a side of the first transparent conductive film layer away from the N-type interface layer; and forming a second metal gate electrode on a side of the second transparent conductive film layer away from the P-type interface layer. Thus, the method has all the features and advantages of the aforementioned solar cell, which will not be described in detail here.

[0016] According to an embodiment of the present invention, the N-type interface layer is formed by any one of plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition; when forming the N-type interface layer, the reaction gas includes PH3 and silane, and the doping concentration of PH3 is 2 to 15%; the substrate temperature is 150 to 250°C, the process chamber pressure is 30 to 600 Pa, and the power is 0.2 to 10 kW.

[0017] According to an embodiment of the present invention, the P-type interface layer is formed by any one of plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition; the formation of the P-type interface layer includes: the reaction gas includes B2H6 and silane, the doping concentration of B2H6 is 2~15%, the substrate temperature is 150~250℃, the process chamber pressure is 30~800Pa, and the power is 0.2~10kw.

[0018] According to an embodiment of the present invention, the method satisfies at least one of the following conditions: the formation methods of the first passivation layer, the second passivation layer, the N-type nanocrystal doped layer, and the P-type nanocrystal doped layer are independently selected from any one of plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition; when forming the first passivation layer and forming the second passivation layer, the substrate temperature is 150-250° C., and the process chamber pressure is 10-400 Pa; when forming the N-type nanocrystal doped layer, the reaction gas includes PH3 and silane, the doping concentration of PH3 is 2-10%, and the substrate temperature is 150-250° C. The process chamber pressure is 100-600 Pa, and the power is 0.5-10 kW; when forming the P-type nanocrystal doping layer, the reaction gases include B2H6 and silane, the doping concentration of B2H6 is 0.1-10%, the substrate temperature is 150-250°C, the process chamber pressure is 100-600 Pa, and the power is 0.5-10 kW; the first transparent conductive film layer and the second transparent conductive film layer are formed by physical vapor deposition or chemical vapor deposition; the first metal grid line electrode and the second metal grid line electrode are formed by any one of screen printing, evaporation, magnetron sputtering, inkjet printing, electroplating, and laser transfer. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] FIG1 is a schematic structural diagram of a solar cell according to an embodiment of the present invention;

[0020] FIG2 is a flow chart of a method for preparing a solar cell in another embodiment of the present invention.

[0021] Description of Reference Numerals

[0022] 100 - first metal gate electrode, 200 - first transparent conductive film layer, 300 - N-type interface layer, 400 - N-type nanocrystal doped layer, 500 - first passivation layer, 600 - single crystal silicon substrate, 700 - second passivation layer, 800 - P-type nanocrystal doped layer, 900 - P-type interface layer, 1000 - second transparent conductive film layer, 1100 - second metal gate electrode. DETAILED DESCRIPTION

[0023] The following embodiments of the present invention are described in detail. The embodiments described below are exemplary and are only used to explain the present invention, and are not to be construed as limiting the present invention. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this field or the product specifications are used. Where the manufacturers of the reagents used are not specified, they are all conventional products that can be obtained commercially.

[0024] The present invention provides a solar cell. Referring to FIG1 , the solar cell comprises a stacked arrangement of: a first metal grid electrode 100, a first transparent conductive film layer 200, an N-type interface layer 300, an N-type nanocrystal doped layer 400, a first passivation layer 500, a single-crystal silicon substrate 600, a second passivation layer 700, a P-type nanocrystal doped layer 800, a P-type interface layer 900, a second transparent conductive film layer 1000, and a second metal grid electrode 1100. At least one of the N-type interface layer 300 and the P-type interface layer 900 is an amorphous doped interface layer. Thus, the present invention can improve contact between the nanocrystal doped layer and the transparent conductive film layer, reduce the series resistance of the solar cell, and increase the fill factor, thereby improving the conversion efficiency of the cell.

[0025] According to an embodiment of the present invention, only one of the N-type interface layer 300 and the P-type interface layer 900 may be an amorphous doped interface layer, or both may be amorphous doped interface layers. When only one of the N-type interface layer 300 and the P-type interface layer 900 is an amorphous doped interface layer, and one of them is an amorphous doped interface layer, the other may be a nanocrystalline interface layer.

[0026] According to some embodiments of the present invention, the N-type interface layer 300 can be μc-Si:H(n+) (N-type nanocrystalline silicon interface layer), a-Si:H(n+) (N-type amorphous silicon interface layer), and the P-type interface layer 900 can be μc-Si:H(p+) (P-type nanocrystalline silicon interface layer), a-Si:H(p+) (P-type amorphous silicon interface layer), as long as at least one of the N-type interface layer 300 and the P-type interface layer 900 is an amorphous doped interface layer.

[0027] According to an embodiment of the present invention, the doping concentration of the N-type interface layer 300 is greater than the doping concentration of the N-type nanocrystal doping layer 400. This can further improve the fill factor of the battery and thus improve the conversion efficiency of the battery.

[0028] According to an embodiment of the present invention, the doping concentration of the P-type interface layer 900 is greater than the doping concentration of the P-type nanocrystal doping layer 800. This can further improve the fill factor of the battery, thereby improving the conversion efficiency of the battery.

[0029] It should be noted that the doping concentration refers to the flow ratio of the dopant to the silane used when fabricating the N-type interface layer 300 , the N-type nanocrystal doped layer 400 , the P-type interface layer 900 , and the P-type nanocrystal doped layer 800 .

[0030] According to an embodiment of the present invention, the thickness of the N-type interface layer 300 is 1-2 nm, for example, 1 nm or 2 nm.

[0031] According to an embodiment of the present invention, the thickness of the P-type interface layer 900 is 1-2 nm, for example, 1 nm or 2 nm.

[0032] According to an embodiment of the present invention, the thickness of the single crystal silicon substrate 600 is 50-300 μm, for example, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, or 300 μm.

[0033] According to an embodiment of the present invention, the single crystal silicon substrate 600 is an N-type single crystal silicon wafer or a P-type single crystal silicon wafer.

[0034] According to an embodiment of the present invention, the thickness of the first passivation layer 500 and the second passivation layer 700 are independently selected from 5 to 10 nm, for example, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, and 10 nm.

[0035] According to an embodiment of the present invention, the first passivation layer 500 and the second passivation layer 700 are independently selected from a-Si:H(i) (intrinsic amorphous silicon layer), a-SiO x :H(i) (intrinsic amorphous silicon oxide layer), a-SiC x : Any one of H(i) (intrinsic amorphous silicon carbon layer).

[0036] According to an embodiment of the present invention, the N-type nanocrystalline doping layer 400 is μc-SiO x : H(n) (N-type nanocrystalline silicon oxide layer).

[0037] According to an embodiment of the present invention, the thickness of the N-type nanocrystal doping layer 400 is 20-30 nm, for example, 20 nm, 25 nm, or 30 nm.

[0038] According to an embodiment of the present invention, the P-type nanocrystalline doped layer 800 is μc-Si:H(p) (P-type nanocrystalline silicon layer).

[0039] According to an embodiment of the present invention, the thickness of the P-type nanocrystal doping layer 800 is 30-40 nm, for example, 30 nm, 35 nm, or 40 nm.

[0040] According to an embodiment of the present invention, the thickness of the first transparent conductive film layer 200 and the second transparent conductive film layer 1000 are independently selected from 70 to 100 nm, for example, 70 nm, 80 nm, 90 nm, and 100 nm.

[0041] According to an embodiment of the present invention, the material forming the first transparent conductive film layer 200 and the material forming the second transparent conductive film layer 1000 are independently selected from any one of ITO (indium doped tin oxide), IWO (indium doped tungsten oxide), ICO (indium doped cesium oxide), and AZO (zinc doped aluminum oxide).

[0042] According to an embodiment of the present invention, the first metal gate electrode 100 and the second metal gate electrode 1100 are independently selected from any one of a silver electrode, a silver-clad copper electrode, and an electroplated copper electrode.

[0043] The present invention also provides a method for preparing the aforementioned solar cell. Referring to FIG. 2 , the method comprises:

[0044] S100 , forming a first passivation layer 500 and a second passivation layer 700 on opposite sides of a single crystal silicon substrate 600 ;

[0045] According to some embodiments of the present invention, the method further includes the steps of cleaning and double-sided chemical polishing the single crystal silicon substrate 600 to remove oil stains and cutting damage layers on the surface of the single crystal silicon substrate 600 to form a clean pyramid light trapping structure.

[0046] According to an embodiment of the present invention, the formation methods of the first passivation layer 500 and the second passivation layer 700 are independently selected from any one of plasma enhanced chemical vapor deposition (PECVD), hot wire chemical vapor deposition (HWCVD), and chemical vapor deposition (CVD).

[0047] According to an embodiment of the present invention, when forming the first passivation layer 500 and the second passivation layer 700, the substrate temperature is 150-250°C (e.g., 150°C, 200°C, 250°C), and the process chamber pressure is 10-400Pa (e.g., 10Pa, 30Pa, 120Pa, 400Pa).

[0048] S200, forming an N-type nanocrystal doped layer 400 on a side of the first passivation layer 500 away from the single crystal silicon substrate 600;

[0049] According to an embodiment of the present invention, the N-type nanocrystal doping layer 400 is formed by independently selecting any one of plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition.

[0050] According to an embodiment of the present invention, when forming the N-type nanocrystal doped layer 400, the reaction gases include PH3 and silane, the doping concentration of PH3 is 2-10% (e.g., 2%, 5%, 10%), the substrate temperature is 150-250° C. (e.g., 150° C., 200° C., 250° C.), the process chamber pressure is 100-600 Pa (e.g., 100 Pa, 400 Pa, 600 Pa), and the power is 0.5-10 kW (e.g., 0.5 kW, 4 kW, 10 kW). It should be noted that the doping concentration of PH3 refers to the percentage of the flow rate of PH3 to the flow rate of silane.

[0051] S300, forming a P-type nanocrystal doped layer 800 on a side of the second passivation layer 700 away from the single crystal silicon substrate 600;

[0052] According to an embodiment of the present invention, the P-type nanocrystal doping layer 800 is formed by independently selecting any one of plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition.

[0053] According to an embodiment of the present invention, when forming the P-type nanocrystal doping layer 800, the reaction gases include B2H6 and silane, the doping concentration of B2H6 is 0.1-10% (e.g., 0.1%, 1%, 5%, 10%), the substrate temperature is 150-250°C (e.g., 150°C, 200°C, 250°C), the process chamber pressure is 100-600Pa (e.g., 100Pa, 400Pa, 600Pa), and the power is 0.5-10kW (e.g., 0.5kW, 6kW, 10kW). It should be noted that the doping concentration of B2H6 refers to the percentage of the flow rate of B2H6 to the flow rate of silane.

[0054] S400, forming an N-type interface layer 300 on a side of the N-type nanocrystal doped layer 400 away from the first passivation layer 500;

[0055] According to an embodiment of the present invention, the N-type interface layer 300 is formed by any one of plasma enhanced chemical vapor deposition (PECVD), hot filament chemical vapor deposition (HWCVD), and chemical vapor deposition (CVD).

[0056] According to an embodiment of the present invention, when forming the N-type interface layer 300, the reaction gases include PH3 and silane, and the doping concentration of the PH3 is 2-15% (e.g., 2%, 6%, 10%, 15%); the substrate temperature is 150-250°C (e.g., 150°C, 200°C, 250°C), the process chamber pressure is 30-600 Pa (e.g., 30 Pa, 80 Pa, 100 Pa, 300 Pa, 600 Pa), and the power is 0.2-10 kW (e.g., 0.2 kW, 0.4 kW, 1 kW, 5 kW, 10 kW). It should be noted that the doping concentration of the PH3 refers to the percentage of the flow rate of the PH3 to the flow rate of the silane.

[0057] S500, forming a P-type interface layer 900 on a side of the P-type nanocrystal doped layer 800 away from the second passivation layer 700, wherein at least one of the N-type interface layer 300 and the P-type interface layer 900 is an amorphous doped interface layer;

[0058] According to an embodiment of the present invention, the P-type interface layer 900 is formed by using any one of plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition.

[0059] According to an embodiment of the present invention, forming a P-type interface layer 900 includes: the reaction gases include B2H6 and silane, the doping concentration of the B2H6 is 2-15% (e.g., 2%, 10%, 15%), the substrate temperature is 150-250°C (e.g., 150°C, 200°C, 250°C), the process chamber pressure is 30-800 Pa (e.g., 30 Pa, 400 Pa, 800 Pa), and the power is 0.2-10 kW (e.g., 0.2 kW, 6 kW, 10 kW). It should be noted that the doping concentration of B2H6 refers to the percentage of the flow rate of B2H6 to the flow rate of silane.

[0060] S600 , forming a first transparent conductive film layer 200 on a side of the N-type interface layer 300 away from the N-type nanocrystal doped layer 400 ;

[0061] According to an embodiment of the present invention, the first transparent conductive film layer 200 is formed by physical vapor deposition (PVD) or chemical vapor deposition (CVD). Physical vapor deposition methods include vacuum evaporation, sputtering, pulsed laser, ion plating, etc.

[0062] S700 , forming a second transparent conductive film layer 1000 on a side of the P-type interface layer 900 away from the P-type nanocrystal doped layer 800 ;

[0063] According to an embodiment of the present invention, the second transparent conductive film layer 1000 is formed by physical vapor deposition or chemical vapor deposition. Physical vapor deposition includes vacuum evaporation, sputtering, pulse laser, ion plating, and the like.

[0064] S800 , forming a first metal gate electrode 100 on a side of the first transparent conductive film layer 200 away from the N-type interface layer 300 ;

[0065] According to an embodiment of the present invention, the first metal gate electrode 100 is formed by any one of screen printing, evaporation, magnetron sputtering, inkjet printing, electroplating, and laser transfer.

[0066] According to some embodiments of the present invention, the first metal gate line electrode 100 includes a main gate and a fine gate, the height of the fine gate is 5 to 50 μm (for example, 5 μm, 18 μm, 50 μm), and the width of the fine gate is 10 to 100 μm (for example, 10 μm, 48 μm, 100 μm), the height of the main gate is 5 to 50 μm (for example, 5 μm, 40 μm, 50 μm), and the width of the main gate is 50 to 150 μm (for example, 50 μm, 100 μm, 150 μm).

[0067] S900 , forming a second metal gate electrode 1100 on a side of the second transparent conductive film layer 1000 away from the P-type interface layer 900 .

[0068] According to an embodiment of the present invention, the second metal gate electrode 1100 is formed by any one of screen printing, evaporation, magnetron sputtering, inkjet printing, electroplating, and laser transfer.

[0069] According to some embodiments of the present invention, the second metal gate line electrode 1100 includes a main gate and a fine gate, the height of the fine gate is 5 to 50 μm (for example, 5 μm, 18 μm, 50 μm), and the width of the fine gate is 10 to 100 μm (for example, 10 μm, 48 μm, 100 μm), the height of the main gate is 5 to 50 μm (for example, 5 μm, 40 μm, 50 μm), and the width of the main gate is 50 to 150 μm (for example, 50 μm, 100 μm, 150 μm).

[0070] The present invention is described below with reference to specific examples. It should be noted that these examples are merely illustrative and do not limit the present invention in any way.

[0071] Example 1

[0072] The solar cell in Example 1 includes a stacked arrangement of: a first metal gate electrode 100, a first transparent conductive film layer 200, an N-type interface layer 300, an N-type nanocrystal doped layer 400, a first passivation layer 500, a single crystal silicon substrate 600, a second passivation layer 700, a P-type nanocrystal doped layer 800, a P-type interface layer 900, a second transparent conductive film layer 1000, and a second metal gate electrode 1100, wherein the N-type interface layer 300 is an amorphous doped interface layer, and the P-type interface layer 900 is a nanocrystal interface layer.

[0073] The method for preparing a solar cell comprises:

[0074] 1. Preparation of a single crystal silicon substrate 600: After pre-cleaning, the single crystal silicon wafer is chemically polished on both sides to remove oil stains and cutting damage layers on the surface of the silicon wafer, forming a clean pyramid light-trapping structure to obtain a single crystal silicon substrate 600. The thickness of the single crystal silicon substrate 600 is 150 μm.

[0075] 2. Preparation of a first passivation layer 500 and a second passivation layer 700: Plasma-enhanced chemical vapor deposition (PECVD) was used to deposit an intrinsic amorphous silicon layer and an intrinsic amorphous silicon layer on the front and back surfaces of a single-crystal silicon substrate 600, respectively. The first passivation layer 500 and the second passivation layer 700 were formed on the front and back surfaces of the single-crystal silicon substrate 600, respectively. The thickness of the first passivation layer 500 and the second passivation layer 700 was 10 nm. The substrate temperature was 200° C. and the process chamber pressure was 30-120 Pa.

[0076] 3. Preparation of N-type nanocrystal doping layer 400: Deposit N-type nanocrystal doping layer 400 on the first passivation layer 500 by PECVD. The N-type nanocrystal doping layer 400 is μc-SiO x : H(n) (N-type nanocrystalline silicon oxide layer), the thickness of the N-type nanocrystalline doped layer 400 is 25 nm, and when forming the N-type nanocrystalline doped layer 400, the reaction gases include PH3 and silane, and the doping concentration of PH3 is 5%; the substrate temperature is 200° C., the process chamber pressure is 400 Pa, and the power is 4 kW;

[0077] 4. Preparation of N-type interface layer 300: PECVD (chemical vapor deposition) was used to deposit N-type interface layer 300 on N-type nanocrystal doped layer 400. N-type interface layer 300 was a-Si:H(n+) (N-type amorphous silicon layer) with a thickness of 1 nm. During the formation of N-type interface layer 300, the reaction gases included PH3 and silane, with a PH3 doping concentration of 6%. The substrate temperature was 200° C., the process chamber pressure was 80 Pa, and the power was 0.4 kW.

[0078] 5. Preparation of a P-type nanocrystal doped layer 800: A P-type nanocrystal doped layer 800 was deposited on the second passivation layer 700 using PECVD (chemical vapor deposition). The P-type nanocrystal doped layer 800 was composed of μc-Si:H(p) (a P-type nanocrystal silicon layer) and had a thickness of 35 nm. During the formation of the P-type nanocrystal doped layer 800, the reaction gases included B2H6 and silane, with a B2H6 doping concentration of 1%. The substrate temperature was 200° C., the process chamber pressure was 400 Pa, and the power was 6 kW.

[0079] 6. Preparation of P-type interface layer 900: Using PECVD (chemical vapor deposition), a P-type interface layer 900 is deposited on the P-type nanocrystalline doped layer 800. The P-type interface layer 900 is μc-Si:H(p+) (P-type nanocrystalline silicon layer) and has a thickness of 1 nm. The formation of the P-type interface layer 900 includes: reactant gases including B2H6 and silane, with a B2H6 doping concentration of 10%; substrate temperature of 200° C., process chamber pressure of 400 Pa, and power of 6 kW;

[0080] 7. Preparation of a first transparent conductive film layer 200 and a second transparent conductive film layer 1000: Using a PVD method (physical vapor deposition), the first transparent conductive film layer 200 and the second transparent conductive film layer 1000 are deposited on the N-type interface layer 300 and the P-type interface layer 900, respectively. The thickness of the first transparent conductive film layer 200 and the second transparent conductive film layer 1000 is 80 nm.

[0081] 8. Preparation of the first metal grid line electrode 100 and the second metal grid line electrode 1100: The first metal grid line electrode 100 and the second metal grid line electrode 1100 are respectively prepared by screen printing on the first transparent conductive film layer 200 and the second transparent conductive film layer 1000. The first metal grid line electrode 100 and the second metal grid line electrode 1100 are made of silver paste material. The fine grid has a height of 18 μm and a width of 48 μm, and the main grid has a height of 40 μm and a width of 100 μm.

[0082] Example 2

[0083] The structure of the solar cell in Example 2 is similar to that of the cell in Example 1, except that the P-type interface layer 900 in Example 2 is an amorphous doped interface layer, and the N-type interface layer 300 in Example 2 is a nanocrystalline interface layer.

[0084] The method for preparing a solar cell is the same as that in Example 1, except that: the N-type interface layer 300 in the fourth step of Example 2 adopts the same process as that in the third step (nanocrystalline process), the doping concentration of PH3 is 10%, and the P-type interface layer 900 in the sixth step of Example 2 adopts a-Si:H(p+) (P-type amorphous silicon), the thickness of the P-type interface layer 900 is 1nm, the doping concentration of B2H6 is 10%, and the substrate temperature is 200°C; the process chamber pressure is 80Pa, and the power is 1kw.

[0085] Example 3

[0086] The structure of the solar cell in Example 3 is similar to that of the cell in Example 1, except that the N-type interface layer 300 in Example 3 is an amorphous doped interface layer, and the P-type interface layer 900 is an amorphous doped interface layer.

[0087] The method for preparing a solar cell is the same as that in Example 1, except that: in Step 6 of Example 3, the P-type interface layer 900 uses a-Si:H(p+) (P-type amorphous silicon), the thickness of the P-type interface layer 900 is 1 nm, the doping concentration of B2H6 is 10%, the substrate temperature is 200°C, the process chamber pressure is 80 Pa, and the power is 1 kW.

[0088] Comparative Example 1

[0089] The structure of the solar cell in Comparative Example 1 is similar to that of the cell in Example 1, except that: the N-type interface layer 300 and the P-type interface layer 900 in Comparative Example 1 are both nanocrystalline interface layers, and the doping concentration of the N-type interface layer 300 is greater than the doping concentration of the N-type nanocrystal doping layer 400 disposed adjacent thereto, and the doping concentration of the P-type interface layer 900 is greater than the doping concentration of the P-type nanocrystal doping layer 800 disposed adjacent thereto.

[0090] The method for preparing the solar cell is the same as that in Example 1, except that: in step 4 of Comparative Example 1, the same process (nanocrystalline process) as that in step 3 is adopted, and the doping concentration of PH3 is 10%.

[0091] Comparative Example 2

[0092] The structure of the solar cell in Comparative Example 2 is similar to that of the cell in Example 1, except that: the N-type interface layer 300 and the P-type interface layer 900 in Comparative Example 1 are both nanocrystalline interface layers, and the doping concentration of the N-type interface layer 300 is equal to the doping concentration of the N-type nanocrystal doping layer 400 disposed adjacent thereto, and the doping concentration of the P-type interface layer 900 is equal to the doping concentration of the P-type nanocrystal doping layer 800 disposed adjacent thereto.

[0093] The method for preparing a solar cell is the same as that in Example 1, except that: step 4 adopts the same process as step 3 (nanocrystal process), and the doping concentration of PH3 in the N-type interface layer 300 is the same as the doping concentration of PH3 in the N-type nanocrystal doping layer 400, which is 5%; step 6 adopts the same process as step 5 (nanocrystal process), and the doping concentration of B2H6 in the P-type interface layer 900 is the same as the doping concentration of B2H6 in the P-type nanocrystal doping layer 800, which is 1%.

[0094] A plurality of solar cells were manufactured according to the methods of Examples 1-3 and Comparative Examples 1-2. The electrical performance of the solar cells manufactured in Examples 1-3 and Comparative Examples 1-2 was tested using an IV tester. The test results are shown in Table 1 below.

[0095] Table 1

[0096] Among them, Eff refers to conversion efficiency, Max-Eff is the maximum conversion efficiency among multiple groups of batteries with the same structure, Voc refers to open circuit voltage, Isc refers to short circuit current, FF refers to fill factor, Rs refers to series resistance, Rsh refers to parallel resistance, and IRev2 refers to leakage current.

[0097] In Comparative Examples 1-2, the N-type interface layer 300 and the P-type interface layer 900 are both nanocrystalline interface layers. The doping concentration of the interface layer in Comparative Example 1 is greater than the doping concentration of the nanocrystalline doping layer adjacent thereto. As can be seen from Table 1, the performance of the battery in Comparative Example 1 is better than that of the battery in Comparative Example 2. Although further increasing the doping concentration of the nanocrystalline doping layer can reduce the series resistance (Rs) of the battery, increase the fill factor (FF), and slightly improve the efficiency, the extent of the increase in the fill factor (FF) and efficiency is small. In Examples 1-3, at least one of the N-type interface layer 300 and the P-type interface layer 900 is an amorphous doped interface layer. As shown in Table 1, the series resistance (Rs) of the battery of Example 1-3 is significantly lower than the series resistance (Rs) of the battery of Comparative Example 1-2, the fill factor (FF) of the battery of Example 1-3 is significantly greater than the fill factor (FF) of the battery of Comparative Example 1-2, and the efficiency (Eff) of the battery of Example 1-3 is significantly greater than the efficiency (Eff) of the battery of Comparative Example 1-2. Other electrical performance parameters of the battery of Example 1-3 are similar to those of the battery of Comparative Example 1-2. This demonstrates that when at least one of the N-type interface layer 300 and the P-type interface layer 900 is an amorphous doped interface layer, the series resistance (Rs) of the battery can be significantly reduced, the fill factor (FF) of the battery can be significantly improved, and ultimately the battery conversion efficiency (Eff) can be significantly improved, while ensuring product quality and other electrical performance parameters are not affected. Moreover, in Example 1 and Example 2, one of the N-type interface layer 300 and the P-type interface layer 900 is an amorphous doped interface layer and the other is a nanocrystalline interface layer. In Example 3, both the N-type interface layer 300 and the P-type interface layer 900 are amorphous doped interface layers. It can be seen from Table 1 that the filling factor and conversion efficiency of the battery in Example 3 are better than those of the batteries in Example 1 and Example 2, indicating that when both the N-type interface layer 300 and the P-type interface layer 900 are amorphous doped interface layers, the conversion efficiency (Eff) of the battery can be more effectively improved.

[0098] It should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the quantity of the technical features indicated. Terms such as "upper," "lower," "top," and "bottom" indicate positions or relationships based on those shown in the accompanying drawings and are intended solely to facilitate and simplify the description of the present invention. They do not indicate or imply that the devices or components indicated must have, be constructed, or operate in a specific orientation. Therefore, they should not be construed as limitations on the present invention.

[0099] In the description of this specification, the reference terms "one embodiment", "another embodiment", "some embodiments", "example", "specific example", or "some examples" mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.

[0100] Although the embodiments of the present invention have been shown and described above, it will be understood that the above embodiments are illustrative and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A solar cell, characterized in that: The solar cell comprises a stacked arrangement of: a first metal grid electrode, a first transparent conductive film layer, an N-type interface layer, an N-type nanocrystal doping layer, a first passivation layer, a single crystal silicon substrate, a second passivation layer, a P-type nanocrystal doping layer, a P-type interface layer, a second transparent conductive film layer, and a second metal grid electrode; At least one of the N-type interface layer and the P-type interface layer is an amorphous doped interface layer.

2. The solar cell according to claim 1, characterized in that: When one of the N-type interface layer and the P-type interface layer is an amorphous doped interface layer, the other is a nanocrystalline interface layer.

3. The solar cell according to claim 1 or 2, characterized in that: The doping concentration of the N-type interface layer is greater than the doping concentration of the N-type nanocrystal doping layer.

4. The solar cell according to any one of claims 1 to 3, characterized in that The doping concentration of the P-type interface layer is greater than the doping concentration of the P-type nanocrystal doping layer.

5. The solar cell according to any one of claims 1 to 4, characterized in that The thickness of the N-type interface layer is 1-2 nm, and the thickness of the P-type interface layer is 1-2 nm.

6. The solar cell according to any one of claims 1 to 5, characterized in that The solar cell meets at least one of the following conditions: The thickness of the single crystal silicon substrate is 50 to 300 μm; The single crystal silicon substrate is an N-type single crystal silicon wafer or a P-type single crystal silicon wafer; The thickness of the first passivation layer and the second passivation layer are independently selected from 5 to 10 nm; The first passivation layer and the second passivation layer are independently selected from any one of an intrinsic amorphous silicon layer, an intrinsic amorphous silicon oxygen layer, and an intrinsic amorphous silicon carbon layer; The N-type nanocrystal doped layer is an N-type nanocrystal silicon oxygen layer; The thickness of the N-type nanocrystal doping layer is 20 to 30 nm; The P-type nanocrystal doped layer is a P-type nanocrystal silicon layer; The thickness of the P-type nanocrystal doping layer is 30-40 nm; The thickness of the first transparent conductive film layer and the second transparent conductive film layer are independently selected from 70 to 100 nm; The material forming the first transparent conductive film layer and the material forming the second transparent conductive film layer are independently selected from any one of indium oxide doped with tin, indium oxide doped with tungsten, indium oxide doped with cesium, and zinc oxide doped with aluminum; The first metal grid line electrode and the second metal grid line electrode are independently selected from any one of a silver electrode, a silver-clad copper electrode, and an electroplated copper electrode.

7. A method for preparing the solar cell according to any one of claims 1 to 6, characterized in that: The method comprises: forming a first passivation layer and a second passivation layer on opposite sides of the single crystal silicon substrate; forming an N-type nanocrystal doping layer on a side of the first passivation layer away from the single crystal silicon substrate; forming a P-type nanocrystal doping layer on a side of the second passivation layer away from the single crystal silicon substrate; forming an N-type interface layer on a side of the N-type nanocrystal doped layer away from the first passivation layer; A P-type interface layer is formed on a side of the P-type nanocrystal doped layer away from the second passivation layer, and at least one of the N-type interface layer and the P-type interface layer is an amorphous doped interface layer; Forming a first transparent conductive film layer on a side of the N-type interface layer away from the N-type nanocrystal doped layer; forming a second transparent conductive film layer on a side of the P-type interface layer away from the P-type nanocrystal doped layer; forming a first metal gate electrode on a side of the first transparent conductive film layer away from the N-type interface layer; A second metal gate line electrode is formed on a side of the second transparent conductive film layer away from the P-type interface layer.

8. The method according to claim 7, characterized in that The N-type interface layer is formed by any one of plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition; When forming the N-type interface layer, the reaction gas includes PH3 and silane, the doping concentration of PH3 is 2-15%, the substrate temperature is 150-250° C., the process chamber pressure is 30-600 Pa, and the power is 0.2-10 kW.

9. The method according to claim 7 or 8, characterized in that: The P-type interface layer is formed by any one of plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition; The formation of the P-type interface layer includes: the reaction gas includes B2H6 and silane, the doping concentration of B2H6 is 2-15%, the substrate temperature is 150-250° C., the process chamber pressure is 30-800 Pa, and the power is 0.2-10 kW.

10. The method according to any one of claims 7 to 9, characterized in that: The method satisfies at least one of the following conditions: The first passivation layer, the second passivation layer, the N-type nanocrystal doped layer, and the P-type nanocrystal doped layer are formed independently by plasma enhanced chemical vapor deposition, hot wire chemical vapor deposition, and chemical vapor deposition. When forming the first passivation layer and forming the second passivation layer, the substrate temperature is 150-250° C. and the process chamber pressure is 10-400 Pa; When forming the N-type nanocrystal doping layer, the reaction gas includes PH3 and silane, the doping concentration of PH3 is 2-10%, the substrate temperature is 150-250° C., the process chamber pressure is 100-600 Pa, and the power is 0.5-10 kW; When forming the P-type nanocrystal doping layer, the reaction gas includes B2H6 and silane, the doping concentration of B2H6 is 0.1-10%, the substrate temperature is 150-250° C., the process chamber pressure is 100-600 Pa, and the power is 0.5-10 kW; The first transparent conductive film layer and the second transparent conductive film layer are formed by physical vapor deposition or chemical vapor deposition; The first metal gate line electrode and the second metal gate line electrode are formed by any one of screen printing, evaporation, magnetron sputtering, inkjet printing, electroplating, and laser transfer.

Citation Information

Patent Citations

  • Monocrystalline silicon-based heterojunction solar cell and preparation method thereof

    CN106206781A

  • Solar cell and preparation method thereof

    CN116469946A

  • High-efficiency heterojunction solar cell

    CN217387170U

  • High-efficiency heterojunction solar cell

    CN218788382U

  • Plasma treatment at a p-i junction for increasing open circuit voltage of a photovoltaic device

    US20110308583A1