Ultra-thin full-frame high-temperature-resistant semiconductor strain gauge and preparation method therefor

By adopting a full-frame closed hole structure and a sub-nanometer silicon crystal film in the pressure sensor, the problem of pressure leakage and insufficient temperature adaptability under high temperature and high pressure is solved, and stability and efficiency over a wide temperature range are achieved Measurement.

WO2024234979A1PCT designated stage expired Publication Date: 2024-11-21GUANGDONG RUNYU SENSOR CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/090285
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-04-28
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing pressure sensors are prone to pressure leakage problems under high temperature and high pressure conditions, and the traditional sputtering film structural process is complex and costly. Although glass micro-melting technology is easy to mass production, it is difficult to meet the application needs of a wide temperature range.

Method used

The semiconductor strain gauge adopts a fully framed closed hole structure, including a high-resistance silicon substrate layer, an oxide layer, a resistive grid and an aluminum presser foot, is wrapped with a silicon nitride insulating passivation film to form a stable structure, and two forms on the force varistor The silicon oxide layer is used to match stress, and a thin film of sub-nano-silicon crystal as a resistor to reduce the temperature coefficient and improve sensitivity.

Benefits of technology

The stability and low temperature drift characteristics in the range of -60℃~+180℃ are achieved, which enhances the high temperature resistance of the strain gauge, avoids cracks and stress uneven caused by structural expansion and contraction, and improves the temperature adaptability of the sensor and Finished product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024090285_21112024_PF_FP_ABST
    Figure CN2024090285_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of pressure sensors, and in particular to an ultra-thin full-frame high-temperature-resistant semiconductor strain gauge and a preparation method therefor. The strain gauge has a full-frame closed hole structure, the strain gauge having the full-frame closed hole structure comprises two resistive grids and three aluminum pressure pins, wherein the two resistive grids are formed by connecting four force-sensitive resistors in series, each of the force-sensitive resistors is composed of a sub-nanometer silicon crystal film grown on the surface of a silicon dioxide oxide layer by a low-pressure vapor deposition method, and the crystal nucleus size of the sub-nanometer silicon crystal film is between that of nanometer silicon and that of polysilicon. The strain gauge of the present invention has a wide application temperature range, for example, an operating temperature ranging from -60°C to +180°C, and the strain gauge has low temperature drift characteristics and high stability.
Need to check novelty before this filing date? Find Prior Art

Description

An ultra-thin full-frame high-temperature resistant semiconductor strain gauge and its preparation method Technical Field

[0001] The present invention belongs to the technical field of pressure sensors, and more specifically, relates to an ultra-thin full-frame, high-temperature-resistant semiconductor strain gauge and a preparation method thereof. Background Art

[0002] In the field of pressure sensors with a range of 3 MPa to 200 MPa, pressure sealing packaging structures face significant challenges. The commonly used rubber ring seal is no longer sufficient for applications under high temperature and high pressure, making it difficult to resolve pressure leakage issues. Currently, two structural types are used for large-range pressure sensors / transmitters both domestically and internationally: sputtered diaphragm and glass-fused strain gauge. The sputtered diaphragm structure is complex and requires high manufacturing processes, making it cost-effective. Glass-fused technology, on the other hand, is easier to mass-produce, offers the same reliability and stability, and is less expensive. Using glass-fused technology, two semiconductor strain gauges are sintered onto a 17-4 PH stainless steel pressure seat using glass adhesive to form a Wheatstone bridge. The pressure seat is then welded to the pressure port of the stainless steel housing using processes such as argon arc welding, electron beam welding, and high-energy laser beam welding. When pressure is applied to the elastic membrane area behind the pressure seat, the Wheatstone bridge formed by the two strain gauges generates an electrical signal linearly proportional to the stress. This signal is amplified by the transmitter circuit and then transmitted to the computer's central processing unit for processing. The actuator then directs various actions, achieving intelligent measurement and control.

[0003] In the early days of glass micro-melting sensor / transmitter production, all semiconductor strain gauges were imported. In 2015, a subsidiary of our company successfully developed a semiconductor strain gauge and applied for an invention patent, publication number CN105091730B, titled "A Novel Structure of a DSOI Strain Gauge." This semiconductor strain gauge, with independent intellectual property rights, has an annual production capacity of 10 million units and is already widely used in the production of various sensors and transmitters.

[0004] With the expansion of application fields, in response to market demand, the invention of new semiconductor strain gauges that are suitable for a wide application temperature range, such as an operating temperature of -60℃~+180℃, low temperature drift characteristics, and high stability has become an urgent problem that needs to be solved. Summary of the Invention

[0005] The present invention provides a novel semiconductor strain gauge suitable for a wide application temperature range, such as an operating temperature of -60°C to +180°C, and having low temperature drift characteristics and high stability.

[0006] The purpose of the present invention is to provide an ultra-thin full-frame high-temperature resistant semiconductor strain gauge.

[0007] Another object of the present invention is to provide a preparation method for an ultra-thin full-frame high-temperature-resistant semiconductor strain gauge.

[0008] The above object of the present invention is achieved by the following technical solutions:

[0009] An ultra-thin full-frame high-temperature-resistant semiconductor strain gauge, the strain gauge adopts a full-frame closed-hole structure; the strain gauge with the full-frame closed-hole structure includes a high-resistance silicon substrate layer, a silicon dioxide oxide layer, two resistor grids, three aluminum pressure feet, and a silicon nitride insulating and passivating film;

[0010] Among them, the two resistor grids are connected to each other to form a half-bridge Wheatstone measurement circuit, and each resistor grid is composed of four piezoresistors connected in series in a "bow" shape. Each horizontally arranged piezoresistor is connected in series through a heavily doped boron shorting bar. One end of the two resistor grids is commonly connected to an aluminum pressure foot. There is a hole area between the three aluminum pressure feet. The three aluminum pressure feet are arranged around the hole area in a "pin" shape. Finally, the surface and side of the strain gauge are wrapped by a silicon nitride insulating and passivating layer to form a full-frame closed-hole structure; among them, a layer of silicon dioxide oxide layer is formed on both the upper surface and the lower surface of the high-resistance silicon substrate layer.

[0011] Furthermore, the thickness of the silicon dioxide oxide layer on the upper surface of the high-resistance silicon substrate layer is the same as that of the silicon dioxide oxide layer on the lower surface.

[0012] For the above technical solutions, for a semiconductor strain gauge with a relatively thin thickness, due to the poor toughness of its own silicon material, it is prone to fracture under stress. By adopting a full-frame closed structure for the entire strain gauge, each structure of the strain gauge is connected and supported with each other, so as to achieve the stability of the strain gauge structure. However, after connecting each structure of the strain gauge, there are differences in stress between different components. Therefore, by arranging the three aluminum pressure feet in a "pin" shape and forming a hole area in the middle of the strain gauge, in this way, it can effectively ensure that at the plane center position of the entire strain gauge, a uniform and stable stress difference between each component can be relieved, playing a good role in stress dispersion. In particular, it can prevent the strain gauge with a full-frame closed structure from being affected by high temperature or low temperature, causing cracks at the joints of different components of the strain gauge due to inconsistent expansion and contraction of different component structures, and at the same time, it can prevent cracks from occurring in the strain gauge itself under stress.

[0013] Secondly, by forming a silicon dioxide oxide layer on both the upper and lower surfaces of the high-resistance silicon substrate layer, stress matching can be achieved in the structure, so that the strain gauge can maintain stress balance in a free state, the structure of the strain gauge is stable, and the resistance value of the resistor is stable; and the thickness of this silicon dioxide oxide layer is controlled to remain consistent, which can ensure the flatness of the strain gauge, thereby overcoming the unevenness of the strain gauge caused by the mismatch between the thermal expansion coefficient of the oxide layer and the silicon single crystal.

[0014] Furthermore, the front and side surfaces of the force-sensitive resistor strip are covered with a silicon nitride insulating passivation film.

[0015] The above technical solution separates the force-sensitive resistor from the external environment by covering the surface and sides of the force-sensitive resistor with an insulating passivation film, thereby effectively protecting the force-sensitive resistor and reducing the influence of external water vapor, impurities or mobile ions on the force-sensitive resistor, while also increasing the temperature range of the strain gauge.

[0016] Furthermore, the inner lead of the strain gauge is formed by covering the surface of a boron-doped sub-nanometer silicon crystal film with an aluminum lead.

[0017] Furthermore, the connections between the force-sensitive resistor strips are connected via concentrated boron short-circuit strips.

[0018] The above technical solution can reduce the negative piezoresistive effect by doping concentrated boron between each bend connecting the force-sensitive resistor.

[0019] Furthermore, the thickness of the strain gauge is 9-12 um.

[0020] Furthermore, the force-sensitive resistor is composed of a sub-nanometer silicon crystal film, and the size of the crystal core of the sub-nanometer silicon crystal film is between nano-silicon and polycrystalline silicon.

[0021] This technical solution uses sub-nanometer silicon crystal thin films as the strain gauge's resistor, eliminating the PN junction structure of traditional diffused silicon semiconductor strain gauges. This eliminates the formation of a potential barrier region when operating at high temperatures. This results in a stable impedance and a low temperature coefficient, enabling the gauge to operate at high temperatures. Furthermore, sub-nanometer silicon crystal thin films can improve the strain gauge's sensitivity.

[0022] Furthermore, the sub-nanometer silicon crystalline film is grown on the surface of the silicon dioxide oxide layer by low-pressure vapor deposition.

[0023] The above technical solution can make the grains of the obtained sub-nanometer silicon crystals more uniform and also grow thinner sub-nanometer silicon crystal films by adopting the low-pressure vapor deposition method to prepare the sub-nanometer silicon crystal films.

[0024] Furthermore, a silicon dioxide oxide layer is formed on the upper layer of the force-sensitive resistor strip.

[0025] The above technical solution can protect the strain gauge resistance structure from contamination by forming a low-stress silicon dioxide oxide layer on the upper layer of the force-sensitive resistor.

[0026] A method for preparing an ultra-thin, full-frame, high-temperature-resistant semiconductor strain gauge comprises the following steps:

[0027] (1) Take a high-resistance silicon wafer with a thickness of 400-600 μm as a sacrificial layer, then oxidize the surface of the high-resistance silicon wafer, bond another high-resistance silicon wafer on top of the high-resistance silicon wafer, and then use a thinning machine to thin the high-resistance silicon wafer on top to form a high-resistance silicon substrate layer;

[0028] (2) A silicon dioxide oxide layer is grown on the surface of the high-resistance silicon substrate layer, and a sub-nanometer silicon crystal film is grown by low-pressure vapor deposition; then the concentrated boron area is photolithographically processed, ion implanted with a resist, annealed and redistributed after the concentrated boron ion implantation, and then the resistance area is photolithographically processed, ion implanted with a resist, and annealed and redistributed after the dilute boron ion implantation;

[0029] (3) Photolithography of lead holes, aluminum vaporization, reverse etching, alloying, and then photolithography of the hole area, dry etching with glue, ICP etching of the deep area 10um to self-termination, then removing the surface photoresist, depositing the insulating passivation layer, and then photolithography of the aluminum pressure foot, removing the surface photoresist, protecting the front side of the wafer, and etching to remove the sacrificial layer on the back to form a 9-12um thick semiconductor strain gauge.

[0030] Beneficial effects:

[0031] (1) This technical solution is suitable for semiconductor strain gauges with relatively thin thickness. Since the toughness of its silicon material is poor, it is easy to break under stress. By adopting a full-frame closed structure for the entire strain gauge, each structure of the strain gauge is connected and supported to each other, the stability of the strain gauge structure can be achieved. However, after each structure of the strain gauge is connected to each other, there are differences in stress between different components. Therefore, three aluminum pressure feet are distributed in a herringbone shape in the middle of the strain gauge to form a hole area. In this way, it can effectively ensure that a uniform and stable stress difference between each component is formed at the center of the plane of the entire strain gauge, which can play a good stress dispersion role. In particular, it can prevent the strain gauge with a full-frame closed structure from being affected by high or low temperature, causing the expansion and contraction of different component structures to be inconsistent, resulting in cracks at the connection between different components of the strain gauge. At the same time, it can prevent the strain gauge with a full-frame closed structure from cracking under the stress of itself.

[0032] Secondly, by forming a silicon dioxide oxide layer on both the upper and lower surfaces of the high-resistance silicon substrate layer, stress matching can be achieved in the structure, so that the strain gauge can maintain stress balance in a free state, the structure of the strain gauge is stable, and the resistance value of the resistor is stable; and the thickness of this silicon dioxide oxide layer is controlled to remain consistent, which can ensure the flatness of the strain gauge, thereby overcoming the unevenness of the strain gauge caused by the mismatch between the thermal expansion coefficient of the oxide layer and the silicon single crystal.

[0033] (2) This technical solution separates the force-sensitive resistor from the external environment by covering the surface and sides of the force-sensitive resistor with an insulating passivation film, effectively protecting the force-sensitive resistor while reducing the influence of external water vapor, impurities or mobile ions on the force-sensitive resistor, and at the same time increasing the temperature range of the strain gauge.

[0034] (3) This technical solution can reduce the negative piezoresistive effect by doping concentrated boron between each bend connecting the force-sensitive resistor.

[0035] (4) This technical solution uses sub-nanometer silicon crystal thin films as the resistor of the strain gauge, eliminating the PN junction structure of the traditional diffused silicon semiconductor strain gauge. This prevents the strain gauge from forming a potential barrier region when operating at high temperatures. The strain gauge has a stable impedance and a low temperature coefficient, enabling the strain gauge to meet the requirements of high-temperature use. Secondly, the sub-nanometer silicon crystal thin film can also improve the sensitivity of the strain gauge.

[0036] (5) This technical solution uses a low-pressure vapor deposition method to prepare a sub-nanometer silicon crystal film, which can make the grains of the obtained sub-nanometer silicon crystals more uniform and can also grow a thinner sub-nanometer silicon crystal film.

[0037] (6) This technical solution can protect the strain gauge resistance structure from contamination by forming a low-stress silicon dioxide oxide layer on the upper layer of the force-sensitive resistor. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] FIG1 is a top view of a strain gauge according to the present invention.

[0039] FIG2 is a cross-sectional view of the strain gauge of the present invention.

[0040] 1-force sensitive resistor, 2-boron-doped short-circuit bar, 3-aluminum pressure foot, 4-silicon nitride insulating passivation layer, 5-hole area, 6-high-resistance silicon substrate layer, 7-silicon dioxide oxide layer, 8-silicon dioxide oxide layer, 9-silicon dioxide oxide layer. DETAILED DESCRIPTION

[0041] The present invention is further described below with reference to specific examples, which, however, are not intended to limit the present invention in any way. Unless otherwise specified, the reagents, methods, and equipment used in the present invention are conventional reagents, methods, and equipment in the art.

[0042] Unless otherwise specified, the reagents and materials used in the following examples are all commercially available.

[0043] Please refer to Figure 1: The strain gauge with a full-frame enclosed hole structure includes two resistance grids and three aluminum pressure feet; among them, the two resistance grids are connected to form a half-bridge Wheatstone measurement circuit, and each resistance grid is composed of four force-sensitive resistors 1 in a "bow" shape in series. Each horizontally arranged force-sensitive resistor is connected in series by a heavily doped boron shorting bar 2. One end of the two resistance grids is commonly connected to an aluminum pressure foot 3. There is a hole area 5 between the three aluminum pressure feet 3. The three aluminum pressure feet 3 surround the hole area 5 in a "pin" shape. Finally, the surface and side of the strain gauge are wrapped by a silicon nitride insulating passivation layer 4 to form a closed structure.

[0044] Example 1

[0045] Please refer to Figures 1 - 2:

[0046] Take a high-resistance silicon wafer with a thickness of 400 um as the sacrificial layer. Then, oxidize the surface of the high-resistance silicon wafer to obtain a silicon dioxide oxide layer 9 with a thickness of 100 nm, and bond another high-resistance silicon wafer on the silicon dioxide oxide layer 9. Then, use a thinning machine to thin the upper high-resistance silicon wafer to 9 um to form a high-resistance silicon substrate layer 6;

[0047] Grow a silicon dioxide oxide layer 8 with a thickness of 100 nm on the surface of the high-resistance silicon substrate layer 6, and use low-pressure chemical vapor deposition method to grow a sub-nanometer silicon crystal thin film force-sensitive resistor 1 with a thickness of 600 nm on the silicon dioxide oxide layer 8 at 620 °C, so that each resistance grid is composed of four force-sensitive resistors 1 in a "bow" shape in series; then photolithograph the heavily doped boron shorting bar 2, and connect each horizontally arranged force-sensitive resistor 1 in series by doping with 1×10 16 cm -3 heavily doped boron shorting bar 2. After the ion implantation of heavily doped boron, perform rapid annealing for 12 min at a temperature of 900 °C and redistribution through an RTP-200 type rapid annealing furnace, then coat the photoresist area by photolithography to obtain a resistance pattern, and then send it with glue for 3×10 15 cm -3 light boron ion implantation. After the light boron ion implantation, anneal at 1000 °C for 30 min and perform redistribution to eliminate lattice defects; among them, the crystal nucleus size of the sub-nanometer silicon crystal thin film is between that of nanometer silicon and polycrystalline silicon;

[0048] Finally, photolithograph the lead holes, evaporate aluminum with a thickness of 1.3 um, perform reverse etching, alloy the internal leads, then photolithograph the hole area 5, perform dry etching with glue, terminate the deep etching area to 10 um through ICP etching to obtain a hole structure, then clean to remove the photoresist on the surface, deposit a silicon nitride insulating passivation layer 4, and wrap and connect the strain gauge components through the silicon nitride insulating passivation layer 4 to form a full-frame closed structure. Then, apply glue according to the graphic structure where three aluminum pressure feet 3 surround the hole area 5 in a "pin" shape, then photolithograph the three aluminum pressure feet 3, remove the photoresist on the surface, protect the front side of the wafer, and then etch away the back sacrificial layer to form a semiconductor strain gauge with a 10 um thick full-frame closed hole structure;

[0049] During the above manufacturing process, the glue coating thickness is controlled at 1.5 um, and the silicon dioxide oxide layer thickness is controlled at 100 nm.

[0050] Example 2

[0051] Please refer to Figures 1 - 2:

[0052] Take a 500 um thick high-resistance silicon wafer as the sacrificial layer, then oxidize the surface of the high-resistance silicon wafer to obtain a 600 nm thick silicon dioxide oxide layer 9, combine another high-resistance silicon wafer on the silicon dioxide oxide layer 9, and then use a thinning machine to thin the upper high-resistance silicon wafer to 10 um to form a high-resistance silicon substrate layer 6;

[0053] Grow a 600 nm thick silicon dioxide oxide layer 8 on the surface of the high-resistance silicon substrate layer 6, and grow a 100 nm thick sub-nanometer silicon crystal thin film force-sensitive resistor 1 on the silicon dioxide oxide layer 8 by low-pressure chemical vapor deposition at 620 °C, and let each resistor grid be composed of four force-sensitive resistors 1 in a "bow" shape in series; then photolithograph the thick boron shorting bar 2, and connect each horizontally arranged force-sensitive resistor 1 through doping with 1×10 [[ID=1】] 16 cm -3 thick boron shorting bars 2 in series, send it with glue for ion implantation, after the thick boron ion implantation, perform rapid annealing for 15 min and redistribution at a temperature of 1000 °C through an RTP-200 type rapid annealing furnace, then apply glue and photolithograph the resistor area to obtain a resistor pattern, and then send it with glue for 3×10 15 cm -3 light boron ion implantation, after the light boron ion implantation, anneal for 35 min and redistribute at 1100 °C to eliminate lattice defects; where the crystal nucleus size of the sub-nanometer silicon crystal thin film is between that of nanometer silicon and polycrystalline silicon;

[0054] Finally, the lithography lead holes are made, the aluminum evaporation thickness is 1.2 um, the reverse etching is carried out, the internal lead alloying is performed, and then the hole area 5 is lithographed. The dry etching with glue is carried out, and the deep etching area is etched deeply to 12 um by ICP etching and then terminated to obtain a hole structure. Then, the surface photoresist is removed by cleaning, and the silicon nitride insulating passivation layer 4 is deposited. The silicon nitride insulating passivation layer 4 is used to wrap and connect between the strain gauge components to form a full-frame closed structure. Then, according to the graphic structure that three aluminum pressure feet 3 are arranged around the hole area 5 in a "pin" shape, glue is applied, and then the three aluminum pressure feet 3 are lithographed, and the surface photoresist is removed. The front side of the wafer is protected, and then the backside sacrificial layer is removed by etching to form a semiconductor strain gauge with a full-frame closed hole structure with a thickness of 12 um;

[0055] During the above manufacturing process, the glue coating thickness is controlled at 1.0 um, and the silicon dioxide oxide layer thickness is controlled at 600 nm. <000013​​​​​​​​​​​​​​​​​​​​Finally, lithograph the lead holes, evaporate aluminum with a thickness of 1.5 um, perform reverse lithography, and alloy the internal leads. Then, lithograph the hole area 5, perform dry etching with glue, terminate the deep etching area to 12 um through ICP etching to obtain a hole structure. Then, clean to remove the photoresist on the surface, deposit a silicon nitride insulating and passivating layer 4, and wrap and connect the strain gauge components through the silicon nitride insulating and passivating layer 4 to form a full-frame closed structure. Then, apply glue according to the graphic structure where three aluminum pressure feet 3 surround the hole area 5 in a "pin" shape, and then lithograph the three aluminum pressure feet 3, remove the photoresist on the surface, protect the front side of the wafer, and then etch away the back sacrificial layer to form a semiconductor strain gauge with a full-frame closed hole structure with a thickness of 12 um;

[0061] During the above manufacturing process, the glue coating thickness is controlled at 1.9 um, and the silicon dioxide oxide layer thickness is controlled at 600 nm.

[0062] Example 4

[0063] Please refer to Figures 1 - 2:

[0064] Compared with Example 1, the difference in this example is that the order of the high boron ion implantation and the light boron ion implantation is reversed. First, the light boron is doped and then the high boron is doped, and the other conditions remain unchanged. [[ID=1 / 4]]

[0065] Comparative Example 1

[0066] Please refer to Figures 1 - 2:

[0067] Compared with Example 1, the difference in this comparative example is that the hole area is not lithographed, and the other conditions remain unchanged.

[0068] Comparative Example 2

[0069] Please refer to Figures 1 - 2:

[0070] Compared with Example 1, the difference in this comparative example is that the thickness of the upper silicon dioxide oxide layer 8 and the lower silicon dioxide oxide layer 9 of the high-resistance silicon substrate layer is different, and the other conditions remain unchanged.

[0071] Comparative Example 3

[0072] Please refer to Figures 1 - 2:

[0073] Compared with Example 1, the difference in this comparative example is that:

[0074] Take a high-resistance silicon wafer with a thickness of 400 um as the sacrificial layer. Then, oxidize the surface of the high-resistance silicon wafer to obtain a silicon dioxide oxide layer 9 with a thickness of 100 nm, combine another high-resistance silicon wafer on the silicon dioxide oxide layer 9, and then use a thinning machine to thin the upper high-resistance silicon wafer to 9 um to form a high-resistance silicon substrate layer 6;

[0075] Grow a 100-nm-thick silicon dioxide oxidation layer 8 on the surface of the high-resistance silicon substrate layer 6, and grow a sub-nanometer silicon crystal thin film force-sensitive resistor 1 with a thickness of 600 nm on the silicon dioxide oxidation layer 8 by low-pressure chemical vapor deposition at 620 °C. Let each resistor grid be composed of four force-sensitive resistors 1 connected in series in a "bow" shape; then photolithograph the thick boron shorting bar 2, and connect the force-sensitive resistors arranged horizontally in series through the doped 1×10 16 cm -3 Thick boron shorting bar 2. After the glue is applied and ion implantation is carried out, after the thick boron ion implantation, rapid annealing for 12 minutes and redistribution are carried out in a RTP-200 type rapid annealing furnace at a temperature of 900 °C, and then the glue is applied and the resistor area is photolithographed to obtain a resistor pattern. Then, the glue is applied and 3×10 15 cm -3 of light boron ion implantation. After the light boron ion implantation, annealing for 30 minutes and redistribution are carried out at 1000 °C to eliminate lattice defects; the crystal nucleus size of the sub-nanometer silicon crystal thin film is between that of nanometer silicon and polycrystalline silicon;

[0076] Finally, photolithograph the lead holes, evaporate aluminum with a thickness of 1.3 um, reverse etch, alloy the internal leads, and then photolithograph the hole area 5. Apply glue and perform dry etching. Stop etching deeply to 10 um through ICP etching to obtain a hole structure. Then clean the surface photoresist, deposit a silicon nitride insulating passivation layer 4, and make the silicon nitride insulating passivation layer 4 form a fault between the two aluminum pressure feet 3 in a horizontal "Lü" shape below. Do not perform a full-frame closed connection. Apply glue according to the graphic structure where three aluminum pressure feet 3 surround the hole area 5 in a "pin" shape, and then photolithograph the three aluminum pressure feet 3, remove the surface photoresist, protect the front of the wafer, and then etch away the back sacrificial layer to form a semiconductor strain gauge with a thickness of 10 um;

[0077] During the above manufacturing process, the glue coating thickness is controlled at 1.5 um, and the silicon dioxide oxidation layer thickness is controlled at 100 nm.

[0078] The strain gauges obtained in Examples 1-4 and Comparative Examples 1-3 are made into glass micro-melt pressure sensors for performance testing. The specific testing methods and test results are as follows:

[0079] Zero-point temperature coefficient: Measure the output voltage of the sensor under the condition of 0 pressure at 25 °C, 100 °C, 160 °C, 170 °C, 190 °C, 180 °C, 190 °C, and 200 °C respectively, and calculate the zero-point temperature coefficient of the sensor;

[0080] Sensitivity temperature coefficient: Measure the output voltage of the sensor under the conditions of 0 pressure and full pressure at 25 °C, 10 °C, 160 °C, 170 °C, 190 °C, 180 °C, 190 °C, and 200 °C respectively, and calculate the sensitivity temperature coefficient of the sensor;

[0081] The specific test results are shown in Table 1;

[0082] Table 1: Product performance test results

[0083]

[0084] The test results in Table 1 show that the ultra-thin, full-frame, high-temperature-resistant semiconductor strain gauge obtained by the present invention is only approximately 10 μm thick. To ensure the strain gauge's flatness, the oxide layer grown on both sides of the strain gauge maintains a consistent thickness. This overcomes the unevenness of the strain gauge caused by the mismatch between the thermal expansion coefficients of the oxide layer and the silicon single crystal. Because the strain gauge utilizes a full-frame structure and a stress-distributing design, the strain gauge is subjected to balanced stress and structurally stable. The resulting product yield after etching and separation is high, exceeding 90%. The polysilicon resistor strips in the strain gauge are isolated by silicon dioxide at the bottom and feature an insulating passivation layer on the top and sides, effectively addressing the high-temperature leakage current issues associated with conventional PN junction structures. The strain gauge can operate normally at 180°C and exhibits excellent stability in high-temperature environments. Actual tests have shown that the uncompensated zero-point temperature coefficient and sensitivity temperature coefficient of this strain gauge, manufactured using a micro-melting process, can reach -0.023% / °C at 180°C.

[0085] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. An ultra-thin full-frame high-temperature resistant semiconductor strain gauge, characterized in that: The strain gauge adopts a full-frame closed-hole structure; the strain gauge with the full-frame closed-hole structure includes a high-resistance silicon substrate layer, a silicon dioxide oxide layer, two resistor grids, three aluminum pressure feet, and a silicon nitride insulation passivation film; Among them, the two resistor grids are connected to form a half-bridge Wheatstone measurement circuit, and each resistor grid is composed of four force-sensitive resistors connected in series in a "bow" shape. Each horizontally arranged force-sensitive resistor is connected in series through a heavily doped boron shorting bar. One end of the two resistor grids is commonly connected to an aluminum pressure foot. There is a hole area between the three aluminum pressure feet. The three aluminum pressure feet surround the hole area in a "pin" shape. Finally, the surface and side of the strain gauge are wrapped by a silicon nitride insulation passivation layer to form a full-frame closed-hole structure; among them, a layer of silicon dioxide oxide layer is formed on both the upper surface and the lower surface of the high-resistance silicon substrate layer.

2. The ultra-thin full-frame high-temperature resistant semiconductor strain gauge according to claim 1, characterized in that: The thickness of the silicon dioxide oxide layer on the upper surface of the high-resistance silicon substrate layer is the same as that on the lower surface.

3. The ultra-thin full-frame high-temperature resistant semiconductor strain gauge according to claim 1, characterized in that: The front and side surfaces of the force-sensitive resistor bars are covered with a silicon nitride insulation passivation film.

4. The ultra-thin full-frame high-temperature resistant semiconductor strain gauge according to claim 1, characterized in that: The internal lead of the strain gauge is composed of an aluminum lead covered on the surface of a heavily doped boron sub-nanometer silicon crystal thin film.

5. The ultra-thin full-frame high-temperature resistant semiconductor strain gauge according to claim 1, characterized in that: The connections between the force-sensitive resistor bars are all connected through a heavily doped boron shorting bar.

6. The ultra-thin full-frame high-temperature resistant semiconductor strain gauge according to claim 1, characterized in that: The thickness of the strain gauge is 9 - 12 um.

7. The ultra-thin full-frame high-temperature resistant semiconductor strain gauge according to claim 1, characterized in that: The force-sensitive resistor is composed of a sub-nanometer silicon crystal thin film, and the crystal nucleus size of the sub-nanometer silicon crystal thin film is between that of nanometer silicon and polycrystalline silicon.

8. The ultra-thin full-frame high temperature resistant semiconductor strain gauge according to claim 7, characterized in that: The sub-nanometer silicon crystal thin film is grown above the surface of the silicon dioxide oxide layer by low-pressure chemical vapor deposition.

9. The ultra-thin full-frame high temperature resistant semiconductor strain gauge according to claim 1, characterized in that: A layer of silicon dioxide oxide layer is formed on the upper layer of the force-sensitive resistor bar.

10. A method for preparing an ultra-thin full-frame high-temperature resistant semiconductor strain gauge, characterized in that: Specifically, it includes the following steps: (1) Take a high-resistance silicon wafer with a thickness of 400 - 600 um as a sacrificial layer, then oxidize the surface of the high-resistance silicon wafer, bond another high-resistance silicon wafer on the high-resistance silicon wafer, and then use a thinning machine to thin the upper high-resistance silicon wafer to form a high-resistance silicon substrate layer; (2) Grow a layer of silicon dioxide oxide layer on the surface of the high-resistance silicon substrate layer, and grow a sub-nanometer silicon crystal thin film by low-pressure chemical vapor deposition; then photolithograph the heavily doped boron area, send it with glue for ion implantation. After the heavily doped boron ion implantation, anneal and redistribute. Then photolithograph the resistor area, send it with glue for ion implantation. After the lightly doped boron ion implantation, anneal and redistribute; (3) Photolithograph the lead holes, evaporate aluminum, reverse etch, alloy, then photolithograph the hole area, send it with glue for dry etching, use ICP etching to deeply etch the area by 10 um until self-termination, then remove the surface photoresist, deposit the insulation passivation layer, then photolithograph the aluminum pressure feet, remove the surface photoresist, protect the front of the wafer, and etch away the back sacrificial layer to form a semiconductor strain gauge with a thickness of 9 - 12 um.

Citation Information

Patent Citations

  • DSOI (Double Silicon Oxide Insulation) strain gage and manufacturing method thereof

    CN105091730A

  • Single crystal doped film, piezoelectric film for acoustic resonator and preparation method of piezoelectric film

    CN113285014A

  • Ultra-thin full-frame high-temperature-resistant semiconductor strain gauge and preparation method thereof

    CN116242246A

  • Pressure sensor based on graphene piezoresistive effect

    CN210464750U