Semiconductor device, storage device, and method for manufacturing semiconductor device
The semiconductor device employs a cylindrical oxide semiconductor layer structure with a gate-all-around configuration to enhance on-state current and integration density, address parasitic capacitance, and ensure low power consumption and reliability, overcoming existing challenges in oxide transistor performance.
Patent Information
- Application Number
- PCT/IB2024/054223
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-05-02
- Publication Date
- 2024-11-21
AI Technical Summary
Current semiconductor devices face challenges in achieving high on-state current, low parasitic capacitance, miniaturization, high integration, high definition displays, low power consumption, and high-speed operation, particularly in transistors using oxide semiconductors, where electrical characteristics and reliability are compromised by impurities and oxygen vacancies.
A semiconductor device with a cylindrical oxide semiconductor layer structure, featuring a gate-all-around configuration, where the semiconductor layer is sandwiched by oxide semiconductor layers with reduced impurity and oxygen vacancy concentrations, and surrounded by insulating layers to minimize parasitic capacitance and enhance electrical performance.
The solution enables transistors with improved on-state current, reduced parasitic capacitance, and increased integration density, while maintaining low power consumption and high reliability by optimizing the oxide semiconductor layer structure and insulating layers to suppress impurities and oxygen vacancies.
Smart Images

Figure IB2024054223_21112024_PF_FP_ABST
Abstract
Description
Semiconductor device, memory device, and method for manufacturing semiconductor device
[0001] 1. Field of the Invention One embodiment of the present invention relates to a semiconductor device, a memory device, a display device, and an electronic device. Another embodiment of the present invention relates to a manufacturing method of a semiconductor device.
[0002] One embodiment of the present invention is not limited to the above technical field, and examples of the technical field of one embodiment of the present invention include semiconductor devices, display devices, light-emitting devices, power storage devices, memory devices, electronic devices, lighting devices, input devices (e.g., touch sensors), input / output devices (e.g., touch panels), driving methods thereof, and manufacturing methods thereof.
[0003] In this specification and the like, a semiconductor device is a device that utilizes semiconductor characteristics, and refers to a semiconductor element (transistor, diode, photodiode, etc.), a circuit including a semiconductor element, a device having a circuit including a semiconductor element, etc. Also, it refers to any device that can function by utilizing semiconductor characteristics. For example, an integrated circuit, a chip including an integrated circuit, and an electronic component in which a chip is housed in a package are examples of semiconductor devices. Furthermore, a memory device, a display device, a light-emitting device, a lighting device, and an electronic device may themselves be semiconductor devices and each may have a semiconductor device.
[0004] In recent years, the development of semiconductor devices has progressed, and semiconductor devices mainly use LSIs (Large Scale Integration), CPUs (Central Processing Units), memories, etc. A CPU is an aggregate of semiconductor elements that have semiconductor integrated circuits (including at least transistors) formed into chips by processing a semiconductor wafer and on which electrodes serving as connection terminals are formed.
[0005] 2. Description of the Related Art Semiconductor circuits (IC chips) such as LSIs, CPUs, and memories are mounted on circuit boards, such as printed wiring boards, and are used as components of various electronic devices.
[0006] Furthermore, a technology for constructing a transistor using a semiconductor thin film formed on a substrate having an insulating surface has attracted attention. Such transistors are widely applied to electronic devices such as integrated circuits (ICs) and display devices. While silicon-based semiconductor materials are widely known as semiconductor thin films applicable to transistors, oxide semiconductors have also attracted attention as other materials.
[0007] Furthermore, it is known that a transistor using an oxide semiconductor has an extremely small leakage current in an off state. For example, Patent Document 1 discloses a CPU with low power consumption that utilizes the property of a transistor using an oxide semiconductor having a small leakage current. Furthermore, Patent Document 2 discloses a memory device that can retain stored data for a long period of time by utilizing the property of a transistor using an oxide semiconductor having a small leakage current.
[0008] In addition, with the recent trend toward smaller and lighter electronic devices, there is an increasing demand for higher density integrated circuits. There is also a demand for improved productivity of semiconductor devices including integrated circuits. For example, Patent Document 3 and Non-Patent Document 1 disclose a technique for increasing the density of integrated circuits by stacking a first transistor using an oxide semiconductor film and a second transistor using an oxide semiconductor film to provide multiple memory cells in an overlapping manner. Patent Document 4 discloses a technique for increasing the density of integrated circuits by vertically arranging the channel of a transistor using an oxide semiconductor film.
[0009] JP 2012-257187 A JP 2011-151383 A WO 2021 / 053473 JP 2013-211537 A
[0010] M. Oota et al. , “3D-Stacked CAAC-In-Ga-Zn Oxide FETs with Gate Length of 72nm”, IEDM Tech. Dig. , 2019, pp. 50-53
[0011] An object of one embodiment of the present invention is to provide a transistor with favorable electrical characteristics.An object of one embodiment of the present invention is to provide a transistor with high on-state current.An object of one embodiment of the present invention is to provide a transistor with low parasitic capacitance.An object of one embodiment of the present invention is to provide a transistor, a semiconductor device, or a memory device that can be miniaturized or highly integrated.An object of one embodiment of the present invention is to provide a display device with high definition or a high aperture ratio.An object of one embodiment of the present invention is to provide a highly reliable transistor, a semiconductor device, a display device, or a memory device.An object of one embodiment of the present invention is to provide a semiconductor device, a display device, or a memory device with low power consumption.An object of one embodiment of the present invention is to provide a memory device with high operating speed.An object of one embodiment of the present invention is to provide a manufacturing method of the transistor, the semiconductor device, the display device, or the memory device.
[0012] Note that the description of these problems does not preclude the existence of other problems. One embodiment of the present invention does not necessarily have to solve all of these problems. Problems other than these can be extracted from the description in the specification, drawings, and claims.
[0013] One embodiment of the present invention is a semiconductor device including a cylindrical semiconductor layer, a first conductive layer in contact with a bottom surface of the semiconductor layer, a second conductive layer in contact with a top surface of the semiconductor layer, a first insulating layer covering at least a part of a side surface of the semiconductor layer, and a third conductive layer facing the side surface of the semiconductor layer with the first insulating layer interposed therebetween. The first insulating layer has a first region between the semiconductor layer and the third conductive layer and a second region between the first conductive layer and the third conductive layer. The width of the first region in a direction from the semiconductor layer toward the third conductive layer is equal to or approximately equal to the width of the second region in a direction from the first conductive layer toward the third conductive layer.
[0014] In the semiconductor device, the height of the semiconductor layer is preferably greater than the width of the lower surface of the semiconductor layer.
[0015] In the above semiconductor device, the first insulating layer preferably has a region in contact with the second conductive layer.
[0016] In the above semiconductor device, it is preferable that the semiconductor layer includes a first oxide semiconductor layer, and a second oxide semiconductor layer and a third oxide semiconductor layer sandwiching the first oxide semiconductor layer, and that each of the second oxide semiconductor layer and the third oxide semiconductor layer has a lower resistance than the first oxide semiconductor layer and has a region facing the third conductive layer with the first insulating layer interposed therebetween.
[0017] In the above semiconductor device, it is preferable that the first oxide semiconductor layer contains one or both of indium and zinc, and that each of the second oxide semiconductor layer and the third oxide semiconductor layer contains one or both of indium and zinc and nitrogen.
[0018] The semiconductor device preferably has a second insulating layer between the first conductive layer and the first insulating layer, and the second insulating layer preferably covers another part of the side surface of the semiconductor layer.
[0019] In the above semiconductor device, it is preferable that the first insulating layer has a stacked structure of a first insulating film located on the semiconductor layer side and a second insulating film located on the third conductive layer side, the first insulating film containing silicon and oxygen, and the second insulating film containing silicon and nitrogen.
[0020] Preferably, the semiconductor device has a third insulating layer covering the third conductive layer, and the third conductive layer is surrounded by the third insulating layer and the second insulating film.
[0021] Another embodiment of the present invention is a semiconductor device including: a cylindrical first semiconductor layer; a first conductive layer in contact with a bottom surface of the first semiconductor layer; a second conductive layer in contact with a top surface of the first semiconductor layer; a second semiconductor layer covering a side surface of the first semiconductor layer; a first insulating layer covering at least a portion of the side surface of the second semiconductor layer; and a third conductive layer facing the side surface of the first semiconductor layer via the first insulating layer. The first insulating layer has a first region between the first semiconductor layer and the third conductive layer and a second region between the first conductive layer and the third conductive layer. The width of the first region in a direction from the first semiconductor layer to the third conductive layer is equal to or approximately equal to the width of the second region in a direction from the first conductive layer to the third conductive layer.
[0022] In the above semiconductor device, the height of the first semiconductor layer is preferably greater than the width of the lower surface of the first semiconductor layer.
[0023] In the above semiconductor device, it is preferable that the first insulating layer and the second semiconductor layer each have a region in contact with the second conductive layer.
[0024] In the above semiconductor device, the first semiconductor layer and the second semiconductor layer preferably contain one or both of indium and zinc.
[0025] The semiconductor device preferably has a second insulating layer between the first conductive layer and the first insulating layer, and the second insulating layer preferably covers another part of the side surface of the second semiconductor layer.
[0026] Another embodiment of the present invention is a memory device including the above semiconductor device and a capacitor, wherein the first conductive layer has a region that functions as one of a pair of electrodes of the capacitor.
[0027] Another embodiment of the present invention is a memory device including the above semiconductor device and a capacitor, wherein the second conductive layer has a region which functions as one of a pair of electrodes of the capacitor.
[0028] Another embodiment of the present invention is a method for manufacturing a semiconductor device, including forming a first conductive layer, forming a cylindrical semiconductor layer over the first conductive layer, depositing a first insulating layer over the first conductive layer and the semiconductor layer, processing the first insulating layer to expose part of a side surface of the semiconductor layer, depositing a second insulating layer and a conductive film in this order over the first insulating layer and the semiconductor layer, and processing the conductive film to form a second conductive layer whose top surface is located closer to the first conductive layer than the top surface of the semiconductor layer, and forming a third conductive layer over the semiconductor layer and the second insulating layer.
[0029] In the above-described method for manufacturing a semiconductor device, the semiconductor layer is preferably formed so that the height thereof is greater than the width of the bottom surface thereof.
[0030] In the above-described method for manufacturing a semiconductor device, the second insulating layer is preferably formed by atomic layer deposition.
[0031] According to one embodiment of the present invention, a transistor with favorable electrical characteristics can be provided. According to one embodiment of the present invention, a transistor with large on-state current can be provided. According to one embodiment of the present invention, a transistor, a semiconductor device, or a memory device that can be miniaturized or highly integrated can be provided. According to one embodiment of the present invention, a display device with high definition or a high aperture ratio can be provided. According to one embodiment of the present invention, a highly reliable transistor, a semiconductor device, a display device, or a memory device can be provided. According to one embodiment of the present invention, a semiconductor device, a display device, or a memory device with low power consumption can be provided. According to one embodiment of the present invention, a memory device with high operating speed can be provided. According to one embodiment of the present invention, a manufacturing method of the above-described transistor, semiconductor device, display device, or memory device can be provided.
[0032] Note that the description of these effects does not preclude the existence of other effects. One embodiment of the present invention does not necessarily have all of these effects. Effects other than these can be extracted from the description in the specification, drawings, and claims.
[0033] 1A to 1C are perspective views showing a structural example of a semiconductor device. FIG. 2A is a plan view showing a structural example of a semiconductor device. FIGS. 2B to 2D are cross-sectional views showing a structural example of a semiconductor device. FIGS. 3A and 3B are cross-sectional views showing a structural example of a semiconductor device. FIGS. 4A and 4B are cross-sectional views showing a structural example of a semiconductor device. FIGS. 5A to 5F are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 6A to 6F are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 7A to 7F are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 8A to 8F are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 9A to 9F are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 10A to 10D are cross-sectional views showing a manufacturing method example of a semiconductor device. FIG. 11A is a plan view showing a structural example of a semiconductor device. FIGS. 11B to 11D are cross-sectional views showing a structural example of a semiconductor device. FIGS. 12A to 12F are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 13A to 13D are cross-sectional views showing a structural example of a semiconductor device. FIGS. 14A and 14B are cross-sectional views showing a structural example of a semiconductor device. FIGS. 15A to 15F are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 16A to 16F are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 17A to 17D are cross-sectional views showing a structural example of a semiconductor device. FIGS. 18A to 18D are cross-sectional views showing a manufacturing method example of a semiconductor device. FIGS. 19A to 19D are cross-sectional views showing a structural example of a semiconductor device. FIGS. 20A to 20D are cross-sectional views showing a structural example of a memory device. FIGS. 21A to 21D are cross-sectional views showing a structural example of a memory device. FIGS. 22A and 22B are cross-sectional views showing a structural example of a memory device. FIG. 23A is a plan view showing an example of a memory device. FIG. 23B is a cross-sectional view showing an example of a memory device. FIG. 24 is a cross-sectional view showing an example of a memory device. FIG. 25 is a cross-sectional view showing an example of a memory device. FIG. 26 is a cross-sectional view showing an example of a memory device. FIG. 27 is a block diagram illustrating a structural example of a semiconductor device. FIGS. 28A to 28H are diagrams illustrating circuit configuration examples of memory cells. 29A and 29B are perspective views illustrating a configuration example of a semiconductor device. Fig. 30 is a block diagram illustrating a CPU.FIGS. 31A and 31B are perspective views of a semiconductor device. FIGS. 32A and 32B are perspective views of a semiconductor device. FIGS. 33A and 33B are views showing various storage devices by layer. FIGS. 34A and 34B are perspective views showing an example of a display device. FIG. 35 is a cross-sectional view showing an example of a display device. FIG. 36 is a cross-sectional view showing an example of a display device. FIGS. 37A to 37C are views showing an example of the configuration of a display device. FIGS. 38A and 38B are views showing an example of electronic components. FIGS. 39A to 39C are views showing an example of a mainframe computer. FIG. 39D is a view showing an example of space equipment. FIG. 39E is a view showing an example of a storage system applicable to a data center. FIGS. 40A to 40F are views showing an example of electronic equipment. FIGS. 41A to 41G are views showing an example of electronic equipment. FIGS. 42A to 42F are views showing an example of electronic equipment.
[0034] The embodiments will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various changes can be made in form and detail without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0035] In the configuration of the invention described below, the same parts or parts having similar functions are denoted by the same reference numerals in different drawings, and repeated explanations thereof will be omitted. Furthermore, when referring to similar functions, the same hatching pattern may be used and no particular reference numeral may be assigned.
[0036] Furthermore, for ease of understanding, the position, size, range, etc. of each component shown in the drawings may not represent the actual position, size, range, etc. Therefore, the disclosed invention is not necessarily limited to the position, size, range, etc. disclosed in the drawings.
[0037] In this specification, the ordinal numbers "first" and "second" are used for convenience and do not limit the number of components or the order of the components (for example, the order of processes or the order of stacking). Furthermore, the ordinal numbers assigned to components in one part of this specification may not match the ordinal numbers assigned to the same components in other parts of this specification or in the claims.
[0038] A transistor is a type of semiconductor element that can amplify current or voltage, and perform a switching operation to control conduction or non-conduction. The term "transistor" as used herein includes an insulated gate field effect transistor (IGFET) and a thin film transistor (TFT).
[0039] In this specification and the like, a transistor using an oxide semiconductor or a metal oxide for a semiconductor layer and a transistor having an oxide semiconductor or a metal oxide in a region where a channel is formed (also referred to as a channel formation region) may be referred to as an OS transistor. A transistor having silicon in a channel formation region may be referred to as a Si transistor.
[0040] In this specification and the like, a transistor is an element having at least three terminals including a gate, a drain, and a source. A transistor has a region (also referred to as a channel formation region) where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode), and current can flow between the source and the drain through the channel formation region. Note that in this specification and the like, the channel formation region refers to a region through which current mainly flows.
[0041] Furthermore, the functions of "source" and "drain" may be interchangeable when transistors of different polarities are used, or when the direction of current flow changes during circuit operation, etc. For this reason, the terms "source" and "drain" may be used interchangeably in this specification.
[0042] Note that impurities in a semiconductor refer to, for example, elements other than the main components constituting the semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be considered an impurity. The presence of impurities may increase the density of defect states in the semiconductor or reduce the crystallinity, for example. When the semiconductor is an oxide semiconductor, impurities that change the characteristics of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor. Specific examples include hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, and nitrogen. Note that water may also function as an impurity. For example, the inclusion of impurities may cause oxygen deficiency (V) in the oxide semiconductor. O In some cases, a nucleus (also referred to as a nucleus) may be formed.
[0043] In this specification and the like, an oxynitride refers to a material having a composition in which oxygen is contained in a larger amount than nitrogen, and a nitride oxide refers to a material having a composition in which nitrogen is contained in a larger amount than oxygen.
[0044] To analyze the content of elements such as hydrogen, oxygen, carbon, and nitrogen contained in a film, for example, secondary ion mass spectrometry (SIMS) or X-ray photoelectron spectroscopy (XPS) can be used. XPS is suitable when the content of the target element is high (e.g., 0.5 atomic% or more, or 1 atomic% or more). On the other hand, SIMS is suitable when the content of the target element is low (e.g., 0.5 atomic% or less, or 1 atomic% or less). When comparing the content of elements, it is more preferable to perform a combined analysis using both SIMS and XPS analytical techniques.
[0045] The terms "film" and "layer" can be interchangeable depending on the circumstances. For example, the term "conductive layer" can be changed to the term "conductive film." Or, for example, the term "insulating film" can be changed to the term "insulating layer."
[0046] Furthermore, in this specification, "parallel" refers to a state in which two straight lines are arranged at an angle of -10 degrees or more and 10 degrees or less. Therefore, it also includes cases in which the angle is -5 degrees or more and 5 degrees or less. "Approximately parallel" refers to a state in which two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. "Perpendicular" refers to a state in which two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it also includes cases in which the angle is 85 degrees or more and 95 degrees or less. "Approximately perpendicular" refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less. Here, two straight lines have been used as an example, but the same applies to two surfaces. The same applies to a single straight line and a single surface.
[0047] In this specification, "electrically connected" includes connection via "something that has some kind of electrical function." Here, "something that has some kind of electrical function" is not particularly limited as long as it allows electrical signals to be transmitted and received between the connected objects. For example, "something that has some kind of electrical function" includes electrodes or wiring, as well as switching elements such as transistors, resistive elements, coils, and other elements with various functions.
[0048] In this specification and the like, unless otherwise specified, the off-state current refers to the leakage current between the source and drain when the transistor is in an off state (also referred to as a non-conducting state or a cut-off state). Unless otherwise specified, the off-state current refers to the leakage current between the source and the gate when the voltage V gs is the threshold voltage V th (For p-channel transistors, V th This refers to a state of being (higher than)
[0049] In this specification, the term "normally-on" refers to a state in which a channel exists and a current flows through a transistor even when no voltage is applied to the gate, whereas the term "normally-off" refers to a state in which no current flows through a transistor when no potential is applied to the gate or when a ground potential is applied to the gate.
[0050] In this specification, the top surface shape of a certain component refers to the contour shape of the component in a plan view. The plan view refers to a view from the normal direction of the surface on which the component is formed or the surface of a support (e.g., a substrate) on which the component is formed.
[0051] In this specification, the phrase "top surface shapes that are approximately the same" refers to at least a portion of the contours of stacked layers overlapping. For example, this includes cases where the upper and lower layers are processed using the same mask pattern or a portion of the same mask pattern. However, strictly speaking, the contours may not overlap, and the upper layer may be located inside the lower layer, or the upper layer may be located outside the lower layer. In these cases, the phrase "top surface shapes that are approximately the same" may also be used. Furthermore, when the top surface shapes are the same or approximately the same, it can also be said that the positions in plan view are the same or approximately the same, the edges are aligned or approximately aligned, or the side edges are aligned or approximately the same.
[0052] In this specification and the like, a tapered shape refers to a shape in which at least a portion of the side surface of a structure is inclined with respect to the substrate surface or the surface to be formed. For example, there is a region in which the angle (also called the taper angle) between the inclined side surface and the substrate surface or the surface to be formed is greater than 0 degrees and less than 90 degrees. Note that the side surface of the structure, the substrate surface, and the surface to be formed do not necessarily need to be completely flat, and may be approximately planar with a slight curvature or approximately planar with a slight unevenness.
[0053] In this specification and the like, when it is stated that A is in contact with B, it means that at least a part of A is in contact with B. Therefore, for example, it can be rephrased as saying that A has a region in contact with B.
[0054] In this specification and the like, when it is stated that A is located on B, it means that at least a part of A is located on B. Therefore, for example, it can be rephrased as, A has a region located on B.
[0055] In this specification and the like, when it is stated that A covers B, it means that at least a part of A covers B. Therefore, for example, it can be rephrased as saying that A has a region that covers B.
[0056] In this specification and the like, when it is stated that A overlaps with B, it means that at least a part of A overlaps with B. Therefore, for example, it can be rephrased as saying that A has an overlapping region with B.
[0057] In this specification, etc., a device fabricated using a metal mask or an FMM (fine metal mask, high-resolution metal mask) may be referred to as a device with an MM (metal mask) structure. Also, in this specification, etc., a device fabricated without using a metal mask or an FMM may be referred to as a device with an MML (metal maskless) structure.
[0058] In this specification and the like, a structure in which different light-emitting layers are formed for light-emitting elements (also referred to as light-emitting devices) with different emission wavelengths is sometimes referred to as an SBS (Side By Side) structure. The SBS structure allows the materials and configuration to be optimized for each light-emitting element, increasing the degree of freedom in selecting materials and configurations and making it easier to improve brightness and reliability.
[0059] In this specification and the like, holes or electrons may be referred to as "carriers." Specifically, a hole injection layer or an electron injection layer may be referred to as a "carrier injection layer," a hole transport layer or an electron transport layer may be referred to as a "carrier transport layer," and a hole block layer or an electron block layer may be referred to as a "carrier block layer." Note that the above-mentioned carrier injection layer, carrier transport layer, and carrier block layer may not be clearly distinguishable. Furthermore, one layer may have two or three functions among the carrier injection layer, carrier transport layer, and carrier block layer.
[0060] In this specification and the like, a light-emitting element has an EL layer between a pair of electrodes. The EL layer has at least a light-emitting layer. Here, examples of layers (also referred to as functional layers) included in the EL layer include a light-emitting layer, a carrier injection layer (a hole injection layer and an electron injection layer), a carrier transport layer (a hole transport layer and an electron transport layer), and a carrier block layer (a hole block layer and an electron block layer). In this specification and the like, a light-receiving element (also referred to as a light-receiving device) has at least an active layer that functions as a photoelectric conversion layer between a pair of electrodes. In this specification and the like, one of the pair of electrodes may be referred to as a pixel electrode, and the other as a common electrode.
[0061] In this specification and the like, the sacrificial layer (which may also be referred to as a mask layer) is located above at least the light-emitting layer (more specifically, a layer that is processed into an island shape among the layers that make up the EL layer), and has the function of protecting the light-emitting layer during the manufacturing process.
[0062] In this specification and the like, the term "step discontinuity" refers to a phenomenon in which a layer, film, or electrode is separated due to the shape of the surface on which it is formed (for example, a step or the like).
[0063] In the drawings and the like relating to this specification, arrows indicating the X direction, Y direction, and Z direction may be used. In this specification and the like, the "X direction" refers to the direction along the X axis, and there may be no distinction between the forward direction and the reverse direction unless explicitly stated. The same applies to the "Y direction" and the "Z direction." The X direction, Y direction, and Z direction are directions that intersect with each other. For example, the X direction, Y direction, and Z direction are directions that are perpendicular to each other.
[0064] Embodiment 1 In this embodiment, a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. 1A to 19D. FIG.
[0065] A semiconductor device according to one embodiment of the present invention includes a semiconductor layer, a first conductive layer, a second conductive layer, a third conductive layer, and a first insulating layer.
[0066] The semiconductor layer has a cylindrical shape. The first conductive layer contacts the bottom surface of the semiconductor layer, and the second conductive layer contacts the top surface of the semiconductor layer. The first insulating layer covers at least a portion of a side surface of the semiconductor layer. The third conductive layer faces the side surface of the semiconductor layer via the first insulating layer. The first insulating layer has a first region and a second region. The first region is located between the semiconductor layer and the third conductive layer, and the second region is located between the first conductive layer and the third conductive layer. The width of the first region in a direction from the semiconductor layer toward the third conductive layer is equal to or approximately equal to the width of the second region in a direction from the first conductive layer toward the third conductive layer.
[0067] In the present embodiment and the like, the semiconductor layer has been exemplified as having a cylindrical shape, but the shape of the semiconductor layer is not limited thereto. For example, as long as the semiconductor layer has a lower surface and an upper surface that are parallel or approximately parallel to each other and at least one side surface, the semiconductor layer may have a structure other than a cylindrical shape, such as an elliptical cylindrical shape, a truncated cone shape, a prismatic shape, or a prismatic shape with rounded corners.
[0068] The first conductive layer functions as one of a source electrode and a drain electrode of the transistor, the second conductive layer functions as the other of the source electrode and the drain electrode of the transistor, and the third conductive layer functions as a gate electrode of the transistor. The first insulating layer functions as a gate insulating layer of the transistor. A channel is formed in the semiconductor layer in a region facing the third conductive layer with the first insulating layer interposed therebetween.
[0069] In a transistor according to one embodiment of the present invention, a source electrode and a drain electrode are located at different heights, and a current flows in the height direction through a semiconductor layer. In other words, it can be said that the channel length direction has a component in the height direction (vertical direction). Therefore, the transistor according to one embodiment of the present invention can also be called a VFET (Vertical Field Effect Transistor), a vertical transistor, a vertical channel transistor, a vertical channel type transistor, or the like.
[0070] In the transistor of one embodiment of the present invention, a source electrode, a semiconductor layer, and a drain electrode can be provided in a stacked manner, and therefore the occupied area can be significantly reduced compared to a so-called planar transistor in which a semiconductor layer is arranged in a planar shape. Therefore, a transistor that can be miniaturized or highly integrated can be provided.
[0071] Furthermore, the semiconductor device of one embodiment of the present invention can include a second insulating layer between the first conductive layer and the first insulating layer. The second insulating layer covers another part of the side surface of the semiconductor layer. By providing the second insulating layer, the physical distance between the first conductive layer and the third conductive layer can be increased, and parasitic capacitance generated between the first conductive layer and the third conductive layer can be reduced. Therefore, a transistor with low parasitic capacitance can be provided.
[0072] <Structural Example 1 of Semiconductor Device> A structure of a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. 1A to 18D. FIG.
[0073] FIG. 1A is a perspective view illustrating a configuration example of a semiconductor device according to one embodiment of the present invention. The perspective view illustrated in FIG. 1B is a perspective view obtained by cutting the perspective view illustrated in FIG. 1A along a plane including a dashed-dotted line A1-A2. The perspective view illustrated in FIG. 1C is a perspective view obtained by cutting the perspective view illustrated in FIG. 1A along a plane including a dashed-dotted line A3-A4. FIG. 2A is a plan view of the semiconductor device. FIG. 2B is a cross-sectional view of the semiconductor device corresponding to a portion indicated by a dashed-dotted line A1-A2 in FIG. 2A. FIG. 2C is a cross-sectional view of the semiconductor device corresponding to a portion indicated by a dashed-dotted line A3-A4 in FIG. 2A. The dashed-dotted line A1-A2 is a straight line parallel to the Y direction in the drawing, and the dashed-dotted line A3-A4 is a straight line parallel to the X direction in the drawing. Some elements are omitted from the perspective view and the plan view for clarity. Some elements may also be omitted from the subsequent plan views.
[0074] 1A to 2C includes an insulating layer 210 over a substrate (not shown), a transistor 200 over the insulating layer 210, an insulating layer 280, an insulating layer 281 over the insulating layer 280, and an insulating layer 283 over the transistor 200. The insulating layer 210, the insulating layer 280, the insulating layer 281, and the insulating layer 283 function as interlayer films.
[0075] The transistor 200 has a conductive layer 220 on an insulating layer 210, a semiconductor layer 230 on the conductive layer 220, an insulating layer 250 on the insulating layer 280, a conductive layer 260 on the insulating layer 250, and a conductive layer 240 on the semiconductor layer 230, the insulating layer 250, and the insulating layer 281.
[0076] The insulating layer 280 is provided over the conductive layer 220 and the insulating layer 210. The insulating layer 281 is provided over the insulating layer 250 and the conductive layer 260. The insulating layer 283 is provided over the conductive layer 240 and the insulating layer 281.
[0077] The side surfaces of the semiconductor layer 230 are preferably perpendicular to the upper surface of the insulating layer 210. This configuration allows for miniaturization or high integration of the semiconductor device. In this case, the films provided on the outer side of the semiconductor layer 230 are preferably formed using atomic layer deposition (ALD). The ALD method allows atoms to be deposited layer by layer, and therefore has the advantages of enabling ultrathin film formation, film formation on structures with high aspect ratios, film formation with fewer defects such as pinholes, film formation with excellent coverage, and film formation at low temperatures. Therefore, the films can be formed on the side surfaces of the semiconductor layer 230 with good coverage. For example, the insulating layer 250 and the conductive layer 260 are preferably formed using the ALD method.
[0078] When the side surface of the semiconductor layer 230 is perpendicular to the upper surface of the insulating layer 210, the semiconductor layer 230 has a cylindrical shape, as shown in Figures 2B and 2C. The semiconductor layer 230 is provided extending in the Z direction. That is, the normal to the lower surface and the normal to the upper surface of the semiconductor layer 230 are parallel to the Z direction. Furthermore, the lower surface of the semiconductor layer 230 contacts a portion of the upper surface of the conductive layer 220, the upper surface of the semiconductor layer 230 contacts a portion of the lower surface of the conductive layer 240, and at least a portion of the side surface of the semiconductor layer 230 contacts the insulating layer 250. Furthermore, in the configuration shown in Figures 2B and 2C, another portion of the side surface of the semiconductor layer 230 contacts the insulating layer 280.
[0079] The height of the upper surface of the semiconductor layer 230 is equal to or approximately equal to the height of the upper surface of the insulating layer 250 and the height of the upper surface of the insulating layer 281, respectively.
[0080] The insulating layer 250 covers at least a portion of the side surface of the semiconductor layer 230. The insulating layer 250 has a region in contact with the conductive layer 240. The insulating layer 250 has a first region between the semiconductor layer 230 and the conductive layer 260 and a second region between the conductive layer 220 and the conductive layer 260. The second region can also be said to be located between the insulating layer 280 and the conductive layer 260. In FIG. 2B , the width W250 of the first region of the insulating layer 250 in the direction from the semiconductor layer 230 toward the third conductive layer (X direction or Y direction) is indicated by an outer arrow of a two-dot chain line. The width H250 of the second region of the insulating layer 250 in the direction from the first conductive layer toward the third conductive layer (Z direction) is also indicated by an outer arrow of a two-dot chain line. For example, when the insulating layer 250 is formed using an ALD method, the width W250 is equal to or approximately equal to the width H250.
[0081] In this specification, the expression "the first width and the second width are the same" means that the value obtained by dividing the absolute value of the difference between the first width and the second width by the first width is 0.1 or less, or the value obtained by dividing the absolute value of the difference between the first width and the second width by the second width is 0.1 or less.
[0082] The upper surface of the portion of the conductive layer 260 that runs along the side surface of the semiconductor layer 230 is located lower (closer to the insulating layer 210) than the upper surface of the semiconductor layer 230. The conductive layer 260 has a first region that faces the side surface of the semiconductor layer 230 with the insulating layer 250 interposed therebetween, and a second region that overlaps with the conductive layer 220 with the insulating layer 250 interposed therebetween. For example, when the conductive layer 260 is formed using the ALD method, the width of the first region of the conductive layer 260 in the X direction or Y direction matches or approximately matches the width of the second region of the conductive layer 260 in the Z direction.
[0083] In the semiconductor device shown in FIGS. 2B and 2C, the conductive layer 260 is provided extending in the X direction, and the conductive layers 220 and 240 are provided extending in the Y direction.
[0084] In the transistor 200, the semiconductor layer 230 functions as a semiconductor layer, the conductive layer 260 functions as a gate electrode, the insulating layer 250 functions as a gate insulating layer, the conductive layer 220 functions as one of a source electrode and a drain electrode, and the conductive layer 240 functions as the other of the source electrode and the drain electrode.
[0085] The transistor 200 has a structure in which one of the source electrode and the drain electrode (here, the conductive layer 220) is located on the bottom and the other of the source electrode and the drain electrode (here, the conductive layer 240) is located on the top, so that current flows in the vertical direction. That is, a channel is formed along the side surface of the semiconductor layer 230. The transistor 200 also has a structure in which the gate electrode surrounds the channel formation region. Therefore, the transistor 200 can be said to have a GAA (Gate-All-Around) structure.
[0086] The transistor 200 preferably includes a metal oxide (also referred to as an oxide semiconductor) functioning as a semiconductor in the semiconductor layer 230 including a channel formation region. In this case, the transistor 200 can be referred to as an OS transistor. Note that a semiconductor layer including an oxide semiconductor may be referred to as an oxide semiconductor layer.
[0087] An OS transistor has an oxygen vacancy (V O If there are impurities and oxygen vacancies, the electrical characteristics may be easily changed and reliability may be reduced. O H) may generate electrons that serve as carriers. Therefore, if oxygen vacancies are present in the channel formation region of the oxide semiconductor, the OS transistor is likely to have normally-on characteristics. Therefore, it is preferable that oxygen vacancies and impurities are reduced as much as possible in the channel formation region of the oxide semiconductor. In other words, it is preferable that the carrier concentration of the channel formation region of the oxide semiconductor is reduced and the channel formation region of the oxide semiconductor is made i-type (intrinsic) or substantially i-type.
[0088] On the other hand, the source and drain regions of an OS transistor have more oxygen vacancies than the channel formation region.O The source and drain regions of an OS transistor are preferably n-type regions having a high carrier concentration and low resistance compared to a channel formation region, and the source and drain regions of the OS transistor preferably have a high carrier concentration and low resistance due to a high concentration of H or an impurity such as hydrogen, nitrogen, or a metal element.
[0089] In the transistor 200, a region of the semiconductor layer 230 that is covered with the conductive layer 260 with the insulating layer 250 interposed therebetween functions as a channel formation region. A region of the semiconductor layer 230 in contact with the conductive layer 220 functions as one of the source region and the drain region, and a region of the semiconductor layer 230 in contact with the conductive layer 240 functions as the other of the source region and the drain region. In other words, the channel formation region is sandwiched between the source region and the drain region.
[0090] When the semiconductor layer 230 and the conductive layer 220 come into contact with each other, a metal compound or oxygen vacancy is formed, and the region of the semiconductor layer 230 that comes into contact with the conductive layer 220 becomes less resistant. This reduces the contact resistance between the semiconductor layer 230 and the conductive layer 220. Similarly, when the semiconductor layer 230 and the conductive layer 240 come into contact with each other, the region of the semiconductor layer 230 that comes into contact with the conductive layer 240 becomes less resistant. This reduces the contact resistance between the semiconductor layer 230 and the conductive layer 240.
[0091] When the conductive layer 260 functions as a gate electrode, the channel length of the transistor 200 is the length of a region of the semiconductor layer 230 that overlaps with the conductive layer 260 with the insulating layer 250 interposed therebetween, in a cross-sectional view. In other words, it can be said that the channel length of the transistor 200 is determined by the height of the conductive layer 260. In Figure 2B, the channel length L of the transistor 200 is indicated by a dashed double-headed arrow.
[0092] In a planar transistor, the channel length is limited by the exposure limit of photolithography, making further miniaturization difficult. However, in the present invention, the channel length can be set by the height of the conductive layer 260. Therefore, the channel length L of the transistor 200 can be made into an extremely fine structure that is equal to or less than the exposure limit of photolithography (e.g., 0.1 nm to 100 nm, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, 5 nm to 30 nm, 5 nm to 20 nm, or 5 nm to 10 nm). This increases the on-state current of the transistor 200, thereby improving its frequency characteristics.
[0093] Furthermore, as described above, a channel formation region, a source region, and a drain region can be formed in the semiconductor layer 230. This allows the transistor 200 to occupy a smaller area than a planar transistor in which the channel formation region, the source region, and the drain region are separately provided on the XY plane. Therefore, the semiconductor device can be highly integrated. Furthermore, when the semiconductor device of one embodiment of the present invention is used in a memory device, the memory capacity per unit area can be increased.
[0094] The height of the semiconductor layer 230 needs to be greater than the channel length L of the transistor 200. On the other hand, the height of the semiconductor layer 230 needs to be large enough so that the semiconductor layer 230 processed into a cylindrical shape does not collapse. Therefore, the height of the semiconductor layer 230 is, for example, preferably 20 nm to 200 nm, more preferably 50 nm to 200 nm, still more preferably 80 nm to 200 nm, still more preferably 80 nm to 150 nm, and still more preferably 80 nm to 120 nm.
[0095] FIG. 2D shows an enlarged cross-sectional view in the XY plane including the semiconductor layer 230, the insulating layer 250, the conductive layer 260, and the insulating layer 281. Note that FIG. 2D can also be considered a cross-sectional view in the XY plane including the channel formation region of the semiconductor layer 230. As shown in FIG. 2D , the insulating layer 250 and the conductive layer 260 are concentrically arranged. Therefore, the side surface of the semiconductor layer 230 located at the center faces the side surface of the conductive layer 260 with the insulating layer 250 interposed therebetween. In other words, the entire periphery of the semiconductor layer 230 forms the channel formation region in a planar view. In this case, for example, the channel width of the transistor 200 is determined by the outer periphery of the semiconductor layer 230. In other words, the channel width of the transistor 200 can be determined by the width of the semiconductor layer 230 (or the diameter if the semiconductor layer 230 is circular in a planar view). In FIGS. 2B and 2D , the width D of the semiconductor layer 230 is indicated by a double-headed, dashed line. 2D, the channel width W of the transistor 200 is indicated by a dashed line with a double-headed arrow. By increasing the width D of the semiconductor layer 230, the channel width can be increased, and the on-state current can be increased.
[0096] When the semiconductor layer 230 is formed using photolithography, the width D of the semiconductor layer 230 is limited by the exposure limit of photolithography. The width D of the semiconductor layer 230 can be 5 nm to 100 nm, 5 nm to 60 nm, 5 nm to 50 nm, or 5 nm to 40 nm. When the semiconductor layer 230 is circular in plan view, the width D of the semiconductor layer 230 corresponds to the diameter of the semiconductor layer 230, and the channel width W can be calculated as "D × π".
[0097] From the above, the ratio of the height of the semiconductor layer 230 to the width D of the semiconductor layer 230 can be set to 0.2 or more and 40 or less, or 1 or more and 40 or less.
[0098] The height of the semiconductor layer 230 is preferably greater than the width D of the semiconductor layer 230. In other words, the width D of the semiconductor layer 230 is preferably smaller than the height of the semiconductor layer 230. By adopting such a structure, miniaturization or high integration of the semiconductor device can be achieved. Furthermore, when the height of the semiconductor layer 230 is increased to lengthen the channel length L of the transistor 200, the Vth When the height of the semiconductor layer 230 is increased to increase the physical distance between the conductive layer 260 and the conductive layer 240, the parasitic capacitance occurring between the conductive layer 260 and the conductive layer 240 can be reduced. Note that the height of the semiconductor layer 230 can be set to be the same as the width D of the semiconductor layer 230 or smaller than the width D of the semiconductor layer 230.
[0099] The channel length L of the transistor 200 can be made shorter than the channel width W of the transistor 200. The channel length L of the transistor 200 is preferably 0.1 to 0.99 times, more preferably 0.5 to 0.8 times, the channel width W of the transistor 200. With such a structure, a transistor with favorable electrical characteristics and high reliability can be realized.
[0100] In this embodiment, the semiconductor layer 230 has a circular shape in plan view, but the present invention is not limited to this. For example, the semiconductor layer 230 may have a substantially circular shape such as an oval, a polygonal shape such as a square, or a polygonal shape such as a square with rounded corners in plan view.
[0101] The insulating layer 280 is in contact with another part of the side surface of the semiconductor layer 230. The insulating layer 280 is in contact with the top surface and side surface of the conductive layer 220. The insulating layer 280 has a region located between the conductive layer 220 and the insulating layer 250. The film thickness of the insulating layer 280 on the conductive layer 220 is preferably 1 nm to 50 nm, more preferably 3 nm to 30 nm, still more preferably 5 nm to 30 nm, and still more preferably 10 nm to 20 nm. With this configuration, the physical distance between the conductive layer 220 and the conductive layer 260 can be increased, and the parasitic capacitance generated between the conductive layer 220 and the conductive layer 260 can be reduced.
[0102] The insulating layer 281 has a region located between the upper surface of the portion of the conductive layer 260 that is along the side surface of the semiconductor layer 230 and the lower surface of the conductive layer 240. This configuration can prevent short-circuiting between the conductive layer 260 and the conductive layer 240. Furthermore, by increasing the height of this region (the shortest distance from the upper surface of the portion of the conductive layer 260 that is along the side surface of the semiconductor layer 230 to the lower surface of the conductive layer 240), parasitic capacitance occurring between the conductive layer 260 and the conductive layer 240 can be reduced. The height of this region can be, for example, 5 nm to 50 nm, 5 nm to 30 nm, or 5 nm to 20 nm. The height (film thickness) of the insulating layer 281 in the region that does not overlap with the conductive layer 260 is the sum of the height of this region and the height (channel length L) of the conductive layer 260.
[0103] <Constituent Materials of Semiconductor Device> Materials that can be used in the semiconductor device of this embodiment will be described below. Note that each layer constituting the semiconductor device of this embodiment may have a single-layer structure or a stacked-layer structure. FIGS. 2B and 2C show an example in which the conductive layer 220, the semiconductor layer 230, the conductive layer 240, the insulating layer 250, and the conductive layer 260 each have a single-layer structure. FIGS. 3A to 4B show an example in which the conductive layer 220, the semiconductor layer 230, the conductive layer 240, the insulating layer 250, and the conductive layer 260 each have a stacked-layer structure.
[0104] [Semiconductor Layer 230] As described above, the semiconductor layer 230 has a channel formation region. The channel formation region is i-type (intrinsic) or substantially i-type. The semiconductor layer 230 further has a source region and a drain region. The source region and the drain region are n-type regions (low-resistance regions) with higher carrier concentrations than the channel formation region.
[0105] The crystallinity of the semiconductor material used for the semiconductor layer 230 is not particularly limited, and any of an amorphous semiconductor, a single crystal semiconductor, and a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part) may be used. Use of a single crystal semiconductor or a crystalline semiconductor is preferable because it can suppress deterioration of transistor characteristics.
[0106] The band gap of a metal oxide functioning as a semiconductor is preferably 2.0 eV or more, more preferably 2.5 eV or more. By using a metal oxide with a wide band gap, the off-state current of a transistor can be reduced. Because the off-state current of an OS transistor is low, the power consumption of a semiconductor device can be sufficiently reduced. Furthermore, because the frequency characteristics of an OS transistor are high, the semiconductor device can operate at high speed.
[0107] Examples of metal oxides that can be used for the semiconductor layer 230 include indium oxide, gallium oxide, and zinc oxide. The metal oxide preferably contains at least indium (In) or zinc (Zn). The metal oxide preferably contains two or three elements selected from indium, element M, and zinc. The metal oxide preferably contains one or both of indium and zinc. The element M is a metal element or a metalloid element having a high bond energy with oxygen, such as a metal element or a metalloid element having a bond energy with oxygen higher than that of indium. Specific examples of the element M include aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony. The element M contained in the metal oxide is preferably one or more of the above elements, more preferably one or more selected from aluminum, gallium, tin, and yttrium, and even more preferably gallium. In this specification and the like, metal elements and metalloid elements may be collectively referred to as "metal elements," and the "metal elements" described in this specification and the like may include metalloid elements.
[0108] The semiconductor layer 230 may be formed of, for example, indium oxide (In oxide), indium zinc oxide (In—Zn oxide, also referred to as IZO (registered trademark)), indium tin oxide (In—Sn oxide), indium titanium oxide (In—Ti oxide), indium gallium oxide (In—Ga oxide), indium gallium aluminum oxide (In—Ga—Al oxide), indium gallium tin oxide (In—Ga—Sn oxide, also referred to as IGTO), gallium zinc oxide (Ga—Zn oxide, also referred to as GZO), aluminum zinc oxide (Al—Zn oxide, also referred to as AZO), or indium Examples of usable materials include indium aluminum zinc oxide (In-Al-Zn oxide, also referred to as IAZO), indium tin zinc oxide (In-Sn-Zn oxide, also referred to as ITZO (registered trademark)), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium zinc oxide (In-Ga-Zn oxide, also referred to as IGZO), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide, also referred to as IGZTO), and indium gallium aluminum zinc oxide (In-Ga-Al-Zn oxide, also referred to as IGAZO, IGZAO, or IAGZO). Alternatively, silicon-containing indium tin oxide, gallium tin oxide (Ga-Sn oxide), aluminum tin oxide (Al-Sn oxide), and the like can be used.
[0109] By increasing the ratio of the number of indium atoms to the total number of atoms of all metal elements contained in the metal oxide, the field-effect mobility of the transistor can be increased, and a transistor with a large on-state current can be realized.
[0110] Note that the metal oxide may contain one or more metal elements having a higher period number in the periodic table instead of or in addition to indium. The greater the overlap of the orbitals of metal elements, the greater the carrier conduction in the metal oxide. Therefore, including a metal element having a higher period number in the periodic table may improve the field-effect mobility of a transistor. Examples of metal elements having a higher period number in the periodic table include metal elements belonging to the fifth period and the sixth period. Specific examples of such metal elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium. Lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium are called light rare earth elements.
[0111] The metal oxide may also contain one or more nonmetallic elements. The presence of a nonmetallic element in the metal oxide may increase the carrier concentration or narrow the band gap, thereby increasing the field-effect mobility of the transistor. Examples of nonmetallic elements include carbon, nitrogen, phosphorus, sulfur, selenium, fluorine, chlorine, bromine, and hydrogen.
[0112] Furthermore, by increasing the ratio of the number of zinc atoms to the sum of the numbers of atoms of all metal elements contained in the metal oxide, the metal oxide can be made highly crystalline, and the diffusion of impurities in the metal oxide can be suppressed, thereby suppressing fluctuations in the electrical characteristics of the transistor and improving its reliability.
[0113] Furthermore, by increasing the ratio of the number of atoms of element M to the sum of the number of atoms of all metal elements contained in the metal oxide, a metal oxide with a wide band gap can be obtained. Furthermore, the formation of oxygen vacancies in the metal oxide can be suppressed. Therefore, carrier generation due to oxygen vacancies can be suppressed, resulting in a transistor with a low off-state current. Furthermore, a shift in the threshold voltage of the transistor can be suppressed. Furthermore, fluctuations in the electrical characteristics of the transistor can be suppressed, resulting in improved reliability.
[0114] The electrical characteristics and reliability of a transistor vary depending on the composition of the metal oxide used in the semiconductor layer 230. Therefore, by varying the composition of the metal oxide depending on the electrical characteristics and reliability required of the transistor, a semiconductor device that has both excellent electrical characteristics and high reliability can be obtained.
[0115] When the metal oxide is an In-M-Zn oxide, the atomic ratio of In in the In-M-Zn oxide is preferably equal to or greater than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxides include In:M:Zn=1:1:0.5, In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=1:1:2, In:M:Zn=2:1:3, In:M:Zn=3:1:1, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:3, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, and compositions close to these. Note that the term "nearby composition" includes a range of ±30% of the desired atomic ratio. By increasing the atomic ratio of indium in the metal oxide, the on-state current, field-effect mobility, and the like of the transistor can be increased.
[0116] Furthermore, the atomic ratio of In in the In-M-Zn oxide may be less than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxide include In:M:Zn=1:3:2, In:M:Zn=1:3:3, In:M:Zn=1:3:4, and compositions close to these. By increasing the proportion of M atoms in the metal oxide, the generation of oxygen vacancies can be suppressed.
[0117] When the element M contains a plurality of metal elements, the total proportion of the number of atoms of the metal elements can be used as the proportion of the number of atoms of the element M.
[0118] In this specification and the like, the ratio of the number of indium atoms to the sum of the numbers of atoms of all contained metal elements may be referred to as the indium content. The same applies to other metal elements.
[0119] Furthermore, when the metal oxide is an In-Zn oxide, the atomic ratio of the metal elements in the In-Zn oxide may be, for example, In:Zn = 1:1, In:Zn = 2:1, In:Zn = 4:1, or a composition in the vicinity thereof. The In-Zn oxide may also contain a trace amount of element M. For example, when Sn is contained as element M, the atomic ratio of the metal elements in the metal oxide may be, for example, In:Sn:Zn = 2:0.1:1, In:Sn:Zn = 4:0.1:1, or a composition in the vicinity thereof.
[0120] The composition of the metal oxide used in the semiconductor layer 230 can be analyzed using, for example, energy dispersive X-ray spectrometry (EDX), XPS, inductively coupled plasma mass spectrometry (ICP-MS), or inductively coupled plasma atomic emission spectrometry (ICP-AES). Alternatively, the analysis may be performed by combining a plurality of these techniques. Note that for elements with low content, the actual content may differ from the content obtained by analysis due to the influence of analytical accuracy. For example, when the content of element M is low, the content of element M obtained by analysis may be lower than the actual content.
[0121] The sputtering method or the ALD method can be suitably used for forming the metal oxide. When forming the metal oxide by the sputtering method, the composition of the metal oxide after film formation may differ from the composition of the target. In particular, the zinc content in the metal oxide after film formation may decrease to about 50% compared to the target. In addition, the metal oxide film may be formed by a chemical vapor deposition (CVD) method, a molecular beam epitaxy (MBE) method, a pulsed laser deposition (PLD) method, or the like.
[0122] The semiconductor layer 230 preferably includes a crystalline metal oxide layer. Examples of the structure of a crystalline metal oxide include a c-axis aligned crystal (CAAC) structure, a polycrystalline structure, and a nanocrystalline (nc) structure. By using a crystalline metal oxide layer for the semiconductor layer 230, the density of defect states in the semiconductor layer 230 can be reduced, and a highly reliable semiconductor device can be realized.
[0123] The higher the crystallinity of the metal oxide layer used for the semiconductor layer 230, the more the density of defect states in the semiconductor layer 230 can be reduced. On the other hand, by using a metal oxide layer with low crystallinity, a transistor capable of passing a large current can be realized.
[0124] When a metal oxide layer is formed by a sputtering method, the higher the substrate temperature (stage temperature) during formation, the higher the crystallinity of the formed metal oxide layer.Furthermore, the higher the ratio of the flow rate of oxygen gas to the total film formation gas used during formation (hereinafter also referred to as the oxygen flow rate ratio), the higher the crystallinity of the formed metal oxide layer.
[0125] The crystallinity of the semiconductor layer 230 can be analyzed by, for example, X-ray diffraction (XRD), transmission electron microscope (TEM), or electron diffraction (ED). Alternatively, the analysis may be performed by combining a plurality of these techniques.
[0126] Hydrogen contained in the oxide semiconductor reacts with oxygen that bonds to metal atoms to form water, and oxygen vacancies (V O ) may be formed. O H functions as a donor and may generate electrons as carriers. Furthermore, some of the hydrogen may bond with oxygen, which is bonded to a metal atom, to generate electrons as carriers. Therefore, a transistor using an oxide semiconductor containing a large amount of hydrogen is likely to have normally-on characteristics (for example, an n-channel transistor has a negative threshold voltage). Furthermore, hydrogen in an oxide semiconductor is easily mobile due to stresses such as heat and an electric field. Therefore, if an oxide semiconductor contains a large amount of hydrogen, the reliability of the transistor may be reduced.
[0127] V in the semiconductor layer 230 O It is preferable to reduce H as much as possible to make the semiconductor layer 230 highly intrinsic or substantially highly intrinsic. OTo obtain an oxide semiconductor in which H is sufficiently reduced, it is important to remove impurities such as water and hydrogen from the oxide semiconductor (sometimes referred to as dehydration or dehydrogenation treatment) and to supply oxygen to the oxide semiconductor to repair oxygen vacancies. O Stable electrical characteristics can be obtained by using an oxide semiconductor in which impurities such as H are sufficiently reduced for a channel formation region of a transistor. Note that supplying oxygen to an oxide semiconductor to repair oxygen vacancies is sometimes referred to as oxygen-adding treatment.
[0128] The carrier concentration of the oxide semiconductor in the region functioning as a channel formation region is 1×10 18 cm −3 Preferably, it is 1×10 or less. 17 cm −3 More preferably, it is less than 1×10 16 cm −3 More preferably, it is less than 1×10 13 cm −3 More preferably, it is less than 1×10 12 cm −3 The lower limit of the carrier concentration of the oxide semiconductor in the region functioning as a channel formation region is not particularly limited, but is preferably, for example, 1×10 −9 cm −3 It can be said that:
[0129] Here, the influence of each impurity in a metal oxide (oxide semiconductor) will be described.
[0130] When an oxide semiconductor contains silicon or carbon, which is one of the Group 14 elements, defect levels are formed in the oxide semiconductor. Therefore, the carbon concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3Less than or equal to 3×10 18 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 The silicon concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3 Less than or equal to 3×10 18 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 The following applies.
[0131] Furthermore, when nitrogen is contained in an oxide semiconductor, electrons serving as carriers are generated, the carrier concentration increases, and the semiconductor tends to become n-type. As a result, a transistor using an oxide semiconductor containing nitrogen in a semiconductor layer tends to have normally-on characteristics. Alternatively, when nitrogen is contained in an oxide semiconductor, trap states may be formed. As a result, the electrical characteristics of the transistor may become unstable. Therefore, the nitrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3 Less than or equal to 5×10, more preferably 18 atoms / cm 3 Less than 1×10, more preferably 1×10 18 atoms / cm 3 or less, more preferably 5 × 10 17 atoms / cm 3 The following applies.
[0132] Furthermore, hydrogen contained in an oxide semiconductor reacts with oxygen bonded to a metal atom to form water, which may form an oxygen vacancy. Hydrogen entering the oxygen vacancy may generate electrons as carriers. Furthermore, some of the hydrogen may bond with oxygen bonded to a metal atom to generate electrons as carriers. Therefore, a transistor using an oxide semiconductor containing hydrogen is likely to have normally-on characteristics. Therefore, it is preferable to reduce hydrogen as much as possible in the channel formation region of the oxide semiconductor. Specifically, the hydrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Less than 5×10 19 atoms / cm 3 less than 1×10 19 atoms / cm 3 less than 5×10 18 atoms / cm 3 less than 1×10 18 atoms / cm 3 Less than.
[0133] Furthermore, when an oxide semiconductor contains an alkali metal or an alkaline earth metal, defect levels may be formed and carriers may be generated. Therefore, a transistor using an oxide semiconductor containing an alkali metal or an alkaline earth metal is likely to have normally-on characteristics. Therefore, when the concentration of the alkali metal or the alkaline earth metal in the channel formation region of the oxide semiconductor obtained by SIMS is set to 1×10 18 atoms / cm 3 Below 2 × 10, preferably 16 atoms / cm 3 Do the following:
[0134] When an oxide semiconductor with sufficiently reduced impurities is used for a channel formation region of a transistor, stable electrical characteristics can be obtained.
[0135] The semiconductor layer 230 may have a stacked structure including two or more metal oxide layers. The two or more metal oxide layers included in the semiconductor layer 230 may have the same or substantially the same composition. By using a stacked structure of metal oxide layers having the same composition, for example, the same sputtering target can be used for formation, thereby reducing manufacturing costs.
[0136] The two or more metal oxide layers included in the semiconductor layer 230 may have different compositions.
[0137] 3A shows an example in which the semiconductor layer 230 has a three-layer structure including a semiconductor layer 230a, a semiconductor layer 230b on the semiconductor layer 230a, and a semiconductor layer 230c on the semiconductor layer 230b. In this case, the semiconductor layer 230 has the semiconductor layer 230b, and the semiconductor layer 230a and the semiconductor layer 230c sandwiching the semiconductor layer 230b.
[0138] In the transistor 200, the semiconductor layer 230b functions as a channel formation region, the semiconductor layer 230a functions as one of a source region and a drain region, and the semiconductor layer 230c functions as the other of the source region and the drain region.
[0139] The semiconductor layer 230b can be made of any of the metal oxides applicable to the semiconductor layer 230 described above.
[0140] The semiconductor layer 230a and the semiconductor layer 230c are preferably made of a material having higher conductivity than the semiconductor layer 230b. The semiconductor layer 230a and the semiconductor layer 230c are preferably made of a material having lower resistance than the semiconductor layer 230b. For example, the semiconductor layer 230a and the semiconductor layer 230c are preferably made of a degenerate oxide semiconductor. By using a material having high conductivity for the semiconductor layer 230a in contact with the conductive layer 220 and the semiconductor layer 230c in contact with the conductive layer 240, the contact resistance between the semiconductor layer 230 and the conductive layer 220 and the contact resistance between the semiconductor layer 230 and the conductive layer 240 can be reduced, and a transistor with a large on-state current can be obtained.
[0141] 3A , each of the semiconductor layer 230a and the semiconductor layer 230c preferably has a region facing the conductive layer 260 with the insulating layer 250 interposed therebetween. With such a structure, the on-state current of the transistor 200 can be further increased.
[0142] 3B , the semiconductor device can be configured so that the semiconductor layer 230a and the semiconductor layer 230c do not have a region where they face the conductive layer 260 with the insulating layer 250 interposed therebetween. This configuration can suppress an increase in the parasitic capacitance generated between the semiconductor layer 230a and the conductive layer 260 and between the semiconductor layer 230c and the conductive layer 260. Therefore, the operating speed of the semiconductor device can be increased.
[0143] For example, the semiconductor layer 230a and the semiconductor layer 230c can be made of a material obtained by adding nitrogen to a metal oxide applicable to the semiconductor layer 230b. For example, when the semiconductor layer 230b contains one or both of indium and zinc, each of the semiconductor layer 230a and the semiconductor layer 230c preferably contains one or both of indium and zinc, and nitrogen. Specifically, it is preferable to use a metal oxide (also referred to as a metal oxynitride) containing indium, the above-described element M, zinc, and nitrogen. More specifically, an oxide containing indium (In), gallium (Ga), zinc (Zn), and nitrogen (also referred to as an oxynitride having In, Ga, and Zn, or nitrogen-added IGZO), an oxide containing indium (In), aluminum (Al), zinc (Zn), and nitrogen (also referred to as an oxynitride having In, Al, and Zn, or nitrogen-added IAZO), or an oxide containing indium (In), aluminum (Al), gallium (Ga), zinc (Zn), and nitrogen (also referred to as an oxynitride having In, Al, Ga, and Zn, nitrogen-added IAGZO, nitrogen-added IGAZO, or nitrogen-added AGIZO), or the like can be used.
[0144] For example, nitrogen-doped IGZO tends to have a wurtzite crystal structure. The wurtzite crystal structure has high lattice matching with the crystal structure of the crystal of In-M-Zn oxide. Therefore, by using a metal oxynitride having a wurtzite crystal structure as the semiconductor layer 230a, the crystallinity of the semiconductor layer 230b can be improved. In other words, it is easy to form a metal oxide having a CAAC structure as the semiconductor layer 230b.
[0145] As described above, when the CAAC-OS is used for the semiconductor layer 230b, the crystals of the semiconductor layer 230b are c-axis oriented with respect to the substrate surface. Note that impurities in the CAAC-OS tend not to diffuse in the c-axis direction. That is, by using the CAAC-OS for the semiconductor layer 230b, the incorporation of impurities into the semiconductor layer 230b can be suppressed. For example, the incorporation of nitrogen into the semiconductor layer 230b can be suppressed. Therefore, the conductivity of the semiconductor layer 230b can be suppressed from increasing.
[0146] Although the above description has been given of a material obtained by adding nitrogen to a metal oxide that can be used for the semiconductor layer 230b as the semiconductor layer 230a and the semiconductor layer 230c, the element added to the metal oxide that can be used for the semiconductor layer 230b may be an element that increases the conductivity of the metal oxide. Examples of such elements that can be used include one or more selected from the group consisting of hydrogen, Group 15 elements (typically nitrogen (N), phosphorus (P), arsenic (As), and antimony (Sb)), boron (B), aluminum (Al), argon (Ar), helium (He), neon (Ne), indium (In), fluorine (F), chlorine (Cl), titanium (Ti), and zinc (Zn).
[0147] Note that the metal oxide used for the semiconductor layer 230a and the semiconductor layer 230c may have higher conductivity than the semiconductor layer 230b. For example, the semiconductor layer 230a and the semiconductor layer 230c may use a metal oxide that has a common element other than oxygen as a main component and has a different chemical composition from the semiconductor layer 230b.
[0148] When the semiconductor layer 230a, the semiconductor layer 230c, and the semiconductor layer 230b contain a common element other than oxygen as a main component, the semiconductor layer 230 preferably has a stacked structure of multiple oxide layers with different chemical compositions. For example, when an In-M-Zn oxide is used as the semiconductor layer 230b, the ratio of the number of indium atoms to the sum of the numbers of atoms of the metal elements that are the main components in the metal oxide used for the semiconductor layer 230a or the semiconductor layer 230c is preferably greater than the ratio of the number of indium atoms to the sum of the numbers of atoms of the metal elements that are the main components in the metal oxide used for the semiconductor layer 230b. Furthermore, the ratio of the number of indium atoms to the element M in the metal oxide used for the semiconductor layer 230a or the semiconductor layer 230c is preferably greater than the ratio of the number of indium atoms to the element M in the metal oxide used for the semiconductor layer 230b.
[0149] The semiconductor layer 230 a and the semiconductor layer 230 c contain a common element other than oxygen as a main component, which can reduce the defect state density at the interface between the semiconductor layer 230 a or the semiconductor layer 230 c and the semiconductor layer 230 b. Since the defect state density at the interface between the semiconductor layer 230 a or the semiconductor layer 230 c and the semiconductor layer 230 b can be reduced, the effect of interface scattering on carrier conduction is reduced, and a large on-current can be obtained.
[0150] Alternatively, titanium oxide, molybdenum oxide, zinc oxide, indium oxide, tungsten oxide, magnesium oxide, calcium oxide, tin oxide, indium zinc oxide, indium tin oxide, indium tin oxide containing silicon, or the like may be used for the semiconductor layer 230a and the semiconductor layer 230c.
[0151] A transistor according to one embodiment of the present invention includes a cylindrical semiconductor layer 230. When a semiconductor material (typically, silicon) other than the above-described metal oxide is used for the semiconductor layer 230, a complicated ion implantation process is required. On the other hand, when the above-described metal oxide is used for the semiconductor layer 230, a complicated ion implantation process is not necessary. Therefore, when the above-described metal oxide is used for the cylindrical semiconductor layer 230, the transistor can be manufactured more easily than when silicon is used.
[0152] The semiconductor device of this embodiment may also be applied to a transistor using another semiconductor material for the semiconductor layer 230. Examples of such another semiconductor material include semiconductors made of simple elements and compound semiconductors. Examples of semiconductors made of simple elements include silicon and germanium. Examples of compound semiconductors include gallium arsenide and silicon germanium. Other examples of compound semiconductors include organic semiconductors and nitride semiconductors. The aforementioned oxide semiconductor is also a type of compound semiconductor. These semiconductor materials may contain impurities as dopants.
[0153] Silicon that can be used as a semiconductor material for a transistor includes single crystal silicon, polycrystalline silicon, microcrystalline silicon, and amorphous silicon. An example of polycrystalline silicon is low temperature polysilicon (LTPS).
[0154] Compound semiconductors that can be used for the semiconductor layer 230 include silicon carbide, silicon germanium, gallium arsenide, indium phosphide, boron nitride, and boron arsenide. The boron nitride that can be used for the semiconductor layer 230 preferably has an amorphous structure. The boron arsenide that can be used for the semiconductor layer 230 preferably has a cubic crystal structure.
[0155] The semiconductor layer 230 may include a layered material that functions as a semiconductor. A layered material is a general term for a group of materials that have a layered crystal structure. A layered crystal structure is a structure in which layers formed by covalent or ionic bonds are stacked via bonds weaker than covalent or ionic bonds, such as van der Waals forces. A layered material has high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, a transistor with a large on-current can be provided.
[0156] Examples of the layered material include graphene, silicene, and chalcogenides. Chalcogenides are compounds containing chalcogen (an element belonging to Group 16). Examples of chalcogenides include transition metal chalcogenides and Group 13 chalcogenides. Specific examples of transition metal chalcogenides that can be used as semiconductor layers of transistors include molybdenum sulfide (typically MoS 2 ), molybdenum selenide (typically MoSe 2 ), molybdenum telluride (typically MoTe 2 ), tungsten sulfide (typically WS 2 ), tungsten selenide (typically WSe 2 ), tungsten tellurium (typically WTe 2 ), hafnium sulfide (typically HfS 2 ), hafnium selenide (typically HfSe 2 ), zirconium sulfide (typically ZrS 2 ), zirconium selenide (typically ZrSe 2 ) etc.
[0157] [Insulating Layer] It is preferable to use an inorganic insulating film for each of the insulating layers (insulating layer 210, insulating layer 250, insulating layer 280, insulating layer 281, insulating layer 283, etc.) included in the semiconductor device. Examples of inorganic insulating films include an oxide insulating film, a nitride insulating film, an oxynitride insulating film, and a nitride oxide insulating film. Examples of oxide insulating films include a silicon oxide film, an aluminum oxide film, a magnesium oxide film, a gallium oxide film, a germanium oxide film, a yttrium oxide film, a zirconium oxide film, a lanthanum oxide film, a neodymium oxide film, a hafnium oxide film, a tantalum oxide film, a cerium oxide film, a gallium zinc oxide film, and a hafnium aluminate film. Examples of nitride insulating films include a silicon nitride film and an aluminum nitride film. Examples of oxynitride insulating films include a silicon oxynitride film, an aluminum oxynitride film, a gallium oxynitride film, an yttrium oxynitride film, and a hafnium oxynitride film. Examples of nitride oxide insulating films include a silicon nitride oxide film and an aluminum nitride oxide film. Furthermore, an organic insulating film may be used for the insulating layer of the semiconductor device.
[0158] For example, as transistors become more miniaturized and highly integrated, problems such as leakage current may occur due to thinner gate insulating layers. Using a high-dielectric-constant (high-k) material for the gate insulating layer allows for lower voltage operation of the transistor while maintaining the physical film thickness. Furthermore, the equivalent oxide thickness (EOT) of the gate insulating layer can be reduced. On the other hand, using a material with a low dielectric constant for the insulating layer that functions as an interlayer film can reduce the parasitic capacitance that occurs between wirings. Therefore, materials can be selected depending on the function of the insulating layer. Note that materials with a low dielectric constant also have high dielectric strength.
[0159] Examples of high-k materials include aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium zirconium oxide, oxides having aluminum and hafnium, oxynitrides having aluminum and hafnium, oxides having silicon and hafnium, oxynitrides having silicon and hafnium, and nitrides having silicon and hafnium.
[0160] Examples of materials with a low dielectric constant include inorganic insulating materials such as silicon oxide, silicon oxynitride, and silicon nitride oxide, and resins such as polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate, and acrylic resin. Other inorganic insulating materials with a low dielectric constant include silicon oxide doped with fluorine, silicon oxide doped with carbon, and silicon oxide doped with carbon and nitrogen. Another example is silicon oxide having vacancies. These silicon oxides may contain nitrogen.
[0161] Furthermore, a material capable of exhibiting ferroelectricity may be used for the insulating layer of a semiconductor device. Examples of materials capable of exhibiting ferroelectricity include metal oxides such as hafnium oxide, zirconium oxide, and hafnium zirconium oxide. Examples of materials capable of exhibiting ferroelectricity include a material obtained by adding element J1 (here, element J1 is one or more selected from zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) to hafnium oxide. Here, the ratio of the number of hafnium atoms to the number of element J1 atoms can be appropriately set; for example, the ratio of the number of hafnium atoms to the number of element J1 atoms can be set to 1:1 or close to 1:1. Examples of materials capable of exhibiting ferroelectricity include a material obtained by adding element J2 (here, element J2 is one or more selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) to zirconium oxide. The ratio of the number of zirconium atoms to the number of atoms of element J2 can be set appropriately, for example, the ratio of the number of zirconium atoms to the number of atoms of element J2 can be set to 1:1 or close to 1:1. Furthermore, as a material that can have ferroelectricity, lead titanate (PbTiO X Piezoelectric ceramics having a perovskite structure, such as barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), and barium titanate, may also be used.
[0162] Furthermore, examples of materials that can exhibit ferroelectricity include metal nitrides containing elements M1, M2, and nitrogen. Here, element M1 is one or more elements selected from aluminum, gallium, indium, etc. Furthermore, element M2 is one or more elements selected from boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, etc. The ratio of the number of atoms of element M1 to the number of atoms of element M2 can be set as appropriate. Furthermore, metal oxides containing element M1 and nitrogen may exhibit ferroelectricity even without containing element M2. Furthermore, examples of materials that can exhibit ferroelectricity include materials in which element M3 is added to the above metal nitrides. Furthermore, element M3 is one or more elements selected from magnesium, calcium, strontium, zinc, cadmium, etc. Here, the ratio of the number of atoms of element M1 to the number of atoms of element M2 to the number of atoms of element M3 can be set as appropriate.
[0163] Furthermore, materials that can have ferroelectricity include SrTaO 2 N, BaTaO 2 Perovskite-type oxynitrides such as N, GaFeO with κ-alumina structure 3 Examples include:
[0164] Although the above description has been given with reference to metal oxides and metal nitrides, the present invention is not limited to these. For example, metal oxynitrides in which nitrogen is added to the above metal oxides, or metal oxynitrides in which oxygen is added to the above metal nitrides, may also be used.
[0165] Furthermore, as a material capable of exhibiting ferroelectricity, for example, a mixture or compound made of multiple materials selected from the materials listed above can be used. Alternatively, the insulating layer can have a laminated structure made of multiple materials selected from the materials listed above. However, since the crystal structure (characteristics) of the materials listed above can change not only depending on the film formation conditions but also on various processes, in this specification, not only materials that exhibit ferroelectricity are referred to as ferroelectrics, but also as materials capable of exhibiting ferroelectricity.
[0166] Metal oxides containing either or both of hafnium and zirconium can have ferroelectricity even in thin films of a few nanometers. Furthermore, metal oxides containing either or both of hafnium and zirconium can have ferroelectricity even in very small areas. Therefore, by using metal oxides containing either or both of hafnium and zirconium, miniaturization of semiconductor devices can be achieved.
[0167] In this specification, a layer of a material that can have ferroelectricity may be referred to as a ferroelectric layer, a metal oxide film, or a metal nitride film. Also, in this specification, a device having such a ferroelectric layer, a metal oxide film, or a metal nitride film may be referred to as a ferroelectric device.
[0168] Ferroelectricity is believed to be exhibited by the displacement of oxygen or nitrogen in crystals contained in the ferroelectric layer due to an external electric field. Furthermore, it is believed that the exhibiting of ferroelectricity depends on the crystal structure of the crystals contained in the ferroelectric layer. Therefore, for an insulating layer to exhibit ferroelectricity, the insulating layer must contain crystals. In particular, an insulating layer containing crystals with an orthorhombic crystal structure is preferred because it exhibits ferroelectricity. The crystal structure of the crystals contained in the insulating layer may be one or more selected from the group consisting of tetragonal, orthorhombic, monoclinic, and hexagonal. The insulating layer may also have an amorphous structure. In this case, the insulating layer may have a composite structure having an amorphous structure and a crystalline structure.
[0169] Furthermore, a transistor using a metal oxide can have stable electrical characteristics by being surrounded by an insulating layer that has a function of suppressing the permeation of impurities and oxygen. The insulating layer that has a function of suppressing the permeation of impurities and oxygen can be, for example, a single-layer or stacked insulating layer containing one or more elements selected from boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum. Specifically, the insulating layer that has a function of suppressing the permeation of impurities and oxygen can be made of a metal oxide such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, or tantalum oxide, or a metal nitride such as aluminum nitride, silicon nitride oxide, or silicon nitride.
[0170] Specifically, examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide. Examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include oxides containing aluminum and hafnium (hafnium aluminate). Examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include metal nitrides such as aluminum nitride, aluminum titanium nitride, titanium nitride, silicon nitride oxide, and silicon nitride.
[0171] An insulating layer, such as a gate insulating layer, that is in contact with an oxide semiconductor layer or that is provided near the oxide semiconductor layer is preferably an insulating layer having a region containing oxygen that is released by heating (hereinafter, sometimes referred to as excess oxygen). For example, when an insulating layer having a region containing excess oxygen is in contact with an oxide semiconductor layer or is located near the oxide semiconductor layer, oxygen vacancies in the oxide semiconductor layer can be reduced. Examples of insulating layers that are likely to have a region containing excess oxygen include silicon oxide, silicon oxynitride, and silicon oxide having vacancies.
[0172] For example, an insulating layer having a region containing excess oxygen can be formed by sputtering in an oxygen-containing atmosphere. The hydrogen concentration in the insulating layer can be reduced by using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas.
[0173] Since the insulating layer 210 functions as an interlayer film, it is preferable that the insulating layer 210 has a low dielectric constant. By using a material with a low dielectric constant for the interlayer film, the parasitic capacitance generated between wirings can be reduced. Silicon oxide and silicon oxynitride are both thermally stable, and therefore are suitable for the insulating layer 210.
[0174] In addition, the concentration of impurities such as water and hydrogen in the insulating layer 210 is preferably reduced. This can prevent impurities such as water and hydrogen from entering the channel formation region of the semiconductor layer 230.
[0175] Furthermore, a barrier insulating layer against hydrogen is preferably used for the insulating layer 210. When the insulating layer 210 provided below the semiconductor layer 230 has a barrier property against hydrogen, diffusion of hydrogen into the semiconductor layer 230 can be suppressed.
[0176] Examples of materials for the barrier insulating layer against hydrogen include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide.
[0177] In this specification and the like, a barrier insulating layer refers to an insulating layer having barrier properties. The barrier properties are also referred to as a property that makes it difficult for a corresponding substance to diffuse (a property that makes it difficult for a corresponding substance to permeate, a property that the permeability of a corresponding substance is low, or a function that suppresses the diffusion of a corresponding substance). Note that hydrogen when described as a corresponding substance includes, for example, a hydrogen atom, a hydrogen molecule, a water molecule, and OH. − Furthermore, unless otherwise specified, impurities when described as corresponding substances refer to impurities in the channel formation region or semiconductor layer, and include, for example, hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, and nitrogen oxide molecules (N 2 O, NO, NO 2 The term "oxygen" refers to at least one of an oxygen atom, an oxygen molecule, etc., when described as a corresponding substance.
[0178] The insulating layer 210 preferably has a function of capturing or fixing hydrogen. Thus, hydrogen in the semiconductor layer 230 can be captured or fixed through the conductive layer 220 or the insulating layer 280, and the hydrogen concentration in the semiconductor layer 230 (particularly, the hydrogen concentration in the channel formation region of the transistor) can be reduced. Therefore, the V O By reducing H, the channel forming region can be made i-type or substantially i-type.
[0179] Examples of materials for insulating layers capable of capturing or adhering hydrogen include metal oxides such as oxides containing hafnium, oxides containing magnesium, oxides containing aluminum, and oxides containing aluminum and hafnium (hafnium aluminate). These metal oxides may further contain zirconium, such as oxides containing hafnium and zirconium. Metal oxides with an amorphous structure have dangling bonds in some oxygen atoms, which enhance their ability to capture or adsorb hydrogen. Therefore, these metal oxides preferably have an amorphous structure. For example, an amorphous structure may be achieved by including silicon in these oxides. For example, an oxide containing hafnium and silicon (hafnium silicate) is preferably used. Metal oxides may have crystalline regions and / or grain boundaries in some regions.
[0180] The ability to capture or fix a corresponding substance can also be said to have the property of making it difficult for the corresponding substance to diffuse. Therefore, the ability to capture or fix a corresponding substance can be rephrased as barrier properties.
[0181] For example, a silicon nitride film is preferably used for the insulating layer 210. Alternatively, for example, the insulating layer 210 can have a stacked structure of a silicon nitride film and an aluminum oxide film over the silicon nitride film.
[0182] It is preferable to use a barrier insulating layer against hydrogen for the insulating layer 280. When the insulating layer 280 has a barrier property against hydrogen, it is possible to prevent hydrogen contained in the structure located below the insulating layer 280 from diffusing into the semiconductor layer 230 via the insulating layer 250. For example, it is preferable to use a silicon nitride film for the insulating layer 210. By using a silicon nitride film for the insulating layer 210 that is in contact with the conductive layer 220, it is possible to prevent the conductive layer 220 from being oxidized.
[0183] The insulating layer 280 preferably has a low dielectric constant. By using a material with a low dielectric constant for the insulating layer 280, it is possible to reduce the parasitic capacitance that occurs between the conductive layer 220 and the conductive layer 260. Silicon oxide and silicon oxynitride are both thermally stable and therefore suitable for the insulating layer 280.
[0184] The insulating layer 281 preferably has a region containing excess oxygen. By using an insulating layer having a region containing excess oxygen for the insulating layer 281 provided near the semiconductor layer 230, oxygen can be supplied to the semiconductor layer 230, and oxygen vacancies and V in the semiconductor layer 230 can be reduced. O H can be reduced.
[0185] The concentrations of impurities such as water and hydrogen are preferably reduced in the insulating layers 280 and 281. This can prevent impurities such as water and hydrogen from entering the channel formation region of the semiconductor layer 230.
[0186] A barrier insulating layer against hydrogen is preferably used for the insulating layer 283. This can suppress diffusion of hydrogen from above the insulating layer 283 to the semiconductor layer 230. A silicon nitride film and a silicon nitride oxide film each have the characteristics of releasing little impurities (for example, water and hydrogen) from themselves and being less permeable to oxygen and hydrogen, and therefore can be suitably used for the insulating layer 283.
[0187] It is particularly preferable to use silicon nitride deposited by a sputtering method for the insulating layer 283. The sputtering method does not require the use of molecules containing hydrogen in the deposition gas, and therefore can reduce the hydrogen concentration in the insulating layer 283. Furthermore, by depositing the insulating layer 283 by a sputtering method, silicon nitride with high density can be formed.
[0188] Furthermore, an insulating layer having a function of capturing or fixing hydrogen can be used for the insulating layer 283. With such a structure, hydrogen can be prevented from diffusing from above the insulating layer 283 to the semiconductor layer 230, and hydrogen contained in the semiconductor layer 230 can be captured or fixed. Therefore, the hydrogen concentration in the semiconductor layer 230 can be reduced. Hafnium silicate or the like can be used for the insulating layer 283.
[0189] Alternatively, the insulating layer 283 may have a stacked structure of an insulating layer having a function of capturing or fixing hydrogen and a barrier insulating layer against hydrogen. For example, the insulating layer 283 may be a stacked film of aluminum oxide and silicon nitride over the aluminum oxide.
[0190] The insulating layer 250 preferably has a function of capturing or fixing hydrogen. This can reduce the hydrogen concentration in the semiconductor layer 230 (particularly, the hydrogen concentration in the channel formation region of the transistor). Therefore, the V O By reducing H, the channel forming region can be made i-type or substantially i-type.
[0191] For example, it is preferable to use an oxide containing one or both of aluminum and hafnium for the insulating layer 250, it is more preferable to use an oxide having an amorphous structure and containing one or both of aluminum and hafnium, and it is even more preferable to use aluminum oxide having an amorphous structure.
[0192] The insulating layer 250 is in contact with the semiconductor layer 230. When an oxide semiconductor is used for the semiconductor layer 230, the insulating layer 250 preferably has a region containing excess oxygen. When the insulating layer 250 has a region containing excess oxygen, oxygen vacancies in the semiconductor layer 230 can be reduced. In particular, silicon oxide, silicon oxynitride, or the like are insulating layers with a structure that is stable against heat, and therefore can be suitably used for the insulating layer 250.
[0193] The insulating layer 250 preferably has a barrier insulating layer against oxygen, which can prevent the conductive layer 260 from being oxidized. In addition, it can prevent oxygen contained in the semiconductor layer 230 from diffusing into the conductive layer 260 and forming oxygen vacancies in the semiconductor layer 230.
[0194] Examples of the barrier insulating layer against oxygen include oxides containing one or both of aluminum and hafnium, magnesium oxide, gallium oxide, gallium zinc oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide. Examples of oxides containing one or both of aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate).
[0195] It is preferable to use a high-k material for the insulating layer 250. An example of a high-k material is an oxide containing one or both of aluminum and hafnium. Using a high-k material for the insulating layer 250 makes it possible to reduce the gate potential applied during transistor operation while maintaining the physical thickness of the gate insulating layer. It also makes it possible to reduce the equivalent oxide thickness (EOT) of the insulating layer that functions as the gate insulating layer.
[0196] The thickness of the insulating layer 250 is preferably 0.1 nm or more and 30 nm or less, preferably 0.1 nm or more and 20 nm or less, preferably 0.1 nm or more and 10 nm or less, more preferably 0.1 nm or more and 5.0 nm or less, more preferably 0.5 nm or more and 5.0 nm or less, more preferably 1.0 nm or more and less than 5.0 nm, and even more preferably 1.0 nm or more and 3.0 nm or less.
[0197] 3A and 3B show an example in which the insulating layer 250 has a two-layer structure including an insulating layer 250a and an insulating layer 250b on the insulating layer 250a. The insulating layer 250a is located on the semiconductor layer 230 side, and the insulating layer 250b is located on the conductive layer 260 side.
[0198] The insulating layer 250a is preferably made of a material with a low dielectric constant. Silicon oxide or silicon oxynitride is preferably used as the material with a low dielectric constant. In this case, the insulating layer 250a contains at least silicon and oxygen. The insulating layer 250a is a layer in contact with the semiconductor layer 230. By using an oxide insulating layer for the insulating layer 250a, oxygen can be supplied to the semiconductor layer 230. Furthermore, by providing the insulating layer 250b, oxygen contained in the insulating layer 250a can be prevented from diffusing into the conductive layer 260, thereby preventing the conductive layer 260 from being oxidized. Furthermore, a decrease in the amount of oxygen supplied from the insulating layer 250a to the semiconductor layer 230 can be prevented.
[0199] The insulating layer 250a preferably has a function of capturing or fixing hydrogen. When the insulating layer 250a has the function of capturing or fixing hydrogen, the hydrogen contained in the semiconductor layer 230 can be captured or fixed. Therefore, the hydrogen concentration in the semiconductor layer 230 can be reduced. For example, hafnium silicate or the like can be used for the insulating layer 250a. Furthermore, the insulating layer 250a preferably has an amorphous structure.
[0200] By making the insulating layer 250a amorphous, it is possible to suppress the formation of crystal grain boundaries. By suppressing the formation of crystal grain boundaries, it is possible to improve the flatness of the insulating layer 250a. This makes the film thickness distribution of the insulating layer 250a uniform, and it is possible to reduce extremely thin film thickness portions, thereby improving the breakdown voltage of the insulating layer 250a. It is also possible to make the film thickness distribution of the film provided on the insulating layer 250a uniform.
[0201] Furthermore, by suppressing the formation of grain boundaries in the insulating layer 250a, it is possible to reduce leakage current caused by defect levels in the grain boundaries, and thus the insulating layer 250a can function as an insulating film with low leakage current.
[0202] Furthermore, since hafnium oxide is a high-k material, hafnium silicate can also be a high-k material depending on the silicon content. Therefore, when the insulating layer 250a is used as a gate insulating layer, it is possible to reduce the gate potential applied during transistor operation while maintaining the physical thickness of the gate insulating layer. Furthermore, it is possible to reduce the equivalent oxide thickness (EOT) of the gate insulating layer.
[0203] The insulating layer 250b preferably has a barrier insulating layer against hydrogen. By using a barrier insulating layer against hydrogen for the insulating layer 250b, it is possible to suppress diffusion of impurities contained in the conductive layer 260 into the semiconductor layer 230. Silicon nitride has a high barrier property against hydrogen and is therefore suitable for the insulating layer 250b. When silicon nitride is used for the insulating layer 250b, the insulating layer 250b contains silicon and nitrogen.
[0204] The insulating layer 250b preferably has a barrier insulating layer against oxygen, which can prevent the conductive layer 260 from being oxidized. In addition, it can prevent oxygen contained in the semiconductor layer 230 from diffusing into the conductive layer 260 and forming oxygen vacancies in the semiconductor layer 230.
[0205] With such a structure, a semiconductor device having good electrical characteristics, high reliability, little variation in the electrical characteristics of the transistors, and a large on-state current can be provided.
[0206] FIG. 4A also shows an example in which the insulating layer 250 has a three-layer structure including an insulating layer 250a, an insulating layer 250c on the insulating layer 250a, and an insulating layer 250b on the insulating layer 250c.
[0207] For example, it is preferable to use a material with a low relative dielectric constant for the insulating layer 250a and an insulating layer having the function of capturing or fixing hydrogen for the insulating layer 250c. Specifically, it is preferable to use silicon oxide for the insulating layer 250a and hafnium oxide for the insulating layer 250c. In this case, the insulating layer 250a contains silicon and oxygen, and the insulating layer 250c contains hafnium and oxygen. With this structure, oxygen can be supplied to the semiconductor layer 230. Furthermore, hydrogen contained in the semiconductor layer 230 can be captured or fixed.
[0208] Alternatively, for example, it is preferable to use an insulating layer having the function of capturing or fixing hydrogen as the insulating layer 250a, and to use a material with a low relative dielectric constant as the insulating layer 250c. Specifically, it is preferable to use hafnium oxide as the insulating layer 250a, and silicon oxide as the insulating layer 250c. In this case, the insulating layer 250a contains hafnium and oxygen, and the insulating layer 250c contains silicon and oxygen. With this structure, oxygen can be supplied to the semiconductor layer 230. Furthermore, hydrogen contained in the semiconductor layer 230 can be captured or fixed.
[0209] The insulating layer 250b can have the same structure as described above.
[0210] FIG. 4B also shows an example in which insulating layer 250 has a four-layer structure including insulating layer 250d, insulating layer 250a on insulating layer 250d, insulating layer 250c on insulating layer 250a, and insulating layer 250b on insulating layer 250c.
[0211] The above-described structures can be applied to the insulating layers 250a to 250c.
[0212] The insulating layer 250d preferably has a barrier property against oxygen. The insulating layer 250d is a layer in contact with the semiconductor layer 230. When the insulating layer 250d has a barrier property against oxygen, it is possible to suppress oxygen from being released from the semiconductor layer 230. For example, aluminum oxide can be used for the insulating layer 250d. In this case, the insulating layer 250d contains aluminum and oxygen. Aluminum oxide has the function of capturing or fixing hydrogen, and is therefore suitable as the insulating layer 250d in contact with the semiconductor layer 230.
[0213] To miniaturize the transistors, the insulating layers 250a to 250d preferably have thin film thicknesses. The insulating layers 250a to 250d each have a film thickness of preferably 0.1 nm to 10 nm, more preferably 0.1 nm to 5 nm, more preferably 0.5 nm to 5 nm, still more preferably 1 nm to less than 5 nm, and still more preferably 1 nm to 3 nm. Note that each of the insulating layers 250a to 250d may have a region with the above film thickness at least in part.
[0214] Typically, the thicknesses of the insulating layer 250d, the insulating layer 250a, the insulating layer 250c, and the insulating layer 250b are 1 nm, 2 nm, 2 nm, and 1 nm, respectively. With such a structure, the transistor can have good electrical characteristics even when miniaturized or highly integrated.
[0215] [Conductive Layer] The conductive layers (conductive layer 220, conductive layer 240, conductive layer 260, etc.) of the semiconductor device preferably contain a metal element selected from aluminum, chromium, copper, silver, gold, platinum, zinc, tantalum, nickel, titanium, iron, cobalt, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing the above-mentioned metal element as a component, or an alloy combining the above-mentioned metal elements. As the alloy containing the above-mentioned metal element as a component, a nitride of the alloy or an oxide of the alloy may be used. For example, tantalum nitride, titanium nitride, tungsten, a nitride containing titanium and aluminum, a nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, an oxide containing lanthanum and nickel, etc. are preferably used. Furthermore, semiconductors with high electrical conductivity, such as polycrystalline silicon containing impurity elements such as phosphorus, and silicides such as nickel silicide may also be used.
[0216] Nitrogen-containing conductive materials, such as nitrides containing tantalum, nitrides containing titanium, nitrides containing molybdenum, nitrides containing tungsten, nitrides containing ruthenium, nitrides containing tantalum and aluminum, or nitrides containing titanium and aluminum; oxygen-containing conductive materials, such as ruthenium oxide, oxides containing strontium and ruthenium, or oxides containing lanthanum and nickel; and materials containing metal elements, such as titanium, tantalum, or ruthenium, are preferred because they are conductive materials that are resistant to oxidation, have a function of suppressing oxygen diffusion, or maintain conductivity even after absorbing oxygen. Examples of oxygen-containing conductive materials include indium oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide (also referred to as ITO), indium tin oxide containing titanium oxide, indium tin oxide with added silicon (also referred to as ITSO), indium zinc oxide (also referred to as IZO®), and indium zinc oxide containing tungsten oxide. In this specification and the like, a conductive film formed using a conductive material containing oxygen may be referred to as an oxide conductive film.
[0217] Conductive materials based on tungsten, copper, or aluminum are preferred because they have high conductivity.
[0218] Furthermore, a plurality of conductive layers formed from the above materials may be stacked. For example, a stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing oxygen. A stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing nitrogen. A stacked structure may be formed by combining the above-described material containing a metal element, a conductive material containing oxygen, and a conductive material containing nitrogen.
[0219] When a metal oxide is used for the channel formation region of a transistor, the conductive layer that functions as a gate electrode preferably has a stacked structure that combines a material containing the metal element and a conductive material containing oxygen. In this case, the conductive material containing oxygen is preferably provided on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen desorbed from the conductive material is easily supplied to the channel formation region.
[0220] The conductive layer 220 and the conductive layer 240 are conductive layers in contact with the semiconductor layer 230, and therefore, it is preferable to use a conductive material that is resistant to oxidation, a conductive material that maintains low electrical resistance even when oxidized, an oxide conductive material, or a conductive material that has a function of suppressing oxygen diffusion. Examples of such conductive materials include a conductive material containing nitrogen and a conductive material containing oxygen. This can suppress a decrease in the conductivity of the conductive layer 220 and the conductive layer 240.
[0221] By using a conductive material containing oxygen for the conductive layer 220 or the conductive layer 240, the conductive layer 220 or the conductive layer 240 can maintain its conductivity even if it absorbs oxygen. In addition, even when an insulating layer containing oxygen, such as hafnium oxide, is used as the insulating layer 210, the conductive layer 220 is preferable because it can maintain its conductivity. For each of the conductive layer 220 and the conductive layer 240, it is preferable to use, for example, ITO, ITSO, IZO (registered trademark), or the like.
[0222] 3A and 3B show an example in which the conductive layer 220 has a two-layer structure including a conductive layer 220a and a conductive layer 220b on the conductive layer 220a. In this case, for example, it is preferable to use a highly conductive material for the conductive layer 220a and a conductive material containing oxygen for the conductive layer 220b. Specifically, it is preferable to use tungsten for the conductive layer 220a and ITO or ITSO for the conductive layer 220b. In this case, ITO or ITSO is in contact with the semiconductor layer 230. With this structure, the conductive layer 220 can maintain its conductivity even when in contact with the semiconductor layer 230. Furthermore, the use of highly conductive tungsten for the conductive layer 220a can increase the conductivity of the conductive layer 220.
[0223] 4A and 4B show an example in which the conductive layer 220 has a three-layer structure including a conductive layer 220c, a conductive layer 220a on the conductive layer 220c, and a conductive layer 220b on the conductive layer 220a.
[0224] The conductive layer 220a and the conductive layer 220b may have the same configuration as described above.
[0225] The conductive layer 220c is preferably made of a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion. Specifically, titanium nitride is preferably used for the conductive layer 220c. In this case, the titanium nitride is in contact with the insulating layer 210. With such a structure, when an oxide insulating layer is used for the insulating layer 210, the insulating layer 210 can suppress oxidation of the conductive layer 220.
[0226] 3A to 4B show an example in which the conductive layer 240 has a two-layer structure including a conductive layer 240a and a conductive layer 240b over the conductive layer 240a. In this case, for example, it is preferable to use a conductive material containing oxygen for the conductive layer 240a and a material having higher conductivity than the conductive layer 240a for the conductive layer 240b. Specifically, it is preferable to use ITO or ITSO for the conductive layer 240a and tungsten for the conductive layer 240b. In this case, ITO or ITSO is in contact with the semiconductor layer 230. With this structure, the conductive layer 240 can maintain conductivity even when in contact with the semiconductor layer 230. Furthermore, by using a material having higher conductivity than the conductive layer 240a for the conductive layer 240b, the conductivity of the conductive layer 240 can be increased.
[0227] It is preferable to use a highly conductive material such as tungsten for the conductive layer 260. It is also preferable to use a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion for the conductive layer 260. As described above, examples of such conductive materials include conductive materials containing nitrogen (e.g., titanium nitride or tantalum nitride) and conductive materials containing oxygen (e.g., ruthenium oxide). This can suppress a decrease in the conductivity of the conductive layer 260.
[0228] The conductive layer 260 is preferably made of a conductive material containing oxygen and a metal element contained in the metal oxide in which the channel is formed. Alternatively, the conductive material containing the above-mentioned metal element and nitrogen (e.g., titanium nitride, tantalum nitride, etc.) may be used. Alternatively, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide doped with silicon may be used. Alternatively, indium gallium zinc oxide containing nitrogen may be used. Using such a material may allow hydrogen contained in the metal oxide in which the channel is formed to be captured. Alternatively, hydrogen introduced from an outer insulating layer or the like may be captured.
[0229] The thickness of the conductive layer 260 is equal to or less than the channel length L of the transistor 200. The thickness of the conductive layer 260 can be, for example, 2 nm to 100 nm, 3 nm to 50 nm, or 5 nm to 30 nm.
[0230] 3A to 4B show an example in which the conductive layer 260 has a two-layer structure consisting of a conductive layer 260a and a conductive layer 260b on the conductive layer 260a. In this case, it is preferable to use titanium nitride for the conductive layer 260a and tungsten for the conductive layer 260b. This can increase the conductivity of the conductive layer 260.
[0231] [Substrate] Substrates on which transistors are formed can be, for example, insulating substrates, semiconductor substrates, or conductive substrates. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconia substrates (e.g., yttria-stabilized zirconia substrates), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon or germanium, or compound semiconductor substrates made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, and gallium oxide. Examples of semiconductor substrates include those having an insulating region within the semiconductor substrate, such as an SOI (Silicon-On-Insulator) substrate. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Other examples include substrates having a metal nitride or a metal oxide. Examples of other substrates include a substrate having a conductor or semiconductor provided on an insulating substrate, a substrate having a conductor or insulator provided on a semiconductor substrate, and a substrate having a semiconductor or insulator provided on a conductive substrate. Alternatively, a substrate provided with elements may be used, such as a capacitor element, a resistor element, a switch element, a light-emitting element, a memory element, and the like.
[0232] <Example of Manufacturing Method of Semiconductor Device> Next, a manufacturing method of a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. 5A to 10D . In FIGS. 5A to 9F , (A), (C), and (E) are cross-sectional views of the semiconductor device as viewed from the X direction, and (B), (D), and (F) are cross-sectional views of the semiconductor device as viewed from the Y direction. FIGS. 10A and 10C are cross-sectional views of the semiconductor device as viewed from the X direction, and FIGS. 10B and 10D are cross-sectional views of the semiconductor device as viewed from the Y direction. Note that the description of the materials and formation methods of each element that are the same as those previously described may be omitted.
[0233] Thin films (insulating films, semiconductor films, conductive films, etc.) constituting a semiconductor device can be formed by a sputtering method, a CVD method, a vacuum evaporation method, a PLD method, an ALD method, or the like.
[0234] Sputtering methods include RF sputtering, which uses a high-frequency power supply as the sputtering power source, DC sputtering, which uses a direct current power supply, and pulsed DC sputtering, which changes the voltage applied to the electrode in a pulsed manner. RF sputtering is mainly used to deposit insulating films, while DC sputtering is mainly used to deposit metal conductive films. Pulsed DC sputtering is mainly used to deposit films of compounds such as oxides, nitrides, and carbides using reactive sputtering.
[0235] CVD methods can be further classified into plasma-enhanced CVD (PECVD), which utilizes plasma, thermal CVD (TCVD), which utilizes heat, and photo-CVD (photo-CVD), which utilizes light. CVD methods can also be further classified into metal CVD (MCVD) and metal organic CVD (MOCVD), depending on the source gas used.
[0236] The plasma CVD method can produce high-quality films at relatively low temperatures. Furthermore, the thermal CVD method is a film formation method that can minimize plasma damage to the workpiece because it does not use plasma. For example, wiring, electrodes, elements (transistors, capacitors, etc.) included in a semiconductor device may become charged up by receiving electric charge from the plasma. In this case, the accumulated electric charge may destroy the wiring, electrodes, elements, etc. included in the semiconductor device. On the other hand, the thermal CVD method, which does not use plasma, does not cause such plasma damage, and therefore can increase the yield of semiconductor devices. Furthermore, the thermal CVD method does not cause plasma damage during film formation, so films with fewer defects can be obtained.
[0237] As the ALD method, a thermal ALD method in which a precursor and a reactant are reacted using only thermal energy, a PEALD method in which a plasma-excited reactant is used, or the like can be used.
[0238] The CVD and ALD methods differ from sputtering, in which particles emitted from a target or the like are deposited. Therefore, they are film formation methods that are less affected by the shape of the workpiece and have good step coverage. In particular, the ALD method has excellent step coverage and excellent thickness uniformity, making it suitable for coating the surfaces of openings with high aspect ratios. However, because the ALD method has a relatively slow film formation rate, it may be preferable to use it in combination with other film formation methods, such as the CVD method, which has a faster film formation rate.
[0239] Furthermore, the CVD method allows deposition of a film with any composition by adjusting the flow rate ratio of the source gases. For example, the CVD method allows deposition of a film with a continuously changing composition by changing the flow rate ratio of the source gases during deposition. When deposition is performed while changing the flow rate ratio of the source gases, the time required for deposition can be shortened compared to deposition using multiple deposition chambers because no time is required for transport or pressure adjustment. Therefore, the productivity of semiconductor devices can be improved in some cases.
[0240] Furthermore, in the ALD method, a film of any composition can be formed by simultaneously introducing multiple different precursors, or by controlling the number of cycles of each precursor when multiple different precursors are introduced.
[0241] Furthermore, thin films (insulating films, semiconductor films, conductive films, etc.) constituting the semiconductor device can be formed by a wet film formation method such as spin coating, dip coating, spray coating, inkjet printing, dispensing, screen printing, offset printing, doctor knife method, slit coating, roll coating, curtain coating, or knife coating.
[0242] Furthermore, when processing a thin film that constitutes a semiconductor device, a photolithography method or the like can be used. Alternatively, the thin film may be processed by a nanoimprint method, a sandblasting method, a lift-off method, or the like. Furthermore, an island-shaped thin film may be directly formed by a film formation method using a shielding mask such as a metal mask.
[0243] There are two typical photolithography methods: one is to form a resist mask on the thin film to be processed, process the thin film by etching or the like, and then remove the resist mask; the other is to form a photosensitive thin film, and then process the thin film into the desired shape by exposure and development.
[0244] In photolithography, the light used for exposure may be, for example, i-line (wavelength 365 nm), g-line (wavelength 436 nm), h-line (wavelength 405 nm), or a mixture of these. Other light sources that can be used include ultraviolet light, KrF laser light, ArF laser light, etc. Exposure may also be performed by immersion exposure technology. Extreme ultraviolet (EUV) light or X-rays may also be used as the light used for exposure. An electron beam may also be used instead of the light used for exposure. Extreme ultraviolet light, X-rays, or an electron beam are preferred because they enable extremely fine processing. When exposure is performed by scanning a beam such as an electron beam, a photomask is not required.
[0245] For etching the thin film, dry etching, wet etching, sandblasting, or the like can be used.
[0246] First, as shown in FIGS. 5A and 5B, an insulating layer 210 is formed on a substrate (not shown), and a conductive layer 220 is formed on the insulating layer 210. As shown in FIG.
[0247] 5C and 5D , a semiconductor film 230F is formed on the insulating layer 210 and the conductive layer 220. The semiconductor film 230F is preferably formed by sputtering. High crystallinity of the semiconductor layer 230 suppresses diffusion of impurities in the semiconductor layer 230, making it difficult for the electrical characteristics of the transistor to fluctuate and improving reliability. When the semiconductor film 230F is formed by sputtering, it is easier to form a layer with high crystallinity than when an ALD method is used.
[0248] When the semiconductor film 230F is formed by sputtering, oxygen or a mixed gas of oxygen and a noble gas is used as the sputtering gas. By increasing the proportion of oxygen contained in the sputtering gas, the amount of excess oxygen in the semiconductor film to be formed can be increased. In addition, a sputtering target such as the above-mentioned In-M-Zn oxide can be used.
[0249] The sputtering gas is preferably highly purified. For example, oxygen gas, nitrogen gas, or argon gas used as the sputtering gas is purified to a dew point of −40° C. or less, preferably −80° C. or less, more preferably −100° C. or less, and more preferably −120° C. or less, thereby preventing moisture and the like from being taken into the metal oxide film as much as possible.
[0250] When the semiconductor film 230F is formed by a sputtering method, an oxygen-excessive oxide semiconductor is formed when the percentage of oxygen contained in the sputtering gas is set to more than 30% and less than or equal to 100%, preferably 70% to 100%. A transistor using an oxygen-excessive oxide semiconductor for a channel formation region can have relatively high reliability. However, one embodiment of the present invention is not limited thereto. When the semiconductor film 230F is formed by a sputtering method, an oxygen-deficient oxide semiconductor is formed when the percentage of oxygen contained in the sputtering gas is set to 1% to 30%, preferably 5% to 20%. A transistor using an oxygen-deficient oxide semiconductor for a channel formation region can have relatively high field-effect mobility. Furthermore, by performing film formation while heating the substrate, the crystallinity of the oxide film can be improved.
[0251] The film thickness of the semiconductor film 230F corresponds to the height of the above-mentioned semiconductor layer 230. Therefore, it is preferable that the semiconductor film 230F is provided so that the film thickness falls within the above-mentioned range.
[0252] As shown in FIGS. 3A to 4B , when the semiconductor layer 230 has a three-layer structure of semiconductor layer 230a, semiconductor layer 230b, and semiconductor layer 230c, the semiconductor film 230F can be formed in this order as a first semiconductor film that becomes semiconductor layer 230a, a second semiconductor film that becomes semiconductor layer 230b, and a third semiconductor film that becomes semiconductor layer 230c.
[0253] The method for forming the second semiconductor film can refer to the method for forming the semiconductor film 230F described above.
[0254] When nitrogen-doped metal oxide films are formed by sputtering as the first and third semiconductor films, the nitrogen-doped metal oxide films can be formed even if the sputtering target does not contain nitrogen by including nitrogen gas in the sputtering gas. When the nitrogen gas is added to form the metal oxide films, the carrier mobility of the metal oxide films can be increased as the nitrogen flow rate ratio increases.
[0255] The nitrogen flow rate ratio can be appropriately set within a range of 10% to 100% depending on the characteristics desired for the semiconductor layer 230a and the semiconductor layer 230c. In this case, for example, the sputtering gas can be a mixed gas of nitrogen gas and argon gas. The sputtering gas may also be a mixed gas of nitrogen gas and oxygen gas, or a mixed gas of nitrogen gas, oxygen gas, and argon gas.
[0256] When a target containing nitrogen is used as the target, even when a metal oxide film containing nitrogen is formed, nitrogen may not be used as the sputtering gas.
[0257] It is preferable that the first semiconductor film, the second semiconductor film, and the third semiconductor film are successively formed without exposure to the atmosphere. For example, a multi-chamber film forming apparatus can be used. By forming the films without exposure to the atmosphere, impurities or moisture from the atmospheric environment can be prevented from adhering to the first semiconductor film and the second semiconductor film, and the interface between the first semiconductor film and the second semiconductor film and the vicinity thereof, and the interface between the second semiconductor film and the third semiconductor film and the vicinity thereof can be kept clean.
[0258] In a case where nitrogen-doped metal oxide films are formed by sputtering as the first and third semiconductor films, and a metal oxide film is formed by sputtering as the second semiconductor film, the second semiconductor film is formed by switching the type of gas introduced into the sputtering apparatus, i.e., stopping the introduction of nitrogen, after the first semiconductor film is formed. Furthermore, the third semiconductor film is formed by switching the type of gas introduced into the sputtering apparatus, i.e., introducing nitrogen, after the second semiconductor film is formed. This makes it possible to form the first, second, and third semiconductor films consecutively, which is suitable for mass production.
[0259] In this embodiment, as the semiconductor film 230F, a metal oxide film is formed by sputtering using an oxide target with an atomic ratio of In:Ga:Zn = 4:2:4.1, an oxide target with an atomic ratio of In:Ga:Zn = 1:1:1, an oxide target with an atomic ratio of In:Ga:Zn = 1:1:1.2, or an oxide target with an atomic ratio of In:Ga:Zn = 1:1:2. When the semiconductor film 230F has a three-layer structure, metal oxide films doped with nitrogen are formed by sputtering as the first and third semiconductor films, and the above metal oxide film is formed as the second semiconductor film. Note that each semiconductor film can be formed to suit the characteristics desired for the semiconductor layers 230a, 230b, and 230c by appropriately selecting the film formation conditions and atomic ratios.
[0260] Next, heat treatment is preferably performed. The heat treatment may be performed within a temperature range in which the semiconductor film 230F does not become polycrystallized, such as 250° C. to 650° C., preferably 400° C. to 600° C. Note that the heat treatment is performed in a nitrogen gas or inert gas atmosphere, or an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more. For example, when the heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas concentration can be set to about 20%. The heat treatment may also be performed under reduced pressure. Alternatively, after the heat treatment in the nitrogen gas or inert gas atmosphere, the heat treatment may be performed in an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more to compensate for the desorbed oxygen.
[0261] Furthermore, it is preferable that the gas used in the heat treatment be highly purified. For example, the amount of moisture contained in the gas used in the heat treatment can be set to 1 ppb or less, preferably 0.1 ppb or less, and more preferably 0.05 ppb or less. By performing the heat treatment using a highly purified gas, it is possible to prevent moisture and the like from being taken into the semiconductor film 230F as much as possible.
[0262] In this embodiment, the heat treatment is performed at a temperature of 400° C. for one hour with a flow rate ratio of nitrogen gas to oxygen gas of 4:1. This heat treatment using oxygen gas can reduce impurities such as carbon, water, and hydrogen in the semiconductor film 230F. Reducing the impurities in the film in this manner improves the crystallinity of the semiconductor film 230F, resulting in a denser, more compact structure. This increases the crystalline region in the semiconductor film 230F, reducing the in-plane variation of the crystalline region in the semiconductor film 230F. Therefore, the in-plane variation of the electrical characteristics of the transistor can be reduced.
[0263] 5C and 5D , an insulating film 271F is formed on the semiconductor film 230F. The insulating film 271F is preferably an insulating film that has a function of suppressing oxygen permeation. For example, the insulating film 271F is preferably a silicon nitride film, an aluminum oxide film, a silicon oxide film, or the like, formed by a sputtering method. Even when the mask 272 described later is formed using a tungsten film that is easily oxidized, the insulating film 271F has a function of suppressing oxygen permeation, thereby suppressing oxygen contained in the semiconductor film 230F from diffusing into the mask 272 and forming oxygen vacancies in the semiconductor film 230F.
[0264] 5C and 5D, a mask 272 is formed on the insulating film 271F. When the cylindrical semiconductor layer 230 is formed using the mask 272, the mask 272 is preferably circular in plan view.
[0265] The mask 272 is preferably made of a material with a low etch selectivity relative to the workpiece (here, the semiconductor film 230F). For example, if the etch rate of the semiconductor film 230F is 1, the etch rate of the material used for the mask 272 is preferably 0.5 or less, and more preferably 0.1 or less. Specifically, the mask 272 can be made of a metal material or an inorganic insulating material. More specifically, a tungsten film formed by sputtering can be used. Note that the mask 272 can be made of, for example, a molybdenum film or a titanium film. This configuration maintains the shape of the hard mask during etching, preventing the workpiece from being deformed. The material of the hard mask can be appropriately selected depending on the workpiece. Furthermore, the etch rate varies depending on conditions (also referred to as etching conditions) such as source power, bias power, etching gas flow rate, etching gas type, and pressure. Therefore, the etching conditions can be appropriately selected depending on the hard mask and the workpiece.
[0266] 5E and 5F, a mask 272 is used to process a portion of the insulating film 271F and a portion of the semiconductor film 230F until the upper surfaces of the conductive layer 220 and the insulating layer 210 are exposed. This processing can be performed by dry etching or wet etching. Dry etching is suitable for microfabrication. The insulating film 271F and the semiconductor film 230F may be processed under different conditions.
[0267] The above processing forms an insulating layer 271 and a semiconductor layer 230 whose shapes (outline) in a plan view are the same as or approximately the same as the shape of the mask 272 in a plan view. That is, in a plan view, the end of the insulating layer 271 and the end of the semiconductor layer 230 coincide or approximately coincide. Furthermore, each of the insulating layer 271 and the semiconductor layer 230 has a cylindrical shape. Therefore, the above processing forms a cylindrical semiconductor layer 230 on the conductive layer 220. As described above, the semiconductor layer 230 is preferably formed so that its height is greater than the width of its lower surface. Note that the semiconductor layer 230 can also be formed so that its height is the same as or smaller than the width of its lower surface.
[0268] The above processing may cause impurities to adhere to the side surfaces of the semiconductor layer 230 or diffuse into the interior of the semiconductor layer 230. A step of removing such impurities may be performed. Furthermore, the above processing may cause damaged regions to be formed on the surface of the semiconductor layer 230. Such damaged regions may be removed. Examples of such impurities include those originating from components contained in the insulating film 271F, components contained in the components of the equipment used in the above processing, and components contained in the gas or liquid used in etching. Examples of such impurities include hafnium, aluminum, silicon, tantalum, fluorine, and chlorine.
[0269] In particular, impurities such as silicon may reduce the crystallinity of the semiconductor layer 230. Therefore, it is preferable to remove the impurities from the surface of the semiconductor layer 230 and its vicinity. It is also preferable to reduce the concentration of the impurities. For example, the concentration of silicon atoms in the surface of the semiconductor layer 230 and its vicinity is preferably 5.0 atomic % or less, more preferably 2.0 atomic % or less, more preferably 1.5 atomic % or less, even more preferably 1.0 atomic % or less, and even more preferably less than 0.3 atomic %.
[0270] In addition, due to the impurities, the density of the crystal structure is reduced in the region of low crystallinity of the semiconductor layer 230. O A large amount of H is formed, which makes it easier for the transistor 200 to become normally on. Therefore, it is preferable that the region with low crystallinity in the semiconductor layer 230 be reduced or removed.
[0271] It is preferable to perform a cleaning treatment in order to remove impurities and the like that have adhered to the surface of the semiconductor layer 230 during the above processing. Examples of cleaning methods include wet cleaning using a cleaning solution or the like (also referred to as wet etching treatment), plasma treatment using plasma, and the like, and the above cleaning methods may be combined as appropriate.
[0272] Wet cleaning may be performed using an aqueous solution of one or more of ammonia water, oxalic acid, phosphoric acid, and hydrofluoric acid diluted with carbonated water or pure water, pure water, carbonated water, etc. Alternatively, ultrasonic cleaning may be performed using these aqueous solutions, pure water, or carbonated water. Alternatively, these cleaning methods may be combined as appropriate.
[0273] In this specification and the like, an aqueous solution obtained by diluting hydrofluoric acid with pure water may be referred to as diluted hydrofluoric acid, and an aqueous solution obtained by diluting ammonia water with pure water may be referred to as diluted ammonia water. The concentration, temperature, etc. of the aqueous solution are adjusted appropriately depending on the impurities to be removed and the configuration of the semiconductor device to be cleaned. The ammonia concentration of the diluted ammonia water is preferably 0.01% or more and 5% or less, and more preferably 0.1% or more and 0.5% or less. The hydrogen fluoride concentration of the diluted hydrofluoric acid is preferably 0.01 ppm or more and 100 ppm or less, and more preferably 0.1 ppm or more and 10 ppm or less.
[0274] Note that ultrasonic cleaning preferably uses a frequency of 200 kHz or more, and more preferably a frequency of 900 kHz or more, because use of such a frequency can reduce damage to the semiconductor layer 230 and the like.
[0275] The cleaning process may be performed multiple times, and the cleaning solution may be changed for each cleaning process. For example, the first cleaning process may be performed using diluted hydrofluoric acid or diluted ammonia water, and the second cleaning process may be performed using pure water or carbonated water.
[0276] As the cleaning treatment, for example, wet cleaning is performed using diluted hydrofluoric acid. By performing this cleaning treatment, it is possible to remove impurities that have adhered to the surface of the semiconductor layer 230 or that have diffused into the interior of the semiconductor layer 230. Furthermore, it is possible to remove portions of the semiconductor layer 230 with low crystallinity and improve the crystallinity of the entire semiconductor layer 230.
[0277] A heat treatment may be performed after the above processing or after the above cleaning. The above-mentioned contents can be referred to for the heat treatment. The heat treatment may be performed under reduced pressure. Alternatively, after the heat treatment in an oxygen atmosphere, the heat treatment may be performed in a nitrogen atmosphere without exposure to the air. By performing the heat treatment, oxygen can be supplied to the semiconductor layer 230, thereby reducing oxygen vacancies. Furthermore, the crystallinity of the semiconductor layer 230 can be improved. Furthermore, the hydrogen in the semiconductor layer 230 reacts with the supplied oxygen to convert the hydrogen into H 2 O can be removed (dehydrated).
[0278] Note that the heat treatment may not be performed. For example, when a tungsten film that is easily oxidized is used as the conductive layer 220, the heat treatment may not be performed. This can prevent the conductive layer 220 from being oxidized by the heat treatment.
[0279] 6A and 6B , an insulating layer 280 is formed on the insulating layer 210, the conductive layer 220, and the mask 272. For example, silicon nitride or silicon oxide can be used for the insulating layer 280. By using silicon nitride, which has a barrier property against hydrogen, as the insulating layer 280, it is possible to prevent hydrogen contained in the structure located below the insulating layer 280 from diffusing into the semiconductor layer 230 via the insulating layer 250 to be formed later. Furthermore, by using silicon oxide, which has a low relative dielectric constant, as the insulating layer 280, it is possible to reduce the parasitic capacitance generated between the conductive layer 220 and the conductive layer 260 to be formed later.
[0280] Next, as shown in FIGS. 6C and 6D, planarization treatment (also referred to as CMP treatment) using a chemical mechanical polishing (CMP) method is performed to planarize the top surface of the insulating layer 280.
[0281] 6E and 6F, a thinning treatment is performed to reduce the thickness of the insulating layer 280. The thinning treatment may be dry etching, wet etching, or a combination of both. Such uniform etching and planarization is also called an etch-back treatment. By performing the thinning treatment to reduce the thickness of the insulating layer 280, part of the side surface of the semiconductor layer 230 is exposed.
[0282] 7A and 7B, the mask 272 is removed. The mask 272 can be removed by wet etching or dry etching. By removing the mask 272 while the insulating layer 271 remains, damage to the semiconductor layer 230 when the mask 272 is removed can be reduced. Furthermore, by removing the mask 272, the CMP process to be performed later can be facilitated.
[0283] Next, as shown in FIGS. 7C and 7D, an insulating layer 250 and a conductive layer 260 are formed in this order on the insulating layer 280 and the insulating layer 271 .
[0284] The insulating layer 250 is formed in contact with the semiconductor layer 230 having a large aspect ratio. Therefore, the insulating layer 250 is preferably formed by a film formation method with good coverage, and more preferably by a CVD method, an ALD method, or the like.
[0285] The conductive layer 260 is formed in contact with the insulating layer 250 having protrusions with a large aspect ratio. Therefore, the conductive layer 260 is preferably formed by a film formation method with good coverage, and more preferably by a CVD method, an ALD method, or the like.
[0286] 7E and 7F, a resist 273 is formed on the conductive layer 260. The resist 273 can be formed, for example, by forming a resist film, exposing the resist film through a mask, and removing the exposed region using a developer or leaving it.
[0287] 8A and 8B , a thinning treatment is performed to thin the resist 273. The thinning treatment may be performed by ashing using oxygen plasma or the like. By thinning the resist 273 through the thinning treatment, a part of the conductive layer 260 is exposed. At this time, the thickness of the resist 273 is thinned so that the top surface of the resist 273 is located lower than the top surface of the semiconductor layer 230 (closer to the insulating layer 210).
[0288] Next, as shown in Figures 8C and 8D, a portion of the conductive layer 260 is removed. Specifically, the region of the conductive layer 260 exposed from the resist 273 is removed. A dry etching method or a wet etching method can be used to remove the portion of the conductive layer 260. Processing using the dry etching method is suitable for fine processing. As a result of this processing, the upper surface of the portion of the conductive layer 260 that is along the side surface of the semiconductor layer 230 is positioned lower (closer to the insulating layer 210) than the upper surface of the semiconductor layer 230. In addition, the upper surface of the insulating layer 250 in the region that does not overlap with the resist 273 and the conductive layer 260 is exposed.
[0289] Next, as shown in FIGS. 8E and 8F, the resist 273 is removed.
[0290] 9A and 9B , an insulating layer 281 is formed on the insulating layer 250 and the conductive layer 260. For example, silicon oxide can be used for the insulating layer 281. By using silicon oxide, which has a low relative dielectric constant, as the insulating layer 281, it is possible to reduce parasitic capacitance that occurs between the conductive layer 240 and the conductive layer 260, which will be formed later. Furthermore, silicon oxide can be easily processed by a CMP process, which will be described later, and therefore can be suitably used for the insulating layer 281.
[0291] 9C and 9D , CMP treatment is performed to expose the top surfaces of the semiconductor layer 230 and the insulating layer 250. At this time, the insulating layer 271 is removed. The CMP treatment is performed so that the top surface of the conductive layer 260 is not exposed. By performing the CMP treatment, the surface on which the conductive layer 240 to be formed later is to be formed can be flattened, and discontinuity of the conductive layer 240, which functions as a wiring, can be suppressed.
[0292] Note that since the insulating layer 281 and the mask 272 are made of different materials, it is difficult to simultaneously remove the mask 272 by the CMP process. Therefore, it is preferable to remove the mask 272 in advance, as described with reference to Figures 7A and 7B. Note that if the pattern density of the mask 272 is low, it is possible to remove it by the CMP process, and therefore the step of removing the mask 272 described with reference to Figures 7A and 7B does not need to be performed.
[0293] In this specification, the pattern density refers to the area ratio of the structure formed in an arbitrary region. For example, when a conductive film is formed over the entire surface of an arbitrary region, the pattern density is 100%. On the other hand, when a portion of the conductive film is removed to form multiple conductive layers, the pattern density of the conductive layers can be calculated by dividing the area of the remaining conductive layer by the area of the arbitrary region.
[0294] Note that the method for exposing the upper surface of the semiconductor layer 230 is not limited to the above. For example, after forming the insulating layer 281, the upper surface of the insulating layer 271 may be exposed by performing CMP treatment, and the upper surface of the semiconductor layer 230 may be exposed by removing the insulating layer 271. In this case, the upper surface of the semiconductor layer 230 is located lower than the upper surface of the insulating layer 281 (on the insulating layer 210 side).
[0295] 9E and 9F , an insulating layer 282 is formed over the insulating layer 250, the conductive layer 260, and the insulating layer 281. The insulating layer 282 can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, or an ALD method. The insulating layer 282 is preferably formed by a sputtering method. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating layer 282 can be reduced.
[0296] The insulating layer 282 is preferably an insulating layer containing a large amount of oxygen. Thus, oxygen contained in the insulating layer 282 can be supplied to the semiconductor layer 230 during deposition of the insulating layer 282 and by heat treatment or the like after deposition, thereby reducing oxygen vacancies in the semiconductor layer 230. Furthermore, oxygen contained in the insulating layer 282 can be supplied to the semiconductor layer 230 through the insulating layer 281, thereby reducing oxygen vacancies in the semiconductor layer 230. Thus, the transistor 200 can have favorable electrical characteristics and reliability.
[0297] For example, the insulating layer 282 is formed by pulsed DC sputtering using an aluminum target in an atmosphere containing oxygen gas. By using pulsed DC sputtering, the film thickness distribution can be made more uniform, and the sputtering rate and film quality can be improved. In addition, the RF power applied to the substrate is 1.86 W / cm. 2 Preferably, 0 W / cm 2 0.62W / cm or more 2 The RF power is set to 0 W / cm or less. 2This is synonymous with not applying RF power to the substrate. The amount of oxygen implanted into layers below the insulating layer 282 can be controlled by the magnitude of the RF power applied to the substrate. For example, the smaller the RF power, the smaller the amount of oxygen implanted into layers below the insulating layer 282, and the more likely the amount of oxygen is saturated even if the insulating layer 282 is thin. Furthermore, the larger the RF power, the greater the amount of oxygen implanted into layers below the insulating layer 282. By reducing the RF power, the amount of oxygen implanted into the semiconductor layer 230 can be suppressed.
[0298] The RF frequency is preferably 10 MHz or higher, typically 13.56 MHz. The higher the RF frequency, the less damage can be caused to the substrate.
[0299] Furthermore, by depositing the insulating layer 282 in an oxygen-containing atmosphere by a sputtering method, oxygen can be added to the semiconductor layer 230 during deposition. Furthermore, excess oxygen can be contained in the insulating layer 281. At this time, the insulating layer 282 is preferably deposited while heating the substrate.
[0300] Note that heat treatment may be performed before the insulating layer 282 is formed. The heat treatment may be performed under reduced pressure, and the insulating layer 282 may be formed successively without exposure to air. By performing such treatment, moisture and hydrogen adsorbed on the surface of the insulating layer 281 can be removed and the moisture and hydrogen concentrations in the insulating layer 281 can be further reduced. The temperature of the heat treatment is preferably 100° C. or higher and 400° C. or lower. For example, the temperature of the heat treatment is 250° C.
[0301] 10A and 10B , the insulating layer 282 is removed. Dry etching, wet etching, or CMP can be used to remove the insulating layer 282. By this removal, the top surfaces of the semiconductor layer 230, the insulating layer 250, and the insulating layer 281 are exposed.
[0302] 9E to 10B , a process using an ion implantation method, an ion doping method, a plasma immersion ion implantation method, a plasma treatment, or the like may be performed, which can supply oxygen to the semiconductor layer 230 and reduce oxygen vacancies in the semiconductor layer 230.
[0303] 9E to 10B can be omitted if the oxygen vacancies in the semiconductor layer 230 are sufficiently reduced, which makes it possible to reduce the number of steps, reduce production costs, and improve productivity.
[0304] 9E to 10B may be performed after forming the insulating layer 280 (see FIGS. 6A and 6B) or after planarizing the top surface of the insulating layer 280 (see FIGS. 6C and 6D). This allows oxygen to be supplied to the semiconductor layer 230, thereby reducing oxygen vacancies in the semiconductor layer 230. This allows the transistor 200 to have favorable electrical characteristics and reliability.
[0305] Next, as shown in FIGS. 10C and 10D, a conductive layer 240 is formed over the semiconductor layer 230, the insulating layer 250, and the insulating layer 281.
[0306] Next, the insulating layer 283 is formed over the insulating layer 281 and the conductive layer 240 .
[0307] Through the above steps, a semiconductor device of one embodiment of the present invention can be manufactured.
[0308] 11A to 11C , another structure of a semiconductor device according to one embodiment of the present invention will be described. Fig. 11A is a plan view of the semiconductor device. Fig. 11B is a cross-sectional view of the semiconductor device corresponding to the portion indicated by the dashed dotted line along A1-A2 in Fig. 11A . Fig. 11C is a cross-sectional view of the semiconductor device corresponding to the portion indicated by the dashed dotted line along A3-A4 in Fig. 11A .
[0309] 11A to 11C differ from the semiconductor device shown in Figures 2A to 2C in that it has semiconductor layers 231 and 232. In the following, differences from the above content will be mainly explained, and overlapping parts will be referred to and explanations thereof may be omitted.
[0310] The semiconductor device shown in Figures 11A to 11C includes an insulating layer 210 on a substrate (not shown), a transistor 200A on the insulating layer 210, a layer 232, an insulating layer 280, an insulating layer 281 on the insulating layer 280, and an insulating layer 283 on the transistor 200A.
[0311] The transistor 200A includes a conductive layer 220, a semiconductor layer 230 and a semiconductor layer 231 over the conductive layer 220, an insulating layer 250 over the insulating layer 280, a conductive layer 260 over the insulating layer 250, and a conductive layer 240 over the semiconductor layer 230, the insulating layer 250, and the insulating layer 281. The transistor 200A differs from the transistor 200 in that the transistor 200A includes the semiconductor layer 231.
[0312] The side surface of the semiconductor layer 230 is in contact with the semiconductor layer 231. In other words, the semiconductor layer 231 covers the side surface of the semiconductor layer 230. At least a portion of the side surface of the semiconductor layer 230 is covered by the insulating layer 250 via the semiconductor layer 231, and another portion of the side surface of the semiconductor layer 230 is covered by the insulating layer 280 via the semiconductor layer 231. In other words, the insulating layer 250 covers at least a portion of the side surface of the semiconductor layer 231, and the insulating layer 280 covers another portion of the side surface of the semiconductor layer 231. The insulating layer 250 and the semiconductor layer 231 each have a region in contact with the conductive layer 240.
[0313] 11D is an enlarged cross-sectional view in the XY plane including the semiconductor layer 230, the semiconductor layer 231, the insulating layer 250, the conductive layer 260, and the insulating layer 281. As shown in FIG. 11D, the semiconductor layer 231, the insulating layer 250, and the conductive layer 260 are provided concentrically.
[0314] The composition of the semiconductor layer 231 may be the same as, or approximately the same as, or different from, the composition of the semiconductor layer 230. For example, by making the composition of the semiconductor layer 231 the same as or approximately the same as the composition of the semiconductor layer 230, the channel width of the transistor can be increased, and the on-state current of the transistor can be increased.
[0315] When the composition of the semiconductor layer 231 and the composition of the semiconductor layer 230 are different, the band gap of the semiconductor layer 231 is preferably larger than the band gap of the semiconductor layer 230. Covering the semiconductor layer 230 with the semiconductor layer 231 having a larger band gap than the semiconductor layer 230 allows for a buried channel configuration. This allows the semiconductor layer 230 to serve as the main current path. Furthermore, covering the semiconductor layer 230 with the semiconductor layer 231 reduces trap levels at the interface and in the vicinity of the interface of the semiconductor layer 230. This allows for a transistor with a large on-current and high reliability. Therefore, a semiconductor device that achieves both high-speed operation and high reliability can be achieved. As an example, the atomic ratio of In to the element M in the semiconductor layer 230 is preferably larger than the atomic ratio of In to the element M in the semiconductor layer 231.
[0316] Furthermore, the atomic ratio of the element M to In in the semiconductor layer 231 is preferably larger than the atomic ratio of the element M to In in the semiconductor layer 230. With this configuration, it is possible to suppress the diffusion of impurities from structures formed outside the semiconductor layer 231 into the semiconductor layer 230.
[0317] 11A to 11C , a layer 232 is provided on a side surface of the conductive layer 220. As will be described in detail later, the layer 232 is formed in the step of forming the semiconductor layer 231. Therefore, the layer 232 has the same material as the semiconductor layer 231.
[0318] A method for manufacturing the semiconductor device shown in Figures 11A to 11C will be described with reference to Figures 12A to 12F. Figures 12A, 12C, and 12E are cross-sectional views of the semiconductor device as viewed from the X direction, and Figures 12B, 12D, and 12F are cross-sectional views of the semiconductor device as viewed from the Y direction.
[0319] The manufacturing method up to the formation of the semiconductor layer 230 can be explained using the contents described with reference to FIGS. 5A to 5F, and therefore detailed description thereof will be omitted.
[0320] Next, as shown in FIGS. 12A and 12B, a semiconductor film 231F is formed over the insulating layer 210, the conductive layer 220, and the mask 272.
[0321] The semiconductor film 231F is formed in contact with the semiconductor layer 230 having a large aspect ratio. Therefore, the semiconductor film 231F is preferably formed using a film formation method with good coverage, and more preferably using a CVD method, an ALD method, or the like.
[0322] The semiconductor film 231F preferably has crystallinity. The crystallinity of the semiconductor film 231F can suppress oxygen from being released from the side surface of the semiconductor layer 230, and can suppress the formation of oxygen vacancies in the semiconductor layer 230. Furthermore, the incorporation of impurities from the side surface of the semiconductor layer 230 can be suppressed.
[0323] When a CAAC-OS is used for the semiconductor layer 231, the crystals of the semiconductor layer 231 are c-axis oriented with respect to a surface where the semiconductor layer 231 is formed. For example, the crystals in the vicinity of the side surfaces of the semiconductor layer 230 are c-axis oriented with respect to the side surfaces of the semiconductor layer 230. Note that when a CAAC-OS is used for the semiconductor layer 230, the c-axis of the crystals of the semiconductor layer 230 is perpendicular to the c-axis of the crystals of the semiconductor layer 231.
[0324] When a metal oxide film is formed using the ALD method, elements contained in the precursor and reactant other than those constituting the metal oxide film can become impurities in the metal oxide film. Examples of elements other than those constituting the metal oxide film include hydrogen, carbon, nitrogen, and chlorine. If excess precursor, excess reactant, reaction products, etc. are not sufficiently discharged from the chamber during metal oxide film formation, the concentration of impurities such as hydrogen, carbon, nitrogen, and chlorine in the metal oxide film may increase. The higher the impurity concentration, the lower the crystallinity of the metal oxide film tends to be.
[0325] After forming a metal oxide film using the ALD method, it is preferable to perform, for example, a microwave treatment. Furthermore, after forming a metal oxide film using the ALD method, it is more preferable to perform a microwave treatment continuously without exposing the film to the atmosphere. Note that the microwave treatment is preferably performed in an oxygen-containing atmosphere.
[0326] By performing microwave treatment in an oxygen-containing atmosphere, oxygen gas can be converted into plasma using high-frequency waves such as microwaves and RF, and the oxygen plasma can be applied to the metal oxide. At this time, high-frequency waves such as microwaves and RF can also be irradiated onto the metal oxide. In other words, high-frequency waves such as microwaves and RF, oxygen plasma, etc. can be applied to the metal oxide.
[0327] The impurity concentration of the metal oxide can be reduced by the action of high frequency, oxygen plasma, etc. For example, hydrogen in the metal oxide can be desorbed as water molecules. In addition, for example, carbon in the metal oxide can be converted into carbon oxides (CO and / or CO 2 In addition, oxygen radicals generated by oxygen plasma are supplied to the metal oxide, and oxygen vacancies in the metal oxide, V O H etc. can be reduced.
[0328] Furthermore, the action of high frequency, oxygen plasma, etc. provides atoms in the metal oxide with energy at or above the processing temperature of microwave treatment. This promotes rearrangement of metal atoms and oxygen atoms in the metal oxide, improving the crystallinity of the metal oxide. In addition, the impurity concentration and defects (oxygen deficiency, V O The crystallinity of the metal oxide tends to improve as the amount of oxygen (H, etc.) is reduced. In other words, microwave treatment in an oxygen-containing atmosphere reduces the impurity concentration and defect amount in the metal oxide and improves the crystallinity of the metal oxide.
[0329] As described above, by performing microwave treatment in an oxygen-containing atmosphere, the impurity concentration and the amount of defects in the metal oxide can be reduced. Furthermore, the rearrangement of metal atoms and oxygen atoms in the metal oxide can be promoted. Therefore, the crystallinity of the metal oxide is improved, and a metal oxide having a CAAC structure can be formed. In other words, the metal oxide has a crystalline region that is approximately parallel to the normal vector of the surface on which the metal oxide is formed or the normal vector of the surface of the metal oxide.
[0330] The oxygen-containing atmosphere may be, for example, oxygen gas and a noble gas (argon, helium, krypton, etc.). When oxygen gas and argon gas are used as the oxygen-containing atmosphere, the ratio of the flow rate of oxygen gas to the sum of the flow rates of oxygen gas and argon gas is called the oxygen flow rate ratio (O 2 / (O 2 +Ar)). 2 / O 2 The oxygen flow ratio (O + Ar) can be greater than 0% and less than 100%, preferably greater than 0% and less than 50%, more preferably greater than 10% and less than 40%, and even more preferably greater than 10% and less than 30%. In addition, when oxygen gas and helium gas or krypton gas are used as the oxygen-containing atmosphere, the oxygen flow ratio (O 2 / (O 2 + He) or O 2 / (O 2 +Kr)) can be greater than 0% and less than 100%, preferably greater than 0% and less than 50%, more preferably 10% to 40%, and even more preferably 10% to 30%.
[0331] The microwave treatment is preferably carried out under reduced pressure, for example, at a pressure of 10 Pa or more and 1000 Pa or less, and preferably at a pressure of 300 Pa or more and 700 Pa or less.
[0332] The microwave treatment is not limited to being performed after forming a metal oxide film using the ALD method. The microwave treatment may be performed, for example, during the process of forming a metal oxide film using the ALD method. That is, the set may be repeated once or multiple times, followed by the microwave treatment, and then the set may be repeated once or multiple times. The microwave treatment may be performed once or multiple times during the process of forming a metal oxide film using the ALD method.
[0333] 12C and 12D, the semiconductor film 231F is processed using anisotropic etching to expose a portion of the upper surface of the mask 272, a portion of the upper surface of the conductive layer 220, and a portion of the upper surface of the insulating layer 210. This allows the formation of a sidewall-shaped semiconductor layer 231 that covers the side surfaces of the semiconductor layer 230, the side surfaces of the insulating layer 271, and the side surfaces of the mask 272. Note that the above processing may result in the formation of a layer 232 on the side surface of the conductive layer 220. The above anisotropic etching is preferably anisotropic dry etching. Processing using dry etching is preferable because it is suitable for fine processing.
[0334] 12E and 12F, an insulating layer 280 is formed over the insulating layer 210 and the conductive layer 220. Note that for the method of forming the insulating layer 280, the contents described with reference to FIGS. 6A to 6F can be referred to.
[0335] For the manufacturing method after the insulating layer 280 is formed, the contents described with reference to FIGS. 7A to 10D can be referred to, and therefore detailed description thereof will be omitted.
[0336] In this manner, the semiconductor device shown in FIGS. 11A to 11C can be manufactured.
[0337] <Structural Example 3 of Semiconductor Device> Another structure of a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. 13A to 13D.
[0338] Fig. 13A is a cross-sectional view of the semiconductor device as viewed from the X direction. Fig. 13B is a cross-sectional view of the semiconductor device as viewed from the Y direction. Note that Fig. 2A can be referred to for plan views of the semiconductor device shown in Figs. 13A and 13B.
[0339] 13A and 13B differs from the semiconductor device shown in Figures 2A to 2C in that it does not have an insulating layer 280. Hereinafter, differences from the above content will be mainly described, and overlapping parts will be referred to and may not be described again.
[0340] The semiconductor device shown in Figures 13A and 13B has an insulating layer 210 on a substrate (not shown), a transistor 200B on the insulating layer 210, an insulating layer 281 on the insulating layer 210, and an insulating layer 283 on the transistor 200B.
[0341] The transistor 200B shown in Figures 13A and 13B includes a conductive layer 220, a semiconductor layer 230 on the conductive layer 220, an insulating layer 250 on the insulating layer 210 and the conductive layer 220, a conductive layer 260 on the insulating layer 250, and a conductive layer 240 on the semiconductor layer 230, the insulating layer 250, and the insulating layer 281.
[0342] The insulating layer 250 has a region in contact with the upper surface of the insulating layer 210 , a region in contact with the side and upper surface of the conductive layer 220 , a region in contact with the side of the semiconductor layer 230 , and a region in contact with the upper surface of the conductive layer 240 .
[0343] If the parasitic capacitance generated between the conductive layer 260 and the conductive layer 220 can be reduced by increasing the thickness of the insulating layer 250, it is possible to adopt a configuration in which the insulating layer 280 is not provided, as shown in Figures 13A and 13B. By adopting such a configuration, the step of forming the insulating layer 280 can be omitted. Therefore, productivity can be improved by reducing the number of steps.
[0344] Fig. 13C is a cross-sectional view of the semiconductor device as viewed from the X direction. Fig. 13D is a cross-sectional view of the semiconductor device as viewed from the Y direction. Note that Fig. 2A can be referred to for plan views of the semiconductor device shown in Figs. 13C and 13D.
[0345] 2A to 2C in that the semiconductor device shown in Figures 13C and 13D does not have an insulating layer 280, but has an insulating layer 285. Hereinafter, differences from the above content will be mainly described, and overlapping portions will be referred to and may not be described again.
[0346] The semiconductor device shown in Figures 13C and 13D has an insulating layer 210 on a substrate (not shown), a transistor 200B on the insulating layer 210, an insulating layer 285 on the insulating layer 210, an insulating layer 281 on the insulating layer 285, and an insulating layer 283 on the transistor 200B.
[0347] The transistor 200B shown in Figures 13C and 13D includes a conductive layer 220, a semiconductor layer 230 on the conductive layer 220, an insulating layer 250 on the insulating layer 285 and the conductive layer 220, a conductive layer 260 on the insulating layer 250, and a conductive layer 240 on the semiconductor layer 230, the insulating layer 250, and the insulating layer 281.
[0348] The conductive layer 220 is provided by being embedded in an opening formed in the insulating layer 285. Note that a portion of the conductive layer 220 may be embedded in the insulating layer 210. The height of the upper surface of the conductive layer 220 is the same as the height of the upper surface of the insulating layer 285.
[0349] The insulating layer 285 can be formed using an insulating material that can be used for the insulating layer 280. By providing the insulating layer 285, the surface on which the semiconductor film 230F is to be formed can be flattened. Therefore, the thickness distribution of the semiconductor film 230F can be made uniform, and the characteristics of the transistor 200B can be improved.
[0350] The insulating layer 285 and the conductive layer 220 can be formed by, for example, forming the insulating layer 285, forming an opening in the insulating layer 285, forming a conductive film to be the conductive layer 220, and performing CMP treatment until the top surface of the insulating layer 285 is exposed. Alternatively, the insulating layer 285 may be formed by performing the etch-back treatment described with reference to FIGS. 6E and 6F until the top surface of the conductive layer 220 is exposed.
[0351] <Structural Example 4 of Semiconductor Device> Another structure of a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. 14A and 14B. FIG. 14A is a cross-sectional view of the semiconductor device as seen from the X direction. FIG. 14B is a cross-sectional view of the semiconductor device as seen from the Y direction. Note that FIG. 2A can be referred to for plan views of the semiconductor device illustrated in FIGS. 14A and 14B.
[0352] 14A and 14B differs from the semiconductor device shown in Figures 2B and 2C in that the conductive layer 260 is formed so as to have a uniform film thickness. Hereinafter, differences from the above content will be mainly described, and overlapping portions will be referred to and may not be described again.
[0353] The semiconductor device shown in Figures 14A and 14B has an insulating layer 210 on a substrate (not shown), a transistor 200C on the insulating layer 210, an insulating layer 280, an insulating layer 281 on the insulating layer 280, and an insulating layer 283 on the transistor 200C.
[0354] The transistor 200C has a conductive layer 220, a semiconductor layer 230 on the conductive layer 220, an insulating layer 250 on the insulating layer 280, a conductive layer 260 on the insulating layer 250, and a conductive layer 240 on the semiconductor layer 230, the insulating layer 250, and the insulating layer 281.
[0355] The conductive layer 260 is formed so that the film thickness of the conductive layer 260 is approximately uniform in the direction (X direction) in which the conductive layer 260 extends. With this configuration, the conductivity of the conductive layer 260, which functions as a wiring, can be increased.
[0356] 15A to 16F, a method for manufacturing the semiconductor device shown in Fig. 14A and Fig. 14B will be described. In each figure, (A), (C), and (E) are cross-sectional views of the semiconductor device as seen from the X direction, and (B), (D), and (F) are cross-sectional views of the semiconductor device as seen from the Y direction.
[0357] The manufacturing method up to the formation of the insulating layer 250 can be referred to the contents described with reference to FIGS. 5A to 7D, and therefore detailed description thereof will be omitted.
[0358] 15A and 15B , a conductive layer 260 is formed on the insulating layer 250. The conductive layer 260 is formed in contact with the insulating layer 250, which has protrusions with a large aspect ratio. Therefore, the conductive layer 260 is preferably formed using a film formation method with good coverage, and more preferably, a CVD method, an ALD method, or the like.
[0359] When the conductive layer 260 has a stacked structure, the first conductive film in contact with the insulating layer 250 is preferably formed by the above-described CVD method, ALD method, or the like. The conditions for forming the second conductive film on the first conductive film are not particularly limited. For example, the second conductive film may be formed by a sputtering method, a CVD method, or the like, which has a faster film formation rate than the ALD method. This allows the semiconductor device to be manufactured with high productivity.
[0360] Next, as shown in FIGS. 15C and 15D, a CMP process is performed to flatten the upper surface of the conductive layer 260.
[0361] 15E and 15F, a thinning treatment (etch-back treatment) is performed to reduce the thickness of the conductive layer 260. The thinning treatment may be an etching treatment using one or both of dry etching and wet etching. By performing the thinning treatment to reduce the thickness of the conductive layer 260, part of the top surface of the insulating layer 250 is exposed. At this time, the thickness of the conductive layer 260 is reduced so that the top surface of the conductive layer 260 is located lower than the top surface of the semiconductor layer 230 (closer to the insulating layer 210).
[0362] 16A and 16B, a resist 273 is formed on the conductive layer 260. The method for forming the resist 273 can be described with reference to the contents explained with reference to FIGS. 7E and 7F, and therefore detailed explanation thereof will be omitted.
[0363] 16C and 16D, a portion of the conductive layer 260 is removed. Specifically, the region of the conductive layer 260 that is exposed from the resist 273 is removed. A dry etching method or a wet etching method can be used to remove the portion of the conductive layer 260. Processing using the dry etching method is suitable for fine processing. By this processing, the upper surface of the insulating layer 250 in the region that does not overlap with the resist 273 is exposed.
[0364] Next, as shown in FIGS. 16E and 16F, the resist 273 is removed.
[0365] For the manufacturing method after removing the resist 273, the contents explained using FIGS. 9A to 10D can be referred to, and therefore detailed explanation will be omitted.
[0366] In this manner, the semiconductor device shown in FIGS. 14A and 14B can be manufactured.
[0367] <Structure Example 5 of Semiconductor Device> Another structure of a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. 17A to 17D.
[0368] Fig. 17A is a cross-sectional view of the semiconductor device as viewed from the X direction. Fig. 17B is a cross-sectional view of the semiconductor device as viewed from the Y direction. Note that Fig. 2A can be referred to for plan views of the semiconductor device shown in Figs. 17A and 17B.
[0369] 17A and 17B differs from the semiconductor device shown in Figures 2B and 2C in that it has an insulating layer 275. In the following, differences from the above content will be mainly explained, and overlapping parts will be referred to and explanations thereof may be omitted.
[0370] The semiconductor device shown in Figures 17A and 17B has an insulating layer 210 on a substrate (not shown), a transistor 200D on the insulating layer 210, an insulating layer 275 on the insulating layer 210, an insulating layer 281 on the insulating layer 275, and an insulating layer 283 on the transistor 200D.
[0371] The transistor 200D shown in Figures 17A and 17B includes a conductive layer 220, a semiconductor layer 230 on the conductive layer 220, an insulating layer 250 on the insulating layer 210 and the conductive layer 220, a conductive layer 260 on the insulating layer 250, and a conductive layer 240 on the semiconductor layer 230, the insulating layer 250, the insulating layer 275, and the insulating layer 281.
[0372] The insulating layer 275 is provided to cover the conductive layer 260. The insulating layer 275 is provided between the insulating layer 281 and the insulating layer 250 and conductive layer 260. The insulating layer 275 has a region in contact with the upper surface and side surfaces of the insulating layer 250, a region in contact with the side surfaces and upper surface of the conductive layer 260, a region in contact with the lower surface of the insulating layer 281, and a region in contact with the lower surface of the conductive layer 240.
[0373] It is preferable to use a barrier insulating layer against hydrogen for the insulating layer 275. When the insulating layer 275 provided on the outside of the semiconductor layer 230 has a barrier property against hydrogen, it is possible to suppress diffusion of hydrogen into the semiconductor layer 230. For example, silicon nitride or the like can be used for the insulating layer 275.
[0374] Furthermore, a barrier insulating layer against oxygen can be used for the insulating layer 275. By providing the insulating layer 275 between the insulating layer 281 and the conductive layer 260, the conductive layer 260 can be prevented from being oxidized and the resistance of the conductive layer 260 can be prevented from increasing.
[0375] Furthermore, an insulating layer having a function of capturing or fixing hydrogen can be used as the insulating layer 275. With such a structure, diffusion of hydrogen from above the insulating layer 275 to the semiconductor layer 230 can be suppressed, and further, hydrogen contained in the semiconductor layer 230 can be captured or fixed. Therefore, the hydrogen concentration in the semiconductor layer 230 can be reduced. For example, magnesium oxide, aluminum oxide, hafnium oxide, or an oxide containing hafnium and silicon can be used for the insulating layer 275.
[0376] 17C and 17D , when the insulating layer 250 has a stacked structure of an insulating layer 250a and an insulating layer 250b on the insulating layer 250a, the conductive layer 260 is surrounded by the insulating layer 275 and the insulating layer 250b. By using barrier insulating layers against oxygen as the insulating layer 275 and the insulating layer 250b, it is possible to prevent the conductive layer 260 from being oxidized.
[0377] A method for manufacturing the semiconductor device shown in Figures 17A and 17B will be described with reference to Figures 18A to 18D. Figures 18A and 18C are cross-sectional views of the semiconductor device as seen from the X direction, and Figures 18B and 18D are cross-sectional views of the semiconductor device as seen from the Y direction.
[0378] The manufacturing method up to the removal of the resist 273 can be explained using the contents explained with reference to FIGS. 5A to 8F, and therefore detailed explanation will be omitted.
[0379] Next, as shown in FIGS. 18A and 18B, an insulating layer 275 and an insulating layer 281 are formed in this order over the insulating layer 250 and the conductive layer 260.
[0380] The insulating layer 275 is formed in contact with the protrusions having a large aspect ratio. Therefore, the insulating layer 275 is preferably formed by a film formation method with good coverage, and more preferably by a CVD method, an ALD method, or the like. For example, the insulating layer 275 is preferably formed of silicon nitride by a PEALD method.
[0381] The method for forming the insulating layer 281 can be described with reference to FIGS. 9A and 9B, and therefore detailed description thereof will be omitted.
[0382] 18C and 18D , CMP treatment is performed to expose the top surfaces of the semiconductor layer 230, the insulating layer 250, and the insulating layer 275. At this time, the CMP treatment is performed so as not to expose the top surface of the conductive layer 260. Note that by performing the CMP treatment, the surface on which the conductive layer 240, which functions as a wiring, is formed can be flattened, and discontinuity of the conductive layer 240 can be suppressed.
[0383] Regarding the manufacturing method after the CMP process, the contents explained with reference to FIGS. 9E to 10D can be referred to, and therefore detailed explanation will be omitted.
[0384] In this manner, the semiconductor device shown in FIGS. 17A and 17B can be manufactured.
[0385] <Modifications of Semiconductor Device> Modifications of the semiconductor device shown in FIGS. 2A to 2C will be described with reference to FIGS. 19A to 19D.
[0386] 2B and 2C, the semiconductor layer 230 is provided so that the side surface of the semiconductor layer 230 is perpendicular to the upper surface of the insulating layer 210, but the present invention is not limited to this. For example, as shown in FIGS. 19A and 19B, the side surface of the semiconductor layer 230 can be tapered. In this case, the semiconductor layer 230 has a truncated cone shape. Note that FIG. 2A can be referred to for plan views of the semiconductor device shown in FIGS. 19A and 19B.
[0387] As shown in FIGS. 19A and 19B , tapering the side surface of the semiconductor layer 230 improves the coverage of the insulating layer 250 and the conductive layer 260, thereby reducing defects such as voids. When tapering the side surface of the semiconductor layer 230, for example, the angle θ between the side surface of the semiconductor layer 230 and the top surface of the insulating layer 210 is preferably 45 degrees or greater and less than 90 degrees. Specifically, as described above, a semiconductor device can be miniaturized or highly integrated when the angle θ is 80 degrees or greater and less than 90 degrees, which is preferable. Furthermore, when the angle θ is 45 degrees or greater and less than 80 degrees, 45 degrees or greater and less than 75 degrees, 50 degrees or greater and less than 75 degrees, 50 degrees or greater and less than 70 degrees, 50 degrees or greater and less than 65 degrees, or 50 degrees or greater and less than 60 degrees, the coverage of the film formed on the side surface of the semiconductor layer 230 is improved, which is preferable.
[0388] In this specification, etc., the cylindrical shape also includes a truncated cone shape in which the angle θ is equal to or greater than 80 degrees and less than 90 degrees. In addition, in this specification, etc., the cylindrical shape also includes a case in which the shape in plan view is a substantially circular shape such as an ellipse.
[0389] 19A and 19B , when the side surface of the semiconductor layer 230 is tapered, the channel length L of the transistor 200 is determined by the height of the conductive layer 260 and the angle θ. The width D of the semiconductor layer 230 varies in the depth direction. In this specification and the like, the width D of the semiconductor layer 230 is particularly defined as the width of the bottom surface of the semiconductor layer 230 on the conductive layer 220 side. In other words, the maximum width of the semiconductor layer 230 is defined as the width D of the semiconductor layer 230.
[0390] 2B and 2C show a configuration in which the top surface of the conductive layer 220 is flat, but the present invention is not limited to this. For example, as shown in FIGS. 19C and 19D , the conductive layer 220 may have different thicknesses in the region that overlaps with the semiconductor layer 230 and the region that does not overlap with the semiconductor layer 230. For example, when processing the semiconductor layer 230, a portion of the conductive layer 220 may be removed, making the thickness of the region that does not overlap with the semiconductor layer 230 thinner than the thickness of the overlapping region. If the film thickness of the region of the insulating layer 280 that does not overlap with the conductive layer 220 shown in FIGS. 2B and 2C is the same as the film thickness of the region of the insulating layer 280 that does not overlap with the conductive layer 220 shown in FIGS. 19C and 19D , the configuration shown in FIGS. 19C and 19D can increase the physical distance between the conductive layer 220 and the conductive layer 260, thereby reducing the parasitic capacitance generated between the conductive layer 220 and the conductive layer 260. Note that FIG. 2A can be referred to for plan views of the semiconductor device shown in FIGS. 19C and 19D.
[0391] This embodiment mode can be combined with other embodiment modes as appropriate. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be combined as appropriate.
[0392] 20A to 26 , 28A, and 28E , a memory device of one embodiment of the present invention will be described. The memory device of one embodiment of the present invention includes a memory cell. The memory cell includes a transistor and a capacitor.
[0393] 20A to 20D , a structure of a memory device including a transistor and a capacitor will be described. Fig. 20A is a cross-sectional view of the memory device as viewed from the X direction. Fig. 20B is a cross-sectional view of the memory device as viewed from the Y direction.
[0394] 20A and 20B includes an insulating layer 140 over a substrate (not shown), a conductive layer 110 over the insulating layer 140, a memory cell 150 over the conductive layer 110, an insulating layer 180 over the conductive layer 110, an insulating layer 181 over the insulating layer 180, an insulating layer 280 over the insulating layer 181, an insulating layer 281 over the insulating layer 280, and an insulating layer 283 over the memory cell 150. The insulating layer 140, the insulating layer 180, the insulating layer 181, the insulating layer 280, the insulating layer 281, and the insulating layer 283 function as interlayer films. The conductive layer 110 functions as a wiring.
[0395] The memory cell 150 includes a capacitor 100 over a conductive layer 110 and a transistor 200 over the capacitor 100 .
[0396] The capacitor 100 includes a conductive layer 115 on the conductive layer 110, an insulating layer 130 on the conductive layer 115, and a conductive layer 120 on the insulating layer 130. In the capacitor 100, the conductive layer 120 functions as one of a pair of electrodes (sometimes referred to as an upper electrode), the conductive layer 115 functions as the other of the pair of electrodes (sometimes referred to as a lower electrode), and the insulating layer 130 functions as a dielectric. That is, the capacitor 100 constitutes a metal-insulator-metal (MIM) capacitor.
[0397] As shown in FIGS. 20A and 20B , an opening 190 is provided in the insulating layer 180, reaching the conductive layer 110. At least a portion of the conductive layer 115 is disposed in the opening 190. Note that the conductive layer 115 has a region in contact with the top surface of the conductive layer 110 in the opening 190, a region in contact with the side surface of the insulating layer 180 in the opening 190, and a region in contact with at least a portion of the top surface of the insulating layer 180. At least a portion of the insulating layer 130 is disposed in the opening 190. At least a portion of the conductive layer 120 is disposed in the opening 190. Note that, as shown in FIGS. 20A and 20B , the conductive layer 120 is preferably provided so as to fill the opening 190. Note that the film provided in the opening 190 is preferably formed using a CVD method or an ALD method, respectively. This improves the coverage of the film. For example, the conductive layer 115, the insulating layer 130, and the conductive layer 120 are preferably formed by a CVD method or an ALD method.
[0398] The capacitor 100 has a configuration in which the upper electrode and the lower electrode face each other across a dielectric not only on the bottom surface but also on the side surface of the opening 190, allowing for a larger capacitance per unit area. Therefore, the deeper the opening 190, the larger the capacitance of the capacitor 100 can be. Increasing the capacitance per unit area of the capacitor 100 in this way can stabilize the read operation of the memory device. Furthermore, this can promote miniaturization or high integration of memory devices.
[0399] 20A and 20B show an example in which the sidewall of the opening 190 is perpendicular to the top surface of the conductive layer 110. In this case, the opening 190 has a cylindrical shape. With such a structure, miniaturization or high integration of the memory device can be achieved.
[0400] A conductive layer 115 and an insulating layer 130 are stacked along the sidewall of the opening 190 and the upper surface of the conductive layer 110. A conductive layer 120 is provided on the insulating layer 130 so as to fill the opening 190. The capacitor element 100 having such a configuration may be called a trench capacitor or a trench capacitor.
[0401] An insulating layer 181 is disposed over the insulating layer 180. The conductive layer 120 and the insulating layer 181 preferably have flat top surfaces. Planarizing the top surfaces of the conductive layer 120 and the insulating layer 181 facilitates subsequent steps and can increase the yield of memory devices.
[0402] An insulating layer 280 is disposed on the capacitor element 100. That is, the insulating layer 280 is disposed on the insulating layer 181 and the conductive layer 120.
[0403] The insulating layers 180 and 181 preferably have a low dielectric constant because they function as interlayer films. By using a material with a low dielectric constant as the interlayer film, parasitic capacitance occurring between wirings can be reduced. As the insulating layers 180 and 181, insulating layers containing a material with a low dielectric constant can be used in a single layer or stacked layers. Silicon oxide and silicon oxynitride are preferable because they are thermally stable.
[0404] 20A and 20B, the insulating layer 180 and the insulating layer 181 are shown as single layers, but the present invention is not limited to this. The insulating layer 180 may have a stacked structure of two layers, or a stacked structure of three or more layers. The insulating layer 181 may have a stacked structure of two or more layers.
[0405] The transistor 200 includes a conductive layer 120 (corresponding to the conductive layer 220 in FIG. 2B , etc.), a semiconductor layer 230 over the conductive layer 120, an insulating layer 250 over the insulating layer 280, a conductive layer 260 over the insulating layer 250, and a conductive layer 240 over the semiconductor layer 230, the insulating layer 250, and the insulating layer 281. In the transistor 200, the semiconductor layer 230 functions as a semiconductor layer, the conductive layer 260 functions as a gate electrode, the insulating layer 250 functions as a gate insulating layer, the conductive layer 120 functions as one of a source electrode and a drain electrode, and the conductive layer 240 functions as the other of the source electrode and the drain electrode.
[0406] The detailed description of the transistor 200 is omitted here because the description in Embodiment 1 (FIGS. 1A to 10D) can be referred to. The transistor included in the memory cell 150 is not limited to the transistor 200, and any of the transistors 200A to 200D illustrated in Embodiment 1 can be used.
[0407] As shown in FIGS. 20A and 20B , the transistor 200 is provided to overlap with the capacitor 100. The semiconductor layer 230 of the transistor 200 has a region overlapping with the opening 190 where part of the structure of the capacitor 100 is provided. In particular, the conductive layer 120 functions as one of the source electrode and drain electrode of the transistor 200 and as the upper electrode of the capacitor 100. Therefore, the transistor 200 and the capacitor 100 share part of their structures. With this structure, the transistor 200 and the capacitor 100 can be provided without significantly increasing the occupied area in a plan view. This reduces the occupied area of the memory cell 150, thereby enabling the memory cells 150 to be arranged at a high density and increasing the storage capacity of the storage device. In other words, the storage device can be highly integrated.
[0408] Furthermore, by providing the transistor 200 above the capacitor 100, the transistor 200 is not affected by heat treatment during manufacturing of the capacitor 100. Therefore, in the transistor 200, deterioration of electrical characteristics such as a change in threshold voltage and an increase in parasitic resistance, as well as an increase in variation in electrical characteristics due to the deterioration of the electrical characteristics, can be suppressed.
[0409] 28A shows a circuit diagram of the memory device described in this embodiment. As shown in FIG. 28A, the configuration shown in FIGS. 20A and 20B functions as a memory cell. The memory cell 951 includes a transistor M1 and a capacitor CA. Here, the transistor M1 corresponds to the transistor 200, and the capacitor CA corresponds to the capacitor 100.
[0410] One of the source and drain of the transistor M1 is connected to one of a pair of electrodes of the capacitor CA. The other of the source and drain of the transistor M1 is connected to a wiring BIL. The gate of the transistor M1 is connected to a wiring WOL. The other of the pair of electrodes of the capacitor CA is connected to a wiring CAL.
[0411] Here, the wiring BIL corresponds to the conductive layer 240 , the wiring WOL corresponds to the conductive layer 260 , and the wiring CAL corresponds to the conductive layer 110 .
[0412] As shown in Figures 20A and 20B, it is preferable that the conductive layer 260 extends in the X direction, and the conductive layer 240 extends in the Y direction. With this configuration, the wiring BIL and the wiring WOL are arranged to intersect with each other. Also, in Figure 20A, the wiring CAL (conductive layer 110) is arranged parallel to the wiring BIL (conductive layer 240), but the present invention is not limited to this. For example, the wiring CAL may be arranged parallel to the wiring WOL (conductive layer 260), or may be arranged in a planar shape.
[0413] The memory cells will be described in detail in a later embodiment.
[0414] [Capacitor 100] The capacitor 100 includes a conductive layer 115, an insulating layer 130, and a conductive layer 120. The conductive layer 110 is provided below the conductive layer 115. The conductive layer 115 has a region in contact with the conductive layer 110.
[0415] The conductive layer 110 is provided on the insulating layer 140. The conductive layer 110 functions as a wiring CAL and can be provided extending in the Y direction, for example. The conductive layer 110 can be formed as a single layer or a stacked layer using the conductive material described in the section [Conductive Layer] of Embodiment 1. For example, a conductive material with high conductivity, such as tungsten, can be used for the conductive layer 110. By using such a conductive material with high conductivity, the conductivity of the conductive layer 110 can be improved, allowing it to function sufficiently as a wiring CAL.
[0416] The conductive layer 115 is preferably formed using a single layer or a stacked layer of a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion. For example, titanium nitride or indium tin oxide to which silicon is added may be used. Alternatively, for example, a structure in which titanium nitride is stacked over tungsten may be used. Alternatively, for example, a structure in which tungsten is stacked over a first titanium nitride and a second titanium nitride is stacked over the tungsten may be used. With such a structure, when an oxide insulating layer is used for the insulating layer 130, the insulating layer 130 can suppress oxidation of the conductive layer 110. Furthermore, when an oxide insulating layer is used for the insulating layer 180, the insulating layer 180 can suppress oxidation of the conductive layer 110.
[0417] The insulating layer 130 is provided over the conductive layer 115. The insulating layer 130 is provided so as to be in contact with the top surface of the conductive layer 115. It is preferable that the side edges of the insulating layer 130 coincide with the side edges of the conductive layer 115. With this structure, the insulating layer 130 and the conductive layer 115 can be formed using the same mask, which can simplify the manufacturing process of the memory device.
[0418] 20C and 20D, the insulating layer 130 can cover the conductive layer 110. This can prevent the conductive layer 115 and the conductive layer 120 from shorting out.
[0419] It is preferable to use a material with a high relative dielectric constant (high-k) for the insulating layer 130. By using a high-k material for the insulating layer 130, the insulating layer 130 can be made thick enough to suppress leakage current, and the capacitance of the capacitive element 100 can be sufficiently ensured.
[0420] Furthermore, the insulating layer 130 is preferably formed by stacking insulating layers made of high-k materials, and preferably by using a stack structure of a material with a high dielectric constant (high-k) and a material with a higher dielectric strength than the high-k material. For example, the insulating layer 130 can be formed by stacking zirconium oxide, aluminum oxide, and zirconium oxide in this order. Alternatively, the insulating layer 130 can be formed by stacking zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide in this order. Alternatively, the insulating layer 130 can be formed by stacking hafnium zirconium oxide, aluminum oxide, hafnium zirconium oxide, and aluminum oxide in this order. Using stacked insulating layers with a relatively high dielectric strength, such as aluminum oxide, improves the dielectric strength and suppresses electrostatic breakdown of the capacitor element 100.
[0421] Furthermore, a material that can have ferroelectricity can be used for the insulating layer 130. For details of the material that can have ferroelectricity, refer to the description in Embodiment 1.
[0422] Metal oxides containing one or both of hafnium and zirconium can have ferroelectricity even when the thickness is as thin as a few nanometers, and are therefore preferable as the insulating layer 130. The film thickness of the insulating layer 130 is preferably 100 nm or less, more preferably 50 nm or less, even more preferably 20 nm or less, and even more preferably 10 nm or less (typically, 2 nm to 9 nm). Furthermore, for example, the film thickness is preferably 8 nm to 12 nm. By using a ferroelectric layer that can be thinned, the capacitor element 100 can be combined with a semiconductor element such as a miniaturized transistor to form a semiconductor device.
[0423] Furthermore, a metal oxide containing one or both of hafnium and zirconium can have ferroelectricity even in a small area, and is therefore preferable as the insulating layer 130. For example, when the area (occupied area) of the ferroelectric layer in a plan view is 100 μm 2 Below, 10μm 2 Below, 1μm 2 or less than 0.1 μm 2 Even if the thickness is less than 10,000 nm, the film can still have ferroelectricity. 2 or less than 1000 nm 2 Even if the thickness is less than 100 Å, the ferroelectric layer may have ferroelectricity. By using a ferroelectric layer with a small area, the area occupied by the capacitor element 100 can be reduced.
[0424] A ferroelectric material is an insulator that generates polarization internally when an external electric field is applied, and the polarization remains even when the electric field is removed. Therefore, a nonvolatile memory element can be formed using a capacitor element (hereinafter sometimes referred to as a ferroelectric capacitor) that uses this material as a dielectric. A nonvolatile memory element using a ferroelectric capacitor is sometimes called a Ferroelectric Random Access Memory (FeRAM), a ferroelectric memory, or the like. For example, a ferroelectric memory includes a transistor and a ferroelectric capacitor, and one of the source and drain of the transistor is electrically connected to one terminal of the ferroelectric capacitor. Therefore, when a ferroelectric capacitor is used as the capacitor element 100, the memory device described in this embodiment functions as a ferroelectric memory.
[0425] The conductive layer 120 is provided in contact with the upper surface of the insulating layer 130. It is preferable that the side edges of the conductive layer 120 coincide with the side edges of the insulating layer 130. With this structure, the conductive layer 120 and the insulating layer 130 can be formed using the same mask, which can simplify the manufacturing process of the memory device.
[0426] The side edges of the conductive layer 120 can be positioned more inward than the side edges of the conductive layer 115 in both the X and Y directions. This configuration can prevent short-circuiting between the conductive layer 120 and the conductive layer 115. Furthermore, as shown in Figures 20C and 20D, when the insulating layer 130 covers the conductive layer 115, the side edges of the conductive layer 120 can be positioned more outward than the side edges of the conductive layer 115.
[0427] The conductive layer 120 can be formed as a single layer or a stacked layer using the conductive material described in the section [Conductive Layer] of Embodiment 1. It is preferable to use a conductive material that is not easily oxidized or a conductive material that has a function of suppressing oxygen diffusion for the conductive layer 120. For example, titanium nitride or tantalum nitride can be used. Alternatively, for example, a structure in which tantalum nitride is stacked on titanium nitride may be used. In this case, titanium nitride is in contact with the insulating layer 130, and tantalum nitride is in contact with the semiconductor layer 230. With such a structure, excessive oxidation of the conductive layer 120 by the semiconductor layer 230 can be suppressed. Furthermore, when an oxide insulating layer is used for the insulating layer 130, excessive oxidation of the conductive layer 120 by the insulating layer 130 can be suppressed. Alternatively, for example, the conductive layer 120 may have a structure in which tungsten is stacked on titanium nitride.
[0428] Furthermore, since the conductive layer 120 has a region in contact with the semiconductor layer 230, it is preferable to use a conductive material containing oxygen. By using a conductive material containing oxygen for the conductive layer 120, the conductive layer 120 can maintain its conductivity even if it absorbs oxygen. Furthermore, even when an insulating layer containing oxygen, such as zirconium oxide, is used for the insulating layer 130, the conductive layer 120 is preferable because it can maintain its conductivity. For example, ITO, ITSO, IZO (registered trademark), or the like can be used for the conductive layer 120 as a single layer or a stacked layer.
[0429] 21A to 21D , another structure of a memory device including a transistor and a capacitor will be described. Fig. 21A is a cross-sectional view of the memory device as viewed from the X direction. Fig. 21B is a cross-sectional view of the memory device as viewed from the Y direction.
[0430] 21A and 21B differs from the memory device shown in Figures 20A and 20B in that a transistor 200 is provided below a capacitor 100. Hereinafter, differences from the above content will be mainly described, and overlapping portions will be referred to and may not be described again.
[0431] The memory device shown in Figures 21A and 21B has an insulating layer 210 on a substrate (not shown), a memory cell 150A on the insulating layer 210, an insulating layer 280 on the insulating layer 210, an insulating layer 281 on the insulating layer 280, an insulating layer 180 on the insulating layer 281, and an insulating layer 183 on the memory cell 150A.
[0432] The insulating layer 183 functions as an interlayer film. The insulating layer 183 can be formed using an insulating material that can be used for the insulating layer 283.
[0433] The memory cell 150A includes a transistor 200 and a capacitor 100 over the transistor 200.
[0434] The transistor 200 has a conductive layer 220 on an insulating layer 210, a semiconductor layer 230 on the conductive layer 220, an insulating layer 250 on the insulating layer 280, a conductive layer 260 on the insulating layer 250, and a conductive layer 240 on the semiconductor layer 230, the insulating layer 250, and the insulating layer 281.
[0435] The detailed description of the transistor 200 is omitted here because the description in Embodiment 1 (FIGS. 1A to 10D) can be referred to. The transistor included in the memory cell 150A is not limited to the transistor 200, and any one of the transistors 200A to 200D illustrated in Embodiment 1 can be used.
[0436] The capacitor 100 includes a conductive layer 115 on a conductive layer 240 , an insulating layer 130 on the conductive layer 115 , and a conductive layer 120 on the insulating layer 130 .
[0437] The capacitor 100 can be described in the previous <Configuration Example 1 of Memory Device>, and therefore detailed description thereof will be omitted.
[0438] 21C and 21D, the insulating layer 130 can cover the conductive layer 115. This can prevent the conductive layer 115 and the conductive layer 120 from shorting out.
[0439] As shown in FIGS. 21A and 21B , the capacitor 100 is provided to overlap with the transistor 200. The opening 190, where part of the structure of the capacitor 100 is provided, has a region overlapping with the semiconductor layer 230 of the transistor 200. In particular, the conductive layer 240 functions as the other of the source electrode and drain electrode of the transistor 200 and as a conductive layer connected to the lower electrode of the capacitor 100. Therefore, the capacitor 100 and the transistor 200 share part of their structures. With this structure, the capacitor 100 and the transistor 200 can be provided without significantly increasing the occupied area in a plan view. This reduces the occupied area of the memory cell 150A, thereby enabling the memory cells 150A to be arranged at a high density and increasing the storage capacity of the storage device. In other words, the storage device can be highly integrated.
[0440] 28A shows a circuit diagram of the memory device described in this embodiment. Here, the wiring BIL corresponds to the conductive layer 220, the wiring WOL corresponds to the conductive layer 260, and the wiring CAL corresponds to the conductive layer 120.
[0441] <Configuration Example 3 of Memory Device> Another configuration of a memory device will be described with reference to Figures 22A and 22B. Figure 22A is a cross-sectional view of the memory device as seen from the X direction. Figure 22B is a cross-sectional view of the memory device as seen from the Y direction.
[0442] 22A and 22B differs from the memory device shown in Figures 20A and 20B in that it includes a transistor 1200 instead of the capacitor 100. Hereinafter, differences from the above content will be mainly described, and overlapping parts will be referred to and may not be described again.
[0443] 22A and 22B includes an insulating layer 1210 over a substrate (not shown), a memory cell 150B over the insulating layer 1210, an insulating layer 1280 over the insulating layer 1210, an insulating layer 1281 over the insulating layer 1280, an insulating layer 280 over the insulating layer 1281, an insulating layer 281 over the insulating layer 280, and an insulating layer 283 over the memory cell 150B. The insulating layer 1210, the insulating layer 1280, and the insulating layer 1281 function as interlayer films.
[0444] The insulating layer 1210 can be made of an insulating material that can be used for the insulating layer 210 .
[0445] The insulating layers 1280 and 1281 preferably have a low dielectric constant because they function as interlayer films. By using a material with a low dielectric constant as the interlayer film, parasitic capacitance occurring between wirings can be reduced. A single layer or stacked layers of insulating layers containing a material with a low dielectric constant can be used for the insulating layers 1280 and 1281. Silicon oxide and silicon oxynitride are preferable because they are thermally stable.
[0446] 22A and 22B, the insulating layer 1280 and the insulating layer 1281 are shown as single layers, but the present invention is not limited to this. The insulating layer 1280 may have a stacked structure of two layers or a stacked structure of three or more layers. The insulating layer 1281 may have a stacked structure of two or more layers.
[0447] The memory cell 150B includes a transistor 1200 and a transistor 200 above the transistor 1200.
[0448] The transistor 1200 includes a conductive layer 1220, a conductive layer 1240 over an insulating layer 1280, a semiconductor layer 1230 over the conductive layer 1220, an insulating layer 1250 over the semiconductor layer 1230, and a conductive layer 1260 over the insulating layer 1250. In the transistor 1200, the semiconductor layer 1230 functions as a semiconductor layer, the conductive layer 1260 functions as a gate electrode, the insulating layer 1250 functions as a gate insulating layer, the conductive layer 1220 functions as one of a source electrode and a drain electrode, and the conductive layer 1240 functions as the other of the source electrode and drain electrode.
[0449] The conductive layer 1240 and the insulating layer 1280 have openings 1290 that reach the conductive layer 1220. At least a portion of the semiconductor layer 1230 is disposed in the openings 1290. Note that the semiconductor layer 1230 has a region in contact with the top surface of the conductive layer 1220 in the openings 1290, a region in contact with the side surface of the insulating layer 1280 in the openings 1290, a region in contact with the side surface of the conductive layer 1240 in the openings 1290, and a region in contact with at least a portion of the top surface of the conductive layer 1240. At least a portion of the insulating layer 1250 is disposed in the openings 1290. At least a portion of the conductive layer 1260 is disposed in the openings 1290. Note that the films provided in the openings 1290 are preferably formed by a CVD method or an ALD method. This improves the coverage of the films. For example, the semiconductor layer 1230, the insulating layer 1250, and the conductive layer 1260 are preferably formed by a CVD method or an ALD method.
[0450] The transistor 1200 has a structure in which one of the source electrode and the drain electrode (here, the conductive layer 1220) is located below and the other of the source electrode and the drain electrode (here, the conductive layer 1240) is located above, and thus current flows vertically. That is, a channel is formed along the side surface of the semiconductor layer 1230. The transistor 1200 also has a structure in which the channel formation region surrounds the gate electrode. Therefore, the transistor 1200 can be said to have a channel-all-around (CAA) structure.
[0451] The semiconductor layer 1230 can be formed using a semiconductor material applicable to the semiconductor layer 230. The insulating layer 1250 can be formed using an insulating material applicable to the insulating layer 250. The conductive layer 1220 can be formed using a conductive material applicable to the conductive layer 220. The conductive layer 1240 can be formed using a conductive material applicable to the conductive layer 240. The conductive layer 1260 can be formed using a conductive material applicable to the conductive layer 260.
[0452] The transistor 200 has a conductive layer 1260 (corresponding to the conductive layer 220 in FIG. 2B, etc.), a semiconductor layer 230 on the conductive layer 1260, an insulating layer 250 on the insulating layer 280, a conductive layer 260 on the insulating layer 250, and a conductive layer 240 on the semiconductor layer 230, the insulating layer 250, and the insulating layer 281.
[0453] The detailed description of the transistor 200 is omitted here because the description in Embodiment 1 (FIGS. 1A to 10D) can be referred to. The transistor included in the memory cell 150B is not limited to the transistor 200, and any one of the transistors 200A to 200D illustrated in Embodiment 1 can be used.
[0454] As shown in FIGS. 22A and 22B , the transistor 200 is provided to overlap with the transistor 1200. The semiconductor layer 230 of the transistor 200 has a region overlapping with an opening 1290 in which part of the structure of the transistor 1200 is provided. In particular, the conductive layer 1260 functions as one of the source electrode and drain electrode of the transistor 200 and as the gate electrode of the transistor 1200. Therefore, the transistors 200 and 1200 share part of their structures. With this structure, the transistors 200 and 1200 can be provided without significantly increasing the occupied area in a plan view. This reduces the occupied area of the memory cell 150B, thereby enabling the memory cells 150B to be arranged at a high density and increasing the storage capacity of the storage device. In other words, the storage device can be highly integrated.
[0455] 28E shows a circuit diagram of the memory device described in this embodiment. As shown in FIG. 28E, the configuration shown in FIGS. 22A and 22B functions as a memory cell. The memory cell 955 includes a transistor M2 and a transistor M3. Here, the transistor M2 corresponds to the transistor 200, and the transistor M3 corresponds to the transistor 1200.
[0456] One of the source and drain of transistor M2 is connected to the gate of transistor M3. The other of the source and drain of transistor M2 is connected to wiring WBL. The gate of transistor M2 is connected to wiring WOL. One of the source and drain of transistor M3 is connected to wiring SL. The other of the source and drain of transistor M3 is connected to wiring RBL.
[0457] Here, the wiring WBL corresponds to the conductive layer 240, the wiring WOL corresponds to the conductive layer 260, the wiring SL corresponds to the conductive layer 1220, and the wiring RBL corresponds to the conductive layer 1240. Note that the wiring SL and the wiring RBL can be interchanged. The conductive layer 1240 may function as the wiring SL, and the conductive layer 1220 may function as the wiring RBL.
[0458] The memory cells will be described in detail in a later embodiment.
[0459] <Configuration Example 4 of Memory Device> The memory cell 150 including the transistor 200 and the capacitor 100 shown in FIGS. 20A and 20B can be used as a memory cell of a memory device. An OS transistor is preferably used as the transistor 200. In this case, the transistor 200 has a low off-state current; therefore, by using the transistor 200 in a memory device, stored data can be retained for a long period of time. That is, refresh operation is not required or the frequency of refresh operation is extremely low; therefore, the power consumption of the memory device can be sufficiently reduced. Furthermore, the high frequency characteristics of the transistor 200 enable high-speed reading and writing of data from and to the memory device.
[0460] A memory cell array can be configured by arranging the memory cells 150 in a three-dimensional matrix.
[0461] 23A is a plan view of a memory device, showing an example in which 2×2 memory cells (memory cells 150a to 150d) are arranged in the X and Y directions.
[0462] Fig. 23B is a cross-sectional view taken along dashed line A3-A4 in Fig. 23A. In Fig. 23A and Fig. 23B, two memory cells (memory cell 150a and memory cell 150b in Fig. 23B) are connected to a common wiring (conductive layer 246).
[0463] Here, each of the memory cells 150a and 150b shown in FIGS. 23A and 23B has a configuration similar to that of the memory cell 150. The memory cell 150a includes a capacitor 100a and a transistor 200a, and the memory cell 150b includes a capacitor 100b and a transistor 200b. The memory cells 150c and 150d shown in FIG. 23A also have a configuration similar to that of the memory cell 150. Therefore, in the memory device shown in FIGS. 23A and 23B, structures having the same functions as those of the structures constituting the memory device shown in FIGS. 20A and 20B are denoted by the same reference numerals. For details of the memory cells 150a to 150d, the description of the memory cell 150 in <Configuration Example 1 of Memory Device> can be referred to.
[0464] 23A and 23B, a conductive layer 260 functioning as part of the wiring WOL is provided in each of the memory cells 150a and 150b. Also, as shown in FIG. 23A, one conductive layer 260 is provided in common to the memory cells 150a and 150c, and another conductive layer 260 is provided in common to the memory cells 150b and 150d. Also, one conductive layer 240 functioning as part of the wiring BIL is provided in common to the memory cells 150a and 150b. Also, another conductive layer 240 is provided in common to the memory cells 150c and 150d.
[0465] 23A and 23B includes conductive layers 245 and 246 that are electrically connected to the memory cell 150a and the memory cell 150b and function as plugs (which can also be referred to as connection electrodes). The conductive layer 245 is disposed in openings formed in the insulating layers 140, 180, 181, 280, 250, and 281, and is in contact with the bottom surface of the conductive layer 240. The conductive layer 246 is disposed in openings formed in the insulating layers 287 and 283, and is in contact with the top surface of the conductive layer 240. Note that the conductive layers 245 and 246 can be formed using a conductive material that can be used for the conductive layer 240.
[0466] 23A and 23B , by configuring the side edge of the insulating layer 130 to coincide with the side edge of the conductive layer 120, the insulating layer 130 does not overlap the conductive layer 245. This makes it relatively easy to process the opening in which the conductive layer 245 is to be provided.
[0467] The insulating layer 287 preferably has a low relative dielectric constant because it functions as an interlayer film. By using a material with a low relative dielectric constant as the interlayer film, parasitic capacitance occurring between wirings can be reduced.
[0468] The concentration of impurities such as water and hydrogen in the insulating layer 287 is preferably reduced. This can prevent impurities such as water and hydrogen from entering the channel formation region of the semiconductor layer 230.
[0469] The conductive layers 245 and 246 function as plugs or wirings for electrically connecting circuit elements, wirings, electrodes, or terminals, such as switches, transistors, capacitors, inductors, resistors, and diodes, to the memory cells 150a and 150b. For example, the conductive layer 245 can be electrically connected to a sense amplifier (not shown) provided below the memory device shown in FIG. 23B, and the conductive layer 246 can be electrically connected to a similar memory device (not shown) provided above the memory device shown in FIG. 23B. In this case, the conductive layers 245 and 246 function as part of the wiring BIL. In this way, by providing a memory device above or below the memory device shown in FIG. 23B, the memory capacity per unit area can be increased.
[0470] The memory cell 150a and the memory cell 150b are symmetrical with respect to the perpendicular bisector of the dashed-dotted line A3-A4. Therefore, the transistor 200a and the transistor 200b are also arranged symmetrically with the conductive layer 245 and the conductive layer 246 sandwiched therebetween. The conductive layer 240 functions as the other of the source and drain electrodes of the transistor 200a and the other of the source and drain electrodes of the transistor 200b. The transistor 200a and the transistor 200b share the conductive layer 245 and the conductive layer 246, which function as plugs. By configuring the connections between the two transistors and the plugs as described above, a memory device that can be miniaturized or highly integrated can be provided.
[0471] Note that the conductive layer 110 functioning as the wiring CAL may be provided in each of the memory cells 150 a and 150 b, or may be provided in common to the memory cells 150 a and 150 b. However, as shown in FIG. 23B , the conductive layer 110 is provided apart from the conductive layer 245 to prevent a short circuit between the conductive layer 110 and the conductive layer 245.
[0472] 24 shows an example in which the four memory cells shown in FIG. 23A are stacked in n layers (n is an integer of 3 or more) in the Z direction. FIG. 24 is a cross-sectional view taken along dashed line A3-A4 shown in FIG. 23A.
[0473] The memory device shown in FIG. 24 has n memory layers 160. Specifically, memory layer 160[2] is provided on memory layer 160[1], and (n-3) memory layers are further provided on memory layer 160[2], with memory layer 160[n] provided at the top. The number of memory cells included in one memory layer 160 is not particularly limited, and two or more memory cells may be included. The memory cells included in the n memory layers 160 are electrically connected to a sense amplifier (not shown) provided below the n memory layers 160 by conductive layers 245, 246, 247, etc.
[0474] 24, by stacking a plurality of memory cells, the cells can be integrated and arranged without increasing the area occupied by the memory cell array, that is, a 3D memory cell array can be configured.
[0475] The memory device may also include the memory cell 150 described above in <Configuration Example 1 of Semiconductor Device> and the memory cell 150A described above in <Configuration Example 2 of Semiconductor Device>.
[0476] A cross-sectional view of a memory device having memory cells 150 and 150A is shown in Fig. 25. Fig. 25 shows an example in which the four memory cells shown in Fig. 23A are stacked in n layers (n is an integer of 4 or more) in the Z direction. Fig. 25 is a cross-sectional view taken along dashed line A3-A4 shown in Fig. 23A.
[0477] The memory device shown in FIG. 25 has n memory layers 160. Specifically, memory layer 160[2] is provided on memory layer 160[1], and (n-3) memory layers are further provided on memory layer 160[2], with memory layer 160[n] provided on the topmost level. The number of memory cells included in one memory layer 160 is not particularly limited, and each memory layer 160 may have two or more memory cells. The memory cells included in the n memory layers 160 are electrically connected to a sense amplifier (not shown) provided below the n memory layers 160 by conductive layers 245, 246, etc.
[0478] 25, memory cells 150 are provided in memory layers 160[1] and 160[3], and memory cells 150A are provided in memory layers 160[2] and 160[4]. The conductive layer 240 in contact with the upper surface of the conductive layer 245 and the lower surface of the conductive layer 246 is electrically connected to the memory cell 150 included in the memory layer 160[1] and the memory cell 150A included in the memory layer 160[2]. That is, the memory cell 150 included in the memory layer 160[1] and the memory cell 150A included in the memory layer 160[2] share part of their structure. Furthermore, the conductive layer 120 included in the memory layer 160[2] is electrically connected to the lower electrode of the capacitor included in the memory layer 160[3]. That is, the memory cell 150A included in the memory layer 160[2] and the memory cell 150 included in the memory layer 160[3] share part of their structure. Such a configuration contributes to lower costs and improved throughput.
[0479] FIG. 26 shows an example of a cross-sectional configuration of a memory device in which a layer having memory cells is stacked over a layer in which a driver circuit including a sense amplifier is provided.
[0480] In FIG. 26, a memory cell 150 (a transistor 200 and a capacitor 100 ) is provided above a transistor 300 .
[0481] The transistor 300 is one of the transistors included in the sense amplifier.
[0482] For the memory cell 150 shown in FIG. 26, the description of the memory cell 150 in <Configuration example 1 of memory device> can be referred to.
[0483] 26, the bit lines can be shortened by providing a sense amplifier so as to overlap the memory cells 150. This reduces the bit line capacitance, enabling the memory device to be driven at high speed.
[0484] 26 can correspond to the semiconductor device 900 described in Embodiment 3. Specifically, the transistor 300 corresponds to a transistor included in a sense amplifier 927 in the semiconductor device 900. The memory cell 150 corresponds to a memory cell 950.
[0485] The transistor 300 is provided over a substrate 311 and includes a conductive layer 316 functioning as a gate, an insulating layer 315 functioning as a gate insulating layer, a semiconductor region 313 formed of part of the substrate 311, and a low-resistance region 314 a and a low-resistance region 314 b functioning as a source region or a drain region. The transistor 300 may be either a p-channel type or an n-channel type.
[0486] Here, in the transistor 300 shown in FIG. 26 , a semiconductor region 313 (a part of a substrate 311) where a channel is formed has a convex shape. A conductive layer 316 is provided to cover the side and top surfaces of the semiconductor region 313 with an insulating layer 315 interposed therebetween. Note that the conductive layer 316 may be made of a material that adjusts the work function. Such a transistor 300 is also called a FIN-type transistor because it utilizes the convex portion of the semiconductor substrate. Note that an insulating layer that is in contact with the top of the convex portion and functions as a mask for forming the convex portion may be provided. Here, the case where the convex portion is formed by processing a part of the semiconductor substrate is shown, but a semiconductor film having a convex shape may also be formed by processing an SOI substrate.
[0487] Note that the transistor 300 illustrated in FIG. 26 is just an example, and the structure is not limited thereto. An appropriate transistor can be used depending on the circuit configuration or driving method.
[0488] Between each structure, a wiring layer provided with an interlayer film, wiring, plugs, etc. may be provided. Furthermore, multiple wiring layers may be provided depending on the design. Here, for a conductive layer functioning as a plug or wiring, multiple structures may be collectively assigned the same reference numeral. Furthermore, in this specification and the like, the wiring and the plug electrically connected to the wiring may be integrated. That is, there are cases where a part of the conductive layer functions as the wiring, and cases where a part of the conductive layer functions as the plug.
[0489] For example, an insulating layer 320, an insulating layer 322, an insulating layer 324, and an insulating layer 326 are stacked in this order as an interlayer film over the transistor 300. A conductive layer 328 is embedded in the insulating layer 320 and the insulating layer 322, and a conductive layer 330 is embedded in the insulating layer 324 and the insulating layer 326. The conductive layer 328 and the conductive layer 330 function as plugs or wirings.
[0490] The insulating layer serving as an interlayer film may also function as a planarizing film that covers the underlying unevenness. For example, the top surface of the insulating layer 322 may be planarized by a planarization process using a CMP method or the like to improve the planarity.
[0491] A wiring layer may be provided over the insulating layer 326 and the conductive layer 330. For example, in Fig. 26, an insulating layer 350, an insulating layer 352, and an insulating layer 354 are stacked in this order. A conductive layer 356 is formed in the insulating layer 350, the insulating layer 352, and the insulating layer 354. The conductive layer 356 functions as a plug or a wiring.
[0492] The insulating layer 352, the insulating layer 354, and the like, which function as interlayer films, can be formed using the above-described insulating layer that can be used in a semiconductor device or a memory device.
[0493] For conductive layers functioning as plugs or wirings, such as the conductive layer 328, the conductive layer 330, and the conductive layer 356, a conductive material applicable to the conductive layer 240 can be used. A high-melting-point material that has both heat resistance and conductivity, such as tungsten or molybdenum, is preferably used, and tungsten is preferably used. Alternatively, a low-resistance conductive material, such as aluminum or copper, is preferably used. The use of a low-resistance conductive material can reduce wiring resistance.
[0494] The conductive layer 240 of the transistor 200 is electrically connected to the low-resistance region 314b functioning as a source region or a drain region of the transistor 300 through the conductive layer 643, the conductive layer 645, the conductive layer 646, the conductive layer 356, the conductive layer 330, and the conductive layer 328.
[0495] The conductive layer 643 is buried in the insulating layer 281, the insulating layer 250, the insulating layer 280, the insulating layer 641, and the insulating layer 180. The conductive layer 645 is buried in the insulating layer 647. The conductive layer 645 can be manufactured using the same material and in the same process as the conductive layer 110. The conductive layer 646 is buried in the insulating layer 648. The insulating layer 648 electrically insulates the transistor 300 from the conductive layer 110.
[0496] As described above, the memory device of this embodiment has a transistor with reduced parasitic capacitance, and therefore the operating speed can be increased. In addition, the memory device of this embodiment has a capacitor and a transistor stacked on top of each other, and therefore the area occupied by the memory cell in a plan view can be reduced, and a memory device with high integration can be realized.
[0497] This embodiment mode can be combined with other embodiment modes as appropriate.
[0498] Embodiment 3 In this embodiment, a semiconductor device 900 according to one embodiment of the present invention will be described. The semiconductor device 900 can function as a memory device.
[0499] Fig. 27 is a block diagram showing a configuration example of a semiconductor device 900. The semiconductor device 900 shown in Fig. 27 has a driver circuit 910 and a memory array 920. The memory array 920 has one or more memory cells 950. Fig. 27 shows an example in which the memory array 920 has a plurality of memory cells 950 arranged in a matrix.
[0500] The memory cell 950 can be any of the memory devices described in Embodiment 2 (such as the memory cell 150 ).
[0501] The drive circuit 910 includes a PSW 931 (power switch), a PSW 932, and a peripheral circuit 915. The peripheral circuit 915 includes a peripheral circuit 911, a control circuit 912, and a voltage generation circuit 928.
[0502] In the semiconductor device 900, each circuit, signal, and voltage can be appropriately selected or omitted as needed. Alternatively, other circuits or signals may be added. The signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are input signals from the outside, and the signal RDA is an output signal to the outside. The signal CLK is a clock signal.
[0503] Furthermore, signals BW, CE, and GW are control signals. Signal CE is a chip enable signal, signal GW is a global write enable signal, and signal BW is a byte write enable signal. Signal ADDR is an address signal. Signal WDA is write data, and signal RDA is read data. Signals PON1 and PON2 are power gating control signals. Note that signals PON1 and PON2 may be generated by the control circuit 912.
[0504] The control circuit 912 is a logic circuit having a function of controlling the overall operation of the semiconductor device 900. For example, the control circuit 912 performs a logical operation on the signals CE, GW, and BW to determine the operation mode (e.g., write operation, read operation) of the semiconductor device 900. Alternatively, the control circuit 912 generates a control signal for the peripheral circuit 911 so that this operation mode is executed.
[0505] The voltage generating circuit 928 has a function of generating a negative voltage. The signal WAKE has a function of controlling the input of the signal CLK to the voltage generating circuit 928. For example, when an H-level signal is given as the signal WAKE, the signal CLK is input to the voltage generating circuit 928, and the voltage generating circuit 928 generates a negative voltage.
[0506] The peripheral circuit 911 is a circuit for writing and reading data to and from the memory cells 950. The peripheral circuit 911 includes a row decoder 941, a column decoder 942, a row driver 923, a column driver 924, an input circuit 925, an output circuit 926, and a sense amplifier 927.
[0507] The row decoder 941 and the column decoder 942 have the function of decoding the signal ADDR. The row decoder 941 is a circuit for specifying a row to be accessed, and the column decoder 942 is a circuit for specifying a column to be accessed. The row driver 923 has the function of selecting the row specified by the row decoder 941. The column driver 924 has the function of writing data to the memory cells 950, reading data from the memory cells 950, and retaining the read data.
[0508] The input circuit 925 has a function of holding a signal WDA. The data held by the input circuit 925 is output to the column driver 924. The output data of the input circuit 925 is data (Din) to be written to the memory cell 950. The data (Dout) read from the memory cell 950 by the column driver 924 is output to the output circuit 926. The output circuit 926 has a function of holding Dout. In addition, the output circuit 926 has a function of outputting Dout to the outside of the semiconductor device 900. The data output from the output circuit 926 is a signal RDA.
[0509] The PSW 931 is a V DD The PSW 932 has the function of controlling the supply of V to the row driver 923. HM Here, the high power supply potential of the semiconductor device 900 is V DD and the low power supply potential is GND (ground potential). HM is the high power supply potential used to drive the word line high, and V DD 27, in the peripheral circuit 915, V DD Although the number of power domains to which power is supplied is set to one, it is also possible to set it to a plurality of power domains. In this case, a power switch may be provided for each power domain.
[0510] 28A to 28H, examples of memory cell configurations that can be applied to the memory cell 950 will be described.
[0511] In the following description, when two components are said to be connected, this includes being electrically connected via a circuit element (such as a transistor, a switch, a diode, or a resistor). Electrical connection means that a current can flow between the two components. Note that when two components are connected via a switch or a transistor, this is also included in the term "electrical connection," because a current can flow when these are in the on state.
[0512] 28A shows an example of a circuit configuration of a DRAM memory cell. In this specification and the like, a DRAM using an OS transistor is referred to as a DOSRAM (Dynamic Oxide Semiconductor Random Access Memory). A memory cell 951 includes a transistor M1 and a capacitor CA.
[0513] The transistor M1 may have a gate (sometimes referred to as a top gate) and a back gate. In this case, the back gate may be connected to a wiring to which a constant potential or a signal is applied, or the front gate and the back gate may be connected to each other.
[0514] A first terminal of the transistor M1 is connected to a first terminal of the capacitance element CA, a second terminal of the transistor M1 is connected to the wiring BIL, and a gate of the transistor M1 is connected to the wiring WOL. The second terminal of the capacitance element CA is connected to the wiring CAL.
[0515] The wiring BIL functions as a bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitance element CA. When writing and reading data, it is preferable to apply a low-level potential (sometimes referred to as a reference potential) to the wiring CAL.
[0516] Data is written and read by applying a high-level potential to the wiring WOL, turning on the transistor M1, and bringing the wiring BIL and the first terminal of the capacitor CA into a conductive state (a state in which current can flow).
[0517] Furthermore, the memory cell that can be used as the memory cell 950 is not limited to the memory cell 951, and the circuit configuration can be changed. For example, the memory cell 952 shown in FIG. 28B may be used. The memory cell 952 is an example in which the capacitor CA and the wiring CAL are not included. The first terminal of the transistor M1 is in an electrically floating state.
[0518] In the memory cell 952, the potential written through the transistor M1 is held in a capacitance (also referred to as a parasitic capacitance) between the first terminal and the gate, which is indicated by a dashed line. With this configuration, the configuration of the memory cell can be significantly simplified.
[0519] Note that an OS transistor is preferably used as the transistor M1. An OS transistor has a characteristic of extremely low off-state current. By using an OS transistor as the transistor M1, the leakage current of the transistor M1 can be made extremely small. That is, written data can be held by the transistor M1 for a long time, so that the frequency of refreshing the memory cell can be reduced. Alternatively, the refresh operation of the memory cell can be made unnecessary. Furthermore, because the leakage current is extremely small, multilevel data or analog data can be held in the memory cell 951 and the memory cell 952.
[0520] 28C shows an example circuit configuration of a gain cell type memory cell having two transistors and one capacitor. The memory cell 953 includes a transistor M2, a transistor M3, and a capacitor CB. In this specification and the like, a memory device having a gain cell type memory cell in which the transistor M2 is an OS transistor is referred to as a nonvolatile oxide semiconductor RAM (NOSRAM).
[0521] The first terminal of transistor M2 is connected to the first terminal of capacitance element CB, the second terminal of transistor M2 is connected to wiring WBL, and the gate of transistor M2 is connected to wiring WOL. The second terminal of capacitance element CB is connected to wiring CAL. The first terminal of transistor M3 is connected to wiring RBL, the second terminal of transistor M3 is connected to wiring SL, and the gate of transistor M3 is connected to the first terminal of capacitance element CB.
[0522] The wiring WBL functions as a write bit line, the wiring RBL functions as a read bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitance element CB. When writing data, while retaining data, and when reading data, it is preferable to apply a low-level potential (sometimes referred to as a reference potential) to the wiring CAL.
[0523] Data is written by applying a high-level potential to the wiring WOL, turning on the transistor M2, and establishing electrical continuity between the wiring WBL and the first terminal of the capacitor CB. Specifically, when the transistor M2 is on, a potential corresponding to the information to be recorded is applied to the wiring WBL, and the potential is written to the first terminal of the capacitor CB and the gate of the transistor M3. Then, a low-level potential is applied to the wiring WOL, turning off the transistor M2, thereby maintaining the potential of the first terminal of the capacitor CB and the potential of the gate of the transistor M3.
[0524] Data is read by applying a predetermined potential to the wiring SL. The current flowing between the source and drain of the transistor M3 and the potential of the first terminal of the transistor M3 are determined by the potential of the gate of the transistor M3 and the potential of the second terminal of the transistor M3. Therefore, the potential held in the first terminal of the capacitor CB (or the gate of the transistor M3) can be read by reading the potential of the wiring RBL connected to the first terminal of the transistor M3. In other words, information written in this memory cell can be read from the potential held in the first terminal of the capacitor CB (or the gate of the transistor M3).
[0525] Alternatively, for example, the wiring WBL and the wiring RBL may be combined into a single wiring BIL. An example circuit configuration of such a memory cell is shown in FIG. 28D. The memory cell 954 is configured such that the wiring WBL and the wiring RBL of the memory cell 953 are combined into a single wiring BIL, and the second terminal of the transistor M2 and the first terminal of the transistor M3 are connected to the wiring BIL. In other words, the memory cell 954 is configured to operate as a write bit line and a read bit line using a single wiring BIL.
[0526] 28E is an example in which the capacitor element CB and the wiring CAL are omitted from the memory cell 953. Also, a memory cell 956 shown in Fig. 28F is an example in which the capacitor element CB and the wiring CAL are omitted from the memory cell 954. With such a configuration, the integration degree of the memory cells can be increased.
[0527] Note that at least the transistor M2 is preferably an OS transistor, and in particular, the transistors M2 and M3 are preferably OS transistors.
[0528] Since the OS transistor has an extremely low off-state current, written data can be held by the transistor M2 for a long time, which reduces the frequency of refreshing the memory cell. Alternatively, the refresh operation of the memory cell can be eliminated. Furthermore, since the leakage current is extremely low, multilevel data or analog data can be held in the memory cell 953, the memory cell 954, the memory cell 955, and the memory cell 956.
[0529] The memory cell 953, the memory cell 954, the memory cell 955, and the memory cell 956, each of which uses an OS transistor as the transistor M2, are one embodiment of an NOSRAM.
[0530] Note that a Si transistor may be used as the transistor M3. The Si transistor can increase the field effect mobility and can also be used as a p-channel transistor, thereby increasing the degree of freedom in circuit design.
[0531] When an OS transistor is used as the transistor M3, the memory cell can be configured as a unipolar circuit.
[0532] 28G shows a three-transistor, one-capacitor gain cell type memory cell 957. The memory cell 957 has transistors M4 to M6 and a capacitor CC.
[0533] The first terminal of transistor M4 is connected to the first terminal of capacitor CC, the second terminal of transistor M4 is connected to wiring BIL, and the gate of transistor M4 is connected to wiring WOL. The second terminal of capacitor CC is connected to the first terminal of transistor M5 and wiring GNDL. The second terminal of transistor M5 is connected to the first terminal of transistor M6, and the gate of transistor M5 is connected to the first terminal of capacitor CC. The second terminal of transistor M6 is connected to wiring BIL, and the gate of transistor M6 is connected to wiring RWL.
[0534] The wiring BIL functions as a bit line, the wiring WOL functions as a write word line, and the wiring RWL functions as a read word line. The wiring GNDL is a wiring that applies a low-level potential.
[0535] Data is written by applying a high-level potential to the wiring WOL, turning on the transistor M4, and establishing electrical continuity between the wiring BIL and the first terminal of the capacitor CC. Specifically, when the transistor M4 is on, a potential corresponding to the information to be recorded is applied to the wiring BIL, and the potential is written to the first terminal of the capacitor CC and the gate of the transistor M5. Then, a low-level potential is applied to the wiring WOL, turning off the transistor M4, thereby maintaining the potential of the first terminal of the capacitor CC and the potential of the gate of the transistor M5.
[0536] Data is read by precharging the wiring BIL to a predetermined potential, then electrically floating the wiring BIL, and applying a high-level potential to the wiring RWL. Because the wiring RWL is at a high-level potential, the transistor M6 is turned on, and the wiring BIL and the second terminal of the transistor M5 are electrically connected. At this time, the potential of the wiring BIL is applied to the second terminal of the transistor M5. The potential of the second terminal of the transistor M5 and the potential of the wiring BIL change depending on the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5). By reading the potential of the wiring BIL, the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5) can be read. In other words, information written in this memory cell can be read from the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5).
[0537] Note that at least the transistor M4 is preferably an OS transistor.
[0538] Note that Si transistors may be used as the transistors M5 and M6. As described above, Si transistors may have higher field-effect mobility than OS transistors depending on the crystalline state of silicon used in the semiconductor layer.
[0539] When OS transistors are used as the transistors M5 and M6, the memory cell can be configured as a unipolar circuit.
[0540] 28H shows an example of an SRAM (Static Random Access Memory) using an OS transistor. In this specification and the like, an SRAM using an OS transistor is referred to as an OS-SRAM (Oxide Semiconductor-SRAM). Note that a memory cell 958 shown in FIG. 28H is a memory cell of an SRAM capable of backing up data.
[0541] The memory cell 958 includes transistors M7 to M10, transistors MS1 to MS4, and capacitors CD1 and CD2. Note that the transistors MS1 and MS2 are p-channel transistors, and the transistors MS3 and MS4 are n-channel transistors.
[0542] A first terminal of transistor M7 is connected to wiring BIL, and a second terminal of transistor M7 is connected to a first terminal of transistor MS1, a first terminal of transistor MS3, the gate of transistor MS2, the gate of transistor MS4, and a first terminal of transistor M10. The gate of transistor M7 is connected to wiring WOL. A first terminal of transistor M8 is connected to wiring BILB, and a second terminal of transistor M8 is connected to a first terminal of transistor MS2, the first terminal of transistor MS4, the gate of transistor MS1, the gate of transistor MS3, and a first terminal of transistor M9. The gate of transistor M8 is connected to wiring WOL.
[0543] A second terminal of the transistor MS1 is connected to the wiring VDL. A second terminal of the transistor MS2 is connected to the wiring VDL. A second terminal of the transistor MS3 is connected to the wiring GNDL. A second terminal of the transistor MS4 is connected to the wiring GNDL.
[0544] A second terminal of the transistor M9 is connected to a first terminal of the capacitor CD1, and a gate of the transistor M9 is connected to the wiring BRL. A second terminal of the transistor M10 is connected to a first terminal of the capacitor CD2, and a gate of the transistor M10 is connected to the wiring BRL.
[0545] A second terminal of the capacitance element CD1 is connected to the wiring GNDL, and a second terminal of the capacitance element CD2 is connected to the wiring GNDL.
[0546] The wirings BIL and BILB function as bit lines, the wiring WOL functions as a word line, and the wiring BRL is a wiring that controls the on / off states of the transistors M9 and M10.
[0547] The wiring VDL is a wiring that applies a high-level potential, and the wiring GNDL is a wiring that applies a low-level potential.
[0548] Data is written by applying a high-level potential to the wiring WOL and a high-level potential to the wiring BRL. Specifically, when the transistor M10 is on, a potential corresponding to information to be written is applied to the wiring BIL, and the potential is written to the second terminal of the transistor M10.
[0549] Since the memory cell 958 includes an inverter loop formed by the transistors MS1 and MS2, an inverted signal of the data signal corresponding to the potential is input to the second terminal of the transistor M8. Because the transistor M8 is on, the potential applied to the wiring BIL, i.e., the inverted signal of the signal input to the wiring BIL, is output to the wiring BILB. Because the transistors M9 and M10 are on, the potentials of the second terminals of the transistors M7 and M8 are held in the first terminals of the capacitors CD2 and CD1, respectively. After that, a low-level potential is applied to the wiring WOL and a low-level potential is applied to the wiring BRL to turn off the transistors M7 to M10, thereby holding the potentials of the first terminals of the capacitors CD1 and CD2.
[0550] Data is read by precharging the wirings BIL and BILB to a predetermined potential in advance, and then applying a high-level potential to the wiring WOL and a high-level potential to the wiring BRL. The potential of the first terminal of the capacitor CD1 is refreshed by the inverter loop of the memory cell 958 and output to the wiring BILB. The potential of the first terminal of the capacitor CD2 is refreshed by the inverter loop of the memory cell 958 and output to the wiring BIL. The potentials of the wirings BIL and BILB change from the precharged potentials to the potentials of the first terminal of the capacitor CD2 and the first terminal of the capacitor CD1, respectively. Therefore, the potential held in the memory cell can be read from the potential of the wiring BIL or BILB.
[0551] Note that OS transistors are preferably used as the transistors M7 to M10. This allows written data to be held by the transistors M7 to M10 for a long time, which reduces the frequency of refreshing the memory cells. Alternatively, refreshing the memory cells can be eliminated.
[0552] Note that Si transistors may be used as the transistors MS1 to MS4.
[0553] The driver circuit 910 and memory array 920 of the semiconductor device 900 may be provided on the same plane. Alternatively, as shown in FIG. 29A, the driver circuit 910 and memory array 920 may be provided overlapping each other. By providing the driver circuit 910 and memory array 920 overlapping each other, the signal propagation distance can be shortened. Alternatively, as shown in FIG. 29B, the memory array 920 may be provided in multiple layers on the driver circuit 910.
[0554] Next, an example of a processing unit that can include a semiconductor device such as the memory device will be described.
[0555] 30 shows a block diagram of the arithmetic device 960. The arithmetic device 960 shown in FIG. 30 can be applied to, for example, a CPU. The arithmetic device 960 can also be applied to processors such as a GPU (Graphics Processing Unit), a TPU (Tensor Processing Unit), and an NPU (Neural Processing Unit) that have a larger number (several tens to several hundreds) of processor cores capable of parallel processing than a CPU.
[0556] The arithmetic device 960 shown in FIG. 30 has an ALU 991 (ALU: Arithmetic logic unit, arithmetic circuit), an ALU controller 992, an instruction decoder 993, an interrupt controller 994, a timing controller 995, a register 996, a register controller 997, a bus interface 998, a cache 999, and a cache interface 989 on a substrate 990. The substrate 990 may be a semiconductor substrate, an SOI substrate, a glass substrate, or the like. It may also have a rewritable ROM and a ROM interface. The cache 999 and the cache interface 989 may also be provided on separate chips.
[0557] The cache 999 is connected to a main memory provided on a separate chip via a cache interface 989. The cache interface 989 has a function of supplying part of the data held in the main memory to the cache 999. The cache interface 989 also has a function of outputting part of the data held in the cache 999 to the ALU 991, register 996, etc. via the bus interface 998.
[0558] As will be described later, a memory array 920 can be provided stacked on the arithmetic unit 960. The memory array 920 can be used as a cache. In this case, the cache interface 989 may have a function of supplying data held in the memory array 920 to the cache 999. In this case, it is preferable that a drive circuit 910 be included as part of the cache interface 989.
[0559] It is also possible to use only the memory array 920 as a cache without providing the cache 999 .
[0560] The arithmetic device 960 shown in FIG. 30 is merely an example of a simplified configuration, and actual arithmetic devices 960 have a wide variety of configurations depending on their applications. For example, it is preferable to use a configuration including the arithmetic device 960 shown in FIG. 30 as one core, and to include multiple such cores, each of which operates in parallel, in a so-called multi-core configuration. The greater the number of cores, the higher the computational performance. The greater the number of cores, for example, two, preferably four, more preferably eight, even more preferably twelve, and even more preferably sixteen or more. Furthermore, when extremely high computational performance is required, such as for server applications, a multi-core configuration having 16 or more, preferably 32 or more, and even more preferably 64 or more cores is preferable. Furthermore, the number of bits that the arithmetic device 960 can handle in its internal computation circuit, data bus, etc. can be, for example, 8 bits, 16 bits, 32 bits, 64 bits, etc.
[0561] An instruction input to the arithmetic unit 960 via the bus interface 998 is input to the instruction decoder 993, decoded, and then input to the ALU controller 992, interrupt controller 994, register controller 997, and timing controller 995.
[0562] The ALU controller 992, interrupt controller 994, register controller 997, and timing controller 995 perform various controls based on the decoded instructions. Specifically, the ALU controller 992 generates signals for controlling the operation of the ALU 991. Furthermore, the interrupt controller 994 determines and processes interrupt requests from external input / output devices, peripheral circuits, etc. based on their priority, mask status, etc. while the arithmetic unit 960 is executing a program. The register controller 997 generates addresses for registers 996 and reads and writes data from and to the registers 996 depending on the state of the arithmetic unit 960.
[0563] Furthermore, the timing controller 995 generates signals that control the timing of the operations of the ALU 991, the ALU controller 992, the instruction decoder 993, the interrupt controller 994, and the register controller 997. For example, the timing controller 995 includes an internal clock generation unit that generates an internal clock signal based on a reference clock signal, and supplies the internal clock signal to the various circuits described above.
[0564] 30, the register controller 997 selects the holding operation of the register 996 in accordance with an instruction from the ALU 991. That is, it selects whether the memory cells of the register 996 will hold data using flip-flops or using capacitors. If holding data using flip-flops is selected, a power supply potential is supplied to the memory cells in the register 996. If holding data using capacitors is selected, the data is rewritten to the capacitors, and the supply of power supply potential to the memory cells in the register 996 can be stopped.
[0565] The memory array 920 and the arithmetic unit 960 can be provided overlapping each other. Perspective views of a semiconductor device 970A are shown in Figures 31A and 31B. The semiconductor device 970A has a layer 930 on which memory arrays are provided above the arithmetic unit 960. The layer 930 is provided with memory arrays 920L1, 920L2, and 920L3. The arithmetic unit 960 and each memory array have overlapping regions. To make the configuration of the semiconductor device 970A easier to understand, the arithmetic unit 960 and the layer 930 are shown separately in Figure 31B.
[0566] By stacking the layer 930 having the memory array and the arithmetic unit 960, the connection distance between them can be shortened, thereby increasing the communication speed between them. In addition, the short connection distance reduces power consumption.
[0567] As a method for stacking the layer 930 having a memory array and the arithmetic device 960, a method (also called monolithic stacking) in which the layer 930 having a memory array is stacked directly on the arithmetic device 960 may be used, or a method in which the arithmetic device 960 and the layer 930 are formed on different substrates, the two substrates are bonded together, and the two substrates are electrically connected using a through-via or a conductive film bonding technique (such as Cu-Cu bonding) may be used. The former method does not require consideration of misalignment during bonding, and therefore can not only reduce the chip size but also reduce the manufacturing cost.
[0568] Here, the arithmetic unit 960 does not have a cache 999, and the memory arrays 920L1, 920L2, and 920L3 provided in the layer 930 can each be used as a cache. In this case, for example, the memory array 920L1 can be used as an L1 cache (also referred to as a level 1 cache), the memory array 920L2 can be used as an L2 cache (also referred to as a level 2 cache), and the memory array 920L3 can be used as an L3 cache (also referred to as a level 3 cache). Of the three memory arrays, the memory array 920L3 has the largest capacity and the lowest access frequency. Furthermore, the memory array 920L1 has the smallest capacity and the highest access frequency.
[0569] When the cache 999 provided in the arithmetic unit 960 is used as an L1 cache, each memory array provided in the layer 930 can be used as a lower-level cache or a main memory. The main memory has a larger capacity than the cache and is accessed less frequently.
[0570] 31B, a driving circuit 910L1, a driving circuit 910L2, and a driving circuit 910L3 are provided. The driving circuit 910L1 is connected to the memory array 920L1 via a connection electrode 940L1. Similarly, the driving circuit 910L2 is connected to the memory array 920L2 via a connection electrode 940L2, and the driving circuit 910L3 is connected to the memory array 920L3 via a connection electrode 940L3.
[0571] Although the number of memory arrays functioning as caches is three in this example, the number may be one or two, or four or more.
[0572] When the memory array 920L1 is used as a cache, the drive circuit 910L1 may function as part of the cache interface 989, or may be configured so that the drive circuit 910L1 is connected to the cache interface 989. Similarly, the drive circuits 910L2 and 910L3 may also function as part of the cache interface 989, or may be configured so that they are connected thereto.
[0573] Whether the memory array 920 is made to function as a cache or as a main memory is determined by a control circuit 912 included in each drive circuit 910. The control circuit 912 can cause some of the memory cells 950 included in the semiconductor device 900 to function as RAM based on a signal supplied from the arithmetic device 960.
[0574] The semiconductor device 900 can cause some of the memory cells 950 to function as a cache and the other memory cells to function as a main memory. That is, the semiconductor device 900 can function as both a cache and a main memory. The semiconductor device 900 according to one embodiment of the present invention can function as, for example, a universal memory.
[0575] Furthermore, a layer 930 having one memory array 920 may be provided over the arithmetic device 960. Figure 32A shows a perspective view of a semiconductor device 970B.
[0576] In the semiconductor device 970B, one memory array 920 can be divided into multiple areas, each of which can be used for a different function. Fig. 32A shows an example in which area L1 is used as an L1 cache, area L2 is used as an L2 cache, and area L3 is used as an L3 cache.
[0577] Furthermore, in the semiconductor device 970B, the capacity of each of the areas L1 to L3 can be changed depending on the situation. For example, if it is desired to increase the capacity of the L1 cache, this can be achieved by increasing the area of the area L1. This configuration can improve the efficiency of calculation processing and increase the processing speed.
[0578] Also, multiple memory arrays may be stacked. Figure 32B shows a perspective view of a semiconductor device 970C.
[0579] The semiconductor device 970C includes a layer 930L1 having a memory array 920L1, a layer 930L2 having a memory array 920L2 on top of that, and a layer 930L3 having a memory array 920L3 on top of that. The memory array 920L1, which is physically closest to the arithmetic unit 960, can be used as a higher-level cache, and the memory array 920L3, which is farthest, can be used as a lower-level cache or main memory. This configuration allows the capacity of each memory array to be increased, thereby further improving processing power.
[0580] This embodiment mode can be combined with other embodiment modes as appropriate.
[0581] Embodiment 4 In this embodiment, an application example of a memory device according to one embodiment of the present invention will be described.
[0582] Generally, various memory devices are used in semiconductor devices such as computers depending on the application. FIG. 33A shows various memory devices used in semiconductor devices by layer. The higher the layer, the faster the operating speed of the memory device is required, while the lower the layer, the larger the memory capacity and recording density are required. In FIG. 33A , from the top layer, there are memories embedded as registers in a processing unit such as a CPU, an L1 cache, an L2 cache, an L3 cache, a main memory, and storage. Note that while an example having up to an L3 cache is shown here, lower-level caches may also be included.
[0583] The memory embedded as a register in a processing unit such as a CPU is used for temporary storage of calculation results, and is therefore frequently accessed by the processing unit. Therefore, a higher operating speed is required than a larger memory capacity. Registers also have the function of storing setting information for the processing unit.
[0584] A cache has the function of duplicating and storing a portion of the data stored in main memory. By duplicating frequently used data and storing it in the cache, the access speed to the data can be increased. The storage capacity required for a cache is smaller than that of main memory, but it is required to operate at a faster speed than main memory. In addition, data rewritten in the cache is duplicated and supplied to the main memory.
[0585] The main memory has a function of holding programs, data, etc. read from storage.
[0586] Storage has the function of storing data that requires long-term storage, various programs used by processing units, etc. Therefore, storage requires a large memory capacity and high recording density rather than an operating speed. For example, high-capacity, non-volatile storage devices such as 3D NAND can be used.
[0587] A storage device (OS memory) using an oxide semiconductor according to one embodiment of the present invention has high operating speed and can retain data for a long period of time. Therefore, as shown in FIG. 33A , the storage device according to one embodiment of the present invention can be suitably used in both a tier where a cache is located and a tier where a main memory is located. The storage device according to one embodiment of the present invention can also be applied to a tier where a storage is located.
[0588] FIG. 33B also shows an example in which an SRAM is used as part of a cache and an OS memory of one embodiment of the present invention is used as the other part of the cache.
[0589] The lowest level cache can be called a last level cache (LLC). While an LLC does not require faster operation speed than higher level caches, it is desirable for the LLC to have a large storage capacity. The OS memory of one embodiment of the present invention has a high operation speed and can retain data for a long period of time, and therefore can be suitably used for an LLC. The OS memory of one embodiment of the present invention can also be applied to a final level cache (FLC).
[0590] For example, as shown in Fig. 33B, a configuration can be adopted in which SRAM is used for the higher-level caches (L1 cache, L2 cache, etc.) and the OS memory according to one aspect of the present invention is used for the LLC. Also, as shown in Fig. 33B, not only the OS memory but also DRAM can be applied to the main memory.
[0591] This embodiment mode can be combined with other embodiment modes as appropriate.
[0592] Embodiment 5 In this embodiment, a display device according to one embodiment of the present invention will be described.
[0593] The semiconductor device of one embodiment of the present invention can be used for a display device or a module including the display device. Examples of the module including the display device include a module in which a connector such as a flexible printed circuit (hereinafter referred to as FPC) or a tape carrier package (TCP) is attached to the display device, and a module in which an integrated circuit (IC) is mounted by a chip-on-glass (COG) method, a chip-on-film (COF) method, or the like.
[0594] The display device of this embodiment may also have a function as a touch panel. For example, various detection elements (also referred to as sensor elements) that can detect the proximity or contact of a detection target such as a finger can be applied to the display device.
[0595] Examples of sensor types include a capacitance type, a resistive film type, a surface acoustic wave type, an infrared type, an optical type, and a pressure-sensitive type.
[0596] The capacitance type includes, for example, a surface capacitance type and a projected capacitance type. The projected capacitance type includes, for example, a self-capacitance type and a mutual capacitance type. The mutual capacitance type is preferable because it enables simultaneous multi-point detection.
[0597] Examples of touch panels include out-cell, on-cell, and in-cell types. Note that an in-cell touch panel is a type in which electrodes constituting a detection element are provided on one or both of a substrate supporting a display element and an opposing substrate.
[0598] 34A shows a perspective view of the display module 170. The display module 170 includes a display device 600A and an FPC 298. Note that the display device included in the display module 170 is not limited to the display device 600A, and may be a display device 600B described later.
[0599] The display module 170 includes a substrate 291 and a substrate 299. The display module 170 includes a display portion 297. The display portion 297 is a region that displays an image in the display module 170, and is a region where light from each pixel provided in a pixel portion 294 (described later) can be viewed.
[0600] 34B is a perspective view schematically illustrating the configuration on the substrate 291 side. A circuit portion 292, a pixel circuit portion 293 on the circuit portion 292, and a pixel portion 294 on the pixel circuit portion 293 are stacked on the substrate 291. A terminal portion 295 for connecting to an FPC 298 is provided in a portion of the substrate 291 that does not overlap with the pixel portion 294. The terminal portion 295 and the circuit portion 292 are electrically connected by a wiring portion 296 composed of a plurality of wirings.
[0601] The semiconductor device of one embodiment of the present invention can be applied to one or both of the circuit portion 292 and the pixel circuit portion 293 .
[0602] The pixel section 294 has a plurality of periodically arranged pixels 294a. An enlarged view of one pixel 294a is shown on the right side of Fig. 34B. Fig. 34B shows an example in which one pixel 294a has a sub-pixel 289R that emits red light, a sub-pixel 289G that emits green light, and a sub-pixel 289B that emits blue light.
[0603] Each subpixel has a display element. Various elements can be used as the display element, including, for example, a liquid crystal element and a light-emitting element. Other examples include shutter-type or optical interference-type MEMS (Micro Electro Mechanical Systems) elements, display elements using microcapsules, electrophoresis, electrowetting, or electronic liquid powder (registered trademark) methods, etc. Furthermore, a QLED (Quantum-dot LED) using a light source and color conversion technology using quantum dot materials may also be used.
[0604] Examples of the light-emitting element include self-luminous light-emitting elements such as LEDs (Light Emitting Diodes), OLEDs (Organic LEDs), semiconductor lasers, etc. Examples of the LED that can be used include mini LEDs and micro LEDs.
[0605] The pixel arrangement in the display device of this embodiment is not particularly limited, and various methods can be applied. Examples of pixel arrangements include a stripe arrangement, an S-stripe arrangement, a matrix arrangement, a delta arrangement, a Bayer arrangement, and a pentile arrangement. Figure 34B shows an example in which a stripe arrangement is applied to the pixel arrangement.
[0606] The pixel circuit section 293 has a plurality of pixel circuits 293a arranged periodically.
[0607] One pixel circuit 293a is a circuit that controls the driving of multiple elements included in one pixel 294a. One pixel circuit 293a can be configured to have three circuits that control the light emission of one light-emitting element. For example, the pixel circuit 293a can be configured to have at least one selection transistor, one current control transistor (drive transistor), and a capacitor for each light-emitting element. In this case, a gate signal is input to the gate of the selection transistor, and a source signal is input to the source. This realizes an active matrix display device.
[0608] The circuit portion 292 includes a circuit for driving each pixel circuit 293a of the pixel circuit portion 293. For example, it is preferable that the circuit portion 292 includes one or both of a gate line driver circuit and a source line driver circuit. In addition, the circuit portion 292 may include at least one of an arithmetic circuit, a memory circuit, a power supply circuit, and the like.
[0609] The FPC 298 functions as wiring for supplying a video signal, a power supply potential, or the like from the outside to the circuit portion 292. An IC may be mounted on the FPC 298.
[0610] The display module 170 can be configured such that one or both of the pixel circuit portion 293 and the circuit portion 292 are provided overlapping below the pixel portion 294, thereby making it possible to extremely increase the aperture ratio (effective display area ratio) of the display portion 297. In addition, the pixels 294a can be arranged at extremely high density, making it possible to extremely increase the resolution of the display portion 297.
[0611] Because such a display module 170 has extremely high resolution, it can be suitably used in VR devices such as HMDs or eyeglass-type AR devices. For example, even in a configuration in which the display unit of the display module 170 is viewed through lenses, the display module 170 has an extremely high-resolution display unit 297, so even when the display unit is enlarged with lenses, the pixels are not visible, allowing for a highly immersive display. Furthermore, the display module 170 is not limited to this, and can be suitably used in electronic devices with relatively small displays. For example, it can be suitably used in the display unit of a wearable electronic device such as a wristwatch.
[0612] 35 shows a cross-sectional view of a display device 600A. The display device 600A is an example of a display device to which an MML (metal maskless) structure is applied. In other words, the display device 600A has light-emitting elements fabricated without using a fine metal mask.
[0613] The island-shaped light-emitting layers in the light-emitting elements of a display device employing the MML structure are formed by depositing a light-emitting layer on one surface and then processing it using photolithography. This allows for the realization of high-definition display devices or display devices with a high aperture ratio, which have been difficult to achieve until now. Furthermore, since the light-emitting layers can be created separately for each color, a display device with extremely vivid images, high contrast, and high display quality can be realized. For example, if a display device is composed of three types of light-emitting elements, namely, light-emitting elements that emit blue light, light-emitting elements that emit green light, and light-emitting elements that emit red light, the deposition of the light-emitting layers and the processing by photolithography can be repeated three times to form the three types of island-shaped light-emitting layers.
[0614] Because devices with an MML structure can be manufactured without using a metal mask, they can exceed the upper limit of resolution imposed by the alignment accuracy of the metal mask. Furthermore, when devices are manufactured without using a metal mask, the equipment required for manufacturing the metal mask and the metal mask cleaning process are unnecessary. Furthermore, since photolithography processing can be performed using the same or similar equipment as that used to manufacture transistors, there is no need to introduce special equipment to manufacture devices with an MML structure. As such, the MML structure allows for low manufacturing costs, making it suitable for mass production of devices.
[0615] In a display device to which the MML structure is applied, there is no need to artificially increase the resolution by applying a special pixel arrangement such as a pentile arrangement, and therefore it is possible to realize a display device with high resolution (for example, 500 ppi or more, 1000 ppi or more, 2000 ppi or more, 3000 ppi or more, or 5000 ppi or more) using a so-called stripe arrangement in which R, G, and B sub-pixels are each arranged in one direction.
[0616] Furthermore, by providing a sacrificial layer on the light-emitting layer, damage to the light-emitting layer during the manufacturing process of the display device can be reduced, and the reliability of the light-emitting element can be improved. Note that the sacrificial layer may remain in the completed display device or may be removed during the manufacturing process. For example, the sacrificial layer 618a shown in Figures 35 and 36 is a part of the sacrificial layer provided on the light-emitting layer.
[0617] Furthermore, by employing a film formation step using an area mask and a processing step using a resist mask, a light-emitting element can be manufactured through a relatively simple process.
[0618] A display device 600A illustrated in Figure 35 is a cross-sectional schematic diagram of a display device (semiconductor device) of one embodiment of the present invention. The display device 600A has a structure in which a pixel circuit, a driver circuit, and the like are provided over a substrate 410. Note that in the display device 600A illustrated in Figure 35, in addition to element layers 620, 630, and 660, a wiring layer 670 is also illustrated. The wiring layer 670 is a layer in which wirings are provided.
[0619] A pixel circuit of the display device is preferably provided in the element layer 630. A driver circuit of the display device (either a gate driver or a source driver, or both) is preferably provided in the element layer 620. The element layer 620 may also be provided with one or more types of circuits such as an arithmetic circuit and a memory circuit.
[0620] The element layer 620 includes, for example, a substrate 410 over which a transistor 400d is formed. A wiring layer 670 is provided above the transistor 400d. The wiring layer 670 includes a wiring that electrically connects the transistor 400d to a conductive layer or a transistor (the conductive layer 514 in FIG. 35 ) provided in the element layer 630. An element layer 630 and an element layer 660 are provided above the wiring layer 670. The element layer 630 includes, for example, a transistor MTCK. The element layer 660 includes a light-emitting element 650 (a light-emitting element 650R, a light-emitting element 650G, and a light-emitting element 650B in FIG. 35 ).
[0621] The transistor 400d is an example of a transistor included in the element layer 620. The transistor MTCK is an example of a transistor included in the element layer 630. The light-emitting elements (light-emitting element 650R, light-emitting element 650G, and light-emitting element 650B) are an example of light-emitting elements included in the element layer 660.
[0622] The substrate 410 can be, for example, a semiconductor substrate (e.g., a single-crystal substrate made of silicon or germanium). Other than a semiconductor substrate, the substrate 410 can be, for example, an SOI substrate, a glass substrate, a quartz substrate, a plastic substrate, a sapphire glass substrate, a metal substrate, a stainless steel substrate, a substrate having stainless steel foil, a tungsten substrate, a substrate having tungsten foil, a flexible substrate, a lamination film, paper containing a fibrous material, or a base film. In this embodiment, the substrate 410 will be described as a semiconductor substrate made of silicon. Therefore, the transistor included in the element layer 620 can be a Si transistor.
[0623] The transistor 400d includes an element isolation layer 412, a conductive layer 416, an insulating layer 415, an insulating layer 417, a semiconductor region 413 formed of a part of the substrate 410, and low-resistance regions 414a and 414b that function as source and drain regions. Therefore, the transistor 400d is a Si transistor. Note that although Figure 35 illustrates a structure in which one of the source and drain of the transistor 400d is electrically connected to the conductive layer 514 provided in the element layer 630 through the conductive layer 428, the conductive layer 430, and the conductive layer 456, the electrical connection structure of the display device of one embodiment of the present invention is not limited thereto.
[0624] The transistor 400d can be a Fin type by, for example, covering the top surface and the side surfaces in the channel width direction of the semiconductor region 413 with a conductive layer 416 via an insulating layer 415 that functions as a gate insulating layer. By making the transistor 400d a Fin type, the effective channel width can be increased, and the on-state characteristics of the transistor 400d can be improved. Furthermore, the contribution of the electric field of the gate electrode can be increased, and the off-state characteristics of the transistor 400d can be improved. The transistor 400d may be a planar type instead of a Fin type.
[0625] Note that the transistor 400d may be either a p-channel transistor or an n-channel transistor. Alternatively, a plurality of transistors 400d may be provided, and both p-channel and n-channel transistors may be used.
[0626] The region in the semiconductor region 413 where the channel is formed, the region nearby, and the low-resistance region 414a and low-resistance region 414b that will become the source region or drain region preferably contain a silicon-based semiconductor, specifically, single-crystal silicon. Alternatively, each of the above-mentioned regions may be formed using, for example, germanium, silicon germanium, gallium arsenide, aluminum gallium arsenide, or gallium nitride. Alternatively, a configuration using silicon in which the effective mass is controlled by applying stress to the crystal lattice and changing the lattice spacing may be used. Alternatively, the transistor 400d may be, for example, a high electron mobility transistor (HEMT) using gallium arsenide and aluminum gallium arsenide.
[0627] The conductive layer 416 functioning as a gate electrode can be made of a semiconductor material such as silicon containing an element that imparts n-type conductivity, such as arsenic or phosphorus, or an element that imparts p-type conductivity, such as boron or aluminum. Alternatively, the conductive layer 416 can be made of a conductive material such as a metal material, an alloy material, or a metal oxide material.
[0628] Since the work function is determined by the material of the conductive layer, the threshold voltage of the transistor can be adjusted by selecting the material of the conductive layer. Specifically, it is preferable to use one or both of titanium nitride and tantalum nitride for the conductive layer. Furthermore, in order to achieve both conductivity and embeddability, it is preferable to use one or both of tungsten and aluminum as a stacked layer for the conductive layer, and tungsten is particularly preferable in terms of heat resistance.
[0629] The element isolation layer 412 is provided to isolate a plurality of transistors formed on the substrate 410. The element isolation layer can be formed using, for example, a local oxidation of silicon (LOCOS) method, a shallow trench isolation (STI) method, or a mesa isolation method.
[0630] An insulating layer 420 and an insulating layer 422 are stacked in this order from the substrate 410 side over a transistor 400d shown in FIG.
[0631] The insulating layer 420 and the insulating layer 422 can be formed using, for example, one or more selected from silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, aluminum oxynitride, aluminum nitride oxide, and aluminum nitride.
[0632] The insulating layer 422 may function as a planarizing film that planarizes steps caused by the insulating layer 420 and the transistor 400d covered with the insulating layer 422. For example, the top surface of the insulating layer 422 may be planarized by planarization treatment using a CMP method or the like to improve the planarity.
[0633] A conductive layer 428 is buried in the insulating layer 420 and the insulating layer 422 and connected to the transistor MTCK and the like provided above the insulating layer 422. Note that the conductive layer 428 functions as a plug or a wiring.
[0634] In the display device 600A, a wiring layer 670 is provided over the transistor 400d. The wiring layer 670 includes, for example, an insulating layer 424, an insulating layer 426, a conductive layer 430, an insulating layer 450, an insulating layer 452, an insulating layer 454, and a conductive layer 456.
[0635] An insulating layer 424 and an insulating layer 426 are stacked in this order over the insulating layer 422 and the conductive layer 428. An opening is formed in the insulating layer 424 and the insulating layer 426 in a region overlapping with the conductive layer 428. A conductive layer 430 is embedded in the opening.
[0636] An insulating layer 450, an insulating layer 452, and an insulating layer 454 are stacked in this order over the insulating layer 426 and the conductive layer 430. In addition, openings are formed in the insulating layer 450, the insulating layer 452, and the insulating layer 454 in regions overlapping with the conductive layer 430. A conductive layer 456 is embedded in the openings.
[0637] The conductive layer 430 and the conductive layer 456 function as a plug or a wiring connected to the transistor 400d.
[0638] Note that, for example, the insulating layers 424 and 450 are preferably insulating layers having a barrier property against one or more selected from hydrogen, oxygen, and water, similar to the insulating layer 592 described later. Furthermore, the insulating layers 426, 452, and 454 are preferably insulating layers having a relatively low relative dielectric constant in order to reduce parasitic capacitance between wirings, similar to the insulating layer 594 described later. Furthermore, the insulating layers 426, 452, and 454 function as interlayer insulating films and planarizing films.
[0639] The conductive layer 456 preferably includes a conductive layer having a barrier property against one or more selected from hydrogen, oxygen, and water.
[0640] Note that, for example, tantalum nitride may be used as the conductive layer having a barrier property against hydrogen. Furthermore, by stacking tantalum nitride and tungsten, which has high conductivity, it is possible to suppress diffusion of hydrogen from the transistor 400d while maintaining the conductivity of the wiring. In this case, a structure in which the tantalum nitride layer having a barrier property against hydrogen is in contact with the insulating layer 450 having a barrier property against hydrogen is preferable.
[0641] An insulating layer 513 is provided above the insulating layer 454 and the conductive layer 456. An insulating layer IS1 is provided over the insulating layer 513. A conductive layer functioning as a plug or a wiring is embedded in the insulating layer IS1 and the insulating layer 513. This allows the transistor 400d to be electrically connected to the conductive layer 514 provided in the element layer 630. Alternatively, one of the source or drain of the transistor MTCK may be electrically connected to one of the source or drain of the transistor 400d.
[0642] A transistor MTCK is provided on the insulating layer IS1. An insulating layer IS3, an insulating layer 574, and an insulating layer 581 are stacked in this order on the transistor MTCK. A conductive layer MPG functioning as a plug or wiring is buried in the insulating layers IS3, 574, and 581.
[0643] The insulating layer 574 preferably has a function of suppressing diffusion of impurities such as water and hydrogen (e.g., hydrogen atoms and / or hydrogen molecules...
Claims
A cylindrical semiconductor layer; a first conductive layer in contact with a lower surface of the semiconductor layer; a second conductive layer in contact with an upper surface of the semiconductor layer; a first insulating layer covering at least a portion of a side surface of the semiconductor layer; a third conductive layer facing a side surface of the semiconductor layer via the first insulating layer; having the first insulating layer has a first region between the semiconductor layer and the third conductive layer and a second region between the first conductive layer and the third conductive layer; A semiconductor device, wherein the width of the first region in a direction from the semiconductor layer toward the third conductive layer is equal to or approximately equal to the width of the second region in a direction from the first conductive layer toward the third conductive layer. In claim 1, A semiconductor device, wherein the height of the semiconductor layer is greater than the width of a lower surface of the semiconductor layer. In claim 1, The first insulating layer has a region in contact with the second conductive layer. In claim 1, the semiconductor layer includes a first oxide semiconductor layer, and a second oxide semiconductor layer and a third oxide semiconductor layer sandwiching the first oxide semiconductor layer; each of the second oxide semiconductor layer and the third oxide semiconductor layer has a lower resistance than the first oxide semiconductor layer and has a region facing the third conductive layer with the first insulating layer interposed therebetween. In claim 4, the first oxide semiconductor layer contains one or both of indium and zinc, each of the second oxide semiconductor layer and the third oxide semiconductor layer contains one or both of indium and zinc, and nitrogen. In claim 1, a second insulating layer between the first conductive layer and the first insulating layer; The second insulating layer covers another portion of the side surface of the semiconductor layer. In claim 1, the first insulating layer has a laminated structure of a first insulating film located on the semiconductor layer side and a second insulating film located on the third conductive layer side; the first insulating film includes silicon and oxygen; The second insulating film comprises silicon and nitrogen. In claim 7, a third insulating layer covering the third conductive layer; the third conductive layer is surrounded by the third insulating layer and the second insulating film. a cylindrical first semiconductor layer; a first conductive layer in contact with a lower surface of the first semiconductor layer; a second conductive layer in contact with an upper surface of the first semiconductor layer; a second semiconductor layer covering a side surface of the first semiconductor layer; a first insulating layer covering at least a portion of a side surface of the second semiconductor layer; a third conductive layer facing a side surface of the first semiconductor layer via the first insulating layer; having the first insulating layer has a first region between the first semiconductor layer and the third conductive layer and a second region between the first conductive layer and the third conductive layer; A semiconductor device, wherein a width of the first region in a direction from the first semiconductor layer toward the third conductive layer is equal to or approximately equal to a width of the second region in a direction from the first conductive layer toward the third conductive layer. In claim 9, A semiconductor device, wherein the height of the first semiconductor layer is greater than the width of a lower surface of the first semiconductor layer. In claim 9, The first insulating layer and the second semiconductor layer each have a region in contact with the second conductive layer. In claim 9, A semiconductor device, wherein the first semiconductor layer and the second semiconductor layer each contain one or both of indium and zinc. In claim 9, a second insulating layer between the first conductive layer and the first insulating layer; The second insulating layer covers another portion of the side surface of the second semiconductor layer. A semiconductor device comprising: a semiconductor device according to any one of claims 1 to 13; and a capacitive element; The memory device, wherein the first conductive layer has a region that functions as one of a pair of electrodes of the capacitor. A semiconductor device comprising: a semiconductor device according to any one of claims 1 to 13; and a capacitive element; the second conductive layer has a region that functions as one of a pair of electrodes of the capacitor. forming a first conductive layer; forming a cylindrical semiconductor layer on the first conductive layer; forming a first insulating layer on the first conductive layer and the semiconductor layer; The first insulating layer is processed to expose a part of a side surface of the semiconductor layer; a second insulating layer and a conductive film are sequentially formed on the first insulating layer and the semiconductor layer; forming a second conductive layer having an upper surface located closer to the first conductive layer than an upper surface of the semiconductor layer by processing the conductive film; forming a third conductive layer over the semiconductor layer and the second insulating layer. In claim 16, The method for manufacturing a semiconductor device, wherein the semiconductor layer is formed so that a height thereof is greater than a width of a lower surface thereof. In claim 16, The method for manufacturing a semiconductor device, wherein the second insulating layer is formed by atomic layer deposition.
Citation Information
Patent Citations
Method for manufacturing passivated silicon nanowires and devices obtained thereby
JP2012531751A
Semiconductor device
JP2013211537A
Semiconductor device manufacturing method
JP2013251533A
Semiconductor device and manufacturing method of the same
JP2015109426A
Manufacture method for semiconductor device
JP2017157866A
Cited By
Multi-spectral optical detector with vertical structure and preparation method of multi-spectral optical detector
CN121310669A