Positive electrode for lithium secondary battery, and lithium secondary battery
The positive electrode design for lithium secondary batteries, incorporating a current collector film with a resin and metal layers, addresses safety and rate characteristic issues by optimizing particle size ratios and binder composition, resulting in enhanced energy density and performance.
Patent Information
- Application Number
- PCT/JP2023/018604
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-21
AI Technical Summary
Lithium secondary batteries face issues with poor safety and rate characteristics due to the elongation of current collector films during pressing, leading to deterioration of electrode characteristics and reduced energy density.
A positive electrode design featuring a current collector film with a resin layer and metal layers on both sides, combined with specific particle size ratios and binder compositions, which enhances safety and rate characteristics by reducing elongation and improving energy density.
The proposed design achieves high safety, high energy density per weight and volume, and good cycle and rate characteristics by optimizing the particle size ratios and binder composition in the positive electrode composite layer.
Smart Images

Figure JP2023018604_21112024_PF_FP_ABST
Abstract
Description
Positive electrode for lithium secondary battery and lithium secondary battery
[0001] The present invention relates to a positive electrode for a lithium secondary battery and a lithium secondary battery.
[0002] In recent years, technology for converting natural energy such as solar or wind power into electrical energy has been attracting attention. Accordingly, various secondary batteries have been developed as electricity storage devices that are highly safe and capable of storing a large amount of electrical energy.
[0003] Among these, lithium secondary batteries, which are charged and discharged by the movement of lithium ions between a positive electrode and a negative electrode, are known to exhibit high voltage and high energy density. A typical lithium secondary battery is a lithium-ion secondary battery (LIB), which has active materials capable of retaining lithium elements in the positive electrode and the negative electrode, and is charged and discharged by the exchange of lithium ions between the positive electrode active material and the negative electrode active material.
[0004] For example, Patent Document 1 discloses that the safety of a battery cell is improved by using a current collector film in which metal layers are formed on both sides of a resin film.
[0005] Japanese Patent Application Publication No. 11-102711
[0006] In lithium-ion secondary batteries, electrodes are pressed to reduce size and increase density. However, it has been found that a positive electrode using the current collector film described in Patent Document 1 has a problem in that the current collector film has a larger elongation rate when pressed than other parts of the positive electrode, resulting in deterioration of battery characteristics.
[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a positive electrode for a lithium secondary battery that has high safety and good rate characteristics.
[0008] A positive electrode for a lithium secondary battery according to one embodiment of the present invention includes: a current collector film including a resin layer and metal layers provided on both sides of the resin layer; and a positive electrode composite layer formed on the current collector film, wherein the positive electrode composite layer includes first positive electrode active material particles having a median diameter D50 of 10 μm or more and 25 μm or less, second positive electrode active material particles, and two or more binders; and The median diameter D50 ratio of the particles ([median diameter D50 of the second positive electrode active material particles] / [median diameter D50 of the first positive electrode active material particles]) is 0.75 or less, and the mass ratio of the first positive electrode active material particles to the second positive electrode active material particles in the positive electrode ([content of the first positive electrode active material particles in the positive electrode] / [content of the second positive electrode active material particles in the positive electrode]) is 1.5 or more and 9.0 or less.
[0009] In the lithium secondary battery, the positive electrode includes a current collector film having a resin layer and metal layers provided on both sides of the resin layer, thereby providing high safety. Furthermore, the present inventors have found that a positive electrode composite layer includes first positive electrode active material particles and second positive electrode active material particles, each having a median diameter D50 of 10 μm or more and 25 μm or less, and two or more types of binders, and the median diameter D50 ratio of the second positive electrode active material particles to the first positive electrode active material particles ([median diameter D50 of the second positive electrode active material particles] / [median diameter D50 of the first positive electrode active material particles]) is 0.75 or less, and the mass ratio in the positive electrode of the first positive electrode active material particles to the second positive electrode active material particles ([content of the first positive electrode active material particles in the positive electrode] / [content of the second positive electrode active material particles in the positive electrode]) is 1.5 or more and 9.0 or less, thereby exhibiting good rate characteristics. Therefore, it is presumed that the above-mentioned components allow the lithium secondary battery to have both high safety and good rate characteristics, although the reasons for this are not limited to those mentioned above.
[0010] In the positive electrode for a lithium secondary battery according to one embodiment of the present invention, the metal layer is preferably formed of aluminum. According to such an embodiment, the lithium secondary battery tends to be even safer.
[0011] In the positive electrode for a lithium secondary battery according to one embodiment of the present invention, preferably, the mass ratio in the positive electrode of the first positive electrode active material particles to the second positive electrode active material particles ([content of the first positive electrode active material particles in the positive electrode] / [content of the second positive electrode active material particles in the positive electrode]) is 2.0 or more and 9.0 or less. According to such an embodiment, the lithium secondary battery tends to have even more excellent rate characteristics.
[0012] In the positive electrode for a lithium secondary battery according to one embodiment of the present invention, the ratio of the median diameter D50 of the second positive electrode active material particles to the first positive electrode active material particles is preferably 0.1 or more and 0.5 or less. According to such an aspect, the lithium secondary battery tends to have even more excellent rate characteristics.
[0013] In the positive electrode for a lithium secondary battery according to one embodiment of the present invention, the median diameter D50 of the first positive electrode active material particles is preferably 10 μm or more and 20 μm or less. According to such an embodiment, the lithium secondary battery tends to have even more excellent rate characteristics.
[0014] In the positive electrode for a lithium secondary battery according to one embodiment of the present invention, the binder preferably includes a first binder having vinylidene fluoride as a repeating unit and a second binder having tetrafluoroethylene as a repeating unit. According to such an embodiment, the lithium secondary battery tends to have even more excellent rate characteristics.
[0015] In the positive electrode for a lithium secondary battery according to one embodiment of the present invention, preferably, the mass ratio of the second binder to the first binder in the positive electrode ([content of the second binder in the positive electrode] / [content of the first binder in the positive electrode]) is 1.0 or more and 10.0 or less. According to such an embodiment, the lithium secondary battery tends to have even more excellent rate characteristics.
[0016] A positive electrode for a lithium secondary battery according to one embodiment of the present invention preferably includes any one of the positive electrodes described above. According to such an embodiment, the battery tends to have even better safety and rate characteristics.
[0017] According to the present invention, it is possible to provide a positive electrode that achieves both high safety and good rate characteristics in a lithium secondary battery.
[0018] 1 is a diagram showing an example of a cross-sectional structure of a positive electrode according to an embodiment of the present invention; FIG. 2 is a diagram showing another example of a cross-sectional structure of a positive electrode according to an embodiment of the present invention; FIG. 3 is a schematic cross-sectional view of a lithium secondary battery according to an embodiment of the present invention;
[0019] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail with reference to the drawings as necessary. However, the present invention is not limited to this embodiment, and various modifications are possible without departing from the spirit of the present invention. In the drawings, the same elements are given the same reference numerals, and redundant explanations will be omitted. Furthermore, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings unless otherwise specified. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.
[0020] 1. Positive Electrode Fig. 1 is a diagram showing an example of the cross-sectional structure of a positive electrode for a lithium secondary battery according to one embodiment of the present invention, and Fig. 2 is a diagram showing another example. As shown in Fig. 1, a positive electrode 30 of this embodiment includes a current collector film 32A including a resin layer 320A and metal layers 322A provided on both sides of the resin layer 320A, and a positive electrode mixture layer 34A formed on the current collector film 32A. The positive electrode mixture layer 34A includes positive electrode active material particles L (first positive electrode active material particles) and positive electrode active material particles S (second positive electrode active material particles) having a median diameter D50 of 10 µm or more and 25 µm or less. a ratio of a median diameter D50 of the positive electrode active material particles S to the positive electrode active material particles L is 0.75 or less, and a mass ratio in the positive electrode of the positive electrode active material particles L to the positive electrode active material particles S ([content of the positive electrode active material particles L in the positive electrode] / [content of the positive electrode active material particles S in the positive electrode]) is 1.5 or more and 9.0 or less.
[0021] As shown in Fig. 1 , positive electrode composite layer 34A may be formed on both sides of current collector film 32A to form positive electrode 30A, or as shown in Fig. 2 , positive electrode composite layer 34A may be formed on at least one side of current collector film 32A to form positive electrode 30B. In this specification, the term "positive electrode 30" refers to an entity that includes both positive electrode 30A and positive electrode 30B.
[0022] When the current collector film 32A includes a resin layer 320A and metal layers 322A provided on both sides of the resin layer 320A, the resin layer 320A melts in the event of abnormal heat generation due to overcharge or high temperature, and can function to cut off short-circuit current within the battery. This tends to suppress a sudden temperature rise within the battery, suppress battery ignition, and contribute to high safety.
[0023] Furthermore, the current collector film 32A contains a resin that has a lower density than metal, and therefore has a lower weight per volume than a current collector that has only a metal layer. Therefore, lithium secondary batteries using the current collector film 32A tend to have excellent energy density per weight.
[0024] When fabricating lithium secondary batteries, the positive electrode is often pressed to reduce its volume in order to achieve miniaturization and high density. Comparing a positive electrode having only a metal layer as a current collector with a positive electrode having a current collector film having a resin layer and metal layers provided on both sides of the resin layer, when the positive electrode is pressed, the current collector film tends to elongate more in the direction perpendicular to the pressing direction, i.e., to have greater strain, than a current collector having only a metal layer. This is presumably because resins tend to have a smaller Young's modulus than metals, and therefore a current collector film having a resin layer and a metal layer has a smaller Young's modulus than a current collector having only a metal layer. However, the reason for this is not limited to this.
[0025] As described above, when the current collector film stretches, the layer containing the positive electrode active material formed on the current collector film also tends to stretch accordingly. However, because the Young's modulus of the layer containing the positive electrode active material is relatively large, it is unable to fully accommodate this stretching, resulting in cracks and other defects in the layer containing the positive electrode active material. As a result, the characteristics of the positive electrode and the cycle characteristics of the lithium secondary battery tend to deteriorate. This is presumably because the layer containing the positive electrode active material is unable to fully accommodate the stretching of the current collector film, which includes a resin layer and metal layers provided on both sides of the resin layer, resulting in cracks in the layer containing the positive electrode active material, which breaks the electron conduction path in the layer containing the positive electrode active material. However, the cause of this is not limited to this.
[0026] On the other hand, if pressing is not performed or the pressing pressure is reduced in order to avoid deterioration of the cycle characteristics of a lithium secondary battery due to pressing a positive electrode having a current collector film including a resin layer and metal layers provided on both sides of the resin layer, and a layer containing a positive electrode active material formed on the current collector film, it is not possible to achieve miniaturization or high density of the lithium secondary battery, and as a result, the energy density tends to decrease.
[0027] As a result of extensive investigations, the present inventors have found that by using a positive electrode mixture layer 34A containing a positive electrode active material, the layer including positive electrode active material particles L and positive electrode active material particles S, each having a median diameter D50 of 10 μm or more and 25 μm or less, wherein the median diameter D50 ratio of the positive electrode active material particles S to the positive electrode active material particles L is 0.75 or less, and the mass ratio in the positive electrode of the positive electrode active material particles L to the positive electrode active material particles S ([content of the positive electrode active material particles L in the positive electrode] / [content of the positive electrode active material particles S in the positive electrode]) is 1.5 or more and 9.0 or less, it is possible to achieve a high energy density per volume, good cycle characteristics, and good rate characteristics even when using the current collector film 32A of this embodiment. The reason for this is presumed to be, but is not limited to, the following.
[0028] Compared to a case where the median diameter D50 (hereinafter also referred to as "D50") of the positive electrode active material particles in the layer containing the positive electrode active material is uniform, a positive electrode composite layer 34A containing two types of positive electrode active material particles, one with a moderately large D50 and one with a small D50, and in which the two types of positive electrode active material particles are present in an appropriate mass ratio, can achieve a smaller volume at the same pressing pressure. This is thought to be because, when the positive electrode is pressed, the positive electrode active material particles with a small D50 enter the gaps between the positive electrode active material particles with a moderately large D50. Therefore, when a positive electrode composite layer 34A containing two types of positive electrode active material particles, one with a moderately large D50 and one with a small D50, and in which the two types of positive electrode active material particles are present in an appropriate mass ratio, can achieve a smaller positive electrode and higher density with a lower pressing pressure, which tends to result in an improved energy density per volume of the lithium secondary battery. Furthermore, when the pressing pressure is low, the elongation of the collector film 32A, which includes the resin layer 320A and the metal layers 322A provided on both sides of the resin layer 320A, also becomes small. This allows the positive electrode composite layer 34A to follow the elongation of the collector film 32A, preventing the characteristics of the positive electrode from deteriorating. As a result, the cycle characteristics and rate characteristics of the lithium secondary battery tend to improve.
[0029] Furthermore, by using a positive electrode composite layer 34A containing a binder as the layer containing the positive electrode active material, the Young's modulus of the positive electrode composite layer 34A becomes smaller, and the positive electrode composite layer 34A can more easily follow the elongation of the current collector film 32A when the positive electrode 30 is pressed. This means that the characteristics of the positive electrode tend not to deteriorate even if the positive electrode 30 is pressed with a greater pressure. Therefore, it becomes possible to press the positive electrode 30 with a greater pressure, and the energy density per volume tends to increase. However, the factors behind this are not limited to those described above.
[0030] Therefore, it is believed that a lithium secondary battery including the positive electrode 30 of this embodiment can achieve high safety, high energy density per weight, high energy density per volume, good cycle characteristics, and good rate characteristics all at once. However, the factors are not limited to those mentioned above.
[0031] The average thickness of the positive electrode 30 after pressing is not particularly limited, but is, for example, 50 μm to 500 μm, 100 μm to 400 μm, or 150 μm to 350 μm.
[0032] The density of the positive electrode 30 after pressing is preferably 2.5 g / cc or more and 7.5 g / cc or less, 3.0 g / cc or more and 6.5 g / cc or less, or 3.3 g / cc or more and 5.0 g / cc or less.
[0033] Each component contained in the positive electrode 30 will be described in detail below.
[0034] 1.1 Current Collector Film The current collector film 32A according to this embodiment includes a resin layer 320A and metal layers 322A provided on both sides of the resin layer 320A. The metal layers 322A are formed by vapor deposition, sputtering, electrolytic plating, or by bonding with an adhesive to both surfaces of the resin layer 320A. Use of the current collector film 32A tends to result in excellent safety and energy density per weight.
[0035] The thickness of the current collector film 32A before pressing is not particularly limited, but may be, for example, 4.0 μm or more and 20.0 μm or less, 5.0 μm or more and 17.5 μm or less, or 5.5 μm or more and 15.0 μm or less.
[0036] 1.1.1. Resin Layer The resin layer 320A according to this embodiment is an insulator and prevents electrical conduction between the metal layers 322A provided on both sides of the resin layer 320A. The resin constituting the resin layer 320A is not particularly limited, but may be, for example, a sheet-like (film-like) or fibrous resin. Examples of resins include, but are not particularly limited to, polyolefin resins such as polyethylene terephthalate (PET), polyethylene, and polypropylene, and thermoplastic resins such as polystyrene, polyvinyl chloride, and polyamide. The resins in the resin layer 320A may be used alone or in combination of two or more. Furthermore, the above-described resins may be mixed to form a single resin layer 320A, or layers may be formed using the above-described resins alone, and then multiple layers may be combined to form a single resin layer 320A.
[0037] In addition to the resins described above, the resin layer 320A may contain other additives as appropriate depending on the desired physical properties. The additives are not particularly limited, but examples thereof include colorants, flame retardants, surfactants, etc.
[0038] The resin content in resin layer 320A is not particularly limited, but may be, for example, 60% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, or 95% by mass or more and 100% by mass or less, relative to the total amount of resin layer 320A.
[0039] The thickness of the resin layer 320A before pressing is not particularly limited, but may be, for example, 2.0 μm or more and 12.0 μm or less, or 3.0 μm or more and 10.0 μm or less.
[0040] 1.1.2. Metal Layer The metal layer 322A according to this embodiment is in physical and / or electrical contact with the positive electrode composite layer 34A (described below) and functions to donate and receive electrons to the positive electrode composite layer 34A. The metal layer 322A is composed of a conductor such as a metal that does not react with lithium in a battery. The metal constituting the metal layer 322A is not particularly limited, but is at least one selected from the group consisting of aluminum, titanium, stainless steel, nickel, and alloys thereof. Among these, aluminum or an aluminum alloy is preferred, and aluminum is particularly preferred. The metal may be used alone or in combination of two or more.
[0041] The thickness of each metal layer 322A before pressing is not particularly limited, but may be, for example, 0.2 μm or more and 5.0 μm or less, 0.3 μm or more and 4.0 μm or less, or 0.5 μm or more and 3.0 μm or less.
[0042] 1.2. Positive Electrode Mixture Layer The positive electrode mixture layer 34A of the present embodiment contains positive electrode active material particles L and positive electrode active material particles S, which will be described later, and a binder, and may further contain a conductive additive, a sacrificial positive electrode agent, and other components.
[0043] 1.2.1. Cathode Active Material Particles The cathode active material particles of this embodiment are particles formed of a cathode active material. The cathode active material is a material that causes an electrode reaction, i.e., an oxidation reaction and a reduction reaction, at the cathode. Specifically, the cathode active material of this embodiment includes a host material of lithium element (typically, lithium ions). Such cathode active materials include, but are not limited to, metal oxides and metal phosphates. Examples of the metal oxides include, but are not limited to, cobalt oxide-based compounds, manganese oxide-based compounds, and nickel oxide-based compounds. Examples of the metal phosphates include, but are not limited to, iron phosphate-based compounds and cobalt phosphate-based compounds. Typical cathode active materials include LiCoO 2 , Li z Ni x Co y M 1-x-y O 2+α (wherein 0.5≦x≦1.0, 0≦y≦0.35, 0.9≦z≦1.3, −0.2≦α≦0.15, and M is at least one element selected from Mn, Al, V, Mg, Mo, Nb, Ti, Zr, Fe, Cu, Cr, Zn, F, and B. This compound will also be referred to as “LiNCM” hereinafter.), LiNi x Mn y O(x+y=1), LiNiO 2 , LiMn 2 O 4 , LiFePO , LiCoPO , LiFeOF , LiNiOF , and TiS 2 The above positive electrode active materials may be used alone or in combination of two or more.
[0044] The positive electrode active material particles of this embodiment include positive electrode active material particles L (hereinafter also referred to as "particles L") having a median diameter D50 (hereinafter also referred to as "D50") of 10 μm to 25 μm, and positive electrode active material particles S (hereinafter also referred to as "particles S"), wherein the D50 ratio of particles S to particles L is 0.75 or less, and the mass ratio in the positive electrode of particles L to particles S ([content of particles L in the positive electrode] / [content of particles S in the positive electrode]) is 1.5 or more and 9.0 or less. Note that the "median diameter" is the particle diameter corresponding to a cumulative degree of 50% in a particle size distribution measured by a laser diffraction / scattering method, and is a particle diameter determined so that the number of particles larger than the median diameter is the same as the number of particles smaller than the median diameter.
[0045] The particle size distribution can be measured by a known method. More specifically, although not particularly limited, it can be measured by, for example, a laser diffraction particle size distribution analyzer.
[0046] The D50 of the particles L is 10.0 μm or more and 25.0 μm or less, preferably 11.0 μm or more and 24.0 μm or less, 12.0 μm or more and 23.0 μm or less, or 13.0 μm or more and 22.0 μm or less. Also, preferably 10.0 μm or more and 20.0 μm or less. When the D50 of the particles L is within the above range, the energy density per volume, cycle characteristics, and rate characteristics tend to be further improved.
[0047] The D50 of the particles S is preferably 0.5 μm or more and 19.0 μm or less, 0.5 μm or more and 15.0 μm or less, 0.5 μm or more and 10.0 μm or less, 1.0 μm or more and 9.0 μm or less, 2.0 μm or more and 8.0 μm or less, 2.5 μm or more and 7.5 μm or less, 3.0 μm or more and 7.0 μm or less, or 3.5 μm or more and 6.5 μm or less. Also, it is preferably 0.5 μm or more and less than 10.0 μm. When the D50 of the particles S is within the above numerical range, the energy density per volume, cycle characteristics, and rate characteristics tend to be further improved.
[0048] The D50 ratio of particles S to particles L ([median diameter D50 of particles S] / [median diameter D50 of particles L]) is 0.75 or less, preferably 0.05 to 0.75, 0.10 to 0.60, 0.10 to 0.50, 0.15 to 0.45, or 0.20 to 0.40. When the D50 ratio of particles S to particles L is within the above ranges, the energy density per volume, cycle characteristics, and rate characteristics tend to be further improved.
[0049] The particles L preferably have a particle diameter D90 (hereinafter also referred to as "D90") corresponding to 90% cumulative density in a particle size distribution measured by a laser diffraction / scattering method of 25.0 μm or less, 13.0 μm or more and 25.0 μm or less, 13.5 μm or more and 24.5 μm or less, or 14.0 μm or more and 24.0 μm or less. When the D90 of the particles L is within the above numerical range, the energy density per volume, cycle characteristics, and rate characteristics tend to be further improved.
[0050] The particles S preferably have a D90 of 19.0 μm or less, 15.0 μm or less, 10.0 μm or less, 1.5 μm or more to 9.0 μm or less, 2.0 μm or more to 8.0 μm or less, 2.5 μm or more to 7.5 μm or less, 3.0 μm or more to 6.5 μm or less, or 3.5 μm or more to 6.0 μm or less. When the D90 of the particles S is within the above numerical range, the energy density per volume, cycle characteristics, and rate characteristics tend to be further improved.
[0051] Preferably, 75% or more of the particles L exist within a range of ±0.5 μm of D50, 80% or more of the particles exist, 85% or more of the particles exist, 90% or more of the particles exist, or 95% or more of the particles exist within a range of ±0.5 μm of D50.
[0052] Preferably, 75% or more of the particles S exist within a range of ±0.5 μm of D50, 80% or more of the particles exist, 85% or more of the particles exist, 90% or more of the particles exist, or 95% or more of the particles exist within a range of ±0.5 μm of D50.
[0053] When the particle size distribution of a mixture of particles L and particles S is measured, there may be, but is not limited to, a maximum in a region where the particle size is 10.0 μm or more, and another maximum in a region where the particle size is 0.75 times the particle size at the maximum, in which case either of the two maximums may be the maximum peak in the particle size distribution, and the other may be the second-largest peak. Alternatively, there may be a maximum in a region where the particle size is 10.0 μm or more, and another maximum in a region where the particle size is 7.5 μm or less, in which case either the maximum in the region where the particle size is 10.0 μm or more or the maximum in the region where the particle size is 7.5 μm or less may be the maximum peak in the particle size distribution, and the other may be the second-largest peak. Alternatively, a maximum value may exist in a region where the particle size is 12.0 μm or more, and a maximum value may also exist in a region where the particle size is 5.0 μm or less, and in this case, either the maximum value in the region where the particle size is 12.0 μm or more or the maximum value in the region where the particle size is 5.0 μm or less may be the maximum value in the particle size distribution, and the other may be the second largest peak.
[0054] The content of the particles L is preferably 30.0 mass% or more and 90.0 mass% or less, 40.0 mass% or more and 85.0 mass% or less, 50.0 mass% or more and 80.0 mass% or less, 55.0 mass% or more and 77.5 mass% or less, or 60.0 mass% or more and 75.0 mass% or less, relative to the total amount of the positive electrode mixture layer 34A. When the content of the particles L is within the above numerical range, the energy density per volume, the cycle characteristics, and the rate characteristics tend to be further improved.
[0055] The content of particles S is preferably 5.0% by mass to 50.0% by mass, 7.5% by mass to 45.0% by mass, 10.0% by mass to 42.5% by mass, 11.0% by mass to 40.0% by mass, or 12.0% by mass to 37.5% by mass, relative to the total amount of positive electrode mixture layer 34A. When the content of particles S is within the above ranges, the energy density per volume, cycle characteristics, and rate characteristics tend to be further improved.
[0056] The content of the positive electrode active material particles is preferably 60.0 mass % to 99.0 mass % both inclusive, 70.0 mass % to 98.5 mass % both inclusive, 80.0 mass % to 98.0 mass % both inclusive, or 85.0 mass % to 97.5 mass % both inclusive, relative to the total amount of the positive electrode mixture layer 34 A. When the content of the positive electrode active material particles is within the above ranges, the energy density per volume, the cycle characteristics, and the rate characteristics tend to be further improved.
[0057] The mass ratio of particles L to particles S in the positive electrode 30 ([content of particles L in positive electrode 30] / [content of particles S in positive electrode 30]) is 1.5 or more and 9.0 or less, preferably 2.0 or more and 9.0 or less, 2.1 or more and 8.0 or less, or 2.2 or more and 7.0 or less. When the mass ratio of particles L to particles S is within the above numerical range, the energy density per volume, cycle characteristics, and rate characteristics tend to be further improved.
[0058] 1.2.2. Binder The positive electrode composite layer 34A of this embodiment contains two or more binders. The inclusion of a binder improves elongation when force is applied to the positive electrode composite layer 34A, i.e., reduces the Young's modulus. When a positive electrode 30 including the current collector film 32A and the positive electrode composite layer 34A formed on the current collector film 32A is pressed, the positive electrode composite layer 34A tends to be more likely to follow the elongation of the current collector film 32A. Therefore, even if the positive electrode 30 is pressed with a greater pressure, the characteristics of the positive electrode tend not to deteriorate. Therefore, it becomes possible to press the positive electrode 30 with a greater pressure, which tends to increase the energy density per volume.
[0059] The binder is not particularly limited, but examples thereof include binder 1 (first binder) having vinylidene fluoride as a repeating unit, binder 2 (second binder) having tetrafluoroethylene as a repeating unit, styrene butadiene rubber, acrylic resin, polyimide resin, etc. Among these, binder 1 and binder 2 are preferred, and it is more preferred to use binder 1 and binder 2 in combination.
[0060] The binder 1 is not particularly limited, but examples thereof include polyvinylidene fluoride, which is a homopolymer of vinylidene fluoride, and modified polyvinylidene fluoride in which functional groups such as hydroxyl groups, amino groups, carbonyl groups, carboxyl groups, phenyl groups, and methyl groups have been introduced into polyvinylidene fluoride. When the positive electrode mixture layer 34A contains the binder 1, the positive electrode mixture layer 34A tends to be more easily bound to the current collector film 32A. The binder 1 described above may be used alone or in combination of two or more types.
[0061] The binder 2 is not particularly limited, but examples thereof include polytetrafluoroethylene, which is a homopolymer of tetrafluoroethylene; modified polytetrafluoroethylene in which functional groups such as hydroxyl groups, amino groups, carbonyl groups, carboxyl groups, phenyl groups, and methyl groups have been introduced into polytetrafluoroethylene; block copolymers, random copolymers, or graft copolymers having tetrafluoroethylene and vinylidene fluoride as repeating units; block copolymers, random copolymers, or graft copolymers having tetrafluoroethylene and hexafluoropropene as repeating units; and block copolymers, random copolymers, or graft copolymers having tetrafluoroethylene, vinylidene fluoride, and hexafluoropropene as repeating units. Since the positive electrode mixture layer 34A contains the binder 2, the flexibility of the positive electrode mixture layer 34A is improved and the Young's modulus is reduced, so that when the positive electrode 30 including the current collector film 32A and the positive electrode mixture layer 34A formed on the current collector film 32A is pressed, the positive electrode mixture layer 34A can more easily follow the elongation of the current collector film 32A, which tends to increase the energy density per volume. The binder 2 as described above may be used alone or in combination of two or more types.
[0062] The binder may be synthesized by a known method, or a commercially available product may be used. Examples of commercially available binder 1 include, but are not limited to, PVDF (2F) manufactured by Kureha Extron Co., Ltd. and Solef (registered trademark) manufactured by Solvay Japan Co., Ltd. Examples of commercially available binder 2 include, but are not limited to, Dyneon fluororubber manufactured by 3M.
[0063] When the positive electrode mixture layer 34A contains the binder 1, the content of the binder 1 is preferably 0.3 mass % to 20.0 mass %, 0.5 mass % to 15.0 mass %, 1.0 mass % to 10.0 mass %, or 1.5 mass % to 7.5 mass %, relative to the total amount of the positive electrode mixture layer 34A. When the content of the binder 1 is within the above range, the positive electrode mixture layer 34A tends to be more easily bound to the current collector film 32A.
[0064] When the positive electrode mixture layer 34A contains the binder 2, the content of the binder 2 is preferably 0.3 mass% to 20.0 mass%, 0.5 mass% to 15.0 mass%, 1.0 mass% to 10.0 mass%, or 1.5 mass% to 7.5 mass%, relative to the total amount of the positive electrode mixture layer 34A. When the content of the binder 2 is within the above range, when the positive electrode 30 including the current collector film 32A and the positive electrode mixture layer 34A formed on the current collector film 32A is pressed, the positive electrode mixture layer 34A can more easily follow the elongation of the current collector film 32A, and the energy density per volume tends to be higher.
[0065] The content of the binder is preferably 0.5% by mass to 20.0% by mass, 1.0% by mass to 15.0% by mass, 1.5% by mass to 10.0% by mass, or 2.0% by mass to 7.5% by mass, relative to the total amount of the positive electrode composite layer 34A. When the content of the binder is within the above range, when the positive electrode 30 including the current collector film 32A and the positive electrode composite layer 34A formed on the current collector film 32A is pressed, the positive electrode composite layer 34A can more easily follow the elongation of the current collector film 32A, and the energy density per volume tends to be higher.
[0066] When the positive electrode composite layer 34A contains the binder 1 and the binder 2, the mass ratio of the binder 2 to the binder 1 in the positive electrode 30 ([content of the binder 2 in the positive electrode 30] / [content of the binder 1 in the positive electrode 30]) is preferably 1.0 or more and 10.0 or less, 1.0 or more and 5.0 or less, 1.0 or more and 2.5 or less, or 1.0 or more and 2.0 or less.
[0067] 1.2.3. Conductive Aid The positive electrode composite layer 34A of this embodiment may contain a conductive aid. Examples of the conductive aid include, but are not limited to, carbon black, single-walled carbon nanotubes (SWCNT), multi-walled carbon nanotubes (MWCNT), carbon nanofibers (CF), and acetylene black. The conductive aids may be used alone or in combination of two or more.
[0068] The content of the conductive additive is not particularly limited, but is, for example, 0.5 mass % or more and less than 30.0 mass % with respect to the total amount of positive electrode mixture layer 34A.
[0069] 1.2.4. Sacrificial Cathode Agent The cathode composite layer 34A of this embodiment may contain a sacrificial cathode agent. The sacrificial cathode agent of this embodiment is a lithium-containing compound that undergoes an oxidation reaction and substantially no reduction reaction within the charge / discharge potential range of the cathode active material. When the cathode 30 of this embodiment contains a sacrificial cathode agent, upon initial charging of a lithium secondary battery including the cathode 30, the cathode active material and the sacrificial cathode agent release lithium ions and undergo an oxidation reaction, releasing electrons to the negative electrode through an external circuit. As a result, lithium ions derived from the cathode active material and the sacrificial cathode agent are deposited on the surface of the negative electrode. Furthermore, upon discharging such a lithium secondary battery after initial charging (i.e., initial discharging), the lithium metal deposited on the negative electrode surface undergoes electrolytic dissolution, and electrons are transferred from the negative electrode to the positive electrode 30 through an external circuit. Accordingly, the positive electrode active material receives lithium ions and undergoes a reduction reaction, while the sacrificial positive electrode agent does not substantially undergo a reduction reaction within the discharge potential range of the positive electrode active material, making it virtually impossible to return to the state before the oxidation reaction. Therefore, when the lithium secondary battery is discharged after the initial charge, lithium metal derived from the positive electrode active material is electrolytically dissolved from the negative electrode, while most of the lithium metal derived from the sacrificial positive electrode agent remains on the negative electrode, resulting in some lithium metal remaining on the negative electrode even after the battery is fully discharged. This residual lithium metal serves as a scaffold for further lithium metal deposition on the negative electrode during the charge step following the initial discharge, making it easier for lithium metal to be uniformly deposited on the negative electrode during the charge step after the initial discharge. As a result, lithium secondary batteries tend to have better cycle characteristics.
[0070] The sacrificial positive electrode agent is not particularly limited, but for example, Li 2 O 2 Lithium oxides such as Li 3 Lithium nitrides such as N; Li 2 S-P 2 S 5 , Li 2 S-LiCl, Li 2 S-LiBr and Li 2 Lithium sulfide-based solid solutions such as S-LiI; Li 1+x (Ti 1-yFe y ) 1-x O 2 (0<x≦0.25, 0.4<y≦0.9), Li 2-x Ti 1-z Fe z O 3-y (0≦x<2, 0≦y≦1, 0.05≦z≦0.95), Li 5 FeO 4 The above-mentioned sacrificial positive electrode agents may be used singly or in combination of two or more.
[0071] The content of the sacrificial positive electrode agent relative to the total amount of the positive electrode mixture layer 34A is not particularly limited, but is, for example, 1.0 mass % or more and 30.0 mass % or less, 2.0 mass % or more and 20.0 mass % or less, or 3.0 mass % or more and 15.0 mass % or less.
[0072] Furthermore, when the positive electrode composite layer 34A contains a sacrificial positive electrode agent, the total amount of the positive electrode active material particles and the sacrificial positive electrode agent is preferably 60.0 mass % or more and 99.0 mass % or less, 70.0 mass % or more and 98.5 mass % or less, 80.0 mass % or more and 98.0 mass % or less, or 85.0 mass % or more and 97.5 mass % or less, relative to the total amount of the positive electrode composite layer 34A.
[0073] 1.3. Positive Electrode Manufacturing Method The positive electrode 30 of this embodiment is manufactured, for example, as follows, without any particular limitation. Metal layers 322A are formed on both surfaces of a resin layer 320A by vapor deposition, sputtering, electrolytic plating, or bonding with an adhesive, thereby obtaining a current collector film 32A of this embodiment. The above-described positive electrode active material particles L, positive electrode active material particles S, two or more binders, and, if necessary, a conductive additive, a sacrificial positive electrode agent, etc., are then mixed to obtain a positive electrode mixture. The obtained positive electrode mixture is applied to one or both surfaces of the current collector film 32A, followed by press molding to form a positive electrode composite layer 34A on one or both surfaces of the current collector film 32A, thereby obtaining a molded body. The obtained molded body is punched to a predetermined size by a punching process, thereby obtaining a positive electrode 30 of this embodiment. The obtained positive electrode 30 may then be further pressed, if necessary.
[0074] The pressure during press molding is not particularly limited, but may be, for example, a linear pressure of 0.8 to 3.5 t / cm, 1.0 to 3.0 t / cm, 1.2 to 2.8 t / cm, or 1.5 to 2.5 t / cm.
[0075] 2. Lithium Secondary Battery The lithium secondary battery of this embodiment includes the above-described positive electrode 30. By including the above-described positive electrode 30, the lithium secondary battery has high safety, high energy density per weight, high energy density per volume, good cycle characteristics, and good rate characteristics.
[0076] The type of lithium secondary battery is not particularly limited as long as it is charged and discharged by an oxidation-reduction reaction of lithium and has a positive electrode 30, and examples thereof include lithium ion batteries, lithium metal batteries, anode-free lithium secondary batteries, lithium sulfur batteries, lithium oxygen batteries, and lithium air batteries.
[0077] Various types of lithium secondary batteries will be described in detail below.
[0078] 2.1 Anode-Free Battery Figure 3 is a schematic cross-sectional view of a lithium secondary battery according to one embodiment of the present invention. As shown in Figure 3, the anode-free battery 100 of this embodiment includes a positive electrode 30B, a negative electrode 10 that does not include a negative electrode active material, a separator 20 disposed between the positive electrode 30B and the negative electrode 10, and an electrolyte solution not shown in Figure 3. The positive electrode 30B has a positive electrode current collector 32A on the surface opposite to the surface facing the separator 20, and a positive electrode composite layer 34A on the surface facing the separator 20. Each component of the anode-free battery 100 will now be described.
[0079] The anode-free lithium secondary battery (hereinafter also referred to as "anode-free battery" or "AFB") of this embodiment has a negative electrode 10 made of a negative electrode current collector without a negative electrode active material, and uses the above-mentioned electrolyte. The negative electrode active material is a material that causes an electrode reaction, i.e., an oxidation reaction and a reduction reaction, at the negative electrode. Specifically, the negative electrode active material of this embodiment includes lithium metal and a host material of lithium element (lithium ion or lithium metal). The host material of lithium element refers to a material provided to retain lithium ion or lithium metal in the negative electrode. Examples of such retention mechanisms include intercalation, alloying, and metal cluster occlusion, and a typical example is intercalation.
[0080] In an anode-free battery, before initial charging of the battery, the negative electrode 10 does not contain a negative electrode active material and consists only of a negative electrode current collector. Therefore, after the initial charging, lithium metal is deposited on the negative electrode 10, and the deposited lithium metal is electrolytically dissolved, thereby performing charging and discharging. Therefore, in an anode-free battery, the volume and mass occupied by the negative electrode active material are reduced, and the volume and mass of the entire battery are reduced, which has the advantage of, in principle, having a high energy density.
[0081] 2.1.1 Negative Electrode The anode-free battery includes a negative electrode 10 made of a negative electrode current collector that does not contain a negative electrode active material.
[0082] In the anode-free battery herein, the anode "has no anode active material" means that the anode has no or substantially no anode active material. The anode 10 has substantially no anode active material means that the content of the anode active material in the anode 10 is 10.0 mass% or less relative to the entire anode 10. The content of the anode active material in the anode 10 of the anode-free battery is preferably 5.0 mass% or less, 1.0 mass% or less, 0.1 mass% or less, or 0.0 mass% relative to the entire anode 10. When the anode 10 has no anode active material or the content of the anode active material in the anode 10 is within the above range, the energy density of the lithium secondary battery is high.
[0083] In the anode-free battery of this specification, the term "before initial charge" refers to the state of the battery from assembly to the first charge, and the term "at the end of discharge" refers to the state of the battery in which the voltage is preferably 1.0 V or more and 3.8 V or less, and more preferably 1.0 V or more and 3.0 V or less.
[0084] In the anode-free battery of this embodiment, when the battery voltage is 1.0 V or more and 3.5 V or less, the lithium metal content may be 10.0 mass % or less (preferably 5.0 mass % or less, or 1.0 mass % or less) with respect to the entire negative electrode 10; when the battery voltage is 1.0 V or more and 3.0 V or less, the lithium metal content may be 10.0 mass % or less (preferably 5.0 mass % or less, or 1.0 mass % or less) with respect to the entire negative electrode 10; or when the battery voltage is 1.0 V or more and 2.5 V or less, the lithium metal content may be 10.0 mass % or less (preferably 5.0 mass % or less, or 1.0 mass % or less) with respect to the entire negative electrode 10.
[0085] In the anode-free battery of this embodiment, the mass M of lithium metal deposited on the negative electrode 10 when the battery voltage is 4.2 V is 4.2 The mass M of lithium metal deposited on the negative electrode 10 when the battery voltage is 3.0 V 3.0 The ratio M 3.0 / M 4.2 is preferably 40.0% or less, 38.0% or less, or 35.0% or less. 3.0 / M 4.2 may be 1.0% or more, 2.0% or more, 3.0% or more, or 4.0% or more.
[0086] Examples of negative electrode active materials include lithium metal and alloys containing lithium metal, carbon-based materials, metal oxides, and metals that alloy with lithium and alloys containing such metals. Examples of carbon-based materials include, but are not limited to, graphene, graphite, hard carbon, and carbon nanotubes. Examples of metal oxides include, but are not limited to, titanium oxide-based compounds and cobalt oxide-based compounds. Examples of metals that alloy with lithium include silicon, germanium, tin, lead, aluminum, and gallium. Alternatively, a negative electrode active material composition may be prepared by mixing a negative electrode active material with a binder such as carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR), and carbon black.
[0087] The negative electrode 10 of the anode-free battery is not particularly limited as long as it does not have a negative electrode active material and can be used as a current collector. For example, it can be made of at least one material selected from the group consisting of Cu, Ni, Ti, Fe, and other metals that do not react with Li, their alloys, and stainless steel (SUS). Preferably, it can be made of at least one material selected from the group consisting of Cu, Ni, their alloys, and stainless steel (SUS). Use of such a negative electrode tends to further improve the energy density and productivity of the battery. The above-mentioned negative electrode materials can be used alone or in combination of two or more. In this specification, the term "metal that does not react with Li" refers to a metal that does not react with lithium ions or lithium metal to form an alloy under the operating conditions of a lithium secondary battery.
[0088] The negative electrode current collector may also include a resin layer and metal layers provided on both sides of the resin layer, similar to the current collector film 32A of the positive electrode 30. The metal layer is not particularly limited as long as it does not contain a negative electrode active material and can be used as a current collector, and examples thereof include those described above. The resin layer may be any of those listed for the positive electrode current collector film.
[0089] The average thickness of the negative electrode 10 of the anode-free battery is not particularly limited, but is, for example, 3.0 μm to 30.0 μm. From the viewpoint of reducing the volume occupied by the negative electrode 10 in the anode-free battery and improving the energy density, the average thickness of the negative electrode 10 is preferably 4.0 μm to 20.0 μm, 5.0 μm to 18.0 μm, or 6.0 μm to 15 μm.
[0090] 2.1.2 Separator The separator 20 of the anode-free battery is not particularly limited as long as it has the function of physically and / or electrically isolating the positive electrode 30 and the negative electrode 10 and the function of ensuring ionic conductivity of lithium ions. Examples of such a separator include insulating porous materials, polymer electrolytes, gel electrolytes, and inorganic solid electrolytes, and typically includes at least one selected from the group consisting of insulating porous materials, polymer electrolytes, and gel electrolytes. Furthermore, as the separator 20, one type of material may be used alone, or two or more types of materials may be used in combination.
[0091] The anode-free battery preferably uses an insulating porous material, a polymer electrolyte, or a gel electrolyte, either singly or in combination, as the separator 20. When an insulating porous material is used alone as the separator 20, the lithium secondary battery must further include an electrolytic solution.
[0092] The polymer electrolyte is not particularly limited, but examples thereof include solid polymer electrolytes mainly containing a polymer and an electrolyte, and semi-solid polymer electrolytes mainly containing a polymer, an electrolyte, and a plasticizer. The gel electrolyte is not particularly limited, but examples thereof include those mainly containing a polymer and a liquid electrolyte (i.e., a solvent and an electrolyte).
[0093] Polymers that may be contained in polymer electrolytes and gel electrolytes include, but are not limited to, polymers containing functional groups containing oxygen atoms such as ethers and esters, halogen groups, and polar groups such as cyano groups. Specific examples include resins having ethylene oxide units in the main chain and / or side chains such as polyethylene oxide (PEO), resins having propylene oxide units in the main chain and / or side chains such as polypropylene oxide (PPO), acrylic resins, vinyl resins, ester resins, nylon resins, polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polysiloxane, polyphosphazene, polymethyl methacrylate, polyamide, polyimide, aramid, polylactic acid, polyurethane, polyacetal, polysulfone, polyethylene carbonate, polypropylene carbonate, and polytetrafluoroethylene. The above-mentioned resins may be used alone or in combination of two or more.
[0094] Examples of electrolytes contained in the polymer electrolyte and gel electrolyte include salts of Li, Na, K, Ca, and Mg. Typically, in this embodiment, the polymer electrolyte and gel electrolyte contain a lithium salt. The lithium salt is not particularly limited, but examples thereof include LiI, LiCl, LiBr, LiF, and LiBF. 4 , LiPF 6 , LiPF 2 O 2 , LiAsF 6 , LiSO 3 CF 3 , LiN(SO 2 F) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 CF 3 CF 3 ) 2 , LiB(O 2 C 2 H 4 ) 2 , LiB(C 2 O 4 ) 2 , LiB(O 2 C 2 H4 ) F 2 , LiB(OCOCF 3 ) 4 , LiNO 3 , and Li 2 SO 4 LiN(SO 2 F) 2 , LiN(SO 2 CF 3 ) 2 , and LiN(SO 2 CF 3 CF 3 ) 2 The salt or lithium salt may be used alone or in combination of two or more thereof.
[0095] The compounding ratio of the polymer to the lithium salt in the polymer electrolyte and the gel electrolyte may be determined by the ratio of the polar group of the polymer to the lithium atom of the lithium salt. For example, when the polymer contains oxygen atoms, the compounding ratio may be determined by the ratio ([Li] / [O]) of the number of oxygen atoms of the polymer to the number of lithium atoms of the lithium salt. In the polymer electrolyte and the gel electrolyte, the compounding ratio of the polymer to the lithium salt can be adjusted so that the ratio ([Li] / [O]) is, for example, 0.02 to 0.20, 0.03 to 0.15, or 0.04 to 0.12.
[0096] The solvent contained in the gel electrolyte is not particularly limited, and for example, the solvents that can be contained in the electrolyte solution described below can be used alone or in combination of two or more. Examples of preferred solvents are the same as those in the electrolyte solution described below. The plasticizer contained in the semi-solid polymer electrolyte is not particularly limited, and examples include the same components as the solvents that can be contained in the gel electrolyte and various oligomers.
[0097] When the separator 20 includes an insulating porous member, the pores of the member are filled with an ion-conductive substance, thereby causing the member to exhibit ion conductivity. Thus, in this embodiment, the pores are filled with, for example, the electrolytic solution of this embodiment or a gel electrolyte containing the electrolytic solution of this embodiment.
[0098] The material constituting the insulating porous member is not particularly limited, and examples thereof include insulating polymer materials, specifically polyethylene (PE) and polypropylene (PP). That is, the separator 20 may be a porous polyethylene (PE) film, a porous polypropylene (PP) film, or a laminated structure thereof.
[0099] The separator 20 may be coated with a separator coating layer. The separator coating layer may cover both sides of the separator 20, or may cover only one side. From the viewpoint of improving the cycle characteristics of the lithium secondary battery of this embodiment, it is preferable to coat both sides of the separator 20. Note that the separator coating layer of this embodiment is a uniformly continuous film-like coating layer, for example, a film-like coating layer that is uniformly continuous over an area of 50% or more of the surface of the separator 20.
[0100] The separator coating layer is not particularly limited, and is preferably made of a material containing a binder such as polyvinylidene fluoride (PVdF), a mixture of styrene butadiene rubber and carboxymethyl cellulose (SBR-CMC), and polyacrylic acid (PAA). The separator coating layer may contain inorganic particles such as silica, alumina, titania, zirconia, or magnesium hydroxide added to the binder.
[0101] The average thickness of the separator 20 including the separator coating layer is not particularly limited, but is, for example, 3.0 μm to 40.0 μm. In a lithium secondary battery, from the viewpoint of reliably isolating the positive electrode 30 and the negative electrode 10 while reducing the volume occupied by the separator 20 in the battery, the average thickness of the separator 20 is preferably 5.0 μm to 30.0 μm, 7.0 μm to 10.0 μm, or 10.0 μm to 20.0 μm.
[0102] The electrolyte for the anode-free battery is a liquid containing a solvent and an electrolyte, and is not particularly limited as long as it has ionic conductivity. The electrolyte may be impregnated into the separator 20, or the finished anode-free battery may be formed by sealing the electrolyte together with a laminate of the negative electrode 10, the separator 20, and the positive electrode 30.
[0103] The electrolyte contained in the electrolytic solution may be any of the electrolytes that can be contained in polymer electrolytes and gel electrolytes, particularly the lithium salts described above, which may be used alone or in combination of two or more. Preferred lithium salts are the same as those used in the polymer electrolyte and gel electrolyte.
[0104] Examples of the solvent contained in the electrolytic solution include a non-aqueous solvent containing fluorine atoms (hereinafter referred to as a "fluorinated solvent") and a non-aqueous solvent containing no fluorine atoms (hereinafter referred to as a "non-fluorinated solvent").
[0105] The fluorinated solvent is not particularly limited, but examples thereof include 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether, etc. The non-fluorinated solvent is not particularly limited, but examples thereof include triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dimethoxyethane, dimethoxypropane, dimethoxybutane, diethylene glycol dimethyl ether, acetonitrile, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, chloroethylene carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, trimethyl phosphate, triethyl phosphate, and 12-crown-4.
[0106] The above-mentioned fluorinated solvents and / or non-fluorinated solvents can be used alone or in any combination of two or more kinds in any ratio. The contents of the fluorinated solvent and the non-fluorinated solvent are not particularly limited, and the ratio of the fluorinated solvent to the total solvent may be 0 to 100% by volume, or the ratio of the non-fluorinated solvent to the total solvent may be 0 to 100% by volume.
[0107] 2.1.4. Usage Mode One usage mode of a lithium secondary battery, including an anode-free battery, will be described. In one usage mode of a lithium secondary battery, a positive electrode terminal and a negative electrode terminal for connecting the battery to an external circuit are joined to the current collector film 32A and the negative electrode 10, respectively. The lithium secondary battery is charged and discharged by connecting the negative electrode terminal to one end of the external circuit and the positive electrode terminal to the other end of the external circuit. The lithium secondary battery is charged by applying a voltage to the positive electrode terminal and the negative electrode terminal such that a current flows from the negative electrode terminal (negative electrode) through the external circuit to the positive electrode terminal (positive electrode). After charging, the lithium secondary battery is discharged by connecting the positive electrode terminal and the negative electrode terminal via the desired external circuit.
[0108] In an anode-free battery, it is presumed that a solid electrolyte interface layer (SEI layer) is formed on the surface of the negative electrode 10 (the interface between the negative electrode 10 and the separator 20) upon initial charging, but the battery does not necessarily have to have an SEI layer. Charging an anode-free battery causes lithium metal deposition at the interface between the negative electrode 10 and the SEI layer, the interface between the negative electrode 10 and the separator 20, and / or the interface between the SEI layer and the separator 20. Furthermore, in an anode-free battery, the lithium metal deposition formed on the negative electrode 10 undergoes electrolytic dissolution upon discharge. When an SEI layer is formed in the battery, the lithium metal deposition formed at at least one of the interface between the negative electrode 10 and the SEI layer and / or the interface between the SEI layer and the separator 20 undergoes electrolytic dissolution.
[0109] 2.1.5. Manufacturing Method The manufacturing method of the anode-free battery is not particularly limited as long as it is a method that can manufacture a lithium secondary battery having the above-described configuration, and examples thereof include the following methods.
[0110] First, the positive electrode 30 of this embodiment is obtained by the above-described method for producing a positive electrode.
[0111] Next, the negative electrode material of the above-described anode-free battery, for example, a metal foil (e.g., electrolytic Cu foil) having a thickness of 1.0 μm or more and 1.0 mm or less, is washed with a solvent containing sulfamic acid, and then punched out to a predetermined size. The punched piece is then subjected to ultrasonic cleaning with ethanol and then dried to obtain the negative electrode 10.
[0112] Next, the separator 20 having the above-described configuration is prepared. The separator 20 may be manufactured by a conventionally known method, or a commercially available separator may be used. In addition, a fibrous or porous functional buffer layer may be provided between the separator 20 and the negative electrode 10 to mitigate volume expansion and contraction associated with the dissolution and precipitation of lithium metal. The functional buffer layer preferably has ionic conductivity or electrical conductivity, but does not necessarily have to have such conductivity.
[0113] The positive electrode 30, separator 20, and negative electrode 10 thus obtained are stacked in this order so that the positive electrode 30 faces the separator 20 to obtain a laminate. The resulting laminate is sealed together with an electrolyte in a sealed container to obtain an anode-free battery. The sealed container is not particularly limited, but examples thereof include a laminate film.
[0114] 2.2. Lithium Metal Battery A lithium metal battery (hereinafter also referred to as "LMB") is manufactured using an electrode having lithium metal or a lithium metal alloy on its surface, or using lithium metal alone as the negative electrode. The LMB of this embodiment has the positive electrode 30 of this embodiment. As with anode-free batteries, the LMB is charged and discharged by deposition of lithium metal on the surface of the negative electrode and electrolytic leaching of the deposited lithium.
[0115] As mentioned above, LMBs differ from anode-free batteries in that the negative electrode has lithium metal as the negative electrode active material before the initial charge of the battery.
[0116] The lithium metal battery of this embodiment includes the positive electrode 30 of this embodiment, a negative electrode having lithium metal facing the positive electrode 30, a separator disposed between the positive electrode 30 and the negative electrode, and an electrolyte. The configurations and preferred aspects of the electrolyte and separator are the same as those of an anode-free battery, except for the points described below.
[0117] The negative electrode of the LMB is not particularly limited as long as it contains lithium metal or a lithium metal alloy. Because the LMB uses a negative electrode containing lithium metal or a lithium metal alloy with a large specific capacity and a low redox potential, the battery generally has a higher energy density than a lithium-ion battery. Examples of such negative electrodes include a lithium metal electrode, an electrode in which rolled lithium metal foil is laminated onto the surface of a conductive metal foil such as copper to form a clad material, an electrode in which lithium metal is electrochemically deposited on the surface of a metal foil such as copper, and an electrode in which metallic lithium is vacuum-deposited. From the viewpoint of further improving the effects of this embodiment, an electrode in which lithium metal foil is laminated onto the surface of a conductive metal such as copper, or an electrode in which lithium metal is electrochemically deposited, is preferred, and an electrode in which lithium metal foil is laminated onto the surface of a conductive metal such as copper is more preferred.
[0118] The average thickness of the LMB negative electrode is not particularly limited, but is, for example, 5.0 μm to 100.0 μm. From the viewpoint of improving the capacity and / or energy density of the battery, it is preferably 8.0 μm to 50.0 μm, 10.0 μm to 40.0 μm, or 10.0 μm to 20.0 μm.
[0119] The LMB may be fabricated using known materials and known fabrication methods, and may be fabricated in the same manner as the anode-free battery described above, except that lithium metal or a lithium metal alloy is used for the negative electrode.
[0120] 2.3 Lithium-Ion Batteries Lithium-ion batteries (hereinafter also referred to as "LIBs") have a host material of lithium element (lithium ions or lithium metal) in their negative electrode. When the battery is charged, the material is filled with lithium element, and the host material releases lithium element, thereby discharging the battery. LIBs differ from anode-free batteries, particularly in that the negative electrode contains a host material of lithium element. Lithium-ion batteries can be manufactured using known materials and manufacturing methods.
[0121] The shape of the battery of the lithium secondary battery of this embodiment is not particularly limited, and may be, for example, a sheet type, a laminated sheet type, a thin shape, a cylindrical shape with a bottom, a prismatic shape with a bottom, etc. From the viewpoint of more effectively and reliably achieving the effects of this embodiment, the sheet type, laminated sheet type, or thin shape is preferred.
[0122] The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited to the following examples. 5 It was conducted in Pa.
[0123] 1. Fabrication of Anode-Free Lithium Secondary Battery An anode-free lithium secondary battery (AFB) of Example 1 was fabricated as follows.
[0124] 1.1. Preparation of Negative Electrode First, a rolled Cu foil having a thickness of 10 μm was prepared and punched out to a predetermined size (45 mm×45 mm) by a punching process to obtain a negative electrode 10 .
[0125] 1.2. Preparation of the Positive Electrode The material for the positive electrode active material particles is LiNi. 0.85 Co 0.12 Mn 0.03 O 2The large particles and small particles were prepared so that their particle sizes (D50) were the values shown in Table 1. Specifically, large particles and small particles were obtained by sieving the positive electrode active material particles. As a result of sieving, 80% of the large particles and small particles were contained within a range of ±0.5 μm of the target particle size (D50). The particle size distribution was measured using a laser diffraction particle size distribution analyzer, "MT-3000 manufactured by Microtrackbell Corporation." 100 parts by mass of a positive electrode mixture was prepared by mixing 96 parts by mass of the large particles and small particles thus prepared in the mass ratios shown in Table 1 with 2 parts by mass of Binder 1 and 2 parts by mass of Binder 2.
[0126] Regarding large particles and small particles, the larger one is referred to as the large particle and the other as the small particle, comparing D50. Among the large particles, particles with a D50 of 10 μm or more and 25 μm or less are called particles L, and among the small particles, when the ratio of the median diameter D50 of the small particle to the particle L is 0.75 or less, the small particle is called particle S.
[0127] Next, a 1 μm thick film of Al was deposited on both sides of the resin layer 320A, which was a 6 μm thick polyethylene terephthalate (PET) film, to form the metal layer 322A, to obtain a current collector film 32A. Then, a 20 mg / cm2 film was deposited on both sides of the current collector film 32A. 2 The positive electrode mixture was applied to the current collector film 32A at a linear pressure of 2 t / cm, and the positive electrode mixture was applied to the current collector film 32A at a linear pressure of 2 t / cm so as to obtain a density after pressing shown in Table 1. The positive electrode mixture was applied to the current collector film 32A at a linear pressure of 2 t / cm, and a positive electrode mixture layer 34A was formed on both sides of the current collector film 32A, thereby obtaining a molded body. The obtained molded body was punched out into a size of 40 × 40 mm by a punching process, and a positive electrode 30 was obtained.
[0128] 1.3. Preparation of Separator A separator 20 having a predetermined size (50 mm x 50 mm) was prepared, in which both sides of a 12 μm polyethylene microporous film were coated with 2.0 μm polyvinylidene fluoride (PVdF).
[0129] 1.4. Preparation of Electrolyte As the electrolyte, 4M LiN(SO 2 F) 2 A solution of (LiFSI) in dimethoxyethane (DME) was prepared.
[0130] 1.5. Battery Assembly Next, the positive electrode 30, separator 20, and negative electrode 10 were stacked in this order to obtain a laminate. A 100 μm Al terminal and a 100 μm Ni terminal were ultrasonically welded to the current collector film 32A of the positive electrode 30 and the negative electrode 10, respectively, and then inserted into a laminate exterior. The above-mentioned electrolyte solution was then injected into the exterior. The exterior was sealed to obtain a lithium secondary battery.
[0131] Lithium secondary batteries of Examples 2 to 9 and Comparative Examples 1 to 5 were obtained in the same manner as Example 1, except that the large particles, small particles, and binders listed in Table 1 were used and press-molded at the pressures listed in Table 1. In Comparative Example 4, a mass ratio of 10 / 0 and a particle size ratio of 1.00 indicate that one type of positive electrode active material particle was used from the perspective of D50. Specifically, in Comparative Example 4, 96 parts by mass of positive electrode active material particles having a D50 of 15 μm, 2 parts by mass of binder 1, and 2 parts by mass of binder 2 were mixed to prepare 100 parts by mass of a positive electrode mixture.
[0132] The abbreviations in Table 1 correspond to the following compounds: PVdF: polyvinylidene fluoride VDF: vinylidene fluoride TFE: tetrafluoroethylene HFP: hexafluoropropene PTFE: polytetrafluoroethylene
[0133] In Table 1, AFB refers to an anode-free battery. The mass ratio (large particles / small particles) refers to the mass ratio of large particles to small particles in the positive electrode 30 ([content of large particles in the positive electrode 30] / [content of small particles in the positive electrode 30]). The particle size ratio (small particles / large particles) refers to the D50 ratio of small particles to large particles ([median diameter D50 of small particles] / [median diameter D50 of large particles]). The particle size (large particles) refers to the median diameter D50 of large particles.
[0134] The binders shown in Table 1 were prepared as follows: Solef 5130 manufactured by Solvay was used as binder 1. Binder 2 was prepared by mixing VDF, TFE, and HFP and subjecting the mixture to suspension polymerization.
[0135] 2. Evaluation 2.1 Discharge Rate (Rate Characteristics) The fabricated lithium secondary battery was CC charged at a current of 3 mA until the voltage reached 4.2 V, and then CC discharged at a current of 3 mA until the voltage reached 3.0 V (first cycle). CC charging refers to charging at a constant current value, and CC discharging refers to discharging at a constant current value.
[0136] Following the first cycle, the battery was CC charged at 3 mA to a voltage of 4.2 V, then CC discharged at 6 mA to a voltage of 3.0 V (second cycle). Following the second cycle, the battery was CC charged at 3 mA to a voltage of 4.2 V, then CC discharged at 30 mA to a voltage of 3.0 V (third cycle). Following the third cycle, the battery was CC charged at 3 mA to a voltage of 4.2 V, then CC discharged at 60 mA to a voltage of 3.0 V (fourth cycle). Following the fourth cycle, the battery was CC charged at 3 mA to a voltage of 4.2 V, then CC discharged at 120 mA to a voltage of 3.0 V (fifth cycle). Following the fifth cycle, the battery was CC charged at a current of 3 mA until the voltage reached 4.2 V, and then CC discharged at a current of 180 mA until the voltage reached 3.0 V (sixth cycle).
[0137] The ratio ([6th capacity] / [2nd capacity]) of the discharge capacity obtained from the CC discharge in the 6th cycle (hereinafter also referred to as the “6th capacity”) to the discharge capacity obtained from the CC discharge in the 2nd cycle (hereinafter also referred to as the “2nd capacity”) was calculated and recorded in the “Discharge Rate” column in Table 1.
[0138]
[0139] 3. Evaluation Results From Table 1, it can be seen that a current collector film 32A including a resin layer 320A and metal layers 322A provided on both sides of the resin layer 320A, and a positive electrode mixture layer 34A formed on the current collector film 32A, the positive electrode mixture layer 34A including positive electrode active material particles L having a median diameter D50 of 10 μm or more and 25 μm or less, positive electrode active material particles S, and two or more binders, and the median diameter D50 ratio of the positive electrode active material particles S to the positive electrode active material particles L is , 0.75 or less, and the mass ratio in the positive electrode of the positive electrode active material particles L to the positive electrode active material particles S ([content of the positive electrode active material particles L in the positive electrode] / [content of the positive electrode active material particles S in the positive electrode]) is 1.5 or more and 9.0 or less, it can be seen that Examples 1 to 9, which are lithium secondary batteries using a positive electrode 30 for a lithium secondary battery, exhibit a good discharge rate compared to the comparative example of a lithium secondary battery using a positive electrode other than that.
[0140] 4. Fabrication of Lithium-ion Battery Next, we investigated the fabrication of lithium-ion batteries.
[0141] A lithium ion battery (LIB) of Example 10 was fabricated as follows.
[0142] First, a negative electrode was prepared. A 1.0 μm thick Cu film was deposited on both sides of a 6 μm thick polyethylene terephthalate (PET) sheet to prepare a negative electrode current collector film. The negative electrode active material was a mixture of 97 parts by weight of graphite, 0.5 parts by weight of carbon black as a conductive additive, and 1.5 parts by weight of carboxymethyl cellulose (CMC) and 1.0 part by weight of styrene-butadiene rubber (SBR) as binders, mixed with water as a solvent. This mixture was applied to both sides of the negative electrode current collector film in a basis weight of 15 mg / cm. 2 The negative electrode was then fabricated by applying the coating, pressing, and cutting to a predetermined size. 2 O 3 A sheet (thickness: 15 μm) was prepared whose surface was coated with the mixture of the above. Then, both sides of the negative electrode were sandwiched between separators and pressed together to obtain an intermediate laminate.
[0143] Next, a positive electrode was fabricated. The material for the positive electrode active material particles was LiNi. 0.85 Co 0.12 Mn 0.03 O 2 The large particles and small particles were prepared so that their particle sizes (D50) were the values shown in Table 2. Specifically, the large particles and small particles were obtained by sieving the positive electrode active material particles. As a result of sieving, 80% of the large particles and small particles were contained within a range of ±0.5 μm of the target particle size (D50). The particle size distribution was measured using a laser diffraction particle size distribution analyzer, "MT-3000 manufactured by Microtrackbell Corporation." 100 parts by mass of a positive electrode mixture was prepared by mixing 96 parts by mass of the large particles and small particles thus prepared in the mass ratios shown in Table 2 with 2 parts by mass of Binder 1 and 2 parts by mass of Binder 2 shown in Table 2.
[0144] A 6 μm thick film of PET was vapor-deposited with 1.0 μm of Al on both sides, and a film of 23 mg / cm2 was applied to both sides. 2 The positive electrode mixture was applied to the positive electrode sheet by a pressure of 2 t / cm, and then pressed to obtain a molded body so as to have the density after pressing shown in Table 2. The obtained molded body was punched out to a predetermined size by a punching process, to obtain a positive electrode.
[0145] Next, 21 intermediate laminates and 20 positive electrode laminates were alternately stacked. The positive electrode tabs were made of 0.2 mm thick hard aluminum. The negative electrode tabs were made of 0.2 mm thick nickel-plated copper. This structure was inserted into a laminate exterior and sealed together with an electrolyte to obtain a lithium-ion battery. The electrolyte was prepared by dissolving lithium hexafluorophosphate (LiPF) in a 30:35:35 mass part mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) to a 1 M solution. 6 The electrolyte used was prepared by adding 2 parts by mass of vinylene carbonate (VC) to 100 parts by mass of an electrolyte solution in which 1,2-dimethyl-3-pyrrolidone (DMSO) was dissolved.
[0146] 5. Evaluation The discharge rate was evaluated in the same manner as in Table 1.
[0147]
[0148] 6. Evaluation Results Table 2 shows that a lithium ion battery also exhibits a good discharge rate when using a positive electrode for a lithium secondary battery that includes a current collector film including a resin layer and metal layers provided on both sides of the resin layer, and a positive electrode composite layer formed on the current collector film, wherein the positive electrode composite layer includes positive electrode active material particles L and positive electrode active material particles S, each having a median diameter D50 of 10 μm or more and 25 μm or less, and positive electrode active material particles S, and two or more binders, wherein the median diameter D50 ratio of the positive electrode active material particles S to the positive electrode active material particles L is 0.75 or less, and the mass ratio in the positive electrode of the positive electrode active material particles L to the positive electrode active material particles S ([content of the positive electrode active material particles L in the positive electrode] / [content of the positive electrode active material particles S in the positive electrode]) is 1.5 or more and 9.0 or less. Industrial Applicability
[0149] A lithium secondary battery produced using the positive electrode of the present invention has excellent rate characteristics and is therefore industrially applicable as a positive electrode for lithium secondary batteries used in a variety of applications.
[0150] 100... Lithium secondary battery, 10... Negative electrode, 20... Separator, 30A, B... Positive electrode, 32A... Current collector film, 320A... Resin layer, 322A... Metal layer, 34A... Positive electrode composite layer
Claims
1. A current collector film including a resin layer and a metal layer provided on both sides of the resin layer; and a positive electrode composite layer formed on the current collector film, wherein the positive electrode composite layer includes first positive electrode active material particles having a median diameter D50 of 10 μm or more and 25 μm or less, second positive electrode active material particles, and two or more types of binders, wherein a median diameter D50 ratio of the second positive electrode active material particles to the first positive electrode active material particles ([median diameter D50 of the second positive electrode active material particles] / [median diameter D50 of the first positive electrode active material particles]) is 0.75 or less, a mass ratio in the positive electrode of the first positive electrode active material particles to the second positive electrode active material particles ([content of the first positive electrode active material particles in the positive electrode] / [content of the second positive electrode active material particles in the positive electrode]) is 1.5 or more and 9.0 or less.
2. The positive electrode for a lithium secondary battery according to claim 1, wherein the metal layer is made of aluminum.
3. The positive electrode for a lithium secondary battery according to claim 1, wherein a mass ratio in the positive electrode of the first positive electrode active material particles to the second positive electrode active material particles ([content of the first positive electrode active material particles in the positive electrode] / [content of the second positive electrode active material particles in the positive electrode]) is 2.0 or more and 9.0 or less.
4. The positive electrode for a lithium secondary battery according to claim 1, wherein the median diameter D50 ratio of the second positive electrode active material particles to the first positive electrode active material particles is 0.1 or more and 0.5 or less.
5. The positive electrode for a lithium secondary battery according to claim 1, wherein the first positive electrode active material particles have a median diameter D50 of 10 μm or more and 20 μm or less.
6. The positive electrode for a lithium secondary battery according to claim 1, wherein the binder comprises a first binder having vinylidene fluoride as a repeating unit and a second binder having tetrafluoroethylene as a repeating unit.
7. The positive electrode for a lithium secondary battery according to claim 1, wherein a mass ratio in the positive electrode of the second binder to the first binder ([content of the second binder in the positive electrode] / [content of the first binder in the positive electrode]) is 1.0 or more and 10.0 or less.
8. A lithium secondary battery comprising the positive electrode according to any one of claims 1 to 7.
Citation Information
Patent Citations
Thin film magnetic head
JP1989102711A
Lithium ion secondary battery
JP1999102711A
Lithium ion secondary battery
JP2013065468A
Lithium ion secondary battery
WO2009157263A1
Electrode mixture
WO2013176093A1
Cited By
Lithium secondary battery and manufacturing method thereof
WO2026116662A1