Iron-based mixed powder and oxygen reactant

The iron-based mixed powder with manganese sulfide and controlled sulfur content addresses the challenge of hydrogen gas suppression in oxygen reactants, ensuring high reactivity and preventing material damage and odor issues, while simplifying the manufacturing process.

WO2024236860A1PCT designated stage expired Publication Date: 2024-11-21JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/001240
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-01-18
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing iron-based oxygen reactants and exothermic agents face challenges in suppressing hydrogen gas generation during storage, which can lead to material expansion and bursting, and require complex manufacturing processes, such as heating treatments with sulfur.

Method used

An iron-based mixed powder with a sulfur content of 10.000% to 100.000% by mass and a manganese sulfide powder, having an atomic ratio of O/Fe of 0.800 or less, is developed to enhance reactivity with oxygen while minimizing hydrogen gas generation, using a combination of iron-based powder and sulfur-containing powder with a specific particle size and composition.

Benefits of technology

The solution allows for easy production of high-reactivity oxygen reactants that effectively suppress hydrogen gas generation and hydrogen sulfide production, preventing material damage and odor issues, while maintaining excellent exothermic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

Provided are an iron-based mixed powder and an oxygen reactant which can be easily produced, have high reactivity with oxygen, and are inhibited from generating hydrogen gas. The iron-based mixed powder comprises an iron-based powder having a ratio of the number of oxygen atoms to the number of iron atoms, O / Fe, of 0.800 or less and a sulfur-containing powder having a sulfur content of 10.000-100.000 mass%, wherein the content of the sulfur-containing powder is 0.020-5.000 mass% with respect to the sum of the content of the iron-based powder and the content of the sulfur-containing powder.
Need to check novelty before this filing date? Find Prior Art

Description

Iron-based mixed powder and oxygen reactant

[0001] The present disclosure relates to an iron-based mixed powder and an oxygen reactant.

[0002] Oxygen reactants that utilize the reaction between iron-based powder and oxygen are used, for example, as oxygen scavengers or heat generating agents. Oxygen scavengers can create a low-oxygen state inside a container by sealing them together with preserved items such as food or medicines, and are therefore used to prevent quality deterioration of the preserved items due to oxidation or the growth of aerobic mold, etc. Heat generating agents are widely used, for example, in disposable hand warmers. As the oxygen reactant, water, activated carbon, sodium chloride, etc. are added to the iron-based powder to further promote the reaction with oxygen. In addition, additives may be added to the oxygen reactant to adjust the reaction rate and the amount of heat generated, as well as to treat by-product gases such as hydrogen.

[0003] Oxygen absorbers and heat generating agents are often stored sealed in non-breathable packaging immediately after production. However, if oxygen remains in the packaging, oxidation of the iron progresses. As this oxidation occurs, the moisture added to the oxygen absorber or heat generating agent decomposes, generating hydrogen gas. If a large amount of hydrogen gas is generated, the packaging may expand and even explode. Therefore, it is necessary to suppress the generation of hydrogen gas.

[0004] Patent Document 1 discloses a hand warmer. The hand warmer uses iron powder treated with sulfur as the oxidizable agent. Specifically, the oxidizable agent is produced by heating sulfur powder and iron powder, by heating iron powder coated with a sulfur solution or by immersing iron powder in a sulfur solution and then drying the coated iron powder, or by heating iron powder in a solution in which sulfur is dissolved in a solvent. Patent Document 1 discloses the effect of using iron powder treated with sulfur, which reduces the amount of gas generated.

[0005] Patent Document 2 relates to a raw iron powder for a slow-heat-generating composition and a method for producing the same. The raw iron powder is mixed with a reaction aid, water, and a water retention agent to form a composition that slowly heats up in the atmosphere. The raw iron powder is prepared by adding 1 g of iron powder to 100 ml of water, stirring the mixture, and measuring the pH of the supernatant to 8 to 10. Thiosulfate powder is then added to the iron powder to achieve a sulfur content of 0.001% to 0.2% by weight. Patent Document 2 discloses that the use of the raw iron powder effectively suppresses hydrogen gas generation during storage without adding large amounts of substances that adversely affect the heat-generating properties of the slow-heat-generating composition.

[0006] JP-A No. 58-32762 JP-A No. 8-183951

[0007] However, the oxidizable agent disclosed in Patent Document 1 requires heating for treatment using sulfur, which complicates the manufacturing process. Also, there is a demand for effective use of other sulfur-containing powders, not limited to the thiosulfate powder disclosed in Patent Document 2.

[0008] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide an iron-based mixed powder and an oxygen reactant that can be easily produced, have high reactivity with oxygen, and are suppressed in generating hydrogen gas.

[0009] In order to achieve the above object, the iron-based mixed powder and oxygen reactant according to the present disclosure are as follows.

[0010] [1] A mixed powder comprising an iron-based powder having an oxygen to iron atomic ratio (O / Fe) of 0.800 or less, and a sulfur-containing powder having a sulfur content of 10.000 mass% or more and 100.000 mass% or less, wherein the content of the sulfur-containing powder is 0.020 mass% or more and 5.000 mass% or less with respect to the total content of the iron-based powder and the sulfur-containing powder.

[0011] [2] The iron-based mixed powder according to the above [1], wherein the sulfur-containing powder contains manganese sulfide powder.

[0012] [3] The iron-based mixed powder according to the above [1] or [2], wherein the median diameter on a volume basis is 70 μm or more and 100 μm or less.

[0013] [4] An oxygen reactant comprising an iron-based mixed powder comprising an iron-based powder having an oxygen to iron atomic ratio O / Fe of 0.800 or less, and a sulfur-containing powder having a sulfur content of 10.000 mass% or more and 100.000 mass% or less, wherein the content of the sulfur-containing powder is 0.020 mass% or more and 5.000 mass% or less with respect to the total content of the iron-based powder and the content of the sulfur-containing powder.

[0014] [5] The oxygen reactant according to the above [4], wherein the sulfur-containing powder contains manganese sulfide powder.

[0015] [6] The oxygen reactant according to the above [4] or [5], wherein the iron-based mixed powder has a volumetric median diameter of 70 μm or more and 100 μm or less.

[0016] According to the present disclosure, it is possible to provide an iron-based mixed powder and an oxygen reactant that can be easily produced, have high reactivity with oxygen, and suppress the generation of hydrogen gas.

[0017] An iron-based mixed powder and an oxygen reactant according to an embodiment of the present disclosure will be described. Hereinafter, "iron-based powder" refers to a powder containing 50.000 mass% or more of Fe. "Iron-based alloy powder" refers to an alloy powder containing 50.000 mass% or more of Fe. "Iron powder" refers to a powder consisting of Fe and inevitable impurities, and is generally referred to as "pure iron powder" in this technical field.

[0018] The iron-based mixed powder according to this embodiment is a mixed powder comprising an iron-based powder having an oxygen to iron atomic ratio O / Fe of 0.800 or less, and a sulfur-containing powder having a sulfur content of 10.000 mass% or more and 100.000 mass% or less. The content of the sulfur-containing powder in the iron-based mixed powder according to this embodiment is 0.020 mass% or more and 5.000 mass% or less with respect to the total content of the iron-based powder and the sulfur-containing powder.

[0019] The oxygen reactant according to this embodiment includes the iron-based mixed powder.

[0020] The iron-based mixed powder according to this embodiment is suitable for use as an oxygen reactant because it has high reactivity with oxygen and can suppress the generation of hydrogen gas.

[0021] The iron-based mixed powder and the oxygen reactant according to this embodiment will be described in detail below.

[0022] The iron-based mixed powder according to this embodiment is a powder in which an iron-based powder and a sulfur-containing powder are mixed together. The iron-based mixed powder is made up of an iron-based powder and a sulfur-containing powder.

[0023] Examples of the iron-based powder include iron powder and iron-based alloy powder. When the iron-based powder is an iron-based alloy powder, it may further contain elements such as C, S, O, N, Si, Na, Mg, and Ca in addition to Fe. When the iron-based powder is an iron powder, it may contain elements such as C, S, O, N, Si, Na, Mg, and Ca as inevitable impurities.

[0024] When iron is oxidized, its reactivity with oxygen decreases. Therefore, it is preferable to use an iron-based powder that is as non-oxidized as possible. Specifically, in order to ensure the amount of reaction with oxygen, the atomic ratio of oxygen to iron in the iron-based powder (hereinafter, sometimes referred to as O / Fe) is 0.800 or less, preferably 0.700 or less, more preferably 0.600 or less, and even more preferably 0.250 or less. There is no restriction on the lower limit of O / Fe. O / Fe may be 0 or 0.000. However, in consideration of industrial productivity, O / Fe is preferably 0.030 or more, more preferably 0.150 or more.

[0025] The O / Fe ratio of the iron-based powder is measured by X-ray diffraction, specifically by the method described in the examples.

[0026] The method for producing the iron-based powder is not particularly limited, and the powder can be produced by a conventional method. For example, the iron-based powder can be produced by an atomization method, a reduction method, or the like. The atomization method is a method in which water or gas is sprayed onto a molten metal, which is then pulverized and cooled to solidify. Either a water atomization method or a gas atomization method can be used. The reduction method is, for example, a method in which iron oxide (mill scale) or iron ore powder generated on the surface of a steel sheet during hot rolling of the steel material is reduced. That is, the iron-based powder can be an atomized iron-based powder or a reduced iron-based powder. The iron-based powder can be a water atomized iron-based powder or a gas atomized iron-based powder.

[0027] Furthermore, the particle size of the powder may be adjusted by subjecting the powder to one or both of pulverization and classification. The pulverization and classification methods are not particularly limited, and can be carried out by conventional methods.

[0028] In order to remove oxygen from the above-mentioned powder and make the O / Fe ratio of the iron-based powder 0.800 or less, the powder may be heat-treated (deoxidized) using a reducing agent at a maximum temperature of 750°C or higher. The reducing agent may be, for example, carbon such as coke, coal, or graphite, or hydrogen gas. The reducing agent may be added to or mixed with the above-mentioned powder.

[0029] The sulfur-containing powder in this embodiment is preferably a powder containing one or both of elemental sulfur and a sulfur compound. The sulfur-containing powder may be composed of elemental sulfur or a sulfur compound. That is, the sulfur-containing powder preferably contains one or both of a powder of elemental sulfur and a powder of a sulfur compound, and the sulfur-containing powder may be a powder of elemental sulfur or a powder of a sulfur compound. Furthermore, the sulfur contained in the sulfur-containing powder may be derived only from one or both of elemental sulfur and a sulfur compound. In the following description, the term "sulfur powder" refers to a powder of elemental sulfur.

[0030] Examples of the sulfur compound include sulfides. Examples of the sulfides include manganese sulfide, calcium sulfide, sodium sulfide, and nickel sulfide. That is, the sulfur-containing powder may contain any of manganese sulfide powder, calcium sulfide powder, sodium sulfide powder, and nickel sulfide powder, and may be any of manganese sulfide powder, calcium sulfide powder, sodium sulfide powder, and nickel sulfide powder. For example, when a deliquescent sulfur compound such as thiosulfate is used, it may absorb moisture from the air and supply moisture to the surrounding iron particles after mixing, which may cause rust in the iron-based powder before use. From the perspective of preventing deterioration of properties due to rust, the sulfur-containing powder preferably contains one or both of sulfide and elemental sulfur, and more preferably one or both of sulfide powder and sulfur powder. Among sulfides, manganese sulfide powder has a higher specific gravity than sulfur powder and is closer to the iron-based powder, making it easily mixable with the iron-based powder. Furthermore, manganese sulfide is less flammable than calcium sulfide, making it easier to store. Therefore, the sulfur-containing powder preferably contains manganese sulfide, and more preferably is manganese sulfide powder.

[0031] The sulfur-containing powder may also contain, for example, an additive. The additive may or may not contain sulfur. Examples of the additive include silica and carbon. That is, the sulfur-containing powder may contain silica powder or may contain carbonaceous powder. Silica powder is an inert powder that does not contribute to the reaction between iron and oxygen and can be added to more uniformly mix elemental sulfur and sulfur compounds with the iron-based powder. Carbonaceous powder can be added to further promote the reaction between iron and oxygen. Examples of the carbonaceous powder include activated carbon powder, coke powder, carbon black powder, acetylene black powder, and graphite powder.

[0032] The sulfur-containing powder has a sulfur content of 10.000% by mass or more and 100.000% by mass or less. When the sulfur-containing powder has a sulfur content of 10.000% by mass or more, the proportion of sulfur in contact with the surface of the iron-based powder increases, improving the reactivity between iron and oxygen. Furthermore, the generation of hydrogen gas can be suppressed. Therefore, the sulfur content of the sulfur-containing powder is set to 10.000% by mass or more, preferably 43.000% by mass or more, and more preferably 80.000% by mass or more. On the other hand, the upper limit of the sulfur content of the sulfur-containing powder is not particularly limited and can be 100.000% by mass. However, from the viewpoint of adding additives, it may be, for example, 99.900% by mass or less.

[0033] In the iron-based mixed powder according to this embodiment, the content of the sulfur-containing powder is 0.020 mass % or more and 5.000 mass % or less with respect to the total content of the iron-based powder and the sulfur-containing powder. In the following description, the content of the sulfur-containing powder with respect to the total content of the iron-based powder and the sulfur-containing powder may be simply referred to as the content of the sulfur-containing powder.

[0034] If the content of the sulfur-containing powder is 0.050% by mass or more, the reactivity with oxygen is improved and the effect of suppressing hydrogen gas generation is obtained. Therefore, the content of the sulfur-containing powder is 0.050% by mass or more, preferably 0.200% by mass or more, more preferably 0.600% by mass or more, and even more preferably 1.100% by mass or more.

[0035] When the content of the sulfur-containing powder is 5.000% by mass or less, the water on the surface of the iron-based powder is prevented from becoming too acidic, thereby suppressing the generation of hydrogen gas. Furthermore, although a portion of the hydrogen gas is converted to hydrogen sulfide gas by reaction with sulfur, the excessive generation of hydrogen sulfide gas due to this reaction is suppressed, thereby suppressing the generation of the rotten egg odor caused by hydrogen sulfide gas. Therefore, the content of the sulfur-containing powder is 5.000% by mass or less, preferably 3.000% by mass or less.

[0036] In the iron-based mixed powder according to this embodiment, the iron-based powder and the sulfur-containing powder are preferably mixed uniformly. In the production of the iron-based mixed powder, the iron-based powder and the sulfur-containing powder may be mixed using a powder mixing device such as a V-type mixer, a double cone mixer, or a conical blender.

[0037] The volumetric median diameter of the iron-based mixed powder (the median value of the particle diameter calculated from the volumetric particle size distribution, so-called D 50 ) is not particularly limited as long as it does not cause any problems in handling. However, from the viewpoint of further improving the reactivity with oxygen, the volumetric median diameter of the iron-based mixed powder is preferably 1000 μm or less, more preferably 400 μm or less, even more preferably 200 μm or less, and particularly preferably 100 μm or less. In consideration of ease of handling and reactivity with oxygen, the volumetric median diameter of the iron-based mixed powder is preferably 5 μm or more, and more preferably 70 μm or more.

[0038] The volume-based median diameter of the iron-based mixed powder is a value measured by a laser diffraction particle size distribution analyzer.

[0039] Specifically, the volumetric median diameter of the iron-based mixed powder is measured as follows. First, the powder to be measured is placed in ethanol and dispersed by ultrasonic vibration for 30 seconds or more. Then, the volumetric particle size distribution is measured using a laser diffraction particle size distribution analyzer (LA-950V2, manufactured by Horiba, Ltd.) that uses a laser diffraction / scattering method. The median diameter is determined by calculating the cumulative particle size distribution from the volumetric particle size distribution obtained by this measurement.

[0040] The oxygen reactant according to this embodiment includes the iron-based mixed powder according to this embodiment. The oxygen reactant according to this embodiment may use the iron-based mixed powder, and does not exclude the inclusion of other components in addition to the iron-based mixed powder.

[0041] Examples of other components include activated charcoal and saline solution.

[0042] As an example, the reaction mechanism when salt water is added to the iron-based mixed powder will be described below. When the iron-based powder is mixed with a sulfur compound and salt water is added, the sulfur compound dissolves, producing fine sulfur powder at the boundary between the iron particles contained in the iron-based powder and the sulfur compound particles. Then, in the presence of chloride ions derived from the salt water, the iron dissolves at the boundary.

[0043] In the pores on the surface of the iron particles created by the dissolution, hydrolysis by iron ions occurs, causing a decrease in the pH and potential of the aqueous solution, which further accelerates the dissolution of iron in the pores, causing pitting corrosion.

[0044] Furthermore, the sulfur in the fine sulfur powder formed on the surface of the iron particles reacts with the hydrogen generated during the hydrolysis to convert it into hydrogen sulfide, which is thought to suppress the generation of hydrogen gas throughout the system.

[0045] Furthermore, hydrogen sulfide dissolves more easily in water than hydrogen. Therefore, the hydrogen sulfide converted from the hydrogen generated during the hydrolysis dissolves in water. This is thought to be why the generation of hydrogen sulfide gas is suppressed.

[0046] The same effect as in the case of the sulfur compound is believed to occur when elemental sulfur is mixed with an iron-based powder.

[0047] The oxygen reactant according to this embodiment may be enclosed in a bag. Examples of the bag include a breathable packaging bag made by overlapping a nonwoven fabric and perforated polyethylene, or a breathable packaging bag made by overlapping paper and perforated polyethylene.

[0048] The iron-based mixed powder according to this embodiment will be described below based on examples.

[0049] The iron-based mixed powder according to the example was produced by the following procedure.

[0050] Iron ore powder was reduced with coke at 800 to 1000°C to adjust the O / Fe ratio, and iron powder was obtained. The O / Fe ratio was calculated by measuring the content of elemental Fe, compounds of Fe and O, and other compounds using an X-ray diffractometer (SmartLab, manufactured by Rigaku Corporation).

[0051] For Comparative Examples 2 to 15 and Examples 1 to 6, a sulfur-containing powder was used in which sulfur powder (manufactured by Kojundo Chemical Laboratory Co., Ltd., SSE02PB) was mixed with silica powder (manufactured by Kojundo Chemical Laboratory Co., Ltd., SIO09PB) to adjust the sulfur content. For Comparative Examples 16 to 21 and Examples 7 to 8, manganese sulfide powder (manufactured by Kojundo Chemical Laboratory Co., Ltd., MNI09PB) was used as the sulfur-containing powder. For Comparative Examples 22 to 27 and Examples 9 to 10, calcium sulfide powder (manufactured by Kojundo Chemical Laboratory Co., Ltd., CA105PB) was used as the sulfur-containing powder.

[0052] The iron powder and the sulfur-containing powder were mixed to obtain iron-based mixed powders according to Examples and Comparative Examples. In Comparative Example 1, no sulfur-containing powder was mixed. Table 1 shows the O / Fe ratio of the iron powder, the type of sulfur-containing powder, the sulfur content (mass%) of the sulfur-containing powder, the sulfur content (mass%) of the sulfur-containing powder, and the median diameter (D) of the iron-based mixed powder measured by the method described above. 50 ) In Table 1, the underlined values ​​indicate that the values ​​are outside the range of this embodiment.

[0053]

[0054] The reactivity with oxygen, the amount of hydrogen gas generated, and the amount of hydrogen sulfide gas generated of the iron-based mixed powders according to the examples and comparative examples were evaluated as follows.

[0055] The reactivity with oxygen was evaluated as follows. First, 0.006 g of sodium chloride powder (NAH07PB, manufactured by Kojundo Chemical Laboratory Co., Ltd.) was mixed with 1.50 g of iron-based mixed powder. A mixture of 0.95 g of Isolite CG (No. 1, manufactured by Isolite Kogyo Co., Ltd.), a calcined product of diatomaceous earth, and 0.85 g of water was added to the resulting powder, and the mixture was filled into a breathable packaging bag (45 mm long x 40 mm wide) to prepare a sample for evaluation according to the examples or comparative examples. The breathable packaging bag was made of a laminated material composed of a nonwoven fabric and perforated polyethylene.

[0056] Each sample was then sealed together with 3000 mL of air in a gas-barrier bag made of a five-layer laminated material consisting of nylon / polyethylene / aluminum foil / polyethylene / polyethylene. Each sealed bag containing the sample was left standing at 25°C for 72 hours. The oxygen concentration of the gas in the bag was then measured using a gas chromatograph (GC3210D, manufactured by GL Sciences Inc.). The oxygen concentration in the bag was then subtracted from the oxygen concentration in the air to determine the amount of oxygen lost in the bag. Based on this amount of oxygen lost, the oxygen reaction amount (ml / g) per gram of iron-based mixed powder was calculated.

[0057] That is, the oxygen reaction amount in this example refers to the volume (ml) of oxygen that 1 g of the iron-based mixed powder can remove from 3000 mL of air at 25° C. and atmospheric pressure in 72 hours. The larger the oxygen reaction amount, the higher the reactivity with oxygen. In other words, when the iron-based mixed powder is used as an oxygen reactant, it is superior in terms of total heat generation amount, heat generation temperature, and heat generation time (excellent heat generation characteristics).

[0058] The amounts of hydrogen gas and hydrogen sulfide gas generated were evaluated as follows. First, 0.06 g of sodium chloride powder (NAH07PB, manufactured by Kojundo Chemical Laboratory Co., Ltd.) was mixed with 15.00 g of iron-based mixed powder. A mixture of 7.89 g of Isolite CG (No. 1, manufactured by Isolite Kogyo Co., Ltd.), a calcined product of diatomaceous earth, and 7.11 g of water was added to the resulting powder, and the mixture was filled into a breathable packaging bag (80 mm long x 80 mm wide) to prepare a sample for evaluation in the examples or comparative examples. The breathable packaging bag was made of a laminated material composed of a nonwoven fabric and perforated polyethylene.

[0059] Each sample was sealed with 25 mL of air in a gas-barrier bag made of a five-layer laminated material: nylon / polyethylene / aluminum foil / polyethylene / polyethylene. Each sealed sample bag was left standing at 55°C for 72 hours. The hydrogen gas concentration (volume %) in the bag was measured using a gas chromatograph (GC3210D, manufactured by GL Sciences Inc.). Furthermore, the hydrogen sulfide concentration (ppm) in the bag was measured using a gas monitor (GX-3R Pro, manufactured by Riken Keiki Co., Ltd.).

[0060] If the measured hydrogen gas concentration is low, the generation of hydrogen gas is suppressed.

[0061] Furthermore, it was determined that the generation of hydrogen sulfide was prevented if the concentration was less than 0.3 ppm, which is known as the concentration at which humans do not detect a rotten egg smell.

[0062] Table 1 also shows the evaluation results for the oxygen reaction amount, hydrogen gas concentration, and hydrogen sulfide concentration.

[0063] The iron-based mixed powders of the examples were more reactive with oxygen, and generated less hydrogen gas and hydrogen sulfide than the powders of the comparative examples.

[0064] The iron-based mixed powders of Examples 3 to 10, which had a median diameter of 400 μm or less, exhibited higher reactivity with oxygen and further reduced the amount of hydrogen gas generated. In addition, the generation of hydrogen sulfide was also prevented.

[0065] In Examples 5 to 10, the median diameter was set to 200 μm or less, which resulted in higher reactivity with oxygen and less generation of hydrogen gas than in Examples 1 to 4. Furthermore, generation of hydrogen sulfide was also prevented.

[0066] It was confirmed that the above-mentioned effects were obtained when any of a mixed powder of sulfur powder and silica powder, manganese sulfide powder, and calcium sulfide powder was used as the sulfur-containing powder.

[0067] As described above, the iron-based mixed powder according to this example has high reactivity with oxygen, and hydrogen gas generation is suppressed. Furthermore, the iron-based mixed powder according to this example generates a small amount of hydrogen sulfide, and the rotten egg smell is prevented.

[0068] It should be noted that the embodiments disclosed in this specification are merely examples, and the embodiments of the present disclosure are not limited to these, and can be modified as appropriate within the scope of the purpose of the present disclosure.

[0069] The present disclosure is applicable to iron-based mixed powders and oxygen reactants.

Claims

1. A mixed powder comprising an iron-based powder having an oxygen to iron atomic ratio (O / Fe) of 0.800 or less, and a sulfur-containing powder having a sulfur content of 10.000% by mass or more and 100.000% by mass or less, wherein the content of the sulfur-containing powder is 0.020% by mass or more and 5.000% by mass or less with respect to the sum of the content of the iron-based powder and the content of the sulfur-containing powder.

2. The iron-based mixed powder according to claim 1, wherein the sulfur-containing powder comprises manganese sulfide powder.

3. The iron-based mixed powder according to claim 1 or 2, wherein the median diameter on a volume basis is 70 μm or more and 100 μm or less.

4. An oxygen reactant comprising an iron-based mixed powder comprising an iron-based powder having an oxygen to iron atomic ratio O / Fe of 0.800 or less, and a sulfur-containing powder having a sulfur content of 10.000 mass% or more and 100.000 mass% or less, wherein the content of the sulfur-containing powder is 0.020 mass% or more and 5.000 mass% or less with respect to the total content of the iron-based powder and the content of the sulfur-containing powder.

5. The oxygen reactant according to claim 4, wherein the sulfur-containing powder comprises manganese sulfide powder.

6. The oxygen reactant according to claim 4 or 5, wherein the iron-based mixed powder has a volumetric median diameter of 70 μm or more and 100 μm or less.

Citation Information

Patent Citations

  • Kairo (body warmer)

    JP1984074457A

  • Heat-generating composition

    JP1986271378A

  • Raw material iron powder for mildly pyrogenic composition and production thereof

    JP1996041447A

  • Gas treatment method

    WO2017047730A1