Proton conductor, membrane electrode assembly, electrochemical cell and fuel cell stack

The proton conductor BaZr1-x-yYbxCuO3-δ, with specific compositional ranges, addresses the low proton conductivity and fuel utilization rate issues in PCFCs, achieving enhanced power generation efficiency and output by optimizing Cu substitution, thereby maintaining high electromotive force and reducing fuel exhaustion risks.

WO2024236878A1PCT designated stage expired Publication Date: 2024-11-21PANASONIC HOLDINGS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006947
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-02-27
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Proton conducting ceramic fuel cells (PCFCs) face limitations in achieving high power generation efficiency and output due to low proton conductivity and fuel utilization rates, which can lead to reduced electromotive force and increased risk of fuel exhaustion, especially at high fuel utilization rates.

Method used

A proton conductor with the chemical formula BaZr1-x-yYbxCuO3-δ is developed, where 0.95≤a≤1.05, 0.1≤x≤0.4, 0.01

Benefits of technology

The improved proton conductivity of the BaZr1-x-yYbxCuO3-δ material allows for higher power generation efficiency and output in PCFCs, maintaining high electromotive force even at high fuel utilization rates, reducing the risk of fuel exhaustion and increasing current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006947_21112024_PF_FP_ABST
    Figure JP2024006947_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A proton conductor according to the present disclosure contains a compound represented by the chemical formula BaaZr1-x-yYbxCuyO3-δ. In the chemical formula, 0.95 ≤ a ≤ 1.05, 0.1 ≤ x ≤ 0.4, 0.01 < y < 0.20, and 0 < δ ≤ 0.65. An electrolyte membrane 10 according to the present disclosure includes the proton conductor according to the present disclosure.
Need to check novelty before this filing date? Find Prior Art

Description

Proton conductors, membrane electrode assemblies, electrochemical cells and fuel cell stacks

[0001] The present disclosure relates to proton conductors, membrane electrode assemblies, electrochemical cells and fuel cell stacks.

[0002] A solid oxide fuel cell (SOFC) is a fuel cell that uses a solid oxide as the electrolyte that constitutes the electrolyte membrane. Oxide ion conductors, such as stabilized zirconia, are widely used as the solid oxide electrolyte, and SOFCs have the advantage of having higher power generation efficiency than polymer electrolyte fuel cells (PEFCs).

[0003] Proton-conducting ceramic fuel cells (hereinafter referred to as "PCFCs"), a type of SOFC, are characterized by the use of a proton-conducting solid oxide as the electrolyte that constitutes the electrolyte membrane. In typical SOFCs, water vapor is generated at the anode side due to the power generation reaction. Therefore, in an operating environment with a high fuel utilization rate, the hydrogen fuel is diluted by the water vapor, reducing the fuel cell's electromotive force and increasing the risk of cell deterioration due to fuel starvation. Therefore, typical SOFCs cannot achieve a sufficiently high fuel utilization rate.

[0004] On the other hand, in PCFCs that use a proton conductor as the electrolyte, the generation of water vapor due to the power generation reaction occurs on the air electrode side, suppressing the dilution of hydrogen at the fuel electrode. This allows the fuel cell to maintain a high electromotive force even when operated at a high fuel utilization rate, reducing the risk of fuel starvation, making it advantageous for operation at high fuel utilization rates. Since the power generation efficiency of a fuel cell is expressed as the product of the cell voltage and the fuel utilization rate, PCFCs, which can achieve both a high fuel utilization rate and a high electromotive force, are expected to have particularly high power generation efficiency among SOFCs. Furthermore, the ability to maintain a high electromotive force also means that the fuel cell can be operated at a higher current density, which is advantageous in terms of increasing output.

[0005] In order to improve the power generation efficiency and power output of PCFCs, it is important to reduce the internal resistance of the cell during power generation, and for this purpose, it is important to improve the proton conductivity of the proton conductor used as the electrolyte.

[0006] Common proton conductors are BaZrO3, BaCeO3, and Ba(Ce,Zr)O3, which have a perovskite structure, with the Zr or Ce site partially substituted with a metal element having a valence of +3, such as yttrium (Y) or ytterbium (Yb). These materials are known to have relatively high proton conductivity. In particular, BaZrO3-based proton conductors have attracted attention because they have relatively high chemical stability against CO2 contained in the fuel gas or air of fuel cells. In the case of BaZrO3-based proton conductors, when Y is used as a substitution element, NiO, which is used in the anode, and BaY2NiO, a by-product, are formed at high temperatures. 5-δ (δ is the amount of oxygen vacancies) is easily generated. Here, δ represents the amount of oxygen vacancies. BaYNiO 5-δ The generation of ions leads to a decrease in the performance and reliability of the fuel cell. In contrast, when Yb is used as the substitution element, it has the advantage of being less likely to produce by-products. Therefore, materials using Yb as the substitution element in BaZrO3-based proton conductors are considered to be promising materials for practical use. If the proton conductivity can be further improved using Yb-substituted BaZrO3 as a base, it will be advantageous for realizing fuel cells with high power generation efficiency or high power density.

[0007] Non-Patent Document 1 investigates the addition of CuO to Yb-substituted BaZrO. According to Non-Patent Document 1, the addition of 1.0 mol% of CuO to Yb-substituted BaZrO has the effect of promoting the sintering of Yb-substituted BaZrO.

[0008] J. Park et al., “Low temperature sintering of BaZrO3-based proton conductors for intermediate temperature solid oxide fuel cells”, Solid State Ionics 181 163-167 (2010)

[0009] According to Non-Patent Document 1, the addition of 1.0 mol% CuO improves the sinterability of Yb-substituted BaZrO3, but the Yb-substituted BaZrYbO3 obtained by this addition with 1.0 mol% Cu substitution has a lower proton conductivity than that of a material that does not contain Cu.

[0010] An object of the present disclosure is to provide a proton conductor that is applicable to PCFCs and has improved proton conductivity.

[0011] The proton conductor of the present disclosure has the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ wherein 0.95≦a≦1.05, 0.1≦x≦0.4, 0.01<y<0.20, and 0<δ≦0.65 are satisfied.

[0012] The present disclosure provides a proton conductor that is applicable to PCFCs and has improved proton conductivity.

[0013] FIG. 1 shows a cross-sectional view of an electrolyte membrane according to Embodiment 2. FIG. 2 shows a cross-sectional view of a membrane electrode assembly according to Embodiment 3. FIG. 3 shows a cross-sectional view of an electrochemical cell according to Embodiment 4. FIG. 4 shows a fuel cell system including a fuel cell stack according to Embodiment 5. FIG. 5 is a flow chart showing a method for producing proton conductor pellets according to Examples and Comparative Examples. FIG. 6 shows a procedure for producing an electrochemical cell of Example 6 using the proton conductor of Example 2. FIG. 7 is a graph showing the current-voltage characteristics and current output characteristics of the electrochemical cell of Example 6.

[0014] [Background to the Invention of an Aspect of the Present Disclosure] In Non-Patent Document 1, the sinterability of Yb-substituted BaZrO3 is improved by adding 1.0 mol% CuO. However, the Yb-substituted BaZrO3 thus obtained, which is substituted with 1.0 mol% Cu, has a lower proton conductivity than that of a material that does not contain Cu.

[0015] As a result of extensive research into the Cu substitution amount, the inventors discovered that a Cu substitution amount as small as 1.0 mol% reduces proton conductivity, whereas a larger Cu substitution amount can improve proton conductivity, i.e., there is an optimal range for the Cu substitution amount, which led to the present disclosure described below.

[0016] [Embodiments of the Present Disclosure] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.

[0017] (Embodiment 1) The proton conductor according to embodiment 1 is represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ In the above chemical formula, the following conditions are satisfied: 0.95≦a≦1.05, 0.1≦x≦0.4, 0.01<y<0.20, and 0<δ≦0.65.

[0018] As demonstrated in Examples 1 to 5 below, the proton conductor according to the first embodiment has improved proton conductivity. Specifically, the proton conductor according to the first embodiment has the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ In this case, the proton conductor has a higher proton conductivity than a compound not containing Cu, i.e., a compound in which y = 0. Therefore, when the proton conductor according to embodiment 1 is applied to a PCFC, it can realize high power generation efficiency and high output of the PCFC.

[0019] Chemical formula: Ba a Zr 1-x-y Yb x Cu y O 3-δ In this case, 0.04≦y≦0.16 may be satisfied. By containing such a compound, the proton conductor according to embodiment 1 has further improved proton conductivity. As a result, when the proton conductor according to embodiment 1 is applied to a PCFC, it is possible to realize even higher power generation efficiency and higher output of the PCFC.

[0020] Chemical formula: Ba a Zr 1-x-y Yb x Cu y O 3-δ In this case, 0.125≦y≦0.16 may be satisfied. By containing such a compound, the proton conductor according to embodiment 1 has further improved proton conductivity. As a result, when the proton conductor according to embodiment 1 is applied to a PCFC, it is possible to realize even higher power generation efficiency and higher output of the PCFC.

[0021] Chemical formula: Ba a Zr 1-x-y Yb x Cu y O 3-δ In this case, 0.125≦y≦0.15 may be satisfied. By containing such a compound, the proton conductor according to embodiment 1 has further improved proton conductivity. As a result, when the proton conductor according to embodiment 1 is applied to a PCFC, it is possible to realize even higher power generation efficiency and higher output of the PCFC.

[0022] Chemical formula: Ba a Zr 1-x-y Yb x Cu y O 3-δ In this case, y=0.15 may be satisfied. By containing such a compound, the proton conductor according to embodiment 1 has particularly improved proton conductivity. As a result, when the proton conductor according to embodiment 1 is applied to a PCFC, it is possible to realize even higher power generation efficiency and higher output of the PCFC.

[0023] The proton conductor according to embodiment 1 can be synthesized by a citrate complex method, a solid-state sintering method, a co-precipitation method, a nitrate method, or a spray granulation method.

[0024] The proton conductor according to embodiment 1 has the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to the first embodiment may contain a compound represented by the chemical formula Ba a Zr1-x-y Yb x Cu y O 3-δ The proton conductor according to embodiment 1 may contain a compound represented by the chemical formula Ba in a molar ratio of 5% or more, or 20% or more. a Zr 1-x-y Yb x Cu y O 3-δ By including the compound represented by the formula (I), the proton conductor according to the first embodiment can exhibit high proton conductivity.

[0025] The proton conductor according to embodiment 1 has the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to embodiment 1 may be composed of a compound represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ "Comprised of a compound represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to embodiment 1 contains a compound represented by the chemical formula Ba in an amount of 80% or more by mole. a Zr 1-x-y Yb x Cu y O 3-δ When the proton conductor according to the first embodiment is composed of a compound represented by the formula (I), the proton conductor according to the first embodiment can exhibit higher proton conductivity.

[0026] As an example, the proton conductor according to embodiment 1 is substantially of the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to embodiment 1 may be substantially composed of a compound represented by the chemical formula Ba a Zr 1-x-y Ybx Cu y O 3-δ "Comprised of a compound represented by the chemical formula Ba" means that the proton conductor according to embodiment 1 is made of a compound represented by the chemical formula Ba, excluding components contained as inevitable impurities. a Zr 1-x-y Yb x Cu y O 3-δ In this case, in the proton conductor according to embodiment 1, the proton conductor is composed only of a compound represented by the chemical formula BaZr (1-x-y) Yb x Sc y O 3-δ The compound represented by the formula (I) may account for 95% or more in terms of molar ratio.

[0027] The proton conductor according to embodiment 1 has the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to embodiment 1 may further contain other components in addition to the compound represented by the formula (I). The proton conductor according to embodiment 1 may further contain, as other components, impurities generated in the process of synthesizing the above-described compound, for example.

[0028] The proton conductor according to embodiment 1 contains a compound of the formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The average crystal grain size of the compound represented by the formula (I) is, for example, 0.1 μm or more and 10 μm or less. Even if the average crystal grain size is within the above range, or even if it is smaller than 0.1 μm, the proton conductor according to the first embodiment can achieve high proton conductivity. Here, the average crystal grain size can be determined, for example, by using the median diameter (volume basis) obtained from particle size distribution measurement.

[0029] 1 shows a cross-sectional view of an electrolyte membrane 10 according to embodiment 2. The proton conductor contained in the electrolyte membrane 10 is the proton conductor described in embodiment 1.

[0030] The proton conductor contained in the electrolyte membrane 10 according to the second embodiment has improved proton conductivity, as described in the first embodiment. Therefore, the electrolyte membrane 10 according to the second embodiment can have high proton conductivity. As a result, when the electrolyte membrane 10 according to the second embodiment is applied to an electrolyte membrane of a PCFC, it can realize high power generation efficiency and high output of the PCFC.

[0031] The electrolyte membrane 10 contains the proton conductor described in the first embodiment as an electrolyte material. a Zr 1-x-y Yb x Cu y O 3-δ The proton conductive material may further contain other compounds that exhibit proton conductivity other than the compound represented by the chemical formula BaZr 1-x1 M1 x1 O 3-δ A compound represented by the chemical formula BaCe 1-x2 M2 x2 O 3-δ or a compound represented by the chemical formula BaZr 1-x3-y3 Ce x3 M3 y3 O 3-δ where M1, M2, and M3 each contain at least one element selected from the group consisting of Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Y, Sc, In, and Lu, and satisfy the relationships 0<x1<1, 0<x2<1, 0<x3<1, 0<y3<1, and 0<δ<0.5. The electrolyte membrane 10 may further contain an electrolyte material other than a proton conductor.

[0032] The thickness of the electrolyte membrane 10 according to the second embodiment is not particularly limited and can be determined appropriately depending on the application. For example, the thickness of the electrolyte membrane 10 is, for example, 1 to 500 μm, and may be 1 to 50 μm.

[0033] The electrolyte membrane 10 is produced by, for example, tape casting, spin coating, dip coating, sputtering, or PLD (Pulse Laser Deposition).

[0034] 2 shows a cross-sectional view of a membrane electrode assembly 20 according to embodiment 3. The membrane electrode assembly 20 includes an electrolyte membrane 21 and electrodes 22 provided on the electrolyte membrane 21. The electrolyte membrane 21 in the membrane electrode assembly 20 is the electrolyte membrane 10 described in embodiment 2.

[0035] The electrolyte membrane 21 in the membrane electrode assembly 20 according to the third embodiment includes a proton conductor having improved proton conductivity, as described in the second embodiment. Therefore, the electrolyte membrane 21 can have high proton conductivity. As a result, when the membrane electrode assembly 20 according to the third embodiment is applied to the electrodes and electrolyte membrane of a PCFC, it can realize high power generation efficiency and high output of the PCFC.

[0036] As described above, the electrolyte membrane 21 is the electrolyte membrane 10 described in the second embodiment, and therefore a detailed description of the electrolyte membrane 21 will be omitted here.

[0037] The material constituting the electrodes 22 can be selected appropriately depending on the application to which the membrane electrode assembly 20 is to be applied.

[0038] The membrane electrode assembly 20 may be used, for example, as an electrode and electrolyte membrane of a fuel cell, or as an electrode and electrolyte membrane of a PCFC. Thus, for example, the electrode 22 may function as a fuel electrode or as a cathode.

[0039] When the electrode 22 in the membrane electrode assembly 20 is applied to, for example, the anode of a fuel cell, particularly to the anode of a PCFC, the electrode 22 may mainly contain, for example, at least one of the following compounds: (i) a mixture (i.e., cermet) of the electrolyte material contained in the electrolyte membrane 21, and Ni and one or more metals selected from the group consisting of Co, Fe, Pt, and Pd; (ii) a composite oxide containing lanthanum; (iii) a composite oxide containing barium; and (iv) a composite oxide containing strontium.

[0040] When the electrode 22 mainly contains a certain compound, it means that the mass ratio of that compound in the electrode 22 is the largest.

[0041] When the electrode 22 in the membrane electrode assembly 20 is applied to, for example, an air electrode of a fuel cell, particularly an air electrode of a PCFC, the electrode 22 includes, for example, a composite compound. In this case, the electrode 22 may mainly include, for example, lanthanum strontium cobalt oxide, lanthanum strontium cobalt iron oxide, lanthanum barium cobalt oxide, or barium strontium cobalt iron oxide. In this case, the electrode 22 may be formed on the electrolyte membrane 21 by, for example, a screen printing method.

[0042] The electrode 22 has a thickness of, for example, 1 μm to 1000 μm. When the electrode 22 also serves as a support for the cell, the electrode 22 preferably has a thickness of 100 μm to 700 μm. When a component other than the electrode 22 serves as a support for the cell, the electrode 22 preferably has a thickness of 10 μm to 50 μm.

[0043] 2, the electrolyte membrane 21 and the electrode 22 are in contact with each other, but another layer may be provided between the electrolyte membrane 21 and the electrode 22. An example of the another layer is a functional layer. The functional layer is a layer that promotes the movement of electrons or protons between the electrolyte membrane 21 and the electrode 22. The functional layer is made of, for example, a composite of a cermet and a complex oxide.

[0044] Fourth Embodiment FIG. 3 shows a cross-sectional view of an electrochemical cell 30 according to a fourth embodiment.

[0045] The electrochemical cell 30 according to the fourth embodiment includes a first electrode 31, a second electrode 32, and an electrolyte membrane 33. The electrolyte membrane 33 is provided between the first electrode 31 and the second electrode 32. In other words, as shown in Fig. 3 , the electrochemical cell 30 includes the first electrode 31, the electrolyte membrane 33, and the second electrode 32 in this order. The electrolyte membrane 33 in the electrochemical cell 30 is the electrolyte membrane 10 described in the second embodiment.

[0046] The electrolyte membrane 33 in the electrochemical cell 30 according to the fourth embodiment contains a proton conductor having improved proton conductivity, as described in the second embodiment. Therefore, the electrolyte membrane 33 can have high proton conductivity. As a result, when the electrochemical cell 30 according to the fourth embodiment is used as, for example, a PCFC, the PCFC can achieve high power generation efficiency and high output.

[0047] As described above, the electrolyte membrane 33 in the electrochemical cell 30 is the electrolyte membrane 10 described in embodiment 2. Therefore, detailed description of the electrolyte membrane 33 will be omitted here.

[0048] The electrochemical cell 30 according to the fourth embodiment may be used, for example, as a fuel cell or a PCFC. Therefore, for example, the first electrode 31 may function as a fuel electrode, and the second electrode 32 may function as a cathode.

[0049] When the first electrode 31 functions as a fuel electrode of a fuel cell such as a PCFC, the material used for the first electrode 31 is the same as that described in embodiment 3 as the material used when the electrode 22 is used as a fuel electrode.

[0050] When the second electrode 32 functions as an air electrode of a fuel cell such as a PCFC, the material used for the second electrode 32 is the same as that described in embodiment 3 as the material used when the electrode 22 is used as an air electrode.

[0051] 3 , the first electrode 31 and the second electrode 32 are each provided in contact with the electrolyte membrane 33. However, another layer may be provided between the first electrode 31 and the electrolyte membrane 33. Also, another layer may be provided between the second electrode 32 and the electrolyte membrane 33. An example of the another layer is a functional layer. The functional layer is the same as the functional layer described in the third embodiment.

[0052] The electrochemical cell 30 can be used in fuel cells, electrochemical hydrogen pumps, hydrogen sensors and water electrolyzers.

[0053] Fifth Embodiment FIG. 4 shows a fuel cell system 1000 including a fuel cell stack 40 according to a fifth embodiment.

[0054] The fuel cell stack 40 includes a plurality of electrochemical cells 30. The plurality of electrochemical cells 30 are stacked on one another to form the fuel cell stack 40. The electrochemical cells 30 are described in the fourth embodiment.

[0055] In the fuel cell system 1000 according to the fifth embodiment, the electrochemical cell 30 is used as a fuel cell, so that in this case, the first electrode 31 functions as a fuel electrode, and the second electrode 32 functions as a cathode.

[0056] The fuel cell system 1000 further includes a raw material gas supply path 1023 and an oxidizing gas supply path 1024. The raw material gas supply path 1023 is connected to the first electrode 31 and the raw material supplier 1022. The oxidizing gas supply path 1024 is connected to the second electrode 32 and the oxidizing gas supplier 1021.

[0057] As explained in the third embodiment, the electrochemical cell 30 can realize high power generation efficiency and high output of the PCFC, and therefore the fuel cell stack 40 can realize high power generation efficiency and high output as a fuel cell stack.

[0058] The fuel cell stack 40 is housed in, for example, a housing 1014 .

[0059] The housing 1014 may be made of a heat insulating material.

[0060] An oxidant gas is supplied to the second electrodes 32 of the stacked electrochemical cells 30. Specifically, the oxidant gas is supplied from an oxidant gas supplier 1021 through an oxidant gas supply path 1024 to the second electrodes 32 (i.e., cathodes) of the plurality of electrochemical cells 30.

[0061] At the second electrode 32, the following reaction (1) occurs: O + 4H + +4e - → 2H2O (1)

[0062] The oxidant gas is, for example, air.

[0063] The raw material is supplied from a raw material supply device 1022 through a raw material gas supply path 1023 to the first electrodes 31 of the plurality of electrochemical cells 30 .

[0064] At the first electrode 31, the following reaction (2) occurs: 2H → 4H + +4e - (2)

[0065] The raw material is, for example, hydrogen molecules.

[0066] The hydrogen may be produced by a reforming reaction. Alternatively, the hydrogen may be produced by water electrolysis.

[0067] In this way, the fuel cell system 1000 operates and generates electricity.

[0068] [Other Embodiments] (Additional Notes) The above description of the embodiments discloses the following techniques.

[0069] (Technology 1) Chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ wherein 0.95≦a≦1.05, 0.1≦x≦0.4, 0.01<y<0.20, and 0<δ≦0.65 are satisfied.

[0070] This configuration allows the proton conductor according to Technology 1 to have improved proton conductivity. Therefore, when the proton conductor according to Technology 1 is applied to a PCFC, it can realize high power generation efficiency and high output of the PCFC.

[0071] (Technology 2) The proton conductor according to Technology 1, wherein in the chemical formula, 0.04≦y≦0.16 is satisfied.

[0072] With this configuration, when the proton conductor according to Technique 2 is applied to a PCFC, it is possible to realize even higher power generation efficiency and higher output of the PCFC.

[0073] (Technology 3) The proton conductor according to Technology 2, wherein in the chemical formula, 0.125≦y≦0.16 is satisfied.

[0074] With this configuration, when the proton conductor according to Technique 3 is applied to a PCFC, it is possible to realize even higher power generation efficiency and higher output of the PCFC.

[0075] (Technology 4) The proton conductor according to Technology 3, wherein in the chemical formula, 0.125≦y≦0.15 is satisfied.

[0076] With this configuration, when the proton conductor according to Technique 4 is applied to a PCFC, it can realize even higher power generation efficiency and higher output of the PCFC.

[0077] (Technology 5) The proton conductor according to Technology 4, wherein in the chemical formula, y=0.15 is satisfied.

[0078] With this configuration, when the proton conductor according to Technique 5 is applied to a PCFC, it can realize even higher power generation efficiency and higher output of the PCFC.

[0079] (Technology 6) An electrolyte membrane comprising the proton conductor according to any one of Technologies 1 to 5.

[0080] With this configuration, when the electrolyte membrane according to Technique 6 is applied to the electrolyte membrane of a PCFC, it is possible to realize high power generation efficiency and high output of the PCFC.

[0081] (Technology 7) A membrane electrode assembly comprising: the electrolyte membrane according to Technology 6; and an electrode provided on the electrolyte membrane.

[0082] With this configuration, when the membrane electrode assembly according to Technique 7 is applied to the electrodes and electrolyte membrane of a PCFC, it is possible to realize high power generation efficiency and high output of the PCFC.

[0083] (Technology 8) An electrochemical cell comprising: a first electrode; a second electrode; and the electrolyte membrane according to Technology 6 provided between the first electrode and the second electrode.

[0084] With this configuration, when the electrochemical cell according to Technique 8 is used as, for example, a PCFC, it can realize high power generation efficiency and high output of the PCFC.

[0085] (Technology 9) A fuel cell stack comprising a plurality of the electrochemical cells according to Technology 8.

[0086] With this configuration, the fuel cell stack according to Technique 9 can achieve high power generation efficiency and high output.

[0087] The present disclosure will now be described in more detail with reference to the following examples and comparative examples.

[0088] <Proton Conductors> As described below, proton conductors were prepared in Examples 1 to 5 and Comparative Examples 1 to 5. The proton conductivity of each proton conductor was evaluated.

[0089] [Example 1] (Production of proton conductor pellets for evaluation) Fig. 5 is a flowchart showing a method for producing proton conductor pellets according to an example and a comparative example. The production of proton conductor pellets for evaluation will be described with reference to Fig. 5.

[0090] The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.076 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.004 mol

[0091] The starting materials were added to and dissolved in 1000 mL of distilled water to obtain a mixed solution, which was then stirred (S11).

[0092] Next, 0.3 mol of citric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.3 mol of ethylenediaminetetraacetic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to the mixed solution (S12). Hereinafter, "ethylenediaminetetraacetic acid" will be referred to as "EDTA."

[0093] Next, ammonia water (28% by mass, manufactured by Kishida Chemical Co., Ltd.) was added to the mixture, and the pH of the mixture was adjusted to 10 using a pH meter (manufactured by Horiba Ltd.) (S13).

[0094] Next, the mixture was stirred at a temperature of 90° C. (S14).

[0095] The temperature of the mixture was raised to 370°C using a hot stirrer to evaporate the water solvent and degrease the mixture (S15), thereby obtaining a black solid.

[0096] The obtained solid was transferred into a crucible and pre-fired in air at 900° C. for 10 hours (S16).

[0097] The calcined powder was pulverized (S17). The pulverized powder was then transferred to a plastic container together with zirconia balls.

[0098] Then, 100 g of ethanol (manufactured by Kanto Chemical Co., Ltd.) was added to the plastic container. The mixture thus obtained was pulverized in a ball mill for 72 hours (S18).

[0099] After the grinding using the ball mill, the mixture was dried using a lamp to remove the ethanol from the mixture (S19), thus obtaining a powder.

[0100] Next, the obtained powder was pressed into a cylindrical shape using a hydraulic pump (manufactured by Enerpac Co., Ltd.) and a powder molding die with a diameter of 20 mm, and further molded into a pellet using a cold isostatic press (manufactured by Sansho Industry Co., Ltd.) at a pressure of 250 MPa. The obtained circular pellet was sintered at 1500°C for 10 hours in an oxygen atmosphere (S20). This resulted in a sintered pellet of the proton conductor.

[0101] The obtained sintered pellets were cut into disks with a thickness of approximately 500 μm using a low-speed cutter (Isomet 4000). In this way, pellets for evaluation were obtained. Both sides of the evaluation pellets were polished with ethanol dropped onto #500 emery paper.

[0102] Thereafter, Ag paste (manufactured by Tanaka Kikinzoku Kogyo Kogyo) was applied to both polished surfaces of the evaluation pellet by screen printing. The applied Ag paste had a diameter of 8 mm.

[0103] The evaluation pellets coated with the Ag paste were then fired in an air atmosphere at 900° C. for 1 hour, thus producing the evaluation pellets according to Example 1.

[0104] (Evaluation of Proton Conductivity) Using the evaluation pellets according to Example 1, the proton conductivity of the proton conductor was calculated from the resistance and thickness of the pellets. The resistance of the pellets was measured based on the AC impedance method. The proton conductivity was determined as follows.

[0105] Using an LCR meter (HIOKI EE: IM2526), ​​an AC signal with an amplitude of 10 mV was applied to the pellet in the frequency range of 8 MHz to 4 Hz. This measurement was performed in a 1.9% humidified, 1% hydrogen, nitrogen diluted gas atmosphere at 700°C. A Cole-Cole plot was then output. Based on the arc of the output Cole-Cole plot, the intersection of the arc with the real axis was determined. The real axis is the axis where the Y-axis value in the Cole-Cole plot graph is 0. The intersection of the arc on the high frequency side was taken as the resistance of the pellet.

[0106] Based on the determined resistance and thickness of the pellet, the proton conductivity of the proton conductor was calculated.

[0107] Example 2 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.075 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.005 mol

[0108] The subsequent procedures were the same as in Example 1.

[0109] (Evaluation of Proton Conductivity) The proton conductor of Example 2 was evaluated in the same manner as in Example 1.

[0110] Example 3 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.0675 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.0125 mol

[0111] The subsequent procedures were the same as in Example 1.

[0112] (Evaluation of Proton Conductivity) The proton conductor of Example 3 was evaluated in the same manner as in Example 1.

[0113] Example 4 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.065 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.015 mol

[0114] The subsequent procedures were the same as in Example 1.

[0115] (Evaluation of Proton Conductivity) The proton conductor of Example 4 was evaluated in the same manner as in Example 1.

[0116] Example 5 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.064 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.016 mol

[0117] The subsequent procedures were the same as in Example 1.

[0118] (Evaluation of Proton Conductivity) The proton conductor of Example 5 was evaluated in the same manner as in Example 1.

[0119] Comparative Example 1 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.08 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol

[0120] The firing temperature of the pellets was 1650° C. The other procedures were the same as in Example 1.

[0121] (Evaluation of Proton Conductivity) The proton conductor of Comparative Example 1 was evaluated in the same manner as in Example 1.

[0122] Comparative Example 2 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.079 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.001 mol

[0123] The subsequent procedures were the same as in Example 1.

[0124] (Evaluation of Proton Conductivity) The proton conductor of Comparative Example 2 was evaluated in the same manner as in Example 1.

[0125] Comparative Example 3 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.06 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.02 mol

[0126] The subsequent procedures were the same as in Example 1.

[0127] (Evaluation of Proton Conductivity) The proton conductor of Comparative Example 3 was evaluated in the same manner as in Example 1.

[0128] Comparative Example 4 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.0725 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Ni(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.0075 mol

[0129] The subsequent procedures were the same as in Example 1.

[0130] (Evaluation of Proton Conductivity) The proton conductor of Comparative Example 4 was evaluated in the same manner as in Example 1.

[0131] Comparative Example 5 (Preparation of pellets for evaluation of proton conductor) The following materials were prepared as starting materials for the proton conductor: Ba(NO3)2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1 mol ZrO(NO3)2.2H2O (manufactured by Kanto Chemical Co., Ltd.) 0.065 mol Yb(NO3)3.3H2O (manufactured by Mitsuwa Chemical Co., Ltd.) 0.02 mol Ni(NO3)2.3H2O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.015 mol

[0132] The subsequent procedures were the same as in Example 1.

[0133] (Evaluation of Proton Conductivity) The proton conductor of Comparative Example 5 was evaluated in the same manner as in Example 1.

[0134] The proton conductivities measured for Examples 1 to 5 and Comparative Examples 1 to 5 are summarized in Table 1.

[0135]

[0136] The proton conductivities of the proton conductors in Examples 1 to 5 were 0.012 S / cm, 0.013 S / cm, 0.013 S / cm, 0.019 S / cm, and 0.010 S / cm, respectively. The proton conductivity was 0.008 S / cm in Comparative Example 1. This demonstrates that the proton conductivities of the proton conductors in Examples 1 to 5 were improved.

[0137] Furthermore, in Comparative Example 2, where the amount of Cu added was y = 0.01, the proton conductivity was 0.007 S / cm. Therefore, when the amount of Cu added was y = 0.01, the proton conductivity was lower than when no Cu was added. This result reproduces the result of Non-Patent Document 1. It was found that by increasing the value of y, which is the amount of Cu added, to more than 0.01, the effect of improving the proton conductivity was obtained.

[0138] Furthermore, in Comparative Example 3, when the amount of Cu added was y=0.20, the proton conductivity was 0.007 S / cm. Therefore, when the amount of Cu added was y=0.20, the proton conductivity was also lower than when no Cu was added. It was found that by reducing the value of y, which is the amount of Cu added, to less than 0.20, the effect of improving the proton conductivity was obtained.

[0139] In other words, it was found that there is an optimum range for the Cu content y to improve the proton conductivity. a Zr 1-x-y Yb x Cu y O 3-δ It was found that the compound in which Cu was added so that y satisfies the condition 0.01<y<0.20 exhibited improved proton conductivity. In particular, it was found that the proton conductivity was high when y=0.15 as shown in Example 4.

[0140] In Comparative Examples 4 and 5, Ni was used instead of Cu as the additive element. In Comparative Examples 4 and 5, the amount of Ni added was y = 0.075 and y = 0.15, respectively. The proton conductivities of Comparative Examples 4 and 5 were 0.001 S / cm and 0.004 S / cm, respectively, which were lower than the proton conductivity when no Ni was added (i.e., Comparative Example 1). It was found that y = 0.075 and y = 0.15 are within the range of the amount of addition in which proton conductivity is improved when Cu is added, but proton conductivity is not improved when Ni is added. Therefore, it was found that the effect of improving proton conductivity is unique to the addition of Cu.

[0141] Although the mechanisms behind these phenomena are unclear, proton conductivity is expressed as the product of the amount of protons, which are the conduction carriers, and their mobility, so it follows that either or both of these have improved. The amount of protons is the amount of water dissolved in the crystal lattice. Water dissolution proceeds when water molecules fill oxygen vacancies in the crystal, so it is advantageous for the crystal lattice to have many oxygen vacancies. When Cu is added, Cu takes on a lower valence than Zr (+4), so the amount of oxygen vacancies increases to balance the charge in the crystal. Therefore, it is thought that the more Cu is added, the more oxygen vacancies there will be. Therefore, theoretically, this is advantageous for proton dissolution, and the amount of proton dissolution may increase.

[0142] However, in Comparative Examples 2 and 3, proton conductivity decreased despite the addition of Cu. Alternatively, in Comparative Examples 4 and 5, Ni was added, but because Ni also has a lower valence than Zr's +4 valence, it is thought that this increases the amount of oxygen vacancies, and yet proton conductivity decreased. These are presumably due to a decrease in mobility, another factor in proton conductivity. The amount of added element varies depending on the element type, resulting in different local distortions or electronic states in the crystal lattice. Different distortions or electronic states affect mobility, such as localized proton trapping, and therefore it is believed that proton conductivity decreased in Comparative Examples 2 to 5. It is believed that Examples 1 to 5 suppressed the decrease in mobility or improved mobility.

[0143] In Examples 1 to 5, the compound of the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ In the above chemical formula, the effect of adding Cu was confirmed when x = 0.2. A proton conductor in which x satisfies 0.1≦x≦0.4 and y satisfies 0.01<y<0.20 also exhibits the effect of improving proton conductivity.

[0144] <Electrochemical Cell> [Example 6] (Fabrication of Electrochemical Cell) Fabrication of an electrolyte membrane and an electrochemical cell using the same will be described with reference to Fig. 6. Fig. 6 shows the procedure for fabricating the electrochemical cell of Example 6 using the proton conductor of Example 2.

[0145] (1) Preparation of Electrolyte Green Sheet (See S100 to S102) First, an electrolyte ceramic slurry was prepared. The proton conductor used in the electrolyte ceramic slurry was the proton conductor of Example 2. However, instead of the die molding, CIP, and firing processes of S20 shown in the flowchart of FIG. 5, firing was performed in air at 1200°C for 10 hours. Proton conductor powder was obtained by firing in air at 1200°C for 10 hours.

[0146] The proton conductor powder (BaZr 0.75 Yb 0.20 Cu 0.05 O 3-δ The following materials were mixed, including:

[0147] Proton conductor of Example 2 (BaZr 0.75 Yb 0.20 Cu 0.05 O 3-δ ) 50 g Polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd.) 5 g Butyl benzyl phthalate (manufactured by Kanto Chemical Co., Ltd.) 1.25 g Mixed solvent 40 g

[0148] The mixed solvent consisted of butyl acetate (20 g, manufactured by Kanto Chemical Co., Ltd.) and 1-butanol (20 g, manufactured by Kanto Chemical Co., Ltd.) In this way, an electrolyte ceramic slurry was prepared.

[0149] Next, a film made of the electrolyte ceramic slurry was formed on a support sheet made of a polyethylene terephthalate film having a thickness of approximately 50 μm by a doctor blade method. The obtained film made of the slurry was heated at a temperature of 80°C to evaporate the solvent. In this way, an electrolyte green sheet was produced. The electrolyte green sheet had a thickness of approximately 21 μm.

[0150] (2) Preparation of Electrode Green Sheet (see S200 to S202) An electrode ceramic slurry was prepared by mixing the following materials.

[0151] The proton conductor used in the electrode was the proton conductor of Comparative Example 1 (BaZr 0.80 Yb 0.20 O 3-δ ) was used. However, instead of the molding, CIP, and calcination processes of S20 shown in the flowchart of FIG. 5, calcination was carried out in air at 1200°C for 10 hours. By calcining in air at 1200°C for 10 hours, a proton conductor powder was obtained.

[0152] Proton conductor BaZr of Comparative Example 1 0.80 Yb 0.20 O 3-δ ) 10 g Polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd.) 5 g Butyl benzyl phthalate (manufactured by Kanto Chemical Co., Ltd.) 1.25 g NiO (manufactured by Sumitomo Metal Mining Co., Ltd.) 40 g Mixed solvent 40 g

[0153] The mixed solvent consisted of butyl acetate (20 g, manufactured by Kanto Chemical Co., Ltd.) and 1-butanol (20 g, manufactured by Kanto Chemical Co., Ltd.).

[0154] Next, a film made of the electrode ceramic slurry was formed by a doctor blade method on a support sheet made of a polyethylene terephthalate film having a thickness of about 50 μm. The film made of the slurry had a thickness of about 30 μm. The obtained film made of the slurry was heated at a temperature of 80° C. In this way, an electrode green sheet was produced.

[0155] (3) Lamination of Sheets (See S300 to S303) The electrolyte green sheet was cut to obtain one cut electrolyte green sheet. Next, the polyethylene terephthalate film was peeled off from the electrolyte green sheet. The cut electrolyte green sheet had a size of 140 mm x 140 mm. The electrode green sheet was cut to obtain one cut electrode green sheet. The cut electrode green sheet had a size of 140 mm x 140 mm.

[0156] The cut electrode green sheets were stacked to obtain a laminate. The laminate was then hot-pressed at 85°C and 13 MPa. In this manner, a first electrode was produced.

[0157] Furthermore, one cut electrolyte green sheet was laminated on one main surface of the first electrode to obtain a laminate. The obtained laminate was then hot-pressed under conditions of 80°C and 13 MPa. In this way, a compact was obtained.

[0158] The obtained molded body was further pressed at a pressure of 50 MPa (manufactured by Sansho Industry Co., Ltd.) to obtain a laminate. The thickness remained almost unchanged and was about 700 μm.

[0159] The laminate was cut into a size of φ25 mm.

[0160] Finally, the cut laminate was fired at 1475°C for 2 hours in an air atmosphere to produce a membrane electrode assembly. The membrane electrode assembly was an assembly of an electrolyte membrane and a first electrode.

[0161] (4) Formation of Second Electrode (see S304 and S305) Furthermore, a second electrode was provided on the obtained membrane electrode assembly.

[0162] LSC paste (manufactured by Noritake Company Limited, composition La 0.6 Sr 0.4 CoO 3-δ The LSC paste was applied by screen printing to one main surface of the membrane electrode assembly, where the electrolyte membrane was exposed. The applied LSC paste had a diameter of 10 mm. In this way, a cell precursor was obtained.

[0163] The cell precursor was then fired at 950°C for 2 hours in an air atmosphere. In this manner, an electrochemical cell was fabricated comprising a first electrode, an electrolyte membrane, and a second electrode. The first electrode served as a fuel electrode, and the second electrode served as a cathode.

[0164] (Evaluation of Electrochemical Cell) Hydrogen and air were supplied to the electrochemical cell obtained by the above method, and a power generation test of the fuel cell was carried out.

[0165] The electrochemical cell was set in a fuel cell holder (manufactured by Chino Corporation) and placed in an electric furnace. The temperature of the fuel cell holder was raised to 700°C, and the fuel electrode (NiO-BaZr 0.80 Yb 0.20 O 3-δ Humidified hydrogen gas at 20°C was supplied to the anode and humidified air gas at 20°C was supplied to the cathode at 100 cc / min, respectively, and the reduction of the anode was carried out for 3 hours. The electric furnace temperature was then set to 700°C, 600°C, 500°C, 400°C, and 300°C in that order, and after confirming stability of each temperature, electrochemical evaluation was carried out using a potentiogalvanostat (MODULAB XM ECS, manufactured by AMETEC).

[0166] In the electrochemical evaluation, the voltages of the fuel electrode and the air electrode were swept from the open circuit voltage to 0.4 V at 4 mV / sec, and a current-voltage curve and a current-output curve were obtained.

[0167] Figure 7 shows the current-voltage curve and current-output curve obtained in the electrochemical evaluation. The maximum output obtained was 0.83 W / cm at 700°C, 600°C, 500°C, 400°C, and 300°C.2 , 0.62 W / cm 2 , 0.37 W / cm 2 , 0.14 W / cm 2 , 0.02 W / cm 2 It was confirmed that the proton conductor of the present disclosure can be used as an electrolyte to extract a current as an electrochemical cell.

[0168] The proton conductor according to the present disclosure is suitable for systems using electrochemical cells in hydrogen generation systems or fuel cell systems. The membrane electrode assembly according to the present disclosure can also be used in electrochemical hydrogen pumps such as hydrogen purification devices and hydrogen compression devices.

[0169] REFERENCE SIGNS LIST 10 Electrolyte membrane 20 Membrane electrode assembly 21 Electrolyte membrane 22 Electrode 30 Electrochemical cell 31 First electrode 32 Second electrode 33 Electrolyte membrane 40 Fuel cell stack 1000 Fuel cell system 1014 Housing 1021 Oxidant gas supplier 1022 Raw material supplier 1023 Raw material gas supply path 1024 Oxidant gas supply path

Claims

1. Chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ wherein 0.95≦a≦1.05, 0.1≦x≦0.4, 0.01<y<0.20, and 0<δ≦0.65 are satisfied.

2. The proton conductor according to claim 1, wherein in said chemical formula, 0.04≦y≦0.16 is satisfied.

3. The proton conductor according to claim 2, wherein in said chemical formula, 0.125≦y≦0.16 is satisfied.

4. The proton conductor according to claim 3, wherein in said chemical formula, 0.125≦y≦0.15 is satisfied.

5. The proton conductor according to claim 4, wherein in said chemical formula, y=0.15 is satisfied.

6. An electrolyte membrane comprising the proton conductor according to any one of claims 1 to 5.

7. A membrane electrode assembly comprising: the electrolyte membrane according to claim 6; and an electrode provided on the electrolyte membrane.

8. An electrochemical cell comprising: a first electrode; a second electrode; and the electrolyte membrane according to claim 6 provided between the first electrode and the second electrode.

9. A fuel cell stack comprising a plurality of electrochemical cells according to claim 8.

Citation Information

Patent Citations

  • Electrochemical synthesizer for CO2 in-situ hydro-conversion as well as preparation method and application of electrochemical synthesizer

    CN116078314A

  • Proton conductor and membrane electrode assembly

    JP2019106360A

  • Fuel cell and manufacturing method of fuel cell

    JP2020024847A

  • Electrode catalyst, membrane electrode assembly, electrochemical cell, and fuel cell system