Color adjustment plate and solar cell module

The color adjustment plate with a specific optical multilayer film configuration on the solar cell module addresses optical loss and design limitations by controlling reflection and visibility, enhancing the module's efficiency and design flexibility.

WO2024236902A1PCT designated stage expired Publication Date: 2024-11-21NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011598
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-03-25
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing solar cell modules face issues with optical loss due to reflection and reduced productivity caused by the use of harmonic components in visible light regions, leading to increased film thickness and formation time of optical multilayer films, as well as limited design flexibility and visibility.

Method used

A color adjustment plate with a rough surface, featuring a stacked laminate of a transparent substrate, high refractive index layers, and low refractive index layers, where the optical multilayer film has a specific thickness and ratio configuration, is applied on the light incident side of the solar cell module to adjust its color and reduce optical loss.

Benefits of technology

The solution enables high visibility and design flexibility while suppressing optical loss, improving the solar cell module's efficiency and productivity by controlling the reflection spectrum and reducing side peaks, thus enhancing the anti-glare effect and color stability across viewing angles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011598_21112024_PF_FP_ABST
    Figure JP2024011598_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A color adjustment plate (11) is disposed on the light incident side of a solar cell module (1), and adjusts the color of the solar cell module (1). The color adjustment plate (11) comprises: a transparent substrate (12) including a rough surface having an irregular uneven shape; and an optical multilayer film (13) that is a laminate in which a high refractive index layer (131) and a low refractive index layer (132) having a lower refractive index than the high refractive index layer are alternately laminated, the optical multilayer film being formed on the rough surface of the transparent substrate (12). The uneven shape of the rough surface has a root-mean-square height Sq of 0.117 μm to 4.99 μm, and a minimum autocorrelation length Sal of 1.86 μm to 85.0 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Color adjustment plate and solar cell module

[0001] The present invention relates to a color adjusting plate that adjusts the color of a solar cell module, and a solar cell module including the color adjusting plate.

[0002] In recent years, solar cell modules have become widespread, and it has become common to install solar cell modules on roofs or walls of buildings and vehicles, etc. Since the surface color of a solar cell module is generally black or dark blue, solar cell modules with improved design have been developed from the viewpoint of improving design and harmonizing with the surrounding landscape (see, for example, Patent Document 1).

[0003] For example, Patent Document 1 describes a glazing unit in which a first structure surface is formed on the sealing film side of glass laminated on the light-receiving surface of a solar cell, and a photonic structure is provided thereon. In the glazing unit of Patent Document 1, the photonic structure reflects a first partial spectrum and transmits a second partial spectrum. The first partial spectrum reflected by the photonic structure corresponds to a harmonic wave and is within the visible spectrum range.

[0004] Japanese Patent Application Laid-Open No. 2020-511781

[0005] However, the glazing unit of Patent Document 1 uses harmonics as reflected light, which causes many side peaks (sub-reflection peaks) in addition to the main reflection peak, increasing the amount of reflected light and resulting in large optical loss due to reflection.Furthermore, the glazing unit of Patent Document 1 uses harmonic components in the visible light region, which increases the thickness of each film of the optical multilayer film that forms the photonic structure, which increases the time required to form the optical multilayer film and reduces productivity.

[0006] The object of the present invention is to provide a color adjustment plate that can express a highly visible color, has a high designability, and can suppress optical loss due to color expression, and a solar cell module equipped with the same.

[0007] The present invention solves the above problems by the following means: (1) The present invention provides a color adjustment plate that is disposed on the light incident side of a solar cell module and adjusts the color of the solar cell module, the color adjustment plate comprising: a transparent substrate having a rough surface with an irregular asperity shape on one side; and an optical multilayer film that is a laminate in which high refractive index layers and low refractive index layers having a refractive index lower than that of the high refractive index layers are alternately stacked and formed on the one side of the transparent substrate, wherein the asperity shape has a root-mean-square height Sq of 0.117 μm or more and 4.99 μm or less and a minimum autocorrelation length Sal of 1.86 μm or more and 85.0 μm or less.

[0008] (2) In the optical multilayer film, when one unit is defined as a stack of one high refractive index layer and one low refractive index layer, and the ratio of the thickness of the high refractive index layer to the thickness of the unit is defined as a ratio F1, it is preferable that the ratio F1 is 0.025 or more and 0.1 or less.

[0009] (3) The solar cell module of the present invention comprises the color adjustment plate described in (1) or (2) above, a solar cell element, a back surface protection plate that sandwiches the solar cell element together with the color adjustment plate, and a sealing layer that is provided between the color adjustment plate and the back surface protection plate and seals the solar cell element.

[0010] According to the present invention, it is possible to provide a color adjustment plate that can produce a highly visible color, has a high designability, and can suppress optical loss due to color production, and a solar cell module including the color adjustment plate.

[0011] 1 is a diagram illustrating the layer structure of a solar cell module of the present embodiment.

[0023] FIG. 1 is a diagram illustrating an optical multilayer film 13.

[0024] FIG. 1 is a table showing the grit size of the abrasive used in sandblasting and the surface roughness of the first surface 121 of the transparent substrate 12 processed therewith.

[0025] FIG. 1 is a graph showing the reflectance spectra of an optical multilayer film 13 with different unit thicknesses L and ratios F1.

[0026] FIG. 1 is a graph showing the reflectance spectra of an optical multilayer film 13 with different unit thicknesses L and ratios F1.

[0027] FIG. 1 is a graph showing the reflectance spectra of a color adjustment plate including an optical multilayer film 13 in which the thickness L and ratio F1 of one unit are adjusted so that the peak wavelength of reflectance is within a predetermined wavelength range and the peak (maximum) reflectance is different.

[0028] FIG. 1 is a table showing the relationship between the ratio F1, the grit size of the abrasive used to roughen the first surface 121, the L*, a*, and b* values ​​in the L*a*b* color system, and the current loss ΔJsc in a solar cell module 1 using a color adjustment plate 11.

[0029] FIG. 2 is a table showing the diffuse reflectance of 20 measured examples of color adjustment plates 11. 1 is a graph showing the angle dependence of the color that appears in a solar cell module 1 equipped with a color adjustment plate 11. 2 is a table summarizing the chromaticity and the like of solar cell modules using three examples of color adjustment plates 11 that exhibit blue-purple, green, and brown.

[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings, etc. Note that the drawings shown below, including Fig. 1, are schematic diagrams, and the size and shape of each part are appropriately exaggerated to facilitate understanding.

[0013] 1 is a diagram showing the layer structure of a solar cell module of the present embodiment. In Fig. 1, the upper side of the drawing is the light incident side (light receiving side) in use, and the lower side of the drawing is the back side (rear side). The solar cell module 1 of the present embodiment includes, in order from the light incident side, a color adjustment plate 11, a sealant layer 14, a solar cell element 15, a sealant layer 16, and a back protection plate 17.

[0014] The color adjustment plate 11 is a member including a transparent substrate 12 and an optical multilayer film 13. The color adjustment plate 11 is disposed on the light incident side of the solar cell element 15 of the solar cell module 1, with the optical multilayer film 13 side being the light incident side. The color adjustment plate 11 has the function of adjusting the color of the light incident surface of the solar cell module 1.

[0015] The transparent substrate 12 is a plate-shaped member made of glass with high optical transparency. The transparent substrate 12 has a first surface 121, which is the light incident side, that is a rough surface having fine and irregular concave and convex shapes. In addition, the second surface 122, which faces the first surface 121 in the thickness direction of the transparent substrate 12, does not have such an uneven shape. Note that the second surface 122 is not limited to the above example, and may be a smooth surface or a rough surface having an uneven shape like the first surface 121.

[0016] The first surface 121 of the transparent substrate 12 is roughened by sandblasting. However, the first surface 121 of the transparent substrate 12 is not limited to this method, and may be formed by, for example, chemical etching, etc., as long as a preferable surface roughness, which will be described later, can be obtained. In this embodiment, the first surface 121 is roughened by a sandblasting method in which a granular abrasive made of aluminum oxide (Fuji Random A, manufactured by Fuji Manufacturing Co., Ltd.) is sprayed onto the first surface 121 of the transparent substrate 12.

[0017] Fig. 2 is a diagram illustrating the optical multilayer film 13. For ease of understanding, Fig. 2 shows a flat optical multilayer film 13. In Fig. 2, the upper side in the drawing is the light-receiving side, and the lower side is the transparent substrate 12 side. As shown in Fig. 1, the optical multilayer film 13 is formed on the first surface 121 of the transparent substrate 12 so as to follow the uneven shape thereof.

[0018] The optical multilayer film 13 is a laminate in which high-refractive-index layers 131 and low-refractive-index layers 132 having a lower refractive index are alternately stacked in the thickness direction, and is a so-called dielectric multilayer film. The optical multilayer film 13 reflects a portion of light in a predetermined wavelength range, thereby exhibiting a color corresponding to the wavelength range of the reflected light. The optical multilayer film 13 is formed by sputtering on the first surface 121 of the transparent substrate 12. However, the optical multilayer film 13 may be formed by other methods, such as reactive sputtering, vacuum deposition, chemical vapor deposition, or wet coating.

[0019] The high refractive index layer 131 is made of titanium oxide (TiO 2 ) and tantalum pentoxide (Ta 2 O 5 ), alumina (Al 2O 3 ), silicon nitride (SiN X ), niobium pentoxide (Nb 2 O 5 The low refractive index layer 132 is formed using silicon oxide (SiO 2 ), magnesium fluoride (MgF), aluminum fluoride (AlF 3 The high refractive index layer 131 preferably has a refractive index of about 1.8 to 2.8, and the low refractive index layer 132 preferably has a refractive index of about 1.2 to 1.8.

[0020] In this embodiment, the high refractive index layer 131 is made of titanium oxide (TiO 2 The low refractive index layer 132 is made of silicon oxide (SiO 2 The high refractive index layer 131 and the low refractive index layer 132 are formed with a refractive index of 1.5. The materials for forming the high refractive index layer 131 and the low refractive index layer 132 may be selected appropriately depending on the color to be expressed by the optical multilayer film 13, as long as they have a preferable refractive index. In addition, while FIG. 2 shows an example in which the layer closest to the transparent substrate 12 is the high refractive index layer 131, this is not limiting and the low refractive index layer 132 may also be used.

[0021] In this specification, one unit is defined as a state in which one high-refractive index layer 131 and one low-refractive index layer 132 are stacked. In the optical multilayer film 13 of this embodiment, five high-refractive index layers 131 and five low-refractive index layers 132 are alternately stacked, i.e., five units are stacked. From the viewpoint of achieving good color development, it is preferable that three or more units are stacked in the optical multilayer film 13. Furthermore, the greater the number of stacked units, the better the color development can be achieved, but from the viewpoint of production costs, etc., it is preferable that the optical multilayer film 13 be made up of three to five stacked units.

[0022] The encapsulant layers 14 and 16 are members that encapsulate the solar cell elements 15 disposed therebetween. Examples of suitable materials for the encapsulant layers 14 and 16 include transparent materials such as ethylene vinyl acetate (EVA), polyvinyl butyral (PVB), polyolefin-based resins, and ionomer resins. The encapsulant layers 14 and 16 may be made of various materials that have traditionally been used as encapsulants for solar cell modules. Alternatively, the encapsulant layers 14 and 16 may be sheet-like members formed using these materials. While the present embodiment illustrates an example in which two encapsulant layers 14 and 16 are provided, the encapsulant layer may be a single layer depending on the type of solar cell elements 15 used in the solar cell module 1 and the structure of the solar cell module 1. The encapsulant layers 14 and 16 in this embodiment are formed from polyolefin-based resins.

[0023] The solar cell element 15 is a photoelectric conversion element, and may be a solar cell element that has conventionally been used as a solar cell element constituting a solar cell module. For example, the solar cell element 15 may be a crystalline silicon solar cell element fabricated using a single crystal silicon substrate or a polycrystalline silicon substrate, a thin-film silicon solar cell element using amorphous silicon or microcrystalline silicon, a CIS solar cell element, a CIGS solar cell element, a CdTe solar cell element, or a perovskite solar cell element. The solar cell element 15 includes an anti-reflection layer (not shown) on the light-receiving side. The solar cell element 15 also includes electrodes (not shown).

[0024] In this embodiment, an example will be described in which a crystalline silicon solar cell element is used as the solar cell element 15. Also, Fig. 1 shows a simplified configuration of the solar cell module 1, in which one solar cell element 15 is provided between the encapsulant layers 14 and 16. However, when a crystalline silicon solar cell is used as the solar cell element 15 as in this embodiment, a plurality of solar cell elements 15 are arranged between the encapsulant layers 14 and 16 at predetermined intervals in the left-right direction within the screen.

[0025] The rear surface protective plate 17 is a plate-shaped member disposed on the rearmost side of the solar cell module 1. The rear surface protective plate 17 preferably has high weather resistance and water vapor barrier properties. The rear surface protective plate 17 of this embodiment is a glass plate-shaped member. Therefore, the solar cell module 1 of this embodiment is a so-called double-sided glass substrate type solar cell module. The rear surface protective plate 17 is not limited to the above, and may be a plate-shaped member made of resin such as polycarbonate resin, acrylic resin, polyethylene terephthalate (PET), or a metal such as aluminum that does not have light transparency. The rear surface protective plate 17 may also be in the form of a film or sheet.

[0026] The color adjustment plate 11 will now be described in further detail. The transparent substrate 12 of this embodiment is made of optical glass, and the first surface 121 is processed by sandblasting. The first surface 121 of the transparent substrate 12 was sandblasted using abrasives of different grit sizes, and the surface roughness was measured. The abrasives used for sandblasting were aluminum oxide particles (Fuji Random A, manufactured by Fuji Manufacturing Co., Ltd.).

[0027] FIG. 3 is a table showing the grit size of the abrasives used in the sandblasting method and the surface roughness of the first surface 121 of the transparent substrate 12 processed with the abrasives. The larger the grit size of the abrasives used in sandblasting, the smaller the average particle size of the particles. For example, an abrasive with a grit size of #220 has an average particle size (nominal value) of 50 μm, an abrasive with a grit size of #2000 has an average particle size (nominal value) of 6.7 μm, and an abrasive with a grit size of #4000 has an average particle size (nominal value) of 3 μm. The surface roughness of the first surface 121 was measured in accordance with ISO 25178 using a confocal laser microscope (Keyence VK-X3000) in terms of the root mean square height Sq [μm], arithmetic mean height Sa [μm], and minimum autocorrelation length Sal [μm].

[0028] 3, the root mean square height Sq increases as the grit size of the abrasive (the larger the average grain size of the abrasive) decreases, and the minimum autocorrelation length Sal increases as the grit size of the abrasive (the larger the average grain size of the abrasive) decreases, resulting in a large uneven structure in the in-plane direction.

[0029] In this embodiment, it is more preferable that the uneven shape of the first surface 121 has a root-mean-square height Sq of 0.177 μm or more and 4.99 μm or less and a minimum autocorrelation length Sal of 1.86 μm or more and 85.0 μm or less, from the viewpoints of improving the expression of highly visible colors, reducing optical loss due to the expression of color on the surface of the solar cell module, providing an anti-glare effect that suppresses glare from the solar cell module onto the surrounding environment, and suppressing color changes depending on the angle at which the color adjustment plate 11 is observed, i.e., suppressing the angle dependency of color, etc.

[0030] Furthermore, as shown in FIG. 2 , in the optical multilayer film 13, when the thickness of the high-refractive-index layer 131 is L1 and the thickness of the low-refractive-index layer 132 is L2, the thickness L of one unit is L = L1 + L2. If the ratio of the thickness of the high-refractive-index layer 131 to the thickness L of one unit is F1, then F1 = L1 / L. In the optical multilayer film 13 of this embodiment, it is preferable to set the ratio F1 to 0.025 or more and 0.1 or less from the viewpoints of improving the expression of highly visible colors and reducing optical loss due to the expression of colors on the surface of the solar cell module. The optimal value of the ratio F1 within the above range varies depending on the color to be expressed by the color adjustment plate 11. The reasons for this will be explained below.

[0031] 4 and 5 are graphs showing the reflection spectra of the optical multilayer coating 13 with different unit thicknesses L and ratios F1. FIGS. 4 and 5 were obtained by simulation. Various optical simulation software can be used as the simulation tool, such as DiffractMod by RSoft or OptiLayer's optical thin film design software (OptiLayer). FIG. 4 shows the reflection spectra of six examples of the optical multilayer coating 13 in which the unit thickness L is constant and the ratio F1 is varied. FIG. 5 shows the reflection spectra of four examples of the optical multilayer coating 13 in which the unit thickness L is constant and the ratio F1 is varied. In the graphs shown in FIGS. 4 and 5, the vertical axis represents total light reflectance [%] and the horizontal axis represents wavelength [nm].

[0032] The conditions for the optical multilayer film 13 in the simulation are as follows: The optical multilayer film 13 has a high refractive index layer 131 made of titanium oxide (TiO 2 ), the low refractive index layer 132 is silicon oxide (SiO 2 ), and five units are laminated. The optical multilayer coating 13 is assumed to be formed on a smooth surface. The six examples of the optical multilayer coating 13 shown in FIG. 4 have a constant unit thickness L of 130 nm and ratios F1 of 0.1, 0.2, 0.3, 0.5, 0.7, and 0.9. The four examples of the optical multilayer coating 13 shown in FIG. 5 have a constant unit thickness L of 0.2 and ratios F1 of 130 nm, 150 nm, 170 nm, and 210 nm.

[0033] As shown in Figure 4, when the thickness L of one unit is fixed and the ratio F1 is changed, the peak wavelength of the reflectance shifts toward longer wavelengths and the peak also becomes smaller as the ratio F1 increases. Furthermore, the peak (maximum value) of the reflectance is largest when the ratio F1 is 0.2 to 0.5, but as the ratio F1 increases, i.e., when the ratio F1 is 0.7 or 0.9, the side peaks also become very large. Furthermore, as the ratio F1 decreases, i.e., when the ratio F1 is 0.1, the side peaks are suppressed. On the other hand, as shown in Figure 5, when the thickness L of one unit is changed while the ratio F1 is fixed, increasing the thickness L of one unit shifts only the peak wavelength of the reflectance toward longer wavelengths, while the waveform of the reflection spectrum remains approximately constant.

[0034] 6 is a graph showing the reflectance spectrum of a color adjustment plate including an optical multilayer film 13 in which the thickness L and ratio F1 of one unit are adjusted so that the peak wavelength of reflectance is within a predetermined wavelength range and the peak (maximum value) of reflectance is different. The graph shown in FIG. 6 is a graph of the reflectance spectra measured using a spectrophotometer (PerkinElmer Lambda 950) equipped with an integrating sphere for three examples of color adjustment plates. In the graph shown in FIG. 6, the vertical axis represents total light reflectance [%] and the horizontal axis represents wavelength [nm].

[0035] In the three examples of color adjustment plates used in this measurement, the transparent substrate was made of optical glass, and in none of them was sandblasted on the first surface on which the optical multilayer film 13 was formed, and the optical multilayer film 13 was formed on a smooth surface. In addition, in all of the color adjustment plates used in this measurement, the high refractive index layer 131 was made of titanium oxide (TiO 2 ), the low refractive index layer 132 is silicon oxide (SiO 2 ) and includes five units of laminated optical multilayer film 13. Three examples of color adjustment plates were used for the measurement: one in which the thickness of one unit of the optical multilayer film 13 is L=150 nm and the ratio F1=0.2, one in which the thickness of one unit is L=160 nm and the ratio F1=0.1, and one in which the thickness of one unit is L=180 nm and the ratio F1=0.025.

[0036] The three examples of color adjustment plates shown in Figure 6 have a reflection peak (maximum value) in the wavelength range of 500 to 550 nm, but the height of the reflectance peak, i.e., the maximum reflectance value, differs. Therefore, the three examples of color adjustment plates exhibit similar hues but different brightness (lightness). As shown in Figure 6, increasing the thickness L of one unit and decreasing the ratio F1 suppressed the reflectance peak and reduced the brightness (lightness) of the color exhibited by the color adjustment plate. Furthermore, decreasing the thickness L of one unit and increasing the ratio F1 increased the reflectance peak and increased the brightness (lightness) of the color exhibited by the color adjustment plate.

[0037] As described above, the optical multilayer coating 13 can adjust the wavelength at which the main reflectance peak of the optical multilayer coating 13 occurs, the width of that peak, and the reflectance (intensity) of that peak by adjusting the thickness L of one unit and the ratio F1, thereby reducing the reflectance of side peaks. However, while adjusting the ratio F1 and the thickness L of one unit alone can control the color of the optical multilayer coating 13, it cannot adequately control the optical loss caused by that color, resulting in a reduction in the amount of light received by the solar cell element 15. Furthermore, with a flat optical multilayer coating formed on a smooth, non-irregular first surface, the optical interference conditions are angle-dependent, so the color easily changes depending on the observation angle. Furthermore, such a flat optical multilayer coating lacks anti-glare properties, which can result in the solar cell module reflecting light back into the surrounding environment.

[0038] By finding a suitable range for the surface roughness of the first surface 121 (particularly the root-mean-square height Sq and the minimum autocorrelation length Sal), the inventors have realized a color adjustment plate 11 that combines good color development with reduced optical loss, and that also has an anti-glare effect and exhibits little color change depending on the observation angle, and a solar cell module 1 that includes the same. Furthermore, for this color adjustment plate 11, they have further found a suitable range for the ratio F1 of the optical multilayer film 13, and by combining this with the surface roughness of the first surface 121 described above, they have realized a color adjustment plate 11 and a solar cell module 1 that includes the same that further enhance these effects.

[0039] (Regarding Color Development and Current Loss ΔJsc) Here, a plurality of color adjustment plates 11 were produced that exhibited the same hue (green) but differed in the surface roughness of the first surface 121 of the transparent substrate 12, the thickness L of one unit of the optical multilayer film 13, and the ratio F1, and each was applied to a solar cell module 1 to measure the chromaticity, current loss ΔJsc, etc. Fig. 7 is a table showing the ratio F1, the grit size of the abrasive used to roughen the first surface 121, the L*, a*, and b* values ​​in the L*a*b* color system, and the current loss ΔJsc for a solar cell module 1, etc. to which the color adjustment plate 11 was applied.

[0040] In the solar cell module 1 used in this measurement, the solar cell element 15 sealed in the sealing material layers 14 and 16 is an experimental heterojunction crystalline silicon solar cell element. Three examples of the color adjustment plate 11 were prepared, with ratios F1 of 0.2, 0.1, and 0.025. Each of these color adjustment plates 11 includes a transparent substrate 12 made of optical glass and an optical multilayer film 13 in which five units of high-refractive-index layers 131 and low-refractive-index layers 132 are stacked. The optical multilayer film 13 includes a high-refractive-index layer 131 made of titanium oxide (TiO 2 ), the low refractive index layer 132 is silicon oxide (SiO 2 The thickness L of one unit of the optical multilayer film 13 is adjusted in the range of 150 to 180 nm according to F1 so that the hue (green) of the color to be presented is consistent. A color adjustment plate without the optical multilayer film 13 was also prepared.

[0041] Five examples of grit sizes of abrasives were prepared for roughening the first surface 121 of the transparent substrate 12: #220, #1000, #2000, #3000 (only ratio F1 = 0.025), and #4000. Note that "Planar" in Fig. 7, which will be described later, indicates a state in which the surface has not been roughened, i.e., the first surface 121 of the transparent substrate 12 is a smooth surface.

[0042] In the L*a*b* color system, L* indicates lightness (brightness), and a* and b* indicate chromaticity (hue and saturation). The L*, a*, and b* values ​​were measured by placing the center of the surface of each solar cell module 1 in a measurement window provided on the integrating sphere of a spectrophotometer (CM-36dG manufactured by Konica Minolta Japan, Inc.). The measurement mode was SCI (including specular reflection), the reflection measurement conditions were di: 8°, de: 8° (diffuse illumination, 8° directional light reception), the field of view was 8°, the light source was a D65 light source, and the UV conditions were 100% full. The measurements were performed in accordance with JIS Z 8722 Condition c, CIE No. 15 (2004), ISO 7724 / 1, DIN 5033 Teil 7, and ASTM E1164.

[0043] The current loss ΔJsc is the rate of decrease in the short-circuit current value in the solar cell module 1 in which the solar cell element 15 is sealed between the back surface protection plate 17 and the color adjustment plate 11 by the sealing material layers 14, 16, when the short-circuit current value in the solar cell module 1 in each measurement example is taken as the reference value for the solar cell element 15 alone. The smaller the current loss ΔJsc, the better the solar cell module is at efficiently converting incident light into current. For the solar cell module 1, it is preferable that this current loss ΔJsc is small, and it is particularly desirable that the current loss ΔJsc is less than 5.0%.

[0044] The current loss ΔJsc was measured using a class AAA solar simulator (WXS-50S-L2 manufactured by Wacom) as a light source that irradiates the solar cell module with light, and was measured and calculated using a source measure unit (SMU2400 manufactured by Keithley Instruments).

[0045] 7, the greater the ratio F1 of the color adjustment plate 11, the more vivid the apparent color (green) and the greater the lightness (L*). Furthermore, when the ratio F1 of the color adjustment plate 11 was small, the smaller the grit size of the abrasive used to roughen the first surface 121 of the transparent substrate 12, i.e., the greater the surface roughness of the first surface 121 of the transparent substrate 12, the clearer the apparent color and the brighter the green color.

[0046] On the other hand, the solar cell module in which the color adjustment plate 11 does not include the optical multilayer film 13 ("without optical multilayer film" in the table of FIG. 7) exhibited a black color, similar to the conventional solar cell module, due to the surface shape of the silicon and the anti-reflection layer (not shown) provided on the solar cell element 15. Furthermore, the solar cell module in which the first surface 121 of the transparent substrate 12 is a smooth surface ("Planar" in the table of FIG. 7) exhibited a clearer color and a brighter green color when the ratio F1 was larger.

[0047] Next, we will consider the relationship between the lightness (brightness) of the color exhibited by the color adjustment plate 11 and the optical loss (current loss ΔJsc). The color adjustment plate 11 exhibiting a high-lightness color means that the light reflectance is high, which means that the amount of light incident on the solar cell element 15 is small and the optical loss is large. Therefore, a solar cell module including a color adjustment plate 11 exhibiting a high-lightness color will have a large optical loss due to the color adjustment plate 11 and a large current loss ΔJsc. The table in FIG. 7 also shows that there is a trade-off between the lightness L* of the color exhibited and the current loss ΔJsc. It is generally difficult for a solar cell module 1 to exhibit a vivid color while reducing the current loss (optical loss).

[0048] From the measurement results shown in the table of Figure 7, it can be seen that by roughening the first surface 121 of the transparent substrate 12 on which the optical multilayer film 13 is formed with an abrasive of grit size #220 or more and #3000 or less, and by setting the root mean square height Sq of the uneven shape of the first surface 121 to 0.071 μm or more and 4.99 μm or less and the minimum autocorrelation length Sal to 0.688 μm or more and 85.0 μm or less, it is possible to realize a color adjustment plate 11 and a solar cell module 1 that exhibit good color development while suppressing optical loss.

[0049] Furthermore, by setting the surface roughness of the first surface 121 within the above range and further setting the ratio F1 to be 0.025 or more and 0.1 or less, it is possible to achieve good color development while suppressing optical loss. In particular, in the case of a color adjustment plate 11 that exhibits green, by setting the ratio F1 to 0.025 as shown in Figure 7, it is possible to achieve both good color development and reduced optical loss, and to realize a color adjustment plate 11 and a solar cell module 1 with a current loss ΔJsc of 5% or less.

[0050] Furthermore, we will also consider the anti-glare effect of this color adjustment plate 11. If the anti-glare effect of the color adjustment plate 11 is small, the specular reflection from the surface of the solar cell module 1 will be large, and the specular reflection will be observed to be strong depending on the angle of incidence of sunlight and the angle at which the solar cell module 1 is observed. Such specular reflection from the surface of the solar cell module 1 is also called glare, and has an undesirable effect on the surrounding environment.

[0051] Therefore, from the viewpoint of suppressing the reflection of light from the solar cell module 1, it is preferable that the color adjustment plate 11 has an anti-glare effect. The diffuse reflectance of each color adjustment plate 11 was measured as an index of this anti-glare effect. A high diffuse reflectance corresponds to a low regular reflectance. Therefore, a high diffuse reflectance indicates a high proportion of diffusely reflected light and a high anti-glare effect. From the viewpoint of exerting a high anti-glare effect, it is preferable that this diffuse reflectance be 80% or more.

[0052] The color adjustment plate 11 used for measuring the diffuse reflectance was 21 examples, and consisted of a transparent substrate 12 made of optical glass and titanium oxide (TiO 2 ) and a high refractive index layer 131 formed of silicon oxide (SiO 2 ) and an optical multilayer film 13 formed by laminating five units of a low refractive index layer 132 formed by the optical multilayer film 13. However, the 21 examples of color adjustment plates 11 used in measuring the diffuse reflectance differ in the roughness of the uneven shape of the first surface 121, the presence or absence of the optical multilayer film 13, the value of the ratio F1, etc. The surface roughness of the first surface 121 of the transparent substrate 12 is six examples, including examples in which the grit size of the abrasive used for roughening by sandblasting is #220, #1000, #2000, #3000 (only ratio F1 = 0.025), and #4000, and examples in which the first surface 121 is a smooth surface (planar). The optical multilayer film 13 is four examples, including examples without the optical multilayer film 13 and examples with the optical multilayer film 13 and ratios F1 of 0.025, 0.1, and 0.2.

[0053] 8 is a table showing the diffuse reflectance of 20 examples of measured color adjustment plates 11. The diffuse reflectance [%] of each color adjustment plate 11 was measured using a spectrophotometer (CM-36dG manufactured by Konica Minolta Japan, Inc.) and was expressed as the ratio of the L* value measured using the SCE (specular reflection excluded) method to the L* value measured using the SCI (specular reflection included) method. The reflectance measurement conditions were di: 8°, de: 8° (diffuse illumination, light received in an 8° direction), a field of view of 8°, and a D65 light source.

[0054] As shown in the table of Figure 8, the color adjustment plate 11 (Planar) in which the first surface 121 of the transparent substrate 12 was not roughened had a low diffuse reflectance, which is undesirable. Furthermore, the color adjustment plate 11 in which the first surface 121 was roughened with a #4000 abrasive had a low diffuse reflectance and a low, insufficient anti-glare effect compared to when abrasives of other grits were used. Furthermore, the smaller the grit value, the coarser the uneven shape became, resulting in a higher diffuse reflectance.

[0055] Therefore, from the viewpoint of enhancing the anti-glare effect of the color adjustment plate 11, it is preferable that the first surface 121 has an uneven shape that is equal to or larger than the surface roughness when roughened using an abrasive having a grit size of #220 or more and #2000 or less, that is, that the root mean square height Sq of the uneven shape of the first surface 121 is 0.117 μm or more and 4.99 μm or less, and the minimum autocorrelation length Sal is 1.86 μm or more and 85.0 μm or less.

[0056] (Angular Dependence of Color) Next, multiple color adjustment plates with different surface roughnesses of the first surface 121 were prepared, and the angle dependence of color, which changes depending on the direction from which the color adjustment plate is observed, was measured. Figure 9 is a graph showing the angle dependence of color exhibited in a solar cell module 1 equipped with a color adjustment plate 11. In the graph shown in Figure 9, the vertical axis represents color difference ΔE, calculated using a method conforming to CIE DE2000. The horizontal axis represents angle [deg], which is the angle formed with respect to the normal direction to the surface of the solar cell module 1.

[0057] The color difference ΔE was measured using a spectrophotometer (GC-5000 manufactured by Nippon Denshoku Industries Co., Ltd.). The light used for the measurement was a D65 light source with a color temperature of 6500°C, and an angle of 45 degrees corresponds to the position of specular reflection. A white diffuser was used as the reference reflector. The color difference ΔE was measured from angles of 35 degrees to -40 degrees. Note that in the direction of specular reflection (angle 45 degrees), the measured value is saturated with the specular reflection component for some samples, so the color observed at a reflection angle of 35 degrees, which is slightly smaller than specular reflection, was used as the reference color, and the color change relative to this reference color was taken as the color difference ΔE.

[0058] 9 shows the color difference ΔE depending on the observation angle for six examples of color adjustment plates 11: an example in which the grit size of the abrasive used to roughen the first surface 121 of the transparent substrate 12 is #220, #1000, #2000, #3000, or #4000, and an example in which the first surface 121 is a smooth (planar) surface. Each of these seven examples of color adjustment plates 11 has five units of optical multilayer film 13 laminated together, and the high refractive index layer is titanium oxide (TiO 2 ), and the low refractive index layer is silicon oxide (SiO 2 ) In addition, all of the seven examples of the color adjustment plate 11 have a unit thickness L of 160 to 180 nm and a ratio F1 of 0.025, and exhibit a greenish color.

[0059] Generally, differences in color are distinguished by the magnitude of the color difference ΔE. The D-class tolerance for color difference ΔE is 13 to 25, and colors outside this range are perceived as different. Therefore, in the graph shown in Figure 9, the wider the angle range where the color difference ΔE is 25 or less (ΔE≦25), the smaller the angle dependency of the color that is expressed.

[0060] In the graph shown in Figure 9, the color adjustment plate 11 whose first surface 121 is planar has a large angle dependency, with an angle range where ΔE ≦ 25 being only about 10 degrees. However, by roughening the first surface 121, the angle range where ΔE ≦ 25 is expanded to 20 degrees or more. Furthermore, when the surface roughness of the first surface 121 is large, such as in the color adjustment plate 11 whose first surface 121 is roughened using abrasives of grit size #220 or #1000, the angle range where ΔE ≦ 25 is expanded further to 70 degrees or more, and the angle dependency is further reduced.

[0061] Therefore, when making a color adjustment plate 11 with small angular dependence of color, it is preferable to set the grit size of the abrasive used to roughen the first surface 121 to #220 or more and #4000 or less, that is, to set the root mean square height Sq of the uneven shape of the first surface 121 to 0.046 μm or more and 4.99 μm or less, and the minimum autocorrelation length Sal to 0.337 μm or more and 85.0 μm or less.

[0062] As described above, from the viewpoint of minimizing optical loss (current loss) of the solar cell module 1, it is preferable that the surface roughness of the uneven shape of the first surface 121 of the color adjustment plate 11 be small. The first surface 121 is preferably roughened with an abrasive having a grit size of #220 or more and #3000 or less. Furthermore, from the viewpoint of suppressing glare from the solar cell module 1 (enhancing the anti-glare effect), it is preferable that the surface roughness of the uneven shape of the first surface 121 of the color adjustment plate 11 be large. The first surface 121 is preferably roughened with an abrasive having a grit size of #220 or more and #2000 or less. Furthermore, from the viewpoint of reducing the angle dependency of the color of the color adjustment plate 11, it is preferable that the first surface 121 be a rough surface and that the surface roughness of the uneven shape be large. The first surface 121 is preferably roughened with an abrasive having a grit size of #220 or more and #4000 or less.

[0063] From the above results, from the viewpoint of reducing optical loss, exhibiting good color development with high visibility, and obtaining a color adjustment plate 11 in which the angle dependency of color is suppressed, it is preferable that the first surface 121 is roughened with an abrasive having a grit size of #220 or more and #2000 or less, and that the root-mean-square height Sq of the uneven shape of the first surface 121 is 0.117 μm or more and 4.99 μm or less, and the minimum autocorrelation length Sal is 1.86 μm or more and 85.0 μm or less.

[0064] The color adjustment plate 11 and solar cell module 1 of this embodiment are provided with a transparent substrate 12 having a first surface 121 roughened with an abrasive having a grit size of #220 or more and #2000 or less, and having a root-mean-square height Sq of the uneven shape of the first surface 121 of 0.117 μm or more and 4.99 μm or less and a minimum autocorrelation length Sal of 1.86 μm or more and 85.0 μm or less, and an optical multilayer film 13 formed on this roughened first surface 121, thereby enabling the development of good colors with high visibility, improving design, providing an anti-glare effect, and reducing optical loss to improve power generation efficiency.

[0065] In the color adjustment plate 11 and solar cell module 1 of this embodiment, the optical multilayer film 13 has one unit formed by stacking one high-refractive index layer 131 and one low-refractive index layer 132, and the ratio F1 of the thickness L1 of the high-refractive index layer 131 to the thickness L of this unit is 0.025 or more and 0.1 or less, and in particular, since the ratio F1 = 0.025 in the form that exhibits green, it is possible to exhibit good color with high visibility while reducing optical loss. Furthermore, since the thickness ratio of the high-refractive index layer 131 can be reduced, the overall film thickness of the optical multilayer film 13 can be reduced, thereby improving the productivity of the color adjustment plate 11 and solar cell module.

[0066] From the above, according to this embodiment, by adjusting the surface roughness (root-mean-square height Sq, minimum autocorrelation length Sal) of the uneven shape of the first surface 121 on which the optical multilayer film 13 is formed, and further adjusting the thickness L and ratio F1 of one unit of the optical multilayer film 13, it is possible to realize a color adjustment plate 11 and a solar cell module 1 that have small optical loss (current loss ΔJsc) and good color development and anti-glare effect.

[0067] In the above-described embodiment, the color adjustment plate 11 and the solar cell module 1 are described as examples of those that exhibit green color, but by satisfying the above conditions, the color adjustment plate 11 and the solar cell module can also be made to have small current loss and achieve clear color development for other colors.

[0068] 10 is a table summarizing the chromaticity and other properties of solar cell modules using three examples of color adjusting plates 11 that exhibit blue-purple, green, and brown. The color development of each of these three examples of color adjusting plates 11 is adjusted based on the technical concept of this embodiment as described above, and the color adjusting plates 11 and solar cell modules 1 have substantially the same configuration. In the table shown in FIG. 10, Jsc is a function of the short-circuit current [mA / cm 2 ], Voc is the open circuit voltage [V], FF is the fill factor, η is the conversion efficiency [%], and ΔJsc is the current loss [%] as described above.

[0069] The first surface 121 of each of the blue-violet, green, and brown color adjustment plates 11 is roughened by sandblasting with a #2000 abrasive, and the root-mean-square height Sq of the uneven shape of the first surface 121 is 0.117 μm and the minimum autocorrelation length Sal is 1.86 μm. The green color adjustment plate 11 has a ratio F1 = 0.025, and the blue-violet and brown color adjustment plates have a ratio F = 0.05. By appropriately selecting the thickness L of one unit and the materials of each layer of the optical multilayer film 13, the peak wavelength of the reflected light can be adjusted to achieve the desired color.

[0070] As shown in Figure 10, the color adjustment plates 11 exhibiting the above three colors all have a small current loss ΔJsc of less than 5.0% and a power generation efficiency η of more than 21%, making them suitable for use as solar cell modules 1. Furthermore, each color has sufficient chromaticity and brightness to exhibit its respective color. For these reasons, by ensuring that the surface roughness of the first surface 121 on which the optical multilayer film 13 is formed satisfies the above-mentioned preferred range, and further adjusting the thickness L and ratio F1 of one unit of the optical multilayer film 13, it is possible to achieve small current loss, high power generation efficiency, and good color development for a variety of colors.

[0071] (Modifications) The present invention is not limited to the above-described embodiment, and various modifications and variations are possible, and are within the scope of the present invention. (1) The solar cell module 1 may be configured such that, from the light incident side, the color adjustment plate 11, the solar cell element 15, the encapsulant layer 16, and the back surface protection plate 17 are stacked in this order. In this case, the surface of the solar cell element 15 facing the transparent substrate 12 is not covered with the encapsulant layer, and the electrodes and lead wires of the solar cell element 15 are arranged on the back surface of the solar cell element 15 (the back surface protection plate 17 side). In this case, the solar cell element 15 may be a thin-film solar cell element that can be directly deposited on the back surface of the color adjustment plate 11 itself as a substrate. For example, CdTe solar cell elements, some thin-film silicon solar cell elements, and perovskite solar cell elements are suitable. Alternatively, the solar cell element 15 may be integrally formed on the front surface of the back surface protection plate 17, and the encapsulant layer and color adjustment plate 11 may be stacked on that front surface. In this case, the solar cell element 15 can be a thin-film solar cell element formed on an opaque substrate, and for example, a CIS solar cell, some thin-film silicon solar cell elements, perovskite solar cell elements, etc. can be used.

[0072] (2) In the above description, the color adjustment plate 11 is arranged as the light-incident substrate of the two substrates that sandwich the solar cell element in a solar cell module. However, this is not limited to this. For example, the two substrates may be formed of a resin film or the like, and the color adjustment plate 11 may be arranged on the light-incident side of the light-incident substrate.

[0073] (3) While the optical multilayer film 13 is provided on the light-receiving side of the transparent substrate 12 in the example shown, the present invention is not limited thereto. The optical multilayer film 13 may be provided on the back side of the transparent substrate 12, i.e., on the encapsulant layer 14 side. In this case, the second surface 122 is rough and has a fine, irregular uneven shape. Even in this configuration, the root-mean-square height Sq and the minimum autocorrelation length Sal of the uneven shape satisfy the numerical ranges shown in the above-described embodiment, thereby providing a favorable color adjustment plate 11 and solar cell module 1 with good color development and low current loss. In this configuration, the refractive index around the optical multilayer film 13 differs from that in the above-described embodiment, and therefore the thickness L and ratio F1 of one unit, the material of the layer of the optical multilayer film closest to the transparent substrate 12, and the like may be appropriately adjusted.

[0074] (4) The transparent substrate 12 may be made of a resin with high optical transparency, such as polycarbonate resin, acrylic resin, or polyethylene terephthalate (PET), as long as the root-mean-square height Sq and the minimum autocorrelation length Sal of the uneven shape of the first surface 121 can be set within a preferred numerical range.

[0075] (5) A protective sheet made of a resin or glass with high optical transparency may be provided on the light incident side of the color adjustment plate 11 to protect the color adjustment plate 11. Also, a protective layer made of a resin with high optical transparency may be formed on the light incident side of the optical multilayer film 13.

[0076] The present invention is not limited to the above-described embodiments, and the detailed description thereof will be omitted.

[0077] REFERENCE SIGNS LIST 1 solar cell module 11 color adjustment plate 12 transparent substrate 121 first surface 13 optical multilayer film 131 high refractive index layer 132 low refractive index layer 14 encapsulant layer 15 solar cell element 16 encapsulant layer 17 rear surface protection plate

Claims

1. A color adjustment plate disposed on the light incident side of a solar cell module to adjust the color of the solar cell module, comprising: a transparent substrate having one surface roughened with an irregular concave-convex shape; and an optical multilayer film formed on the one surface of the transparent substrate, the optical multilayer film being a laminate of alternating high refractive index layers and low refractive index layers having a lower refractive index than that of the high refractive index layers, the concave-convex shape having a root mean square height Sq of 0.117 μm or more and 4.99 μm or less and a minimum autocorrelation length Sal of 1.86 μm or more and 85.0 μm or less.

2. The color adjustment plate according to claim 1, wherein in the optical multilayer film, a state in which one high refractive index layer and one low refractive index layer are stacked is one unit, and the ratio of the thickness of the high refractive index layer to the thickness of the one unit is taken as F1, the ratio F1 is 0.025 or more and 0.1 or less.

3. A solar cell module comprising: a color adjustment plate as described in claim 1 or claim 2; a solar cell element; a back surface protective plate that holds the solar cell element together with the color adjustment plate; and a sealing layer provided between the color adjustment plate and the back surface protective plate, sealing the solar cell element.

Citation Information

Patent Citations

  • Hard coat film and Anti-reflection film

    JP2008238646A

  • Optical body, wall material, fitting, and sunlight shading device

    JP2012003027A

  • Photovoltaic device

    JP2014107504A

  • Laminated glazing with coloring reflection and high solar transmittance suitable for solar energy systems

    JP2016500799A

  • Coloring structure, display body and manufacturing method of coloring structure

    JP2019109414A