Positive-electrode material, positive electrode, and battery
The positive electrode material configuration with a fibrous carbon second conductive material and a Li-Ti-M first solid electrolyte addresses the issue of high initial resistance and increased resistance in batteries by ensuring uniform electrochemical reactions and preventing electrolyte decomposition, maintaining low resistance and high performance.
Patent Information
- Application Number
- PCT/JP2024/015945
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-21
AI Technical Summary
Batteries using positive electrode materials with surface-coated solid electrolytes tend to have high initial resistance and increased resistance during repeated charging and discharging due to insufficient contact between the active material and conductive materials, leading to non-uniform electrochemical reactions and potential decomposition of the electrolyte.
A positive electrode material configuration that includes a conductive material with a fibrous carbon second conductive material and a first solid electrolyte containing Li, Ti, and M (Ca, Mg, Al, Y, or Zr) to reduce initial resistance and prevent increased resistance, where the first conductive material covers the active material and the second conductive material forms an electron conduction path, and the first solid electrolyte has high oxidation resistance.
The configuration reduces initial battery resistance and prevents resistance increases during repeated charging and discharging by ensuring uniform electrochemical reactions and preventing electrolyte decomposition, maintaining low resistance and high performance.
Smart Images

Figure JP2024015945_21112024_PF_FP_ABST
Abstract
Description
Cathode materials, cathodes, and batteries
[0001] The present disclosure relates to positive electrode materials, positive electrodes, and batteries.
[0002] Patent Document 1 discloses a cathode material including a cathode active material and a first solid electrolyte material that coats at least a portion of the surface of the cathode active material. The first solid electrolyte material includes Li, Ti, M1, and F, where M1 is at least one element selected from the group consisting of Ca, Mg, Al, Y, and Zr. Patent Document 1 also discloses that the cathode material further includes a second electrolyte material that is different from the first solid electrolyte material.
[0003] International Publication No. 2021 / 187391
[0004] An object of the present disclosure is to provide a positive electrode material that can reduce the initial resistance of a battery and can suppress an increase in the resistance of the battery when it is repeatedly charged and discharged.
[0005] The positive electrode material of the present disclosure comprises: a positive electrode active material; a coating material including a first conductive material and a first solid electrolyte, and coating at least a portion of a surface of the positive electrode active material; a second conductive material that is a fibrous carbon material; and a second solid electrolyte, wherein the first solid electrolyte includes Li, Ti, M, and F, and the M is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr, and the second conductive material has an average fiber diameter of 0.4 nm or more and 50 nm or less.
[0006] The present disclosure provides a positive electrode material that can reduce the initial resistance of a battery and suppress an increase in the resistance of the battery when the battery is repeatedly charged and discharged.
[0007] FIG. 1 is a cross-sectional view showing a schematic configuration of a positive electrode material in embodiment 1. FIG. 2 is a cross-sectional view showing a schematic configuration of a positive electrode in embodiment 2. FIG. 3 is a cross-sectional view showing a schematic configuration of a battery in embodiment 3. FIG. 4 is a cross-sectional view showing a schematic configuration of a battery in a modified example. FIG. 5 is a secondary electron image of particles of the basic active material of Example 1 taken with a scanning electron microscope (SEM). FIG. 6 is a backscattered electron image of particles of the basic active material of Example 1 taken with an SEM in the same observation area as FIG. 5. FIG. 7 is a cross-sectional secondary electron image of a positive electrode active material layer of Example 3 taken with an SEM. FIG. 8 is an elemental mapping image showing the distribution of Ni obtained with an SEM-energy dispersive X-ray analyzer (EDS) in the same observation area as FIG. 7. FIG. 9 is an elemental mapping image showing the distribution of Nb obtained with an SEM-EDS in the same observation area as FIG. 7. FIG. 10 is an elemental mapping image showing the distribution of C obtained with an SEM-EDS in the same observation area as FIG. 7. Fig. 11 is an element mapping image showing the distribution of F obtained by SEM-EDS in the same observation region as in Fig. 7. Fig. 12 is an element mapping image showing the distribution of S obtained by SEM-EDS in the same observation region as in Fig. 7. Fig. 13 is a cross-sectional backscattered electron image of the positive electrode active material layer of Example 3 taken by SEM. Fig. 14 is an enlarged view of region A in Fig. 13.
[0008] (Findings underlying the present disclosure) Batteries using a cathode material including a cathode active material and a solid electrolyte that coats at least a portion of the surface of the cathode active material tend to have relatively high initial resistance. Patent Document 1 proposes that a second electrolyte material be added as a material for increasing the ease of Li ion migration, thereby improving ionic conductivity in the cathode, thereby reducing the initial resistance of the battery and suppressing an increase in the battery's internal resistance during charging. However, batteries using the cathode material disclosed in Patent Document 1 are prone to increasing resistance when repeatedly charged and discharged.
[0009] The present inventors have conducted extensive research to develop a positive electrode material that can reduce the initial resistance of a battery and suppress an increase in the resistance of the battery during repeated charge and discharge. As a result, they have arrived at the positive electrode material of the present disclosure.
[0010] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments.
[0011] First Embodiment FIG. 1 is a cross-sectional view showing a schematic configuration of a positive electrode material 100 according to a first embodiment.
[0012] The cathode material 100 includes a cathode active material 11, a coating material 14, a second conductive material 15, and a second solid electrolyte 16. The coating material 14 includes a first conductive material 12 and a first solid electrolyte 13. The coating material 14 coats at least a portion of the surface 11s of the cathode active material 11. The first solid electrolyte 13 includes Li, Ti, M, and F, where M is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr. The second conductive material 15 is a fibrous carbon material having an average fiber diameter of 0.4 nm or more and 50 nm or less. The cathode material 100 of the first embodiment can reduce the initial resistance of a battery and suppress an increase in the battery resistance during repeated charge and discharge.
[0013] In a battery using a positive electrode material such as that disclosed in Patent Document 1, the conductive material serves to ensure electronic conductivity and uniformity of the electrochemical reaction throughout the positive electrode active material layer. On the other hand, if the content of the conductive material in the positive electrode material is too high, the conductive material may narrow the ion conduction path within the positive electrode active material layer, resulting in failure to ensure uniformity of the electrochemical reaction.
[0014] The inventors discovered that by using a fibrous carbon material having an average fiber diameter of 0.4 nm or more and 50 nm or less as the conductive material, the electronic conductivity of the positive electrode active material layer can be ensured even with a low content of the conductive material. However, when a positive electrode active material layer is formed using a positive electrode material including a positive electrode active material whose surface is coated with a first solid electrolyte, a fibrous carbon material, and a second solid electrolyte, the fibrous carbon material does not easily penetrate into the first solid electrolyte. This can result in insufficient contact between the positive electrode active material and the fibrous carbon material. Insufficient contact between the positive electrode active material and the fibrous carbon material can result in insufficient uniformity of the electrochemical reaction in the positive electrode active material layer.
[0015] As a result of further intensive research into ensuring uniformity of the electrochemical reaction in the positive electrode active material layer, the inventors have come up with the idea of including a conductive material in the coating material that coats the positive electrode active material. In a positive electrode active material layer using the positive electrode material 100 of embodiment 1, an electronic conduction path can be formed between the positive electrode active material 11 and the second conductive material 15 via the first conductive material 12, and between the positive electrode active materials 11 and 11 via the first conductive material 12. This makes it easier to ensure uniformity of the electrochemical reaction throughout the positive electrode active material layer. As a result, the initial resistance of the battery can be reduced.
[0016] Furthermore, in the positive electrode material 100 according to the first embodiment, the electronic conductivity of the positive electrode active material layer is ensured even when the content of the second conductive material 15 is small, and therefore the contact area between the second conductive material 15 and the second solid electrolyte 16 can be reduced. As a result, the resistance of the battery is less likely to increase even when the battery is repeatedly charged and discharged.
[0017] Furthermore, in a battery using a cathode material including a cathode active material 11 whose surface is coated with a first solid electrolyte 13, a second conductive material 15, and a second solid electrolyte 16, the potential of the cathode active material 11 and the potential of the second conductive material 15 tend to increase during charging of the battery. When a high-potential cathode active material 11 or a high-potential second conductive material 15 comes into contact with a first solid electrolyte 13 having a narrow potential window on the high-potential side, i.e., low oxidation resistance, the first solid electrolyte 13 decomposes. As a result, an oxidative decomposition layer is formed within the cathode active material layer. The oxidative decomposition layer functions as a resistance layer and can increase the internal resistance of the battery during charging. In the cathode material 100 according to the first embodiment, the first solid electrolyte 13 contains Li, Ti, M, and F, where M is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr. Therefore, the first solid electrolyte 13 is resistant to decomposition even at high potentials and has high oxidation resistance. As a result, the resistance of the battery is less likely to increase even after repeated charging and discharging.
[0018] The average fiber diameter of the second conductive material 15 can be determined, for example, by SEM observation of a cross section of a positive electrode active material layer produced using the positive electrode material 100 .
[0019] 1 , the first conductive material 12 may be in direct contact with the surface 11s of the positive electrode active material 11. The first solid electrolyte 13 may be in direct contact with the first conductive material 12, or may be in direct contact with the surface 11s of the positive electrode active material 11. That is, the surface 11s of the positive electrode active material 11 that is not covered with the first conductive material 12 and a portion of the first conductive material 12 may be covered with the first solid electrolyte 13. Note that a portion of the first conductive material 12 may not be covered with the first solid electrolyte 13 due to, for example, flow of the first solid electrolyte 13 that covered the first conductive material 12 when the positive electrode active material layer is pressed.
[0020] The first conductive material 12 coats at least a portion of the surface 11s of the positive electrode active material 11. Here, the positive electrode active material 11 having at least a portion of its surface 11s coated with the first conductive material 12 is defined as the basic active material 10. The first solid electrolyte 13 coats at least a portion of the surface of the basic active material 10, which includes the first conductive material 12 and the positive electrode active material 11. According to the above configuration, at least a portion of the first conductive material 12 is coated with the first solid electrolyte 13. Therefore, since the contact area between the positive electrode active material 11 and the second solid electrolyte 16 and the contact area between the first conductive material 12 and the second solid electrolyte 16 are small, the second solid electrolyte 16 is less likely to decompose even if the potential of the positive electrode active material 11 and the potential of the first conductive material 12 increase during charging of the battery. As a result, an increase in the battery resistance during repeated charging and discharging is further suppressed.
[0021] Here, the positive electrode active material 11 having at least a portion of its surface 11s coated with the coating material 14 is defined as a composite active material 20. The positive electrode material 100 includes the composite active material 20, a second conductive material 15, and a second solid electrolyte 16. The second conductive material 15 and the second solid electrolyte 16 are located between particles of the composite active material 20 including the positive electrode active material 11 and the coating material 14. With the above configuration, the lithium ion conductivity of the positive electrode active material layer is improved, and the initial resistance of the battery can be reduced.
[0022] (Positive Electrode Active Material) Examples of the positive electrode active material 11 include lithium-containing transition metal oxides, lithium-containing transition metal phosphates, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides, and transition metal oxynitrides. In particular, using a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate as the positive electrode active material can reduce the manufacturing cost of the battery and increase the average discharge voltage. Examples of lithium-containing transition metal oxides include lithium cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, and lithium nickel manganese oxide. Examples of lithium-containing transition metal phosphates include lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, and lithium nickel phosphate. At least one selected from these positive electrode active materials can be used.
[0023] The particles of the positive electrode active material 11 may be primary particles or secondary particles. The positive electrode active material 11 has a median diameter of, for example, 0.1 μm or more and 100 μm or less. In this disclosure, the median diameter refers to the particle size (d50) when the cumulative volume in the volume-based particle size distribution is equal to 50%. The volume-based particle size distribution is measured, for example, using a laser diffraction measurement device or an image analysis device.
[0024] The positive electrode active material 11 may have a particle shape having a plurality of recesses on its surface 11s. In this case, the first conductive material 12 may be disposed in the plurality of recesses of the positive electrode active material 11. This configuration further reduces the initial resistance of the battery and further suppresses an increase in the resistance of the battery during repeated charge and discharge. The fact that the first conductive material 12 is disposed in the plurality of recesses of the positive electrode active material 11 can be confirmed, for example, by a secondary electron image or a backscattered electron image of the particles of the basic active material 10 taken with a scanning electron microscope (SEM).
[0025] The average spacing between the plurality of recesses may be 500 nm or less, and the average height of the plurality of recesses may be 500 nm or less. This configuration facilitates the formation of a state in which the first conductive material 12 is disposed in the recesses of the positive electrode active material 11, and the first conductive material 12 is not disposed in portions of the positive electrode active material 11 other than the recesses. This can suppress an increase in the contact area between the positive electrode active material 11 and the second solid electrolyte 16, and an increase in the contact area between the first conductive material 12 and the second solid electrolyte 16. As a result, the initial resistance of the battery is further reduced, and an increase in the battery resistance during repeated charge and discharge is further suppressed.
[0026] (First Conductive Material) In the present embodiment, the first conductive material 12 is a particulate material. With the above configuration, the first conductive material 12 is easily attached to the surface 11s of the positive electrode active material 11. As a result, the initial resistance of the battery is further reduced, and an increase in the resistance of the battery during repeated charge and discharge is further suppressed.
[0027] The shape of the first conductive material 12 may be, for example, a sphere, an oval sphere, etc. The shape of the first conductive material 12 may be a sphere.
[0028] Examples of the first conductive material 12 that can be used include graphites such as natural graphite or artificial graphite, carbon blacks such as acetylene black and ketjen black, and conductive polymer compounds such as polyaniline, polypyrrole, and polythiophene.
[0029] The first conductive material 12 may contain carbon black. According to the above configuration, the electron conductivity of the positive electrode active material layer can be improved. The first conductive material 12 may be carbon black.
[0030] As the carbon black, for example, acetylene black can be used. When the first conductive material 12 contains acetylene black, the electron conductivity in the positive electrode active material layer can be improved.
[0031] The first conductive material 12 may have a median diameter of 100 nm or less. According to the above configuration, the first conductive material 12 is more likely to adhere to the surface 11s of the positive electrode active material 11. Therefore, in the positive electrode active material layer, an electron conduction path is more likely to be formed by connecting the first conductive material 12 and the second conductive material 15. As a result, the electron conductivity of the positive electrode active material layer can be improved.
[0032] There is no particular limitation on the lower limit of the median diameter of the first conductive material 12. The lower limit of the median diameter of the first conductive material 12 may be, for example, 10 nm.
[0033] (Second Conductive Material) In the present embodiment, the second conductive material 15 is a fibrous carbon material. According to the above configuration, the first conductive material 12 contained in the coating material 14 that coats at least a portion of the surface 11s of the positive electrode active material 11 is easily bonded to the second conductive material 15. As a result, the initial resistance of the battery is further reduced, and an increase in the resistance of the battery during repeated charging and discharging is further suppressed.
[0034] Examples of the second conductive material 15 include vapor-grown carbon fiber, carbon nanotubes, and carbon nanofibers. The second conductive material 15 may contain any one of these materials, or may contain two or more of these materials. The second conductive material 15 may be composed of any one of these materials, or may be composed of two or more of these materials.
[0035] The second conductive material 15 may contain carbon nanotubes. For example, a second conductive material 15 that is a carbon nanotube and a second conductive material 15 other than a carbon nanotube may be present between the plurality of composite active materials 20. The second conductive material 15 may be a carbon nanotube.
[0036] The second conductive material 15 has an average fiber diameter of 0.4 nm or more and 50 nm or less. With the above configuration, the second conductive material 15 easily forms an electron conduction path in the positive electrode active material layer. As a result, the electron conductivity in the positive electrode active material layer can be improved.
[0037] The lower limit of the average fiber diameter of the second conductive material 15 may be 0.8 nm or 1.2 nm, and the upper limit of the average fiber diameter of the second conductive material 15 may be 10 nm, 5 nm, or 2 nm.
[0038] The second conductive material 15 may have an average length of 5 μm or more. According to the above configuration, the second conductive material 15 more easily forms an electron conduction path in the positive electrode active material layer. As a result, the electron conductivity in the positive electrode active material layer can be further improved.
[0039] There is no particular upper limit to the average length of the second conductive material 15. The upper limit to the average length of the second conductive material 15 may be, for example, 20 μm.
[0040] The average length of the second conductive material 15 can be determined by the same method as the method for determining the average fiber diameter of the second conductive material 15 described above.
[0041] The ratio M2 / M1 of the mass M2 of the second conductive material 15 to the sum M1 of the mass of the positive electrode active material 11 and the mass of the second conductive material 15 may be 0.005% or more and 0.02% or less. If the content of the second conductive material 15 in the positive electrode active material layer is too high, the contact area between the second conductive material 15 and the second solid electrolyte 16 increases, making the second solid electrolyte 16 more susceptible to decomposition during battery charging. If the ratio M2 / M1 is 0.02% or less, decomposition of the second solid electrolyte 16 during battery charging is suppressed. Furthermore, if the content of the second conductive material 15 is too high, the second conductive material 15 narrows the ion conduction path in the positive electrode active material layer, which may result in insufficient uniformity of the electrochemical reaction. If the ratio M2 / M1 is 0.02% or less, uniformity of the electrochemical reaction is more likely to be ensured.
[0042] The ratio M2 / M1 can be determined, for example, from the charge ratio.
[0043] (First Solid Electrolyte) The first solid electrolyte 13 contains Li, Ti, M, and F. M is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr. With the above configuration, the first solid electrolyte 13 has high oxidation resistance and is less likely to decompose under high potential.
[0044] The first solid electrolyte 13 may be made of Li, Ti, M, and F. "Made of Li, Ti, M, and F" means that, except for inevitable impurities, no materials other than Li, Ti, M, and F are intentionally added.
[0045] M may contain Al. The above configuration improves the lithium ion conductivity of the first solid electrolyte 13. As a result, the initial resistance of the battery can be reduced.
[0046] The first solid electrolyte 13 may include, for example, a solid electrolyte represented by the following composition formula (1): In composition formula (1), α, β, γ, and δ are each independently a value greater than 0.
[0047] Li α Ti β M γ F δ ...(1)
[0048] The solid electrolyte represented by composition formula (1) has higher ionic conductivity than a solid electrolyte consisting only of Li and a halogen element, and therefore, when the solid electrolyte represented by composition formula (1) is used in a battery, the charge / discharge efficiency of the battery can be improved.
[0049] To further increase the ionic conductivity of the first solid electrolyte 13, M in the composition formula (1) may be Al.
[0050] The first solid electrolyte 13 may include a solid electrolyte represented by the following composition formula (2): In composition formula (2), M2 is at least one selected from the group consisting of Zr, Ni, Fe, and Cr, m is the valence of M2, and 0.1<x<0.9, 0≦y<0.1, 0≦z<0.1, and 0.8<b≦1.2 are satisfied.
[0051] Li6-(4-x-my)b (Ti 1-x-y Al x M2 y ) b F 6-2z O z ...Formula (2)
[0052] In the composition formula (2), when M2 contains a plurality of elements, m is the sum of the products of the composition ratios of the respective elements and the valences of the elements. For example, when M2 contains an element Me1 and an element Me2, and the composition ratio of the element Me1 is a1 and the valence is m1, and the composition ratio of the element Me2 is a2 and the valence of the element Me2 is m2, m is expressed as m1a1+m2a2.
[0053] The solid electrolyte 13 may consist essentially of Li, Ti, Al, and F. Here, "the halide solid electrolyte consists essentially of Li, Ti, Al, and F" means that the molar ratio (i.e., molar fraction) of the total amount of substance of Li, Ti, Al, and F to the total amount of substance of all elements constituting the halide solid electrolyte is 90% or more. As an example, the molar ratio (i.e., molar fraction) may be 95% or more. The solid electrolyte 13 may consist only of Li, Ti, Al, and F.
[0054] To further increase the ionic conductivity of first solid electrolyte 13, the ratio of the amount of substance of Li to the total amount of substance of Ti and Al in the above solid electrolyte may be 1.12 or more and 5.07 or less.
[0055] The first solid electrolyte 13 may include a solid electrolyte represented by the following composition formula (3): In composition formula (3), 0<x<1 and 0<b≦1.5 are satisfied.
[0056] Li 6-(4-x)b (Ti 1-x Al x ) b F6...(3)
[0057] A solid electrolyte having such a composition has high ionic conductivity.
[0058] In order to enhance the ionic conductivity of the first solid electrolyte 13, the relationship 0.1≦x≦0.9 may be satisfied in the composition formula (3).
[0059] In the composition formula (3), 0.1≦x≦0.7 may be satisfied.
[0060] The upper and lower limits of the range of x in composition formula (3) can be defined by any combination selected from the following numerical values: 0.1, 0.3, 0.4, 0.5, 0.6, 0.67, 0.7, 0.8, and 0.9.
[0061] In order to increase the ionic conductivity of the first solid electrolyte 13, the relationship 0.8≦b≦1.2 may be satisfied in the composition formula (3).
[0062] The upper and lower limits of the range of b in composition formula (3) can be defined by any combination selected from the following numerical values: 0.8, 0.9, 0.94, 1.0, 1.06, 1.1, and 1.2.
[0063] The solid electrolyte may be crystalline or amorphous.
[0064] The shape of the first solid electrolyte 13 is not particularly limited and may be, for example, needle-like, spherical, or oval-spherical. For example, the shape of the first solid electrolyte 13 may be particulate.
[0065] When the first solid electrolyte 13 is particulate (e.g., spherical), the first solid electrolyte 13 has an average particle size of, for example, 10 nm to 100 nm. With this configuration, it becomes relatively easy to uniformly coat the first solid electrolyte 13 with the coating material.
[0066] The average particle size of the first solid electrolyte 13 can be measured, for example, using an SEM image. Specifically, the average particle size can be determined by using the SEM image to calculate the average circle-equivalent diameter of 20 arbitrarily selected particles of the first solid electrolyte 13. The average particle size of other materials, such as the second solid electrolyte 16 described below, can also be determined using the same method.
[0067] (Second Solid Electrolyte) The second solid electrolyte 16 includes a solid electrolyte having high ionic conductivity. The second solid electrolyte 16 may include a plurality of solid electrolytes having different chemical compositions. For example, a solid electrolyte having a different chemical composition from the first solid electrolyte 13 and a solid electrolyte having the same chemical composition as the first solid electrolyte 13 may be present as the second solid electrolyte 16 among the plurality of composite active materials 20.
[0068] The second solid electrolyte 16 may contain a halide solid electrolyte. The halide solid electrolyte has high ionic conductivity and excellent high potential stability. Furthermore, the halide solid electrolyte has low electronic conductivity and high oxidation resistance, and is therefore less susceptible to oxidative decomposition upon contact with the composite active material 20. Therefore, when the second solid electrolyte 16 contains a halide solid electrolyte, the output characteristics of the battery can be improved.
[0069] Examples of halide solid electrolytes that can be used include Li(Ca,Y,Gd)X, LiMgX, LiFeX, Li(Al,Ga,In)X, Li(Al,Ga,In)X, and LiI. In these halide solid electrolytes, the element X is at least one selected from the group consisting of Cl, Br, and I.
[0070] The halide solid electrolyte may not contain sulfur. In this case, generation of sulfur-containing gases such as hydrogen sulfide gas from the solid electrolyte can be avoided. A sulfur-free solid electrolyte refers to a solid electrolyte represented by a composition formula that does not contain elemental sulfur. Therefore, a solid electrolyte containing a very small amount of sulfur, for example, a solid electrolyte having a sulfur content of 0.1 mass% or less, is classified as a sulfur-free solid electrolyte. The halide solid electrolyte may further contain oxygen as an anion other than the halogen element.
[0071] The second solid electrolyte 16 may include a sulfide solid electrolyte. Compared to solid electrolytes such as oxide solid electrolytes and halide solid electrolytes, sulfide solid electrolytes have a narrower potential window and are more susceptible to decomposition at high potentials. However, with the above configuration, the contact area between the positive electrode active material 11 and the first conductive material 12 and the second solid electrolyte 16 is reduced, making it difficult for an oxidative decomposition layer to form within the positive electrode active material layer. As a result, the initial resistance of the battery can be reduced.
[0072] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, and Li 3.25 Ge 0.25 P 0.75 S4, Li10 GeP2S 12 LiX, LiO, MO, etc. can be used. q , Li p MO q The element X in "LiX" is at least one element selected from the group consisting of F, Cl, Br, and I. q " and "Li p MO q " The element M is at least one element selected from the group consisting of P, Si, Ge, B, Al, Ga, In, Fe, and Zn. q " and "Li p MO q In the above formula, p and q are independent natural numbers.
[0073] The second solid electrolyte 16 may be a sulfide solid electrolyte. That is, the second solid electrolyte 16 may be made of a sulfide solid electrolyte. "Made of a sulfide solid electrolyte" means that, with the exception of inevitable impurities, no materials other than the sulfide solid electrolyte are intentionally added. For example, the sulfide solid electrolyte may contain lithium sulfide and phosphorus sulfide. For example, the sulfide solid electrolyte may be Li2S-P2S5.
[0074] The shape of the second solid electrolyte 16 is not particularly limited and may be, for example, needle-like, spherical, or oval-spherical. For example, the second solid electrolyte 16 may be particulate.
[0075] When the second solid electrolyte 16 is particulate (e.g., spherical), the average particle size of the second solid electrolyte 16 may be 100 μm or less. If the average particle size is greater than 100 μm, the composite active material 20 and the second solid electrolyte 16 may not form a good dispersed state in the positive electrode material 100. This may result in poor charge-discharge characteristics. The average particle size of the second solid electrolyte 16 may be 10 μm or less. When the average particle size of the second solid electrolyte 16 is within the above range, the composite active material 20 and the second solid electrolyte 16 can form a good dispersed state in the positive electrode material 100.
[0076] The average particle size of the second solid electrolyte 16 may be smaller than the average particle size of the composite active material 20. With this configuration, the composite active material 20 and the second solid electrolyte 16 can be more effectively dispersed in the electrode.
[0077] The average particle size of the composite active material 20 may be 0.1 μm or more and 100 μm or less. When the average particle size of the composite active material 20 is 0.1 μm or more, the composite active material 20 and the second solid electrolyte 16 can form a well-dispersed state in the positive electrode material 100. As a result, the charge / discharge characteristics of the battery are improved. Furthermore, when the average particle size of the composite active material 20 is 100 μm or less, the lithium diffusion rate within the positive electrode active material 11 is improved. This enables the battery to operate at high power.
[0078] The average particle size of the composite active material 20 may be larger than the average particle size of the second solid electrolyte 16. Even with this configuration, the composite active material 20 and the second solid electrolyte 16 can be well dispersed in the electrode.
[0079] The coating material 14 may further include a material such as an oxide material or an oxide solid electrolyte as an underlayer material. The coating material 14 may form a first layer including the underlayer material and a second layer including the first conductive material 12 and the first solid electrolyte 13. The underlayer material may be a material including Nb. The underlayer material typically includes lithium niobate (LiNbO3). This configuration can improve the charge / discharge efficiency of the battery. The oxide solid electrolyte described below can also be used as the oxide solid electrolyte, which is the underlayer material.
[0080] In the positive electrode material 100, the second solid electrolyte 16 and the composite active material 20 may be in contact with each other as shown in FIG.
[0081] The positive electrode material 100 may include a plurality of composite active materials 20 , a plurality of second conductive materials 15 , and a plurality of second solid electrolytes 16 .
[0082] The shape of the positive electrode material 100 is not particularly limited. The positive electrode material 100 may be in the form of a powder or a slurry. Alternatively, the positive electrode material 100 may be in the form of a compact obtained by pressing the positive electrode material 100.
[0083] <Method for Producing Positive Electrode Material> The positive electrode material 100 can be produced, for example, by the following method.
[0084] First, the surfaces of particles of the positive electrode active material 11 are coated with a first conductive material 12 to prepare a base active material 10. Next, the surfaces of particles of the basic active material 10 are coated with a first solid electrolyte 13 to prepare a composite active material 20. The method for coating the first conductive material 12 and the first solid electrolyte 13 is not particularly limited. For example, by mixing particles of the positive electrode active material 11 and particles of the first conductive material 12, particles of the basic active material 10 in which the surfaces of the particles of the positive electrode active material 11 are coated with the first conductive material 12 are obtained. By mixing particles of the basic active material 10 and particles of the first solid electrolyte 13, particles of the composite active material 20 in which the surfaces of the particles of the basic active material 10 are coated with the first solid electrolyte 13 are obtained.
[0085] The particles of the composite active material 20, the particles of the second conductive material 15, and the particles of the second solid electrolyte 16 are mixed together to obtain the positive electrode material 100.
[0086] (Embodiment 2) Figure 2 is a cross-sectional view showing a schematic configuration of a positive electrode 200 in embodiment 2. The positive electrode 200 includes a positive electrode current collector 21 and a positive electrode active material layer 22 supported by the positive electrode current collector 21. The positive electrode active material layer 22 includes the positive electrode material 100 of embodiment 1. That is, the positive electrode active material layer 22 includes a composite active material 20, a second conductive material 15, and a second solid electrolyte 16. The positive electrode 200 in embodiment 2 can reduce the initial resistance of the battery and suppress an increase in the resistance of the battery during repeated charge and discharge.
[0087] The volume ratio "v1:100-v1" of the positive electrode active material 11 to the total of the first conductive material 12, the first solid electrolyte 13, the second conductive material 15, and the second solid electrolyte 16 may satisfy 30≦v1≦95. Here, v1 represents the volume fraction of the positive electrode active material 11 when the total volume of the positive electrode active material 11 contained in the positive electrode active material layer 22 and the first conductive material 12, the first solid electrolyte 13, the second conductive material 15, and the second solid electrolyte 16 is taken as 100. When 30≦v1 is satisfied, it is easy to ensure a sufficient energy density of the battery. When v1≦95 is satisfied, it is easier for the battery to operate at high power.
[0088] The material of the positive electrode current collector 21 is not limited to a specific material, and materials commonly used in batteries can be used. Examples of materials for the positive electrode current collector 21 include aluminum, aluminum alloy, stainless steel, carbon, and conductive resin. The shape of the positive electrode current collector 21 is also not limited to a specific shape. Examples of shapes include foil, film, and sheet. The surface of the positive electrode current collector 21 may be uneven.
[0089] (Embodiment 3) The battery in embodiment 3 includes the positive electrode and negative electrode of embodiment 2. The battery in embodiment 3 may be a solid-state battery or a liquid battery. In this disclosure, a "solid-state battery" refers to a battery that uses a solid electrolyte as the electrolyte. A solid-state battery is typically an all-solid-state battery that does not contain an electrolytic solution. In this disclosure, a "liquid battery" refers to a battery that uses an electrolytic solution. The battery in embodiment 3 can reduce initial resistance and suppress an increase in resistance during repeated charge and discharge.
[0090] 3 is a cross-sectional view showing a schematic configuration of a battery 300 according to Embodiment 3. As shown in FIG. 3, the battery 300 may include the positive electrode 200, the electrolyte layer 201, and the negative electrode 202 according to Embodiment 2. The electrolyte layer 201 is disposed between the positive electrode 200 and the negative electrode 202.
[0091] (Electrolyte Layer) The electrolyte layer 201 is a layer containing an electrolyte. The electrolyte is, for example, a solid electrolyte. The solid electrolyte contained in the electrolyte layer 201 is called a third solid electrolyte. That is, the electrolyte layer 201 may contain the third solid electrolyte.
[0092] The third solid electrolyte may be a halide solid electrolyte, a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, or a complex hydride solid electrolyte. A material that is less likely to decompose at the potential of the negative electrode active material used may be selected from the above materials and used as the third solid electrolyte.
[0093] The third solid electrolyte may include a solid electrolyte having the same composition as the solid electrolyte included in the first solid electrolyte 13 .
[0094] The third solid electrolyte may include a solid electrolyte having the same composition as the solid electrolyte included in the second solid electrolyte 16 .
[0095] The third solid electrolyte may contain a solid electrolyte having a different composition from the solid electrolyte contained in the first solid electrolyte 13 .
[0096] When the third solid electrolyte includes a halide solid electrolyte, the third solid electrolyte may include a halide solid electrolyte having the same composition as the halide solid electrolyte included in the second solid electrolyte 16. In other words, the electrolyte layer 201 may include a halide solid electrolyte having the same composition as the halide solid electrolyte included in the second solid electrolyte 16.
[0097] The third solid electrolyte may include a solid electrolyte having a different composition from the solid electrolyte included in the second solid electrolyte 16 .
[0098] When the third solid electrolyte includes a halide solid electrolyte, the third solid electrolyte may include a halide solid electrolyte having a different composition from the halide solid electrolyte included in the second solid electrolyte 16. In other words, the electrolyte layer 201 may include a halide solid electrolyte having a different composition from the halide solid electrolyte included in the second solid electrolyte 16.
[0099] The third solid electrolyte may include a sulfide solid electrolyte. The third solid electrolyte may include a sulfide solid electrolyte having the same composition as the sulfide solid electrolyte included in the second solid electrolyte 16. That is, the electrolyte layer 201 may include a sulfide solid electrolyte having the same composition as the sulfide solid electrolyte included in the second solid electrolyte 16.
[0100] The above configuration can improve the energy density of the battery 300. Furthermore, when the electrolyte layer 201 contains a sulfide solid electrolyte having the same composition as the sulfide solid electrolyte contained in the first solid electrolyte 13, the initial resistance of the battery 300 can be further reduced.
[0101] The third solid electrolyte may include an oxide solid electrolyte, such as a NASICON-type solid electrolyte material represented by LiTi(PO) and its element substitution products, a (LaLi)TiO-based perovskite-type solid electrolyte material, or a Li 14 ZnGeO 16 , LiSiCON-type solid electrolyte materials such as LiSiO, LiGeO and their elemental substitution products, LiLaZrO 12 Garnet-type solid electrolyte materials, such as LiPO and its element substitution products, LiPO and its N-substituted products, glasses based on Li-B-O compounds such as LiBO and LiBO, and glass ceramics to which LiSO, LiCO, etc. are added, can be used.
[0102] The third solid electrolyte may include a polymer solid electrolyte. Examples of the polymer solid electrolyte include a compound of a polymer compound and a lithium salt. The polymer compound may have an ethylene oxide structure. A polymer compound having an ethylene oxide structure can contain a large amount of lithium salt. This can further increase ionic conductivity. Examples of the lithium salt include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), and LiC(SO2CF3)3. The lithium salt may be used alone or in combination.
[0103] The third solid electrolyte may include a complex hydride solid electrolyte, such as LiBH4-LiI or LiBH4-P2S5.
[0104] (Negative Electrode) The negative electrode 202 includes a negative electrode current collector 23 and a negative electrode active material layer 24 supported by the negative electrode current collector 23. The negative electrode active material layer 24 contains a material capable of absorbing and releasing metal ions (e.g., lithium ions). The negative electrode active material layer 24 contains, for example, a negative electrode active material (e.g., negative electrode active material particles).
[0105] The negative electrode active material may be a metal material, a carbon material, an oxide, a nitride, a tin compound, or a silicon compound. The metal material may be a simple metal. The metal material may be an alloy. Examples of the metal material include lithium metal or a lithium alloy. Examples of the carbon material include natural graphite, spherical carbon, artificial graphite, or amorphous carbon. From the viewpoint of capacity density, silicon, tin, a silicon compound, or a tin compound can be preferably used.
[0106] The anode active material layer 24 may contain a solid electrolyte. The solid electrolyte contained in the anode active material layer 24 is called a fourth solid electrolyte. That is, the anode active material layer 24 may contain the fourth solid electrolyte. With such a configuration, the lithium ion conductivity inside the anode active material layer 24 is improved, enabling the battery 300 to operate at high output. As the fourth solid electrolyte contained in the anode active material layer 24, a material that does not decompose at the potential of the anode active material used can be selected from the materials given as examples of the third solid electrolyte of the electrolyte layer 201.
[0107] The average particle size of the negative electrode active material may be larger than the average particle size of the fourth solid electrolyte contained in the negative electrode active material layer 24. This allows the negative electrode active material and the fourth solid electrolyte to be well dispersed.
[0108] The volume ratio "v2:100-v2" of the negative electrode active material contained in the negative electrode active material layer 24 to the fourth solid electrolyte may satisfy 30≦v2≦95. Here, v2 indicates the volume ratio of the negative electrode active material when the total volume of the negative electrode active material and the fourth solid electrolyte contained in the negative electrode active material layer 24 is taken as 100. When 30≦v2 is satisfied, it is easy to ensure a sufficient energy density of the battery 300. When v2≦95 is satisfied, it is easier for the battery 300 to operate at high power.
[0109] The material of the negative electrode current collector 23 is not limited to a specific material, and materials commonly used in batteries can be used. Examples of materials for the negative electrode current collector 23 include copper, copper alloy, aluminum, aluminum alloy, stainless steel, nickel, and conductive resin. The shape of the negative electrode current collector 23 is also not limited to a specific shape. Examples of shapes include foil, film, and sheet. The surface of the negative electrode current collector 23 may be uneven.
[0110] At least one selected from the group consisting of the positive electrode active material layer 22, the electrolyte layer 201, and the negative electrode active material layer 24 may contain a binder for the purpose of improving adhesion between particles. The binder is used to improve the binding strength of the materials constituting the electrode. Examples of binders that can be used include copolymers of two or more materials selected from the group consisting of polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polymethyl ester of acrylic acid, polyethyl ester of acrylic acid, polyhexyl ester of acrylic acid, polymethacrylic acid, polymethyl ester of methacrylic acid, polyethyl ester of methacrylic acid, polyhexyl ester of methacrylic acid, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene-butadiene rubber, carboxymethyl cellulose, tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene. Alternatively, a mixture of two or more materials selected from these may be used as the binder.
[0111] The negative electrode active material layer 24 may contain a conductive material to enhance electronic conductivity. Examples of the conductive material include graphites such as natural graphite or artificial graphite, carbon blacks such as acetylene black and ketjen black, carbon fiber, and conductive polymer compounds such as polyaniline, polypyrrole, and polythiophene. Using a carbon-based conductive material can reduce costs.
[0112] (Modification) Fig. 4 is a cross-sectional view showing a schematic configuration of a modification of a battery 400. The battery 400 shown in Fig. 4 includes the positive electrode 200, separator 301, and negative electrode 202 of the second embodiment. The battery 400 has the same configuration as the battery 300 described above, except that the battery 400 includes separator 301 instead of electrolyte layer 201.
[0113] The separator 301 is disposed between the positive electrode 200 and the negative electrode 202, and prevents direct contact between the positive electrode 200 and the negative electrode 202. The separator 301 can sufficiently ensure the safety of the battery 400.
[0114] The separator 301 has lithium ion conductivity. There are no particular limitations on the material of the separator 301 as long as it allows lithium ions to pass through.
[0115] Examples of materials for separator 301 include porous materials. Separator 301 may have the shape of a membrane. When separator 301 is a porous membrane, examples of the porous membrane include woven fabric, nonwoven fabric, porous membranes made of polyolefin resin, and porous membranes made of glass paper obtained by weaving glass fibers into nonwoven fabric.
[0116] An electrolyte may be impregnated in separator 301. With the above configuration, battery 400 can achieve both high charge / discharge efficiency and high discharge capacity.
[0117] The electrolyte may contain at least one selected from the group consisting of cyclic ethers, glymes, and sulfolane. The electrolyte may also contain an ether. Examples of the ether include cyclic ethers and glycol ethers. Glycol ethers have the formula CH3(OCH2CH2) n The glyme may be represented by OCH3. In the above composition formula, n is an integer of 1 or more. The electrolyte may contain a mixture of a cyclic ether and a glyme, or a cyclic ether as a solvent.
[0118] Examples of cyclic ethers include tetrahydrofuran (THF), 2-methyltetrahydrofuran (2MeTHF), 2,5-dimethyltetrahydrofuran, 1,3-dioxolane (1,3DO), 4-methyl-1,3-dioxolane (4Me1,3DO), etc. One or a mixture of two or more selected from these can be used.
[0119] Glymes include monoglyme (1,2-dimethoxyethane), diglyme (diethylene glycol dimethyl ether), triglyme (triethylene glycol dimethyl ether), tetraglyme (tetraethylene glycol dimethyl ether), pentaethylene glycol dimethyl ether, polyethylene glycol dimethyl ether, etc. The glyme may be a mixture of tetraglyme and pentaethylene glycol dimethyl ether.
[0120] Sulfolanes include 3-methylsulfolane.
[0121] The electrolyte may contain an electrolyte salt. Examples of the electrolyte salt include lithium salts such as LiPF, LiBF, LiSbF, LiAsF, LiSOCF, LiN(SOCF), LiN(SOCF), LiN(SOCF)(SOCF), LiC(SOCF), LiClO, and lithium bis(oxalate)borate. The electrolyte may contain lithium dissolved therein.
[0122] The battery 300 and the battery 400 can be configured as batteries of various shapes, such as coin type, cylindrical type, square type, sheet type, button type, flat type, and laminate type.
[0123] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.
[0124] (Technology 1) A positive electrode material comprising: a positive electrode active material; a coating material including a first conductive material and a first solid electrolyte, the coating material covering at least a portion of a surface of the positive electrode active material; a second conductive material being a fibrous carbon material; and a second solid electrolyte, wherein the first solid electrolyte includes Li, Ti, M, and F, and the M is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr, and the second conductive material has an average fiber diameter of 0.4 nm or more and 50 nm or less.
[0125] The positive electrode material of Technology 1 can reduce the initial resistance of the battery and also suppress an increase in the resistance of the battery when it is repeatedly charged and discharged.
[0126] (Technology 2) The positive electrode material according to Technology 1, wherein the first conductive material coats at least a portion of the surface of the positive electrode active material, and the first solid electrolyte coats at least a portion of the surface of a base active material including the first conductive material and the positive electrode active material. With this configuration, an increase in the resistance of the battery during repeated charge and discharge is further suppressed.
[0127] (Technology 3) The positive electrode material according to Technology 1 or 2, wherein the second conductive material and the second solid electrolyte are located between particles of a composite active material containing the positive electrode active material and the coating material. With this configuration, the initial resistance of the battery is further reduced, and an increase in the resistance of the battery during repeated charge and discharge is further suppressed.
[0128] (Technology 4) The cathode material according to any one of Technologies 1 to 3, wherein M includes Al. With this configuration, the lithium ion conductivity of the first solid electrolyte is improved, and as a result, the initial resistance of the battery can be reduced.
[0129] (Technology 5) The positive electrode material according to any one of Technologies 1 to 4, wherein a ratio of the mass of the second conductive material to the sum of the mass of the positive electrode active material and the mass of the second conductive material is 0.005% or more and 0.02% or less. With this configuration, uniformity of the electrochemical reaction is easily ensured.
[0130] (Technology 6) The positive electrode material according to any one of Technologies 1 to 5, wherein the second solid electrolyte includes a sulfide solid electrolyte. With this configuration, the initial resistance of the battery can be reduced.
[0131] (Technology 7) The positive electrode material according to any one of Technologies 1 to 6, wherein the first conductive material is a particulate material. With this configuration, the initial resistance of the battery is further reduced, and an increase in the resistance of the battery during repeated charge and discharge is further suppressed.
[0132] (Technology 8) The positive electrode material according to any one of Technologies 1 to 7, wherein the first conductive material has a median diameter of 100 nm or less. With this configuration, in the positive electrode active material layer, an electron conduction path is easily formed by connecting the first conductive material and the second conductive material. As a result, the electron conductivity of the positive electrode active material layer can be improved.
[0133] (Technology 9) The positive electrode material according to any one of Technologies 1 to 8, wherein the positive electrode active material has a particle shape having a plurality of recesses on a surface thereof, and the first conductive material is disposed in the plurality of recesses. With this configuration, the initial resistance of the battery is further reduced, and an increase in the resistance of the battery during repeated charge and discharge is further suppressed.
[0134] (Technology 10) A positive electrode comprising: a positive electrode current collector; and a positive electrode active material layer supported by the positive electrode current collector, wherein the positive electrode active material layer contains the positive electrode material according to any one of Technologies 1 to 9.
[0135] The positive electrode of Technique 10 can reduce the initial resistance of the battery and can suppress an increase in the resistance of the battery when it is repeatedly charged and discharged.
[0136] (Technology 11) A battery comprising: the positive electrode according to Technology 10; and a negative electrode.
[0137] The battery of Technique 11 can reduce the initial resistance and suppress an increase in resistance when charging and discharging are repeated.
[0138] (Technology 12) The battery according to technology 11, further comprising an electrolyte layer located between the positive electrode and the negative electrode.
[0139] The battery of Technique 12 can reduce the initial resistance and suppress an increase in resistance when charging and discharging are repeated.
[0140] Hereinafter, the present disclosure will be described in detail using examples and comparative examples. The following examples are merely illustrative, and the present disclosure is not limited to the following examples.
[0141] Examples 1 to 4 [Positive Electrode Active Material] Core-shell type composite particles (median diameter: 5 μm, density: 4.7 g / cm3 The core-shell composite particles had a core made of Li(Ni, Co, Al)O2 and a shell made of LiNbO3. The median diameter of the positive electrode active material was measured using a laser diffraction measurement device (SALD-2000, manufactured by Shimadzu Corporation).
[0142] [First conductive material] Acetylene black particles (Li-435, manufactured by Denka Co., Ltd., average particle size: 23 nm) were used as the first conductive material. The median diameter of the acetylene black particles measured from an SEM image was 25 nm.
[0143] [First Solid Electrolyte] In a glove box under an argon atmosphere, raw material powders LiF, TiF, and AIF were weighed out so that the molar ratio of LiF:TiF:AIF was 2.7:0.3:0.7. These raw material powders were mixed in an agate mortar to obtain a mixture. Next, the mixture was milled using a planetary ball mill (manufactured by Fritsch, Model P-7) at a rotation speed of 500 rpm for 12 hours or more. As a result, Li 2.7 Ti 0.3 AI 0.7 F6 (hereinafter referred to as LTAF) (average particle size: 10 nm to 100 nm, density: 2.7 g / cm 3 The particles thus obtained were designated as the first solid electrolyte. The average particle size of the first solid electrolyte was determined by calculating the circle-equivalent diameter of 20 particles randomly selected from LTAF particles observed at a magnification of 20,000 times using a scanning electron microscope (Regulus SU8230, manufactured by Hitachi High-Technologies Corporation).
[0144] [First Binder] A solution was prepared by dissolving a styrene-ethylene-butylene-styrene block copolymer polymer (N504, manufactured by Asahi Kasei Corporation) in a dispersion medium as the first binder. The content of the styrene-ethylene-butylene-styrene block copolymer polymer was 5% by mass relative to the total mass of the solution.
[0145] [Second Binder] A solution of a butadiene rubber binder dissolved in a dispersion medium was prepared as the second binder. The content of the butadiene rubber binder was 5% by mass relative to the total mass of the solution.
[0146] [Second Conductive Material] Single-walled carbon nanotubes (TUBALL SWCNT, manufactured by OCSiAl Corporation, fiber diameter: 1.6±0.4 nm, length: 5 μm or more) (hereinafter referred to as CNT) were used as the second conductive material.
[0147] The second conductive material was mixed with the first binder solution and a solvent to prepare a dispersion of the second conductive material. The contents of the CNT and styrene-ethylene-butylene-styrene block copolymer were 0.2% by mass and 0.6% by mass, respectively, relative to the total mass of the dispersion.
[0148] [Second solid electrolyte] As the second solid electrolyte, LiI-LiBr-LiS-P2S5-based glass ceramic particles (average particle size: 1.0 μm, density: 2.2 g / cm 3 The average particle size of the second solid electrolyte was calculated in the same manner as for the first solid electrolyte.
[0149] [First coating step] The positive electrode active material and the first conductive material were mixed in an agate mortar so that the mass ratio of the positive electrode active material to the first conductive material was 99.5:0.5, thereby obtaining particles of the positive electrode active material at least partially coated with the first conductive material, i.e., particles of the base active material.
[0150] [SEM Analysis] Figure 5 shows an example of a secondary electron image of particles of the basic active material of Example 1 taken with a scanning electron microscope (Regulus SU8230, manufactured by Hitachi High-Technologies Corporation). Figure 6 shows an example of a backscattered electron image of particles of the basic active material of Example 1 taken with an SEM in the same observation region as the secondary electron image of Figure 5. The accelerating voltage of the scanning electron microscope was 1 kV.
[0151] A secondary electron image has a characteristic that the surface shape (e.g., unevenness) of the sample is easily reflected in the image contrast. A backscattered electron image has a characteristic that the composition of the sample is easily reflected in the image contrast. In a backscattered electron image, materials with a high atomic number and high density are observed brightly. As shown in FIG. 5, particles with a diameter of approximately 10 nm to 50 nm were particles of acetylene black, which is the first conductive material 12. As shown in FIG. 6, the region of the surface of the positive electrode active material 11 coated with the first conductive material 12 was observed to have a darker color tone than the region of the surface of the positive electrode active material 11 not coated with the first conductive material 12.
[0152] As shown in FIGS. 5 and 6, the positive electrode active material 11 had a plurality of recesses on its surface, and the first conductive material 12 was disposed in the plurality of recesses.
[0153] [Second Coating Step] A mixture was obtained by mixing particles of the base active material and particles of the first solid electrolyte in a container together with a plurality of zirconia balls (diameter: 3 mm) so that the volume ratio of the positive electrode active material to the first solid electrolyte was 90:10. Next, the mixture was mixed using a planetary centrifugal mixer (ARE-310, manufactured by Thinky Corporation) at a rotation speed of 1200 rpm for 6 minutes. This resulted in particles of the base active material, at least a portion of whose surface was coated with the first solid electrolyte, i.e., particles of the composite active material. The obtained composite active material is referred to as composite active material A. The volume ratio of the positive electrode active material to the first solid electrolyte was calculated using the density of the positive electrode active material and the density of the first solid electrolyte.
[0154] [Mixing Step] The composite active material A, the second solid electrolyte, the dispersion medium for CNTs, and the second binder solution were mixed together with a solvent to prepare a positive electrode slurry.
[0155] Positive electrode slurries of Examples 1 to 5 were prepared by varying the content of CNT, which was the second conductive material. Table 1 shows the second solid electrolyte content (volume %), second conductive material content (mass %), and first and second binder contents (mass %) in the positive electrode slurries of Examples 1 to 5. The second solid electrolyte content shown in Table 1 is the ratio of the volume of the second solid electrolyte to the total volume of the positive electrode active material and the second solid electrolyte (100 × second solid electrolyte / (positive electrode active material + second solid electrolyte)). The second conductive material content shown in Table 1 is the ratio of the mass of the second conductive material to the total mass of the positive electrode active material and the second conductive material (100 × second conductive material / (positive electrode active material + second conductive material)). The contents of the first binder and the second binder shown in Table 1 are the ratios of the masses of the first binder and the second binder to the total mass of the positive electrode active material and the first binder and the second binder (100 × first binder and second binder / (positive electrode active material + first binder and second binder)). The same applies to Tables 2 and 3 described below.
[0156] The content of the second solid electrolyte was calculated using the density of the positive electrode active material and the density of the second solid electrolyte. The mass of the second binder was adjusted so that the sum of the mass of the first binder and the mass of the second binder was in the ratio shown in Table 1.
[0157]
[0158] Comparative Examples 1 to 3 [Positive Electrode Active Material] As in Examples 1 to 4, positive electrode active material particles (median diameter: 5 μm, density: 4.7 g / cm 3 ) composed of a plurality of core-shell type composite particles were used as the positive electrode active material. 3 ) was used.
[0159] [First Solid Electrolyte] As in Examples 1 to 4, LTAF particles were used as the first solid electrolyte.
[0160] [First Binder] As in Examples 1 to 4, a solution of a styrene-ethylene-butylene-styrene block copolymer (N504, manufactured by Asahi Kasei Corporation) in a dispersion medium was prepared as the first binder.
[0161] [Second Binder] As the second binder, a solution was prepared by dissolving a butadiene rubber binder in a dispersion medium in the same manner as in Examples 1 to 4.
[0162] [Second conductive material] As the second conductive material, the same CNTs and vapor-grown carbon fibers (VGCF-H, manufactured by Showa Denko K.K., average fiber diameter: 150 nm, average length: 6 μm) (hereinafter referred to as VGCF) as in Examples 1 to 4 were used.
[0163] [Second solid electrolyte] As in Examples 1 to 4, LiI-LiBr-LiS-P2S5-based glass ceramic particles (average particle size: 1.0 μm, density: 2.2 g / cm3) were used as the second solid electrolyte. 3 ) was used.
[0164] [Second Coating Step] In Comparative Examples 1 to 3, the first conductive material was not used, and the first coating step was not performed. Except for using a positive electrode active material instead of the base active material, particles of the positive electrode active material, at least a portion of whose surface was coated with the first solid electrolyte, were obtained in the same manner as in the second coating step of Examples 1 to 4. The obtained coated positive electrode active material is referred to as composite active material B.
[0165] [Mixing step] The composite active material B, the second solid electrolyte, the second conductive material, and the second binder solution were mixed together with a solvent to prepare a positive electrode slurry. In Comparative Example 2, in which CNTs were used as the second conductive material, a dispersion medium for the CNTs was used as the second conductive material, as in the mixing steps of Examples 1 to 4.
[0166] The type and content of the second conductive material were changed to prepare positive electrode slurries for Comparative Examples 1 to 3. Table 2 shows the content (volume %) of the second solid electrolyte, the content (mass %) of the second conductive material, and the contents (mass %) of the first binder and the second binder in the positive electrode slurries of Comparative Examples 1 to 3.
[0167]
[0168] Comparative Examples 4 to 7 As in Examples 1 to 4, composite active material A was used as the composite active material.
[0169] [Second Binder] As the second binder, a solution was prepared by dissolving a butadiene rubber binder in a dispersion medium in the same manner as in Examples 1 to 4.
[0170] [Second Conductive Material] As the second conductive material, acetylene black particles (Li-435, manufactured by Denka Co., Ltd., average particle size: 23 nm) (hereinafter referred to as AB) and the same VGCF as in Comparative Example 3 were used.
[0171] [Second solid electrolyte] As in Examples 1 to 4, LiI-LiBr-LiS-P2S5-based glass ceramic particles (average particle size: 1.0 μm, density: 2.2 g / cm3) were used as the second solid electrolyte. 3 ) was used.
[0172] [Mixing Step] The composite active material A, the second solid electrolyte, the second conductive material, and the second binder solution were mixed together with a solvent to prepare a positive electrode slurry.
[0173] Positive electrode slurries of Comparative Examples 4 to 7 were prepared by varying the type and content of the second conductive material. The contents (volume %) of the second solid electrolyte, the contents (mass %) of the second conductive material, and the contents (mass %) of the second binder in the positive electrode slurries of Comparative Examples 4 to 7 are shown in Table 3. The contents of the second binder shown in Table 3 are the ratio of the mass of the second binder to the total mass of the positive electrode active material and the second binder (100 × second binder / (positive electrode active material + second binder)).
[0174]
[0175] [Evaluation of Electronic Conductivity of Positive Electrode Active Material Layer] The positive electrode slurries of Examples 1 to 4 and Comparative Examples 1 to 7 were applied onto a current collector foil and dried at 100°C to obtain positive electrodes. The positive electrodes were composed of a current collector foil and a positive electrode active material layer formed on the current collector foil. The thickness of the positive electrode active material layer was determined so that the discharge capacity reached 2 mAh / cm in the measurement of the initial battery capacity described below. 2 It was adjusted so that
[0176] Next, two punched positive electrodes were stacked with the positive electrode active material layers facing each other, and roll-pressed at 2 ton / cm to produce a positive electrode molded body. After measuring the thickness of the positive electrode active material layer of the positive electrode molded body, it was housed in an exterior body made of a laminate sheet and restrained at 0.5 MPa. In this way, test pieces of the positive electrodes of Examples 1 to 4 and Comparative Examples 1 to 7 were obtained.
[0177] The test piece was placed in a thermostatic chamber at 25°C. A voltage of 0.05 V was then applied between the two current collector foils of the test piece, and the current was measured after 300 seconds. The electronic conductivity of the positive electrode active material layer was calculated using the following formula (1). The results are shown in Tables 4 to 7. Electronic conductivity = current / (voltage × thickness of positive electrode active material layer) Formula (1)
[0178] [Evaluation of Initial Resistance and Resistance Change Rate] Evaluation cells for Examples 1 to 5 and Comparative Examples 1 to 7 were fabricated by the following method.
[0179] (Preparation of negative electrode) Li4Ti5O was used as the negative electrode active material. 12 Particles (average particle size: 1.1 μm, density: 3.5 g / cm 3 The average diameter of the negative electrode active material was calculated in the same manner as for the positive electrode active material.
[0180] As the solid electrolyte, LiI-LiBr-LiS-P2S5-based glass ceramic particles (average particle size: 1.0 μm, density: 2.2 g / cm3) were used, similar to the second solid electrolyte used in the positive electrode materials of Examples 1 to 5. 3 The average particle size of the solid electrolyte was calculated in the same manner as in the first solid electrolyte of Examples 1 to 4.
[0181] As the binder, a solution was prepared by dissolving a butadiene rubber-based binder in a dispersion medium, similar to the second binder used in the positive electrode materials of Examples 1 to 4. The content of the butadiene rubber-based binder was 5 mass% with respect to the total mass of the solution.
[0182] As the conductive material, VGCF, which is the same as the second conductive material used in the positive electrode materials of Comparative Examples 3, 6, and 7, was used.
[0183] The negative electrode active material, solid electrolyte, binder solution, and conductive material were weighed so that the mass ratio of the negative electrode active material:solid electrolyte:binder solution:conductive material was 73.8:24.8:0.6:0.8, and a dispersion medium was added to and mixed with these to prepare a negative electrode slurry.
[0184] The negative electrode slurry was applied to a current collector foil as a negative electrode current collector and dried at 100°C to obtain a negative electrode. The negative electrode consisted of a current collector foil and a negative electrode active material layer formed on the current collector foil. The thickness of the negative electrode active material layer was adjusted so that the capacity per unit area of the negative electrode was 1.15 times the capacity per unit area of the positive electrode.
[0185] The "capacity per unit area of the negative electrode" refers to the capacity per unit area of the negative electrode when the specific capacity of the negative electrode active material is 175 mAh / g. The "capacity per unit area of the positive electrode" refers to the initial charge capacity in the initial battery capacity measurement described below.
[0186] (Preparation of Electrolyte Layer) As a solid electrolyte, LiI-LiBr-LiS-P2S5-based glass ceramic particles (average particle size: 2.5 μm, density: 2.2 g / cm 3 The average particle size of the solid electrolyte was calculated by the same method as for the first solid electrolyte in Examples 1 to 5. The average particle size of the solid electrolyte used in the electrolyte layer was different from the average particle size of the second solid electrolyte used in the positive electrode material in the Examples and Comparative Examples, and the average particle size of the solid electrolyte used in the negative electrode.
[0187] As the binder, a solution was prepared by dissolving a butadiene rubber-based binder in a dispersion medium, similar to the second binder used in the positive electrode materials of Examples 1 to 4. The content of the butadiene rubber-based binder was 5 mass% with respect to the total mass of the solution.
[0188] The solid electrolyte and the butadiene rubber binder were weighed so that the mass ratio of the solid electrolyte to the butadiene rubber binder was 99.6:0.4, and a dispersion medium was added to and mixed with them to prepare a solid electrolyte slurry.
[0189] (Preparation of Positive Electrode Side Laminate) A solid electrolyte slurry was applied to the surface of the positive electrode active material layer, dried at 100°C, and then applied with a pressure of 2 ton / cm2 The positive electrode side laminate was then subjected to roll pressing at a temperature of 1000° C. to obtain a positive electrode side laminate. The positive electrode side laminate had a positive electrode and a first electrolyte layer formed on the surface of the positive electrode.
[0190] (Preparation of Negative Electrode Side Laminate) The solid electrolyte slurry was applied to the surface of the negative electrode active material layer, dried at 100°C, and then roll-pressed at 2 ton / cm to obtain a negative electrode side laminate. The negative electrode side laminate included a negative electrode and a second electrolyte layer formed on the surface of the negative electrode.
[0191] (Assembly) The positive electrode side laminate and the negative electrode side laminate were each punched. The positive electrode side laminate, the unpressed electrolyte layer (the same as the solid electrolyte layer), and the negative electrode side laminate were stacked in this order to obtain a laminate. In the laminate, the unpressed electrolyte layer was interposed between the first electrolyte layer of the positive electrode side laminate and the second electrolyte layer of the negative electrode side laminate.
[0192] The laminate was pressed at 400 MPa to obtain a power generating element. The power generating element included a positive electrode, an electrolyte layer formed on the positive electrode, and a negative electrode formed on the electrolyte layer. The obtained power generating element was encapsulated in a laminate and constrained at 0.5 MPa. This resulted in a battery used as an evaluation cell.
[0193] (SEM-EDS analysis of positive electrode cross section) The evaluation cell prepared using the positive electrode material of Example 3 was cut, and the cut surface was processed with an ion milling device (ArBlade 5000, manufactured by Hitachi High-Technologies Corporation), after which the cross section of the positive electrode active material layer was subjected to SEM-EDS analysis and SEM analysis. An Ultim Extreme manufactured by Oxford Instruments was used as the EDS detector. The accelerating voltage during SEM-EDS analysis was 5 kV.
[0194] Secondary electron images and element mapping images obtained by EDS of the same location on the cross section of the positive electrode active material layer are shown in Figures 7 to 12. Figure 7 is a secondary electron image, Figure 8 is a mapping of the Ni component (corresponding to the positive electrode active material), Figure 9 is a mapping of the Nb component (corresponding to LiNbO), Figure 10 is a mapping of the C component (corresponding to the first conductive material, second conductive material, first binder, and second binder), Figure 11 is a mapping of the F component (corresponding to the first solid electrolyte), and Figure 12 is a mapping of the S component (corresponding to the second solid electrolyte). In Figures 7 to 12, the light-colored areas indicate the distribution of each component.
[0195] Fig. 13 is a cross-sectional backscattered electron image of the positive electrode active material layer taken at an accelerating voltage of 1 kV, and Fig. 14 is an enlarged view of region A in Fig. 13. The structure of the positive electrode material shown in Fig. 14 was identified from the results of element mapping shown in Figs. 7 to 12 and the color tone appearing in the backscattered electron image.
[0196] 7 to 12, it was found that the first conductive material and the first solid electrolyte were distributed on the surface of the particles of the positive electrode active material consisting of a core made of Li(Ni,Co,Al)O2 and a shell made of LiNbO3. It was also found from Fig. 13 that the second solid electrolyte was present between the positive electrode active materials.
[0197] 13 and 14 , the first conductive material 12 was preferentially disposed inside the recesses on the surface of the positive electrode active material 11. Outside the recesses, there were areas where the first conductive material 12 was not disposed. The first solid electrolyte 13 was disposed in the areas on the surface of the positive electrode active material 11 where the first conductive material 12 was not disposed. Note that the CNT used as the second conductive material 15 had a small fiber diameter and was added in a small amount, so its distribution could not be confirmed in FIGS. 13 and 14 .
[0198] (Measurement of Initial Resistance) First, the evaluation cell was placed in a thermostatic chamber at 25° C. Next, the evaluation cell was charged and then discharged (hereinafter also referred to as a "charge-discharge cycle") twice.
[0199] The evaluation cell was charged at a constant current of 1 / 3 C rate until the voltage of the evaluation cell reached 2.7 V, and then constant voltage charging was performed, which was terminated when the charging current reached the equivalent of 0.01 C. The charging rate was set at the design capacity of the evaluation cell (capacity per unit area of the positive electrode: 2 mAh / cm 2 ) was calculated.
[0200] The evaluation cell was discharged at a constant current of 1 / 3 C rate until the voltage of the evaluation cell reached 1.5 V, and then discharged at a constant voltage, which was terminated when the discharge current reached the equivalent of 0.01 C.
[0201] Next, the evaluation cell was charged at a constant current of 1 / 3 rate until the voltage reached 2.2 V, followed by constant voltage charging, which was terminated when the charging current reached the equivalent of 0.01 C. The evaluation cell was allowed to stand for 1 minute and then discharged for 10 seconds at a 24 C rate. The initial resistance R1 was determined by dividing the voltage drop of the evaluation cell immediately before discharge began and 0.1 seconds after discharge began by the current value. The results are shown in Tables 4 to 7.
[0202] Subsequently, the evaluation cell was discharged at a constant current of 1 / 3 C rate until the voltage reached 1.5 V, and then discharged at a constant voltage, which was terminated when the discharge current reached a value equivalent to 0.01 C.
[0203] (Measurement of Resistance After Cycle Test) A cycle test was carried out by placing the evaluation cell in a thermostatic chamber at 60° C. In the cycle test, charge / discharge cycles were repeated 150 times.
[0204] The evaluation cell was charged at a constant current of 5C until the voltage of the evaluation cell reached 2.7V, and then constant voltage charging was performed, which was terminated when the charging current reached 1 / 3C.
[0205] The current was discharged at a constant current rate of 1C until the voltage of the evaluation cell reached 1.8V.
[0206] Next, the evaluation cell was placed in a thermostatic chamber at 25°C and charged at a constant current of 1 / 3 rate until the evaluation cell voltage reached 2.2 V, followed by constant voltage charging, which was terminated when the charging current reached the equivalent of 0.01 C. The evaluation cell was allowed to stand for 1 minute and then discharged for 10 seconds at a 24 C rate. The voltage drop of the evaluation cell immediately before the start of discharge and 0.1 seconds after the start of discharge was divided by the current value to determine the resistance R2 after the cycle test. The values (R2 / R1) obtained by dividing the resistance R2 after the cycle test by the initial resistance R1 are shown in Tables 4 to 7.
[0207] The content of the second conductive material shown in Tables 4 to 7 is the ratio of the mass of the second conductive material to the total mass of the positive electrode active material and the second conductive material (100 × second conductive material / (positive electrode active material + second conductive material)).
[0208]
[0209] The electronic conductivity of the positive electrode active material layer in Examples 1 and 2 was equivalent to that of the positive electrode active material layer in Comparative Examples 1 and 4 to 7. However, the initial resistance R1 of the evaluation cells in Comparative Examples 1 and 4 to 7 was larger than the initial resistance R1 of the evaluation cells in Examples 1 and 2, being 9.5 Ω cm 2 The results were as above. The initial resistance R1 of the evaluation cell of Comparative Example 1 was higher than the initial resistance R1 of the evaluation cells of Examples 1 and 2. This is presumably because the positive electrode material of Comparative Example 1 did not contain a second conductive material, which prevented uniformity of the electrochemical reaction in the positive electrode active material layer. The initial resistance R1 of the evaluation cells of Comparative Examples 4 to 7 was higher than the initial resistance R1 of the evaluation cells of Examples 1 and 2. This is presumably because the second conductive material contained in the positive electrode materials of Comparative Examples 4 to 7 was not a fibrous carbon material, or because the average diameter or average fiber diameter of the second conductive material was large and the content was high, which narrowed the ion conduction path in the positive electrode active material layer due to the second conductive material, resulting in non-uniformity of the electrochemical reaction.
[0210]
[0211] The content of the second conductive material in the positive electrode material of Example 3 was the same as the content of the second conductive material in the positive electrode material of Comparative Example 2. However, the electronic conductivity of the positive electrode active material layer of Comparative Example 2 was lower than that of Example 3. This is presumably because the positive electrode material of Comparative Example 2 did not contain the first conductive material, which prevented uniformity of the electrochemical reaction in the positive electrode active material layer. Furthermore, the initial resistances R1 and R2 / R1 of the evaluation cell of Comparative Example 2 were both larger than the initial resistances R1 and R2 / R1 of the evaluation cell of Example 3. This is presumably because the positive electrode material of Comparative Example 2 did not contain the first conductive material, which prevented the formation of an electronic conduction path via the first conductive material, preventing uniformity of the electrochemical reaction throughout the positive electrode active material layer.
[0212]
[0213] In the positive electrode material of Comparative Example 3, like the positive electrode material of Comparative Example 2, the coating material coating the positive electrode active material did not contain the first conductive material. As can be seen from a comparison of the electronic conductivity of the positive electrode active material layer of Example 3 and that of Comparative Example 3, when the coating material coating the positive electrode active material did not contain the first conductive material, adding 2.3 mass% of vapor-grown carbon fiber as the second conductive material increased the electronic conductivity of the positive electrode active material layer to a level close to that of Example 3. However, the initial resistances R1 and R2 / R1 of the evaluation cell of Comparative Example 3 were larger than the initial resistances R1 and R2 / R1 of the evaluation cell of Example 3. This is presumably because the content of the second conductive material in the positive electrode material was too high, narrowing the ionic conduction path in the positive electrode active material layer due to the second conductive material, resulting in insufficient uniformity in the electrochemical reaction.
[0214]
[0215] The positive electrode materials of Examples 1 to 4 differed in the content of the second conductive material. As shown in Table 7, the evaluation cells of Examples 1 to 4 had reduced initial resistance R1 and suppressed resistance increases during repeated charge and discharge. Furthermore, as can be seen from a comparison of the electronic conductivities of the positive electrode active material layers of Examples 1 to 4, the evaluation cells of Examples 1 to 3, in which the content of the second conductive material was 0.005% or more and 0.02% or less, had R2 / R1 of 1.5 or less, and the increase in resistance during repeated charge and discharge was further suppressed. This is presumably because the content of the fibrous carbon material in the positive electrode active material layer was not too high, which not only prevented the second solid electrolyte from decomposing during charging of the evaluation cell but also prevented the ion conduction path in the positive electrode active material layer from narrowing.
[0216] As described above, according to the present disclosure, it is possible to provide a positive electrode material that can reduce the initial resistance of a battery and can suppress an increase in the resistance of the battery when it is repeatedly charged and discharged.
[0217] The positive electrode material of the present disclosure is used, for example, in batteries (e.g., all-solid-state lithium-ion secondary batteries).
Claims
1. A positive electrode material comprising: a positive electrode active material; a coating material including a first conductive material and a first solid electrolyte, and coating at least a portion of a surface of the positive electrode active material; a second conductive material which is a fibrous carbon material; and a second solid electrolyte, wherein the first solid electrolyte includes Li, Ti, M, and F, and the M is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr, and the second conductive material has an average fiber diameter of 0.4 nm or more and 50 nm or less.
2. The positive electrode material according to claim 1, wherein the first conductive material covers at least a portion of the surface of the positive electrode active material, and the first solid electrolyte covers at least a portion of the surface of a base active material including the first conductive material and the positive electrode active material.
3. The positive electrode material according to claim 1, wherein the second conductive material and the second solid electrolyte are positioned between particles of a composite active material containing the positive electrode active material and the coating material.
4. The positive electrode material according to claim 1, wherein M comprises Al.
5. The positive electrode material according to claim 1, wherein a ratio of the mass of the second conductive material to the sum of the mass of the positive electrode active material and the mass of the second conductive material is 0.005% or more and 0.02% or less.
6. The positive electrode material according to claim 1, wherein the second solid electrolyte comprises a sulfide solid electrolyte.
7. The positive electrode material of claim 1, wherein the first conductive material is a particulate material.
8. The positive electrode material according to claim 7, wherein the first conductive material has a median diameter of 100 nm or less.
9. The positive electrode material according to claim 1, wherein the positive electrode active material has a particle shape having a plurality of recesses on a surface thereof, and the first conductive material is disposed in the plurality of recesses.
10. A positive electrode comprising: a positive electrode current collector; and a positive electrode active material layer supported by the positive electrode current collector, the positive electrode active material layer comprising the positive electrode material according to any one of claims 1 to 9.
11. A battery comprising: the positive electrode according to claim 10; and a negative electrode.
12. The battery of claim 11, further comprising an electrolyte layer located between said positive electrode and said negative electrode.
Citation Information
Patent Citations
Lithium secondary battery and its manufacturing method
JP2003059492A
Electrode mixture
JP2016207418A
Electrodes for all-solid-state batteries containing solid electrolytes
JP2020507893A
All-solid battery and method of manufacturing the same
JP2023049448A
Electrode body, all-solid cell, and method for manufacturing coated active material
WO2012157046A1
Cited By
Carbon material dispersion, electrode composition, electrode, all-solid battery, and method for manufacturing carbon material dispersion
WO2026116352A1
Coated particles comprising a coating based on an organic compound, method for manufacturing same and use thereof
WO2026161994A1