Electrode catalyst ink for water electrolysis, electrode catalyst, water electrolysis cell, and water electrolysis device
The introduction of a nonionic water-soluble polymer in the electrode catalyst ink for water electrolysis addresses the aggregation issues of solid components, improving dispersibility and stability, resulting in a more efficient and cost-effective electrode catalyst layer formation.
Patent Information
- Application Number
- PCT/JP2024/016614
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-21
AI Technical Summary
The existing electrode catalyst inks for water electrolysis face challenges with aggregation of solid components, leading to nozzle clogging and uneven layer thickness, which affects electrode performance and increases manufacturing costs, due to high apparent particle size of catalysts and carriers, particularly when using transition metal carriers like Ni, resulting in reduced productivity and stability.
Incorporating a nonionic water-soluble polymer, such as polyvinylpyrrolidone, into the electrode catalyst ink to enhance the affinity between the catalyst, carrier, and solvent, preventing aggregation and improving dispersibility, thereby stabilizing the catalyst layer formation and maintaining high activity during water electrolysis.
The addition of a nonionic water-soluble polymer increases the dispersibility of the solid content, reducing variations in catalyst layer thickness and supported amount, enhancing the stability and activity of the electrode catalyst layer, and improving the overall productivity of the manufacturing process.
Smart Images

Figure JP2024016614_21112024_PF_FP_ABST
Abstract
Description
Electrode catalyst ink for water electrolysis, electrode catalyst, water electrolysis cell, and water electrolysis device
[0001] The present disclosure relates to an electrode catalyst ink for water electrolysis, an electrode catalyst, a water electrolysis cell, and a water electrolysis device.
[0002] In recent years, there has been a growing expectation for the development of electrodes for use in water electrolysis devices.
[0003] It has been known that catalyst layers used in water electrolysis are formed using a specific ink. For example, Patent Literature 1 describes a composition for forming a water electrolysis catalyst layer containing a proton reduction catalyst and aqueous resin fine particles. In the composition for forming a water electrolysis catalyst layer, the aqueous resin fine particles are dispersed together with the proton reduction catalyst.
[0004] Japanese Patent Application Laid-Open No. 2017-210637
[0005] The descriptions in the above documents need to be reconsidered from the viewpoint of productivity in producing an electrode catalyst for water electrolysis using the ink. Therefore, the present disclosure provides a novel electrocatalyst ink for water electrolysis that is advantageous from the viewpoint of productivity in producing an electrode catalyst for water electrolysis.
[0006] The present disclosure provides an electrode catalyst ink for water electrolysis, comprising: a catalyst containing one or more transition metals; a support containing a transition metal on which the catalyst is supported; an organic polymer; and a solvent containing water, wherein the organic polymer comprises a water-insoluble polymer and a nonionic water-soluble polymer.
[0007] The present disclosure provides a novel electrocatalytic ink for water electrolysis that is advantageous from the viewpoint of productivity in the production of electrocatalysts for water electrolysis.
[0008] FIG. 1 is a diagram schematically illustrating an electrode catalyst ink for water electrolysis according to a first embodiment. FIG. 2 is a diagram schematically illustrating an example of the crystal structure of a layered double hydroxide (LDH). FIG. 3 is a cross-sectional view schematically illustrating an example of a water electrolysis cell according to a second embodiment. FIG. 4 is a cross-sectional view schematically illustrating an example of a water electrolysis device according to a third embodiment. FIG. 5 is a cross-sectional view schematically illustrating an example of a water electrolysis cell according to a fourth embodiment. FIG. 6 is a cross-sectional view schematically illustrating an example of a water electrolysis device according to a fifth embodiment. FIG. 7 is a graph showing the results of NMR measurement of a sample derived from an electrode catalyst layer.
[0009] (Knowledge forming the basis of the present disclosure) The use of renewable energy such as solar and wind power has been attracting attention as a measure against global warming. In power generation using renewable energy, attention has been focused on improving energy utilization efficiency by utilizing surplus electricity. Therefore, methods for producing and storing hydrogen from surplus electricity have been studied.
[0010] Electrolysis of water is one possible method for producing hydrogen from surplus electricity. To produce hydrogen inexpensively and stably, there is a need for the development of a highly efficient, long-life water electrolysis device. Key components of a water electrolysis device include, for example, a membrane electrode assembly (MEA) equipped with a gas diffusion layer, an electrode catalyst layer, and an electrolyte membrane.
[0011] For example, it is conceivable to prepare an electrode catalyst ink for water electrolysis for the production of an MEA. For example, a mixed solution in which a catalyst and an organic polymer including a water-insoluble polymer are dispersed in a solvent including water can be used as such an ink. For example, when an MEA is produced using the electrode catalyst ink for water electrolysis, the electrode catalyst ink for water electrolysis is applied to a substrate such as an electrolyte membrane or a gas diffusion layer. Examples of methods for applying the electrode catalyst ink for water electrolysis to a substrate include spraying, die coating, slit coating, dipping, and inkjet printing. This results in an electrode catalyst layer containing an electrode catalyst on at least one of the anode and cathode of a water electrolysis device.
[0012] In the water electrolysis electrode catalytic ink, aggregation of solid components such as the catalyst, catalyst support, and water-insoluble polymer increases the apparent particle size of the solid components. This can lead to nozzle clogging in an inkjet device when the water electrolysis electrode catalytic ink is applied to a substrate by an inkjet method, for example. In addition, it becomes difficult to uniformly adjust the film thickness of the electrode catalyst layer. This can result in variations in electrode performance, increased electrode manufacturing costs, and reduced electrode manufacturing productivity. For this reason, it is important to suppress aggregation of solid components such as the catalyst, catalyst support, and water-insoluble polymer in the water electrolysis electrode catalytic ink. In other words, it is important that the water electrolysis electrode catalytic ink is designed so that the components contained in the water electrolysis electrode catalytic ink have appropriate affinity for a solvent containing water.
[0013] An increase in the apparent particle size of solid components such as catalysts, catalyst carriers, and water-insoluble polymers significantly affects the dispersibility of the solid components in an electrode catalyst ink for water electrolysis. The relationship between the particle size of the solid components and the settling velocity can be evaluated, for example, according to the following Stokes' equation (1). In equation (1), v is the settling velocity. ρ S is the density of the solids. W is the density of the solvent. g is the gravitational acceleration. η is the viscosity of the solvent. r is the radius of the solid particle. v = {(ρ S -ρ W ) g / 72η}r 2 Formula (1)
[0014] According to formula (1), an increase in the apparent particle size of the solids contained in the water electrolysis electrode catalytic ink increases the settling rate of the solids. In other words, an increase in the apparent particle size of the solids contained in the water electrolysis electrode catalytic ink reduces the dispersibility of the solids in the water electrolysis electrode catalytic ink. If this dispersibility is insufficient, the amount of catalyst supported on the substrate and the film thickness of the electrode catalyst layer will be unstable when the water electrolysis electrode catalytic ink is applied to the substrate, resulting in a problem of reduced productivity in manufacturing the electrode catalyst layer. A catalyst support containing a transition metal has the advantage of being more resistant to oxidation and therefore more durable than a catalyst support made of a carbon material. On the other hand, a catalyst support containing a transition metal increases the particle size of the solids and reduces the density ρ of the solids compared to a catalyst support made of a carbon material. S Therefore, the settling rate of the solids tends to increase. Therefore, the dispersibility of the solids tends to decrease. For example, the density of a carbon material is 2 g / cm 3 whereas the density of Ni, a transition metal, is about 9 g / cm 3 As a result of extensive research, the present inventors have newly discovered that the dispersibility of solids in an electrode catalyst ink for water electrolysis can be improved by adding an organic polymer containing a nonionic water-soluble polymer to the electrode catalyst ink for water electrolysis. It is believed that the addition of a nonionic water-soluble polymer increases the affinity between the solids, which may include a support containing a transition metal, and the solvent containing water. As a result, the productivity of the production of an electrode catalyst layer is less likely to decrease. For example, when the catalyst support is a carbon material, the settling rate of the solids is low, and therefore the above-mentioned problem is less likely to occur.
[0015] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments. Note that the embodiments described below are all comprehensive or specific examples. Therefore, the numerical values, shapes, materials, components, component placement positions, connection forms, etc. shown in the following embodiments are merely examples and are not intended to limit the present disclosure. Furthermore, among the components in the following embodiments, components that are not recited in the independent claims that represent the highest concepts are described as optional components. Furthermore, the drawings schematically illustrate each component for ease of understanding, and the shapes, dimensional ratios, etc. may not be accurately represented.
[0016] First Embodiment FIG. 1 is a schematic diagram illustrating an electrode catalytic ink for water electrolysis according to a first embodiment. As shown in FIG. 1 , the electrode catalytic ink for water electrolysis 1a contains a catalyst 11, a carrier 15, an organic polymer 12, and a solvent 13. The catalyst 11 contains one or more transition metals. The catalyst 11 is supported on the carrier 15, which contains the transition metals. The solvent 13 contains water. The organic polymer 12 contains a water-insoluble polymer 12b and a nonionic water-soluble polymer 12a. This enhances the affinity between the solvent 13 and the solid components containing the catalyst 11, the carrier 15, and the water-insoluble polymer 12b. In addition, steric hindrance caused by the organic polymer 12 containing the nonionic water-soluble polymer 12a can suppress aggregation of the catalysts 11. As a result, the dispersibility of the solid components in the electrode catalytic ink for water electrolysis 1a is likely to be improved, and productivity in producing an electrode catalyst layer using the electrode catalytic ink for water electrolysis 1a is unlikely to decrease.
[0017] The nonionic water-soluble polymer 12a is present, for example, on at least a portion of the surface of the catalyst 11. The nonionic water-soluble polymer 12a may be present between the catalysts 11. The nonionic water-soluble polymer 12a may be in contact with the catalyst 11, or may cover at least a portion of the surface of the catalyst 11. The type and amount of the nonionic water-soluble polymer 12a contained in the water electrolysis electrode catalytic ink 1a can be determined qualitatively and quantitatively by mass spectrometry (MS) or nuclear magnetic resonance (NMR).
[0018] Because the nonionic water-soluble polymer 12a is water-soluble, it can be eluted and removed from the electrode catalyst layer when water electrolysis is performed using an electrode equipped with the electrode catalyst layer produced using the electrode catalytic ink for water electrolysis 1a, which means that the electrode catalyst layer produced using the electrode catalytic ink for water electrolysis 1a is likely to have high activity.
[0019] The content of the nonionic water-soluble polymer 12a in the solid content of the water electrolysis electrode catalytic ink 1a is not limited to a specific value. The content is, for example, 5 mass% or more. In this case, the nonionic water-soluble polymer 12a is likely to be present in a desired state on the surfaces of the catalysts 11 and between the catalysts 11, and the dispersibility of the solid content in the water electrolysis electrode catalytic ink 1a is likely to be improved.
[0020] The content of the nonionic water-soluble polymer 12a in the solid content of the water electrolysis electrode catalytic ink 1a is preferably 6 mass% or more, more preferably 7.5 mass% or more, and is, for example, 99 mass% or less.
[0021] The nonionic water-soluble polymer 12a is not limited to a specific polymer. The nonionic water-soluble polymer 12a does not have a cationic or anionic functional group. Therefore, it is easy to increase the affinity between the solid content and the solvent 13 while avoiding affecting the electrostatic interaction of the solid content with the catalyst 11.
[0022] The nonionic water-soluble polymer 12a does not have a hydrophobic group such as an alkyl group or a phenyl group, which makes it easier for the nonionic water-soluble polymer 12a to disperse well in the solvent 13 and more likely to exhibit the effect of increasing the affinity between the solid content, including the catalyst 11, the carrier 15, and the organic polymer 12, and the solvent 13.
[0023] The nonionic water-soluble polymer 12a may contain at least one selected from the group consisting of polyvinylpyrrolidone, polyvinyl alcohol, polyethylene oxide, polyacrylamide, and polyethylene glycol, which tends to improve the dispersibility of the solid content in the water electrolysis electrode catalytic ink 1a.
[0024] The catalyst 11 exhibits activity in a gas generation reaction of hydrogen, oxygen, and the like, for example, at the anode or cathode of a water electrolysis cell. The transition metal contained in the catalyst 11 is not limited to a specific transition metal. The transition metal includes, for example, at least one selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, Cu, W, and Ru. In this case, the water electrolysis electrode catalyst ink 1a makes it easy to obtain an electrode catalyst layer exhibiting high activity.
[0025] The transition metal contained in the catalyst 11 may include at least one of Fe and Ni. In this case, an electrode catalyst layer exhibiting high activity is more likely to be obtained using the electrode catalyst ink 1a for water electrolysis.
[0026] The catalyst 11 may be, for example, a hydroxide of a transition metal. In this case, the affinity between the nonionic water-soluble polymer 12a and the catalyst 11 is high, and the dispersibility of the solid content in the water electrolysis electrode catalytic ink 1a is likely to be improved.
[0027] When the catalyst 11 is a hydroxide of a transition metal, the hydroxide may be a layered double hydroxide (LDH). In this case, the affinity between the nonionic water-soluble polymer 12a and the catalyst 11 is high, and the dispersibility of the solid content in the electrode catalyst ink for water electrolysis 1a is likely to be improved. In addition, the electrode catalyst ink for water electrolysis 1a makes it easier to obtain an electrode catalyst layer that exhibits high activity.
[0028] The catalyst 11 may contain, for example, LDH as a main component. In this specification, the main component is the component that is contained in the largest amount by mass. The LDH contains, for example, two or more types of transition metals. The LDH contains, for example, at least two selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, Cu, W, and Ru. The LDH has, for example, a composition represented by the following formula (1). In formula (1), M1 2+is a divalent transition metal ion, and M 3+ is a trivalent transition metal ion, and A n- is an anion between layers. x is a rational number satisfying the condition 0<x<1. y is a number corresponding to the required amount of charge balance. n is an integer, and m is an appropriate rational number. [M1 2+ 1-x M2 3+ x (OH)2][yA n- ・mH2O] Formula (1)
[0029] The LDH contained in the catalyst 11 may contain, for example, Ni and Fe. In this case, M1 is Ni and M2 is Fe in formula (1). In this case, an electrode catalyst layer exhibiting high activity is more likely to be obtained using the electrode catalyst ink 1a for water electrolysis. For example, the electrode catalyst layer is more likely to exhibit high activity than when M1 is Co.
[0030] In the LDH contained in the catalyst 11, the ratio of the amount of Fe to the total amount of Ni and Fe is not limited to a specific value. This ratio may be 0.25 or more and 0.5 or less. In this case, an electrode catalyst layer exhibiting high activity is more likely to be obtained using the electrode catalyst ink 1a for water electrolysis.
[0031] LDH can be composed of primary particles containing one or more minute single-crystal regions and secondary particles formed by aggregation of these. The average particle size of LDH is the value obtained by dividing the area of a two-dimensional distribution diagram by the total number of particles when the relationship between particle size and distribution of particle size distribution obtained by small-angle X-ray scattering (SAXS) is represented on a two-dimensional distribution diagram. The distribution means a value proportional to the total volume occupied by the number of particles of a given particle size. The area of the two-dimensional distribution diagram is, for example, the product of the particle size and the number of particles corresponding to that particle size.
[0032] As described above, in LDH, A n- is an interlayer ion. n- is an inorganic or organic ion. An example of an inorganic ion is CO 2- , NO3 - , Cl - , SO4 2- ,Br - , O.H. - , F- , I - , Si2O5 2- , B4O5(OH)4 2- , and PO 3- An example of an organic ion is CH3(CH2) n SO4 - , CH3 (CH2) n COO - , CH3 (CH2) n PO4 - , and CH3(CH2) n No. 3 - It is. A n- is an anion that is inserted between the layers of the metal hydroxide along with the water molecules. n- The charge and size of the ion are not limited to a specific value. n- or a plurality of types of A n- may also include:
[0033] 2 is a diagram showing a schematic example of the crystal structure of LDH11a represented by composition formula (1). As shown in FIG. 2, LDH11a is a compound having M1 2+ or M2 3+ OH at each vertex of the octahedron centered at - The metal hydroxide has the formula: [(M1) 1-x (M2) x (OH) x+ The metal hydroxide has a layered structure in which hydroxide octahedra are connected two-dimensionally, sharing edges. Anions and water molecules are located between the metal hydroxide layers. The metal hydroxide layers function as host layers 11h, and anions and water molecules are inserted as guest layers. In other words, the LDH 11a as a whole has a sheet-like structure in which host layers 11h of metal hydroxide and guest layers 11g of anions and water molecules are alternately stacked. The LDH 11a is composed of M1 contained in the metal hydroxide layers. 2+ Part of M2 3+ Therefore, the surface of LDH11a is usually positively charged.
[0034] The LDH 11a may contain a chelating agent. In this case, the chelating agent may be coordinated to a transition metal ion in the LDH 11a. This tends to improve the dispersion stability of the catalyst 11 containing the LDH 11a. When the LDH 11a contains a chelating agent, the particle size of the LDH 11a tends to be small. As a result, the surface area of the catalyst 11 containing the LDH 11a tends to be large, and the activity of the electrode catalyst layer obtained using the electrode catalyst ink 1a for water electrolysis tends to be higher. The average particle size of the LDH 11a is not limited to a specific value. The average particle size may be 100 nm or less, 50 nm or less, or 10 nm or less. The average particle size may be 1.5 nm or more, or 2 nm or more.
[0035] The chelating agent contained in LDH 11a is not limited to a specific chelating agent. The chelating agent may be, for example, an organic compound that coordinates with a transition metal in the LDH. The chelating agent may include at least one selected from the group consisting of bidentate organic ligands and tridentate organic ligands. Examples of chelating agents include β-diketones, β-ketoesters, and hydroxycarboxylic acids. Examples of β-diketones include acetylacetone (ACAC), trifluoroacetylacetone, hexafluoroacetylacetone, benzoylacetone, thenoyltrifluoroacetone, dipyrrolylmethane, dibenzoylmethane, and ascorbic acid. Examples of β-ketoesters include methyl acetoacetate, ethyl acetoacetate, allyl acetoacetate, benzyl acetoacetate, n-propyl acetoacetate, isopropyl acetoacetate, n-butyl acetoacetate, isobutyl acetoacetate, tert-butyl acetoacetate, 2-methoxyethyl acetoacetate, and methyl 3-oxopentanoate. Examples of hydroxycarboxylic acids and their salts include tartaric acid, citric acid, malic acid, gluconic acid, ferulic acid, lactic acid, glucuronic acid, and salts thereof. The chelating agent may include at least one selected from the group consisting of acetylacetone and trisodium citrate. The chelating agent may include at least one selected from the group consisting of acetylacetone and trisodium citrate.
[0036] The catalyst 11 is, for example, in the form of particles. The shape of the catalyst 11 is not limited to a specific shape. The shape of the catalyst 11 is, for example, spherical, oval, fibrous, or scale-like.
[0037] As shown in FIG. 1 , the catalyst 11 is supported on a carrier 15. With this configuration, the catalyst 11 is stably disposed on the carrier 15, which tends to further increase the activity of the electrode catalyst layer obtained using the electrode catalytic ink for water electrolysis 1a. The surface of the carrier 15 may be coated with the catalyst 11. The entire surface of the carrier 15 may be coated with the catalyst 11, or only a portion of the surface of the carrier 15 may be coated with the catalyst 11. The catalyst 11 is in contact with the surface of the carrier 15, for example. For example, a coating layer containing the catalyst 11 may be formed on the surface of the carrier 15. The coating layer contains, for example, the catalyst 11 as a main component.
[0038] The material of the support 15 is not limited to a specific material as long as it contains a transition metal and can support the catalyst 11. Examples of transition metals are V, Cr, Mn, Fe, Co, Ni, Cu, W, and Ru. In this case, the activity of the electrode catalyst layer obtained from the water electrolysis electrode catalyst ink 1a is likely to be higher. The support 15 may contain only a single material selected from these materials, or may contain multiple materials. When the support 15 contains multiple transition metals, the support 15 may contain an alloy containing the multiple transition metals. The support 15 may also contain a porous material such as a foam.
[0039] The shape of the support 15 is not limited to a specific shape. The support is, for example, particulate. Examples of the shape of the support 15 include spherical, oval, fibrous, and scale-like shapes. The size of the support 15 is not limited to a specific value. For example, when the support 15 is spherical, the average particle size of the support 15 is not limited to a specific value. The average particle size of the support may be 100 nm or less, 50 nm or less, 20 nm or less, or 10 nm or less. This makes it easy for the support 15 to support a sufficient amount of catalyst 11. Furthermore, with this configuration, the electrode catalyst layer obtained from the water electrolysis electrode catalyst ink 1a is likely to exhibit excellent durability, for example, in the anode reaction of water electrolysis. The average particle size of the support 15 can be determined by observing the support 15 using, for example, a transmission electron microscope (TEM). Specifically, the average particle size can be determined as the arithmetic mean of the particle sizes of any 50 carriers 15 for which the entire carrier 15 can be observed, after determining the average of the maximum and minimum diameters as the particle size of each carrier 15.
[0040] As described above, the organic polymer 12 contains the water-insoluble polymer 12b. This makes it difficult for the water-insoluble polymer 12b to dissolve in water even when the electrode catalyst layer obtained from the water electrolysis electrode catalytic ink 1a comes into contact with water during water electrolysis. This makes it easy to maintain the mechanical strength, shape, and catalytic activity of the electrode catalyst layer. The water-insoluble polymer 12b, for example, disperses the catalyst 11 in the solvent 13. The water-insoluble polymer 12b may be present on the surface of the catalyst 11. The water-insoluble polymer 12b may be present on at least a portion of the surface of the catalyst 11. The water-insoluble polymer 12b may be present between the catalysts 11. The water-insoluble polymer 12b may be in contact with the catalyst 11. At least a portion of the surface of the catalyst 11 may be coated with the water-insoluble polymer 12b. The inclusion of the water-insoluble polymer 12b in the water electrolysis electrode catalytic ink 1a can suppress aggregation of the catalysts 11 due to steric hindrance caused by the water-insoluble polymer 12b. This tends to provide excellent dispersibility for the solid components, including the catalyst 11, the carrier 15, and the water-insoluble polymer 12b, in the water electrolysis electrode catalytic ink 1a. Furthermore, the inclusion of the water-insoluble polymer 12b in the water electrolysis electrode catalytic ink 1a tends to improve the adhesion between the substrate and the electrode catalyst layer when the electrode catalyst ink 1a is used to form the electrode catalyst layer on the substrate. This makes it possible to provide a water electrolysis electrode with excellent durability.
[0041] The water-insoluble polymer 12b is, for example, an organic polymer having ion conductivity. The water-insoluble polymer 12b may have cation conductivity or anion conductivity. The cation conductivity is, for example, proton conductivity. When the water-insoluble polymer 12b has ion conductivity, an electrode catalyst layer exhibiting high activity is more easily obtained using the electrode catalyst ink for water electrolysis 1a.
[0042] The water-insoluble polymer 12b may be, for example, an organic polymer that does not have ion conductivity. In other words, the water-insoluble polymer 12b may be a neutral organic polymer. "Neutral" means that the organic polymer does not contain anion exchange groups or cation exchange groups. In this case, too, aggregation of the catalysts 11 can be suppressed due to steric hindrance caused by the water-insoluble polymer 12b. This makes it easier for the solid content including the catalyst 11, the carrier 15, and the organic polymer 12 to have excellent dispersibility in the water electrolysis electrode catalyst ink 1a. An example of an organic polymer that does not have ion conductivity is polytetrafluoroethylene (PTFE).
[0043] The water-insoluble polymer 12b includes, for example, a fluorine-based polymer. A fluorine-based polymer is an organic polymer containing fluorine atoms. The fluorine-based polymer can function as the water-insoluble polymer 12b. In this case, the thermal stability and electrochemical stability of the water-insoluble polymer 12b are likely to be high. As a result, the mechanical strength and chemical stability of the electrode catalyst layer obtained from the electrode catalyst ink for water electrolysis 1a are likely to be high. In addition, the alkali resistance of the electrode catalyst layer is likely to be high.
[0044] The fluorine-based polymer may be an ion exchange resin containing fluorine, or an organic polymer having fluorine and a sulfonic acid ion group. The organic polymer 12 may contain, for example, a perfluorocarbon polymer or a perfluoroalkylsulfonic acid polymer.
[0045] An example of an organic polymer having fluorine and sulfonic acid ion groups is Nafion (registered trademark). Nafion is an organic polymer with proton conductivity. Nafion has the following chemical formula (I): In formula (I), x and y satisfy 1≦y / x≦9, and n is an integer of 0 or more and 2 or less.
[0046]
[0047] When the organic polymer 12 includes an ion-conductive organic polymer, the equivalent weight (EW) of the ion-conductive organic polymer is not limited to a specific value. The equivalent weight refers to the mass of the organic polymer per mole of anionic functional groups, such as sulfonic acid ion groups. The equivalent weight of the organic polymer may be 1100 g / mol or less or 900 g / mol or less. This more easily suppresses aggregation of the catalyst 11. As a result, in the water electrolysis electrode catalyst ink 1a, the solid content including the catalyst 11, the carrier 15, and the organic polymer 12 is more likely to have excellent dispersibility. The EW of the ion-conductive organic polymer may be 720 g / mol or more or 980 g / mol or more. The EW of the ion-conductive organic polymer is, for example, 720 g / mol or more and 1100 g / mol or less.
[0048] The solvent 13 disperses the catalyst 11 and the organic polymer 12 in the water electrolysis electrode catalytic ink 1a. The water electrolysis electrode catalytic ink 1a can be prepared, for example, by adding a solvent to a dispersion of the catalyst 11 or the organic polymer 12. In this case, the solvent 13 is a mixed solvent of the solvent derived from the dispersion of the catalyst 11 or the organic polymer 12 and the added solvent. The solvent 13 may contain only water, or may contain two or more solvents including water. When the solvent 13 contains multiple types of solvents, the solvents are mutually compatible. It is desirable that the solvents in the solvent 13 are sufficiently compatible with each other and do not undergo phase separation. In the solvent 13, the type and mixing ratio of each solvent are adjusted so that phase separation does not occur, for example, at room temperature.
[0049] As described above, the solvent 13 may include two types of solvents including water, and may include, for example, a first solvent and a second solvent. Each of the first solvent and the second solvent is not limited to a specific solvent. Each of the first solvent and the second solvent is, for example, a polar solvent. It is desirable for the solvent 13 to include water from the viewpoints of raw material costs, disposal costs, and environmental impact. In the solvent 13, the first solvent may be water, and the second solvent may be a solvent having excellent miscibility with water. An example of the second solvent is alcohol. The alcohol may be an aliphatic alcohol. Examples of alcohols are ethanol, 1-propanol, and 2-propanol. The alcohol may include only one alcohol selected from these, or may include multiple types of alcohols.
[0050] The solvent 13 may contain, for example, water and alcohol. This makes it difficult for the organic polymer 12 to aggregate, makes it easy for the nonionic water-soluble polymer 12a to disperse, and makes it easy for the organic polymer 12 to be present on the surface of the catalyst 11 in a state where the catalyst 11 and the organic polymer 12 are adsorbed together. Additionally, in the electrode catalytic ink for water electrolysis 1a, the affinity between the catalyst 11 and the solvent 13 is maintained favorably, making it easy for the catalyst 11 to disperse favorably in the electrode catalytic ink for water electrolysis 1a. Furthermore, in the electrode catalytic ink for water electrolysis 1a, the organic polymer 12 is less likely to detach from the surface of the catalyst 11. As a result, the catalyst 11 and the organic polymer 12 are more likely to have excellent dispersibility in the electrode catalytic ink for water electrolysis 1a.
[0051] The solvent 13 contained in the water electrolysis electrode catalytic ink 1a can be determined qualitatively and quantitatively by, for example, gas chromatography (GC), mass spectrometry (MS), and nuclear magnetic resonance (NMR). If the solvent 13 contained in the water electrolysis electrode catalytic ink 1a is a mixed solvent containing multiple types of solvents, the types of solvents contained in the mixed solvent and the content ratios of each solvent can also be determined by the methods described above.
[0052] In the water electrolysis electrode catalytic ink 1a, for example, a complex 20 is formed by a catalyst 11, a nonionic water-soluble polymer 12a, a water-insoluble polymer 12b, and a carrier 15. This complex 20 can be provided as a catalyst material.
[0053] An electrode catalyst can be provided using the water electrolysis electrode catalytic ink 1a. This electrode catalyst includes a catalyst 11 and an organic polymer 12, which includes a water-insoluble polymer 12b and a nonionic water-soluble polymer 12a. This electrode catalyst can exhibit activity in a reaction to generate gases such as hydrogen and oxygen at the anode or cathode of a water electrolysis cell. This electrode catalyst is, for example, a solidified product of the water electrolysis electrode catalytic ink 1a.
[0054] Second Embodiment Figure 3 is a cross-sectional view schematically illustrating an example of a water electrolysis cell according to a second embodiment. As shown in Figure 3, the water electrolysis cell 2 includes an electrolyte membrane 2p, an anode 2a, and a cathode 2b. The electrolyte membrane 2p is disposed, for example, between the anode 2a and the cathode 2b. At least one selected from the group consisting of the anode 2a and the cathode 2b contains the electrode catalyst described in the first embodiment. This configuration tends to reduce overvoltage in the water electrolysis cell 2.
[0055] The electrolyte membrane 2p may be an ion-conductive electrolyte membrane. The electrolyte membrane 2p is not limited to a specific type. The electrolyte membrane 2p may include an anion exchange membrane. The electrolyte membrane 2p may include a cation exchange membrane.
[0056] The electrolyte membrane 2p is configured to prevent mixing of the oxygen gas generated at the anode 2a and the hydrogen gas generated at the cathode 2b. The anode 2a includes, for example, an electrode catalyst layer 2m. The electrode catalyst layer 2m may be provided on one main surface of the electrolyte membrane 2p. The "main surface" refers to the surface of the electrolyte membrane 2p having the largest area. The electrode catalyst layer 2m may include the electrode catalyst described in the first embodiment. The anode 2a includes, for example, a gas diffusion layer 2n. The gas diffusion layer 2n is a porous and conductive layer and is disposed on the electrode catalyst layer 2m.
[0057] The cathode 2b includes, for example, an electrode catalyst layer 2j. The electrode catalyst layer 2j may be provided on the other main surface of the electrolyte membrane 2p. In other words, the electrode catalyst layer 2j may be provided on the main surface of the electrolyte membrane 2p opposite to the main surface on which the electrode catalyst layer 2m is provided. The electrode catalyst included in the electrode catalyst layer 2j is not limited to a specific catalyst. The electrode catalyst may include a precious metal such as platinum, or may be the electrode catalyst described in the first embodiment. The cathode 2b includes, for example, a gas diffusion layer 2k. The gas diffusion layer 2k is a porous and conductive layer. The gas diffusion layer 2k is disposed on, for example, the electrode catalyst layer 2j.
[0058] Third Embodiment Fig. 4 is a cross-sectional view schematically illustrating an example of a water electrolysis apparatus according to a third embodiment. As shown in Fig. 4, the water electrolysis apparatus 3 includes a water electrolysis cell 2 and a voltage applicator 40. The voltage applicator 40 is connected to the anode 2 a and the cathode 2 b, and applies a voltage between the anode 2 a and the cathode 2 b.
[0059] The voltage applicator 40 increases the potential at the anode 2a and decreases the potential at the cathode 2b. The voltage applicator 40 is not limited to a specific device as long as it can apply a voltage between the anode 2a and the cathode 2b. The voltage applicator 40 may be a device that adjusts the voltage applied between the anode 2a and the cathode 2b. Specifically, when the voltage applicator 40 is connected to a DC power source such as a battery, a solar cell, or a fuel cell, the voltage applicator 40 includes a DC / DC converter. When the voltage applicator 40 is connected to an AC power source such as a commercial power source, the voltage applicator 40 includes an AC / DC converter. The voltage applicator 40 may be a power-type power source that adjusts the voltage applied between the anode 2a and the cathode 2b and the current flowing between the anode 2a and the cathode 2b so that the power supplied to the water electrolysis apparatus 3 is a predetermined set value. With the above configuration, overvoltage in the water electrolysis apparatus 3 is likely to be reduced.
[0060] Fourth Embodiment Figure 5 is a cross-sectional view schematically illustrating an example of a water electrolysis cell according to a fourth embodiment. As shown in Figure 5, the water electrolysis cell 4 includes a diaphragm 4p, an anode 4a, and a cathode 4b. The diaphragm 4p separates a first space 4m from a second space 4n. The anode 4a is provided in the first space 4m. The cathode 4b is provided in the second space 4n. At least one selected from the group consisting of the anode 4a and the cathode 4b contains the electrode catalyst described in the first embodiment. This configuration tends to reduce overvoltage in the water electrolysis cell 4.
[0061] The water electrolysis cell 4 is, for example, an alkaline water electrolysis cell that uses an alkaline aqueous solution. In alkaline water electrolysis, an alkaline aqueous solution is used. Examples of the alkaline aqueous solution include a potassium hydroxide aqueous solution and a sodium hydroxide aqueous solution.
[0062] The water electrolysis cell 4 includes an electrolytic cell 4s. The interior of the electrolytic cell 4s is separated into a first space 4m and a second space 4n by a diaphragm 4p. The anode 4a and the cathode 4b each include, for example, an electrode catalyst layer. These electrode catalyst layers may include, for example, the electrode catalyst described in the first embodiment, or may include a separate electrode catalyst for alkaline water electrolysis.
[0063] The diaphragm 4p is, for example, a diaphragm for alkaline water electrolysis. The anode 4a may be disposed in contact with the diaphragm 4p, or the anode 4a and the diaphragm 4p may be separated. The cathode 4b may be disposed in contact with the diaphragm 4p, or the cathode 4b and the diaphragm 4p may be separated.
[0064] In alkaline water electrolysis, hydrogen gas and oxygen gas are produced by electrolysis of an alkaline aqueous solution. For alkaline water electrolysis, an aqueous solution containing, for example, an alkali metal or alkaline earth metal hydroxide is supplied to the first space 4m of the water electrolysis cell 4. An alkaline aqueous solution may also be supplied to the first space 4m of the water electrolysis cell 4. Electrolysis is performed while an alkaline aqueous solution of a predetermined concentration is discharged from the first space 4m and the second space 4n, producing hydrogen gas and oxygen gas.
[0065] According to the above configuration, at least one of the anode 4a and the cathode 4b contains the electrode catalyst described in the first embodiment, so that the overvoltage in the water electrolysis cell 4 tends to be low.
[0066] Fifth Embodiment Fig. 6 is a cross-sectional view schematically illustrating an example of a water electrolysis apparatus according to a fifth embodiment. As shown in Fig. 6, the water electrolysis apparatus 5 includes a water electrolysis cell 4 and a voltage applicator 40. The voltage applicator 40 is connected to the anode 4a and the cathode 4b, and applies a voltage between the anode 4a and the cathode 4b.
[0067] The water electrolysis device 5 is, for example, an alkaline water electrolysis device that uses an alkaline aqueous solution. The water electrolysis cell 4 has a configuration similar to that of the water electrolysis cell 4 described in the fourth embodiment. With this configuration, the overvoltage in the water electrolysis device 5 is likely to be low.
[0068] (Additional Notes) The above disclosure discloses the following technologies. (Technology 1) An electrode catalyst ink for water electrolysis, comprising: a catalyst containing one or more transition metals; a transition metal-containing support on which the catalyst is supported; an organic polymer; and a solvent, wherein the organic polymer comprises a water-insoluble polymer and a nonionic water-soluble polymer. (Technology 2) The electrode catalyst ink for water electrolysis according to Technology 1, wherein the content of the nonionic water-soluble polymer in the solid content of the electrode catalyst ink for water electrolysis is 5 mass% or more. (Technology 3) The electrode catalyst ink for water electrolysis according to Technology 1 or 2, wherein the nonionic water-soluble polymer does not have a hydrophobic group. (Technology 4) The electrode catalyst ink for water electrolysis according to any one of Technologies 1 to 3, wherein the nonionic water-soluble polymer comprises at least one selected from the group consisting of polyvinylpyrrolidone, polyvinyl alcohol, polyethylene oxide, polyacrylamide, and polyethylene glycol. (Technology 5) The electrode catalyst ink for water electrolysis according to any one of Technologies 1 to 4, wherein the transition metal contained in the catalyst includes at least one of V, Cr, Mn, Fe, Co, Ni, Cu, W, and Ru. (Technology 6) The electrode catalyst ink for water electrolysis according to Technology 5, wherein the transition metal contained in the catalyst includes at least one of Fe and Ni. (Technology 7) The electrode catalyst ink for water electrolysis according to any one of Technologies 1 to 6, wherein the catalyst is a hydroxide of the transition metal. (Technology 8) The electrode catalyst ink for water electrolysis according to Technology 7, wherein the hydroxide is a layered double hydroxide. (Technology 9) The electrode catalyst ink for water electrolysis according to any one of Technologies 1 to 8, wherein the water-insoluble polymer includes a fluorine-based polymer. (Technology 10) The electrode catalyst ink for water electrolysis according to Technology 9, wherein the fluorine-based polymer includes a perfluoroalkylsulfonic acid-based polymer. (Technology 11) An electrode catalyst comprising: a catalyst containing one or more transition metals; a support containing the transition metal on which the catalyst is supported; and an organic polymer, wherein the organic polymer comprises a water-insoluble polymer and a nonionic water-soluble polymer.(Technology 12) A water electrolysis cell comprising an anode, a cathode, and an electrolyte membrane disposed between the anode and the cathode, wherein at least one of the anode and the cathode contains the electrode catalyst described in Technology 11. (Technology 13) The water electrolysis cell according to Technology 12, wherein the electrolyte membrane contains an anion exchange membrane. (Technology 14) The water electrolysis cell according to Technology 12, wherein the electrolyte membrane contains a cation exchange membrane. (Technology 15) A water electrolysis cell comprising a diaphragm separating a first space and a second space, an anode provided in the first space, and a cathode provided in the second space, wherein at least one of the anode and the cathode contains the electrode catalyst described in Technology 11. (Technology 16) A water electrolysis device comprising the water electrolysis cell according to any one of Technology 12 to 15, and a voltage applicator connected to the anode and the cathode and applying a voltage between the anode and the cathode.
[0069] The present disclosure will be described in more detail below with reference to examples. Note that the following examples are examples of the present disclosure, and the present disclosure is not limited to the following examples.
[0070] Example 1: Ni-Fe LDH, an LDH containing Ni and Fe as transition metals, was prepared as follows. A mixed solvent of water and ethanol was prepared. The ethanol used was a special-grade reagent from Fujifilm Wako Pure Chemical Industries, Ltd. The volume ratio of water to ethanol in the mixed solvent was 2:3, expressed as the volume of water:volume of ethanol. Nickel chloride hexahydrate from Fujifilm Wako Pure Chemical Industries, Ltd. and iron chloride hexahydrate from Fujifilm Wako Pure Chemical Industries, Ltd. were dissolved in the mixed solvent to obtain a solution. In this solution, the total concentration of Ni ions and Fe ions was 1.0 mol / L, and the ratio of the mass of Fe ions to the total mass of Ni ions and Fe ions was 0.33. Acetylacetone (ACAC) was added as a chelating agent to the mixed solvent in an amount equivalent to one-third the mass of Ni ions and Fe ions. The resulting solution was stirred for 30 minutes.
[0071] Next, Ni particles were added to the solution as a carrier, with a mass equal to the mass of Ni-Fe LDH that would be produced if all of the Ni and Fe contained in the solution were ideally reacted. The Ni particles were manufactured by US Research Nanomaterials, Inc. and had a particle size of 20 nm. Next, propylene oxide (POX) was added to the solution containing the Ni-Fe LDH and Ni particles as a pH-raising agent in an amount twice the amount of chloride ions in the solution. The resulting solution was stirred for 1 minute. During this time, the POX gradually captured hydrogen ions in the solution, causing the pH of the solution to gradually increase. The resulting solution was allowed to stand for approximately 3 days, after which the target sample, a mixture containing Ni-Fe LDH and Ni particles, was recovered.
[0072] 6.0 g of a mixture containing Ni-Fe LDH and Ni particles and 0.33 g of polyvinylpyrrolidone (product number: 161-03105) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. were placed in a sample tube, and a premixed solvent of 12.8 mL of ethanol and 13.8 mL of water was added. Ultrasonic treatment was then performed for 30 minutes using a tabletop ultrasonic cleaner (product number: W-113MK) manufactured by Honda Electronics Co., Ltd. The mixture was then stirred for 30 minutes using a high-speed mixer (product number: T 18 digital ULTRA-TURRAX) manufactured by IKA Japan Co., Ltd. 4.41 mL of 20% Nafion dispersion solution (product number: 322-86733) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was then added, and the mixture was stirred again for 30 minutes using the high-speed mixer to obtain the ink of Example 1. The polyvinylpyrrolidone content of the solids in the ink of Example 1 was 5% by mass.
[0073] The ink according to Example 1 was loaded into an ultrasonic spray coating system (product name: Exacta-Coat FC) manufactured by Sonotek, and applied to an anion exchange membrane (QPAF-4) manufactured by Takahata Precision Japan, to form an electrode catalyst layer. The shape of the electrode catalyst layer was square in plan view, and the area of the electrode catalyst layer was 25 cm. 2 It was.
[0074] Example 2 An ink was prepared in the same manner as in Example 1, except for the following points: 0.5 g of polyvinylpyrrolidone was added to the ink, and the content of polyvinylpyrrolidone in the solid content of the ink was 7.5% by mass.
[0075] Example 3 An ink was prepared using the same procedure as in Example 2, except for the following points: The amount of ethanol added in the ink preparation was adjusted to 8.98 mL, and the amount of water was adjusted to 9.98 mL. The polyvinylpyrrolidone content of the ink solids was 7.5 mass %.
[0076] Example 4 An ink was prepared in the same manner as in Example 1, except for the following points: 0.69 g of polyvinylpyrrolidone was added to the ink, and the content of polyvinylpyrrolidone in the solid content of the ink was 10% by mass.
[0077] Comparative Example 1 An ink was prepared in the same manner as in Example 1, except that polyvinylpyrrolidone was not used, and an electrode catalyst layer was formed in the same manner as in Example 1 using the ink.
[0078] [Evaluation of Ink Dispersion Stability] 1.0 mL of ink processed using a high-speed stirrer was dispensed and placed in a glass sample tube and allowed to stand. Settling was determined to have occurred when transparent areas were observed in the ink. The time from the start of leaving the ink in the sample tube until settling was determined was measured, and dispersion stability was evaluated. The results are shown in Table 1.
[0079] [Evaluation of variation in catalyst material loading amount] The amount of LDH contained in the electrode catalyst layer was calculated from the weight of the anion exchange membrane before and after application of ink. The maximum, average, and minimum values of the LDH amount contained in five consecutively formed electrode catalyst layers were calculated. The variation in the loading amount was calculated from the calculated maximum, average, and minimum values of the LDH amount based on the following formula (2). The results are shown in Table 1. Loading amount variation [%] = {(maximum value - minimum value) / average value} × 100 / 2 Formula (2)
[0080] [Evaluation of Variation in Catalyst Material Film Thickness] Using a Mitutoyo Corporation Digimatic Indicator (product number: ID-C150XB), the film thickness of the anion exchange membrane without an electrode catalyst layer was measured, and the film thickness of the anion exchange membrane with an electrode catalyst layer was measured. The film thickness of the electrode catalyst layer was calculated by subtracting the film thickness of the anion exchange membrane alone. The film thickness was measured at five arbitrary points on the surface on which the electrode catalyst layer was formed, and the average value of these measurements was taken as the film thickness of the electrode catalyst layer. The maximum, average, and minimum film thicknesses of five consecutively formed electrode catalyst layers were calculated. The film thickness variation was calculated from the calculated maximum, average, and minimum film thickness values using the following formula (3). The results are shown in Table 1. Film Thickness Variation [%] = {(Maximum - Minimum) / Average} × 100 / 2 Formula (3)
[0081] [Viscosity Measurement] The viscosity of each ink was measured using a cone-plate viscometer (product number DV2TLVCJ0) manufactured by Brookfield Co. The results are shown in Table 1.
[0082] [NMR Measurement] The presence of polyvinylpyrrolidone in the electrode catalyst layer was confirmed by NMR measurement. 185 mg of powder obtained by scraping off the electrode catalyst layer formed by the method described in Example 2 was immersed in 0.62 g of heavy water (ISOTEC 151882-100G) for one day. The powder immersed in heavy water was then subjected to ultrasonic treatment at 28 kHz using an AS ONE VS-100III triple-frequency ultrasonic cleaner, and the resulting extract was used as the measurement sample. NMR measurement of the measurement sample was performed using a Bruker AVANCE NEO700 carbon NMR measurement device. In this NMR measurement, polyvinylpyrrolidone powder was used as the reference sample. A 5 mm CryoProbe was used as the probe. The resonant frequency was adjusted to 175 MHz (13C). This measurement was performed using 25,000 measurements. The results are shown in Figure 7. In Figure 7, A indicates the amount of the measurement sample derived from the electrode catalyst layer. 13 C NMR spectrum of the reference sample. 13 C NMR spectrum is shown.
[0083] As shown in Table 1, it was suggested that the inks according to each Example had higher dispersion stability than the ink according to Comparative Example 1. Furthermore, the inks according to each Example had smaller variations in the amount of support and film thickness than the ink according to Comparative Example 1. It is believed that the inclusion of polyvinylpyrrolidone, a nonionic water-soluble polymer, increased the dispersion stability of the solid content in the ink containing Ni particles as a carrier, thereby reducing variations in the amount of support and film thickness. Furthermore, the viscosity of the inks according to each Example was higher than that of the ink according to Comparative Example 1. It is understood that in the inks according to the Examples, polyvinylpyrrolidone increases the affinity between the Ni-Fe LDH and Nafion and the solvent, promoting the dispersion of the solid content in the solvent. As shown in Figure 7, the viscosity of the inks according to A and B 13 In the C NMR spectrum, peaks attributable to polyvinylpyrrolidone were confirmed at 17 to 20 ppm, 31 to 35 ppm, and 42 to 46 ppm, confirming that polyvinylpyrrolidone was contained in the electrode catalyst layer.
[0084]
[0085] The water electrolysis electrode of the present disclosure can be used as an anode or a cathode for water electrolysis.
Claims
1. An electrode catalyst ink for water electrolysis comprising: a catalyst containing one or more transition metals; a support containing a transition metal on which the catalyst is supported; an organic polymer; and a solvent containing water, wherein the organic polymer comprises a water-insoluble polymer and a non-ionic water-soluble polymer.
2. The electrode catalyst ink for water electrolysis according to claim 1, wherein the content of the nonionic water-soluble polymer in the solid content of the electrode catalyst ink for water electrolysis is 5 mass % or more.
3. The electrode catalyst ink for water electrolysis according to claim 1 or 2, wherein the nonionic water-soluble polymer has no hydrophobic group.
4. The electrode catalyst ink for water electrolysis according to any one of claims 1 to 3, wherein the nonionic water-soluble polymer comprises at least one selected from the group consisting of polyvinylpyrrolidone, polyvinyl alcohol, polyethylene oxide, polyacrylamide, and polyethylene glycol.
5. The electrode catalyst ink for water electrolysis according to any one of claims 1 to 4, wherein the transition metal contained in the catalyst includes at least one of V, Cr, Mn, Fe, Co, Ni, Cu, W, and Ru.
6. The electrode catalyst ink for water electrolysis according to claim 5, wherein the transition metal contained in the catalyst includes at least one of Fe and Ni.
7. The electrode catalyst ink for water electrolysis according to any one of claims 1 to 6, wherein the catalyst is a hydroxide of the transition metal.
8. The electrode catalyst ink for water electrolysis according to claim 7, wherein the hydroxide is a layered double hydroxide.
9. The electrode catalyst ink for water electrolysis according to any one of claims 1 to 8, wherein the water-insoluble polymer includes a fluorine-based polymer.
10. The electrode catalyst ink for water electrolysis according to claim 9, wherein the fluorine-based polymer includes a perfluoroalkylsulfonic acid-based polymer.
11. An electrocatalyst comprising: a catalyst containing one or more transition metals; a support containing a transition metal on which the catalyst is supported; and an organic polymer, the organic polymer comprising a water-insoluble polymer and a non-ionic water-soluble polymer.
12. A water electrolysis cell comprising: an anode; a cathode; and an electrolyte membrane disposed between said anode and said cathode, wherein at least one of said anode and said cathode comprises the electrode catalyst according to claim 11.
13. The water electrolysis cell of claim 12, wherein the electrolyte membrane comprises an anion exchange membrane.
14. The water electrolysis cell of claim 12, wherein the electrolyte membrane comprises a cation exchange membrane.
15. A water electrolysis cell comprising: a partition separating a first space and a second space; an anode provided in the first space; and a cathode provided in the second space, wherein at least one of the anode and the cathode contains the electrode catalyst according to claim 11.
16. A water electrolysis device comprising: the water electrolysis cell according to any one of claims 12 to 15; and a voltage applicator connected to the anode and the cathode and applying a voltage between the anode and the cathode.
Citation Information
Patent Citations
Composition for forming catalyst layer to be used for water electrolysis device, catalyst layer and water electrolysis device
JP2017210637A
Membrane electrode assembly and preparation method
CN113517449A
Cathode
JP1979010279A
Hydrogen generating electrode
JP2002317289A
Catalyst coating and process for production thereof
JP2014159027A
Cited By
Catalyst ink, membrane-catalyst layer assembly, and cell stack
WO2026186218A1