High-viscosity antibacterial bio-based waterborne polyurethane emulsion as well as preparation method and application thereof

CN119060286APending Publication Date: 2024-12-03QUZHOU RES INST OF ZHEJIANG UNIV

Patent Information

Application Number
CN202411005925.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-12-03

Smart Images

  • Figure CN119060286A_ABST
    Figure CN119060286A_ABST
Patent Text Reader

Abstract

The invention discloses a high-viscosity antibacterial bio-based waterborne polyurethane emulsion as well as a preparation method and application thereof. The preparation method comprises the following steps: carrying out prepolymerization reaction on diisocyanate, bio-based polyol and a catalyst in an organic solvent to obtain a prepolymer; sequentially adding a bio-based alcohol chain extender and a cationic amine chain extender for reaction, then adding a phenolic acid neutralizer for neutralization salifying reaction, and shearing and emulsifying to obtain a bio-based waterborne polyurethane emulsion; the phenolic acid neutralizer is prepared from one or more of gallic acid, caffeic acid, dihydrocaffeic acid, 3, 4-dihydroxy-L-phenylalanine, tannic acid and chlorogenic acid. According to the method, bio-based polyol is used as a raw material, a prepolymer is subjected to chain extension through bio-based alcohol and an amine chain extender, and the polyurethane emulsion obtained after neutralization through a phenolic acid compound has high binding power, excellent mechanical performance and a lasting antibacterial function.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterborne polyurethane, and in particular to a high-viscosity antibacterial bio-based waterborne polyurethane emulsion and a preparation method and application thereof. Background Art

[0002] Polyurethane is characterized by containing many repeated carbamate groups on the macromolecular chain. The performance can be adjusted in a wide range by changing the structure and molecular weight of the compound. Waterborne polyurethane coatings are widely used as artificial leather finishing agents because of their high film-forming properties, high gloss, high wear resistance, high elasticity, and the finished leather feels plump and comfortable. Artificial leather is a leather substitute made of synthetic materials. Its main component is usually polyvinyl chloride (PVC), which is widely used in the production of clothing, shoes, furniture, car interior decoration, bags and other products. During the use of the above products, they are easily interfered by bacteria and microorganisms, endangering people's lives and health. At present, general antibacterial waterborne polyurethane emulsions are achieved by adding antibacterial agents, but in actual use, the antibacterial properties of the added antibacterial agents are not durable. Waterborne polyurethane emulsions with intrinsic antibacterial function have received more and more attention. On the other hand, due to the smooth surface and low initial adhesion of polymer materials such as PVC and PET, the bonding strength of waterborne polyurethane with them is usually poor. The resin coating is easily peeled off during use, thus affecting the service life.

[0003] With the massive consumption of fossil resources, as well as the increasingly serious energy crisis and environmental pollution problems, the need for sustainable development and long-term strategic planning has prompted humans to develop and utilize bio-based materials. CN112300386A discloses a chitosan-modified guanidine salt polymer, which can be chemically bonded to the main chain structure of waterborne polyurethane by the amino functional group in the chitosan-type guanidine salt antibacterial agent structure and the isocyanate group in the waterborne polyurethane to form a urea group, thereby ensuring that the antibacterial agent will not be freed from the coating system, thereby ensuring the long-term and continuous antibacterial effect.

[0004] CN115626973A discloses a bio-based antibacterial water-based polyurethane dispersion. During the reaction process, diphenolic acid is used as a bio-based hydrophilic chain extender and citric acid is used as an antibacterial end-capping agent. After being added, antibacterial groups are formed on the molecular chain of the polyurethane product, thereby obtaining an intrinsic antibacterial resin, which can achieve a very excellent antibacterial effect without the need for an external antibacterial agent.

[0005] CN115386290A discloses an antibacterial polyurethane coating and a preparation method thereof. The antibacterial efficiency and antibacterial breadth of the coating are further improved by using a composite of organic and inorganic antibacterial agents. The low eutectic formed by modifying castor oil with [DHmin][NTF2] greatly reduces the viscosity of castor oil and avoids the use of low molecular weight solvents. CN110218440A discloses a preparation method for a UV-curable castor oil-based antibacterial waterborne polyurethane emulsion. Through UV curing technology, polylysine modified with glycidyl methacrylate is combined with castor oil-based waterborne polyurethane to improve the antibacterial properties of waterborne polyurethane.

[0006] However, although the antibacterial waterborne polyurethane resins reported above have antibacterial properties and are prepared by using bio-based compounds to partially replace petroleum-based raw materials, the bio-based content is usually low. In addition, the problem of weak adhesion between antibacterial waterborne polyurethane emulsions and PVC and PET polymer substrates has not been effectively solved.

[0007] Therefore, the synthesis of waterborne polyurethane emulsions with high adhesion, antibacterial function and high bio-based content has broad application prospects. The use of these green renewable materials can greatly promote the sustainability of resin synthesis, and high adhesion can further broaden its application in waterborne adhesives, coatings and inks. Summary of the invention

[0008] Aiming at the problem that waterborne polyurethane cannot have high adhesion, antibacterial property and high bio-based content at the same time, the present invention provides a method for preparing a high-viscosity antibacterial bio-based waterborne polyurethane emulsion. The method uses bio-based polyol as a raw material, and the prepolymer is chain extended by bio-based alcohol and an amine chain extender. The polyurethane emulsion obtained after neutralization with a phenolic acid compound has high adhesion, excellent mechanical properties and lasting antibacterial function at the same time.

[0009] To achieve the above object, the technical solution adopted by the present invention is:

[0010] A method for preparing a highly viscous antibacterial bio-based waterborne polyurethane emulsion comprises the following steps:

[0011] Step 1, prepolymerizing diisocyanate, bio-based polyol and a catalyst in an organic solvent to obtain a prepolymer;

[0012] Step 2, adding a bio-based alcohol chain extender and a cationic amine chain extender to the reaction system of step 1 in sequence to react to obtain a solution of a bio-based waterborne polyurethane resin;

[0013] Step 3, cooling the reaction system of step 2 to below 40° C., adding a phenolic acid neutralizer to carry out a neutralization and salt-forming reaction, and then adding water for shear emulsification, and removing the organic solvent to obtain the bio-based waterborne polyurethane emulsion;

[0014] The phenolic acid neutralizer includes one or more of gallic acid, caffeic acid, dihydrocaffeic acid, 3,4-dihydroxy-L-phenylalanine, tannic acid, and chlorogenic acid.

[0015] In the present invention, firstly, bio-based polyols are used as raw materials to replace traditional petroleum-based polyols to react with diisocyanates to obtain prepolymers, and then bio-based alcohol compounds and cationic amine chain extenders are used to extend the chains. Finally, phenolic acid structure bio-based compounds are selected for neutralization and salt formation reaction, and water is added for self-emulsification to obtain an antibacterial bio-based waterborne polyurethane emulsion with high adhesion. Amine chain extenders can provide good antibacterial effects, and the catechol groups in the neutralizers can form cationic π interactions between molecular chains, optimize dense molecular cross-linking networks and physical interaction forces, and help dissipate energy under external forces. The benzene ring structure can also improve the rigidity of the molecular chain, and can provide excellent adhesion and mechanical properties for polyurethane resins. At the same time, the inherent antibacterial function can further improve the antibacterial effect of the polyurethane emulsion, and the antibacterial effect of the emulsion can be greatly improved under synergistic effects, and the long-term antibacterial performance can be maintained.

[0016] The diisocyanate includes one or more of L-lysine diisocyanate, toluene diisocyanate, phenylene diisocyanate, xylene diisocyanate, tetramethylxylene diisocyanate, isophorone diisocyanate, naphthalene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate or dicyclohexylmethane diisocyanate; the amount of the diisocyanate is 15% to 35% of the mass of the bio-based waterborne polyurethane resin. Preferably, the diisocyanate is L-lysine diisocyanate, which is a bio-based material and can increase the bio-based content of the system.

[0017] The bio-based polyol includes one or more of hydroxylated epoxidized soybean oil, hydroxylated linseed oil, hydroxylated sunflower seed oil, hydroxylated cottonseed oil, hydroxylated rapeseed oil or castor oil; the amount thereof accounts for 40% to 55% of the mass of the bio-based waterborne polyurethane resin. All of the above are bio-based polyol vegetable oils, and the bio-based alcohol chain extender and phenolic acid neutralizer are all bio-based raw materials, and the bio-based content in the obtained polyurethane can be as high as more than 90%.

[0018] Preferably, the bio-based polyol is castor oil. Ricin contained in castor oil is a natural antibacterial substance that has an inhibitory effect on various types of microorganisms such as bacteria, molds and yeasts.

[0019] The bio-based alcohol chain extender includes one or more of 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,2-pentanol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,3-hexanediol, 1,4-hexanediol, 1,5-hexanediol, and 1,6-hexanediol; and the amount used is 5% to 10% of the mass of the bio-based waterborne polyurethane resin.

[0020] Preferably, the bio-based alcohol chain extender is 1,3-propylene glycol and 1,4-butanediol. Short-chain polyols with hydroxyl groups at both ends as chain extenders can effectively avoid gelation during the polymerization process, and the polymerization effect is better.

[0021] The cationic amine chain extender includes one or more of 3-dimethylamino-1,2-propylene glycol, N-methyldiethanolamine, diethanolamine, triethanolamine, N-ethyldiethanolamine, N-propyldiethanolamine, and tert-butyldiethanolamine; and its usage accounts for 6% to 12% of the mass of the bio-based waterborne polyurethane resin.

[0022] Preferably, the cationic amine chain extender is diethanolamine or triethanolamine, and the prepared polyurethane emulsion has a smaller particle size and better storage stability.

[0023] Preferably, the phenolic acid neutralizer is caffeic acid and / or gallic acid. The final emulsion obtained by using these two neutralizers has stronger adhesion. It is further preferred that the phenolic acid neutralizer is gallic acid, which has a structure of pyrogallol and has stronger and better adhesion.

[0024] The amount of the phenolic acid neutralizer added accounts for 7% to 13% of the mass of the bio-based waterborne polyurethane resin.

[0025] In step 1, the reaction temperature of the system is 70-90° C., the reaction time is 2-3 hours, and the reaction can be carried out in an air atmosphere. The catalyst is one or more of dibutyltin dilaurate, stannous octoate, and stannous oleate, and the added amount accounts for 0.1% to 0.5% of the mass of the bio-based waterborne polyurethane resin.

[0026] In the percentage of the raw material addition amount mentioned above to the mass percentage of the bio-based waterborne polyurethane resin, the bio-based waterborne polyurethane resin is calculated based on the ideal theoretical value of the synthesized bio-based waterborne polyurethane resin.

[0027] After adding the bio-based alcohol chain extender in step 2, the reaction is carried out at 70-90° C. for 2-3 hours; after adding the cationic amine chain extender in step 2, the reaction is carried out at 65-80° C. for 2-3 hours; within the above temperature and time range, the isocyanate group and the hydroxyl group can fully react under the action of the catalyst.

[0028] The reaction temperature of step 3 is 25-40° C. and the reaction time is 0.5-1 hour. Within the above temperature and time range, the salt-forming reaction can be ensured to proceed more fully, which is beneficial to the preparation of the aqueous emulsion.

[0029] The water added during emulsification was calculated based on a final emulsion solid content of 35%.

[0030] The present invention also provides a high-viscosity antibacterial bio-based waterborne polyurethane emulsion prepared according to the preparation method.

[0031] The antibacterial bio-based water-based polyurethane emulsion of the present invention has high adhesion, excellent and lasting antibacterial performance, strong adhesion to PVC and PET polymer base materials, high bio-based content, and is in line with the sustainable development strategy. It is expected to be used in coatings, adhesives, fabric coatings and finishing agents, leather finishing agents, paper surface treatment agents or fiber surface treatment agents and other fields, and is of great significance to the development of the industry.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The quaternary ammonium salt structure brought by the cationic amine chain extender in the present invention, the antibacterial property of the neutralizer, and the tertiary ammonium structure on the polyurethane side chain work together to provide the polyurethane emulsion with excellent wash resistance and long-lasting antibacterial property.

[0034] (2) In the present invention, a bio-based phenolic acid compound containing a catechol structure is selected as a neutralizer, which can provide abundant hydrogen bonding reaction sites and form a compact molecular network structure inside the polyurethane resin, giving it a super strong adhesion function similar to that of mussels and excellent mechanical properties.

[0035] (3) The present invention uses bio-based polyol vegetable oil, diol chain extender and phenolic acid structure neutralizer as synthetic raw materials to replace the petrochemical materials used in the preparation process of traditional water-based polyurethane emulsions, which can reduce the use of petrochemical resources. The bio-based content can be as high as 90% or more, which is in line with the development concept of green chemistry and has the advantage of being environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Infrared spectrum of the polyurethane synthesized in Example 1.

[0037] Figure 2 Infrared spectrum of the polyurethane synthesized in Example 2. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0039] The raw materials used in the following specific embodiments are all purchased from the market.

[0040] Example 1

[0041] Step 1, adding 666.6 g of isophorone diisocyanate, 933.4 g of castor oil and 11 mL of dibutyltin dilaurate catalyst into a reactor, and then adding 2000 mL of acetone to adjust the viscosity to prevent the reaction system from being too large, and reacting at 80° C. for 3 hours under air atmosphere to obtain a prepolymer;

[0042] Step 2, adding 135.1 g of 1,4-butanediol to the reaction system of step 1, and performing a chain extension reaction at 80° C. for 2 hours;

[0043] Step 3, after lowering the reaction temperature to 65° C., 178.6 mL of N-methyldiethanolamine cationic amine chain extender was added to the reaction step 2, and the reaction was continued for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0044] Step 4: After the reaction in step 3 is completed, the temperature is lowered to 30°C, 270g of caffeic acid is dissolved in 250mL of anhydrous ethanol, and the mixture is added to a reaction bottle for neutralization and salt formation reaction for 0.5 hours. Deionized water is added for shear emulsification for 0.5 hours according to the solid content of the emulsion of 35%. The organic solvent is removed by vacuum distillation to obtain an antibacterial bio-based waterborne polyurethane emulsion with high adhesion.

[0045] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0046] Figure 1 The infrared spectrum of the synthesized polyurethane resin is shown in Figure 1. -1 、1730cm -1 、2854cm -1 and 3403cm -1 The absorption peaks at 2250-2270cm correspond to the stretching vibrations of COC, C=O, -CH2 and -OH, respectively. -1 There is no peak in the range, which proves that the free -NCO groups in the polyurethane structure are exhausted and the polymerization reaction is successful.

[0047] Example 2

[0048] Step 1, adding 888.8 g of isophorone diisocyanate, 1244.5 g of castor oil and 13 mL of dibutyltin dilaurate catalyst into a reactor, and then adding 2800 mL of butanone to adjust the viscosity to prevent the reaction system from being too large, and reacting at 80° C. in an air atmosphere for 2.5 hours to obtain a prepolymer;

[0049] Step 2, adding 148.2 mL of 1,3-propylene glycol to the reaction system of step 1, and performing a chain extension reaction at 80° C. for 2.5 hours;

[0050] Step 3, after lowering the reaction temperature to 65° C., add 232 mL of 3-dimethylamino-1,2-propylene glycol cationic amine chain extender to the reaction step 2, and continue the reaction for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0051] Step 4: After the reaction in step 3 is completed, the temperature is lowered to 30°C, 331.5 g of gallic acid is dissolved in 500 mL of anhydrous ethanol, and the mixture is added to the reaction bottle for neutralization and salt formation reaction for 1 hour. Deionized water is added for shear emulsification for 0.5 hour according to the solid content of the emulsion of 35%. The organic solvent is removed by vacuum distillation to obtain an antibacterial bio-based waterborne polyurethane emulsion with high adhesion.

[0052] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0053] Figure 2 The infrared spectrum of the synthesized polyurethane resin is shown in Figure 2. -1 It is the methylene stretching vibration absorption peak at 2850cm -1 The stretching vibration absorption peak of the CH bond in the methylene group is at 1460 cm -1 In the infrared spectrum of PU, 3370cm -1 The peaks on the left and right are the absorption peaks of -NH in polyurethane, at 2260 cm -1 The characteristic absorption peak of -NCO did not appear, indicating that -NCO has completely participated in the reaction.

[0054] Example 3

[0055] Step 1, 696.4 g of 2,4-toluene diisocyanate, 1231.1 g of hydroxylated epoxy soybean oil and 8 mL of dibutyltin dilaurate catalyst were added to a reactor, and 2000 mL of butanone was added to adjust the viscosity to prevent the reaction system from being too large, and the reaction was carried out at 80° C. in an air atmosphere for 2.5 hours to obtain a prepolymer;

[0056] Step 2, adding 180.2 mL of 1,4-butanediol to the reaction system of step 1, and performing a chain extension reaction at 80° C. for 2.5 hours;

[0057] Step 3, after lowering the reaction temperature to 65° C., 298.2 mL of triethanolamine cationic amine chain extender was added to the reaction step 2, and the reaction was continued for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0058] Step 4: After the reaction in step 3 is completed, the temperature is lowered to 30°C, 360.2 g of caffeic acid is dissolved in 350 mL of water, and the mixture is added to a reaction bottle for neutralization and salt formation reaction for 1 hour. Deionized water is added for shear emulsification for 0.5 hour according to the solid content of the emulsion of 35%. The organic solvent is removed by vacuum distillation to obtain an antibacterial bio-based waterborne polyurethane emulsion with high adhesion.

[0059] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0060] Example 4

[0061] Step 1, 336.2 g of hexamethylene diisocyanate, 627 g of hydroxylated linseed oil and 5 mL of dibutyltin dilaurate catalyst were added to a reactor, and 1000 mL of acetone was added to adjust the viscosity to prevent the reaction system from being too large, and the reaction was carried out at 80° C. for 2 hours under air atmosphere to obtain a prepolymer;

[0062] Step 2, adding 90.1 mL of 1,4-butanediol to the reaction system of step 1, and performing a chain extension reaction at 80° C. for 2 hours;

[0063] Step 3, after lowering the reaction temperature to 65° C., 149.2 mL of triethanolamine cationic amine chain extender was added to the reaction step 2, and the reaction was continued for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0064] Step 4: After the reaction in step 3 is completed, the temperature is lowered to 25°C, 182.1 g of dihydrocaffeic acid is dissolved in 300 mL of anhydrous ethanol, and the mixture is added to a reaction bottle for neutralization and salt formation reaction for 1 hour. Deionized water is added for shear emulsification for 0.5 hour according to the emulsion solid content of 35%. The organic solvent is removed by vacuum distillation to obtain an antibacterial bio-based waterborne polyurethane emulsion with high adhesion.

[0065] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0066] Example 5

[0067] Step 1, 678.9 g of L-lysine diisocyanate, 933.4 g of castor oil and 10 mL of dibutyltin dilaurate catalyst were added to a reactor, and 2000 mL of acetone was added to adjust the viscosity to prevent the reaction system from being too large, and the reaction was carried out at 80° C. for 2 hours under air atmosphere to obtain a prepolymer;

[0068] Step 2, adding 156.1 mL of 1,5-pentanediol to the reaction system of step 1, and performing a chain extension reaction at 80° C. for 2 hours;

[0069] Step 3, after lowering the reaction temperature to 65° C., 220.8 mL of N-propyldiethanolamine cationic amine chain extender was added to the reaction step 2, and the reaction was continued for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0070] Step 4. After the reaction in step 3 is completed, the temperature is lowered to 25°C, 531.4 g of chlorogenic acid is dissolved in 900 mL of anhydrous ethanol, and the solution is added to the reaction bottle for neutralization and salt formation reaction for 1 hour. According to the solid content of the emulsion of 35%, deionized water is added for shear emulsification for 0.5 hour, and the organic solvent is removed by vacuum distillation to obtain an antibacterial bio-based waterborne polyurethane emulsion with high adhesion.

[0071] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0072] Example 6

[0073] Step 1, 678.9 g of L-lysine diisocyanate, 933.4 g of castor oil and 9 mL of dibutyltin dilaurate catalyst were added to a reactor, and 2000 mL of acetone was added to adjust the viscosity to prevent the reaction system from being too large, and the reaction was carried out at 80° C. for 2 hours under air atmosphere to obtain a prepolymer;

[0074] Step 2, adding 156.1 mL of 1,5-pentanediol to the reaction system of step 1, and performing a chain extension reaction at 80° C. for 2 hours;

[0075] Step 3, after lowering the reaction temperature to 65° C., 220.8 mL of N-propyldiethanolamine cationic amine chain extender was added to the reaction step 2, and the reaction was continued for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0076] Step 4: After the reaction in step 3 is completed, the temperature is lowered to 25°C, 255.1 g of gallic acid is dissolved in 400 mL of anhydrous ethanol, and the mixture is added to the reaction bottle for neutralization and salt formation reaction for 1 hour. Deionized water is added for shear emulsification for 0.5 hour according to the solid content of the emulsion of 35%. The organic solvent is removed by distillation under reduced pressure to obtain an antibacterial bio-based waterborne polyurethane emulsion with high adhesion.

[0077] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0078] Comparative Example 1

[0079] Step 1, adding 666.6 g of isophorone diisocyanate, 933.4 g of castor oil and 9 mL of dibutyltin dilaurate catalyst into a reactor, and then adding 2000 mL of acetone to adjust the viscosity, and reacting at 80° C. for 3 hours under air atmosphere to obtain a prepolymer;

[0080] Step 2, adding 135.1 mL of 1,4-butanediol to the reaction system of step 1, and performing a chain extension reaction at 80° C. for 2 hours;

[0081] Step 3, after lowering the reaction temperature to 65° C., 178.6 mL of N-methyldiethanolamine cationic amine chain extender was added to the reaction step 2, and the reaction was continued for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0082] Step 4: After the reaction in step 3 is completed, the temperature is lowered to 30°C, 90 mL of glacial acetic acid is dripped into the reaction bottle for neutralization and salt formation reaction for 0.5 hours, deionized water is added according to the emulsion solid content of 35% for shear emulsification for 0.5 hours, and the organic solvent is removed by vacuum distillation to obtain an antibacterial bio-based waterborne polyurethane emulsion.

[0083] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0084] Comparative Example 2

[0085] Step 1, adding 696.4 g of 2,4-toluene diisocyanate, 1263.4 g of hydroxylated epoxy soybean oil and 10 mL of dibutyltin dilaurate catalyst into a reactor, then adding 2500 mL of acetone to adjust the viscosity, and reacting at 85° C. for 3 hours under air atmosphere to obtain a prepolymer;

[0086] Step 2, adding 180.2 mL of 1,4-butanediol to the reaction system of step 1, and performing a chain extension reaction at 85° C. for 2 hours;

[0087] Step 3, after lowering the reaction temperature to 65° C., 210.2 mL of diethanolamine cationic amine chain extender was added to the reaction step 2, and the reaction was continued for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0088] Step 4: After the reaction in step 3 is completed, the temperature is lowered to 25°C, 152 mL of glycolic acid is dripped into the reaction bottle for neutralization and salt formation reaction for 1 hour, deionized water is added according to the emulsion solid content of 35% for shear emulsification for 1 hour, and the organic solvent is removed by vacuum distillation to obtain an antibacterial bio-based waterborne polyurethane emulsion.

[0089] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0090] Comparative Example 3

[0091] Step 1, adding 666.6 g of isophorone diisocyanate, 933.4 g of castor oil and 8 mL of dibutyltin dilaurate catalyst into a reactor, and then adding 2000 mL of acetone to adjust the viscosity to prevent the reaction system, reacting at 80° C. under air atmosphere for 3 hours to obtain a prepolymer;

[0092] Step 2, adding 114.1 mL of 1,3-propylene glycol to the reaction system of step 1, and performing a chain extension reaction at 80° C. for 2 hours;

[0093] Step 3, after lowering the reaction temperature to 65° C., 223.8 mL of triethanolamine cationic amine chain extender was added to the reaction step 2, and the reaction was continued for 2 hours to obtain a bio-based waterborne polyurethane resin;

[0094] Step 4: After the reaction in step 3 is completed, the temperature is lowered to 30°C, 90 mL of glacial acetic acid is dripped into the reaction bottle for neutralization and salt formation reaction for 0.5 hours, deionized water is added according to the solid content of the emulsion of 35% for shear emulsification for 0.5 hours, and the organic solvent is removed by vacuum distillation to obtain an antibacterial bio-based waterborne polyurethane emulsion.

[0095] Step 5, take 50 mL of the polyurethane emulsion prepared above, apply it on the surface of the polypropylene sheet, and leave it naturally at room temperature until all the water evaporates to obtain a coating with a film thickness of about 50 microns.

[0096] The antibacterial properties and tensile properties of the waterborne polyurethane films prepared in the examples and comparative examples were tested in accordance with GB / T 21866-2008 and GB / T19250-2013, respectively. The degree of peeling of the coating from the substrate was evaluated by a peeling test in accordance with GB / T9286-1998. The particle sizes of the polyurethane emulsions prepared in the examples and comparative examples were tested using a nanoparticle size analyzer, and the results are shown in Table 1.

[0097] Table 1 Performance parameters of different polyurethane emulsions

[0098]

[0099] As can be seen from Table 1, in Comparative Examples 1-3, no neutralizer containing a phenolic acid structure was used, and the antibacterial performance of the product was not ideal, and the mechanical properties and adhesion were significantly reduced. In Examples 1-6, the polyurethane emulsions prepared using bio-based phenolic acids such as caffeic acid and gallic acid as neutralizers have significant antibacterial properties and better adhesion. The biobased content in Examples 5 and 6 is greater than 90%, which is much higher than the biobased content in the currently reported high-viscosity antibacterial water-based polyurethane emulsions. As can be seen from Table 2, the polyurethane resins synthesized in Examples 1-6 have better uniformity of molecular chain length and a narrower molecular weight distribution, and therefore have better tensile properties than the comparative examples.

[0100] Table 2 Molecular weight and molecular weight distribution of different polyurethane resins

[0101]

[0102]

Claims

1. A method for preparing a highly viscous antibacterial bio-based waterborne polyurethane emulsion, characterized in that: Includes steps: Step 1, prepolymerizing diisocyanate, bio-based polyol and a catalyst in an organic solvent to obtain a prepolymer; Step 2, adding a bio-based alcohol chain extender and a cationic amine chain extender to the reaction system of step 1 in sequence to react and obtain a solution of a bio-based waterborne polyurethane resin; Step 3, cooling the reaction system of step 2 to below 40° C., adding a phenolic acid neutralizer to carry out a neutralization and salt-forming reaction, and then adding water for shear emulsification, and removing the organic solvent to obtain the bio-based waterborne polyurethane emulsion; The phenolic acid neutralizer includes one or more of gallic acid, caffeic acid, dihydrocaffeic acid, 3,4-dihydroxy-L-phenylalanine, tannic acid, and chlorogenic acid.

2. The method for preparing the highly viscous antibacterial bio-based aqueous polyurethane emulsion according to claim 1, characterized in that: The diisocyanate includes one or more of L-lysine diisocyanate, toluene diisocyanate, phenylene diisocyanate, xylene diisocyanate, tetramethylxylene diisocyanate, isophorone diisocyanate, naphthalene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate or dicyclohexylmethane diisocyanate; the amount of the diisocyanate is 15% to 35% of the mass of the bio-based waterborne polyurethane resin.

3. The method for preparing the highly viscous antibacterial bio-based aqueous polyurethane emulsion according to claim 1, characterized in that: The bio-based polyol includes one or more of hydroxylated epoxidized soybean oil, hydroxylated linseed oil, hydroxylated sunflower seed oil, hydroxylated cottonseed oil, hydroxylated rapeseed oil or castor oil; and the amount of the bio-based polyol accounts for 40% to 55% of the mass of the bio-based waterborne polyurethane resin.

4. The method for preparing the highly viscous antibacterial bio-based aqueous polyurethane emulsion according to claim 1, characterized in that: The bio-based alcohol chain extender includes one or more of 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,2-pentanol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,3-hexanediol, 1,4-hexanediol, 1,5-hexanediol, and 1,6-hexanediol; and the amount used is 5% to 10% of the mass of the bio-based waterborne polyurethane resin.

5. The method for preparing the highly viscous antibacterial bio-based aqueous polyurethane emulsion according to claim 1, characterized in that: The cationic amine chain extender includes one or more of 3-dimethylamino-1,2-propylene glycol, N-methyldiethanolamine, diethanolamine, triethanolamine, N-ethyldiethanolamine, N-propyldiethanolamine, and tert-butyldiethanolamine; and its usage accounts for 6% to 12% of the mass of the bio-based waterborne polyurethane resin.

6. The method for preparing the highly viscous antibacterial bio-based aqueous polyurethane emulsion according to claim 1, characterized in that: In step 1, the reaction temperature of the system is 70-90° C., the reaction time is 2-3 hours, and the reaction can be carried out in an air atmosphere. The catalyst is one or more of dibutyltin dilaurate, stannous octoate, and stannous oleate, and the added amount accounts for 0.1% to 0.5% of the mass of the bio-based waterborne polyurethane resin.

7. The method for preparing the highly viscous antibacterial bio-based aqueous polyurethane emulsion according to claim 1, characterized in that: The amount of the phenolic acid neutralizer added accounts for 7% to 13% of the mass of the bio-based waterborne polyurethane resin.

8. The method for preparing the highly viscous antibacterial bio-based aqueous polyurethane emulsion according to claim 1, characterized in that: After adding the bio-based alcohol chain extender in step 2, the reaction is carried out at 70-90° C. for 2-3 hours; after adding the cationic amine chain extender in step 2, the reaction is carried out at 65-80° C. for 2-3 hours; The reaction temperature of step 3 is 25-40° C., and the reaction time is 0.5-1 hour.

9. A highly viscous antibacterial bio-based waterborne polyurethane emulsion prepared according to the preparation method according to any one of claims 1 to 8.

10. Use of the bio-based waterborne polyurethane emulsion according to claim 9 as a coating, an adhesive, a fabric coating and finishing agent, a leather finishing agent, a paper surface treatment agent or a fiber surface treatment agent.

Citation Information

Patent Citations

  • Preparation method of tannic acid modified waterborne polyurethane

    CN107840939A

  • Preparation method of self-antibacterial castor oil based aqueous polyurethane emulsion

    CN110760046A

  • Bio-based antibacterial waterborne polyurethane dispersion as well as preparation method and application thereof

    CN115626973A

  • Cationic vegetable oil-based waterborne polyurethane ink binder and preparation method thereof

    CN117417501A

Cited By

  • Full-degradable ultraviolet barrier film material as well as preparation method and application thereof

    CN119661796A

  • Waterborne polyurethane emulsion and synthetic leather pressure change base

    CN119661807A

  • Antibacterial, self-toughening, self-healing and recoverable vegetable oil-based waterborne polyurethane as well as preparation method and application thereof

    CN119955053A

  • Antibacterial, self-toughening, self-healing, recyclable vegetable oil-based waterborne polyurethane and its preparation method and application

    CN119955053B

  • Photo-thermal antibacterial, self-enhanced and self-healing vegetable oil-based waterborne polyurethane as well as preparation method and application thereof