Inorganic coated sand and method for producing same, casting mould, and method for improving storage stability of inorganic coated sand
By controlling the cation exchange capacity and applying metasilicate layers on inorganic coated sand, the storage stability and environmental footprint are improved, addressing the wetness issues and energy consumption concerns in traditional inorganic binder processes.
Patent Information
- Application Number
- PCT/JP2024/017151
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-08
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-21
AI Technical Summary
Inorganic coated sand used in casting processes becomes wet during storage, leading to instability and environmental concerns due to high-energy roasting processes required for stabilization, which increases CO2 emissions and energy consumption.
Applying a specific cation exchange capacity (CEC) range of 3 mmol(+)/kg to 40 mmol(+)/kg to foundry sand by forming a metasilicate hydrate layer on recycled or refractory aggregates, using a first coating layer of aluminosilicate and a second metasilicate layer, to prevent moisture absorption and enhance storage stability without the need for high-temperature roasting.
The method improves the storage stability of inorganic coated sand, reduces environmental impact by minimizing energy consumption and emissions, and maintains the sand's dry state for effective mold formation, while maintaining mold quality and strength.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Inorganic coated sand, its manufacturing method, casting mold, and method for improving storage stability of inorganic coated sand
[0001] The present invention relates to inorganic coated sand, a method for producing the same, a casting mold, and a method for improving the storage stability of inorganic coated sand.
[0002] In recent years, the importance of product design that takes people and the environment into consideration has been increasing from the perspective of the Sustainable Development Goals (SDGs). 2 Technological development of environmentally friendly casting processes that reduce emissions and VOCs is accelerating. Known examples of environmentally friendly casting processes include a wet sand inorganic binder process that uses refractory aggregate and an inorganic binder made of liquid water glass. For example, the process described in Patent Document 1 (JP-A-2010-519042) can be cited.
[0003] Patent Document 2 (JP 2021-536367 A) describes that by mixing recycled sand with particulate amorphous oxides containing silicon dioxide to obtain a mixture, and then heat-treating the mixture at a temperature of 400°C or higher, the usable time can be improved, the surface quality of the casting can be improved, and significant energy savings can be achieved.
[0004] Patent Document 3 (JP 2014-117740 A) describes a method for producing dry coated sand having room temperature fluidity, in which a specific water glass aqueous solution is mixed with heated refractory aggregate as a binder, and the water is evaporated to form a coating layer of binder on the surface of the refractory aggregate.
[0005] JP 2010-519042 A JP 2021-536367 A JP 2014-117740 A
[0006] After casting, the coated sand used in the molds is usually crushed (disassembled) to produce single particles of recovered sand, which is then recycled by various methods. From the standpoints of economy and waste reduction, it has become essential for foundries to manufacture molds using recycled sand.
[0007] The present inventors have found that when inorganic-coated sand is produced by forming a metasilicate hydrate layer on foundry sand made from recycled sand produced by a conventional inorganic binder process using an inorganic binder as described in Patent Documents 2 and 3, the sand quickly becomes wet during storage, making it impossible to mold the desired mold. Furthermore, when inorganic-coated sand is produced by forming a metasilicate hydrate layer using a refractory aggregate with a relatively high degree of amorphization, the sand also tends to become wet during storage.
[0008] A conventional regeneration method for inorganic binder processes is roasting regeneration, as described in Patent Document 1. However, it is not possible to sufficiently suppress the formation of wet materials, and high-temperature treatment at 600 to 800°C is required, which leads to energy consumption and CO emissions. 2 There are also problems in terms of waste disposal. Patent Document 1 also relates to an inorganic binder process for wet sand that uses an inorganic binder made of liquid water glass. In other words, the object of the present invention is to prevent inorganic-coated sand made using recycled sand or the like from becoming wet during storage, and to reduce the environmental impact when using the same to produce foundry sand for inorganic-coated sand.
[0009] Therefore, the present inventors have developed a method for producing recycled sand or SiO 2 The inventors have found that applying a coating layer to refractory aggregate containing the above-mentioned compound and adjusting the cation exchange capacity (CEC) of the foundry sand to a specific value is effective in solving the above problems, and have completed the present invention.
[0010] According to the present invention, there is provided a dry inorganic coated sand comprising foundry sand in which a first coating layer is disposed on the surface of one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), and a second coating layer containing metasilicate on the first coating layer of the foundry sand, wherein the refractory aggregate (B) is a SiO 2 and a cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.
[0011] The present invention also provides a casting mold made from the above inorganic coated sand.
[0012] According to the present invention, the method comprises the steps of: (1) mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with aluminate or aluminum hydroxide to form a first coating layer on the surface of the aggregate to obtain foundry sand; (2) mixing the foundry sand obtained with a molten liquid of metasilicate hydrate to obtain a mixture; and (3) cooling the mixture to a temperature below the melting point of the metasilicate hydrate, wherein the refractory aggregate (B) is SiO 2 A method for producing inorganic coated sand is provided, which includes:
[0013] According to the present invention, the method comprises: a step (4) of mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with aluminate or aluminum hydroxide to form a first coating layer on the surface of the aggregate to obtain foundry sand; and a step (5) of mixing the obtained foundry sand with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate, wherein the refractory aggregate (B) is SiO 2 A method for producing inorganic coated sand is provided, which includes:
[0014] According to the present invention, there is also provided a method for improving the storage stability of inorganic coated sand, which comprises foundry sand containing one or two aggregates selected from recycled sand (A) and refractory aggregate (B), and a second coating layer containing metasilicate that coats the foundry sand, wherein the refractory aggregate (B) is SiO 2 and preparing the dry inorganic-coated sand so that the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.
[0015] According to the present invention, the environmental load during the production of foundry sand for inorganic-coated sand can be reduced, while the storage stability of inorganic-coated sand can be improved.
[0016] Hereinafter, embodiments of the present invention will be described. Furthermore, in this specification, "A to B" indicating a numerical range represents a range from A to B, unless otherwise specified. Furthermore, the components and elements described in each embodiment can be combined as appropriate as long as the effects of the invention are not impaired.
[0017] Furthermore, the "coating" and "coating layer" are not limited to being continuous, and may have discontinuous portions.
[0018] <Inorganic Coated Sand> The inorganic coated sand of this embodiment is dry inorganic coated sand comprising foundry sand including one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), a first coating layer covering the aggregate and positioned on the surface, and a second coating layer containing metasilicate on the first coating layer of the foundry sand. 2 The cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.
[0019] That is, in the inorganic coated sand of this embodiment, when inorganic coated sand is produced using one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), the storage stability of the inorganic coated sand using one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B) can be improved by laminating a first coating layer and a second coating layer containing silicate in this order on the surface of the aggregate and by controlling the cation exchange capacity (CEC) of the foundry sand.
[0020] Although the details of the reason for this are not clear, it is presumed as follows: (i) Residues of inorganic binders once used in casting may adhere to the surface of the recycled sand (A). When inorganic-coated sand is produced by coating the surface of recycled sand (A) having residues of inorganic binders with metasilicate hydrate, components in the residues react with the metasilicate hydrate, causing the metasilicate hydrate crystals to melt and the inorganic-coated sand to become wet. (ii) On the other hand, SiO 2In the case where inorganic coated sand is produced by coating the surface of the refractory aggregate (B) containing silicate hydrate, the SiO 2 Since the components may react with silicate hydrate, the silicate hydrate crystals may melt, causing the inorganic coated sand to become wet. (iii) Therefore, by forming the first coating layer to cover the surface of the recycled sand (A) or the refractory aggregate (B) and using foundry sand with a specific CEC, it is possible to suppress the reaction with the residue, and even if a second coating layer containing metasilicate is then laminated, it is possible to suppress the melting of the metasilicate hydrate in the second coating layer, which is presumably capable of suppressing the inorganic coated sand from becoming wet and improving its storage stability.
[0021] Furthermore, when the first coating layer that coats the surface of the recycled sand (A) or the refractory aggregate (B) is formed from an aluminosilicate-containing material, it can be formed at a relatively low temperature. Therefore, the roasting step at 600 to 800°C that was required in the conventional inorganic binder regeneration process can be omitted, and the consumption of thermal energy and CO 2 This reduces emissions and reduces the burden on the environment.
[0022] The inorganic coated sand of this embodiment will be described in more detail below.
[0023] The inorganic coated sand is in a dry state. Dry coated sand means coated sand for which a measured value can be obtained when measuring the dynamic angle of repose regardless of the moisture content. The dynamic angle of repose is preferably 80° or less, more preferably 45° or less, and even more preferably 30° or less. Here, the dynamic angle of repose can be measured by the following method. (Method for measuring the dynamic angle of repose) Coated sand is placed in a cylindrical transparent plastic bottle to half its volume, and the bottle is held with its axis horizontal and rotated around the horizontal axis at a rotation speed of 60 rpm. The inclined surface of the coated sand layer flowing within the cylinder becomes flat. The angle formed between this inclined surface and the horizontal plane is measured. Note that if the coated sand does not flow within the cylinder, or if the inclined surface of the coated sand layer does not form a flat surface even if it flows, and as a result the dynamic angle of repose cannot be measured, the coated sand is in a wet state.
[0024] Specifically, the inorganic coated sand is composed of a group of inorganic coated sand particles.
[0025] From the viewpoint of improving fluidity and further improving the fillability into a molding die, the inorganic coated sand is preferably spherical. Here, "spherical" inorganic coated sand refers to sand having a round, ball-like shape. More specifically, from the viewpoint of improving fluidity, mold quality, and mold strength, and from the viewpoint of ease of mold formation, the sphericity of the inorganic coated sand is preferably 0.75 or more, more preferably 0.80 or more, and even more preferably 0.82 or more. The upper limit of the sphericity is specifically 1. In this embodiment, the sphericity of the inorganic coated sand specifically matches the sphericity of the refractory aggregate described below.
[0026] The sphericity of the inorganic coated sand is determined by analyzing the image (photograph) of the particle obtained by an optical microscope or a digital scope (for example, Keyence VH-8000 model) to determine the area of the projected cross section of the particle and the perimeter of the cross section, and then calculating the sphericity = [area of the projected cross section of the particle (mm 2 The particle diameter can be determined by calculating the perimeter (mm) of a circle having the same area as the particle diameter (mm) / the perimeter (mm) of the projected cross section of the particle, and averaging the values obtained for any 50 particles.
[0027] The average particle size of the inorganic-coated sand is preferably 0.05 mm or more, more preferably 0.1 mm or more, from the viewpoints of improving mold quality and mold strength, ease of mold production, and storage stability. Furthermore, if the average particle size of the inorganic-coated sand is equal to or greater than the above-mentioned lower limit, the amount of the second coating layer, etc. used during mold production can be reduced, making it easier to regenerate the inorganic-coated sand. From the viewpoints of improving mold quality and mold strength and ease of mold production, the average particle size of the inorganic-coated sand is preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less. Furthermore, if the average particle size of the inorganic-coated sand is equal to or less than the above-mentioned upper limit, the porosity during mold production is reduced, thereby increasing mold strength.
[0028] In this embodiment, the average particle size of the inorganic coated sand and the refractory aggregate described later can be specifically measured by the following method.
[0029] (Method for Measuring Average Particle Diameter) When the sphericity of a particle from a projected cross section is 1, the diameter (mm) is measured. On the other hand, when the sphericity is <1, the major axis diameter (mm) and minor axis diameter (mm) of randomly oriented particles are measured to calculate (major axis diameter + minor axis diameter) / 2, and the average of the values obtained for 100 randomly selected particles is used as the average particle diameter (mm). The major axis diameter and minor axis diameter are defined as follows: When a particle is stabilized on a flat surface and its projected image on the flat surface is sandwiched between two parallel lines, the width of the particle at the smallest distance between the parallel lines is called the minor axis diameter, and the distance when the particle is sandwiched between two parallel lines perpendicular to the parallel lines is called the major axis diameter. The major axis diameter and minor axis diameter of a particle can be determined by taking an image (photograph) of the particle using an optical microscope or a digital scope (e.g., Keyence Corporation, VH-8000 model) and analyzing the obtained image.
[0030] Each component of the inorganic coated sand will be described below.
[0031] [Reclaimed Sand (A)] Reclaimed sand (A) is an aggregate, a refractory material recycled from used casting molds or cores formed from refractory aggregate and a binder. Preferably, reclaimed sand (A) comprises refractory aggregate and an inorganic binder layer formed on the surface of the refractory aggregate and containing one or more selected from silicates and silicate reaction products. Reclaimed sand (A) is obtained, for example, by the manufacturing method described below.
[0032] (Refractory aggregate) The material of the refractory aggregate constituting the recycled sand (A) may be one or more selected from the group consisting of natural sand and artificial sand. Specifically, the refractory aggregate is composed of a group of refractory aggregate particles.
[0033] Examples of natural sand include one or more types selected from the group consisting of silica sand, which is mainly composed of quartz, chromite sand, zircon sand, olivine sand, and alumina sand.
[0034] Examples of artificial sand include synthetic mullite sand, SiO 2 SiO 2 Al-based foundry sand 2 O 3 Al, the main component of which is 2 O 3 Foundry sand of the SiO 2 / Al 2 O 3 Foundry sand of the SiO 2 / MgO-based foundry sand, SiO 2 / Al 2 O 3 / ZrO 2 Foundry sand of the SiO 2 / Al 2 O 3 / Fe 2 O 3 Examples of suitable foundry sand include one or more selected from the group consisting of foundry sand derived from refractory aggregates and slag-based foundry sand. Here, the term "main component" refers to the component that is most abundant among the components contained in the sand. Artificial sand refers to foundry sand that is not naturally occurring, but is made by artificially preparing metal oxide components and melting or sintering them. Also usable are recycled sand made from recovered refractory aggregates and recycled sand that has been reclaimed.
[0035] In addition, SiO in the refractory aggregate 2 , Al 2 O 3 , Fe 2 O 3 The content of each component, such as ammonium nitrate, ammonium nitrate, and ammonium hydroxide, can be measured using the following X-ray fluorescence method. Refractory aggregate is adjusted to a size of approximately 0.1 μm or less using a vibration mill and heated at 1050°C for 1 hour. Then, 5 g of lithium tetraborate and 0.5 g of refractory aggregate are mixed, heated at 1200°C for 10 minutes to melt, and then cooled to prepare a glassy sample (glass bead method). The sample is subjected to X-ray fluorescence analysis using a ZSX Primus II X-ray fluorescence analyzer (manufactured by Rigaku Corporation) using the fundamental parameter (FP) method.
[0036] In this embodiment, the sphericity of the refractory aggregate is the same as that of the inorganic-coated sand, and therefore the preferred conditions are the same. Furthermore, the average particle diameter of the refractory aggregate is preferably 0.05 mm or more, more preferably 0.1 mm or more, from the viewpoints of improving mold quality and mold strength, and ease of mold production. Furthermore, having the average particle diameter of the refractory aggregate at or above the lower limit mentioned above is also preferable in that the amount of inorganic binder layer used as the second coating layer during mold production can be reduced, making it easier to regenerate the inorganic-coated sand. From the viewpoints of improving mold quality and mold strength, and ease of mold production, the average particle diameter of the refractory aggregate is preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less. Furthermore, having the average particle diameter of the refractory aggregate at or below the upper limit mentioned above is also preferable in that the porosity during mold production is reduced, thereby increasing mold strength.
[0037] The amorphization degree of the refractory aggregate is preferably 20% or more, more preferably 30% or more, and even more preferably 40% or more, from the viewpoint of improving mold strength by making the surface of the aggregate smoother and obtaining low thermal expansion. The upper limit of the amorphization degree of the refractory aggregate is not limited, but may be, for example, 100% or less, or may be 99% or less.
[0038] The degree of amorphization of the refractory aggregate can be measured by the following X-ray diffraction method. (X-ray diffraction method) The refractory aggregate is pulverized in a mortar and then pressed onto an X-ray glass holder of a powder X-ray diffractometer for measurement. The powder X-ray diffractometer is a MultiFlex (CuKα radiation source, 40 kV tube voltage, 40 mA tube current) manufactured by Rigaku Denki Co., Ltd., and is measured at a scanning interval of 0.01°, a scanning speed of 2° / min, and slits DS1, SS1, and RS0.3 mm in the range of 2θ = 5° to 90°. A straight line is drawn between the X-ray intensities on the low-angle side and the high-angle side in the range of 2θ = 10° to 50°, and the area under the line is used as the background. The degree of crystallinity is calculated using the software provided with the instrument and subtracted from 100 to obtain the degree of amorphization. Specifically, for the area above the background, the amorphous peak (halo) and each crystalline component are separated by curve fitting, the area of each is determined, and the amorphous degree (%) is calculated using the following formula: Amorphous degree (%) = halo area / (crystalline component area + halo area) × 100
[0039] There are various methods for controlling the degree of amorphization of refractory aggregate, but it is generally preferable to use a manufacturing method that rapidly cools a molten material. For example, there is a method in which the raw material is melted and rapidly cooled by air-crushing, or a method in which it is treated in a flame and rapidly cooled. In either case, the cooling method may be selected appropriately at various speeds depending on the material and particle size. Another possible method is to amorphize a material that has been crystallized by heat treatment and cooling treatment. Among these, the flame fusion method, which allows easy control of heating and cooling, is preferred.
[0040] (Inorganic Binder Layer) The reclaimed sand (A) preferably has an inorganic binder layer. Specifically, the inorganic binder layer contains one or more selected from silicates and reaction products of silicates, and coats the surface of the refractory aggregate. Note that the coating is not limited to a continuous layer, and may have discontinuous portions.
[0041] The inorganic binder layer is intended to be a layer in which, when a refractory aggregate and inorganic-coated sand having an inorganic binder formed on the surface of the refractory aggregate are molded into a casting mold, used as a mold, and then reclaimed to produce reclaimed sand, the inorganic binder remains on the surface of the refractory aggregate as a residual inorganic binder. That is, the silicate and silicate reaction product contained in the inorganic binder layer are intended to be a layer in which the residual inorganic binder remains on the surface of the refractory aggregate. Specific examples of the silicate and silicate reaction product include silicate and metasilicate, and examples of the reaction product include a reaction product of silicate with amorphous silica and a reaction product of silicate with amorphous silica, each of which may be present alone or in combination. Furthermore, examples of cations constituting the salt include monovalent cations such as sodium, potassium, lithium, and ammonium, and divalent cations such as magnesium, calcium, and zinc.
[0042] Methods for confirming that the inorganic binder layer contains silicates or silicate reaction products include, for example, a method in which recycled sand is stirred in a hydrochloric acid solution and the dissolved components are analyzed with an ICP emission spectrometer to determine the concentrations of silicate ions, sodium ions, etc., a method in which the recycled sand surface is subjected to elemental analysis with a scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX) to confirm the presence of silicon, sodium, etc., or 23 Na, 29 One method is to confirm the silicate-derived structure by Si solid-state NMR.
[0043] [Refractory aggregate (B)] The refractory aggregate (B) has an amorphous degree of at least 20% or more, preferably 30% or more, from the viewpoint of smoothing the aggregate surface to further improve mold strength and obtaining low thermal expansion, and from the viewpoint of improving storage stability, it is preferably 99% or less, more preferably 80% or less, even more preferably 70% or less, and even more preferably 60% or less.
[0044] In addition, the SiO of the refractory aggregate (B) 2From the viewpoint of storage stability, the content of SiO of the refractory aggregate (B) is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more, and from the viewpoint of further improving mold strength, the content is preferably 99% or less, more preferably 80% or less, and even more preferably 70% or less. 2 The content is preferably 50% or less, more preferably 40% or less.
[0045] The degree of amorphization of the refractory aggregate (B) is determined by the same X-ray diffraction method as that of the refractory aggregate of the recycled sand (A). 2 The content can be measured by the same X-ray fluorescence method as in the case of the refractory aggregate of the reclaimed sand (A).
[0046] [Foundry Sand] Foundry sand has a first coating layer formed on the surface of one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B) as its outermost layer. The foundry sand can function as inorganic coated sand by further forming a second coating layer on the first coating layer. The cation exchange capacity (CEC) of the foundry sand needs to be controlled to a specific value in order to prevent the inorganic coated sand from becoming wet. The cation exchange capacity (CEC) can be controlled by combining known methods, for example, by selecting the material of the coating layer, adjusting the content, and adjusting the firing temperature and time. Specifically, foundry sand is composed of foundry sand particles.
[0047] The CEC of foundry sand is determined by the ammonium acetate method (Fertilizer Analysis Method (National Institute for Agro-Environmental Sciences, Ministry of Agriculture, Forestry and Fisheries) 5.31.1) shown below. First, a small piece of absorbent cotton is placed at the bottom of the permeation tube as a support layer, and then a layer of filter paper pulp made by cutting filter paper into small pieces and stirring it in hot water is packed on top to a thickness of approximately 5 mm to create a flat filtration surface. Next, a stopper is placed at the bottom of the permeation tube, and several mL of 1M ammonium acetate solution is added. 2-4 g of the analytical sample (foundry sand) is weighed and allowed to drop and settle little by little until the sample is filled. After that, the stopper is removed, the apparatus is reassembled, and washing with ammonium acetate solution begins. 100 mL of 1M ammonium acetate solution is used, and the drip rate is adjusted so that permeation is complete within 4-20 hours. After permeation is complete, the upper inside surface of the permeation tube is washed with a small amount of alcohol, and the sample layer is washed with 50 mL of 80% alcohol to remove excess ammonium acetate solution. The NH4O2 thus obtained is then measured and stored in a cool, dry place. 4 + The analytical sample saturated with NH was washed with 100 mL of 10% sodium chloride solution. 4 + The amount of ammonia nitrogen in the leachate is determined by steam distillation and alkali titration, and is expressed as millimole equivalents per kg of analytical sample, which is the cation exchange capacity.
[0048] From the viewpoint of enhancing storage stability, the cation exchange capacity (CEC) is 3 mmol(+) / kg or more, and preferably 6 mmol(+) / kg or more, while from the viewpoint of enhancing storage stability, the cation exchange capacity (CEC) is 40 mmol(+) / kg or less, preferably 20 mmol(+) / kg or less, and more preferably 10 mmol(+) / kg or less.
[0049] (First Coating Layer) The first coating layer constituting the foundry sand is a layer for coating the surface of one or two types of aggregate selected from the recycled sand (A) and the refractory aggregate (B). The first coating layer constitutes the outermost layer of the foundry sand, and in the case of inorganic coated sand, it is located between the second coating layer (described below) and the surface of the aggregate.
[0050] The first coating layer is made of a different material from the second coating layer, and preferably does not contain metasilicate, and more preferably is made of aluminosilicate, which effectively prevents silicates in the second coating layer from acting on the aggregate and accelerating the wetting of the inorganic-coated sand.
[0051] Examples of aluminosilicates include reaction products of one or more selected from silicates and reaction products of silicates with aluminates or aluminum hydroxide. Here, silicate refers to a substance containing an anionic group with one or more silicon atoms at the center surrounded by electronegative ligands. Specifically, it refers to either or both of the residual inorganic binder present on the surface of the refractory aggregate and the refractory aggregate (B). To facilitate improved storage stability, the aluminosilicate preferably contains at least one reaction product of one or more selected from silicates and reaction products of silicates with sodium aluminate or aluminum hydroxide. The form of the sodium aluminate is not particularly limited, and it may be either a powder or an aqueous solution.
[0052] The aluminum content in the first coating layer is Al 2 O 3 In terms of improving storage stability, the aluminum content in the first coating layer is preferably 0.1 parts by mass or more, more preferably 0.4 parts by mass or more, relative to 100 parts by mass of the aggregate. 2 O 3 In terms of increasing mold strength and obtaining good storage stability, the amount is preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of aggregate.
[0053] The aluminum content in the first coating layer can be determined by the following method: It can be calculated from the analytical values of the aggregate obtained by the X-ray fluorescence method and the analytical values of the molding sand containing the first coating layer using the aggregate obtained by the X-ray fluorescence method, using the following formula: 2 O 3 [Parts by mass] = {Al of molding sand} 2 O 3[parts by mass]} - {Al of aggregate 2 O 3 [Parts by mass]}
[0054] From the viewpoint of improving storage stability and obtaining a high-strength casting mold, the content of the first coating layer is preferably 0.02 parts by mass or more, more preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more, per 100 parts by mass of aggregate. From the viewpoint of achieving both storage stability and strength, the content of the first coating layer is preferably 10 parts by mass or less, more preferably 9.5 parts by mass or less, per 100 parts by mass of aggregate.
[0055] [Second Coating Layer] The second coating layer is a layer formed on the first coating layer, and is the outermost layer of the inorganic coated sand.
[0056] The second coating layer contains metasilicate and is used to impart the function of a binder to the aggregate. This is preferable because it improves the crystallinity of the second coating layer and also makes the inorganic coated sand dry, resulting in excellent room temperature fluidity.
[0057] Examples of metasilicates include one or more selected from sodium metasilicate, potassium metasilicate, lithium metasilicate, ammonium metasilicate, etc., and hydrates thereof. Among these, sodium metasilicate and potassium metasilicate are preferred. The amount of water of hydration of the metasilicate hydrate is not particularly limited, but is preferably 5 to 9. Specifically, at least one selected from sodium metasilicate pentahydrate and sodium metasilicate nonahydrate is preferred, with sodium metasilicate nonahydrate being more preferred.
[0058] From the viewpoint of improving storage stability and obtaining a high-strength casting mold, the content of the second coating layer is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.5 parts by mass or more, particularly preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, per 100 parts by mass of aggregate. On the other hand, from the viewpoint of achieving both storage stability and strength, the content of the second coating layer is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less, per 100 parts by mass of aggregate.
[0059] From the viewpoints of improving mold strength, excellent productivity, and ease of availability, the content of metasilicate in the second coating layer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably substantially 100% by mass. Here, "substantially" means that it may contain unintentionally contained components, for example, components other than metasilicate contained in the metasilicate raw material. The total content of metasilicate in the second coating layer refers to the total content of metasilicate relative to all components other than water in the second coating layer.
[0060] The content of metasilicate in the second coating layer (anhydride equivalent) is preferably 0.03 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.5 parts by mass or more, and even more preferably 0.9 parts by mass or more, per 100 parts by mass of aggregate, from the viewpoint of improving storage stability and obtaining a high-strength casting mold. On the other hand, the content of metasilicate is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, per 100 parts by mass of aggregate, from the viewpoint of achieving both storage stability and strength.
[0061] (Inorganic Fine Particles) In this embodiment, the inorganic coated sand may further contain inorganic fine particles. When inorganic fine particles are contained, it is preferable that the inorganic fine particles form part of the second coating layer. Specifically, it is preferable that the second coating layer further contains inorganic fine particles on at least one of the surface and the interior of the layer, and it is more preferable that the second coating layer further contains inorganic fine particles on the layer. The inorganic fine particles may be contained both on and in the second coating layer. In this way, the particles of the inorganic coated sand are more firmly bonded to each other via the inorganic fine particles, thereby further improving the strength of the resulting mold. The inorganic fine particles on the second coating layer may be partially embedded in the second coating layer.
[0062] The inorganic fine particles are not limited, but may be one or more kinds of fine particles selected from silica, silicon, zinc oxide, aluminum hydroxide, tin oxide, etc. Among them, silica particles are preferred from the viewpoint of improving the strength of the mold, and amorphous silica particles are more preferred from the viewpoint of having a large specific surface area and high reactivity with silicates. These inorganic fine particles may be used alone or in combination of two or more kinds.
[0063] (Other Additives) In addition to the components described above, the second coating layer may contain various additives as needed. Examples of other additives include coupling agents, humectants, moisture resistance improvers, lubricants, surfactants, and release agents. Examples of coupling agents include, but are not limited to, silane coupling agents, zirconium coupling agents, and titanium coupling agents. Examples of humectants include polyhydric alcohols, water-soluble polymers, hydrocarbons, sugars, proteins, and inorganic compounds other than those described above. Examples of moisture resistance improvers include metal oxides (excluding those listed above), carbonates, borates, sulfates, and phosphates. Examples of lubricants include waxes; fatty acid amides; alkylene fatty acid amides; stearic acid; stearyl alcohol; metal stearates such as lead stearate, zinc stearate, calcium stearate, and magnesium stearate; stearic acid monoglyceride; stearyl stearate; and hydrogenated oils. Examples of the release agent include paraffin, wax, light oil, machine oil, spindle oil, insulating oil, waste oil, vegetable oil, fatty acid ester, organic acid, graphite fine particles, mica, vermiculite, fluorine-based release agents, and silicone-based release agents.
[0064] (Water content) The content of water, including crystal water, in the second coating layer is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of silicate (anhydrous equivalent) from the viewpoint of obtaining a high-strength mold.In addition, based on the viewpoint of filling into the molding die and obtaining a high-strength mold, the content of water in the second coating layer is preferably 180 parts by mass or less, more preferably 160 parts by mass or less, even more preferably 150 parts by mass or less, and even more preferably 140 parts by mass or less, based on 100 parts by mass of silicate.
[0065] The content of water, including water of crystallization, in the second coating layer contained in the inorganic coated sand can be adjusted depending on the type of silicate.
[0066] When the metasilicate is sodium metasilicate, from the viewpoint of obtaining a high-strength mold and from the viewpoint of easily manufacturing the mold, the content of water including water of crystallization in the second coating layer is preferably 60 parts by mass or more, more preferably 65 parts by mass or more, even more preferably 90 parts by mass or more, and even more preferably 110 parts by mass or more, per 100 parts by mass of sodium metasilicate (anhydrous equivalent); from the viewpoint of improving fluidity and further improving fillability into a molding die, it is preferably 180 parts by mass or less, more preferably 160 parts by mass or less, even more preferably 150 parts by mass or less, and even more preferably 140 parts by mass or less. For example, when the silicate constituting the second coating layer is only sodium metasilicate pentahydrate, the water content is 74 parts by mass per 100 parts by mass of sodium metasilicate, and when it is only sodium metasilicate nonahydrate, the water content is 133 parts by mass per 100 parts by mass of sodium metasilicate.
[0067] <Method for Producing Reclaimed Sand (A) / Method for Reclaiming Used Foundry Sand> Methods for reclaiming waste mold sand after casting can be based on known methods (e.g., "Mold Making Methods," 4th Edition, Japan Foundry Technology Association, November 18, 1996, pp. 327-330). For example, known methods include dry grinding (mechanical abrasion), wet grinding, roasting, and combinations of these methods.
[0068] Dry grinding can remove part of the inorganic binder layer residue present on the surface of the refractory aggregate. For example, methods using a sand reclaimer, which uses a high-speed airflow to raise sand within the device and collide it against an impact plate, thereby grinding the sand through collisions and friction between the sand particles; a high-speed rotary reclaimer, which charges sand onto a rotor rotating at high speed and grinds the sand through collisions and friction between the thrown sand generated by the centrifugal force and the falling sand; or an agitator mill, which grinds the sand by utilizing friction between the sand particles. Wet grinding can also be performed using a trough grinder, which uses rotating blades to grind the sand through friction between the sand particles in a trough.
[0069] The roasting treatment may involve, for example, using a roasting furnace such as a fluidized bed roasting furnace or a rotary kiln, rapidly charging sand into the roasting furnace, and firing at a temperature in the range of 200 to 1000° C. It is also known that roasting at a temperature in the range of 600 to 800° C. can be used to further improve accuracy.
[0070] Any method may be used for regeneration, but wet treatment and roasting treatment are complicated steps and require a large energy load, so dry grinding treatment is preferred.
[0071] <Method for manufacturing inorganic coated sand> Next, a method for manufacturing inorganic coated sand of this embodiment will be described. The method for manufacturing inorganic coated sand of this embodiment is a method for manufacturing dry inorganic coated sand having foundry sand comprising one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), a first coating layer covering the aggregate and positioned on the surface, and a second coating layer containing metasilicate on the first coating layer of the foundry sand, wherein the refractory aggregate (B) is SiO 2 wherein the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.
[0072] According to the manufacturing method of this embodiment, by forming a first coating layer on the surface of the aggregate and controlling the cation exchange capacity (CEC) of the foundry sand, it is possible to improve storage stability while eliminating the process of roasting the aggregate, thereby reducing thermal energy consumption and mitigating the environmental burden.
[0073] First, as an example of a method for producing the inorganic coated sand of this embodiment, the refractory aggregate (B) is SiO 2The manufacturing method includes the following steps (1) to (3): Step (1): Mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with aluminate or aluminum hydroxide, and forming the first coating layer on the surface of the aggregate to obtain molding sand; Step (2): Mixing the obtained molding sand with a molten liquid of metasilicate hydrate to obtain a mixture; Step (3): Cooling the obtained mixture to a temperature below the melting point of the metasilicate hydrate, and forming the second coating layer on the first coating layer.
[0074] In step (1), an aluminate or aluminum hydroxide is mixed with aggregate to form a first coating layer that covers the surface of the aggregate. Among these, heating to 25°C or higher but lower than 400°C is preferred to form the first coating layer. Examples of methods for forming the first coating layer by heating to 25°C or higher but lower than 400°C in step (1) include a method in which an aluminate is added to aggregate heated to 25°C or higher but lower than 400°C, or a method in which an aluminate or aluminum hydroxide is added to aggregate and then heated to 25°C or higher but lower than 400°C. Of these, the latter method is preferred from the viewpoint of forming a uniform coating layer. Furthermore, the heating temperature is preferably 40°C or higher but lower than 300°C, more preferably 70°C or higher but lower than 200°C, from the viewpoint of improving storage stability.
[0075] Examples of methods for forming the first coating layer in step (1) by heating to 25°C or higher but lower than 400°C include adding aluminate or aluminum hydroxide to aggregate heated to 25°C or higher but lower than 400°C, or adding aluminate or aluminum hydroxide to the aggregate and then heating to 25°C or higher but lower than 400°C. The latter method is preferred from the viewpoint of forming a uniform coating layer. Furthermore, the heating temperature is preferably 40°C or higher but lower than 300°C, more preferably 70°C or higher but lower than 200°C, from the viewpoint of improving storage stability. Mixing conditions, such as the stirring speed and processing time, when mixing the aggregate with the aluminate or aluminum hydroxide can be appropriately determined depending on the amount of the mixture processed. This method produces foundry sand having a cation exchange capacity (CEC) of 3 mmol(+) / kg or higher but lower than 40 mmol(+) / kg.
[0076] In step (2), the foundry sand is mixed with a molten solution of metasilicate hydrate to obtain a mixture. Examples of methods for mixing the molten solution of metasilicate hydrate with foundry sand in step (2) include adding the metasilicate to foundry sand heated to or above the melting point of the metasilicate hydrate, or adding the metasilicate heated to or above the melting point of the metasilicate hydrate to foundry sand. The latter method is preferred because it shortens the coating time. Mixing conditions, such as the stirring speed and processing time, when mixing the foundry sand and metasilicate hydrate can be determined appropriately depending on the amount of the mixture to be processed.
[0077] In step (3), the mixture obtained in step (2) is cooled to a temperature below the melting point of the metasilicate hydrate to reduce the fluidity of the metasilicate hydrate and fix the metasilicate hydrate to the surface of the foundry sand, thereby forming a metasilicate hydrate layer, i.e., a second coating layer, thereby obtaining the inorganic-coated sand according to this embodiment.
[0078] Next, as another example of the method for producing the inorganic coated sand of this embodiment, the refractory aggregate (B) is SiO 2The manufacturing method includes the following steps (4) and (5): Step (4): Mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with an aluminate or aluminum hydroxide, and forming the first coating layer on the surface of the aggregate to obtain foundry sand; Step (5): Mixing the foundry sand with a solution containing water glass, caustic alkali, and water to obtain a mixture containing sodium metasilicate hydrate.
[0079] Step (4) can be carried out in the same manner as step (1) above.
[0080] In step (5), SiO in a solution containing water glass, caustic alkali, and water is 2 / M 2 O (M represents an alkali metal) / H 2 By adjusting the molar ratio of O to 1:1:n (5≦n≦9), metasilicate hydrate with the desired amount of water of hydration can be formed. Furthermore, by mixing the above solution containing water glass, caustic alkali, and water with the molding sand, the surface of the molding sand can be coated with metasilicate hydrate to form a second coating layer. The conditions for mixing the water glass, caustic alkali, and water are not particularly limited, and known methods can be used. For example, mixing may be performed at ambient temperature, or if heat is generated in the molten liquid, mixing may be continued and then allowed to cool to ambient temperature.
[0081] In this way, the inorganic coated sand according to this embodiment can be obtained.
[0082] <Mold> The casting mold of this embodiment includes the inorganic coated sand of this embodiment described above, and is formed using the inorganic coated sand. Examples of methods for making the casting mold include a molding method using a heated molding die, and a molding method in which water vapor is passed through a heated molding die and then hot air is passed through it.
[0083] <Method for Improving Storage Stability> The method for improving the storage stability of inorganic coated sand according to this embodiment is a method for improving the storage stability of inorganic coated sand, which comprises foundry sand containing one or two aggregates selected from recycled sand (A) and refractory aggregate (B), and a second coating layer containing metasilicate that coats the foundry sand, wherein the refractory aggregate (B) is SiO 2 The method includes the step of preparing dry inorganic-coated sand so that the cation exchange capacity (CEC) of the foundry sand satisfies 3 mmol(+) / kg or more and 40 mmol(+) / kg or less. This improves the storage stability of the inorganic-coated sand. The step of adjusting the cation exchange capacity (CEC) of the foundry sand so that the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less is achieved by adjusting the manufacturing methods of the inorganic-coated sand and the foundry sand. Details are the same as those explained in the above-mentioned method of manufacturing inorganic-coated sand. Furthermore, details such as the composition of the inorganic-coated sand and the foundry sand are also the same as those explained above.
[0084] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations can also be adopted.
[0085] In relation to the above-described embodiments, the present invention further discloses the following inorganic-coated sand, a method for manufacturing the inorganic-coated sand, and a method for manufacturing a casting mold.
[0086] <1> A dry inorganic coated sand comprising foundry sand including one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), a first coating layer covering the aggregate and positioned on the surface, and a second coating layer containing metasilicate on the first coating layer of the foundry sand, wherein the refractory aggregate (B) is SiO 2and a cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more, preferably 6 mmol(+) / kg or more, and 40 mmol(+) / kg or less, preferably 20 mmol(+) / kg or less, and more preferably 10 mmol(+) / kg or less. <2> The inorganic-coated sand according to <1>, wherein the content of the first coating layer is 0.02 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more, and 10 parts by mass or less, preferably 9.5 parts by mass or less, relative to 100 parts by mass of the aggregate. <3> The inorganic-coated sand according to <1> or <2>, wherein the content of the second coating layer is 0.05 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more, per 100 parts by mass of the aggregate, and is 10 parts by mass or less, preferably 8 parts by mass or less, and more preferably 6 parts by mass or less. <4> The inorganic-coated sand according to any one of <1> to <3>, wherein the first coating layer of the foundry sand contains an aluminosilicate, and the aluminosilicate contains a reaction product of one or more selected from silicates and reaction products of silicates with an aluminate or aluminum hydroxide. <5> The inorganic coated sand according to any one of <1> to <4>, wherein the aluminosilicate comprises at least one reaction product of one or more selected from the group consisting of silicates and reaction products of silicates with sodium aluminate or aluminum hydroxide. <6> The inorganic coated sand according to any one of <1> to <5>, wherein the dynamic angle of repose of the inorganic coated sand is preferably 80° or less, more preferably 45° or less, and even more preferably 30° or less.<7> The inorganic coated sand according to any one of <1> to <6>, wherein the degree of amorphization of the refractory aggregate (B) is preferably 30% or more, more preferably 50% or more, even more preferably 65% or more, and even more preferably 80% or more, and is preferably 100% or less, and more preferably 99% or less. <8> The inorganic coated sand according to any one of <1> to <7>, wherein the SiO of the refractory aggregate (B). 2 <9> The inorganic coated sand according to any one of <1> to <8>, wherein the aluminum content in the first coating layer is preferably 10% or more, preferably 20% or more, more preferably 30% or more, and on the other hand, preferably 99% or less, more preferably 80% or less, even more preferably 70% or less, particularly preferably 50% or less, and even more particularly preferably 40% or less. 2 O 3The inorganic coated sand according to any one of <1> to <9>, wherein the content of metasilicate in the second coating layer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, still more preferably 98% by mass or more, and still more preferably substantially 100% by mass. <11> The inorganic-coated sand according to any one of <1> to <10>, wherein the content of water including water of crystallization in the second coating layer is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, relative to 100 parts by mass of silicate (anhydrous equivalent), and is preferably 180 parts by mass or less, more preferably 160 parts by mass or less, even more preferably 150 parts by mass or less, and still more preferably 140 parts by mass or less. <12> A casting mold comprising the inorganic-coated sand according to any one of <1> to <11>. <13> A method for producing inorganic coated sand, comprising: a step (1) of mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with aluminate or aluminum hydroxide to form the first coating layer on the surface of the aggregate to obtain the foundry sand; a step (2) of mixing the obtained foundry sand with a molten liquid of metasilicate hydrate to obtain a mixture; and a step (3) of cooling the mixture to a temperature below the melting point of the metasilicate hydrate, wherein the refractory aggregate (B) is SiO 2<14> A method for producing inorganic coated sand, comprising: a step (4) of mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with aluminate or aluminum hydroxide to form the first coating layer on the surface of the aggregate to obtain the foundry sand; and a step (5) of mixing the obtained foundry sand with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate, wherein the refractory aggregate (B) is SiO 2 <15> A method for producing inorganic-coated sand according to <13> or <14>, wherein in step (1) or step (4), the first coating layer is formed by heating the inorganic-coated sand to 25°C or higher but lower than 400°C, preferably 40°C or higher but lower than 300°C, and more preferably 70°C or higher but lower than 200°C. <16> A method for producing inorganic-coated sand according to <14>, wherein in step (5), the first coating layer is formed by heating the inorganic-coated sand to 25°C or higher but lower than 400°C, preferably 40°C or higher but lower than 300°C, and more preferably 70°C or higher but lower than 200°C. 2 / M 2 O (M represents an alkali metal) / H 2 <17> A method for improving the storage stability of inorganic-coated sand, the method comprising: foundry sand containing one or two aggregates selected from recycled sand (A) and refractory aggregate (B); and a second coating layer containing metasilicate that coats the foundry sand, wherein the refractory aggregate (B) is SiO 2 and preparing the dry inorganic-coated sand so that the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.
[0087] EXAMPLES The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these.
[0088] (1) Materials The materials used in the following Examples and Comparative Examples are described below. [Refractory Aggregates] Refractory aggregate 1: Espearl #60L (manufactured by Yamakawa Sangyo Co., Ltd., average particle size: 241 μm, degree of amorphization: 45%) Refractory aggregate (B1): spherical fused silica (natural silica sand sphericalized by flame fusion method, average particle size: 200 μm, degree of amorphization: 95% or more) Refractory aggregate (B2): Naigai Cerabeads 60 #650 (manufactured by Itochu Ceratec Co., Ltd., average particle size: 200 μm, degree of amorphization: 30%)
[0089] [Inorganic fine particles] Amorphous silica fine particles: Denka fused silica SFP-20M (manufactured by Denka, average particle size: 0.4 μm, degree of amorphousness: 99.5% or more) Calcined kaolin: Satington W (manufactured by BASF, average particle size: 0.4 μm)
[0090] [Reclaimed Sand (A)] Reclaimed sand (A1) was prepared according to the following procedure. (i) Preparation of Inorganic Coated Sand: 100 parts by mass of refractory aggregate 1 (Espearl #60L) was added to a mixer. Next, sodium metasilicate nonahydrate (2.00 parts by mass) heated to 80°C and melted was added to the mixer and mixed for 4 minutes to obtain dry sand with room temperature fluidity. Then, amorphous silica fine particles (0.6 parts by mass) were added and mixed for 2 minutes to obtain dry inorganic coated sand used for preparing reclaimed sand (A1). (ii) Preparation of Mold: A portion of 10 kg of the obtained inorganic coated sand was poured into the center of a truncated cone mold for preparing a test mold, measuring 298 mm in upper diameter, 205 mm in lower diameter, and 265 mm in height, to a height of 50 mm. Next, a metal core with a truncated cone shape, measuring 280 mm in upper diameter, 200 mm in lower diameter, and 220 mm in height, heated to 180°C, was placed in the mold. The remaining inorganic-coated sand was poured into the space between the mold and the metal core, and the mold was heated in a heating furnace at 180°C for 20 minutes to obtain a test mold. (iii) Casting: 10 kg of aluminum alloy AC4C (720°C) was poured into the obtained test mold. After pouring, the mold was left to cool at room temperature. (iv) Preparation of Reclaimed Sand: After casting, the casting was removed from the test mold, crushed with a hammer, etc., and further crushed in a mini crusher (manufactured by Taiyo Machinery Co., Ltd.) until the mold was reduced to single particles, obtaining recovered sand. (v) Preparation of Reclaimed Sand 100 kg of recovered sand was placed in a dry foundry sand reclamation device equipped with a fluidized bed (Hybrid Sand Master, manufactured by Nippon Chuzo Co., Ltd.) and batch-processed for 60 minutes at a rotor speed of 2400 rpm to obtain reclaimed sand (A1). Fine powder derived from the binder generated during the process was removed using a dust collector.
[0091] [Materials for the first coating layer] 50% sodium aluminate: sodium aluminate #2019 (50% sodium aluminate aqueous solution manufactured by Asada Chemical Industry Co., Ltd.) Aluminum hydroxide (Al(OH) 3 ): aluminum hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., powder form, average particle size: 2.01 μm) No. 2 water glass: No. 2 sodium silicate (manufactured by Fuji Chemical Industry Co., Ltd., Si / Na molar ratio 2.4)
[0092] [Material for second coating layer] Sodium metasilicate nonahydrate: sodium metasilicate nonahydrate (manufactured by Nippon Chemical Industry Co., Ltd.)
[0093] (2) Preparation of Inorganic Coated Sand Each inorganic coated sand having the composition shown in Table 1 was prepared by the following procedure.
[0094] Example 1: 100 parts by mass of recycled sand (A1) was added to a mixer as a refractory aggregate. Next, 2.3 parts by mass of a 50% aqueous sodium aluminate solution was added and stirred for 2 minutes to obtain a mixture. The resulting mixture was then heated in a kiln at a roasting temperature of 80°C for 12 hours, cooled to room temperature, and sieved through a 20-mesh sieve to remove any aggregates. This resulted in a foundry sand with a first coating layer made of aluminosilicate formed on the surface of the recycled sand (A1). Next, the foundry sand and 3.50 parts by mass of sodium metasilicate nonahydrate (heated to 80°C and melted) were added to the mixer and kneaded for 4 minutes to form a second coating layer on the first coating layer, thereby obtaining the inorganic-coated sand of Example 1. Table 1 shows the composition of the inorganic-coated sand.
[0095] Examples 2 to 3 The inorganic coated sands of Examples 2 and 3 listed in Table 1 were obtained in the same manner as in Example 1, except that the amount of 50% sodium aluminate aqueous solution added when forming the first coating layer made of aluminosilicate on the surface of the reclaimed sand (A1) was changed to the parts by mass shown in Table 1.
[0096] Example 4 The inorganic coated sand of Example 4 shown in Table 1 was obtained in the same manner as in Example 1, except that 0.1 parts by mass of No. 2 water glass was added when the 50% sodium aluminate aqueous solution was added to form a first coating layer made of aluminosilicate on the surface of the reclaimed sand (A1).
[0097] Examples 5 to 8 Inorganic-coated sand was obtained in the same manner as in Example 1, except that the roasting temperature for forming a first coating layer made of aluminosilicate on the surface of the reclaimed sand (A1) was changed to the temperatures shown in Table 1. Table 1 shows the blending compositions of the inorganic-coated sand of Examples 5 to 8.
[0098] Example 9 Inorganic-coated sand was obtained in the same manner as in Example 1, except that a suspension of aluminum hydroxide previously suspended in water (aluminum hydroxide:water = 1:1 mass ratio) was used instead of the 50% aqueous sodium aluminate solution. Table 1 shows the composition of the inorganic-coated sand of Example 9.
[0099] Examples 10 and 12 Inorganic coated sand was obtained in the same manner as in Example 2, except that the reclaimed sand (A1) used as the refractory aggregate was changed to the refractory aggregate shown in Table 2. Table 2 shows the blending compositions of the inorganic coated sands of Examples 10 and 12.
[0100] Example 11 Inorganic coated sand was obtained in the same manner as in Example 3, except that the reclaimed sand (A1) used as the refractory aggregate was changed to the refractory aggregate shown in Table 2. Table 2 shows the blending composition of the inorganic coated sand of Example 11.
[0101] Example 13: Using the inorganic coated sand obtained in Example 2, reclaimed sand (A2) was obtained in the same manner as in Example 2, following steps (ii) to (v) for reclaimed sand (A1). This reclaimed sand (A2) was used to prepare inorganic coated sand in the same manner as in Example 2, and steps (ii) to (v) for reclaimed sand (A1) were repeated again to obtain reclaimed sand (A3). Furthermore, the process of obtaining reclaimed sand (A3) from reclaimed sand (A2) was repeated twice using reclaimed sand (A3), to obtain reclaimed sand (A5). Reclaimed sand (A5) was used to obtain inorganic coated sand in the same manner as in Example 2. The storage stability results are shown in Table 3.
[0102] Comparative Example 1 Inorganic-coated sand of Comparative Example 1 containing an inorganic binder and not containing a first coating layer made of aluminosilicate was obtained in the same manner as in Example 1, except that neither the addition of 50% sodium aluminate nor the heat treatment was performed. Table 1 shows the blending composition of the inorganic-coated sand of Comparative Example 1.
[0103] <Comparative Examples 2 to 3> Inorganic coated sands of Comparative Examples 2 to 3 were obtained in the same manner as in Example 1, except that 50% sodium aluminate was not added and heat treatment was carried out at the temperatures shown in Table 1. Table 1 shows the blending compositions of the inorganic coated sands of Comparative Examples 2 to 3.
[0104] Comparative Example 4: 100 parts by mass of recycled sand (A1) was prepared as a refractory aggregate and placed in a mixer. Next, 0.25 parts by mass of calcined kaolin, 0.25 parts by mass of amorphous silica fine particles, and 0.50 parts by mass of water were added and stirred for 2 minutes. The resulting mixture was then heated in an electric furnace at 730 ° C for 1 hour, and then the heating of the electric furnace was stopped and the mixture was left in the electric furnace for 4 hours. The mixture was then removed from the electric furnace and cooled to room temperature at room temperature. After that, the aggregates were removed from the mixture through a sieve (20 mesh). The resulting mixture and sodium metasilicate nonahydrate (3.50 parts by mass) heated to 80 ° C and melted were added to a mixer and kneaded for 4 minutes to obtain the inorganic coated sand of Comparative Example 4. Table 1 shows the composition of the inorganic coated sand.
[0105] <Comparative Examples 5 to 6> Inorganic coated sands of Comparative Examples 5 and 6 were obtained in the same manner as in Comparative Example 1, except that the recycled sand (A1) used as the refractory aggregate was changed to the type of refractory aggregate shown in Table 2. Table 2 shows the blending compositions of the inorganic coated sands of Comparative Examples 5 and 6.
[0106] (3) Evaluation and Measurement The following evaluation and measurement were carried out using the obtained inorganic coated sand. The results are shown in Tables 1 and 2.
[0107] <Storage Stability; Measurement of Time to Wetness> Immediately after preparing the inorganic-coated sand, the dynamic angle of repose of the inorganic-coated sand was measured using the following procedure. Separately, immediately after preparing the inorganic-coated sand, 2 kg of the inorganic-coated sand was placed in a plastic bag, sealed, and left in a constant temperature room at 25°C / 55%RH. Every 24 hours, the dynamic angle of repose of the inorganic-coated sand was measured using the following procedure, and the state of the inorganic-coated sand (dry or wet) was confirmed as follows. If the inorganic-coated sand had become wet, the time from placing it in the plastic bag until it became wet was recorded as the "time to wetness" (days).
[0108] (i) Procedure (Measurement of dynamic angle of repose) Half the volume of inorganic-coated sand was placed in a cylindrical transparent plastic bottle with a diameter of 76 mm and a height of 125 mm. The bottle was held so that its axis was horizontal and rotated around the horizontal axis at room temperature (25°C) at a speed of 60 rpm. The inclined surface of the inorganic-coated sand layer flowing inside the cylinder became flat, and the angle formed between this inclined surface and the horizontal plane (dynamic angle of repose) was measured. (ii) Confirmation (Determination of dry or wet state) In the above procedure, a case where the angle could be measured was judged to be "dry state." A case where the inorganic-coated sand did not flow inside the cylinder, or the inclined surface of the inorganic-coated sand layer did not form a flat surface even if it flowed, and as a result, the dynamic angle of repose could not be measured, was judged to be "wet state."
[0109]
[0110]
[0111]
Claims
1. A dry inorganic coated sand comprising a molding sand in which a first coating layer is arranged on the surface of one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), and a second coating layer containing metasilicate on the first coating layer of the molding sand, wherein the refractory aggregate (B) is SiO 2 wherein the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.
2. Inorganic coated sand according to claim 1, wherein the content of the first coating layer is 0.02 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the aggregate.
3. Inorganic coated sand according to claim 1 or 2, wherein the content of the second coating layer is 0.05 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the aggregate.
4. Inorganic coated sand according to any one of claims 1 to 3, wherein the first coating layer contains an aluminosilicate, and the aluminosilicate contains a reaction product of one or more selected from the group consisting of silicates and reaction products of silicates, with an aluminate or aluminum hydroxide.
5. The inorganic coated sand according to claim 4, wherein the aluminosilicate comprises at least one of a reaction product of one or more selected from the group consisting of silicates and reaction products of silicates, and sodium aluminate or aluminum hydroxide.
6. A casting mold made of the inorganic coated sand according to any one of claims 1 to 5.
7. A method for producing a molding sand comprising the steps of: (1) mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with an aluminate or aluminum hydroxide to form a first coating layer on the surface of the aggregate, (2) mixing the obtained molding sand with a molten liquid of metasilicate hydrate to obtain a mixture, and (3) cooling the mixture to a temperature below the melting point of the metasilicate hydrate, wherein the refractory aggregate (B) is SiO 2The method for producing inorganic coated sand comprises:
8. A method for producing molding sand comprising the steps of: (4) mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with an aluminate or aluminum hydroxide to form a first coating layer on the surface of the aggregate to obtain molding sand; and (5) mixing the obtained molding sand with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate, wherein the refractory aggregate (B) is SiO 2 The method for producing inorganic coated sand comprises:
9. A method for producing inorganic coated sand according to claim 7 or 8, wherein in step (1) or (4), the first coating layer is formed by heating the sand to a temperature of 25°C or higher and lower than 400°C.
10. A method for improving the storage stability of inorganic coated sand, comprising: foundry sand containing one or two aggregates selected from reclaimed sand (A) and refractory aggregate (B); and a second coating layer containing metasilicate that coats the foundry sand, wherein the refractory aggregate (B) is SiO 2 and preparing a dry inorganic coated sand so that the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.
Citation Information
Patent Citations
Thermal regeneration of foundry sand
JP2010519042A
Coated sand production method, coated sand obtained by the same, and cast production method
JP2014117740A
Method for producing a particulate refractory composition for use in the production of foundry moulds and cores, corresponding uses and regenerating mixtures for heat treatment - Patents.com
JP2021536367A
Porous masses or moulded bodies consisting of inorganic polymers and production thereof
US20160068440A1
Particulate refractory compositions for use in the manufacture of foundry moulds and cores, methods of preparing same and corresponding uses