Thermally conductive sheet
The thermally conductive sheet, made from a silicone composition with specific components, addresses the need for low assembly stress and resilience by achieving a balance in compressibility and restorability, ensuring effective heat dissipation and adaptability in automotive applications.
Patent Information
- Application Number
- PCT/JP2024/017187
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-21
AI Technical Summary
Thermally conductive sheets used in automotive environments face challenges in achieving a low maximum stress during assembly while maintaining resilience to follow component fluctuations due to vehicle vibration, requiring a balance between compressibility and restorability.
A thermally conductive sheet composed of a silicone composition containing an organopolysiloxane with 2 to 10 alkenyl groups, organohydrogenpolysiloxane, thermal conductive filler, platinum-based curing catalyst, and dimethylpolysiloxane with a trialkoxysilyl group, which achieves a hardness of 7 or less, maximum stress of 0.7 MPa or less, and residual stress of 0.1 MPa or more, with a ratio of maximum to residual stress of 7/1 or less, ensuring excellent thermal conductivity and balance between compressibility and restorability.
The sheet provides a balance between ease of crushing and resilience, allowing it to effectively dissipate heat and adapt to component movements, making it suitable for various in-vehicle electrical components with improved thermal conductivity and reduced stress differences.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Thermally conductive sheet
[0001] The present invention relates to a thermally conductive sheet.
[0002] Due to the miniaturization and high integration of electronic components, thermally conductive sheets are required to have not only excellent thermal conductivity but also softness that reduces maximum stress during assembly and minimizes load on heat-generating components. Patent Document 1 proposes a sheet that can conform to electronic components with low load by specifying the average particle size of the thermally conductive filler. Patent Document 2 reports an example in which the flexibility is improved and the compressive load is reduced by providing irregularities on the surface of the thermally conductive sheet. Patent Document 3 proposes a sheet with excellent flexibility that exhibits a compressive residual stress of 0.1 MPa or less by specifying the viscosity of the polymer component.
[0003] However, for various electronic components for automotive use, while a low maximum stress during assembly is preferable, they also need to have the resilience (a certain level of residual stress) to accommodate fluctuations in the clearance between the thermally conductive sheet and the electronic components caused by vehicle vibrations after installation.In other words, thermally conductive sheets used in automotive environments need to have a small difference between maximum stress and residual stress, and must be both easy to crush and have the right amount of resilience due to rubber elasticity, and further improvement was needed in this regard.
[0004] Japanese Patent Application Laid-Open No. 2003-253136 Japanese Patent Application Laid-Open No. 2001-217360 Japanese Patent No. 6705067
[0005] The present invention aims to provide a thermally conductive sheet that has excellent thermal conductivity, a small difference between maximum stress and residual stress, and a good balance of compressibility and recovery properties, making it suitable for use as a heat dissipation member for a wide range of automotive electrical equipment.
[0006] The present invention has been made to solve the above problems, and provides the following thermally conductive sheet.
[0007] That is, the present invention provides a thermally conductive sheet comprising a cured product of a silicone composition comprising: (a) 100 parts by mass of an organopolysiloxane having 2 to 10 alkenyl groups only on molecular side chains; (b) an organohydrogenpolysiloxane having hydrosilyl groups at both terminals, in an amount such that the number of moles of hydrosilyl groups is in the range of 0.75 to 1.3 of the number of moles of alkenyl groups derived from component (a); (c) 1,000 to 4,200 parts by mass of a thermally conductive filler; (d) a platinum-based curing catalyst, in an amount calculated as 0.1 to 1,000 ppm by weight of platinum group element relative to component (a); and (e) 15 to 200 parts by mass of a dimethylpolysiloxane having one terminal blocked with a trialkoxysilyl group, wherein the hardness of the thermally conductive sheet as measured with an Asker C hardness scale is 7 or less; The thermal conductive sheet is characterized in that when the thermal conductive sheet having an initial thickness of 1.5 mm is compressed 50% at a compression speed of 3 mm / min, the maximum stress is 0.7 MPa or less, the residual stress is 0.1 MPa or more, and the ratio of the maximum stress to the residual stress is 7 / 1 or less.
[0008] Such a thermally conductive sheet has excellent thermal conductivity, a small difference between the maximum stress and the residual stress, and a good balance between compressibility and restorability.
[0009] The thermally conductive filler (c) is preferably one or more selected from aluminum oxide, aluminum hydroxide, magnesium oxide, and aluminum nitride.
[0010] A thermally conductive sheet using such a thermally conductive filler has good thermal conductivity and filling properties.
[0011] The shape of the thermally conductive filler (c) may be crushed, rounded, or spherical.
[0012] The average particle size of the thermally conductive filler (c) is preferably 0.5 to 100 μm.
[0013] Those having an average particle size of 0.5 to 10 μm or crushed or rounded shapes can form an efficient heat conduction path, thereby increasing the thermal conductivity.
[0014] In this case, the thermal conductivity is preferably 2.0 W / mK or more.
[0015] If the thermal conductivity of the thermally conductive sheet is 2.0 W / mK or more, the thermally conductive sheet can be applied to a heat generating element that generates a large amount of heat.
[0016] According to the present invention, by appropriately crosslinking an organopolysiloxane having alkenyl groups only on the molecular side chains with an organohydrogenpolysiloxane having hydrosilyl groups at both ends, it is possible to achieve an appropriate crosslink density and obtain a silicone polymer that maintains good compressibility and residual stress. Furthermore, by blending a thermally conductive filler that imparts thermal conductivity with a surface treatment agent having a trialkoxy group at one end, the interaction between the filler surface and the polymer is strengthened, thereby improving residual stress. Such a sheet has an excellent balance between maximum stress and residual stress, making it suitable for use in various electronic components for automotive applications.
[0017] The present inventors have searched for a silicone composition that exhibits a small difference between maximum stress and residual stress, which is required for a thermally conductive sheet, and that combines ease of crushing with rebound characteristics due to appropriate rubber elasticity. They have found that the above-mentioned object can be achieved by a silicone composition comprising an organopolysiloxane having 2 to 10 alkenyl groups only on the molecular side chains, an organohydrogenpolysiloxane having hydrosilyl groups at both ends, a thermally conductive filler, a platinum-based curing catalyst, and a dimethylpolysiloxane having one end capped with a trialkoxysilyl group, wherein the thermally conductive sheet has a hardness of 7 or less as measured with an Asker C hardness tester, and when the thermally conductive sheet has an initial thickness of 1.5 mm and is compressed 50% at a compression rate of 3 mm / min, the maximum stress is 0.7 MPa or less, the residual stress is 0.1 MPa or more, and the ratio of the maximum stress to the residual stress is 7 / 1 or less, and thus have completed the present invention. Each component will be explained below.
[0018] (a) Organopolysiloxanes Having 2 to 10 Alkenyl Groups Only in Side Chains of the Molecular Chain The alkenyl-group-containing organopolysiloxane of component (a) contains 2 to 10 alkenyl groups only in the side chain portion of each molecule, and is generally a straight-chain organopolysiloxane whose main chain is essentially composed of repeating diorganosiloxane units and whose molecular chain is terminated at both ends with triorganosiloxy groups. The organopolysiloxane may contain a branched structure or may be cyclic, but linear diorganopolysiloxanes are preferred in terms of physical properties such as the mechanical strength of the cured product. An example of component (a) is the structure represented by the following general formula (1): (In general formula (1), R 1 are independently a group selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms, X is an alkenyl group having 2 to 6 carbon atoms, n is 0 or an integer of 1 or more, and m is an integer of 2 or more. The bonding of the siloxane units enclosed in parentheses with m and n may be block or random.
[0019] In general formula (1), R 1 Examples of R include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, and hexyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, and xylyl; and aralkyl groups such as benzyl and 2-phenylethyl. Typical groups have 1 to 7 carbon atoms, and particularly typical groups have 1 to 5 carbon atoms, and preferred are alkyl groups such as methyl, ethyl, and propyl, and phenyl. 1 A compound in which some of the hydrogen atoms are substituted with halogen atoms such as fluorine atoms may also be used.
[0020] In general formula (1), examples of the alkenyl group represented by X include those having 2 to 6 carbon atoms, such as vinyl, allyl, propenyl, isopropenyl, butenyl, and hexenyl. Of these, vinyl and allyl are preferred, with vinyl being particularly preferred. In general formula (1), n is an integer of 0 or 1 or greater, and m is an integer of 2 to 10. Furthermore, n and m are preferably integers that satisfy 10≦n+m≦5,000, more preferably 50≦n+m≦1,000, and even more preferably 100≦n+m≦500 and 0.001≦m / (n+m)≦0.05. The bonding of the siloxane units enclosed in parentheses with m and n above may be block or random.
[0021] (b) Organohydrogenpolysiloxane The organohydrogenpolysiloxane of component (b) must have at least two, preferably two to four, hydrogen atoms directly bonded to silicon atoms (hydrosilyl groups) per molecule, with hydrosilyl groups at both ends. If the number of hydrosilyl groups is less than two, there is a risk of the product not curing. An example of an organohydrogenpolysiloxane is represented by the following general formula (2): (In general formula (2), R 1 is the same as above. o is an integer of 0 or more and less than 200, and p is an integer of 0 or more and less than 200. The bonding of the siloxane units enclosed in parentheses with o and p above may be block or random.
[0022] In the above general formula (2), R 1 As in the general formula (1) above, are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. Specific examples and preferred embodiments thereof are the same as those listed for the general formula (1) above. In the general formula (2) above, o represents an integer of 0 or more and less than 200, and p represents an integer of 0 or more and less than 200. These numerical values indicate the numerical values of the average structural formula of component (b), and are not limited at the molecular level. The bonding of the siloxane units enclosed in parentheses with o and p above may be block or random.
[0023] The amount of component (b) added is such that the ratio of hydrosilyl groups derived from component (b) is 0.75 to 1.3, preferably 0.78 to 1.25, and more preferably 0.9 to 1.2 moles per mole of alkenyl groups derived from component (a). When a sheet is formed with component (b) in this range, the difference between maximum stress and residual stress is reduced, resulting in a sheet with well-balanced compression properties.
[0024] (c) Thermally conductive filler The thermally conductive filler, which is component (c), can be a material generally considered to be a thermally conductive filler, such as a non-magnetic metal such as copper or aluminum, a metal oxide such as aluminum oxide, silicon dioxide, magnesium oxide, beryllium oxide, titanium oxide or zirconium oxide, a metal nitride such as aluminum nitride, silicon nitride or boron nitride, a metal hydroxide such as aluminum hydroxide or magnesium hydroxide, artificial diamond or silicon carbide.
[0025] In particular, from the viewpoint of thermal conductivity and filling ability with silicone, it is preferable to use aluminum oxide, aluminum hydroxide, magnesium oxide, and aluminum nitride. These thermally conductive fillers preferably have an average particle size of 0.5 to 100 μm, more preferably 1 to 80 μm. These fillers may be used alone or in combination. It is also possible to use two or more types of particles with different average particle sizes. The particle size of the thermally conductive filler is measured using a laser diffraction / scattering particle size distribution analyzer, such as the Microtrac MT3300EX (Nikkiso), and the average particle size is a volume-based value (when measuring the volume distribution of particles, the particle size is divided into two at the average particle size, and the larger and smaller particles are equal in size).
[0026] The thermally conductive filler preferably has a crushed, rounded, or spherical shape, and a combination of different shapes can be used. In particular, those with an average particle size of 10 to 100 μm are preferably spherical from the perspective of packing properties, while those with an average particle size of 0.5 to 10 μm are preferably crushed or rounded because they penetrate between larger particle size fillers and efficiently form heat conduction paths. In the present invention, "spherical" refers to a thermally conductive filler with an aspect ratio of 1.5 or less, and "crushed" or "rounded" refers to a thermally conductive filler with an aspect ratio of more than 1.5. Furthermore, "crushed" refers to the inclusion of angular portions, and "rounded" refers to a rounded shape.
[0027] The blending amount of component (c) must be 1,000 to 4,200 parts by mass, preferably 1,500 to 3,800 parts by mass, per 100 parts by mass of component (a). If this blending amount is less than 1,000 parts by mass, the resulting composition will have poor thermal conductivity and the thermal conductive sheet will have poor storage stability. On the other hand, if it exceeds 4,200 parts by mass, the sheet will become hard and brittle, the maximum stress will increase, and high compression will be difficult.
[0028] (d) Platinum-based curing catalyst The platinum-based curing catalyst of component (d) is a catalyst for promoting the addition reaction between the alkenyl group derived from component (a) and the Si—H group derived from component (b), and examples thereof include platinum-based catalysts well known as catalysts used in hydrosilylation reactions. Specific examples thereof include platinum group metals such as platinum (including platinum black), rhodium, and palladium; 2 PtCl 4 ・nH 2 O, H 2 PtCl 6 ・nH 2 O, NaHPtCl 6 ・nH 2 O, KHPtCl 6 ・nH 2 O, Na 2 PtCl 6 ・nH 2 O.K. 2 PtCl 4 ・nH 2 O, PtCl 4 ・nH 2 O, PtCl 2, Na 2 HPtCl 4 ・nH 2 O (wherein n is an integer of 0 to 6, preferably 0 or 6), chloroplatinic acid and chloroplatinate salts, alcohol-modified chloroplatinic acid (see U.S. Pat. No. 3,220,972), complexes of chloroplatinic acid with olefins (see U.S. Pat. Nos. 3,159,601, 3,159,662 and 3,775,452), platinum black, platinum group metals such as palladium supported on a support such as alumina, silica or carbon, rhodium-olefin complexes, chlorotris(triphenylphosphine)rhodium (Wilkinson's catalyst), complexes of platinum chloride, chloroplatinic acid or chloroplatinate salts with vinyl group-containing siloxanes, particularly vinyl group-containing cyclic siloxanes. The amount of component (d) used is 0.1 to 1,000 ppm, preferably 1 to 500 ppm, calculated as the volume of platinum group metal element relative to component (a).
[0029] (e) Dimethylpolysiloxane having one end capped with a trialkoxysilyl group Component (e) dimethylpolysiloxane having one end capped with a trialkoxysilyl group is used as a surface treatment agent. Specifically, it can be represented by the following general formula (3):
[0030] In the above general formula, R2 is independently an alkyl group having 1 to 6 carbon atoms, preferably a methyl group or an ethyl group. q is an integer from 5 to 100, preferably an integer from 10 to 60. The amount of component (e) added is 15 to 200 parts by mass, preferably 30 to 150 parts by mass, per 100 parts by mass of component (a). If the amount of component (e) is less than 15 parts by mass, the wettability of the thermally conductive filler (component (c)) with the polymer is poor, resulting in difficulties in the formability of the sheet and the maximum stress during compression. On the other hand, if the amount exceeds 200 parts by mass, oil separation is likely to occur, the storage stability of the material is poor, and the residual stress during compression is reduced.
[0031] [Other Optional Components] In addition to the above, it is possible to add effective amounts of various additives for improving functionality, such as a reaction control agent for adjusting the curing rate, a pigment or dye for coloring, a flame retardant, an internal release agent for facilitating release from a mold or separator film, and a plasticizer for adjusting the viscosity of the composition or the hardness of a molded product.
[0032] Examples of the reaction inhibitor and plasticizer are given below, but the present invention is not limited to these.
[0033] [(f) Plasticizer] The composition of the present invention further contains, as a plasticizer (f), a compound represented by the following general formula (4): (R 6 are each independently a monovalent hydrocarbon group having 1 to 8 carbon atoms and containing no aliphatic unsaturated bonds, and d is an integer of 5 to 2,000, and have a kinematic viscosity of 10 to 100,000 mm at 25°C as measured with a Cannon-Fenske viscometer. 2 The thermally conductive composition may contain an organopolysiloxane having the formula (I) / s. The component is not particularly limited as long as it is used appropriately to impart properties such as viscosity modifier to the thermally conductive composition. One type may be used alone, or two or more types may be used in combination.
[0034] The above R 6 are each independently a monovalent hydrocarbon group having 1 to 8 carbon atoms and containing no aliphatic unsaturated bonds, and are specifically selected from an alkyl group having 1 to 8 carbon atoms, an aryl group having 6 to 8 carbon atoms, and an aralkyl group having 7 to 8 carbon atoms. Examples include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, and octyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, and xylyl; and aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl. Preferred are methyl, ethyl, propyl, and phenyl, and particularly preferred are methyl and phenyl.
[0035] The kinematic viscosity of the organopolysiloxane at 25°C measured with a Canon-Fenske viscometer is preferably 10 to 100,000 mm 2 / s, and particularly preferably 100 to 10,000 mm 2 / s. The kinematic viscosity is 10 mm 2 If the kinematic viscosity is 100,000 mm / s or more, the resulting cured product of the composition will not exhibit oil bleeding. 2 / s or less, the resulting thermally conductive composition has good flexibility. In the above general formula (4), d may be any value that allows the kinematic viscosity of the organopolysiloxane to fall within the above-mentioned range. It is preferably an integer of 5 to 2,000, and more preferably an integer of 10 to 1,000.
[0036] The amount of component (f) in the composition of the present invention is not particularly limited, as long as it is an amount that achieves the desired effect as a plasticizer. Typically, it is preferably 1 to 20 parts by mass, and more preferably 2 to 10 parts by mass, per 100 parts by mass of component (a). When the amount of component (f) is within the above range, the thermally conductive composition before curing tends to maintain good fluidity and workability, and it also becomes easier to fill the composition with the thermally conductive filler of component (c).
[0037] [(g) Reaction Retardant] The reaction retardant (g) can be any known addition reaction retardant used in ordinary addition reaction curable silicone compositions. Examples include acetylene compounds such as 1-ethynyl-1-hexanol and 3-butyn-1-ol, various nitrogen compounds, organic phosphorus compounds, oxime compounds, and organic chloro compounds. The amount used is preferably about 0.01 to 1 part by mass.
[0038] [Viscosity of Composition] The viscosity of the thermally conductive silicone composition of the present invention at 25°C is preferably 500 Pa·s or less, more preferably 350 Pa·s or less. Within this range, the thermally conductive silicone composition can be discharged using a pump, allowing for good yields of thermally conductive sheets. A viscosity of 300 Pa·s or less is particularly preferred, as this improves moldability. There are no particular restrictions on the lower limit of the viscosity, but it is usually around 10 Pa·s. The viscosity is measured using a modular rheometer, MARS40, manufactured by HAAKE.
[0039] [Method for producing a thermally conductive sheet] A thermally conductive sheet can be obtained by applying the thermally conductive silicone composition of the present invention to a substrate such as a resin film and curing it. The resin film can be selected appropriately from those that can withstand heat treatment after lamination and have a heat distortion temperature of 100°C or higher, such as PET, PBT, and polycarbonate films. The coating device used to apply the organohydrogenpolysiloxane oil to the resin film in a uniform thickness can be a post-metering blade coater, gravure coater, kiss roll coater, spray coater, or the like.
[0040] The curing conditions may be the same as those for known addition reaction curable silicone rubber compositions, and the composition may be cured at room temperature, or may be heated as necessary. The curing is preferably carried out at 100°C to 150°C for 1 to 40 minutes, and more preferably at 110 to 130°C for 10 to 20 minutes.
[0041] [Hardness of Thermally Conductive Sheet] The hardness of the thermally conductive sheet of the present invention, measured at 25°C with an Asker C hardness tester, is preferably 7 or less, more preferably 5 or less. If the hardness exceeds 7, it is difficult to obtain the desired good maximum stress. The lower limit of the hardness is not particularly specified, but can be 1 or more.
[0042] [Thermal Conductivity of Thermally Conductive Sheet] The thermal conductivity of the molded body of the present invention is desirably 2.0 W / m-K or more, more preferably 2.5 W / m-K or more, as measured at 25°C by the hot disc method. If the thermal conductivity is 2.0 W / m-K or more, it can be applied to a heat generating body with a large amount of heat generation. The upper limit of the thermal conductivity is preferably as high as possible, but can be set to 5.0 W / m-K.
[0043] [Compressive Stress of Thermally Conductive Sheet] The compressive stress of the thermally conductive sheet of the present invention was measured using an autograph manufactured by Shimadzu Corporation. This device is equipped with a sample stage and a compression load cell. The thermally conductive sheet is sandwiched between aluminum plates of a specified size, placed on the stage, and compressed to a specified thickness using the load cell. The maximum stress at 50% compression and the residual stress after stress relaxation by holding the sheet compressed for one minute were measured for an initial thickness of 1.5 mm. The detailed measurement conditions are described below.
[0044] [Measurement conditions] Sample: Round (diameter: 32 mm, thickness: 1.5 mm) Aluminum plate size: Round (diameter: 32 mm, thickness: 2.0 mm) Compression amount: 50% Compression speed: 3 mm / min Compression method: Trigger method (After detecting a load of 2 N, the compression amount is counted)
[0045] In the present invention, when the thermally conductive sheet having an initial thickness of 1.5 mm is compressed 50% at a compression rate of 3 mm / min, the maximum stress is 0.7 MPa or less, although the lower limit can be 0.1 MPa. The residual stress under the above compression conditions is 0.1 MPa or more, although the upper limit can be 0.7 MPa. Furthermore, the thermally conductive sheet of the present invention has a ratio of the maximum stress to the residual stress of 7 / 1 or less, although the lower limit can be 1. This results in a thermally conductive sheet with a small difference between the maximum stress and the residual stress, and a good balance between compressibility and recovery. Therefore, it can be used for various electronic components, such as those for automotive applications.
[0046] The present invention will be specifically explained below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0047] [Preparation of Composition] The components (a) to (f) used in the following examples and comparative examples are shown below: Component (a): Alkenyl group-containing organopolysiloxane
[0048] Component (b): organohydrogenpolysiloxane
[0049] (c) Component: Thermally conductive filler having the following average particle size: (c-1) Average particle size: 1 μm: aluminum hydroxide (c-2) Average particle size: 8 μm: aluminum hydroxide (c-3) Average particle size: 50 μm: aluminum hydroxide (c-4) Average particle size: 1 μm: alumina (c-5) Average particle size: 10 μm: alumina (c-6) Average particle size: 45 μm: alumina (c-7) Average particle size: 75 μm: alumina The above average particle sizes were measured using a Microtrac MT3300EX (Nikkiso).
[0050] Component (d): 5% chloroplatinic acid 2-ethylhexanol solution
[0051] (e) Ingredients:
[0052] Component (f): Dimethylpolysiloxane as a plasticizer.
[0053] Component (g): 3-butyn-2-ol as an addition reaction inhibitor
[0054] [Examples 1 to 6 and Comparative Examples 1 to 6] Components (a), (c), (e), and (f) were added in the specified amounts shown in Tables 1 and 2 and kneaded for 60 minutes using a planetary mixer. Components (d) and (g) were then added in the specified amounts shown in Tables 1 and 2, and an effective amount of an internal release agent that promotes release from the separator was added, followed by kneading for an additional 30 minutes. Component (b) was then added in the specified amount shown in Tables 1 and 2, and kneaded for 30 minutes to obtain a composition.
[0055] [Method of Molding Thermally Conductive Sheet] The resulting composition was poured into a mold of 60 mm x 60 mm x 6 mm or a mold of 170 mm x 130 mm x 1.5 mm and molded at 110°C for 10 minutes using a press molding machine.
[0056] [Evaluation Methods] Hardness: Each of the compositions obtained in Examples 1 to 6 and Comparative Examples 1 to 6 was cured into a 6 mm thick sheet, and two of the sheets were stacked and measured using an Asker C hardness tester. The results are shown in Tables 1 and 2.
[0057] Thermal conductivity: The compositions obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were cured into sheets having a thickness of 6 mm, and the thermal conductivity of two of these sheets was measured using a thermal conductivity meter (TPA-501, product name, manufactured by Kyoto Electronics Manufacturing Co., Ltd.) The results are shown in Tables 1 and 2.
[0058] Compressive stress: The compositions obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were cured into sheets having a thickness of 1.5 mm, and the maximum stress and residual stress at 50% compression were measured under the conditions described above using an autograph manufactured by Shimadzu Corporation. The results are shown in Tables 1 and 2.
[0059]
[0060]
[0061] In Examples 1 to 6, thermally conductive sheets were molded within the ranges described in the present invention, exhibiting good thermal conductivity and a ratio of maximum stress to residual stress at 50% compression of 7 / 1 or less, providing heat dissipation components suitable for automotive electronic components, etc. In Comparative Example 1, the ratio (H / Vi) of the number of moles of hydrosilyl groups derived from component (b) to the number of moles of vinyl groups derived from component (a) exceeded 1.3, resulting in an increased maximum stress of the sheet and making high compression difficult. In Comparative Example 2, the H / Vi was below 0.75, resulting in a residual stress of the sheet below 0.1 MPa and difficulty in restoring the sheet. In Comparative Example 3, the amount of thermally conductive filler exceeded 4,200 parts by mass, resulting in a maximum stress of the sheet above 0.7 MPa and difficulty in compressibility. In Comparative Example 4, the amount of thermally conductive filler was below 1,000 parts by mass, resulting in poor thermal conductivity of the sheet and making it difficult to apply to high-heat-generating elements. In Comparative Example 5, the amount of the surface treatment agent was less than 15 parts by mass, so the maximum stress of the sheet was high and high compression was difficult.In Comparative Example 6, the amount of the surface treatment agent was more than 200 parts by mass, so the residual stress of the sheet was low and there was a problem with recovery.
[0062] This specification encompasses the following aspects. [1]: A thermally conductive sheet comprising a cured product of a silicone composition comprising: (a) 100 parts by mass of an organopolysiloxane having 2 to 10 alkenyl groups only on molecular side chains; (b) an organohydrogenpolysiloxane having hydrosilyl groups at both terminals, in an amount such that the number of moles of hydrosilyl groups is in the range of 0.75 to 1.3 of the number of moles of alkenyl groups derived from component (a); (c) 1,000 to 4,200 parts by mass of a thermally conductive filler; (d) a platinum-based curing catalyst, in an amount calculated as 0.1 to 1,000 ppm by weight of platinum group elements relative to component (a); and (e) 15 to 200 parts by mass of a dimethylpolysiloxane having one terminal blocked with a trialkoxysilyl group, wherein the thermally conductive sheet has a hardness of 7 or less as measured with an Asker C hardness scale. A thermally conductive sheet characterized in that, when the thermally conductive sheet having an initial thickness of 1.5 mm is compressed 50% at a compression rate of 3 mm / min, the maximum stress is 0.7 MPa or less, the residual stress is 0.1 MPa or more, and the ratio of the maximum stress to the residual stress is 7 / 1 or less. [2]: The thermally conductive sheet according to [1], characterized in that the thermally conductive filler (c) is one or more selected from aluminum oxide, aluminum hydroxide, magnesium oxide, and aluminum nitride. [3]: The thermally conductive sheet according to [1] or [2], characterized in that the shape of the thermally conductive filler (c) is crushed, rounded, or spherical. [4]: The thermally conductive sheet according to any one of [1] to [3], characterized in that the average particle size of the thermally conductive filler (c) is 0.5 to 100 μm. [5]: The thermally conductive sheet according to any one of [1] to [4], characterized in that the thermal conductivity is 2.0 W / m-K or more.
[0063] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.
Claims
1. A thermally conductive sheet comprising a cured product of a silicone composition comprising: (a) an organopolysiloxane having 2 to 10 alkenyl groups only on the molecular chain side chains: 100 parts by mass; (b) an organohydrogenpolysiloxane having hydrosilyl groups on both ends: an amount such that the number of moles of hydrosilyl groups is in the range of 0.75 to 1.3 of the number of moles of alkenyl groups derived from component (a); (c) a thermally conductive filler: 1,000 to 4,200 parts by mass; (d) a platinum-based curing catalyst: 0.1 to 1,000 ppm in terms of the weight of platinum group elements relative to component (a); and (e) a dimethylpolysiloxane having one end blocked with a trialkoxysilyl group: 15 to 200 parts by mass, wherein the hardness of the thermally conductive sheet as measured with an Asker C hardness scale is 7 or less, A thermally conductive sheet characterized in that, when the thermally conductive sheet having an initial thickness of 1.5 mm is compressed 50% at a compression speed of 3 mm / min, the maximum stress is 0.7 MPa or less, the residual stress is 0.1 MPa or more, and the ratio of the maximum stress to the residual stress is 7 / 1 or less.
2. The thermally conductive sheet according to claim 1, wherein the thermally conductive filler (c) is at least one selected from the group consisting of aluminum oxide, aluminum hydroxide, magnesium oxide, and aluminum nitride.
3. The thermally conductive sheet according to claim 1, characterized in that the shape of the thermally conductive filler (c) is crushed, rounded, or spherical.
4. The thermally conductive sheet according to claim 1, characterized in that the average particle size of the thermally conductive filler (c) is 0.5 to 100 μm.
5. The thermally conductive sheet according to claim 1, characterized in that the thermal conductivity is 2.0 W / m-K or more.
Citation Information
Patent Citations
Flexible heat-radiation spacer
JP2001217360A
Heat conductive sheet
JP2003253136A
Thermally conductive sheet and manufacturing method thereof
JP6705067B1
Platinum-olefin complex catalyzed addition of hydrogen- and alkenyl-substituted siloxanes
US3159601A
Addition reaction
US3159662A