Method for recovering battery material from used battery

The method employs a neutralization reaction between lithium hydroxide and acid to efficiently recycle lithium-ion battery cathode materials, addressing inefficiencies and environmental concerns of existing methods by eliminating the need for separate pretreatment and purification, and achieving cost-effective and environmentally friendly recycling.

WO2024237578A1PCT designated stage expired Publication Date: 2024-11-21EASYMINING CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006328
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-01-16
Filing Date
2024-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods for recycling lithium-ion battery cathode materials require separate pretreatment processes, wastewater purification facilities, and high investment costs, making them inefficient and environmentally unfriendly.

Method used

A method involving the use of a neutralization reaction between an aqueous lithium hydroxide solution and acid to recover aluminum and other materials from used batteries, eliminating the need for separate pretreatment and purification facilities, and achieving efficient recycling through a simple process without heat treatment.

Benefits of technology

This method effectively recycles aluminum and other materials at low cost and high efficiency, reducing energy consumption and environmental impact by avoiding harmful gas and wastewater generation, and enabling Al separation and relithiation in a single step.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006328_21112024_PF_FP_ABST
    Figure KR2024006328_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for recovering a battery material from a used battery by utilizing a neutralization reaction between an aqueous lithium hydroxide solution and an acid.
Need to check novelty before this filing date? Find Prior Art

Description

Method for recovering battery materials from used batteries

[0001] The present invention relates to a method for recovering battery materials from used batteries, and more particularly, to a method for recovering battery materials from used batteries by utilizing a neutralization reaction between an aqueous lithium hydroxide solution and an acid.

[0002] Driven by global greenhouse gas reduction policies, the electric vehicle (EV) industry is rapidly developing. The use of energy storage systems (ESS) linked to renewable energy sources is also increasing significantly, driving a significant increase in demand for lithium-ion batteries (LIBs). Typically, LIBs are disposed of after approximately 10 years of use, as their capacity diminishes. The generation of spent lithium-ion batteries is also expected to surge in the future.

[0003] Accordingly, interest in the processing and recycling of used batteries has increased, and various studies have been conducted on technologies for recycling aluminum and NCM materials from the cathodes of used batteries.

[0004] There are two representative methods for separating and extracting Al and NCM from the cathode materials of these used batteries: wet and dry methods.

[0005] In the case of the wet method, as shown in Figure 1, the used cathode material is dissolved in acid and then the valuable metal is extracted through a chemical reaction, but there was a disadvantage in that a separate wastewater purification facility was required and pretreatment with black powder was required.

[0006] In the case of the dry method, as shown in Figure 2, the valuable metal is extracted by melting at a high temperature. However, in the case of Li, most of it is volatile, and it is difficult to recover metals other than Co and Ni. If separate gas treatment is required, there is a disadvantage in that a high investment cost is required.

[0007] Accordingly, there is a need for a new method of recycling cathode materials that does not require a separate pretreatment process or purification facility and can reduce investment costs.

[0008] [Patent Document]

[0009] (Patent Document 1) Korean Patent Publication No. 10-2403455

[0010] The purpose of the present invention is to recover aluminum from used batteries with high efficiency, fast process, and low cost, and to remanufacture the aluminum through insertion of Li into the cathode.

[0011] The purposes of the present invention are not limited to those mentioned above, and other purposes not mentioned will be clearly understood from the description below.

[0012] A method for recovering a battery material according to one embodiment of the present invention comprises the steps of: 1) preparing a cathode powder containing Al, NCM, and C6; 2) immersing the cathode powder in a LiOH aqueous solution to prepare an aqueous solution; 3) filtering the prepared aqueous solution to separate a LiOH aqueous solution containing dissolved Al ions and a solid phase containing NCM and C6; and 4) adding an acid to the LiOH aqueous solution, and then filtering and drying the solution to obtain Al powder and Li compound powder.

[0013] In the above step 2), the molar concentration of the LiOH aqueous solution may be 1 M to 4 M.

[0014] After the above step 3), the solid phase may be separated into NCM and C6 through a floating process.

[0015] In the above step 4), the Al powder and the Li compound aqueous solution may be separated through a neutralization reaction treatment.

[0016] In the above step 4), the acid may be at least one acid selected from the group consisting of acids capable of neutralization reaction, such as hydrochloric acid, sulfuric acid, and acetic acid.

[0017] In the above step 4), the concentration of the acid may be 0.1 to 1 M.

[0018] In the above step 4), acid can be added until the pH of the aqueous solution is adjusted to 5 to 6.

[0019] The method for recovering battery materials of the present invention has the effect of recovering positive electrode materials such as aluminum from used batteries at low cost and high efficiency through a simple process and recycling them.

[0020] In addition, the method for recovering battery materials of the present invention is environmentally friendly because it does not use heat treatment, so no harmful gases are generated, and no acid-base wastewater is generated through a neutralization reaction.

[0021] In addition, compared to existing technologies, existing technologies go through a Li insertion process through ball milling and high-temperature heat treatment after separating the Al electrode and cathode material, but the battery material recovery method of the present invention enables Al separation and relithiation in one step, thereby reducing energy consumption, time, and cost incurred during process operation.

[0022] The technical effects of the present invention are not limited to those mentioned above, and other technical effects not mentioned will be clearly understood by those skilled in the art from the description below.

[0023] Figure 1 illustrates a process flow diagram of a method for recovering a cathode material among battery materials according to conventional technology.

[0024] Figure 2 illustrates another process flow chart of a method for recovering a cathode material among battery materials according to the prior art.

[0025] Figure 3 is a schematic diagram illustrating a process of a method for recovering battery materials according to one embodiment of the present invention.

[0026] Figure 4 is a schematic diagram showing the mechanism of a reaction according to one embodiment of the present invention.

[0027] Figure 5 is a comparative XRD graph before and after Al extraction through a LiOH solution immersion method according to one embodiment of the present invention.

[0028] Figure 6 is an XRD graph showing an Al aqueous solution obtained after immersion according to one embodiment of the present invention, extracted in salt form through a neutralization reaction, and then analyzed.

[0029] Figure 7 is a graph showing a LiOH leaching process performed to remove residual Al from a cathode material extracted with Al by a LiOH solution immersion method according to one embodiment of the present invention, followed by XRD analysis.

[0030] Figure 8 is an XRD graph showing that Al appears to have been removed as a result of dissolving a 60Ah cathode material and graphite mixture in a 4M LiOH aqueous solution according to one embodiment of the present invention.

[0031] FIG. 9 is an XRD graph showing that Al appears to have been removed as a result of dissolving a 60Ah cathode material and graphite mixture in a 1M LiOH aqueous solution according to one embodiment of the present invention.

[0032] Figure 10 is a graph showing the results of XRD analysis of a LiCl aqueous solution obtained after neutralization using HCl in an Al saturated aqueous solution from which a cathode material was separated according to one embodiment of the present invention.

[0033] Figure 11 is a graph showing that Al(OH)3 and Al compounds are generated after a neutralization reaction using HCl in an Al saturated aqueous solution from which a cathode material is separated according to one embodiment of the present invention.

[0034] Figure 12 is a graph showing the results of measuring Al saturation according to LiOH molar concentration of a battery material according to one embodiment of the present invention.

[0035] Figure 13 is a graph showing changes in the solubility of Al according to pH according to one embodiment of the present invention.

[0036] Hereinafter, embodiments of the present invention will be described in detail to facilitate easy implementation by those skilled in the art. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein. Furthermore, like reference numbers represent like elements throughout the specification.

[0037]

[0038] Figure 3 illustrates a process flow diagram of a method for recovering battery materials according to one embodiment of the present invention.

[0039] Referring to FIG. 3, a method for recovering a battery material according to an embodiment of the present invention includes: 1) preparing a cathode powder containing Al, NCM, and C6; 2) immersing the cathode powder in a LiOH aqueous solution to prepare an aqueous solution; 3) filtering the prepared aqueous solution to separate the LiOH aqueous solution containing dissolved Al ions and a solid phase containing NCM and C6; and 4) adding an acid to the LiOH aqueous solution, and then filtering and drying the solution to obtain Al powder and LiCl powder.

[0040]

[0041] A method for recovering battery materials according to one embodiment of the present invention includes step 1) of preparing cathode powder containing Al, NCM, and C6.

[0042] Step 1 above prepares cathode powder obtained from the spent battery, thereby preparing recyclable materials among the remaining cathode materials in the spent battery. The spent battery may include a lithium transition metal oxide, C6, as a cathode material, and aluminum foil (Al foil) as a cathode substrate.

[0043]

[0044] A method for recovering a battery material according to one embodiment of the present invention includes step 2) of preparing an aqueous solution by immersing the cathode material powder in a LiOH aqueous solution.

[0045] Referring to FIG. 3, the cathode powder is immersed in a LiOH aqueous solution, thereby ionizing and dissolving the Al contained in the cathode powder, and inserting Li ions into the cathode. That is, this is a process in which cathode powder separated from a used battery is immersed in a LiOH solution, thereby dissolving and separating Al, and simultaneously inserting Li into the NCM. In step 2), the molar concentration of the LiOH aqueous solution may be 1 M to 4 M.

[0046]

[0047] Specifically, it proceeds through the following mechanisms.

[0048] First, Al in the electrode powder is dissolved into ions in a LiOH aqueous solution according to the following reaction equation.

[0049] Al + 4Li + + 4OH - ↔ Al(OH)4 - + Li + + 3e -

[0050] After this, the generated electrons and water react to produce hydroxide ions.

[0051] 3e - + H2O → 3 / 2·H2+ 3OH - (HER reaction)

[0052] Finally, the following reaction equation is completed.

[0053] Al + 4Li + + 4OH - + H2O ↔ 3 / 2·H2+ Al(OH)4 - + 3OH -

[0054]

[0055] In the above reaction formula, Al dissolves in a strong base to form Al(OH)4 - It exists in the form of electrons, water and Al(OH)4 that are created - It reacts with HER reaction (acid-base equilibrium) to produce hydrogen. Also, some Al(OH)4 - Ga Li + It reacts with and forms a precipitate (byproduct) of LiAl2(OH)7(H2O)2.

[0056] Accordingly, the following reaction equation is completed.

[0057] 2Al(OH)4- + Li + + H2O ↔ LiAl2(OH)7(H2O)2+ OH -

[0058]

[0059] The process of step 2) above can be a high-efficiency, short-time, and low-cost regeneration process compared to existing processes as a direct recovery method in the form of regenerated cathode material rather than in the form of precious metal. In addition, when the cathode powder is immersed in LiOH, Al is converted to Al(OH). 4- It dissolves into ions, and only the positive and negative electrode materials precipitate to the bottom of the solution, allowing for easy separation.

[0060]

[0061] A method for recovering a battery material according to one embodiment of the present invention includes step 3) of filtering the prepared aqueous solution to separate a LiOH aqueous solution containing dissolved Al ions and a solid phase containing NCM and C6.

[0062]

[0063] In the above step 3), the aqueous solution prepared in step 2) is filtered and washed to separate NCM, C6, and Al.

[0064] Figure 4 is a diagram disclosed in GRAHAM, Trent R., et al. Unraveling gibbsite transformation pathways into LiAl-LDH in concentrated lithium hydroxide. Inorganic chemistry, 2019, 58.18: 12385-12394. As disclosed in Figure 4, the LiAl2(OH)7(H2O)2 formation reaction is a reversible reaction in a basic solution (OH - ) and react with Li + and Al(OH)4 - It can be converted into . At this time, through the washing process during filtering of the precipitated powder (positive electrode material + negative electrode material + LiAl2(OH)7(H2O)2), LiAl2(OH)7(H2O)2 is converted into a Li aqueous solution, and is separated from the mixture into pure positive electrode material and negative electrode material.

[0065]

[0066] In addition, after the above step 3), the solid phase in which NCM and C6 are mixed can be separated into the positive electrode and C6 by using centrifugation using the density difference between the graphite and the positive electrode or by using the flotation process (froth flotation) using the difference in hydrophilicity.

[0067]

[0068] A method for recovering battery materials according to one embodiment of the present invention includes step 4) of adding acid to a LiOH aqueous solution, then filtering and drying the solution to obtain Al powder and LiCl powder.

[0069] In the above step 4), a separation process of aluminum compounds is performed using HCl neutralization reaction.

[0070] In the above step 4), Al ions (Al(OH)) dissolved in the LiOH aqueous solution4- ) can be separated by precipitating Al(OH)3 salt using HCl neutralization reaction and recovered as a recyclable raw material. At this time, the LiCl produced can also be utilized as a circulating resource.

[0071] For this purpose, in the step 4) above, LiCl, Al(OH)3 salt can be generated through a neutralization reaction by adding acid, and as a preferred example, when hydrochloric acid is used, the reaction formula is as follows.

[0072]

[0073] Li + + Al(OH)4 - + HCl = LiCl + Al(OH)3+ H2O

[0074]

[0075] In the above neutralization reaction, Al(OH)4 - The reaction is completed when the ion changes into Al(OH)3 salt.

[0076]

[0077] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.

[0078] Hereinafter, the present invention will be described in detail through examples.

[0079]

[0080] Example 1. Confirmation of aluminum dissolution

[0081] As a used battery separated from a 60Ah cell, the composition of the cathode is Li 0.3 1.52 g of anode powder having NiCoMnO2 was prepared. This was mixed with 4M LiOH (40.2816 g) and 240 mL of Di water, stirred, and then immersed for 96 hours.

[0082] After stirring at 60℃ at 200 rpm, all Al was dissolved, and the cathode materials separated from the Al foil settled to the bottom. The solution containing dissolved Al was filtered, and the filtered powder was subjected to XRD analysis.

[0083] The XRD peaks of the anode before and after immersion were measured and shown in Fig. 5.

[0084] In addition, the Al compound matching the XRD peak of the powder obtained after immersion was confirmed and compared as shown in Fig. 6. Through this, it was confirmed that the powder obtained after immersion was LiAl2(OH)7(H2O)2.

[0085]

[0086] Example 2. Confirmation of final separation of NCM and Al through filtration / cleaning

[0087] The same positive electrode powder used in Example 1 was immersed in a 4M LiOH solution. Thereafter, the precipitated powder was filtered, leached 10 times with LiOH solution, and once with water to recover the positive electrode material.

[0088] The XRD of the reference LiAl2(OH)7(H2O)2, the cathode material that was leached 10 times, and the cathode material that was not leached were measured and shown in Figure 7.

[0089] Through Fig. 7, the precipitated powder was filtered and leached 10 times with 1M LiOH solution to obtain LiAl2(OH)7(H2O). - It was found that a pure cathode material could be obtained by converting it back to the Al ion form.

[0090]

[0091] In addition, the XRD values ​​for the powder prepared by immersing the same positive electrode powder used in Example 1 in a 4M LiOH solution with stirring for 6 hours and immersing the powder in a 1M LiOH solution with stirring for 6 hours, then filtering and washing the precipitate are shown in FIGS. 8 and 9, respectively.

[0092] As a result of XRD analysis of the separated final powder, no peaks of Al or LiAl2(OH)7(H2O)2 were observed, and only peaks of a material such as graphite were found.

[0093] The positive electrode powder used in this example is a powder separated from a 60Ah cell, and exists as a mixture of positive electrode, graphite, and Al. As described above, when immersed in a high-concentration LiOH solution, only Al was dissolved, and the positive electrode and graphite sank to the bottom. Through this, it was confirmed that all residual Al was dissolved into the aqueous solution through separation and alkaline solution leaching.

[0094]

[0095] Example 3. Confirmation of separation of Al-LiOH aqueous solution

[0096] In the above Example 2, a neutralization reaction was performed by mixing 49.167 ml of 10% hydrochloric acid with 500 ml of the filtered Al saturated aqueous solution (LiOH 1 M). LiCl and AlOH3 obtained through the above reaction were separated, and their XRD peaks were measured, which are shown in Figs. 10 and 11, respectively.

[0097] Through Fig. 10, which shows the peak of LiCl, it was found that LiCl was formed through the neutralization reaction of LiOH and HCl. Through Fig. 11, which shows the peak of AlOH3, it was found that the solution that had been dissolved as AlOH4- ions after the neutralization reaction was converted to AlOH3 and Al lithium salt.

[0098]

[0099] Example 4. Aluminum dissolution according to LiOH concentration

[0100]

[0101] *The experiment was prepared in the same manner as Example 1, but the experiment was conducted by dividing it into cases where LiOH was 0 M, 0.2 M, 1 M, 2 M, and 4 M.

[0102] The Al saturation was measured according to the molar concentration of LiOH, and the data are shown in Fig. 12. As can be seen in Fig. 12, it was confirmed that the solubility of aluminum was high when the concentration of LiOH satisfied the range of 1 to 4 M.

[0103] In addition, ICP-OES data of Al saturation, which changes depending on the pH of the aqueous solution, were measured and shown in Fig. 13, and the residual dissolved amount of Al according to the change in pH is shown in Table 1 below. Fig. 13 illustrates the data described in GEORGANTAS, DA; GRIGOROPOULOU, HP Orthophosphate and metaphosphate ion removal from aqueous solution using alum and aluminum hydroxide. Journal of colloid and interface science, 2007, 315.1: 70-79.

[0104] ICP-OESpH5.5pH7pH8Calc Conc.0.105 mg / L0.253 mg / L0.125 mg / L

[0105] As shown in the above Figure 13 and Table 1, when neutralized to about pH 5.5, it was found that Al was formed as a salt and precipitated from the solution. Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.

Claims

1. 1) Step of preparing cathode powder containing Al, NCM and C6; 2) A step of preparing an aqueous solution by immersing the above cathode material powder in a LiOH aqueous solution; 3) A step of filtering the prepared aqueous solution to separate the LiOH aqueous solution containing dissolved Al ions and the solid phase containing NCM and C6; and 4) A step of adding acid to a LiOH aqueous solution, then filtering and drying it to obtain Al powder and LiCl powder; Method for recovering battery materials.

2. In paragraph 1, In the above step 2), the molar concentration of the LiOH aqueous solution is 1 M to 4 M. Method for recovering battery materials.

3. In paragraph 1, After the above step 3), the solid phase is separated into NCM and C6 by a floating process. Method for recovering battery materials.

4. In paragraph 1, In the above step 4), Al powder and LiCl powder are separated through neutralization reaction treatment. Method for recovering battery materials.

5. In paragraph 3, In the above step 4), the acid is at least one acid selected from the group consisting of hydrochloric acid, sulfuric acid, and acetic acid. Method for recovering battery materials.

6. In paragraph 1, In the above step 4), the concentration of the acid is 0.1 to 1 M, Method for recovering battery materials.

7. In paragraph 1, In the above step 4), the acid is added until the pH of the aqueous solution is adjusted to 5 to 6. Method for recovering battery materials.

Citation Information

Patent Citations

  • Method for concentrating lithium and recovering aluminum oxide by adding aluminum and sulfate source from lithum solution

    KR102054344B1

  • Air pollution prevention facility

    KR102398148B1

  • Method for recovering valuable metals and material containing zeolite from waste cathode material reaction vessel

    KR102408888B1

  • Method for enhancement of antibacterial activity of Ag nanomaterials and Ag nano article using the same

    KR102595543B1

  • KR20210150687A