Positive electrode sheet, electrode assembly, battery cell, battery, and electric device

By using two layers of active material layer structure in lithium-ion batteries, the difference in shrinkage rate and particle size distribution are optimized, and the transition layer is formed, the problem of low kinetic performance caused by the difference in shrinkage rate of active material layer in existing batteries is solved, and the problem of low kinetic performance is achieved. Improve battery dynamics and lithium ion conduction effect.

WO2024239154A1PCT designated stage expired Publication Date: 2024-11-28CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/095338
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

In existing lithium-ion secondary batteries, the difference in shrinkage rates of different materials in the active material layer leads to low kinetic performance, and the contact interface between materials is affected, resulting in a growth in the battery impedance.

Method used

The structure of at least two layers of active material layers, wherein the adjacent two layers of active material layers include the first and second positive electrode active materials, respectively, and the maximum shrinkage difference is ≥0.3%, and a transition is formed by optimizing particle size and layer thickness. layer to improve conductive network and lithium ion conduction.

Benefits of technology

It significantly improves the dynamic performance of the battery, reduces impedance growth, improves the lithium ion conduction effect, and enhances the battery's charge and discharge cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023095338_28112024_PF_FP_ABST
    Figure CN2023095338_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a positive electrode sheet, a battery, and an electric apparatus. The positive electrode sheet comprises at least two active material layers, wherein two adjacent active material layers respectively comprise a first positive active material and a second positive active material; and under the same test condition, the maximum shrinkage rate of the first positive active material during charging and discharging is T1, the maximum shrinkage rate of the second positive active material during charging and discharging is T2, and T1 and T2 satisfy the following relationship: T1-T2≥0.3%. Compared with directly physically mixing a first positive active material with a second positive active material to form a single positive active material layer, configuring a positive electrode sheet to comprise at least two positive active material layers, the maximum shrinkage rates of which satisfy T1-T2≥0.3%, is conducive to improving the deterioration of an active material conductive network caused by different frequency changes of active substances having different shrinkage rates, thereby helping to improve the dynamic performance of a battery.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode sheets, electrode assemblies, battery cells, batteries and electrical equipment Technical Field

[0001] The present application relates to a positive electrode sheet, a battery, and an electrical device. Background Art

[0002] In recent years, with the development of lithium-ion secondary battery technology, lithium-ion secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As lithium-ion secondary batteries have achieved great development, higher requirements have been placed on their dynamic performance.

[0003] Summary of the Invention

[0004] The purpose of this application is to provide a positive electrode sheet, a battery, and an electrical device.

[0005] In order to improve the energy density and safety performance of the battery, different active materials are usually mixed and used. That is, different active materials are mixed into a slurry, which is coated on the surface of the current collector to form a mixed active material layer.

[0006] The inventors of the present application discovered in experiments that when the active material layer contains different materials with greatly different shrinkage rates, the dynamic performance of the battery is relatively low. However, when materials with different shrinkage rates are layered, the dynamic performance of the battery is significantly improved.

[0007] The embodiment of the present application is implemented as follows:

[0008] In a first aspect, an embodiment of the present application provides a positive electrode sheet, the positive electrode sheet comprising at least two active material layers;

[0009] The two adjacent active material layers include a first positive electrode active material and a second positive electrode active material, respectively; the maximum shrinkage rate of the first positive electrode active material is T1, and the maximum shrinkage rate of the second positive electrode active material is T2; T1 and T2 satisfy the following relationship:

[0010] T1-T2 ≥ 0.3%;

[0011] The maximum shrinkage rate refers to the maximum change in the volume shrinkage or expansion of the unit cell of the positive electrode active material during the charge and discharge process.

[0012] Compared with a single-layer mixed positive electrode active material layer formed by directly physically mixing the first positive electrode active material and the second positive electrode active material, in the above technical solution, when the first positive electrode active material and the second positive electrode active material T1-T2 ≥ 0.3%, the positive electrode plate is provided with at least two layers of positive electrode active material layers, which can improve the deterioration of the conductive network of the active material caused by the different frequency changes of active materials with different shrinkage rates, thereby improving the battery kinetic performance.

[0013] In some optional implementation schemes, the value of T1 ranges from 1% to 7%.

[0014] In some optional implementation schemes, the value range of T1 is 3%-6.5%.

[0015] When T1 is too large, the material shrinks severely, affecting the contact interface between materials and reducing the dynamic performance. Reasonable setting of the T1 value range is conducive to improving the battery dynamic performance.

[0016] In some optional embodiments, the value of T2 ranges from 0.3% to 5.5%.

[0017] In some optional embodiments, the value of T2 ranges from 0.5% to 3%.

[0018] Among the currently available positive electrode materials, the smaller maximum shrinkage rate is mainly within this range. When used together with materials with a larger maximum shrinkage rate, the difference in material shrinkage rate is large, and the layered arrangement of the active material layer of the present application is more suitable.

[0019] In some optional embodiments, the average particle size Dv50 of the first positive electrode active material is 5 μm-15 μm.

[0020] The first positive electrode active material with the maximum shrinkage of T1 is selected as D V The size of 50 is 5μm-15μm. The larger particle size can form more pores during the charge and discharge process, which is beneficial to electrolyte infiltration and ion conduction.

[0021] In some optional embodiments, the average particle size Dv50 of the second positive electrode active material is 0.2 μm-5 μm.

[0022] The second positive electrode active material with the maximum shrinkage of T2 is selected as D V The size of 50 is 0.2μm-5μm, which is a small particle size and can cooperate with the first positive electrode active material with a larger particle size to further improve the battery charge and discharge cycle effect.

[0023] In some optional embodiments, the D of the first positive electrode active material V The value of 50 is equal to or greater than 5 times the D of the second positive electrode active material V A value of 50.

[0024] Control the D of the first positive electrode active material and the second positive electrode active material V 50 satisfies the above proportional relationship; the high mechanical strength of the active material with smaller particle size at the same compaction density will alleviate this situation to a certain extent, and the gaps between the large-size particles will not be completely filled, and the ion conduction is better than that of the mixed system. The two effects complement each other, thereby effectively improving the battery dynamics.

[0025] In some optional embodiments, the D of the first positive electrode active material V The value of 50 is equal to or greater than 5 times the D of the second positive electrode active material V 50, and less than or equal to 50 times the D of the second positive electrode active material V A value of 50.

[0026] In some optional embodiments, the D of the first positive electrode active material V The value of 50 is equal to or greater than 5 times the D of the second positive electrode active material V 50, and less than or equal to 35 times the D of the second positive electrode active material V A value of 50.

[0027] By further limiting the particle size ratio of the first positive electrode active material and the second positive electrode active material within the above range, it is beneficial to improve the excessive filling of the large particle size active material with the small particle size material when the particle size difference is too large, resulting in insufficient gaps, reduced porosity and worsened ionic impedance.

[0028] In some optional embodiments, D V 90-D V 10≤20μm; Optionally, the particle size distribution of the first positive electrode active material satisfies: 9≤D V 90-D V 10≤20μm.

[0029] The above mentioned method is to define D in the first positive electrode active material. V 90-D V 10≤20 μm, so that the active material particle size in the first positive electrode active material layer is relatively concentrated.

[0030] In some optional embodiments, D V 90-D V 10≤9μm.

[0031] The above mentioned method is to define D in the second positive electrode active material. V 90-D V 10≤9 μm, so that the active material particle size in the second positive electrode active material layer is relatively concentrated.

[0032] In some optional embodiments, any positive electrode active material layer includes multiple active materials; and the difference in maximum shrinkage of the multiple active materials does not exceed 0.3%;

[0033] T1 is the minimum value among the maximum shrinkage rates of the plurality of active materials in the first positive electrode active material;

[0034] T2 is the maximum value among a plurality of maximum shrinkage rates of a plurality of active materials in the second positive electrode active material.

[0035] By setting the maximum shrinkage of multiple active materials in any positive electrode active material layer to differ by no more than 0.3% during charge and discharge, this combination of active particles with shrinkage differences of no more than 0.3% is beneficial for improving battery impedance and dynamic performance.

[0036] In some optional embodiments, any positive electrode active material layer includes multiple active materials; the difference in maximum shrinkage of the multiple active materials exceeds 0.3%;

[0037] In terms of mass percentage, the multiple active materials include 85%-100% main active substances; 0-15% trace active substances;

[0038] T1 and T2 are the maximum shrinkage rates of the main active substance.

[0039] The same active material layer includes active particles with different shrinkage rates that differ by more than 0.3%. By maintaining the mass proportion of trace active substances between 0-15%, the negative impact of different frequency shrinkage and expansion can be reduced.

[0040] In some optional embodiments, T1-T2≥6%, the thickness of the positive electrode active material layer where the first positive electrode active material is located is H1; the thickness of the positive electrode active material layer where the second positive electrode active material is located is H2; H1:H2 is (7:3) to (1:9).

[0041] When T1-T2 ≥ 6%, when the shrinkage difference between the first positive electrode active material and the second positive electrode active material between the two layers of positive electrode active material is too large, by setting H1:H2 to (7:3) ~ (1:9), the expansion of the entire active layer can be limited, the integrity of the electrode structure can be ensured, and the rapid deterioration of dynamics (impedance) caused by changes in the electrode structure during the cycle can be slowed down.

[0042] In some optional embodiments, the positive electrode sheet includes a positive electrode current collector;

[0043] The positive electrode active material layer where the first positive electrode active material is located is close to the current collector;

[0044] The positive electrode active material layer where the second positive electrode active material is located is away from the current collector.

[0045] The first cathode active material has a larger particle size and a higher shrinkage rate, which easily forms more pores during the charge and discharge process, facilitating lithium-ion transport. The first cathode active material layer is closer to the current collector, while the second cathode active material has a smaller particle size and a lower shrinkage rate, further away from the current collector. During the charge and discharge cycle, the outer layer can somewhat limit the shrinkage and expansion of the inner layer, reducing electrode deformation, deterioration of the active material conductive network, and lowering impedance growth. At the same time, the shrinkage and expansion of the inner layer's larger particle size and larger shrinkage rate create more pores, accommodating more electrolyte than in its initial state, thus achieving a more liquid-retaining effect.

[0046] In some optional embodiments, a transition layer is formed between the positive electrode active material layer where the first positive electrode active material is located and the positive electrode active material layer where the second positive electrode active material is located.

[0047] The particle size of the active material in the first positive electrode active material is relatively large; the particle size of the active material in the first positive electrode active material is larger than that of the second positive electrode active material. The difference in particle size between the first and second positive electrode active material layers creates a transition layer between the layers where active material particles of varying sizes coexist. This improves the bonding between the active layers and improves the dynamic performance between the layers.

[0048] In some optional embodiments, the transition layer has a thickness of 0.2 μm to 2 μm.

[0049] If the thickness of the transition layer is too small or too large, it will have a negative impact on the dynamic performance of the battery. If the transition layer is too thick, it will form a structure similar to a mixed layer, affecting the dynamic performance; if the transition layer is too thin, the adhesion between the two layers will be weakened, affecting the dynamic performance.

[0050] In some optional embodiments, the second positive electrode active material includes at least one of a spinel structure positive electrode material or an olivine structure positive electrode material.

[0051] The second positive electrode active material includes at least one of a spinel structure positive electrode material and an olivine structure positive electrode material, which makes it easy to obtain a positive electrode active material layer with a smaller shrinkage rate.

[0052] In some optional embodiments, the second positive electrode active material includes LiMPO4, and M includes Mn and non-Mn elements;

[0053] Optionally, the non-Mn element includes one or both of a first doping element and a second doping element, the first doping element is a manganese doping element, and the second doping element is a phosphorus doping element;

[0054] Optionally, the first doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge;

[0055] Optionally, the first doping element includes at least two of Fe, Ti, V, Ni, Co and Mg;

[0056] Optionally, the second doping element includes one or more elements selected from B, S, Si and N;

[0057] Optionally, the second positive electrode active material includes Li 1+x Mn 1-y A y P 1-z R z O4, wherein x is any value in the range of -0.100 to 0.100, y is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and R includes one or more elements selected from the group consisting of B, S, Si, and N;

[0058] Optionally, the second positive electrode active material includes Li a A e Mn 1-f B f P 1-g C g O 4-n D n ;

[0059] wherein A comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W;

[0060] B includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb, and Ge;

[0061] C includes one or more elements selected from B, S, Si and N;

[0062] D includes one or more elements selected from the group consisting of S, F, Cl, and Br;

[0063] a is selected from the range of 0.9 to 1.1, e is selected from the range of 0.001 to 0.1, f is selected from the range of 0.001 to 0.5, g is selected from the range of 0.001 to 0.1, n is selected from the range of 0.001 to 0.1, and the second positive active material is electrically neutral.

[0064] In some optional embodiments, the first positive electrode active material includes a layered structure positive electrode material.

[0065] The first positive electrode active material includes a layered structure positive electrode material, which makes it easy to obtain a positive electrode active material layer with a large shrinkage rate.

[0066] In some optional embodiments, the first positive electrode active material includes at least one of a nickel cobalt manganese oxide ternary material, a nickel cobalt aluminum oxide ternary material, and a nickel cobalt manganese aluminum oxide ternary material, or includes at least one of doped or coated materials of the above ternary materials.

[0067] In some optional embodiments, the positive electrode sheet includes a current collector;

[0068] At least two active material layers are stacked in sequence and formed on the surface of the current collector, and the porosity of the at least two active material layers decreases in sequence in a direction away from the current collector.

[0069] At least two active material layers are stacked in sequence on the surface of the current collector, and the porosity of the at least two active material layers decreases in sequence as they move away from the current collector, so that the electrolyte and the positive electrode plate can be fully infiltrated, ensuring that the conduction of lithium ions is not affected.

[0070] In some optional embodiments, the porosity of the active material layer in contact with the current collector is ≥45%; optionally, the porosity of the active material layer in contact with the current collector is ≥60%.

[0071] Within the above ratio range, the lithium ion conduction effect is improved.

[0072] In some optional embodiments, the porosity of the outermost active material layer is ≥25%; optionally, the porosity of the outermost active material layer is ≥50%.

[0073] Within the above ratio range, the lithium ion conduction effect is further improved.

[0074] In a second aspect, an embodiment of the present application provides a battery, which includes the positive electrode plate provided in the first aspect.

[0075] In the above technical solution, the battery has better dynamic performance by being provided with the positive electrode plate provided by the first aspect.

[0076] In a third aspect, an embodiment of the present application provides an electrical device, which includes the battery provided in the second aspect.

[0077] In the above technical solution, the electrical device has better dynamic performance by being equipped with the battery provided by the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0078] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0079] FIG1 is a schematic structural diagram of a vehicle provided in some embodiments of the present application;

[0080] FIG2 is an exploded view of a battery provided in some embodiments of the present application;

[0081] FIG3 is an exploded view of the battery cell shown in FIG2 ;

[0082] FIG4 is a schematic diagram of a partial structure of an electrode assembly provided in some embodiments of the present application;

[0083] FIG5 is a schematic diagram of a partial structure of a positive electrode plate provided in some embodiments of the present application.

[0084] icon:

[0085] Vehicles 1000;

[0086] Battery 100; Controller 200; Motor 300;

[0087] Box body 10; first part 11; second part 12; accommodating space 13;

[0088] Battery cell 20; housing 21; electrode assembly 22; electrode terminal 23; pressure relief structure 24;

[0089] Housing 211; cover 212; positive electrode sheet 221; negative electrode sheet 222; separator 223;

[0090] Positive electrode current collector 2211; positive electrode active material layer 2212;

[0091] Negative electrode current collector 2221 ; negative electrode active material layer 2222 . DETAILED DESCRIPTION

[0092] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.

[0093] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0094] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.

[0095] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "inside" and "outside" are based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the embodiments of the present application.

[0096] In the description of the embodiments of this application, unless otherwise specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; they can refer to direct connections or indirect connections through an intermediate medium. Those skilled in the art will understand the specific meanings of the above terms in the embodiments of this application based on specific circumstances.

[0097] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0098] In the embodiments of this application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components in different embodiments are omitted. It should be understood that the heights, lengths, widths, and other dimensions of the various components in the embodiments of this application, as well as the overall heights, lengths, widths, and other dimensions of the integrated device shown in the drawings are merely illustrative and do not constitute any limitation on this application.

[0099] Batteries made of positive electrode sheets obtained by physically mixing different active substances can give full play to the advantages of different materials and improve battery performance. However, the inventors of this application found that some mixed positive electrode sheets have the problem of poor dynamic performance. After analysis, it is believed that this may be due to the difference in the maximum shrinkage rate of the two active substances during the cycle, which cannot shrink or expand synchronously, resulting in the separation of the two materials, the failure of the contact between them, and the deterioration of the conductive network, which leads to a significant increase in impedance.

[0100] The embodiment of the present application provides a positive electrode sheet, the positive electrode sheet comprising at least two layers of positive electrode active material;

[0101] The two adjacent positive electrode active material layers include a first active material and a second active material, respectively; the maximum shrinkage rate of the first active material is T1, and the maximum shrinkage rate of the second active material is T2;

[0102] T1 and T2 satisfy the following relationship:

[0103] T1-T2 ≥ 0.3%;

[0104] The maximum shrinkage rate refers to the maximum change in the volume shrinkage or expansion of the unit cell of the positive electrode active material during the charge and discharge process.

[0105] It should be noted that the above-mentioned “maximum change degree” refers to the change degree of the unit cell volume in the fully charged state and the fully discharged state.

[0106] Specifically, a full charge refers to charging the battery cell to 100% SOC. Charge and discharge strategy: At 25°C, the battery is charged at a constant current of 0.3C to the upper limit of the operating voltage range of the active material, and then charged at this upper limit voltage to a current of 0.02C. This state is considered a full charge.

[0107] The unit cell volume of the positive electrode material in the initial state corresponds to the unit cell volume of the battery in the fully discharged state. The fully discharged state refers to the battery being discharged at a constant current of 0.3C to the lower limit of the operating voltage range of the active material.

[0108] The battery using the above-mentioned positive electrode plate can improve the dynamic performance of the battery.

[0109] The electrical device comprising the battery has more excellent dynamic performance.

[0110] For the convenience of description, the following embodiments are described using a lithium-ion battery according to an embodiment of the present application as an example of a battery and a vehicle according to an embodiment of the present application as an example of an electrical device.

[0111] Refer to Figure 1, which is a structural schematic diagram of a vehicle 1000 provided in some embodiments of the present application. The vehicle 1000 can be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle can be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is provided inside the vehicle 1000, and the battery 100 can be provided at the bottom, head or tail of the vehicle 1000. The battery 100 can be used to power the vehicle 1000. For example, the battery 100 can serve as an operating power source for the vehicle 1000. The vehicle 1000 may also include a controller 200 and a motor 300. The controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the vehicle 1000.

[0112] In some embodiments of the present application, the battery 100 can not only serve as the operating power source of the vehicle 1000, but also serve as the driving power source of the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.

[0113] In this application, battery 100 refers to a single physical module that includes one or more battery cells 20 to provide voltage and capacity. Battery 100 generally includes a housing 10 for enclosing one or more battery cells 20. Housing 10 prevents liquids or other foreign matter from affecting the charging or discharging of battery cells 20.

[0114] Referring to Figure 2, which is an exploded view of a battery 100 provided in some embodiments of the present application, the battery 100 may include a housing 10 and a battery cell 20, with the battery cell 20 housed within the housing 10. The housing 10 is used to house the battery cell 20 and may have various structures. In some embodiments, the housing 10 may include a first portion 11 and a second portion 12, which overlap each other and together define a storage space 13 for accommodating the battery cell 20. The second portion 12 may be a hollow structure with one end open, and the first portion 11 may be a plate-like structure, which overlaps the open side of the second portion 12 to form the housing 10 with the storage space 13. Alternatively, the first portion 11 and the second portion 12 may both be hollow structures with one end open, with the open side of the first portion 11 overlapping the open side of the second portion 12 to form the housing 10 with the storage space 13. Of course, the first portion 11 and the second portion 12 may have various shapes, such as a cylinder, a rectangular parallelepiped, etc.

[0115] In the battery 100, there can be one or more battery cells 20. If there are multiple battery cells 20, the multiple battery cells 20 can be connected in series, in parallel, or in a mixed connection. Mixed connection means that the multiple battery cells 20 are connected in series and in parallel. The multiple battery cells 20 can be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple battery cells 20 is accommodated in the case 10. Alternatively, multiple battery cells 20 can be first connected in series, in parallel, or in a mixed connection to form a module, and the multiple modules are then connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in the case 10. The battery 100 can also include other structures. For example, the multiple battery cells 20 can be electrically connected through a busbar component to achieve parallel, series, or mixed connection of the multiple battery cells 20.

[0116] Each battery cell 20 may be a lithium-ion battery, such as a secondary battery or a primary battery; it may also be a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, but is not limited thereto.

[0117] Referring to Figure 3 , which is an exploded view of the battery cell 20 shown in Figure 2 , the battery cell 20 is the smallest unit that makes up the battery 100. The battery cell 20 may include a housing 21 , an electrode assembly 22 , and an electrolyte, with both the electrode assembly 22 and the electrolyte being housed within the housing 21 .

[0118] The outer shell 21 may include a shell 211 and a cover 212. The shell 211 is a component used to cooperate with the cover 212 to form an internal sealed space of the battery cell 20, wherein the formed sealed space can be used to accommodate the electrode assembly 22, electrolyte and other components. The cover 212 refers to a component that covers the opening of the shell 211 to isolate the internal environment of the battery cell 20 from the external environment. The shape of the cover 212 can be adapted to the shape of the shell 211 to cooperate with the shell 211. Functional components such as electrode terminals 23 and pressure relief structures 24 can also be provided on the cover 212. A sealing ring can be configured between the opening of the shell 211 and the cover 212 to achieve sealing between the shell 211 and the cover 212.

[0119] The shell 211 and the cover 212 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shapes of the shell 211 and the cover 212 can be determined according to the specific shape and size of the electrode assembly 22. The material of the shell 211 and the cover 212 can be various, such as but not limited to metals such as copper, iron, aluminum, stainless steel, and aluminum alloy. The material of the sealing ring can be various, such as but not limited to PP (polypropylene), PC (polycarbonate), PET (polyethylene terephthalate) and other materials that are resistant to electrolyte corrosion, high toughness and fatigue resistance. A coating can be formed on the outer surface of the shell 211, and the material of the coating can be various, such as but not limited to corrosion-resistant materials such as Ni and Cr.

[0120] Referring to Figure 4 , the electrode assembly 22 may be composed of a positive electrode sheet 221, a negative electrode sheet 222, and a separator 223. The separator 223 is located between the positive electrode sheet 221 and the negative electrode sheet 222 to provide isolation. The electrode assembly 22 may be a wound or laminated structure, but the present invention is not limited thereto.

[0121] 4 , the negative electrode sheet 222 includes a negative electrode current collector 2221 and a negative electrode active material layer 2222 . The negative electrode current collector 2221 may be made of copper, and the negative electrode active material layer 2222 includes a negative electrode active material. The negative electrode active material includes at least one of graphite, silicon, a silicon alloy, or a tin alloy.

[0122] 5 , the positive electrode sheet 221 includes a positive current collector 2211 and a positive active material layer 2212 . Taking the lithium-ion battery cell 20 as an example, the positive current collector 2211 may be made of aluminum. The positive active material layer 2212 includes positive active materials.

[0123] Furthermore, in some embodiments of the present application, the positive electrode sheet 221 includes at least two positive electrode active material layers 2212 .

[0124] The two adjacent positive electrode active material layers include a first positive electrode active material and a second positive electrode active material, respectively; under the same test conditions, the maximum shrinkage rate of the first positive electrode active material during the charge and discharge process is T1, and the maximum shrinkage rate of the second positive electrode active material during the charge and discharge process is T2;

[0125] T1 and T2 satisfy the following relationship:

[0126] T1-T2 ≥ 0.3%;

[0127] The maximum shrinkage rate refers to the degree of volume shrinkage or expansion of the unit cell of the positive electrode active material during the charge and discharge process.

[0128] Compared with a single-layer mixed positive electrode active material layer formed by directly physically mixing the first positive electrode active material and the second positive electrode active material, in the above technical solution, when the first positive electrode active material and the second positive electrode active material T1-T2 ≥ 0.3%, the positive electrode plate is provided with at least two layers of positive electrode active material layers, which can improve the deterioration of the conductive network of the active material caused by the different frequency changes of active materials with different shrinkage rates, thereby improving the battery kinetic performance.

[0129] Furthermore, in some embodiments of the present application, the maximum shrinkage rate is tested as follows:

[0130] A certain active material is used as the only positive electrode active material, and the binder and conductive agent are mixed at a ratio of 97% wt: 1.5% wt:

[0131] A fresh electrode was prepared by mixing in a ratio of 1.5% wt, and the unit cell volume a of the positive electrode active material in the initial state was tested by XRD; a battery was prepared by using the electrode, and the electrode was disassembled after the battery was fully charged, and the fully charged electrode was tested by XRD to obtain the unit cell volume b of the positive electrode active material in the fully charged state; the maximum shrinkage rate of the positive electrode active material is (ab) / a.

[0132] Where: the unit cell volume a of the positive electrode active material in the initial state corresponds to the unit cell volume of the battery in the fully discharged state. The fully discharged state refers to the battery being discharged at a constant current of 0.3C to the lower limit of the operating voltage range of the active material;

[0133] Full charge means charging the cell to 100% SOC. Charge and discharge strategy: At 25°C, the battery is charged at a constant current of 0.3C to the upper limit of the operating voltage range of the active material, and then charged at the upper limit voltage to a current of 0.02C. This state is fully charged.

[0134] The electrode was tested using XRD to obtain an X-ray diffraction pattern of the active material, and the structure was refined using the Rietveld method to obtain the unit cell volume of the active material.

[0135] Furthermore, in some embodiments of the present application, T1 has a value range of 1%-7%. Furthermore, in some embodiments of the present application, T1 has a value range of 3%-6.5%. When T1 is too large, the material shrinks severely, affecting the contact interface between the materials and reducing dynamic performance. Properly setting the T1 value range is beneficial to improving battery dynamic performance.

[0136] Furthermore, in some embodiments of the present application, the value range of T2 is 0.3%-5.5%.

[0137] Further optionally, in some embodiments of the present application, the value range of T2 is 0.5%-3%.

[0138] Among the currently available positive electrode materials, the smaller maximum shrinkage rate is mainly within this range. When used together with materials with a larger maximum shrinkage rate, the difference in material shrinkage rate is large, and the layered arrangement of the active material layer of the present application is more suitable.

[0139] Furthermore, in some embodiments of the present application, the D of the first positive electrode active material is V 50 Size is 5μm-15μm.

[0140] The above D V 50 means: when the first positive electrode active material particles are added up from small to large, when the accumulated volume accounts for 50% of the total volume, the particle size of the first positive electrode active material particles is less than a certain value, and this value is the Dv50 value.

[0141] The first positive electrode active material with the maximum shrinkage of T1 is selected as D V The size of 50 is 5μm-15μm. The larger particle size can form more pores during the charge and discharge process, which is beneficial to electrolyte infiltration and ion conduction.

[0142] Furthermore, in some embodiments of the present application, the D of the second positive electrode active material is V 50 Size is 0.2μm-5μm.

[0143] The second positive electrode active material with the maximum shrinkage of T2 is selected as D V The size of 50 is 0.2μm-5μm, which is a small particle size and can cooperate with the first positive electrode active material with a larger particle size to further improve the battery charge and discharge cycle effect.

[0144] The above D V 50 means: when the second positive electrode active material particles are added up from small to large, and the accumulated volume accounts for 50% of the total volume, the particle size of the second positive electrode active material particles is less than a certain value, and this value is Dv50.

[0145] Furthermore, in some embodiments of the present application, the D of the first positive electrode active material is V The value of 50 is equal to or greater than 5 times the D of the second positive electrode active material V A value of 50.

[0146] Control the D of the first positive electrode active material and the second positive electrode active material V 50 satisfies the above proportional relationship; the high mechanical strength of the active material with smaller particle size at the same compaction density will alleviate this situation to a certain extent, and the gaps between the large-size particles will not be completely filled, and the ion conduction is better than that of the mixed system. The two effects complement each other, thereby effectively improving the battery dynamics.

[0147] In some optional embodiments, the D of the first positive electrode active material V The value of 50 is equal to or greater than 5 times the D of the second positive electrode active material V 50, and less than or equal to 50 times the D of the second positive electrode active material V A value of 50.

[0148] In some optional embodiments, the D of the first positive electrode active material V The value of 50 is equal to or greater than 5 times the D of the second positive electrode active material V 50, and less than or equal to 35 times the D of the second positive electrode active material V A value of 50.

[0149] By further limiting the particle size ratio of the first positive electrode active material and the second positive electrode active material to the above range, it is helpful to improve the situation where the small particle size material overfills the large particle size active material when the particle size difference is too large, resulting in insufficient voids, reduced porosity, and worsened ionic impedance. Furthermore, in some embodiments of the present application, a transition layer is formed between the positive electrode active material layer containing the first positive electrode active material and the positive electrode active material layer containing the second positive electrode active material.

[0150] By setting the first positive electrode active material D V 50 size is 5μm-15μm, D in the second positive electrode active material V The particle size of the active material in the first positive electrode active material layer is 0.2 μm to 5 μm, resulting in a relatively large particle size of the active material in the first positive electrode active material layer. Furthermore, the particle size of the active material in the first positive electrode active material layer is larger than that of the second positive electrode active material layer. The difference in particle size between the first and second positive electrode active material layers creates a transition layer where active material particles of different sizes coexist. This improves the bonding between the active layers and ensures improved dynamics between the active layers.

[0151] It should be noted that the above-mentioned transition layer can be clearly seen by enlarging the cross section.

[0152] Further optionally, the thickness of the transition layer is 0.2 μm to 2 μm.

[0153] The thickness of the transition layer refers to the average thickness of the transition layer. If the thickness of the transition layer is too small or too large, it will have a bad effect on the dynamic performance of the battery. If the transition layer is too thick, it will form a structure similar to a mixed layer, affecting the dynamic performance; if the transition layer is too thin, the adhesion between the two layers will be weakened, affecting the dynamic performance.

[0154] Further optionally, the thickness of the transition layer is 0.3 μm to 1.9 μm.

[0155] Exemplarily, the thickness of the transition layer is 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm or 1.8 μm.

[0156] Further optionally, in some embodiments of the present application, the D of the first positive electrode active material is V 50 size is 6μm-14μm. D of the second positive electrode active material V 50 The size is 0.3μm-4.9μm.

[0157] For example, in some embodiments of the present application, the D of the first positive electrode active material is V50 size is 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm or 14μm.

[0158] For example, in some embodiments of the present application, the D of the second positive electrode active material is V 50 The size is 0.2μm, 0.3μm, 0.5μm, 0.8μm, 1μm, 1.2μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm or 4.5μm.

[0159] Furthermore, in some embodiments of the present application, Dv90-Dv10 in the first positive electrode active material is ≤20 μm. Further optionally, the particle size distribution of the first positive electrode active material satisfies: 9≤D V 90-D V 10≤20μm.

[0160] In the above embodiment, Dv90 means: when the first positive electrode active material particles are accumulated from small to large, when the accumulation accounts for 90% of the total volume, the particle size of the first positive electrode active material particles is less than a certain value, and the value is the value of Dv90; Dv10 means: when the first positive electrode active material particles are accumulated from small to large, when the accumulation accounts for 10% of the total volume, the particle size of the first positive electrode active material particles is less than a certain value, and the value is the value of Dv10.

[0161] By limiting the D V 90-D V 10 is within the above range, so that the active material particle size in the first positive electrode active material layer is relatively concentrated. The first active material particle size is large, D V 90 and D V A larger difference of 10 is acceptable.

[0162] Furthermore, in some embodiments of the present application, D V 90-D V 10≤9μm.

[0163] In the above embodiment, Dv90 means: when the second positive electrode active material particles are accumulated from small to large, and when the accumulated amount accounts for 90% of the total volume, the particle size of the second positive electrode active material particles is all less than a certain value, and the value is the value of Dv90; Dv10 means: when the second positive electrode active material particles are accumulated from small to large, and when the accumulated amount accounts for 90% of the total volume, the particle size of the second positive electrode active material particles is all less than a certain value, and the value is the value of Dv90.

[0164] The above mentioned method is to define D in the second positive electrode active material. V90-D V 10≤9μm, so that the active material particle size in the second positive electrode active material layer is relatively concentrated. The second active material particle size is small, so D V 90 and D V A difference of 10 is relatively small.

[0165] Furthermore, in some embodiments of the present application, the D V 90-D V 10≤20μm, D in the second positive electrode active material V 90-D V 10≤9μm. By making the active material particle size in the first positive electrode active material layer relatively concentrated and the active material particle size in the second positive electrode active material layer relatively concentrated, it can be ensured that the contraction and expansion of the active material particles in the single layer are more synchronized, the contact between the particles will not be deteriorated, and the kinetic improvement effect in the single layer (the first positive electrode active material layer or the second positive electrode active material layer) is better.

[0166] For example, in some embodiments of the present application, the first positive electrode active material D V 90-D V 10 = 19 μm; or D V 90-D V 10 = 18 μm; or D V 90-D V 10 = 17 μm; or D V 90-D V 10 = 16 μm; or D V 90-D V 10 = 15 μm; or D V 90-D V 10 = 10 μm; or D V 90-D V 10=5μm.

[0167] Further illustratively, in some embodiments of the present application, the second positive electrode active material D V 90-D V 10 = 8 μm; or D V 90-D V 10 = 7 μm; or D V 90-D V 10 = 6 μm; or D V 90-D V 10 = 5 μm; or D V 90-D V 10 = 4 μm; or D V 90-D V 10 = 3 μm; or DV 90-D V 10 = 2 μm; or D V 90-D V 10=1μm.

[0168] According to the embodiments of the present application, the aforementioned Dv10, Dv50 or Dv90 is determined by a particle size analyzer-laser diffraction method. Specifically, reference can be made to the standard GB / T 19077-2016, and the measurement can be performed using a laser diffraction scattering particle size analyzer according to the manufacturer's instructions.

[0169] Furthermore, in some embodiments of the present application, any positive electrode active material layer includes multiple active materials; and the difference in maximum shrinkage of the multiple active materials does not exceed 0.3%;

[0170] T1 is the minimum value among the maximum shrinkage rates of the plurality of active materials in the first positive electrode active material;

[0171] T2 is the maximum value among a plurality of maximum shrinkage rates of a plurality of active materials in the second positive electrode active material.

[0172] By setting the maximum shrinkage of multiple active materials in any positive electrode active material layer to differ by no more than 0.3% during charge and discharge, this combination of active particles with shrinkage differences of no more than 0.3% is beneficial for improving battery impedance and dynamic performance.

[0173] Furthermore, in some embodiments of the present application, any positive electrode active material layer includes multiple active materials; the difference in maximum shrinkage of the multiple active materials exceeds 0.3%;

[0174] In terms of mass percentage, the multiple active materials include 85%-100% main active substances; 0-15% trace active substances;

[0175] T1 and T2 are the maximum shrinkage rates of the main active substance.

[0176] The same active material layer includes active particles with different shrinkage rates that differ by more than 0.3%. By maintaining the mass proportion of trace active substances between 0-15%, the negative impact of different frequency shrinkage and expansion can be reduced.

[0177] For example, in the above embodiment, if the maximum shrinkage rate of a trace active substance with a small proportion (such as 10%) among the multiple active substances in the same layer differs from the maximum shrinkage rate of other main active substances by more than 0.3%, then the maximum shrinkage rate of this layer refers to the shrinkage rate of the main active substance.

[0178] Further optionally, in terms of mass percentage, the above-mentioned main active substance is 86%-99%; and the above-mentioned trace active substance is 1-14%.

[0179] Illustratively, in terms of mass percentage, the main active substance is 86% and the trace active substance is 14%; or the main active substance is 90% and the trace active substance is 10%; or the main active substance is 95% and the trace active substance is 5%.

[0180] Furthermore, in some embodiments of the present application, T1-T2≥6%, the thickness of the positive electrode active material layer where the first positive electrode active material is located is H1; the thickness of the positive electrode active material layer where the second positive electrode active material is located is H2;

[0181] H1:H2 is (7:3) to (1:9).

[0182] When T1-T2 ≥ 6%, when the shrinkage difference between the first positive electrode active material and the second positive electrode active material between the two layers of positive electrode active material is too large, by setting H1:H2 to (7:3) ~ (1:9), the expansion of the entire active layer can be limited, the integrity of the electrode structure can be ensured, and the rapid deterioration of dynamics (impedance) caused by changes in the electrode structure during the cycle can be slowed down.

[0183] Furthermore, in some embodiments of the present application, the positive electrode sheet includes a positive electrode current collector;

[0184] The positive electrode active material layer where the first positive electrode active material is located is close to the current collector;

[0185] The positive electrode active material layer where the second positive electrode active material is located is away from the current collector.

[0186] The first cathode active material has a larger particle size and a higher shrinkage rate, which easily forms more pores during the charge and discharge process, facilitating lithium-ion transport. The first cathode active material layer is closer to the current collector, while the second cathode active material has a smaller particle size and a lower shrinkage rate, further away from the current collector. During the charge and discharge cycle, the outer layer can somewhat limit the shrinkage and expansion of the inner layer, reducing electrode deformation, deterioration of the active material conductive network, and lowering impedance growth. At the same time, the shrinkage and expansion of the inner layer's larger particle size and larger shrinkage rate create more pores, accommodating more electrolyte than in its initial state, thus achieving a more liquid-retaining effect.

[0187] Furthermore, in some embodiments of the present application, the second positive electrode active material includes at least one of a spinel structure positive electrode material or an olivine structure positive electrode material.

[0188] The second positive electrode active material includes at least one of a spinel structure positive electrode material and an olivine structure positive electrode material, which makes it easy to obtain a positive electrode active material layer with a smaller shrinkage rate.

[0189] Furthermore, in some embodiments of the present application, the second positive electrode active material includes: LiMPO4, and M includes Mn and non-Mn elements.

[0190] It should be noted that the above-mentioned LiMPO4 is not a specific molecular structure formula, but a general expression of lithium manganese phosphate.

[0191] Furthermore, in some embodiments of the present application, the non-Mn element includes one or both of a first doping element and a second doping element, the first doping element is a manganese doping element, and the second doping element is a phosphorus doping element.

[0192] Furthermore, in some embodiments of the present application, the first doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge.

[0193] Furthermore, in some embodiments of the present application, the first doping element includes at least two of Fe, Ti, V, Ni, Co and Mg.

[0194] Furthermore, in some embodiments of the present application, the second doping element includes one or more elements selected from the group consisting of B, S, Si, and N.

[0195] In some embodiments, the compound Li 1+x Mn 1-y A y P 1-z R z The preparation method of O4 may include the following steps:

[0196] (1) dissolving a manganese source, a source of element A to be doped at the manganese position, and an acid in a solvent and stirring to generate a suspension of a manganese salt doped with element A, filtering the suspension and drying the filter cake to obtain a manganese salt doped with element A;

[0197] (2) adding a lithium source, a phosphorus source, an element R source, a solvent, and the manganese salt doped with element A obtained in step (1) into a reaction vessel, grinding and mixing to obtain a slurry;

[0198] (3) transferring the slurry obtained in step (2) to a spray drying device for spray drying and granulation to obtain granules;

[0199] (4) Sintering the particles obtained in step (3) to obtain a positive electrode active material.

[0200] In any embodiment, the manganese source may be a manganese-containing substance known in the art that can be used to prepare lithium manganese phosphate. For example, the manganese source may be selected from elemental manganese, manganese dioxide, manganese phosphate, manganese oxalate, manganese carbonate, or a combination thereof.

[0201] The acid is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and organic acids such as oxalic acid, and may be, for example, oxalic acid. The source of element R is selected from at least one of sulfates, borates, nitrates, and silicates of element R. The source of element A is selected from at least one of a simple substance, oxide, phosphate, oxalate, carbonate, and sulfate of A.

[0202] Furthermore, in some embodiments of the present application, the second positive electrode active material includes Li 1+x Mn 1-y A y P 1-z R z O4, wherein x is any value in the range of -0.100 to 0.100, y is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and R includes one or more elements selected from the group consisting of B, S, Si and N.

[0203] Furthermore, in some embodiments of the present application, the second positive electrode active material includes Li a A e Mn 1-f B f P 1-g C g O 4-n D n ;

[0204] wherein A comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W;

[0205] B includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb, and Ge;

[0206] C includes one or more elements selected from B, S, Si and N;

[0207] D includes one or more elements selected from the group consisting of S, F, Cl, and Br;

[0208] a is selected from the range of 0.9 to 1.1, e is selected from the range of 0.001 to 0.1, f is selected from the range of 0.001 to 0.5, g is selected from the range of 0.001 to 0.1, n is selected from the range of 0.001 to 0.1, and the second positive active material is electrically neutral.

[0209] It should be noted that Li a A x Mn 1-y By P 1-z C z O 4-n D n The compound is actually a specific LiMPO4 material. Its preparation method can refer to Li 1+x Mn 1-y A y P 1-z R z O4, no limitation here.

[0210] In some embodiments, the positive electrode active material further has a coating layer comprising carbon.

[0211] The introduction of a carbon-containing coating layer improves the conductivity of the positive electrode active material. At this time, the structure of the positive electrode active material is actually a core-shell structure with LiMPO4 as the core and the surface of the core covered with a coating layer.

[0212] Optionally, the carbon content of the carbon layer is not less than 1.2%.

[0213] Furthermore, in some embodiments of the present application, the first positive electrode active material includes a layered structure positive electrode material.

[0214] The first positive electrode active material includes a layered structure positive electrode material, which makes it easy to obtain a positive electrode active material layer with a large shrinkage rate.

[0215] Furthermore, in some embodiments of the present application, the first positive electrode active material includes at least one of a nickel cobalt manganese oxide ternary material, a nickel cobalt aluminum oxide ternary material, and a nickel cobalt manganese aluminum oxide ternary material, or includes at least one of doped or coated materials of the above ternary materials.

[0216] The battery is accompanied by Li deintercalation and consumption during the charging and discharging process, and the molar content of Li is different when the battery is discharged to different states.

[0217] In the list of positive electrode materials in this application, the molar content of Li is the initial state of the material, that is, the state before adding the material. When the positive electrode material is used in a battery system, the molar content of Li will change after charge and discharge cycles.

[0218] In addition, the preparation process and conditions of the materials are different, and the molar content of the O element is usually not strictly the coefficient of the O element in the chemical formula, and there will be fluctuations, such as Li 1+x Mn 1-y A y P 1-z R z The molar content of the O element in O4 is not strictly 4.

[0219] Furthermore, in some embodiments of the present application, the positive electrode sheet includes a positive electrode current collector;

[0220] At least two positive electrode active material layers are stacked in sequence and formed on the surface of the positive electrode current collector, and the porosity of the at least two positive electrode active material layers decreases in sequence in a direction away from the positive electrode current collector.

[0221] At least two active material layers are stacked in sequence on the surface of the current collector, and the porosity of the at least two active material layers decreases in sequence as they move away from the current collector, so that the electrolyte and the positive electrode plate can be fully infiltrated, ensuring that the conduction of lithium ions is not affected.

[0222] Furthermore, in some embodiments of the present application, the porosity of the positive electrode active material layer in contact with the positive electrode current collector is ≥45%; optionally, the porosity of the positive electrode active material layer in contact with the positive electrode current collector is ≥60%.

[0223] Within the above ratio range, the lithium ion conduction effect is improved.

[0224] Illustratively, the porosity of the positive active material layer contacting the positive current collector is 46%, 50%, 55%, 65% or 70%.

[0225] Furthermore, in some embodiments of the present application, the porosity of the outermost positive electrode active material layer is ≥25%; optionally, the porosity of the outermost positive electrode active material layer is ≥50%.

[0226] Within the above ratio range, the lithium ion conduction effect is further improved.

[0227] Illustratively, the porosity of the outermost positive electrode active material layer is 30%, 35%, 40%, 40%, 55% or 65%.

[0228] According to the embodiments of the present application, the porosity can be determined by the gas replacement method. Specifically, according to the embodiments of the present application, it can be determined by referring to GB / T 24586-2009 through the following steps: immerse the electrode in dimethyl carbonate (DMC), clean and dry it. If it is a fresh electrode, no cleaning is required. Put the sample into the sample cup, record the number of samples to calculate the apparent volume, place the sample in a true density tester, and use the gas replacement method to determine the true volume. The electrode porosity is the percentage of the pore volume in the electrode to the total volume of the electrode. The calculation formula is: Porosity = (V V0) / V × 100%, where V0 is the true volume and V is the apparent volume; Apparent volume V = S*H*A, S is the surface area of ​​the electrode, H is the thickness of the electrode, and A is the number of electrode samples.

[0229] Furthermore, in some embodiments of the present application, the mass ratio of the active material in each positive electrode active material layer to the total positive electrode active material of the positive electrode sheet is 10%-90%.

[0230] By controlling the active material in each positive electrode active material layer to account for 10%-90% of the total positive electrode active material of the positive electrode sheet, a positive electrode active material layer with an optimal thickness can be obtained to ensure the battery dynamics performance.

[0231] Further optionally, the mass ratio of the active material in each positive electrode active material layer to the total positive electrode active material in the positive electrode sheet is 15%-85%. Exemplarily, the mass ratio of the active material in each positive electrode active material layer to the total positive electrode active material in the positive electrode sheet is 20%, 30%, 40%, 50%, 60%, 70%, or 80%.

[0232] Furthermore, in some embodiments of the present application, the active material layer further includes a conductive agent and a binder;

[0233] In terms of mass percentage, the active material is 89%-98%; the conductive agent is 0.4%-5%; the binder is 0.6%-

[0234] 6%.

[0235] Within the above ratio range, a positive electrode active material slurry with excellent comprehensive performance can be obtained.

[0236] Further optionally, in terms of mass percentage, the active material is 90%-97%; the conductive agent is 0.5%-4.8%; and the binder is 0.7%-5.9%.

[0237] Illustratively, in terms of mass percentage, the active material is 91%, the conductive agent is 4%, and the binder is 5%; or in terms of mass percentage, the active material is 95%, the conductive agent is 1%, and the binder is 4%; or in terms of mass percentage, the active material is 96%, the conductive agent is 0.5%, and the binder is 3.5%.

[0238] Some specific embodiments are listed below to better illustrate the present application.

[0239] Second positive electrode active material

[0240] A. Compound LiMn 0.22 Fe 0.78 The preparation method of PO4 includes:

[0241] Step S1: Preparation of Fe-doped manganese oxalate

[0242] 252.9g of manganese carbonate and 903.7g of ferrous carbonate were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours, mixing until the reaction terminated and no bubbles were generated, resulting in an Fe-doped manganese oxalate suspension. The suspension was then filtered, dried at 120°C, and sand-milled to obtain ferromanganese oxalate particles with a particle size of 100nm.

[0243] Step S2: Preparation of LiMn 0.22 Fe 0.78 PO4

[0244] Take the manganese oxalate iron (C2O4Mn 0.22 Fe 0.78 1791.4 g of 2H2O (calculated as 2H2O), 369.4 g of lithium carbonate, and 1150.1 g of ammonium dihydrogen phosphate were added to 20 L of deionized water, stirred thoroughly, and uniformly mixed at 80°C for 10 hours to obtain a slurry. The slurry was transferred to a spray dryer for spray drying and granulation, and then dried at 250°C to obtain a powder. The powder was sintered in a roller kiln at 700°C for 4 hours in a protective atmosphere (90% nitrogen and 10% hydrogen).

[0245] Carbon-coated LiMn 0.22 Fe 0.78 The preparation method of PO4 includes:

[0246] Take the manganese oxalate iron (C2O4Mn 0.22 Fe 0.78 1791.4 g of 1% nitric acid (based on 2H2O), 369.4 g of lithium carbonate, 1150.1 g of ammonium dihydrogen phosphate, and 0.005 mol of sucrose were added to 20 L of deionized water, stirred thoroughly, and uniformly mixed at 80°C for 10 hours to obtain a slurry. The slurry was transferred to a spray dryer for spray drying and granulation, and then dried at 250°C to obtain a powder. The powder was sintered in a roller kiln at 700°C for 4 hours in a protective atmosphere (90% nitrogen and 10% hydrogen).

[0247] The preparation steps of other undoped lithium manganese iron phosphate materials are the same as those of the aforementioned compound A, with the only difference being that the contents of manganese carbonate and ferrous carbonate are changed to satisfy the molar ratio of manganese to iron in the chemical formula of the corresponding compound.

[0248] You can also buy it directly from the market.

[0249] B. Compound Li 1.001 Mn 0.999 Fe0.001 P 0.999 Si 0.001 The preparation method of O4 includes:

[0250] Step S1: Preparation of Fe-doped manganese oxalate

[0251] 1148.2g of manganese carbonate and 1.2g of ferrous carbonate were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours, mixing until the reaction terminated and no bubbles were generated, resulting in an Fe-doped manganese oxalate suspension. The suspension was then filtered, dried at 120°C, and sand-milled to obtain ferromanganese oxalate particles with a particle size of 100nm.

[0252] Step S2: Preparation of Li 1.001 Mn 0.999 Fe 0.001 P 0.999 Si 0.001 O4

[0253] Take the manganese oxalate iron (C2O4Mn 0.999 Fe 0.001 1789.6 g of 2H2O (calculated as 2H2O), 369.8 g of lithium carbonate, 1148.9 g of ammonium dihydrogen phosphate, and 0.8 g of silicic acid were added to 20 L of deionized water, stirred thoroughly, and uniformly mixed at 80°C for 10 hours to obtain a slurry. The slurry was transferred to a spray dryer for spray drying and granulation, and then dried at 250°C to obtain a powder. The powder was sintered in a roller kiln at 700°C for 4 hours in a protective atmosphere (90% nitrogen and 10% hydrogen).

[0254] The preparation steps of lithium manganese iron phosphate materials doped with other elements (such as Ti) are the same as the preparation steps of the aforementioned compound B. The only difference is that silicic acid is replaced as the source of the corresponding element (such as titanium tetrachloride) and the raw material ratio is adjusted to meet the molar ratio in the chemical formula of the corresponding compound.

[0255] It can also be purchased directly from the market.

[0256]

First positive electrode active material

[0257] The layered structure positive electrode material was purchased from the market.

[0258] Example 1

[0259] 1) Preparation of positive electrode sheet

[0260] The aforementioned first positive electrode active material is selected, mixed with a conductive agent and a binder in a certain mass ratio, and dispersed in N-methylpyrrolidone to prepare a first positive electrode active material slurry; wherein the maximum shrinkage rate of the first positive electrode active material during the charge and discharge process is T1.

[0261] The aforementioned second positive electrode active material is selected and mixed with a conductive agent and a binder in a certain mass ratio and dispersed in N-methylpyrrolidone to prepare a second positive electrode active material slurry; wherein the maximum shrinkage rate of the second positive electrode active material during the charge and discharge process is T2.

[0262] The first positive electrode active material slurry prepared above is coated on the surfaces of both sides of the aluminum foil. At the same time, the second positive electrode active material slurry prepared above is coated on the surface of the positive electrode coated with the first positive electrode active material slurry to obtain a positive electrode plate. The mass proportion of the first positive electrode active material and the second positive electrode active material in the active material layer of the positive electrode plate is 50% respectively.

[0263] 2) Preparation of negative electrode sheet

[0264] The negative electrode active material artificial graphite, hard carbon, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) were mixed evenly in deionized water at a weight ratio of 90:5:2:2:1, coated on copper foil, dried, and cold pressed to obtain the negative electrode sheet. The coating amount was 0.2g / cm 2 , compacted density is 1.7g / cm 3 .

[0265] 3) Preparation of diaphragm

[0266] The polyethylene film is used as the substrate, and a coating is applied on the substrate to prepare the diaphragm.

[0267] 4) Preparation of lithium-ion batteries

[0268] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator positioned between the positive and negative electrodes to separate them. The cells are then wound to form a bare cell. The bare cell is placed in an outer packaging, injected with electrolyte, and sealed to form a battery. The electrolyte consists of a solution of 1 mol / L LiPF6 in a 1:1:1 volume ratio of ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC).

[0269] The differences between Example 2-35 and Example 1 are shown in Table 1 and Table 2.

[0270] Example 36 differs from Example 1 in that, in step 1) of Example 1, the second positive electrode active material slurry is first applied to both surfaces of the aluminum foil, and then the first positive electrode active material slurry is applied to the surface of the second positive electrode active material slurry. Other preparation parameters are the same as in Example 1.

[0271] Comparative Example 1

[0272] The only difference from Example 1 is step 1) preparation of the positive electrode sheet: in Comparative Example 1, the first positive electrode active material slurry and the second positive electrode active material slurry are mixed evenly and then coated on the surfaces of both sides of the aluminum foil; the mass proportions of the first positive electrode active material and the second positive electrode active material are also 50% respectively, and the active layer thickness is 50 μm.

[0273] Detection method:

[0274] Dynamic performance test method: At 25°C, the hard-shell battery is first fully discharged at 0.3C and then tested. The test process is as follows: the hard-shell battery is charged at a constant current of 0.3C to a voltage of 4.25V, then charged at a constant voltage of 4.25V to a current of 0.02C. After standing for 10 minutes, the lithium-ion battery is discharged at a constant current of 0.3C to a voltage of 2.5V. This is a charge and discharge cycle process. The voltage drop in the first 30 seconds of this discharge is divided by the discharge current and recorded as the resistance value of the first cycle. The hard-shell battery is subjected to 500 cycles of charge and discharge tests according to the above method. The ratio of the discharge voltage drop in the first 30 seconds of the hard-shell battery to the discharge current in the 500th cycle is recorded, that is, the resistance value of the 500th cycle. The ratio of the impedance difference between the 500th cycle and the first cycle to the impedance of the first cycle (impedance growth rate) can be used to characterize the dynamic performance.

[0275] The performance of the lithium-ion batteries of various embodiments and comparative examples was tested, and the results are shown in Table 3.

[0276] Table 1

[0277] Table 2

[0278] Table 3 Battery performance

[0279] From the test results in Table 3 above, it can be seen that:

[0280] In the embodiment of the present application, the kinetic performance (the ratio of the impedance difference between the 500th cycle and the first cycle to the impedance of the first cycle) ranged from 3.4% to 78.6%. In contrast, the kinetic performance of Comparative Example 1 (the ratio of the impedance difference between the 500th cycle and the first cycle to the impedance of the first cycle) reached 87.5%. The higher the ratio, the worse the kinetic performance. This shows that the solution of the present application effectively improves the kinetic performance of the battery.

[0281] Furthermore, from the comparison of Examples 5, 6, 16-20, and 1-4, it can be seen that when the value range of T1 is not 1%-7%, the kinetic performance of the battery is generally improved; when the value range of T1 is 1%-7%, the kinetic performance of the battery is better improved; when the value range of T1 is 3%-6.5%, the kinetic performance of the battery is better improved.

[0282] Furthermore, from the comparison between Example 2 and other examples, it can be seen that when the value range of T2 is 0.5%-3%, the kinetic performance of the battery is excellently improved.

[0283] Furthermore, it can be seen from Examples 7 to 14 that when the DV50(1) / DV50(2) of the first positive electrode active material and the second positive electrode active material is greater than 50, the degree of improvement in the kinetic performance of the battery is general; when the DV50(1) / DV50(2) of the first positive electrode active material and the second positive electrode active material is less than 5, the degree of improvement in the kinetic performance of the battery is general; when the DV50(1) / DV50(2) of the first positive electrode active material and the second positive electrode active material is between 5 and 50, the degree of improvement in the kinetic performance of the battery is good; when the DV50(1) / DV50(2) of the first positive electrode active material and the second positive electrode active material is between 5 and 35, the degree of improvement in the kinetic performance of the battery is excellent.

[0284] Furthermore, it can be seen from Examples 26 to 32 that when the particle size distribution of the first positive electrode active material satisfies: DV90-DV10>20μm, the degree of improvement in the battery's kinetic performance is general; when the particle size distribution of the first positive electrode active material satisfies: 9μm≤DV90-DV10≤20μm, the degree of improvement in the battery's kinetic performance is excellent.

[0285] Furthermore, the solution of the present application is widely used: the positive electrode materials include layered materials, spinel structure materials and olivine structure materials. The shrinkage rate of the layered structure is generally greater than that of the spinel and olivine structures. At the same time, the shrinkage rate of the layered structure is also affected by the Ni content. When the design capacity is the same, the shrinkage rate of the ternary layered material with a high Ni content is relatively large, and the shrinkage rate of the ternary layered material with a low Ni content is relatively small. The shrinkage rate of the olivine structure material is relatively consistent, and is smaller than that of the ternary layered material as a whole.

[0286] According to the solution of the embodiment of the present application, the inventors in this field tested the shrinkage rate of the purchased materials. If the shrinkage rate of the material meets the conditions described in this application, a layered structure design (rather than mixing in the same layer) can be preferably adopted to improve the dynamic performance.

[0287] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

Claims

1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises at least two positive electrode active material layers; The two adjacent positive electrode active material layers include a first positive electrode active material and a second positive electrode active material, respectively; the maximum shrinkage rate of the first positive electrode active material is T1, and the maximum shrinkage rate of the second positive electrode active material is T2; T1 and T2 satisfy the following relationship: T1-T2 ≥ 0.3%; The maximum shrinkage rate refers to the maximum degree of change in the unit cell volume shrinkage or expansion of the positive electrode active material during the charge and discharge process.

2. The positive electrode sheet according to claim 1, characterized in that: The value range of T1 is 1%-7%; optionally, the value range of T1 is 3%-6.5%.

3. The positive electrode sheet according to claim 1, characterized in that: The value range of T2 is 0.3%-5.5%; optionally, the value range of T2 is 0.5%-3%.

4. The positive electrode sheet according to claim 1, characterized in that: The D of the first positive electrode active material V 50 is 5 μm-15 μm; D of the second positive electrode active material V 50 is 0.2μm-5μm.

5. The positive electrode sheet according to any one of claims 1 to 4, characterized in that: The D of the first positive electrode active material V The value of D 50 is equal to or greater than 5 times that of the second positive electrode active material. V A value of 50; Optionally, the D of the first positive electrode active material V The value of D 50 is equal to or greater than 5 times that of the second positive electrode active material. V 50, and is less than or equal to 50 times the D of the second positive electrode active material V A value of 50; Optionally, the D of the first positive electrode active material V The value of D 50 is equal to or greater than 5 times that of the second positive electrode active material. V 50, and is less than or equal to 35 times the D of the second positive electrode active material V A value of 50.

6. The positive electrode sheet according to claim 5, characterized in that: The particle size distribution of the first positive electrode active material satisfies: V 90-D V 10≤20μm; Optionally, the particle size distribution of the first positive electrode active material satisfies: 9≤D V 90-D V 10≤20μm; Optionally, the particle size distribution of the second positive electrode active material satisfies: V 90-D V 10≤9μm.

7. The positive electrode sheet according to claim 1, characterized in that: Any of the positive electrode active material layers comprises a plurality of active materials; and the difference in maximum shrinkage of the plurality of active materials does not exceed 0.3% The T1 is the minimum value of the plurality of maximum shrinkage rates of the plurality of active materials in the first positive electrode active material; The T2 is the maximum value among the plurality of maximum shrinkage rates of the plurality of active materials in the second positive electrode active material.

8. The positive electrode sheet according to claim 1, characterized in that: Any of the positive electrode active material layers includes a plurality of active materials; The difference in maximum shrinkage of the plurality of active materials exceeds 0.3%; In terms of mass percentage, the plurality of active materials include: 85%-100% main active substances; 0-15% trace active substances; The T1 and the T2 are both the maximum shrinkage rates of the main active substance.

9. The positive electrode sheet according to claim 1, characterized in that: T1-T2≥6%, the thickness of the positive electrode active material layer where the first positive electrode active material is located is H1; the thickness of the positive electrode active material layer where the second positive electrode active material is located is H2; H1:H2 is (7:3) to (1:9).

10. The positive electrode sheet according to any one of claims 1 to 9, characterized in that: The positive electrode sheet includes a positive electrode current collector; The positive electrode active material layer where the first positive electrode active material is located is close to the current collector; The positive electrode active material layer where the second positive electrode active material is located is far away from the current collector.

11. The positive electrode sheet according to any one of claims 1 to 9, characterized in that: A transition layer is formed between the positive electrode active material layer where the first positive electrode active material is located and the positive electrode active material layer where the second positive electrode active material is located; Optionally, the transition layer has a thickness of 0.2 μm to 2 μm.

12. The positive electrode sheet according to any one of claims 1 to 11, characterized in that: The second positive electrode active material includes at least one of a spinel structure positive electrode material or an olivine structure positive electrode material.

13. The positive electrode sheet according to claim 12, characterized in that: The second positive electrode active material includes LiMPO4, and M includes Mn and non-Mn elements; Optionally, the non-Mn element includes one or both of a first doping element and a second doping element, the first doping element is manganese doping, and the second doping element is phosphorus doping; Optionally, the first doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; Optionally, the first doping element includes at least two of Fe, Ti, V, Ni, Co and Mg; Optionally, the second doping element includes one or more elements selected from the group consisting of B, S, Si and N; Optionally, the second positive electrode active material includes Li 1+x Mn 1-y A y P 1-z R z O4, wherein x is any value in the range of -0.100 to 0.100, y is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and R includes one or more elements selected from the group consisting of B, S, Si and N; Optionally, the second positive electrode active material includes Li a A e Mn 1-f B f P 1-g C g O 4-n D n , Wherein, the A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; The B includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; The C includes one or more elements selected from B, S, Si and N; The D comprises one or more elements selected from the group consisting of S, F, Cl and Br; The a is selected from the range of 0.9 to 1.1, the e is selected from the range of 0.001 to 0.1, the f is selected from the range of 0.001 to 0.5, the g is selected from the range of 0.001 to 0.1, the n is selected from the range of 0.001 to 0.1, and the second positive active material is electrically neutral.

14. The positive electrode sheet according to any one of claims 1 to 11, characterized in that: The first positive electrode active material includes a layered structure positive electrode material.

15. The positive electrode sheet according to claim 14, characterized in that: The first positive electrode active material includes at least one of a nickel-cobalt-manganese-lithium ternary material, a nickel-cobalt-aluminum-lithium ternary material, and a nickel-cobalt-manganese-aluminum-lithium ternary material, or at least one of doped or coated materials including the above ternary materials.

16. The positive electrode sheet according to claim 1, characterized in that: The positive electrode sheet includes a positive electrode current collector; The at least two positive electrode active material layers are stacked in sequence and formed on the surface of the positive electrode current collector, and the porosity of the at least two positive electrode active material layers decreases in sequence in a direction away from the positive electrode current collector.

17. The positive electrode sheet according to claim 16, characterized in that: The porosity of the positive electrode active material layer close to the positive electrode current collector is ≥45%; optionally, the porosity of the positive electrode active material layer contacting the positive electrode current collector is ≥60%.

18. The positive electrode sheet according to claim 17, characterized in that: The porosity of the positive electrode active material layer further away is ≥25%; optionally, the porosity of the positive electrode active material layer on the outermost surface is ≥50%.

19. A battery, characterized in that: The battery comprises the positive electrode sheet according to any one of claims 1 to 18.

20. An electrical device, characterized in that: The electrical device comprises the battery according to claim 19.

Citation Information

Patent Citations

  • Positive plate, preparation method and all-solid-state battery

    CN114628634A

  • Positive plate, roll core and battery

    CN115483365A

  • Positive pole piece and preparation method thereof, secondary battery, battery module, battery pack and power utilization device

    CN115832183A

  • Positive electrode active material, positive electrode plate, electrode assembly, battery monomer, battery and electric equipment

    CN115939322A

  • Lithium secondary battery

    JP2009176449A