Positive electrode sheet, battery, and electric device
By adopting a layered positive electrode sheet design in lithium-ion batteries, combining conductive coatings and high-energy-density materials, the problem of thermal runaway and capacity of lithium-ion batteries is solved, achieving higher battery performance and safety.
Patent Information
- Application Number
- PCT/CN2023/095592
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-11-28
AI Technical Summary
Existing lithium-ion secondary batteries are difficult to take into account both high energy density and safety, and are prone to thermal runaway problems, affecting battery capacity and reliability.
The positive electrode sheet design adopts a layered structure, including a conductive coating, a first active material layer and a second active material layer, the first active material layer is close to the anode, the second active material layer has a capacity of more than 165mAh/g, and the conductive coating is On the surface of the current collector, the probability of thermal runaway is reduced by using olivine or spinel structural materials, and the conductivity and adhesion are improved by conductive coatings.
It effectively reduces the probability of thermal runaway from the battery, improves battery capacity and cycle stability, and improves the energy density and safety performance of the battery.
Smart Images

Figure CN2023095592_28112024_PF_FP_ABST
Abstract
Description
Positive electrode, battery, electrical device Technical Field
[0001] The present application relates to a positive electrode sheet, a battery, and an electrical device. Background Art
[0002] In recent years, with the advancement of lithium-ion secondary battery technology, lithium-ion secondary batteries have been widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. This tremendous development has led to higher requirements for lithium-ion secondary batteries' capacity and the probability of thermal runaway.
[0003] Summary of the Invention
[0004] The purpose of this application is to provide a positive electrode sheet, a battery, and an electrical device.
[0005] The embodiment of the present application is implemented as follows:
[0006] In a first aspect, an embodiment of the present application provides a positive electrode sheet, the positive electrode sheet comprising a current collector, a conductive coating, a first active material layer, and a second active material layer; the conductive coating is formed on a surface of the current collector; the first active material layer is formed on a surface of the conductive coating; and the second active material layer is formed on a surface of the first active material layer.
[0007] The first active material layer includes: a first active material; the second active material layer includes a second active material;
[0008] The first active material does not catch fire in a needle penetration test. The needle penetration test method is as follows: a battery cell is made of the first active material, the battery cell is charged to 100% charge, and the battery cell is restrained by a steel fixture with a hole in the middle. A 2mm diameter steel needle is used to vertically penetrate the battery cell at a speed of 10mm / s at 25°C. The battery cell does not catch fire within 30 minutes of standing.
[0009] The gram capacity of the second active material is greater than or equal to 165 mAh / g.
[0010] In the above technical solution, the first active material layer and the second active material layer are layered and arranged in a specific position relationship, which helps to give full play to their respective characteristics. The upper layer uses a high energy density material (gram capacity greater than or equal to 165mAh / g). Since it is closer to the anode and the separator, Li +The transmission path is shortened, allowing for better utilization of capacity, energy, and power. The lower layer utilizes a high-safety material to prevent direct contact between the upper layer or anode and the current collector, resulting in resistance to internal short circuits and punctures. Furthermore, a conductive coating is applied to the current collector surface, helping to reduce positive electrode impedance and enhance positive electrode lithium deintercalation activity, thereby contributing to higher battery capacity. Therefore, the above technical solution can simultaneously reduce the probability of thermal runaway while increasing battery capacity.
[0011] In some optional embodiments, the first active material is subjected to a cell hot box test and the temperature at which thermal runaway occurs is greater than 160°C.
[0012] The method of the battery cell hot box test is: use the first active material to make a rectangular battery cell, charge the battery cell to 100% charge state, use a steel clamp to restrain the battery cell, place the battery cell in an oven and let it stand, the starting temperature of the oven is 130℃, and let the battery cell stand for 1 hour to confirm the status; if the battery cell does not fail after standing for 1 hour, increase the temperature at 5℃ / min, and let it stand for 30 minutes every time the temperature increases by 5℃, until the battery cell suffers thermal runaway.
[0013] The first active material has been tested in a battery cell hot box and the temperature at which thermal runaway occurs is greater than 160°C. It has excellent resistance to thermal runaway and is further beneficial to reducing the probability of thermal runaway of the battery.
[0014] In some optional embodiments, the first active material includes at least one of an olivine structure material or a spinel structure material.
[0015] By selecting at least one of an olivine structure material or a spinel structure material as the first active material, these materials have the characteristic of reducing the probability of thermal runaway of the battery, thereby facilitating reducing the probability of thermal runaway of the battery.
[0016] In some optional embodiments, the olivine structure material includes at least one of a lithium iron phosphate material, a lithium iron manganese phosphate material, or a lithium vanadium phosphate material.
[0017] In the above technical solution, lithium iron phosphate material, lithium manganese iron phosphate material or lithium vanadium phosphate material has excellent characteristics of reducing the probability of battery thermal runaway, is easy to obtain, and is conducive to obtaining a positive electrode sheet with excellent performance.
[0018] In some optional embodiments, the spinel structure material includes at least one of LiMn2O4, Li2MnNiO4 or lithium titanate materials.
[0019] In the above technical solutions, LiMn2O4, Li2MnNiO4 or lithium titanate materials have the excellent characteristic of reducing the probability of thermal runaway of the battery, which is conducive to obtaining a positive electrode sheet with good performance.
[0020] In some optional embodiments, the thickness of the first active material layer is 7 μm to 80 μm; optionally, the thickness of the first active material layer is 15 μm to 50 μm.
[0021] By setting the thickness of the first active material layer within the above range, the effect of the first active material can be fully exerted, and it is advantageous to miniaturize the battery.
[0022] In some optional embodiments, the D of the particles contained in the first active material layer is v 50 is 0.5μm~20μm.
[0023] Within the above-mentioned particle size range, a first active material layer with good performance can be easily obtained.
[0024] In some alternative embodiments, the second active material has a gram capacity of 175 mAh / g to 250 mAh / g.
[0025] By limiting the gram capacity of the second active material to 175 mAh / g to 250 mAh / g, it is beneficial to improve the battery capacity of the battery.
[0026] In some optional embodiments, the voltage platform of the second active material is greater than or equal to 3.22V. Optionally, the voltage platform of the second active material is 3.5V to 3.9V.
[0027] By limiting the voltage platform of the two active materials to be greater than or equal to 3.22V, it is beneficial to improve the battery capacity of the battery.
[0028] In some optional embodiments, the second active material includes: a layered structure material.
[0029] Layered structural materials have the characteristics of high energy density, which is beneficial to improving the battery capacity of the battery.
[0030] In some optional embodiments, the layered structure material includes at least one of a layered ternary material, lithium cobalt oxide, and a lithium-rich manganese-based material.
[0031] Layered ternary materials, lithium cobalt oxide, and lithium-rich manganese-based materials all have the characteristics of high energy density, which is beneficial to improving the battery capacity of the battery.
[0032] In some optional embodiments, the thickness of the second active material layer is 7 μm to 67 μm; optionally, the thickness of the second active material layer is 15 μm to 50 μm.
[0033] By setting the thickness of the second active material layer to 7 μm to 67 μm, the characteristics of the second active material can be effectively exerted, and the battery can be miniaturized.
[0034] In some optional embodiments, the D of the particles contained in the second active material layer is v 50 is 1μm~20μm.
[0035] By setting the average particle size of the particles contained in the second active material layer to be 1 μm to 20 μm, within the above range, it is advantageous to form a second active material layer with good performance.
[0036] In some optional embodiments, the thickness of the conductive coating is 0.1 μm to 2 μm; optionally, the thickness of the conductive coating is 0.5 μm to 1.5 μm.
[0037] By setting the thickness of the conductive coating within the above range, both the miniaturization of the battery and the effectiveness of the conductive coating can be taken into account.
[0038] In some optional embodiments, the conductive coating includes: a conductive agent and a binder.
[0039] The conductive coating has good conductivity and adhesion: the conductivity is mainly achieved through the conductive agent, which helps to reduce the cathode impedance and improve the cathode lithium deintercalation activity, and the corresponding battery exhibits higher capacity, power and low-temperature performance; the adhesion is mainly achieved through the binder, which helps to connect the first active material layer and the current collector more firmly, reduce the shedding of active materials during the electrode slitting and winding process, and is beneficial to long-term reliability.
[0040] In some optional embodiments, the conductive coating comprises, by weight percentage, 40% to 60% of a conductive agent and 40% to 60% of a binder.
[0041] Within the above-mentioned ratio range, a conductive coating with good conductivity and good adhesion properties can be obtained.
[0042] In some optional embodiments, the conductive coating further comprises: a neutralizing agent.
[0043] Adding a neutralizer to the conductive coating to adjust the pH can improve the corrosion resistance of the positive electrode current collector (aluminum foil). At the same time, the neutralizer can form positive and negative charge attraction between the current collector and the first active material layer, further enhancing the adhesion between the first active material layer and the current collector.
[0044] In some optional embodiments, the conductive coating comprises, by weight percentage, 40% to 55% of a conductive agent, 40% to 55% of a binder, and 1 to 10% of a neutralizer.
[0045] Within the above-mentioned ratio range, a conductive coating having excellent electrical conductivity, excellent adhesion and good corrosion resistance of the current collector can be obtained.
[0046] In some optional embodiments, the conductive agent includes at least one of carbon black, carbon nanotubes, or graphene.
[0047] At least one of the carbon black, carbon nanotubes or graphene as a conductive agent has high electrical conductivity, which can make the conductive coating have high conductivity, which is beneficial for the battery to exhibit higher capacity.
[0048] In some optional embodiments, the binder includes at least one of polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, polyvinylidene fluoride, or styrene-butadiene rubber.
[0049] At least one of polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, polyvinylidene fluoride or styrene-butadiene rubber is used as a binder, which has high bonding properties and can make the conductive coating obtain high bonding properties, which is beneficial for a stronger connection between the first active material layer and the current collector, reduces the shedding of active materials during the electrode slitting and winding processes, and improves long-term reliability.
[0050] In some alternative embodiments, the neutralizing agent includes at least one of calcium hydroxide or lithium hydroxide.
[0051] At least one of calcium hydroxide and lithium hydroxide as a neutralizing agent can effectively adjust the pH of the conductive coating, thereby enhancing the bonding force between the first active material layer and the current collector through electrostatic attraction.
[0052] In a second aspect, an embodiment of the present application provides a battery, comprising the positive electrode plate of the first aspect.
[0053] The battery in the above technical solution, including the positive electrode plate of the first aspect, can reduce the probability of thermal runaway of the battery while improving the battery capacity.
[0054] In a third aspect, an embodiment of the present application provides an electrical device, which includes the battery provided in the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0056] FIG1 is a schematic structural diagram of a vehicle provided in some embodiments of the present application;
[0057] FIG2 is an exploded view of a battery provided in some embodiments of the present application;
[0058] FIG3 is an exploded view of the battery cell shown in FIG2 ;
[0059] FIG4 is a schematic diagram of a partial structure of an electrode assembly provided in some embodiments of the present application;
[0060] FIG5 is a schematic diagram of a partial structure of a positive electrode plate provided in some embodiments of the present application.
[0061] Icons: Vehicle 1000; Battery 100; Controller 200; Motor 300; Housing 10; First portion 11; Second portion 12; Accommodation space 13; Battery cell 20; Housing 21; Electrode assembly 22; Electrode terminal 23; Pressure relief structure 24; Case 211; Cover 212; Positive electrode sheet 221; Negative electrode sheet 222; Separator 223; Positive current collector 2211; Positive active material layer 2212; Negative current collector 2221; Negative active material layer 2222. DETAILED DESCRIPTION
[0062] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.
[0063] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0064] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.
[0065] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "inside" and "outside" are based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the embodiments of the present application.
[0066] In the description of the embodiments of this application, unless otherwise specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; they can refer to direct connections or indirect connections through an intermediate medium. Those skilled in the art will understand the specific meanings of the above terms in the embodiments of this application based on specific circumstances.
[0067] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0068] In the embodiments of this application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components in different embodiments are omitted. It should be understood that the heights, lengths, widths, and other dimensions of the various components in the embodiments of this application, as well as the overall heights, lengths, widths, and other dimensions of the integrated device shown in the drawings are merely illustrative and do not constitute any limitation on this application.
[0069] Positive electrodes made from a single active material cannot meet the requirements for higher battery performance. Mixing two active materials can achieve the properties of both, potentially leading to even higher battery performance. However, this direct mixing method can lead to problems such as gel formation due to differences in properties such as particle size, pH, and specific surface area between the two materials. It can also lead to other issues with battery performance, such as increasing the probability of thermal runaway while pursuing high energy density.
[0070] The present invention provides a positive electrode sheet, which includes a current collector, a conductive coating, a first active material layer, and a second active material layer; the conductive coating is formed on the surface of the current collector; the first active material layer is formed on the surface of the conductive coating; and the second active material layer is formed on the surface of the first active material layer.
[0071] The first active material layer includes: a first active material; the second active material layer includes a second active material;
[0072] The first active material does not catch fire in a needle penetration test. The needle penetration test method is as follows: a battery cell is made of the first active material, the battery cell is charged to 100% charge, and the battery cell is restrained by a steel fixture with a hole in the middle. A 2mm diameter steel needle is used to vertically penetrate the battery cell at a speed of 10mm / s at 25°C. The battery cell does not catch fire within 30 minutes of standing.
[0073] The gram capacity of the second active material is greater than or equal to 165 mAh / g.
[0074] In the above technical solution, the first active material layer and the second active material layer are layered and arranged in a specific position relationship, which helps to give full play to their respective characteristics. The upper layer uses a high energy density material (gram capacity greater than or equal to 165mAh / g). Since it is closer to the anode and the separator, Li + The shortened transmission path allows for better utilization of capacity, energy, and power. The lower layer utilizes a high-safety material to prevent direct contact between the upper layer or anode and the current collector, resulting in resistance to internal short circuits and punctures. Furthermore, a conductive coating on the current collector surface helps reduce positive electrode impedance and enhance positive electrode lithium deintercalation activity, thereby contributing to higher battery capacity. Therefore, the above technical solution can simultaneously reduce the probability of thermal runaway while increasing battery capacity.
[0075] The battery provided in the present application includes the aforementioned positive electrode plate, which is beneficial for increasing the battery capacity of the electrical device while reducing the probability of thermal runaway of the battery.
[0076] The electrical device provided in this application, including the battery proposed above in this application, is conducive to improving the performance of the electrical device.
[0077] For the convenience of description, the following embodiments are described by taking a lithium-ion battery according to an embodiment of the present application as an example.
[0078] Refer to Figure 1, which is a structural schematic diagram of a vehicle 1000 provided in some embodiments of the present application. The vehicle 1000 can be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle can be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is provided inside the vehicle 1000, and the battery 100 can be provided at the bottom, head or tail of the vehicle 1000. The battery 100 can be used to power the vehicle 1000. For example, the battery 100 can serve as an operating power source for the vehicle 1000. The vehicle 1000 may also include a controller 200 and a motor 300. The controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the vehicle 1000.
[0079] In some embodiments of the present application, the battery 100 can not only serve as the operating power source of the vehicle 1000, but also serve as the driving power source of the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.
[0080] In this application, battery 100 can refer to a physical module including a single battery cell, or a single physical module including multiple battery cells 20 to provide higher voltage and capacity. Battery 100 can be in the form of a battery module or battery pack, and can include a housing 10 for enclosing one or more battery cells 20. Housing 10 prevents liquids or other foreign matter from affecting the charging or discharging of battery cells 20.
[0081] Referring to Figure 2, which is an exploded view of a battery 100 provided in some embodiments of the present application, the battery 100 may include a housing 10 and a battery cell 20, with the battery cell 20 housed within the housing 10. The housing 10 is used to house the battery cell 20 and may have various structures. In some embodiments, the housing 10 may include a first portion 11 and a second portion 12, which overlap each other and together define a storage space 13 for accommodating the battery cell 20. The second portion 12 may be a hollow structure with one end open, and the first portion 11 may be a plate-like structure, which overlaps the open side of the second portion 12 to form the housing 10 with the storage space 13. Alternatively, the first portion 11 and the second portion 12 may both be hollow structures with one end open, with the open side of the first portion 11 overlapping the open side of the second portion 12 to form the housing 10 with the storage space 13. Of course, the first portion 11 and the second portion 12 may have various shapes, such as a cylinder, a rectangular parallelepiped, etc.
[0082] In the battery 100, there can be one or more battery cells 20. If there are multiple battery cells 20, the multiple battery cells 20 can be connected in series, in parallel, or in a mixed connection. Mixed connection means that the multiple battery cells 20 are connected in series and in parallel. The multiple battery cells 20 can be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple battery cells 20 is accommodated in the case 10. Alternatively, multiple battery cells 20 can be first connected in series, in parallel, or in a mixed connection to form a module, and the multiple modules are then connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in the case 10. The battery 100 can also include other structures. For example, the multiple battery cells 20 can be electrically connected through a busbar component to achieve parallel, series, or mixed connection of the multiple battery cells 20.
[0083] Each battery cell 20 may be a lithium-ion battery, such as a secondary battery or a primary battery; it may also be a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, but is not limited thereto.
[0084] Referring to Figure 3 , which is an exploded view of the battery cell 20 shown in Figure 2 , the battery cell 20 is the smallest unit that makes up the battery 100. The battery cell 20 may include a housing 21 , an electrode assembly 22 , and an electrolyte, with both the electrode assembly 22 and the electrolyte being housed within the housing 21 .
[0085] The outer shell 21 may include a shell 211 and a cover 212. The shell 211 is a component used to cooperate with the cover 212 to form an internal sealed space of the battery cell 20, wherein the formed sealed space can be used to accommodate the electrode assembly 22, electrolyte and other components. The cover 212 refers to a component that covers the opening of the shell 211 to isolate the internal environment of the battery cell 20 from the external environment. The shape of the cover 212 can be adapted to the shape of the shell 211 to cooperate with the shell 211. Functional components such as electrode terminals 23 and pressure relief structures 24 can also be provided on the cover 212. A sealing ring can be configured between the opening of the shell 211 and the cover 212 to achieve sealing between the shell 211 and the cover 212.
[0086] The shell 211 and the cover 212 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shapes of the shell 211 and the cover 212 can be determined according to the specific shape and size of the electrode assembly 22. The material of the shell 211 and the cover 212 can be various, such as but not limited to metals such as copper, iron, aluminum, stainless steel, and aluminum alloy. The material of the sealing ring can be various, such as but not limited to PP (polypropylene), PC (polycarbonate), PET (polyethylene terephthalate) and other materials that are resistant to electrolyte corrosion, high toughness and fatigue resistance. A coating can be formed on the outer surface of the shell 211, and the material of the coating can be various, such as but not limited to corrosion-resistant materials such as Ni and Cr.
[0087] Referring to Figure 4 , the electrode assembly 22 may be composed of a positive electrode sheet 221, a negative electrode sheet 222, and a separator 223. The separator 223 is located between the positive electrode sheet 221 and the negative electrode sheet 222 to provide isolation. The electrode assembly 22 may be a wound or laminated structure, but the present invention is not limited thereto.
[0088] 4 , the negative electrode sheet 222 includes a negative electrode current collector 2221 and a negative electrode active material layer 2222 . The negative electrode current collector 2221 may be made of copper, and the negative electrode active material layer 2222 includes a negative electrode active material. The negative electrode active material includes at least one of graphite, silicon, a silicon alloy, or a tin alloy.
[0089] 5 , the positive electrode sheet 221 includes a positive electrode current collector 2211 and a positive electrode active material layer 2212. Taking the lithium-ion battery cell 20 as an example, the material of the positive electrode current collector 2211 can be aluminum foil.
[0090] Furthermore, in some embodiments of the present application, the positive electrode sheet includes a current collector, a conductive coating, a first active material layer, and a second active material layer; the conductive coating is formed on the surface of the current collector; the first active material layer is formed on the surface of the conductive coating; and the second active material layer is formed on the surface of the first active material layer.
[0091] The first active material layer includes: a first active material; the second active material layer includes a second active material;
[0092] The first active material does not catch fire in a needle penetration test. The needle penetration test method is as follows: a battery cell is made of the first active material, the battery cell is charged to 100% charge, and the battery cell is restrained by a steel fixture with a hole in the middle. A 2mm diameter steel needle is used to vertically penetrate the battery cell at a speed of 10mm / s at 25°C. The battery cell does not catch fire within 30 minutes of standing.
[0093] The gram capacity of the second active material is greater than or equal to 165 mAh / g.
[0094] In the above technical solution, the first active material does not ignite during the needle penetration test, which helps reduce the probability of thermal runaway. The second active material has a gram capacity of greater than or equal to 165 mAh / g, which helps increase the battery capacity. By arranging the first and second active materials in layers, with the first active material, which does not ignite during the needle penetration test, positioned near the current collector and the second active material, which has a larger gram capacity, positioned above the first active material, their respective properties can be fully utilized. Simultaneously, a conductive coating is provided on the current collector surface, allowing the conductive coating, the first active material, and the second active material to synergistically enhance their respective advantages, reducing the probability of thermal runaway while also increasing the battery capacity.
[0095] Furthermore, the first active material layer and the second active material layer are layered and arranged in a specific position relationship to help give full play to their respective characteristics. The upper layer uses a high energy density material (gram capacity greater than or equal to 165mAh / g). Since it is closer to the anode and the separator, Li + The shortened transmission path maximizes capacity, energy, and power. High-safety materials are used in the lower layer to prevent direct contact between the upper layer or anode and the current collector, resulting in resistance to internal short circuits and punctures. Furthermore, a conductive coating on the current collector surface helps reduce positive electrode impedance and enhance lithium deintercalation activity, resulting in higher battery capacity and cycle capacity retention.
[0096] Furthermore, compared to a physical mixing method (where the first and second active materials are mixed and then applied as a single layer), the first and second active material layers are layered across the thickness of the cathode sheet, avoiding the problem of gel formation caused by significant differences in the properties of the two materials (e.g., particle size, pH, specific surface area). This approach is more suitable for large-scale production.
[0097] Furthermore, in some embodiments of the present application, the first active material is subjected to a battery cell hot box test, and the temperature at which thermal runaway occurs is greater than 160° C.;
[0098] The method of the battery cell hot box test is as follows: a rectangular battery cell is made of the first active material, the battery cell is charged to 100% charge state, the battery cell is restrained by a steel clamp, and the battery cell is placed in an oven for standing. The starting temperature of the oven is 130°C, and the battery cell is left standing for 1 hour to confirm the status; if the battery cell does not fail after standing for 1 hour, the temperature is increased at 5°C / min, and it is left standing for 30 minutes every time the temperature is increased by 5°C, until the battery cell suffers thermal runaway.
[0099] The first active material is capable of not catching fire or exploding at temperatures above 160°C after a cell hot box test, and has excellent resistance to thermal runaway, which further helps reduce the probability of thermal runaway of the battery.
[0100] Furthermore, in some embodiments of the present application, the first active material includes at least one of an olivine structure material or a spinel structure material.
[0101] By selecting at least one of an olivine structure material or a spinel structure material as the first active material, these materials have the characteristic of reducing the probability of thermal runaway of the battery, thereby facilitating reducing the probability of thermal runaway of the battery.
[0102] For example, in some embodiments of the present application, the first active material is selected from either olivine structure material or spinel structure material; or the first active material is selected from a mixture of olivine structure material and spinel structure material, in which the two raw materials can be mixed in any proportion.
[0103] Furthermore, in some embodiments of the present application, the olivine structural material includes at least one of a lithium iron phosphate material, a lithium manganese iron phosphate material, or a lithium vanadium phosphate material.
[0104] The above-mentioned lithium iron phosphate material, lithium manganese iron phosphate material or lithium vanadium phosphate material has excellent characteristics of reducing the probability of battery thermal runaway, is easy to obtain, and is conducive to obtaining a positive electrode sheet with excellent performance.
[0105] Furthermore, in some embodiments of the present application, the lithium manganese iron phosphate material includes:
[0106] Lia A e Mn 1-f B f P 1-g C g O 4-n D n , wherein A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W; B includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb, and Ge; C includes one or more elements selected from the group consisting of B, S, Si, and N; D includes one or more elements selected from the group consisting of S, F, Cl, and Br; a is selected from the range of 0.9 to 1.1, e is selected from the range of 0.001 to 0.1, f is selected from the range of 0.001 to 0.5, g is selected from the range of 0.001 to 0.1, and n is selected from the range of 0.001 to 0.1; and a+e is preferably 0-1.1.
[0107] Furthermore, in some embodiments of the present application, the spinel structure material includes at least one of LiMn2O4, Li2MnNiO4 or lithium titanate materials.
[0108] The above-mentioned LiMn2O4, Li2MnNiO4 or lithium titanate materials have excellent characteristics in reducing the probability of thermal runaway of the battery, which is conducive to obtaining a positive electrode sheet with good performance.
[0109] Furthermore, in some embodiments of the present application, the thickness of the first active material layer is 7 μm to 80 μm.
[0110] By setting the thickness of the first active material layer to 7 μm to 80 μm, within this range, the first active material can fully exert its effectiveness, which is beneficial to miniaturization of the battery.
[0111] Further optionally, in some embodiments of the present application, the thickness of the first active material layer is 15 μm to 50 μm.
[0112] By further limiting the thickness of the first active material layer to 15 μm to 50 μm, within this range, an excellent characteristic of reducing the probability of thermal runaway of the battery can be obtained.
[0113] For example, in some embodiments of the present application, the thickness of the first active material layer is 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm.
[0114] Furthermore, in some embodiments of the present application, the D of the particles contained in the first active material layer is V 50 is 0.5μm~20μm.
[0115] Within the above-mentioned particle size range, a first active material layer with good performance can be easily obtained.
[0116] The above D V 50 means that 50% of the particles in the first active material layer have a diameter larger than this value, and another 50% of the particles have a diameter smaller than this value. Dv50 represents the median particle size of the powder.
[0117] Unless otherwise specified, the particle size distribution parameter Dv50 of the first active material determined by the particle size distribution measurement value in this application is determined by a particle size analyzer-laser diffraction method. Specifically, reference can be made to the standard GB / T19077-2016, using a laser diffraction scattering particle size analyzer and measuring according to the manufacturer's instructions.
[0118] Further optionally, the D of the particles contained in the first active material layer V 50 is 0.6μm~19μm.
[0119] Exemplarily, the D of the particles contained in the first active material layer is V 50 is 0.7μm, 1.0μm, 1.5μm, 2μm, 5μm, 8μm, 10μm or 15μm.
[0120] Furthermore, in some embodiments of the present application, the gram capacity of the second active material is 175 mAh / g to 250 mAh / g.
[0121] By limiting the gram capacity of the second active material to 175 mAh / g to 250 mAh / g, it is beneficial to improve the battery capacity of the battery.
[0122] The above-mentioned gram capacity refers to the capacity per unit mass of the second active material.
[0123] Unless otherwise specified, the test method for gram capacity in this application is: assemble the positive and negative pole pieces disassembled from the battery cell into a pole piece-lithium plate semi-button battery and obtain the button capacity through low-rate charge and discharge, and then divide the capacity by the mass of the pole piece active material to obtain the gram capacity parameter.
[0124] Further optionally, in some embodiments of the present application, the gram capacity of the second active material is 176 mAh / g to 249 mAh / g.
[0125] By further limiting the gram capacity of the second active material to 176 mAh / g to 249 mAh / g, it is beneficial to increase the battery capacity and improve the battery cycle capacity retention rate.
[0126] Illustratively, the gram capacity of the second active material is 178 mAh / g, 190 mAh / g, 195 mAh / g, 200 mAh / g, 210 mAh / g, 220 mAh / g, 230 mAh / g, 240 mAh / g, or 250 mAh / g.
[0127] Furthermore, in some embodiments of the present application, the voltage platform of the second active material is greater than or equal to 3.22V.
[0128] By limiting the voltage platform of the two active materials to be greater than or equal to 3.22V, it is beneficial to improve the battery capacity of the battery.
[0129] Further optionally, the voltage platform of the second active material is 3.5V to 3.9V.
[0130] By further limiting the voltage platform of the second active material to be greater than or equal to 3.22V, it is beneficial to improve the battery capacity of the battery.
[0131] Illustratively, in some embodiments of the present application, the voltage platform of the second active material is 3.6V, 3.7V, 3.8V or 3.9V.
[0132] Furthermore, in some embodiments of the present application, the second active material includes: a layered structure material.
[0133] Layered structural materials have the characteristics of high energy density, which is beneficial to improving the battery capacity of the battery.
[0134] Furthermore, in some embodiments of the present application, the layered structure material includes at least one of a layered ternary material, lithium cobalt oxide, and a lithium-rich manganese-based material.
[0135] Layered ternary materials, lithium cobalt oxide, and lithium-rich manganese-based materials all have the characteristics of high energy density, which is beneficial to improving the battery capacity of the battery.
[0136] Furthermore, in some embodiments of the present application, the layered ternary material includes: Li x (Ni a Co b Mn c ) 1-d M d O 2-y A y , where 0≤a<0.65, 0≤b≤1, 0≤c≤1, 0≤d<1, 0≤y≤1, 0.2≤x≤1.2.
[0137] Furthermore, in some embodiments of the present application, the high nickel ternary material includes: Li x (Ni a Co b Mnc ) 1-d M d O 2-y A y , where 0.65≤a≤1, 0≤b≤1, 0≤c≤1, 0≤d<1, 0≤y≤1, 0.2≤x≤1.2.
[0138] It should be noted that the battery will be accompanied by Li deintercalation and consumption during the charge and discharge process. The molar content of Li is different when the battery is discharged to different states. The limitation of x in the above chemical formula includes the molar content of Li in different charge and discharge states of the battery (usually the battery voltage is between 2-5V).
[0139] Furthermore, in some embodiments of the present application, the lithium-rich manganese-based material includes: nLi2MnO3·(1-n)LiNi b Mn (1-b- c) Z c O2, wherein Z includes at least one element selected from the group consisting of Na, Mg, Al, Ca, Ba, V, Zn, Ti, Fe, Co, Cr, Nb, W, Mo, Zr, Ta, and Hf; 0.1<n<1; 0<b<1; 0<c≤0.2.
[0140] Furthermore, in some embodiments of the present application, the thickness of the second active material layer is 7 μm to 67 μm.
[0141] By setting the thickness of the second active material layer to 7 μm to 67 μm, the characteristics of the second active material can be effectively exerted, and the battery can be miniaturized.
[0142] Furthermore, in some embodiments of the present application, the thickness of the second active material layer is 15 μm to 50 μm.
[0143] By further limiting the thickness of the second active material layer to 15 μm to 50 μm, the battery capacity of the battery can be further improved.
[0144] Illustratively, in some embodiments of the present application, the thickness of the second active material layer is 16 μm, 18 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm or 45 μm.
[0145] Furthermore, in some embodiments of the present application, the D of the particles contained in the second active material layer is V 50 is 1μm~20μm.
[0146] By setting the D of the particles contained in the second active material layer as described above V50 is 1 μm to 20 μm. Within the above range, it is beneficial to form a second active material layer with good performance.
[0147] The above “D V 50 means that 50% of the particles in the second active material layer have a diameter larger than this value, and another 50% of the particles have a diameter smaller than this value. Dv50 represents the median particle size of the powder.
[0148] Unless otherwise specified, the particle size distribution parameter Dv50 of the second active material determined by the particle size distribution measurement value in this application is determined by a particle size analyzer-laser diffraction method. Specifically, reference can be made to the standard GB / T19077-2016, using a laser diffraction scattering particle size analyzer and measuring according to the manufacturer's instructions.
[0149] Further optionally, the D of the particles contained in the second active material layer V 50 is 2μm~19μm.
[0150] For example, in some embodiments of the present application, the D of the particles contained in the second active material layer is V 50 is 3μm, 5μm, 10μm, 12μm or 15μm.
[0151] Furthermore, in some embodiments of the present application, the thickness of the conductive coating is 0.1 μm to 2 μm.
[0152] By setting the thickness of the conductive coating to 0.1 μm to 2 μm, both the miniaturization of the battery and the effectiveness of the conductive layer coating can be taken into account.
[0153] Furthermore, in some embodiments of the present application, the thickness of the conductive coating is 0.5 μm to 1.5 μm.
[0154] The thickness of the conductive coating is further limited to 0.5 μm to 1.5 μm. A thickness less than 0.5 μm is not easy to exert the effect of the conductive coating; a thickness greater than 1.5 μm takes up too much space, which is not conducive to the miniaturization of the battery.
[0155] Illustratively, in some embodiments of the present application, the thickness of the conductive coating is 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm or 1.5 μm.
[0156] Furthermore, in some embodiments of the present application, the conductive coating includes: a conductive agent and a binder.
[0157] The conductive coating has good conductivity and adhesion: the conductivity is mainly achieved through the conductive agent, which helps to reduce the cathode impedance and improve the cathode lithium deintercalation activity, and the corresponding battery exhibits higher capacity, power and low-temperature performance; the adhesion is mainly achieved through the binder, which helps to connect the first active material layer and the current collector more firmly, reduce the shedding of active materials during the electrode slitting and winding process, and is beneficial to long-term reliability.
[0158] Furthermore, in some embodiments of the present application, the conductive coating comprises, by mass percentage, 40% to 60% of a conductive agent and 40% to 60% of a binder.
[0159] Within the above-mentioned ratio range, a conductive coating with good conductivity and good adhesion properties can be obtained.
[0160] Further optionally, in some embodiments of the present application, the conductive coating comprises, by weight percentage, 41% to 59% of a conductive agent and 41% to 59% of a binder.
[0161] For example, in some embodiments of the present application, the conductive coating comprises, by mass percentage, 45% conductive agent and 55% binder; or the conductive coating comprises 48% conductive agent and 52% binder; or the conductive coating comprises 53% conductive agent and 47% binder.
[0162] Furthermore, in some embodiments of the present application, the conductive coating further includes: a neutralizer.
[0163] Adding a neutralizer to the conductive coating to adjust the pH can improve the corrosion resistance of the positive electrode current collector (aluminum foil). At the same time, the neutralizer can form positive and negative charge attraction between the current collector and the first active material layer, further enhancing the adhesion between the first active material layer and the current collector.
[0164] Furthermore, in some embodiments of the present application, the conductive coating comprises, by mass percentage, 40% to 55% of a conductive agent, 40% to 55% of a binder, and 1 to 10% of a neutralizer.
[0165] Within the above-mentioned ratio range, a conductive coating having excellent electrical conductivity, excellent adhesion and good corrosion resistance of the current collector can be obtained.
[0166] Further optionally, in some embodiments of the present application, the conductive coating comprises, by mass percentage, 42% to 50% conductive agent, 42% to 50% binder, and 2% to 8% neutralizer.
[0167] Illustratively, in some embodiments of the present application, the conductive coating comprises, by mass percentage, 50% conductive agent, 43% binder, and 7% neutralizer; or, by mass percentage, the conductive coating comprises, by mass percentage, 45% conductive agent, 45% binder, and 10% neutralizer; or, by mass percentage, the conductive coating comprises, by mass percentage, 48% conductive agent, 45% binder, and 7% neutralizer.
[0168] Furthermore, in some embodiments of the present application, the conductive agent includes at least one of carbon black, carbon nanotubes or graphene.
[0169] At least one of the carbon black, carbon nanotubes or graphene as a conductive agent has high electrical conductivity, which can make the conductive coating have high conductivity, which is beneficial for the battery to exhibit higher capacity.
[0170] Illustratively, in some embodiments of the present application, the conductive agent is selected from any one of carbon black, carbon nanotubes or graphene; or the conductive agent is selected from a mixture of carbon black and carbon nanotubes, and the two can be mixed in any proportion in the mixture; or the conductive agent is selected from a mixture of carbon nanotubes and graphene, and the two can be mixed in any proportion in the mixture; or the conductive agent is selected from a mixture of carbon black and graphene, and the two can be mixed in any proportion in the mixture; or the conductive agent is selected from a mixture of carbon black, carbon nanotubes and graphene.
[0171] Furthermore, in some embodiments of the present application, the binder includes at least one of polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, polyvinylidene fluoride or styrene-butadiene rubber.
[0172] At least one of polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, polyvinylidene fluoride or styrene-butadiene rubber is used as a binder, which has high bonding properties and can make the conductive coating obtain high bonding properties, which is beneficial for a stronger connection between the first active material layer and the current collector, reduces the shedding of active materials during the electrode slitting and winding processes, and improves long-term reliability.
[0173] Illustratively, in some embodiments of the present application, the binder is selected from any one of polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, polyvinylidene fluoride or styrene-butadiene rubber; or, the binder is selected from a mixture of polyacrylic acid and polyvinyl alcohol; or, the binder is selected from a mixture of sodium carboxymethyl cellulose and polyvinylidene fluoride; or, the binder is selected from a mixture of polyvinylidene fluoride and styrene-butadiene rubber; the raw materials in the above mixtures can be mixed in any proportion.
[0174] Furthermore, in some embodiments of the present application, the neutralizing agent includes at least one of calcium hydroxide or lithium hydroxide.
[0175] At least one of calcium hydroxide and lithium hydroxide as a neutralizing agent can effectively adjust the pH of the conductive coating, thereby enhancing the bonding force between the first active material layer and the current collector through electrostatic attraction.
[0176] For example, in some embodiments of the present application, the neutralizing agent is selected from either calcium hydroxide or lithium hydroxide; or the neutralizing agent is selected from a mixture of calcium hydroxide and lithium hydroxide, in which the two raw materials can be mixed in any proportion.
[0177]
[0178] Some specific embodiments are listed below to better illustrate the present application.
[0179] [Positive electrode preparation (I): Olivine structural material]
[0180] Step S1: preparing conductive coating slurry:
[0181] The neutralizer, conductive agent and adhesive are mixed in a specific ratio, then water is added and stirred to form a slurry.
[0182] Step S2: preparing a first active material slurry:
[0183] According to mass percentage, 97.5% of the first active material (olivine structure material), 0.7% of conductive carbon black, and 1.8% of polyvinylidene fluoride (PVDF) were uniformly mixed in an N-methylpyrrolidone (NMP) solvent system and stirred to prepare a slurry.
[0184] Step S3: preparing a second active material slurry:
[0185] According to the mass percentage, 96% of the second active material (layered ternary material), 2% of conductive carbon black, 0.5% of flaky conductive carbon, and 1.5% of polyvinylidene fluoride (PVDF) are mixed uniformly in an N-methylpyrrolidone (NMP) solvent system and stirred to prepare a slurry.
[0186] Step S4: preparing the positive electrode sheet:
[0187] The slurries obtained in step S1, step S2 and step S3 are sequentially coated on the current collector aluminum foil using extrusion coating to form a three-layer coating. The coating weight of the first active material is 150 mg / 1540.25 mm 2 , thickness is 30μm, the coating weight of the second main material is 160mg / 1540.25mm 2 , with a thickness of 40μm.
[0188] Examples 1-21
[0189] A positive electrode sheet is provided, which is prepared using the above-mentioned positive electrode sheet preparation method (I). The material selection, preparation parameters, and performance parameters of each embodiment are shown in Tables 1 to 3.
[0190] Comparative Example 1
[0191] A positive electrode sheet is provided, which is similar to the preparation method of the aforementioned positive electrode sheet, except that: in step S4, the slurries obtained in step S2 and step S3 are first mixed in a mass ratio of 1:1 to obtain a mixed slurry, and then the slurry obtained in step S1 and the mixed slurry are sequentially applied to form two coating layers.
[0192] The material selection, preparation parameters, and performance parameters of Comparative Example 1 are shown in Tables 1 to 3.
[0193] Comparative Example 2
[0194] A positive electrode sheet is provided, which is similar to the preparation method of the above-mentioned positive electrode sheet, except that: in step S4, the slurry obtained in step S1 is not applied; only the slurries obtained in steps S2 and S3 are applied in sequence to form two coating layers.
[0195] The material selection, preparation parameters, and performance parameters of Comparative Example 2 are shown in Tables 1 to 3.
[0196] Comparative Example 3
[0197] A positive electrode sheet is provided, which is similar to the preparation method of the above-mentioned positive electrode sheet, except that: in step S4, the slurry obtained in step S1 is not applied; only the slurries obtained in step S3 and step S2 are applied in sequence to form two coating layers.
[0198] The material selection, preparation parameters, and performance parameters of Comparative Example 3 are shown in Tables 1 to 3.
[0199]
Preparation of lithium-ion batteries
[0200] Lithium-ion batteries were prepared using the positive electrode sheets provided in the aforementioned embodiments and comparative examples, and the performance of the lithium-ion batteries was tested.
[0201] (1) Preparation of lithium-ion batteries:
[0202] The positive electrode sheets provided in the aforementioned embodiments or comparative examples are combined with the negative electrode sheets, injected with electrolyte and packaged to obtain a battery.
[0203] Preparation of negative electrode sheet:
[0204] 95.5 wt% graphite, 1.2 wt% conductive carbon black, 1.8 wt% styrene-butadiene rubber (SBR), and 1.5 wt% sodium carboxymethyl cellulose (CMC) were mixed, deionized water was added, and the mixture was stirred to form a slurry. The slurry was then coated onto a negative electrode current collector copper foil to form a negative electrode sheet. The coating thickness was 50 μm.
[0205] The electrolyte is a solution of 1 mol / L LiPF6 in ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1.
[0206] (2) Test the performance of the battery:
[0207] 1. Needle penetration test method: Charge the battery cell to 100% charge state, restrain the battery cell with a steel fixture with a hole in the middle, use a 2mm diameter steel needle to vertically penetrate the battery cell at 10mm / s at 25℃, and wait for 30 minutes to observe whether the battery cell catches fire.
[0208] 2. Hot box test conditions: Charge the battery cell to 100% state of charge, restrain it with a steel fixture, and place it in an oven. The starting temperature of the oven is 130°C. Let the battery cell stand for 1 hour to confirm the status. If the battery cell does not fail after 1 hour, increase the temperature at 5°C / min and let it stand for 30 minutes every time the temperature rises by 5°C until thermal runaway occurs.
[0209] 3. Capacity test conditions: 1. Let the battery stand at 25℃; 2. Use 0.33C constant current to charge to the cutoff voltage (4.25V for batteries containing high nickel ternary metal and 4.4V for batteries without high nickel ternary metal), then switch to constant voltage charging; 3. Reduce the current to 0.05C and stop charging; 4. Let the battery stand for 30 minutes; 5. Use 0.33C constant current to discharge to the cutoff voltage (such as 2.5V); 6. Let the battery stand for 30 minutes; 7. Repeat steps 2-6 three times, and take the average discharge capacity to measure the capacity.
[0210] 4. Capacity retention rate test conditions: 1. Let the battery cell stand at 25℃; 2. Use 0.33C constant current to charge to the cutoff voltage (4.25V for batteries containing high nickel ternary metal and 4.4V for batteries without high nickel ternary metal), then switch to constant voltage charging; 3. Reduce the current to 0.05C and stop charging; 4. Let the battery cell stand for 30 minutes; 5. Use 0.33C constant current to discharge to the cutoff voltage (such as 2.5V); 6. Let the battery cell stand for 30 minutes; 7. Repeat steps 2-6 200 times, and take the ratio of the discharge capacity in the 500th cycle to the discharge capacity in the first cycle as the capacity retention rate.
[0211] The test results are shown in Table 4.
[0212] Table 1
[0213] Table 2
[0214] Table 3
[0215] Table 4
[0216] From the results in Table 4 above, we can see that:
[0217] In the solutions of Examples 1 to 21 of the present application, the battery did not catch fire when punctured, and did not catch fire when short-circuited. The battery capacity ranged from 127Ah to 221Ah.
[0218] The solution of Comparative Example 1 cannot simultaneously achieve the goal of preventing the battery from catching fire in both the needle puncture and internal short circuit conditions. The battery capacity of Comparative Examples 2 and 3 is only 120 Ah.
[0219] Furthermore, compared with Comparative Examples 2 and 3, the battery hot box test temperature of Example 1 is higher, which shows that Example 1 is more conducive to reducing the probability of battery thermal runaway.
[0220] Furthermore, compared with comparative examples 1-3, Example 1 has a higher capacity retention rate after 500 cycles, showing better cycle stability.
[0221] This shows that the solutions of Examples 1 to 21 of the present application can effectively reduce the probability of battery thermal runaway while also improving battery capacity.
[0222] Furthermore, compared with Comparative Example 1, Example 2 shows that when the first active material is an olivine structure material and the second active material is a layered ternary material: the first active material layer and the second active material layer are layered and arranged in a specific positional relationship; relative to the physical mixing of the first active material and the second active material, the battery capacity is effectively improved; and the probability of thermal runaway of the battery is reduced.
[0223] Furthermore, it can be seen from the comparison between Example 2 and Comparative Example 2 that by providing a conductive coating on the surface of the current collector, it is helpful to reduce the positive electrode impedance and improve the positive electrode lithium insertion and extraction activity, and the battery exhibits a higher capacity.
[0224] Furthermore, compared with Comparative Example 3, Example 1 shows that the hot box test temperature of the battery in Example 1 is higher, which shows that the probability of thermal runaway of the battery in Example 1 is reduced; further, the battery capacity of Example 1 is increased and the capacity retention rate after 500 cycles is higher, showing better capacity performance and cycle stability.
[0225] [Cathode Pole Sheet Preparation (II): Spinel Structure Materials]
[0226] Step S1: preparing conductive coating slurry:
[0227] The neutralizer, conductive agent and adhesive are mixed in a specific ratio, then water is added and stirred to form a slurry.
[0228] Step S2: preparing a first active material slurry:
[0229] According to mass percentage, 94% of the first active material (spinel structure material), 2.5% of conductive carbon black, 1% of graphene, and 2.5% of polyvinylidene fluoride (PVDF) are uniformly mixed in an N-methylpyrrolidone (NMP) solvent system and stirred to prepare a slurry.
[0230] Step S3: preparing a second active material slurry:
[0231] According to the mass percentage, 96% of the second active material (layered ternary material), 2% of conductive carbon black, 0.5% of flaky conductive carbon, and 1.5% of polyvinylidene fluoride (PVDF) are mixed uniformly in an N-methylpyrrolidone (NMP) solvent system and stirred to prepare a slurry.
[0232] Step S4: preparing the positive electrode sheet:
[0233] The slurries obtained in step S1, step S2 and step S3 are sequentially coated on the current collector aluminum foil using extrusion coating to form a three-layer coating. The coating weight of the first active material is 150 mg / 1540.25 mm 2 , thickness is 30μm, the coating weight of the second main body material is 160mg / 1540.25mm 2 , with a thickness of 40μm.
[0234] Example 22-Example 30
[0235] A positive electrode sheet is provided, which is prepared using the above-mentioned positive electrode sheet preparation method (II). The material selection, preparation parameters, and performance parameters of each embodiment are shown in Tables 5 to 7.
[0236] Comparative Example 4
[0237] A positive electrode sheet is provided, which is similar to the preparation method of the aforementioned positive electrode sheet, except that: in step S4, the slurries obtained in step S2 and step S3 are first mixed in a mass ratio of 1:1 to obtain a mixed slurry, and then the slurry obtained in step S1 and the mixed slurry are sequentially applied to form two coating layers.
[0238] The material selection, preparation parameters, and performance parameters of Comparative Example 1 are shown in Tables 5 to 7.
[0239] Comparative Example 5
[0240] A positive electrode sheet is provided, which is similar to the preparation method of the above-mentioned positive electrode sheet, except that: in step S4, the slurry obtained in step S1 is not applied; only the slurries obtained in steps S2 and S3 are applied in sequence to form two coating layers.
[0241] The material selection, preparation parameters, and performance parameters of Comparative Example 2 are shown in Tables 5 to 7.
[0242] Lithium-ion batteries were prepared using the positive electrode sheets provided in the aforementioned Examples 22-30 and Comparative Examples 4-5, and the performance of the lithium-ion batteries was tested.
[0243] The preparation method and the testing method are the same as those of the aforementioned lithium-ion battery.
[0244] The test results are shown in Table 8.
[0245] Table 5
[0246] Table 6
[0247] Table 7
[0248] Table 8
[0249] From the results in Table 8 above, we can see that:
[0250] In the solutions of Examples 22 to 30 of the present application, the battery did not catch fire when punctured, and did not catch fire when short-circuited. The battery capacity ranged from 151Ah to 192Ah.
[0251] However, the solution of Comparative Example 4 cannot satisfy the requirement of preventing the battery from catching fire both in terms of needle puncture and internal short circuit. In Comparative Example 5, the battery capacity is only 145 Ah.
[0252] This shows that the materials selected in the solutions of Examples 22 to 30 of the present application can effectively reduce the probability of battery thermal runaway while also improving battery capacity.
[0253] Furthermore, compared with Comparative Example 4, Example 22 shows that when the first active material is a spinel structure material and the second active material is lithium cobalt oxide: the first active material layer and the second active material layer of Example 22 are layered and arranged in a specific positional relationship; compared with Comparative Example 4, the first active material and the second active material are arranged in a mixed manner, which effectively reduces the probability of thermal runaway of the battery.
[0254] Furthermore, when Example 22 is compared with Comparative Example 5, it can be seen that when the first active material is a spinel structure material and the second active material is lithium cobalt oxide: Example 22 helps to reduce the positive electrode impedance and improve the positive electrode lithium deintercalation activity by setting a conductive coating on the surface of the current collector, and the battery exhibits a higher capacity.
[0255] Compared with comparative examples 4 and 5, the capacity retention rate of Examples 22 to 30 of the present application after 500 cycles is higher, showing better cycle stability.
[0256] [Positive electrode preparation (Part 3): lithium vanadium phosphate, LiMn2O4, Li2MnNiO4]
[0257] Example 31-Example 35
[0258] A positive electrode plate is provided, which is prepared using the above-mentioned positive electrode plate preparation method (II). The material selection, preparation parameters, and performance parameters of Examples 31 to 35 are shown in Tables 9 to 11.
[0259] Lithium-ion batteries were prepared using the positive electrode sheets provided in the aforementioned Examples 31-35, and the performance of the lithium-ion batteries was tested.
[0260] The preparation method and the testing method are the same as those of the aforementioned lithium-ion battery.
[0261] The test results are shown in Table 12.
[0262] Table 9
[0263] Table 10
[0264] Table 11
[0265] Table 12
[0266] From the results in Table 12 above, we can see that:
[0267] In the solutions of Examples 31 to 35 of the present application, the battery did not catch fire when punctured, and did not catch fire when short-circuited. The battery capacity ranged from 105Ah to 166Ah.
[0268] This shows that the materials selected in the solutions of Examples 31 to 35 of the present application can effectively reduce the probability of battery thermal runaway while taking into account the battery capacity.
[0269] Furthermore, the first active material of Example 34 and Example 35 was subjected to a cell hot box test, and the temperature at which thermal runaway occurred was 160°C. Compared with the solution in Examples 31-34 where the first active material was selected to have a thermal runaway temperature greater than 160°C, the battery capacity performance of this solution was average.
[0270] Furthermore, in the solutions of Examples 31 to 35 of the present application, the capacity retention rate of the battery after 500 cycles is 92% to 96%, and the battery has good cycle stability.
[0271] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
Claims
1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a current collector, a conductive coating, a first active material layer, and a second active material layer; the conductive coating is formed on the surface of the current collector; the first active material layer is formed on the surface of the conductive coating; and the second active material layer is formed on the surface of the first active material layer; The first active material layer comprises: a first active material; the second active material layer comprises a second active material; The first active material does not catch fire in a needle puncture test. The method of the needle puncture non-fire test is: a battery cell is made of the first active material, the battery cell is charged to 100% of the charge state, the battery cell is restrained by a steel fixture with a hole in the middle, and a 2mm diameter steel needle is used to vertically penetrate the battery cell at a speed of 10mm / s at 25°C; and the battery cell does not catch fire within 30 minutes of standing; The gram capacity of the second active material is greater than or equal to 165 mAh / g.
2. The positive electrode sheet according to claim 1, characterized in that: The first active material is subjected to a battery cell hot box test, and the temperature at which thermal runaway occurs is greater than 160°C; The method for the battery cell hot box test is: a battery cell is made of the first active material, the battery cell is charged to a 100% charge state, the battery cell is restrained by a steel clamp, the battery cell is placed in an oven and allowed to stand, the starting temperature of the oven is 130°C, and the battery cell is allowed to stand for 1 hour to confirm the state; if the battery cell does not fail after standing for 1 hour, the temperature is increased at 5°C / min, and the battery cell is allowed to stand for 30 minutes every time the temperature is increased by 5°C, until thermal runaway occurs in the battery cell.
3. The positive electrode sheet according to claim 1 or 2, characterized in that: The first active material includes at least one of an olivine structure material and a spinel structure material.
4. The positive electrode sheet according to claim 3, characterized in that: The olivine structure material includes at least one of a lithium iron phosphate material, a lithium iron manganese phosphate material or a lithium vanadium phosphate material.
5. The positive electrode sheet according to claim 3, characterized in that: The spinel structure material includes at least one of lithium titanate, LiMn2O4 or Li2MnNiO4 materials.
6. The positive electrode sheet according to any one of claims 3 to 5, characterized in that: The thickness of the first active material layer is 7 μm to 80 μm.
7. The positive electrode sheet according to any one of claims 3 to 6, characterized in that: The D of the particles contained in the first active material layer v 50 is 0.5μm~20μm.
8. The positive electrode sheet according to any one of claims 3 to 7, characterized in that: The gram capacity of the second active material is 175 mAh / g to 250 mAh / g.
9. The positive electrode sheet according to any one of claims 3 to 8, characterized in that: The voltage platform of the second active material is greater than or equal to 3.22V. Optionally, the voltage platform of the second active material is 3.5V to 3.9V.
10. The positive electrode sheet according to any one of claims 1 to 9, characterized in that: The second active material includes: a layered structure material.
11. The positive electrode sheet according to claim 10, characterized in that: The layered structural material includes at least one of a layered ternary material, lithium cobalt oxide, and a lithium-rich manganese-based material.
12. The positive electrode sheet according to claim 10 or 11, characterized in that: The thickness of the second active material layer is 7 μm to 67 μm; optionally, the thickness of the second active material layer is 15 μm to 50 μm.
13. The positive electrode sheet according to any one of claims 10 to 12, characterized in that: The particles contained in the second active material layer have a D v 50 is 1μm~20μm.
14. The positive electrode sheet according to any one of claims 1 to 13, characterized in that: The thickness of the conductive coating is 0.1 μm to 2 μm; optionally, the thickness of the conductive coating is 0.5 μm to 1.5 μm.
15. The positive electrode sheet according to claim 14, characterized in that: The conductive coating comprises a conductive agent and a binder.
16. The positive electrode sheet according to claim 15, characterized in that: Calculated by mass percentage, the conductive coating comprises: 40% to 60% conductive agent and 40% to 60% binder.
17. The positive electrode sheet according to claim 14, characterized in that: The conductive coating further comprises a neutralizing agent.
18. The positive electrode sheet according to claim 17, characterized in that: Calculated by mass percentage, the conductive coating comprises: 40% to 55% conductive agent, 40% to 55% binder, and 1 to 10% neutralizer.
19. The positive electrode sheet according to any one of claims 15 or 16, characterized in that: The conductive agent includes at least one of carbon black, carbon nanotubes or graphene.
20. The positive electrode sheet according to any one of claims 15 or 16, characterized in that: The binder includes at least one of polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, polyvinylidene fluoride or styrene-butadiene rubber.
21. The positive electrode sheet according to any one of claims 17 or 18, characterized in that: The neutralizing agent includes at least one of calcium hydroxide or lithium hydroxide.
22. A battery, characterized in that: The battery comprises the positive electrode sheet described in any one of claims 1 to 21.
23. An electrical device, characterized in that: The electrical device comprises the battery according to claim 22.
Citation Information
Patent Citations
Lithium ion battery
CN105449269A
Conductive coating slurry as well as preparation method and application thereof
CN113248989A
Lithium supplement positive pole piece, preparation method and lithium ion battery
CN114976312A
High-safety polymer battery positive pole
CN201153140Y
Acupuncture-resistant lithium ion battery pole piece structure
CN218896657U