Synthesis method for layered bimetal-based NANO lanthanum material that synchronously locks phosphorus, removes algae and reduces turbidity, and use thereof
Through the preparation of layered bimetallic nanolanthanum materials, the problems of insufficient loading and weak flocculation capacity of existing phosphorus-locking agents in eutrophication lake management were solved, and efficient flocculation and phosphate adsorption were achieved, which simplified operation The process and reduce costs and significantly improve the phosphorus removal effect.
Patent Information
- Application Number
- PCT/CN2023/095666
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-28
AI Technical Summary
In the treatment of eutrophication lakes, the existing phosphorus locking agent Phoslock has problems such as low loading of lanthanum, weak flocculation capacity, and the inability to effectively exert phosphorus removal performance when there are many solid substances suspended in water. In addition, the traditional management methods are complex, costly and have Ecological risks.
Laminated bimetallic nanolanthanum material is used to regulate the distribution and morphology of lanthanum through co-precipitation reaction and alcohol solution treatment, and combine the anion exchange capacity of LDHs and the complexation reaction in alcohol to prepare nanolanthanum materials with high lanthanum load to achieve Synchronous flocculation and phosphorus locking.
It realizes efficient flocculation and phosphate adsorption, simplifies the operation process, reduces costs, avoids ecological risks, and the lanthanum load is adjustable, which significantly improves the phosphorus removal effect.
Smart Images

Figure CN2023095666_28112024_PF_FP_ABST
Abstract
Description
Synthesis method and application of layered bimetallic nano-lanthanum material for synchronous phosphorus lock, algae removal and turbidity reduction Technical Field
[0001] The present invention belongs to the technical field of environmental functional materials and water treatment, and more specifically relates to a synthesis method and application of a layered bimetallic-based nano-lanthanum material for synchronously locking phosphorus, removing algae and reducing turbidity. Background Art
[0002] Eutrophication of water bodies is a serious global environmental problem, and excessive phosphorus levels in water bodies are a key factor in this problem. Phosphorus control in water bodies has become an important means of curbing eutrophication. In addition to traditional coagulants and precipitants such as iron salts, aluminum salts, and calcium salts, phosphorus control technologies have seen increased research in recent years on high-efficiency phosphorus adsorption agents for natural water bodies such as lakes. Lanthanum, a rare earth element with low toxicity and abundant reserves, has attracted continued attention in the field of phosphorus removal due to its strong affinity for phosphate. Among them, the phosphorus-binding agent Phoslock, used in "Application of Phoslock(TM), an innovative phosphorus binding clay, to two Western Australian waterways: preliminary findings" in Hydrobiologia, Vol. 494, 2003, was developed by the Commonwealth Scientific and Industrial Development Organization (CSIRO) of Australia in the 1990s. Since then, it has been successfully commercialized and used in phosphorus removal efforts in over 200 lakes worldwide, achieving excellent results.
[0003] Phoslcok is a lanthanum-modified bentonite. Douglas (US, 6350383B1.2002-2-26) describes its main synthesis method: a 0.1M LaCl₃ solution is mixed with high-purity bentonite at a liquid-to-solid ratio of 100:1 and stirred for 24 hours for an ion exchange reaction. The mixture is then centrifuged and the ion exchange step repeated once to ensure that La₃⁺ fully replaces the intercalated cations in the bentonite. The final product is washed three times with distilled water to remove any residual La₃⁺, centrifuged, and dried. This product has a lanthanum loading of approximately 5% and a phosphorus removal capacity of approximately 10 mg P / g. This product has been widely used due to its excellent phosphorus-binding properties, its relatively simple synthesis principle and operational steps, and its ease of industrialization. However, this agent still has some drawbacks in practical applications, including low lanthanum loading, weak flocculation ability, and inability to effectively remove phosphorus when the water contains high levels of suspended solids.
[0004] Currently, the Flock and Lock approach is mostly used to manage eutrophic lakes. First, a coagulant such as polyaluminium chloride or ferric chloride is added to remove algae and other particulate matter suspended on the lake surface. Phoslock is then added multiple times to achieve a continuous phosphorus lock. For example, "Management of eutrophication in Lake De Kuil (The Netherlands) using combined flocculant e Lanthanum modified bentonite treatment," published in Water Research (2016, Vol. 97), addresses the eutrophication of Lake De Kuil in the Netherlands. Ferric chloride was added on the first day to settle algae and other suspended matter in the water, followed by multiple additions of Phoslock on the second and third days to achieve phosphorus removal. "Controlling eutrophication by combined bloom precipitation and sediment phosphorus inactivation," published in Water Research (2013, Vol. 47), addresses the eutrophication of Lake Rauwbraken. A mixed agent of PAC and Phoslock was added to precipitate blue-green algae and reduce the total phosphorus content in the lake. Although Flock and Lock can treat eutrophic lakes, it essentially fails to overcome the defects of Phoslock. Moreover, the combined use of coagulants and phosphorus-locking agents will not only increase costs, but also bring more ecological risks.
[0005] Layered double hydroxides (LDHs) are clay minerals with strong anion exchange capacity. They often occur in nature as hydrotalcites and can also be synthesized artificially. The dual properties of LDHs as metal hydroxides and anion exchangers give them great adsorption potential, making them suitable as carrier materials for phosphorus removal agents. Their diverse central metal ions and interlayer anions, along with their flexible and tunable layered structure, offer numerous advantageous properties and have garnered considerable attention in various fields. Numerous studies have examined the use of LDHs for phosphorus removal and coagulation. For example, the article "Adsorption of phosphate by layered double hydroxides in aqueous solutions," published in Applied Clay Science, Vol. 32, 2006, examined the high removal efficiency of various LDHs for orthophosphate (PO4). The article "Size- and surface charge-controlled layered double hydroxides for efficient algal flocculation," published in Environment Science Nano, Vol. 5, 2018, investigated the removal of Microcystis aeruginosa from water using electrostatic adsorption and sediment trapping using Mg / Al-LDHs of varying sizes.
[0006] Lanthanum has attracted attention due to its specific binding to phosphate, but it also has potential coagulation properties. For example, the article "Application of cerium and lanthanum coagulants in wastewater treatment—A comparative assessment to magnesium, aluminum, and iron coagulants" published in Volume 426 of the Chemical Engineering Journal in 2021 studied how LaCl3 can coagulate high-phosphorus wastewater to form dense precipitates and accelerate flocculation. The article "Analysis of the mechanism and application of rare earth lanthanum modified polyferric sulfate" published in Volume 39 of Environmental Chemistry in 2020 studied lanthanum-modified polyferric sulfate. Lanthanum is easily hydrolyzed and robs iron of hydroxyl groups to form cross-copolymers, connecting with each other, growing the chain structure of the flocculant, strengthening the flocculant's precipitation and capturing effect, and accelerating the flocculation rate. Based on the above theory, we hope to use LDHs as a carrier to modify it with lanthanum and develop a new type of lake phosphorus-locking agent. By regulating the distribution and morphology of La, the phosphorus-locking and coagulation capabilities of lanthanum can be exerted.
[0007] Summary of the Invention
[0008] In view of the problems of current methods for treating eutrophic lakes, such as complex operation, increased potential ecological risks, and more manpower and material resources, the present invention provides an LDHs-based nano-lanthanum material that can simultaneously lock phosphorus, remove algae and reduce turbidity.
[0009] The technical solution of the present invention is as follows: a layered bimetallic nano-lanthanum material capable of synchronously flocculating and locking phosphorus, characterized in that it comprises the following steps: 1) preparing a bimetallic salt mixed solution as solution A and a precipitant solution as solution B; 2) measuring a certain amount of solution B, slowly pumping solution A into solution B for a coprecipitation reaction, and continuously stirring the reaction system to mix uniformly, observing that the pH reaches a specific value to terminate the reaction; 3) placing the reaction product obtained in step 2) in a water bath at a certain temperature and allowing it to stand; 4) centrifuging the product in step 3), washing it with distilled water until it is neutral, freeze-drying it, and grinding it into powder to obtain the product LDHs; 5) adding the LDHs to a The method comprises the steps of: stirring the reaction in an alcohol solution of a lanthanum salt having a certain concentration; 6) adjusting the pH of the reaction system in step 5) to a specific value and continuing the stirring reaction; 7) filtering out the product obtained in step 6), washing with alcohol until neutral, and freeze-drying to obtain a layered bimetallic nano-lanthanum material; wherein the bimetallic salt mixed solution in step 1) comprises a divalent metal salt and a trivalent metal salt, wherein the divalent metal salt is a magnesium salt, which is MgCl2 or Mg(NO3)2; and the trivalent metal salt is an iron salt, which is FeCl3 or Fe(NO3)3; the molar ratio of the divalent salt to the trivalent salt of the bimetallic salt is between 2:1 and 4:1, and the total concentration of the bimetallic salt in solution A is 1 to 4 mol·L -1 In step 1), solution B is a NaOH solution with a concentration of 1-3 mol·L -1 ; or the solution B is a mixed solution of NaOH and Na2CO3, wherein the molar concentration of NaOH: the molar concentration of Na2CO3 is between 12:1-8:1; the layered bimetallic nano-lanthanum material is used for flocculation of solid suspended matter in water, and can also adsorb phosphorus in water.
[0010] Furthermore, the pH value at the end of the reaction in step 2) is 9.0-11.0, and the water bath temperature in step 3) is 50° C.-80° C., and the water bath time is 12-24 h.
[0011] Furthermore, in step 5), the lanthanum salt is LaCl3 or La(NO3)3; the lanthanum ion concentration in the alcohol solution of the lanthanum salt is 1-40 g·L -1 ; Step 5) in which the solid-liquid ratio of the reaction mixture is stirred at 1:5-1:200, the stirring time is 12-24h, and the alcohol is methanol or ethanol.
[0012] Furthermore, in step 6), HCl / NaOH is used to adjust the pH of the system, and the concentration of the regulator is 0.1-5 mol·L -1, the system pH is adjusted to 10.0-12.0.
[0013] Furthermore, the layered bimetallic nano-lanthanum material is a Mg / Fe-LDHs-based nano-lanthanum material, referred to as La-MF. The La-MF material is in the form of white powder, the particle size of the La-MF material is 1-10 μm, and the lanthanum loading in the La-MF material is 5-30%.
[0014] Furthermore, the prepared layered bimetallic nano-lanthanum material is used for flocculation of solid suspended matter in water bodies, and can also adsorb phosphorus in water bodies.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) This material uses the hydroxyl groups on the surface of LDHs to adsorb La3+, and [LaCl4] can be generated in the alcohol phase. - 、[LaCl5] 2- The complexed anions are inserted into the LDHs interlayer, thus showing the effect of La 3+ The adsorption capacity is very high, and the lanthanum loading can be controlled by adjusting the lanthanum concentration of the mother liquor. The lanthanum loading of the material can be controlled and adjusted between 5-30%.
[0017] (2) This material is in situ precipitated by adjusting the pH after loading lanthanum, so that the La loaded between the LDHs layers or attached to the surface 3+ Most of them exist in the weak crystalline state of La(OH)3. When the material is added to water, part of the lanthanum will hydrolyze to produce a large amount of positive charge, and complex with the hydroxyl groups on the surface of LDHs to form [La(OH) m (H2O) n ] (3-m)+ The chain structure plays the role of adsorption, electrical neutralization and sediment trapping to quickly settle turbidity and algae suspended matter in the water; and through La 3+ With PO4 3- The specific binding enables the material to exert good long-term phosphorus locking ability.
[0018] (3) Currently, the main method for phosphorus lock in eutrophic lakes is to first add coagulants such as polyaluminium chloride and polyferric chloride to coagulate and settle the solid suspended matter in the lake, and then add the commercial phosphorus passivator Phoslock. During the particle sinking process, it captures and chelates inorganic phosphorus in the water to achieve the effect of phosphorus lock. In contrast, this material can achieve the effect of stable phosphorus removal while flocculating the solid suspended matter. A single addition can achieve multiple effects, which is more convenient and efficient.
[0019] (4) This patent uses a single-drop method to synthesize carrier LDHs, and the single-time synthesis amount can reach dozens or even hundreds of times that of the double-drop method of the patent (CN112237897B). In addition, this patent does not use high-temperature calcination in the synthesis, and the synthesis steps are fewer and simpler, which is conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] FIG1 is a process flow chart of the preparation method of the present invention
[0021] Figure 2a is a SEM image of La-MF-1 prepared in Example 1 of the present invention
[0022] Figure 2b is a TEM image of La-MF-1 prepared in Example 1 of the present invention
[0023] Figure 3 is the XRD pattern of La-MF-1 and the carrier Mg / Fe-LDHs prepared in Example 1 of the present invention
[0024] FIG4 is an XRD pattern of La-MF-2 and carrier Mg / Fe-LDHs prepared in Example 2 of the present invention
[0025] Figure 5 is the XRD pattern of La-MF-3 and the carrier Mg / Fe-LDHs prepared in Example 2 of the present invention
[0026] Figure 6 shows the removal rate of suspended solids and phosphate in water at different dosages of La-MF-1 prepared in Example 1 of the present invention
[0027] FIG7 is a schematic diagram of the structure of La-MF prepared in Example 1 of the present invention DETAILED DESCRIPTION
[0028] The present invention is further described below with reference to specific embodiments.
[0029] Example 1
[0030] 1) Prepare a mixed solution of 0.9 mol·L-1 MgCl2 and 0.3 mol·L-1 FeCl3 double metal salts as solution A, and prepare a precipitant of 2 mol·L-1 NaOH and 0.2 mol·L-1 Na2CO3 as solution B;
[0031] 2) Take a certain amount of solution B and slowly pump solution A into solution B for coprecipitation reaction. Stir the reaction system continuously until the mixture is evenly mixed. When the pH reaches 9.0, the reaction is complete.
[0032] 3) placing the reaction product obtained in step 2) in a 65° C. water bath for 18 hours to perform water bath heating crystallization;
[0033] 4) centrifuging the product from step 3), washing with distilled water until neutral, freeze-drying, and grinding into powder to obtain the product Mg / Fe-LDHs;
[0034] 5) The Mg / Fe-LDHs powder was added to 0.375 g La·L-1 (1 g·L-1 LaCl3·7H2O) ethanol solution and stirred for 12 h. The reaction solid-liquid ratio was 1:50.
[0035] 6) Adjusting the pH of the system in step 5) to 12.0 and continuing stirring for 12 hours;
[0036] 7) Filter out the precipitated reactant in step 6), wash with ethanol until neutral, and freeze-dry to obtain a layered bimetallic nano-lanthanum material (named La-MF-1).
[0037] The material prepared in this example is in the form of a white powder, the carrier Mg / Fe-LDHs presents a flaky structure with a particle size of 1-10 μm, and the lanthanum nanoparticles have a particle size of about 5-10 nm. After digestion, the lanthanum loading was measured by ICP to be 13.12%, indicating that the lanthanum was successfully loaded; lanthanum was distributed in the carrier in the form of nanoparticles, as shown in Figures 2a and 2b; the sample was subjected to XRD testing, and the results are shown in Figure 3. The material retains the characteristic peaks of the carrier LDHs, indicating that the layered structure of the carrier material still exists, and there are no obvious lanthanum-related characteristic peaks in the XRD spectrum, indicating that lanthanum is most likely present in the material in an amorphous or weakly crystalline state; the BET structure shows that the material has a specific surface area of 179.5 m2·g-1, and the pores are mostly mesopores of 2-25 nm. The large specific surface area and rich pore structure are conducive to the adsorption of PO43- by the material.
[0038] Example 2
[0039] 1) Prepare a mixed solution of 0.9 mol·L-1 MgCl2 and 0.3 mol·L-1 FeCl3 double metal salts as solution A, and prepare a precipitant of 2 mol·L-1 NaOH and 0.2 mol·L-1 Na2CO3 as solution B;
[0040] 2) Take a certain amount of solution B and slowly pump solution A into solution B for coprecipitation reaction. Stir the reaction system continuously until the mixture is evenly mixed. When the pH reaches 9.0, the reaction is complete.
[0041] 3) placing the reaction product obtained in step 2) in a 65° C. water bath for 18 hours to perform water bath heating crystallization;
[0042] 4) centrifuging the product from step 3), washing with distilled water until neutral, freeze-drying, and grinding into powder to obtain the product Mg / Fe-LDHs;
[0043] 5) The Mg / Fe-LDHs powder was added to 0.375 g La·L-1 (1 g·L-1 LaCl3·7H2O) ethanol solution and stirred for 12 h. The reaction solid-liquid ratio was 1:50.
[0044] 6) Filter out the precipitated reactant in step 5), wash with ethanol until neutral, and freeze-dry to obtain a layered bimetallic nano-lanthanum material (named La-MF-2).
[0045] The material prepared in this example is in the form of a white powder. The carrier Mg / Fe-LDHs has a flaky structure with a particle size of 1-10 μm. The lanthanum nanoparticles have a particle size of about 5-10 nm. After digestion, the lanthanum loading capacity was measured by ICP to be 8.73%, indicating that the lanthanum was successfully loaded. The sample was subjected to XRD testing, and the results are shown in FIG4 . Since in situ precipitation was not performed after lanthanum loading in this example, the lanthanum is basically present in a free state between the layers and on the surface, and free La cannot be observed by XRD.
[0046] Example 3
[0047] 1) Prepare a mixed solution of 0.9 mol·L-1 MgCl2 and 0.3 mol·L-1 FeCl3 double metal salts as solution A, and prepare a precipitant of 2 mol·L-1 NaOH and 0.2 mol·L-1 Na2CO3 as solution B;
[0048] 2) Take a certain amount of solution B and slowly pump solution A into solution B for coprecipitation reaction. Stir the reaction system continuously until the mixture is evenly mixed. When the pH reaches 9.0, the reaction is complete.
[0049] 3) placing the reaction product obtained in step 2) in a 65° C. water bath for 18 hours to perform water bath heating crystallization;
[0050] 4) centrifuging the product from step 3), washing with distilled water until neutral, freeze-drying, and grinding into powder to obtain the product Mg / Fe-LDHs;
[0051] 5) The Mg / Fe-LDHs powder was added to 0.375 g La·L-1 (1 g·L-1 LaCl3·7H2O) ethanol solution and stirred for 12 h. The reaction solid-liquid ratio was 1:50.
[0052] 6) Filter out the precipitated reaction product in step 5), wash with ethanol until neutral, and freeze-dry.
[0053] 7) The material obtained in step 6) was stirred in 0.2M NH4HCO3 solution for 12 h.
[0054] 8) Filter out the reactant obtained in step 7), wash with distilled water until neutral, and freeze-dry to obtain a layered bimetallic nano-lanthanum material (named La-MF-3).
[0055] The material prepared in this example is in the form of a white powder. The carrier Mg / Fe-LDHs exhibits a flaky structure with a particle size of 1-10 μm. The lanthanum nanoparticles have a particle size of approximately 5-10 nm. After digestion, the lanthanum loading was measured by ICP to be 8.23%, indicating successful lanthanum loading. The sample was subjected to XRD testing, and the results are shown in FIG5 . Since a precipitant was used for in-situ precipitation after lanthanum loading, a large amount of lanthanum was hydrolyzed and combined with carbonate ions to form lanthanum carbonate crystals.
[0056] Application Example 1
[0057] In this application example, La-MF-1 was used as a material to test the flocculation of suspended solids and simultaneous phosphorus removal. A mixed solution containing 2 mg·L-1 of phosphorus, 30 mg·L-1 of kaolin, 10 mg·L-1 of HA, and Microcystis aeruginosa with an absorbance of 0.2 at 680 nm was prepared for the target water treatment. Material dosages were 0.05·L-1, 0.1 g·L-1, 0.2 g·L-1, 0.3 g·L-1, 0.4 g·L-1, and 0.5 g·L-1, respectively. The initial pH was 8.0 to simulate a coagulation experiment. The mixture was stirred at 600 rpm for 2 minutes, then at 120 rpm for 15 minutes. The mixture was allowed to stand for 1 hour, and the supernatant was collected for measurement of turbidity, chlorophyll a concentration, absorbance at 254 nm, and PO₄⁻ concentration.
[0058] As shown in Figure 6, at a La-MF-1 dosage of 0.3 g·L⁻¹, the turbidity removal rate was 97.98%, the chlorophyll a removal rates were 97.86%, the HA removal rates were 91.44%, and the PO₄⁻ ...
[0059] Under the same initial conditions, the La-MF-2 material maintained good removal rates for turbidity, chlorophyll a, and HA, but its phosphorus removal performance was subpar, achieving only a 40% phosphorus removal rate at a material dosage of 0.5 g / L. As shown in Figure 7b, the lanthanum in the material exists in a free state, resulting in hydrolysis and a large positive charge. While this removes suspended matter through adsorption, electrical neutralization, and precipitation capture, it also competes with phosphorus for adsorption sites, significantly reducing phosphorus removal efficiency.
[0060] Application Example 2
[0061] An application example using La-MF-3 as a material to test its basic phosphorus removal and flocculation properties: A solution containing 50 mg·L⁻¹ of phosphorus was prepared to measure its phosphorus adsorption capacity; a solution containing 30 mg·L⁻¹ of kaolin, 10 mg·L⁻¹ of HA, and Microcystis aeruginosa with an absorbance of 0.2 at 680 nm was prepared to test its flocculation performance, with a material dosage of 0.5 g·L⁻¹. With an initial pH of 8.0, the adsorption capacity was measured after reacting at 180 rpm for 72 hours. A simulated coagulation experiment was performed with stirring at 600 rpm for 2 minutes, followed by stirring at 120 rpm for 15 minutes. The mixture was allowed to stand for 1 hour, and the supernatant was collected to measure turbidity, chlorophyll a concentration, and absorbance at 254 nm.
[0062] La-MF-3 has an adsorption capacity of 37.88 mgP / g, demonstrating excellent performance. However, its flocculation performance is poor, with almost no chlorophyll a removal, 9.02% turbidity removal, and 27.42% HA removal. As shown in Figure 7c, the lanthanum in the material exists as stable lanthanum carbonate in the interlayers and on the surface, resulting in good phosphorus removal. However, due to its inability to hydrolyze to produce positive charges and chain structures, its flocculation performance is poor.
[0063] The above-mentioned implementation cases are only some of the implementation cases in the present invention, but the implementation methods of the present invention are not limited to the above-mentioned implementation cases. For example, various forms of combinations of the schemes in the embodiments, and any other changes, modifications, substitutions, and combinations made without departing from the spirit and principles of the present invention should be equivalent replacement methods and are within the scope of protection of the present invention.
Claims
1. A method for preparing a layered bimetallic nano-lanthanum material with synchronous flocculation and phosphorus locking, characterized in that: The method comprises the following steps: 1) preparing a bimetallic salt mixed solution as solution A and a precipitant solution as solution B; 2) measuring a certain amount of solution B, slowly pumping solution A into solution B for coprecipitation reaction, and continuously stirring the reaction system to mix evenly, and observing that the pH reaches a specific value to terminate the reaction; 3) placing the reaction product obtained in step 2) in a water bath at a certain temperature and allowing it to stand; 4) centrifuging the product in step 3), washing with distilled water until neutral, freeze-drying, and grinding into powder to obtain the product LDHs; 5) adding LDHs to an alcohol solution of a certain concentration of lanthanum salt and stirring the solution for reaction; 6) adjusting the pH of the reaction system in step 5) to a specific value and continuing the stirring for reaction; 7) filtering out the product obtained in step 6), washing with alcohol until neutral, and freeze-drying to obtain a layered bimetallic nano-lanthanum material; the bimetallic salt mixed solution in step 1) comprises a divalent metal salt and a trivalent metal salt, wherein the divalent metal salt is a magnesium salt, which is MgCl2 or Mg(NO3)2; the trivalent metal salt is an iron salt, which is FeCl3 or Fe(NO3)3; the molar ratio of the divalent salt to the trivalent salt of the bimetallic salt is between 2:1-4:1, and the total concentration of the bimetallic salt in solution A is 1-4 mol·L -1 In step 1), solution B is a NaOH solution with a concentration of 1-3 mol·L -1 ; or the solution B is a mixed solution of NaOH and Na2CO3, wherein the molar concentration of NaOH: the molar concentration of Na2CO3 is between 12:1-8:1; the layered bimetallic nano-lanthanum material is used for flocculation of solid suspended matter in water, and can also adsorb phosphorus in water.
2. The preparation method according to claim 1, characterized in that: The pH at the end of the reaction in step 2) is 9.0-11.0, and the water bath temperature in step 3) is 50° C.-80° C., and the water bath time is 12-24 hours.
3. The preparation method according to claim 1, characterized in that: In step 5), the lanthanum salt is LaCl3 or La(NO3)3; the lanthanum ion concentration in the alcohol solution of the lanthanum salt is 1-40 g·L -1 ; In step 5), the solid-liquid ratio of the stirring reaction is 1:5-1:200, the stirring time is 12-24h, and the alcohol is methanol or ethanol.
4. The preparation method according to claim 1, characterized in that: In step 6), HCl / NaOH is used to adjust the pH of the system, and the concentration of the regulator is 0.1-5 mol·L -1 , the system pH was adjusted to 10.0-12.
0.
5. The layered bimetallic nano-lanthanum material prepared by the preparation method according to any one of claims 1 to 4 is characterized in that: The layered bimetallic nano-lanthanum material is a Mg / Fe-LDHs-based nano-lanthanum material, referred to as La-MF. The La-MF material is in the form of white powder, the particle size of the La-MF material is 1-10 μm, and the lanthanum loading in the La-MF material is 5-30%.
6. The use of the layered bimetallic nano lanthanum material according to claim 5, characterized in that: The prepared layered bimetallic nano-lanthanum material is used for flocculation of solid suspended matter in water bodies, and can also adsorb phosphorus in water bodies.
Citation Information
Patent Citations
Phosphorus removal agent based on nickel-iron binary hydrotalcite
CN107252674A
Quick-acting water body magnetic nano phosphorus removing agent as well as preparation method and application thereof
CN112138624A
Layered double-metal-based nano lanthanum material as well as preparation method and application thereof
CN112237897A
Synthetic method and application of layered bimetal-based nano lanthanum material capable of synchronously locking phosphorus, removing algae and descending turbidity
CN115072790A
Lanthanide-doped layered double hydroxides and method of producing same
US20200325031A1
Cited By
Lanthanum modified phosphorus removal agent and preparation method thereof
CN120189921A
Composite particle for treating floating algae in water body as well as preparation method and application of composite particle
CN120504377A