Positive electrode material and preparation method therefor, and lithium-ion battery
By using a specific range of microscopic residual stress and average diameter ratios in the positive electrode material, and using cobalt hydroxyl oxide and cobalt hydroxide as cobalt hydroxide as cobalt additives, the problem of excessive surface residual alkali in the preparation of positive electrode material is solved, which is significantly It improves electrochemical performance and thermal stability, and improves the overall performance of lithium-ion batteries.
Patent Information
- Application Number
- PCT/CN2023/097716
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2023-06-01
- Publication Date
- 2024-11-28
AI Technical Summary
During the preparation process, existing positive electrode materials are prone to excessive surface residual alkali, which leads to increased slurry viscosity and jelly phenomenon, affecting battery performance, and there are many types of compounds containing cobalt and unstable performance.
The positive electrode material with a specific range of microscopic residual stress and average diameter to grain diameter ratio is coated by cobalt hydroxyl oxide and cobalt hydroxide as cobalt hydroxide as cobalt additives to make up for lattice defects and improve structural stability and electrochemical performance.
It significantly improves the electrochemical performance and thermal stability of the cathode material, improves the charge and discharge capacity, cycle retention rate and safety performance of lithium-ion batteries, and has a simple process and is easy to mass production.
Smart Images

Figure CN2023097716_28112024_PF_FP_ABST
Abstract
Description
Positive electrode material and preparation method thereof, and lithium ion battery
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Chinese patent application No. 202310575361.8 filed on May 19, 2023, the contents of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to the field of lithium-ion batteries, and in particular to a positive electrode material and a preparation method thereof, and a lithium-ion battery. Background Art
[0004] Power batteries are the energy source for electric vehicles, and battery performance is crucial to the performance of new energy vehicles. As a crucial component of power batteries, positive electrode materials significantly impact battery performance. During the preparation process, positive electrode materials often exhibit excessive amounts of residual alkali on the surface, leading to increased slurry viscosity and even a jelly-like phenomenon during the homogenization process, which is detrimental to battery production and electrical performance. Cobalt-containing compounds, a commonly used coating agent for positive electrode materials, can effectively reduce the amount of residual alkali on the surface.
[0005] However, there are many types of cobalt-containing compounds, including lithium cobaltate, cobalt oxide, cobalt trioxide, etc. Different types of cobalt-containing compounds may improve the electrical performance of the positive electrode material or cause its electrical performance to deteriorate.
[0006] Summary of the Invention
[0007] The object of the present invention is to provide a positive electrode material and a preparation method thereof, and a lithium ion battery, wherein the positive electrode material has a specific range of microscopic residual stress and a specific range of average diameter to grain diameter ratio (D / R), so that the positive electrode material has significantly improved electrochemical performance and thermal stability.
[0008] In order to achieve the above object, the first aspect of the present invention provides a positive electrode material, wherein the microscopic residual stress of the positive electrode material measured by XRD is 0.01-0.15;
[0009] The average diameter of the positive electrode material measured by SEM electron microscopy is D, and the grain diameter measured by XRD is R;
[0010] Among them, D / R is 1.4-2.5.
[0011] A second aspect of the present invention provides a method for preparing a positive electrode material, the method comprising:
[0012] (1) mixing a cathode material precursor, a lithium source, and an additive optionally containing a G element to obtain a mixture I;
[0013] (2) sintering the mixture I in an air or oxygen atmosphere to obtain a cathode material product II;
[0014] (3) mixing the cathode material product II, the cobalt additive, and optionally an additive containing an M element to obtain a mixture III;
[0015] (4) performing a second sintering on the mixture III in an atmosphere of air or oxygen to obtain the positive electrode material;
[0016] The ratio of the peak intensity of the characteristic peak at 38.5° to the peak intensity of the characteristic peak at 37.4° measured by XRD of the cobalt additive is 1:1.1-7.5;
[0017] Wherein, the constant temperature T1 of the first sintering is less than or equal to 1000°C.
[0018] The third aspect of the present invention provides a positive electrode material prepared by the above method.
[0019] A fourth aspect of the present invention provides a lithium-ion battery, comprising the above-mentioned positive electrode material.
[0020] Through the above technical solution, the positive electrode material and preparation method thereof, and the lithium-ion battery provided by the present invention achieve the following beneficial effects:
[0021] The cathode material provided by the present invention has a specific range of microscopic residual stress and a specific range of average diameter to grain diameter ratio (D / R), so that the cathode material has significantly improved electrochemical performance and thermal stability.
[0022] In the method for preparing a positive electrode material provided by the present invention, a cobalt additive containing both cobalt oxyhydroxide and cobaltous hydroxide and having a specific XRD structure, particle size, and particle size distribution is used as a coating agent to prepare the positive electrode material. This can compensate for lattice defects in the positive electrode material matrix, thereby improving the structural stability and electrochemical performance of the positive electrode material prepared thereby.
[0023] In addition, the cobalt additive of the present invention can be used as a coating agent to coat the surface of the positive electrode particles in the coating mixture process without uneven coating or agglomeration of the coating agent.
[0024] Furthermore, compared with traditional single cobalt oxyhydroxide or cobaltous hydroxide, the cobalt additive of the present invention can significantly improve the electrochemical performance of the positive electrode material, so that the charge and discharge capacity, cycle retention rate and safety performance of the lithium-ion battery containing the positive electrode material can be enhanced and improved.
[0025] In addition, the method has simple process and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] FIG1 is an XRD spectrum of the cobalt additives of Example 2 and Comparative Example 1;
[0027] FIG2 is a SEM image of the positive electrode material of Example 1;
[0028] FIG3 is a SEM image of the positive electrode material of Example 12;
[0029] FIG4 is a DSC spectrum of the positive electrode materials of Example 1, Comparative Example 3 and Comparative Example 4. DETAILED DESCRIPTION
[0030] The endpoints of the ranges and any values disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.
[0031] A first aspect of the present invention provides a positive electrode material, characterized in that the microscopic residual stress of the positive electrode material measured by XRD is 0.01-0.15;
[0032] The average diameter of the positive electrode material measured by SEM electron microscopy is D, and the grain diameter measured by XRD is R;
[0033] Among them, D / R is 1.4-2.5.
[0034] In the present invention, the positive electrode material has a specific range of microscopic residual stress and a specific range of the ratio of average diameter to grain diameter (D / R), so that the positive electrode material has excellent electrochemical performance and thermal stability.
[0035] Specifically, in the present invention, when the D / R in the positive electrode material meets the range defined by the present invention, the interface resistance of the positive electrode material particles in contact with each other and the contact area with the electrolyte and the conductive material can be maintained within a reasonable range, while the grains have good crystallinity and size, keeping the lithium ion diffusion path unobstructed and shortening the diffusion distance, thereby increasing the reaction rate, and ultimately making the positive electrode material have low resistance and excellent initial charge and discharge efficiency.
[0036] Furthermore, in the present invention, the positive electrode material is coated and sintered to form a finished product. The cobalt as a coating agent can compensate for the lattice defects inside the positive electrode material and will not cause changes in the valence state of nickel and manganese elements in the positive electrode material. It can improve the stability of the material and ultimately make the positive electrode material have low microscopic residual stress, indicating that the positive electrode material has excellent structural stability and is not prone to cracking during the preparation process.
[0037] In the present invention, the crystallite diameter R of the positive electrode material refers to the crystallite diameter calculated by Rydberg analysis from a powder X-ray diffraction pattern obtained by powder X-ray diffraction measurement using CuKα radiation. Software for Rydberg analysis includes, but is not limited to, TOPAS, Rietan, JANA, and JADE.
[0038] In the present invention, the average particle size D of the positive electrode material is the average diameter of 300 representative particles in a scanning electron microscope image.
[0039] In the present invention, the microscopic residual stress of the positive electrode material is obtained by X-ray diffraction testing and refinement, wherein the XRD test scanning range is 10°≤2θ≤90°, the scanning rate is 5° / min, and Topas refinement software and Pawley full spectrum fitting method are used.
[0040] Furthermore, the microscopic residual stress of the positive electrode material measured by XRD is 0.01-0.15.
[0041] Furthermore, D / R is 1.4-2.
[0042] According to the present invention, the average diameter D of the positive electrode material is 1-3 μm.
[0043] The inventors of the present invention have found that the smaller the average diameter D of the positive electrode material, the smaller the single crystal particles of the positive electrode material; the larger the D, the larger the single crystal particles of the positive electrode material. If the D value is too small, the degree of single crystallization will be reduced, the adhesion between the single crystal particles will increase, and it may even approach a polycrystalline structure due to difficulty in single crystallization, causing the positive electrode material to crack and pulverize during the cycle, resulting in a cycle drop. If the D value is too high, the paths for lithium ion transmission within the particles will increase, reducing the lithium ion transmission capacity and increasing the impedance of its transmission, thereby increasing the internal resistance of the battery and reducing the capacity. In the present invention, when the average diameter of the positive electrode material meets the above range, it can avoid the cracking and pulverization of the positive electrode material and ensure that the positive electrode material has low impedance and high charge and discharge capacity.
[0044] Furthermore, the average diameter D of the positive electrode material is 1.5-2 μm.
[0045] According to the present invention, the grain diameter R of the positive electrode material is 700-1200 nm.
[0046] In the present invention, when the grain diameter R of the positive electrode material meets the above range, the positive electrode material has high grain purity and crystallinity, and can provide a suitable diffusion path for lithium ion diffusion, further reducing the internal resistance of the single crystal particles. If the grain diameter R is too large, the diffusion path of lithium ions during charging and discharging will become longer, resulting in a high internal resistance of the single crystal particles. If R is too small, it indicates that the crystallinity and purity of the positive electrode material particles are low, and the particles contain inactive crystalline phases and non-crystalline impurity phases. This prevents the smooth insertion and removal of lithium ions, resulting in a high resistance.
[0047] Furthermore, the grain diameter R of the positive electrode material is 900-1000 nm.
[0048] In the present invention, when the microscopic residual stress and grain size of the positive electrode material simultaneously meet the ranges defined by the present invention, the positive electrode material can be guaranteed to have high charge and discharge capacity while having excellent cycle performance.
[0049] According to the present invention, the median particle size D50 of the positive electrode material is 3-4.5 μm.
[0050] According to the present invention, the mixed nickel content of the positive electrode material is 0-4 wt%.
[0051] In the present invention, the mixed nickel content refers to the Ni 2+ The proportion of total Ni can be measured by XRD refinement.
[0052] In the present invention, the positive electrode material has a low mixed nickel content, which makes the positive electrode material have a high structural stability. Especially under high voltage, it can effectively inhibit the dissolution and structural destruction of the positive electrode active material particles, thereby improving the chemical stability of the material and extending the battery cycle life.
[0053] Furthermore, the mixed nickel content of the positive electrode material is 0-3 wt%.
[0054] In a specific embodiment of the present invention, the positive electrode material is a cobalt-coated positive electrode material.
[0055] According to the present invention, the positive electrode material includes a substrate and a coating layer coated on the substrate;
[0056] The matrix has a composition shown in Formula I:
[0057] Li 1+a Ni x Mn y Co z G b O2 Formula I;
[0058] Where, -0.05 ≤ a ≤ 0.1, 0 ≤ b ≤ 0.05, 0.5 ≤ x < 1, 0 < y < 0.5, 0 ≤ z < 0.5; G is selected from at least one of W, V, Ta, Zr, La, Ce, Er, Sr, Si, Al, Mg and Y;
[0059] The coating layer comprises a cobalt-containing lithium oxide and / or a cobalt-containing oxide;
[0060] Optionally, the coating layer further comprises a lithium oxide containing M element and / or an oxide containing M element, and M is selected from at least one of B, Al, Nb, Mn, Mo, W, Si, Mg, Ti and Zr.
[0061] Furthermore, in Formula I, 0.01 ≤ a ≤ 0.1, 0 ≤ b ≤ 0.005, 0.5 ≤ x < 1, 0 < y < 0.2, 0 ≤ z < 0.3; G is selected from at least one of W, V, Ta, Zr, Sr, Si and Y;
[0062] M is selected from at least one of B, Al, W, Mg, Ti and Zr.
[0063] In the present invention, for the lithium oxide containing M element and the lithium oxide containing cobalt element, in addition to the metal elements M and Li, or Co and Li, it further comprises at least one of Ni, Mn and G.
[0064] According to the present invention, the molar amount n'(Co) of cobalt element in the coating layer, the molar amount n(M) of M element in the coating layer, and the total molar amount [n(Ni) + n(Co) + n(Mn) + n(G)] of metal elements other than Li in the matrix satisfy:
[0065] 0.001 ≤ n'(Co):[n(Ni) + n(Co) + n(Mn) + n(G)] ≤ 0.05;
[0066] 0 ≤ n(M):[n(Ni) + n(Co) + n(Mn) + n(G)] ≤ 0.05.
[0067] In the present invention, when the contents of the cobalt-containing coating layer and the M-containing coating layer in the cathode material are controlled to meet the above ranges, the migration speed and transmission efficiency of Li + can be increased, and further the conductivity of the cathode material is increased, so that the prepared cathode material has higher reaction activity and utilization rate.
[0068] Furthermore, the molar amount of the cobalt element n'(Co) in the coating layer, the molar amount of the M element n(M) in the coating layer, and the total molar amount of the metal elements other than Li in the matrix [n(Ni)+n(Co)+n(Mn)+n(G)] satisfy the following:
[0069] 0.01≤n'(Co):[n(Ni)+n(Co)+n(Mn)+n(G)]≤0.03;
[0070] 0≤n(M): [n(Ni)+n(Co)+n(Mn)+n(G)]≤0.01.
[0071] According to the present invention, the residual alkali content of the positive electrode material is 1000-10000 ppm.
[0072] In the present invention, the surface of the positive electrode material has a low residual alkali content and is cobalt-coated, so that the positive electrode material has small volume change and heat change during the reaction process, thereby improving the thermal stability of the lithium-ion battery containing the positive electrode material and enhancing the safety.
[0073] Furthermore, the residual alkali content of the positive electrode material is 1000-6000 ppm.
[0074] In a specific embodiment of the present invention, when 0.5≤x<0.8, the residual alkali content of the positive electrode material is 1000-3000 ppm, preferably 2000-3000 ppm.
[0075] In a specific embodiment of the present invention, when 0.8≤x<1, the residual alkali content of the positive electrode material is 4000-6000 ppm, preferably 4000-5000 ppm.
[0076] In the present invention, as long as the positive electrode material has the characteristics described in the first aspect of the present invention, the lithium-ion battery containing the positive electrode material can have excellent electrochemical performance. As for the preparation method of the positive electrode material, as long as it can produce the positive electrode material described in the first aspect of the present invention, it falls within the scope of protection of the present invention.
[0077] In the present invention, in order to further reduce the micro stress and the content of mixed nickel in the positive electrode material and improve the thermal stability, etc., preferably, the second aspect of the present invention also provides a method for preparing the positive electrode material, the method comprising:
[0078] (1) mixing a cathode material precursor, a lithium source, and an additive optionally containing a G element to obtain a mixture I;
[0079] (2) sintering the mixture I in an air or oxygen atmosphere to obtain a cathode material product II;
[0080] (3) mixing the cathode material product II, the cobalt additive, and optionally an additive containing an M element to obtain a mixture III;
[0081] (4) performing a second sintering on the mixture III in an atmosphere of air or oxygen to obtain the positive electrode material;
[0082] The ratio of the peak intensity of the characteristic peak at 38.5° to the peak intensity of the characteristic peak at 37.4° measured by XRD of the cobalt additive is 1:1.1-7.5;
[0083] Wherein, the constant temperature T1 of the first sintering is less than or equal to 1000°C.
[0084] In the method for preparing the positive electrode material provided by the present invention, a cobalt additive containing both cobalt oxyhydroxide and cobaltous hydroxide is used as a coating agent. Cobalt oxyhydroxide and cobaltous hydroxide can be converted into each other, and the Co 2+ and Co 3+ The dynamic balance of ions keeps the coating stable under different environments. The cobalt additive has a specific XRD structure, particle size and particle size distribution, which can compensate for the lattice defects in the cathode material matrix, thereby improving the structural stability and electrochemical performance of the cathode material.
[0085] Specifically, a high-temperature solid-phase method is used to combine a cobalt additive with a cathode material process product II to produce a cobalt additive-coated cathode material. At high temperature, cobaltous hydroxide can reduce the residual alkali content on the surface of the cathode material, improve the homogenization efficiency, and improve the conductivity of the cathode material. The valence of cobalt in cobalt oxyhydroxide is +3, which is the same as the average valence of nickel, cobalt and manganese in the cathode material. It can well enter the interior of the material to compensate for lattice defects without causing changes in the valence of nickel and manganese elements in the material, thereby stabilizing the material and reducing the microscopic residual stress of the cathode material.
[0086] In the present invention, the peak intensity ratio of the peak at 38.5° and the peak at 37.4° in the XRD of the cobalt additive is regulated by adjusting the content ratio of cobalt oxyhydroxide to cobaltous hydroxide. When the peak intensity ratio is within a specific range, the cobalt additive as a coating agent is added to the positive electrode material to effectively improve the electrochemical performance and thermal stability of the positive electrode material.
[0087] In addition, the cobalt additive of the present invention can be well coated on the surface of the positive electrode particles during the coating mixture process as a coating agent, without uneven coating or agglomeration of the coating agent.
[0088] Furthermore, compared with traditional single cobalt oxyhydroxide or cobaltous hydroxide, the cobalt additive of the present invention can significantly improve the electrochemical performance of the positive electrode material, so that the charge and discharge capacity, cycle retention rate and safety performance of the lithium-ion battery containing the positive electrode material can be enhanced and improved.
[0089] In the present invention, controlling the constant temperature T1 of the first sintering process to meet the above range can promote the growth and arrangement of the positive electrode material grains, reduce grain boundaries and voids, and achieve smoother spatial transport of electrons and ions, thereby improving electrochemical performance. It can also change and optimize the material's crystal structure, thereby increasing material stability. Furthermore, this method is simple and amenable to mass production.
[0090] Furthermore, the ratio of the peak intensity of the characteristic peak at 38.5° to the characteristic peak at 37.4° of the cobalt additive measured by XRD is 1:2-4.5.
[0091] Furthermore, the constant temperature T1 of the first sintering is 700-1000°C.
[0092] According to the present invention, the median particle size D of the cobalt additive is (Co)50 The particle size distribution K of the cobalt additive is 0.5-5 μm; (Co)90 =(D (Co)90 -D (Co)10 ) / D (Co)50 Satisfy 0.8≤K 90 ≤2.
[0093] In the present invention, by controlling the median particle size D of the cobalt additive (Co)50 And the particle size distribution K (Co)90 When the range defined by the present invention is met, the obtained cathode material can be guaranteed to have excellent electrochemical properties while reducing production costs and enabling mass production. Specifically, when the powder particles of the cobalt additive are too large, the coating uniformity of the cathode material process product II will be reduced, and it may even be enriched on the surface of the cathode material, causing partial exposure of the cathode material, thereby affecting the electrochemical performance of the product. When the powder particles are too small, more sophisticated production equipment is required, and the degree of damage to the equipment during the production process will increase sharply, resulting in increased production costs and being unfavorable for industrial mass production.
[0094] Furthermore, the median particle size D of the cobalt additive is (Co)50 The particle size distribution K of the cobalt additive is 0.5-3 μm; (Co)90 =(D (Co)90 -D (Co)10 ) / D (Co)50 Satisfy 1≤K (Co)90 ≤1.8.
[0095] In the present invention, there is no particular limitation on the preparation method of the cobalt additive, and the cobalt additive can be prepared by conventional methods in the art, as long as the prepared cobalt additive has the specific XRD structure defined in the present invention. Preferably, in the present invention, cobalt oxyhydroxide and cobaltous hydroxide are mixed and crushed to obtain the cobalt additive.
[0096] In the present invention, the mixture of cobaltous oxyhydroxide and cobaltous hydroxide can be crushed by conventional methods in the art, such as jet milling.
[0097] In the present invention, there is no particular limitation on the amount of cobalt oxyhydroxide and cobaltous hydroxide and the crushing conditions, as long as the cobalt additive can have the ratio of the peak intensity of the characteristic peak at 38.5° to the characteristic peak at 37.4°, the median particle size D 50 And the particle size distribution K 90 That's it.
[0098] According to the present invention, based on the total weight of the cobalt additive, the content of Co element is 55-75 wt%.
[0099] According to the present invention, the constant temperature time t1 of the first sintering is less than or equal to 15 hours, preferably 6-12 hours.
[0100] In the present invention, there is no particular limitation on the constant temperature T2 of the second sintering, as long as 1000° C. ≥ T1 > T2 ≥ 300° C. Specifically, the constant temperature T2 is 300-800° C., preferably 300-700° C.
[0101] In the present invention, there is no particular limitation on the constant temperature time t2 of the second sintering, as long as 15 h ≥ t1 > t2 ≥ 5 h is ensured. Specifically, the constant temperature time t2 is 6-12 h, preferably 6-10 h.
[0102] According to the present invention, the total molar amount of metal elements in the positive electrode material precursor [n(Ni)+n(Mn)+n(Co)], the molar amount of Li element in the lithium source n(Li), and the molar amount of G element in the G element-containing additive n(G) are used in an amount such that: 0.95≤n(Li) / [n(Ni)+n(Mn)+n(Co)]≤1.1;
[0103] 0≤n(G) / [n(Ni)+n(Mn)+n(Co)]≤0.05.
[0104] Furthermore, the total molar amount of metal elements in the positive electrode material precursor [n(Ni)+n(Mn)+n(Co)], the molar amount of Li element in the lithium source n(Li), and the molar amount of G element in the G element-containing additive n(G) are used so that: 1≤n(Li) / [n(Ni)+n(Mn)+n(Co)]≤1.1;
[0105] 0.0005≤n(G) / [n(Ni)+n(Mn)+n(Co)]≤0.03.
[0106] In the present invention, the cathode material precursor is selected from nickel-cobalt-manganese oxide and / or nickel-cobalt-manganese hydroxide.
[0107] In the present invention, there is no particular limitation on the type of lithium source, and it may be a conventional lithium source in the art, such as lithium carbonate and / or lithium hydroxide.
[0108] In the present invention, there is no particular limitation on the type of additive containing the G element, and it may be a conventional compound in the art capable of providing the G element, such as a G-containing oxide, a G-containing hydroxide, or a G-containing carbonate.
[0109] In the present invention, G is selected from at least one of W, V, Ta, Zr, La, Ce, Er, Sr, Si, Al, Mg and Y.
[0110] According to the present invention, the total molar amount of metal elements in the positive electrode material process product II [n(Ni)+n(Co)+n(Mn)+n(G)], the molar amount of cobalt element in the cobalt additive n'(Co) and the molar amount of M element in the M element-containing additive n(M) are used in an amount such that: 0.001≤n'(Co) / [n(Ni)+n(Co)+n(Mn)+n(G)]≤0.05;
[0111] 0≤n(M) / [n(Ni)+n(Co)+n(Mn)+n(G)]≤0.05.
[0112] Furthermore, the total molar amount of metal elements in the positive electrode material process product II [n(Ni)+n(Co)+n(Mn)+n(G)], the molar amount of cobalt element in the cobalt additive n'(Co), and the molar amount of M element in the M element-containing additive n(M) are used so that: 0.001≤n'(Co)[n(Ni)+n(Co)+n(Mn)+n(G)]≤0.03;
[0113] 0≤n(M) / [n(Ni)+n(Co)+n(Mn)+n(G)]≤0.03.
[0114] In the present invention, there is no particular limitation on the type of the additive containing the M element, and it may be a conventional compound in the art capable of providing the M element, such as an M-containing oxide, an M-containing hydroxide, or an M-containing carbonate.
[0115] In the present invention, M is selected from at least one of B, Al, Nb, Mn, Mo, W, Si, Mg, Ti and Zr.
[0116] The third aspect of the present invention provides a positive electrode material prepared by the above method.
[0117] A fourth aspect of the present invention provides a lithium-ion battery, comprising the above-mentioned positive electrode material.
[0118] The present invention will be described in detail below by way of examples.
[0119] (1) Morphology test: obtained by scanning electron microscope S-4800 of Hitachi, Japan; the average particle size D of the positive electrode material was calculated from 300 particles in the electron microscope image;
[0120] (2) Particle size D50, D10, D90: measured by Marvern's Hydro 3000mu laser particle size analyzer;
[0121] (3) XRD test: directly measured by Rigaku Smartlab 9KW rotating target diffractometer or / and obtained by refinement; the grain diameter R of the positive electrode material, the microscopic residual stress and the ratio of the peak intensity of the 38.5° characteristic peak to the 37.4° characteristic value in the cobalt additive are calculated; the lithium nickel mixing value is calculated by refinement;
[0122] (4) The residual alkali content of the positive electrode material is measured by a Swiss Metrohm potentiometric titrator.
[0123] (5) The mass of Co element in the total compound: determined by inductively coupled plasma (ICP) atomic emission spectroscopy;
[0124] (6) Electrochemical performance test:
[0125] In the above embodiments and comparative examples, the electrochemical performance of the positive electrode materials was tested using CR2025 button batteries.
[0126] The preparation process of CR2025 button battery is as follows:
[0127] Pole sheet preparation: The positive electrode material, conductive carbon black and polyvinylidene fluoride (PVDF) were mixed with an appropriate amount of N-methylpyrrolidone (NMP) in a mass ratio of 95:3:2 to form a uniform slurry. The slurry was coated on aluminum foil and dried at 120°C for 12 hours. It was then stamped with a pressure of 100 MPa to form a positive electrode sheet with a diameter of 12 mm and a thickness of 3.2 mm. The positive electrode material loading was 15.5 mg / cm 2 .
[0128] Battery Assembly: In an argon-filled glove box with water and oxygen contents less than 5 ppm, the positive electrode, separator, negative electrode, and electrolyte were assembled into CR2025 button cells and allowed to rest for 6 hours. The negative electrode used a 15.8 mm diameter, 1 mm thick lithium metal sheet; the separator used a 25 μm thick polypropylene microporous membrane (Celgard 2325); and the electrolyte used a 1 mol / L mixture of equal parts LiPF6, ethylene carbonate (EC), and diethyl carbonate (DEC).
[0129] Electrochemical performance test:
[0130] In the following examples and comparative examples, the electrochemical performance of CR2025 button cells was tested using a Shenzhen Xinwell battery testing system. The charge and discharge voltage range was controlled at 2.8-4.5V. At a constant temperature of 60°C, the button cells were charged and discharged twice at 0.1C and then 80 times at 1C to evaluate the high-temperature cycle capacity retention of the positive electrode material.
[0131] Thermal stability test:
[0132] The thermal stability of the material was tested using Mettler DSC3+. The steps are as follows:
[0133] The above battery was charged and discharged twice at 0.2C CC-CV and a voltage range of 3-4.4V, and then charged to 4.4V using 0.2C CC-CV. After charging, the battery was disassembled and the positive electrode material was scraped off the electrode sheet. Then, 1g of the positive electrode material scraped off the electrode sheet was weighed and a DSC test was performed to evaluate the thermal stability of the positive electrode material.
[0134] The raw materials used in the examples and comparative examples are all commercially available products.
[0135] Example 1
[0136] S1, mixing cobalt oxyhydroxide and cobaltous hydroxide, adjusting the air flow mill crushing strength to obtain D 50 The cobalt additive has a diameter of 0.96 μm and the peak intensity ratio of 38.5° to 37.4° in the XRD of the cobalt additive is 1:2. The specific parameters of the cobalt additive are shown in Table 1.
[0137] S2, Ni 0.6 Co 0.2 Mn 0.2 (OH)2 was coated and mixed with lithium carbonate and ZrO2 in a molar ratio of [n(Ni)+n(Co)+n(Mn)]:n(Li):n(Zr)=1:1.03:0.0002 to obtain a mixture I;
[0138] S3. The mixture I is subjected to a first sintering in an air atmosphere in a muffle furnace at a constant temperature T1 of 950° C. for a constant temperature time t1 of 8 h. The mixture is crushed by a jet mill and sieved to obtain a cathode material product II.
[0139] S4, coating and mixing the cathode material product II with the cobalt additive prepared in step (1) and Al2O3 in a molar ratio of [n(Ni)+n(Co)+n(Mn)+n(Zr)]:n(Co):n(Al)=1:0.02:0.0001 to obtain a uniform mixture III;
[0140] S5. Under an air or oxygen atmosphere, the mixture III is subjected to a second sintering process at a constant temperature T2 of 700°C for a constant temperature time t2 of 10 hours. The mixture is then directly sieved to obtain positive electrode material A1. Some process conditions and the composition of positive electrode material A1 are detailed in Table 2.
[0141] The physicochemical parameters of the positive electrode material A1 were tested, and the results are shown in Table 3.
[0142] The positive electrode material A1 was assembled into a CR2025 button cell, and the electrochemical performance and thermal stability of the cell were tested. The results are shown in Table 4.
[0143] Example 2
[0144] The method of Example 1 was followed, except that in step S1, the ratio of cobalt oxyhydroxide to cobaltous hydroxide was adjusted so that the peak intensity ratio of 38.5° to 37.4° in the XRD of the cobalt additive was 1:4, thereby obtaining positive electrode material A2.
[0145] Example 3
[0146] The method of Example 1 is carried out, except that in step S2, Ni 0.8 Co 0.1 Mn 0.1 (OH)2 replaces Ni 0.6 Co 0.2 Mn 0.2 (OH)2, and other factors remain unchanged to obtain positive electrode material A3.
[0147] Example 4
[0148] The method of Example 1 was followed, except that in step S1, the ratio of cobalt oxyhydroxide to cobaltous hydroxide was adjusted so that the peak intensity ratio of 38.5° to 37.4° in the XRD of the cobalt additive was 1:7, thereby preparing positive electrode material A4.
[0149] Example 5
[0150] The method of Example 1 was followed, except that in step S4, no Al2O3 was added, and only a cobalt additive was added, [n(Ni)+n(Co)+n(Mn)+n(Zr)]:n(Co)=1:0.02, and other factors remained unchanged, to produce positive electrode material A5.
[0151] Example 6
[0152] The method of Example 1 is carried out, except that in step S2, Ni 0.6 Co 0.2 Mn 0.2 The positive electrode material A6 is prepared by mixing (OH)2 with lithium carbonate, Al2O3 and SrCO3 in a molar ratio of [n(Ni)+n(Co)+n(Mn)]:n(Li):n(Al):n(Sr)=1:1.03:0.00015:0.00005, with other factors remaining unchanged.
[0153] Example 7
[0154] The method of Example 1 was followed, except that in step S1, the ratio of cobalt oxyhydroxide to cobaltous hydroxide was adjusted so that the peak intensity ratio of 38.5° to 37.4° in the XRD of the cobalt additive was 1:1.4, thereby obtaining positive electrode material A7.
[0155] Example 8
[0156] The method of Example 1 is followed, except that in step S4, the positive electrode material process product II is coated and mixed with the cobalt additive obtained in step S1 and Al2O3 in a molar ratio of [n(Ni)+n(Co)+n(Mn)+n(Zr)]:n(Co):n(Al)=1:0.01:0.0001, and the other factors remain unchanged to obtain the positive electrode material A8.
[0157] Example 9
[0158] The method of Example 1 is followed, except that in step S4, the positive electrode material process product II is coated and mixed with the cobalt additive obtained in step S1 and Al2O3 in a molar ratio of [n(Ni)+n(Co)+n(Mn)+n(Zr)]:n(Co):n(Al)=1:0.04:0.0001, and the other factors remain unchanged to obtain the positive electrode material A9.
[0159] Example 10
[0160] The method of Example 1 was followed, except that in step S3, the mixture I was subjected to a first sintering, the constant temperature T1 was changed to 930° C., the constant temperature time t1 was changed to 9.5 h, and other parameters remained unchanged, thereby obtaining a positive electrode material A10.
[0161] Example 11
[0162] The method of Example 1 was followed, except that in step S3, the mixture I was subjected to a first sintering, the constant temperature T1 was changed to 980° C., the constant temperature time t1 was changed to 7 h, and other parameters remained unchanged, to obtain the positive electrode material A11.
[0163] Example 12
[0164] The method of Example 1 was followed, except that in step S1, the crushing strength of the jet mill was adjusted so that the D 50 The positive electrode material D3 was obtained.
[0165] Example 13
[0166] The method of Example 1 was followed, except that in step S1, the crushing strength of the jet mill was adjusted so that the D 50 1.2μm, K 90 is 2.2, and the positive electrode material A13 is obtained.
[0167] Comparative Example 1
[0168] The method of Example 1 was followed, except that in step S1, the ratio of cobalt oxyhydroxide to cobaltous hydroxide was adjusted so that the peak intensity ratio of 38.5° to 37.4° in the XRD of the cobalt additive was 1:8, thereby preparing the positive electrode material D1.
[0169] Comparative Example 2
[0170] The method of Example 1 was followed, except that in step S1, the ratio of cobalt oxyhydroxide to cobaltous hydroxide was adjusted so that the peak intensity ratio of 38.5° to 37.4° in the XRD of the cobalt additive was 1:0.2, thereby preparing the positive electrode material D2.
[0171] Comparative Example 3
[0172] The method of Example 1 was followed, except that only cobalt oxyhydroxide was used in step S1 to obtain positive electrode material D3.
[0173] Comparative Example 4
[0174] The method of Example 1 was followed, except that only cobaltous hydroxide was used in step S1 to obtain positive electrode material D4.
[0175] Comparative Example 5
[0176] The method of Example 1 was followed, except that in step S3, the constant temperature T1 of the first sintering was 1020° C., and the other conditions remained unchanged to obtain a positive electrode material D5.
[0177] Table 1
[0178] Table 2
[0179] Table 2 (continued)
[0180] Table 2 (continued)
[0181] Table 2 (continued)
[0182] Table 2 (continued)
[0183] Table 2 (continued)
[0184] Table 3
[0185] Table 4
[0186] Figure 1 is the XRD spectra of the cobalt additives of Example 2 and Comparative Example 1. It can be seen from Tables 1 and 4 that the peak intensity ratios of the XRD at 38.5° and 37.4° in the cobalt additive are different, so that when the positive electrode material is used in a lithium ion battery, the electrical performance of the lithium ion battery is also quite different; when the peak intensity ratio of the XRD at 38.5° and 37.4° in the cobalt additive is within the range defined by the present invention, when the positive electrode material prepared therefrom is used in a lithium ion battery, the battery exhibits a higher capacity and excellent cycle retention rate.
[0187] It can be seen from Examples 1, 2, and 7 and Comparative Examples 1 and 2 that when the peak intensity ratio of the cobalt additive XRD in Examples 1 and 2 is within the range defined in the present invention, relative to Examples 1 and 2, the peak intensity ratio of the cobalt addition in Example 7 is not within the preferred range of the present invention, and the capacity and cycle retention rate of the lithium ion battery prepared from the positive electrode material are reduced. When it is still significantly higher than that of Comparative Examples 1 and 2, and the peak intensity ratio of the cobalt additive XRD in Comparative Examples 1 and 2 is not within the range defined in the present invention, the capacity of the lithium ion battery containing the positive electrode materials prepared in Comparative Examples 1 and 2 is reduced, and the rate and cycle retention rate at high temperature are both reduced.
[0188] It can be seen from Examples 1, 5, 6, 8-11 that whether the positive electrode material contains a coating element M, a change in the type of the doping element G, a change in the amount of the cobalt additive, and a change in the first sintering condition will not affect the XRD structural characteristics of the positive electrode material. As long as the positive electrode material contains a coating layer formed by the cobalt additive defined in the present invention, a positive electrode material having the specific XRD structural characteristics of the present invention can be prepared, and when the positive electrode material is used in a lithium-ion battery, the electrical performance of the battery can be significantly improved compared to the prior art.
[0189] Figure 2 is the SEM of the positive electrode material of Example 1, and Figure 3 is the SEM of the positive electrode material of Example 12. As can be seen from Figures 2 and 3, the coating state of the positive electrode material surface of Example 12 is significantly worse than that of Example 1. A large number of cobalt agglomerated particles (especially a large number of small particles enriched in the middle part) appear in the SEM image, and some of the positive electrode material surfaces still have exposed parts after coating. The additives in Example 3 are difficult to mix evenly. This is because the cobalt additive D in Example 12 50 Larger, more particles adhere to each other; It can be seen from Examples 1, 12 and 13 that the K 90 Large, wide particle size distribution, more difficult to mix evenly under the same conditions, therefore, the use of this D 50 Too large and / or K 90 Excessive cobalt additives in product preparation will lead to a significant decrease in the electrical performance of the finished positive electrode material due to uneven mixing.
[0190] In Comparative Examples 3 and 4, the cobalt additive is a single cobalt oxyhydroxide or cobaltous hydroxide, and its D 50 Within the scope defined by the present invention, the performance of the finished cathode materials prepared using the method is worse than that of the material in Example 1. Figure 4 is the DSC spectra of the cobalt cathode materials of Example 1, Comparative Example 3 and Comparative Example 4. From the DSC data in Figure 4, it can be seen that the thermal stability of the cathode material prepared in Example 1 is the best. Since the valence of cobalt in cobalt oxyhydroxide is +3, which is the same as the average valence of nickel, cobalt and manganese in the cathode material, it can well enter the interior of the material to make up for the defects of the lattice, and will not cause the valence state of nickel and manganese elements to change, and can play a role in stabilizing the material. Therefore, the DSC peak values of Example 1 and Comparative Example 3 are higher than the peak value of Comparative Example 4. The higher the temperature corresponding to the peak value, the higher the temperature required for combustion or even explosion, that is, the higher the peak value and the better the stability. Compared with single cobalt oxyhydroxide, the cobalt additive prepared by this method can further increase the DSC peak value and improve the thermal stability. It is also beneficial to improve the stability of the battery prepared with this cathode material.
[0191] In Comparative Example 5, the sintering temperature is too high, resulting in a larger D / R value, which causes the crystal structure of the positive electrode material to increase, the lithium ion transmission ability within the material to weaken, and the lithium-nickel mixing within the material to intensify, ultimately deteriorating the capacity and cycle performance of the material.
[0192] From the XRD refined data in Table 3, it can be seen that the Ni 2+ The positive electrode material provided by the present invention has low microstress, mixed nickel content, and specific XRD structural characteristics, which can make the positive electrode material have excellent stability.
[0193] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.
Claims
1. A cathode material, characterized in that, the micro-residual stress of the cathode material measured by XRD is 0.01 - 0.15; the average diameter of the cathode material measured by SEM is D, and the grain diameter measured by XRD is R; wherein, D / R is 1.4 - 2.
5.
2. The cathode material according to claim 1, wherein, the micro-residual stress of the cathode material measured by XRD is 0.03 - 0.15; preferably, D / R is 1.4 - 2.
3. The cathode material according to claim 1 or 2, wherein, the average diameter D of the cathode material is 1 - 3 μm, preferably 1.5 - 2 μm; preferably, the grain diameter R of the cathode material is 700 - 1200 nm, preferably 900 - 1000 nm; preferably, the median particle size D50 of the cathode material is 3 - 4.5 μm; preferably, the mixed nickel content of the cathode material is 0 - 4 wt%, preferably 0 - 3 wt%.
4. The cathode material according to any one of claims 1 - 3, wherein, the cathode material includes a matrix and a coating layer covering the matrix; the matrix has the composition shown in Formula I: Li 1+a Ni x Mn y Co z G b O 2 Formula I; wherein, -0.05 ≤ a ≤ 0.1, 0 ≤ b ≤ 0.05, 0.5 ≤ x < 1, 0 < y < 0.5, 0 ≤ z < 0.5; G is selected from at least one of W, V, Ta, Zr, La, Ce, Er, Sr, Si, Al, Mg, and Y; the coating layer includes a cobalt-containing lithium oxide and / or a cobalt-containing oxide; optionally, the coating layer further includes a lithium oxide containing M element and / or an oxide containing M element, and M is selected from at least one of B, Al, Nb, Mn, Mo, W, Si, Mg, Ti, and Zr; preferably, the molar amount n'(Co) of cobalt element in the coating layer, the molar amount n(M) of M element in the coating layer, and the total molar amount [n(Ni) + n(Co) + n(Mn) + n(G)] of metal elements other than Li in the matrix satisfy: 0.001 ≤ n'(Co):[n(Ni) + n(Co) + n(Mn) + n(G)] ≤ 0.05; 0 ≤ n(M):[n(Ni) + n(Co) + n(Mn) + n(G)] ≤ 0.
05.
5. The cathode material according to any one of claims 1 - 4, wherein, the residual alkali content of the cathode material is 1000 - 10000 ppm, preferably 1000 - 6000 ppm; preferably, when 0.5 ≤ x < 0.8, the residual alkali content of the cathode material is 1000 - 3000 ppm; or, when 0.8 ≤ x < 1, the residual alkali content of the cathode material is 4000 - 6000 ppm.
6. A method for preparing a cathode material, characterized in that, the method includes: (1) Mixing a cathode material precursor, a lithium source, and optionally an additive containing G element to obtain a mixture I; (2) Subjecting the mixture I to a first sintering in an atmosphere of air or oxygen to obtain a cathode material intermediate product II; (3) mixing the cathode material process product II, the cobalt additive and an additive optionally containing the M element to obtain a mixture III; (4) performing a second sintering on the mixture III in an atmosphere of air or oxygen to obtain the positive electrode material; The ratio of the peak intensity of the characteristic peak at 38.5° to the peak intensity of the characteristic peak at 37.4° measured by XRD of the cobalt additive is 1:1.1-7.5; Wherein, the first sintering constant temperature T 1 Less than or equal to 1000℃.
7. The method according to claim 6, in, The ratio of the peak intensity of the characteristic peak at 38.5° to the characteristic peak at 37.4° measured by XRD of the cobalt additive is 1:2-4.5; Preferably, the median particle size D of the cobalt additive is (Co)50 0.5-5 μm, preferably 0.5-3 μm; the particle size distribution K of the cobalt additive (Co)90 =(D 90 -D 10 ) / D (Co)50 Satisfy 0.8≤K (Co)90 ≤2, preferably, 1≤K (Co)90 ≤1.8; Preferably, the first sintering constant temperature T 1 It is 700-1000℃.
8. The method according to claim 6 or 7, in, Based on the total weight of the cobalt additive, the content of Co element is 55-75wt%; Preferably, the first sintering constant temperature time t 1 Less than or equal to 15h, preferably 6-12h; Preferably, the second sintering constant temperature is T 2 , where T 1 >T 2 ; Preferably, the second sintering constant temperature time is t 1 , where t 1 >t 2 .
9. The method according to any one of claims 6 to 8, in, The total molar amount of metal elements [n(Ni)+n(Mn)+n(Co)] in the positive electrode material precursor, the molar amount of Li element n(Li) in the lithium source and the molar amount of G element n(G) in the G element-containing additive are used so that: 0.95≤n(Li) / [n(Ni)+n(Mn)+n(Co)]≤1.1; 0≤n(G) / [n(Ni)+n(Mn)+n(Co)]≤0.05; Preferably, the total molar amount of metal elements in the positive electrode material process product II [n(Ni)+n(Co)+n(Mn)+n(G)], the molar amount of cobalt element n'(Co) in the cobalt additive and the molar amount of M element The molar amount n(M) of the M element in the additive is such that: 0.001≤n'(Co) / [n(Ni)+n(Co)+n(Mn)+n(G)]≤0.05; 0≤n(M) / [n(Ni)+n(Co)+n(Mn)+n(G)]≤0.
05.
10. A positive electrode material obtained by the method according to any one of claims 6 to 9.
11. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the positive electrode material according to any one of claims 1 to 5 and 10.
Citation Information
Patent Citations
High-capacity and long-cycle nickel-cobalt-manganese ternary positive electrode material and preparation method thereof
CN111969200A
High-nickel single-crystal nickel-cobalt-aluminum ternary positive electrode material and preparation method thereof
CN113422046A
Surface-coated positive electrode material, preparation method thereof and lithium ion battery
CN115084472A
Positive electrode for rechargeable lithium battery, method of preparing the same, and rechargeable lithium battery including the same
US20220093913A1