Preparation method for 52crmov4 spring steel for high-speed railway emu

Through process steps such as electric furnace smelting, LF refining and VD/RH vacuum treatment, the quality control problem of steel 52CrMoV4 for high-speed rail springs is solved, and the uniformity and fatigue performance of steel are improved, ensuring the technical requirements of high-speed rail vehicle bogie springs.

WO2024239454A1PCT designated stage expired Publication Date: 2024-11-28NANJING IRON & STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/111225
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2023-08-04
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the quality of 52CrMoV4 spring steel for high-speed rail springs, especially in terms of steel purity, tissue uniformity, decarbonization and mechanical properties, which fail to meet the technical requirements of high-speed rail vehicle bogie springs.

Method used

Using electric furnace/converter smelting, LF refining, VD/RH vacuum treatment, heating, blanking, material formation, annealing, straightening, peeling, polishing and other process steps, including stepping furnace heating, continuous annealing furnace annealing, ultrasonic + magnetic leakage Flaw detection and silver brightening processing ensure the uniformity of the chemical composition and surface quality of the steel.

Benefits of technology

The structural uniformity and comprehensive performance of steel are improved, meeting or exceeding the quality level of imported materials, ensuring the internal structure and surface defect control of spring steel, and improving the fatigue performance and surface quality of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023111225_28112024_PF_FP_ABST
    Figure CN2023111225_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention is a preparation method for 52CrMoV4 spring steel for high-speed railway emu. The preparation method comprises the steps of electric furnace / converter smelting, LF refining, VD / RH vacuum treatment, heating, cogging, heating, material forming, annealing, straightening, peeling, polishing and flaw detection to achieve the quality control of the 52CrMoV4 spring steel. The present invention solves the quality control problem of 52CrMoV4 steel for high-speed railway springs, and all the indexes thereof satisfy technical requirements.
Need to check novelty before this filing date? Find Prior Art

Description

A preparation method of 52CrMoV4 spring steel for high-speed train Technical Field

[0001] The present invention relates to the field of spring steel, and in particular to a method for preparing 52CrMoV4 spring steel for high-speed train sets. The spring steel is used for manufacturing bogie springs of high-speed train sets. Background Art

[0002] High-speed rail represents China's high-end manufacturing and is one of the nation's hallmarks. With the advancement of China's high-speed rail technology, key technologies have been independently developed and are leading the world. The localization of components such as bogie springs is also being vigorously promoted, making the localization of corresponding spring steel a necessity. 52CrMoV4 is a spring steel used in high-speed rail springs, primarily for springs on the CRH3 350km / h high-speed train. This steel has stringent requirements for purity, microstructure uniformity, decarburization, mechanical properties, and appearance quality, requiring sophisticated production processes to ensure this.

[0003] Therefore, it is necessary to develop a new preparation method for 52CrMoV4 spring steel to ensure its quality.

[0004] Summary of the Invention

[0005] Purpose of the invention: In view of the shortcomings and defects of the existing technology, the present invention provides a preparation method of 52CrMoV4 spring steel for high-speed rail EMUs, which solves the quality control problem of 52CrMoV4 steel for high-speed rail springs, and all indicators meet the technical requirements.

[0006] Technical solution: The present invention provides a method for preparing 52CrMoV4 spring steel for high-speed trains, characterized by comprising the steps of electric furnace / converter smelting, LF refining, VD / RH vacuum treatment, heating, blanking, heating, timbering, annealing, straightening, peeling, polishing, and flaw detection, thereby achieving quality control of the 52CrMoV4 spring steel.

[0007] Wherein, the VD / RH vacuum treatment adopts VD vacuum degassing treatment and then continuous casting of large square billets.

[0008] Wherein, the heating before and after the blanking is both carried out by using a walking beam furnace.

[0009] Wherein, the finished product is produced by rolling.

[0010] Wherein, the annealing is performed in a continuous annealing furnace.

[0011] Wherein, the flaw detection adopts ultrasonic + magnetic leakage flaw detection.

[0012] Wherein, the flaw detection is followed by inspection, and after the inspection, the steps of oiling and packaging are carried out.

[0013] The heating before blanking adopts high temperature and long time heating in a stepping furnace, with a soaking temperature of 1210°C-1270°C and a total heating time of ≥300min.

[0014] Wherein, the continuous annealing furnace annealing has a furnace temperature of 730±10°C and a time from reaching the temperature to taking out of the furnace of 7h-8h.

[0015] Among them, the silver bright processing method of peeling + polishing is adopted, and the grinding amount is 0.06mm-0.10mm.

[0016] Beneficial Effects: Compared with existing technologies, this invention offers the following significant advantages: It addresses the quality control issues associated with 52CrMoV4 steel for high-speed rail springs, achieving all indicators that meet technical requirements and reach or exceed the quality standards of imported materials. The invention utilizes high-temperature, long-duration heating to mitigate chemical segregation in the steel and improve its performance. Proper annealing process control results in fine, evenly distributed cementite in the annealed steel, facilitating subsequent heat treatment control. The finished steel exhibits no decarburization and surface defects. Comprehensive control is provided over the spring steel's internal structure and key indicators of fatigue performance, including uniformity, purity, decarburization, and surface defects.

[0017] The spring steel produced by the present invention has uniform and dense structure, and its comprehensive performance meets the technical requirements of spring steel for high-speed rail springs; the spring steel produced by the present invention has good surface quality and no defects, and improves the fatigue performance of the material; the high compression ratio rolling of the present invention improves the influence of the original surface of the ingot on the surface of the finished product, and improves the surface quality of the finished spring steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] FIG1 is a diagram showing the decarburization of 52CrMoV4 spring steel prepared by the method of the present invention;

[0019] FIG2 is a diagram showing the annealed structure of 52CrMoV4 spring steel prepared by the method of the present invention;

[0020] FIG3 is a diagram showing the austenitization of a finished product sample of 52CrMoV4 spring steel prepared by the method of the present invention after being kept at 860° C. for 60 minutes;

[0021] FIG4 is a surface diagram of a finished product of 52CrMoV4 spring steel prepared by the method of the present invention;

[0022] FIG5 is a macroscopic diagram of the structure of 52CrMoV4 spring steel prepared by the method of the present invention. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific implementation methods.

[0024] Example 1:

[0025] The processing method of 52CrMoV4 spring steel for high-speed train bogie springs in this embodiment includes the following process flow: EBT electric furnace smelting → LF refining furnace → VD treatment → large square bloom continuous casting → walking beam furnace heating (soaking temperature 1220-1260°C, total heating time 335 minutes, high temperature holding time 150 minutes) → cogging → walking beam furnace heating → rolling → continuous annealing furnace annealing (furnace temperature 725°C, time from reaching temperature to unloading 7 hours) → straightening and peeling → polishing (grinding amount 0.08-0.09 mm) → flaw detection (ultrasound + magnetic leakage) → inspection → oiling and packaging.

[0026] The finished products produced by this process have excellent physical and chemical testing performance and good surface condition (rolling number: M30170701).

[0027] 1. Low magnification:

[0028] 2. Depth of decarburized layer:

[0029] 3. Grain size: Heat treatment temperature and holding time: 860℃ for 60min

[0030] 4. Mechanical properties:

[0031] 5. Hardness:

[0032] 6. Surface quality: surface roughness: Ra: 1.3um; no surface defects.

[0033] Example 2:

[0034] The processing method of 52CrMoV4 spring steel for high-speed train bogie springs in this embodiment includes the following process flow: EBT electric furnace smelting → LF refining furnace → VD treatment → large square bloom continuous casting → walking beam furnace heating (soaking temperature 1250-1270°C, total heating time 320 minutes, high temperature holding time 160 minutes) → cogging → walking beam furnace heating → rolling → continuous annealing furnace annealing (furnace temperature 730°C, time from reaching temperature to unloading 7.8 hours) → straightening and peeling → polishing (grinding amount 0.06-0.07 mm) → flaw detection (ultrasound + magnetic leakage) → inspection → oiling and packaging.

[0035] The finished products produced by this process have excellent physical and chemical testing performance and good surface condition (rolling number: M30189501).

[0036] 1. Low magnification:

[0037] 2. Depth of decarburized layer:

[0038] 3. Grain size: Heat treatment temperature and holding time: 860℃ for 60min

[0039] 4. Mechanical properties:

[0040] 5. Hardness:

[0041] 6. Surface quality: surface roughness: Ra: 1.5um; no surface defects.

[0042] After testing, the 52CrMoV4 spring steel prepared by the method of the present invention has the following characteristics: decarburization is 0 (see Figure 1); the cementite in the annealed structure is fine and dispersed (see Figure 2); the finished sample is austenitized after being kept at 860°C for 60 minutes, and the grains are fine (see Figure 3); the surface of the finished material is bright and free of defects (see Figure 4); the steel has a dense macrostructure, a low organizational level, and no defects (see Figure 5).

[0043] 52CrMoV4 spring steel prepared by the method of the present invention: (1) Oxygen content ≤ 12 ppm, hydrogen content ≤ 1.2 ppm. (2) Mechanical properties: Rp ≥ 1300 MPa, R0.2: 1450-1750 MPa, A ≥ 6%, Z ≥ 35%. (3) Impact energy (20°C) AKU (J): ≥ 10 J (5 mm notch). (4) Austenite grain size: ≥ Grade 7. (5) Surface quality: Roughness ≤ 2.5 μm, no defects.

Claims

1. A method for preparing 52CrMoV4 spring steel for high-speed train sets, characterized in that: It includes electric furnace / converter smelting, LF refining, VD / RH vacuum treatment, heating, blanking, heating, timbering, annealing, straightening, peeling, polishing and flaw detection steps to achieve quality control of 52CrMoV4 spring steel.

2. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 1, characterized in that: The VD / RH vacuum treatment adopts VD vacuum degassing treatment and then continuous casting of large square billets.

3. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 1, characterized in that: The heating before and after the blanking is all carried out by a step-beam furnace.

4. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 1, characterized in that: The finished product is produced by rolling.

5. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 1, characterized in that: The annealing is performed in a continuous annealing furnace.

6. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 1, characterized in that: The flaw detection adopts ultrasonic + magnetic leakage flaw detection.

7. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 1, characterized in that: After the flaw detection, an inspection is performed, and after the inspection, oiling and packaging steps are performed.

8. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 3, characterized in that: The heating before blanking adopts high temperature and long time heating in a stepping furnace, the soaking temperature is 1210°C-1270°C, and the total heating time is ≥300min.

9. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 5, characterized in that: The continuous annealing furnace annealing has a furnace temperature of 730±10°C and a time from reaching the temperature to taking out of the furnace of 7h-8h.

10. The method for preparing 52CrMoV4 spring steel for high-speed train sets according to claim 1, characterized in that: The silver bright processing method of peeling + polishing is adopted, and the grinding amount is 0.06mm-0.10mm.

Citation Information

Patent Citations

  • Manufacturing method of directly cold-drawn spring steel wire with excellent fatigue performance

    CN102416411A

  • Manufacturing method of 51CrV4 spring steel for bogie spring of high-speed rail motor train unit

    CN114134303A

  • Steel with high wear resistance and heat treatment deformation resistance for linear guide rail and preparation method of steel

    CN115747647A

  • Nitrogen-containing microalloyed spring steel and preparation method thereof

    US20200190614A1