Composite battery cell suitable for sodium ion battery and sodium ion battery using same
By designing composite battery cells of multiple positive electrode active materials in sodium ion batteries, using flexible matching and layered coating technology, the problem that a single material cannot meet the diverse needs is solved, and the high energy density and circulation of sodium ion batteries are achieved. performance.
Patent Information
- Application Number
- PCT/CN2023/112089
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2023-08-10
- Publication Date
- 2024-11-28
Smart Images

Figure CN2023112089_28112024_PF_FP_ABST
Abstract
Description
A composite battery cell suitable for sodium ion battery and a sodium ion battery using the same
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 23, 2023, with application number 202310588340X. The entire contents of the above application are incorporated by reference into this application. Technical Field
[0002] The present application belongs to the technical field of sodium ion batteries, and specifically relates to a composite battery cell suitable for sodium ion batteries and a sodium ion battery using the composite battery cell. Background Art
[0003] Mainstream sodium-ion battery positive electrode materials include layered transition metal oxides, polyanion compounds, and Prussian blue (white) compounds. Among them, layered transition metal oxide materials have high specific capacity, but poor cycle performance, polyanion compound materials have high redox potential and good cycle stability, but low capacity and poor conductivity, and Prussian blue (white) compound materials have excellent rate performance and low cost, but low capacity and poor cycle performance. It can be seen that there are differences in the performance of mainstream sodium-ion battery positive electrode materials, and with the diversification of user needs, a single sodium-ion battery positive electrode material is difficult to meet the needs.
[0004] However, due to the varying properties of different active materials, even when integrated into the same battery cell, their advantages cannot be fully realized due to uneven mixing and irrational material matching. Therefore, integrating different active materials into the same battery cell and leveraging their synergistic advantages remains a pressing challenge for the industry. Technical issues
[0005] The present application provides a composite battery cell suitable for sodium ion batteries and a sodium ion battery using the same, so that mainstream sodium ion positive electrode active materials can be flexibly matched to adapt to various product requirements. Technical Solutions
[0006] According to one aspect of the present application, a composite battery cell suitable for a sodium ion battery is provided: the composite battery cell includes a positive electrode sheet, the number of types of the positive electrode sheets is greater than one, and among the positive electrode sheets, at least two positive electrode sheets contain positive electrode active material components with different compositions; the positive electrode sheets include at least one of a first positive electrode sheet and a second positive electrode sheet; the first positive electrode sheet contains only one positive electrode active material; the second positive electrode sheet includes at least two positive electrode active materials; the composite battery cell also includes a negative electrode sheet and a separator, and in the composite battery cell, the positive electrode sheet and the negative electrode sheet are spaced apart, and a separator is also provided between the positive electrode sheet and the negative electrode sheet.
[0007] According to a second aspect of the present application, a sodium ion battery is provided, comprising the composite battery cell as described above. The sodium ion battery provided in the present application has good energy density, rate performance, and cycle performance. Beneficial effects
[0008] The composite cell of the sodium ion battery provided in the present application integrates at least two positive electrode active materials. By selecting the types of positive electrode active materials used and adjusting the amounts of different types of positive electrode active materials, the composite cell can be flexibly adapted to various product requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] FIG1 is a schematic structural diagram of a single-component positive electrode sheet in a first positive electrode sheet;
[0010] FIG2 is a schematic diagram of a first feasible structure of the second positive electrode plate;
[0011] FIG3 is a schematic diagram of a second possible structure of the second positive electrode plate;
[0012] FIG4 is a schematic diagram of a third feasible structure of the second positive electrode plate;
[0013] FIG5 is a schematic diagram of a fourth feasible structure of the second positive electrode plate;
[0014] Figure 6 is a schematic diagram of the structure of a single combined battery cell;
[0015] FIG7 is a schematic diagram of the structure of a composite battery cell. Modes for Carrying Out the Invention
[0016] In one embodiment, the positive electrode active material contained in the composite battery cell includes at least two of layered transition metal oxide positive electrode active materials, polyanion compound positive electrode active materials, Prussian blue compound positive electrode active materials, and Prussian white compound positive electrode active materials, and the positive electrode active material is used to construct the positive electrode active coating of the positive electrode sheet.
[0017] In one embodiment, the structural formula of the layered transition metal oxide positive electrode active material is Na x MO2, the M element in the general formula includes at least one of Fe, Co, Ni, Mn, Cr, Ti, V, and Zn. In one embodiment, the above-mentioned polyanion compound positive electrode active material includes a general structural formula of Na x M y (X a O b )Z wA compound, wherein M is at least one of Ti, V, Cr, Mn, Fe, Co, Ni, Ca, Mg, Al, and Nb, X is at least one of Si, S, P, As, B, Mo, W, and Ge, and Z is at least one of F and OH.
[0018] In one embodiment, the polyanion compound-based positive electrode active material includes at least one of an olivine-type polyanion compound, a NASICON-type polyanion compound, and a fluorophosphate-type polyanion compound.
[0019] In one embodiment, in the composite battery cell, the ratio of the total capacity per unit area of any positive electrode sheet to the total capacity per unit area of any other positive electrode sheet is K1=0.9-1.1, and the total capacity per unit area of each positive electrode sheet is expressed by Formula I: In Formula I, Sn represents the areal density of any layer of positive electrode active coating included in the positive electrode sheet. In that layer of positive electrode active coating, Cm represents the gram capacity of any type of positive electrode active material. Wm represents the mass percentage of that type of positive electrode active material in that layer of positive electrode active coating. i represents the number of types of positive electrode active materials included in each layer of positive electrode active coating, i being an integer greater than or equal to 1. k represents the number of layers of positive electrode active coating included in each positive electrode sheet, k being an integer greater than or equal to 1. In the above-described composite battery cell, different positive electrode sheets satisfy a specific K1 value range. As a result, the different positive electrode sheets essentially achieve a state of capacity balance, effectively alleviating other degradation effects, such as impedance, generated by the integration of different types of positive electrode active materials in the composite battery cell. Based on this, the composite battery cell can fully leverage the synergistic advantages of different types of positive electrode active materials, resulting in an overall improvement in the energy density, rate capability, and cycle performance of the composite battery cell compared to cells using a single positive electrode active material.
[0020] The first positive electrode sheet and the second positive electrode sheet are used as examples to illustrate different calculation methods of Formula I. Formula I: For example, the first positive electrode plate uses only one positive electrode active material, and a layer of positive electrode active coating is provided on each side of the positive electrode current collector using the positive electrode active material. The two layers of positive electrode active coatings located on the two layers of the positive electrode current collector are symmetrically arranged. The mass content of the positive electrode active material used in one layer of the positive electrode active coating is W1, the gram capacity of the positive electrode active material is C1, and the surface density of the positive electrode active coating is S1. Then, the capacity of the positive electrode active coating is S1×W1×C1. Correspondingly, the capacity of the other layer of the positive electrode active coating is also calculated according to the above method. Since the two layers of positive electrode active coating are symmetrically arranged, the total capacity of the first positive electrode plate is 2×S1×W1×C1. For example, a first optional implementation of the second positive electrode plate (setting of the positive electrode active coating: layered coating on one side of the current collector and symmetrical setting on both sides): the second positive electrode plate uses two positive electrode active materials, marked as the first positive electrode active material and the second positive electrode active material, and a first positive electrode active coating containing only a single positive electrode active material of the first positive electrode active material and a second positive electrode active coating containing only a single positive electrode active material of the second positive electrode active material are sequentially arranged on one side of the positive electrode current collector, and then positive electrode active coatings symmetrical to the first positive electrode active coating and the second positive electrode active coating are correspondingly arranged on the other side of the positive electrode current collector; on either side of the positive electrode current collector, the mass content of the first positive electrode active material in the first positive electrode active coating is W1, the gram capacity of the first positive electrode active material is C1, and the first positive electrode active The areal density of the coating is S1, then the capacity of the first positive electrode active coating is S1×W1×C1, the mass content of the second positive electrode active material in the second positive electrode active coating is W2, the gram capacity of the second positive electrode active material is C2, and the areal density of the second positive electrode active coating is S2, then the capacity of the second positive electrode active coating is S2×W2×C2, and accordingly, the capacity of the positive electrode active coating on this side is (S1×W1×C1+S2×W2×C2). In addition, the capacity of the positive electrode active coating located on the other side of the positive electrode current collector is also calculated according to the above method. Since the positive electrode active coating arranged on the other side of the positive electrode current collector is symmetrical with the first positive electrode active coating and the second positive electrode active coating, the total capacity of the first positive electrode sheet is 2×(S1×W1×C1+S2×W2×C2).For example, a second optional implementation of the second positive electrode plate (setting of the positive electrode active coating: layered coating or single-layer coating on one side of the current collector, asymmetric setting on both sides): the second positive electrode plate uses two positive electrode active materials, marked as the first positive electrode active material, the second positive electrode active material and the third positive electrode active material, and a first positive electrode active coating containing only the first positive electrode active material and a second positive electrode active coating containing only the second positive electrode active material are sequentially arranged on one side of the positive electrode current collector, and then a third positive electrode active coating containing only the third positive electrode active material is arranged on the other side of the positive electrode current collector; on one side of the positive electrode current collector where a double-layer positive electrode active coating is set, the mass content of the first positive electrode active material in the first positive electrode active coating is W1, the gram capacity of the first positive electrode active material is C1, and the surface density of the first positive active coating is The density is S1, then the capacity of the first positive electrode active coating layer is S1×W1×C1, the mass content of the second positive electrode active material in the second positive electrode active coating layer is W2, the gram capacity of the second positive electrode active material is C2, and the areal density of the second positive electrode active coating layer is S2, then the capacity of the second positive electrode active coating layer is S2×W2×C2, and correspondingly, the capacity of the positive electrode active coating layer on this side is (S1×W1×C1+S2×W2×C2); on the side of the positive electrode current collector where a single layer of positive electrode active coating layer is provided, the mass content of the third positive electrode active material in the third positive electrode active coating layer is W3, the gram capacity of the third positive electrode active material is C3, and the areal density of the third positive electrode active coating layer is S3, then the capacity of the first positive electrode active coating layer is S3×W3×C3; then the total capacity of the first positive electrode sheet is (S1×W1×C1+S2×W2×C2+S3×W3×C3). For example, the third optional embodiment of the second positive electrode plate (setting of the positive electrode active coating: a single layer coating on one side of the current collector and symmetrical setting on both sides): the second positive electrode plate uses two positive electrode active materials, marked as the first positive electrode active material and the second positive electrode active material, and a layer of positive electrode active coating is set on each side of the positive electrode current collector using a slurry blended with the first positive electrode active material and the second positive electrode active material. The two layers of positive electrode active coatings located on the two layers of the positive electrode current collector are symmetrically set to each other, and in one layer of the positive active coating, the first positive electrode active material is The mass content of the material is W1, the gram capacity of the first positive electrode active material is C1, the mass content of the second positive electrode active material is W2, the gram capacity of the second positive electrode active material is C2, and the surface density of this layer of positive electrode active coating is S1. Then the capacity of this layer of positive electrode active coating is S1×(W1×C1+W2×C2). Correspondingly, the capacity of the other layer of positive electrode active coating is also calculated according to the above method. Since the two layers of positive electrode active coating are symmetrically arranged, the total capacity of the second positive electrode sheet is 2×(S1×(W1×C1+W2×C2)).For example, the fourth optional embodiment of the second positive electrode sheet (setting of the positive electrode active coating: single-layer coating on one side of the current collector and asymmetric setting on both sides): a first positive electrode active coating is set on one side of the positive electrode active coating using a slurry formed by blending the first positive electrode active material and the second positive electrode active material, and then a second positive electrode active coating containing only a single positive electrode active material of the second positive electrode active material is set on the other side of the positive electrode current collector; in the first positive electrode active coating, the mass content of the first positive electrode active material is W1, the gram capacity of the first positive electrode active material is C1, and the mass content of the second positive electrode active material is W2. The content of the second positive electrode active material is W2, the gram capacity of the second positive electrode active material is C2, the areal density of the first positive electrode active coating is S1, and the capacity of the first positive electrode active coating is S1×(W1×C1+W2×C2); in the second positive electrode active coating, the mass content of the second positive electrode active material is W3, the gram capacity of the second positive electrode active material is C3, the areal density of the second positive electrode active coating is S2, and the capacity per unit area of the second positive electrode active coating is S2×W3×C3; the total capacity per unit area of the second positive electrode sheet is (S1×(W1×C1+W2×C2)+S2×W3×C3).
[0021] In one embodiment, in the second positive electrode plate, the positive electrode active coatings constructed using different types of positive electrode active materials are layered and composited and / or respectively arranged on both sides of the current collector of the first positive electrode plate. Each layer of the positive electrode active coating of the second positive electrode plate uses only one positive electrode active material, and does not include a positive electrode active coating in which different types of positive electrode active materials are mixed together. As a result, there will be no uneven mixing of different types of positive electrode active materials due to differences in material properties, surface tension, etc., thereby avoiding the degradation effect caused by uneven distribution of positive electrode active materials in the same positive electrode active coating. When it is necessary to integrate more than two positive electrode active materials on the same positive electrode plate, the method of layering different types of positive electrode active materials on the same side or arranging different types of positive electrode active materials on both sides of the current collector can achieve the effect of preventing different types of positive electrode active materials from mixing with each other.
[0022] In one embodiment, the composite battery cell includes two first positive electrode sheets, the first positive electrode sheets include a polyanion compound type positive electrode sheet and a layered transition metal oxide type positive electrode sheet, the positive electrode active material contained in the polyanion compound type positive electrode sheet is a polyanion compound type positive electrode active material, and the positive electrode active material contained in the layered transition metal oxide type positive electrode sheet is a layered transition metal oxide type positive electrode active material.
[0023] In one embodiment, in the composite battery cell, A1 represents the number of polyanion compound type positive electrode sheets (sheets), A2 represents the number of layered transition metal oxide type positive electrode sheets (sheets), and A1 / A2=0.005-200.
[0024] In one embodiment, A1 / A2=0.01-100.
[0025] In the composite battery cell, a positive electrode sheet containing only a single type of polyanionic compound positive electrode active material and a positive electrode sheet containing only a single type of layered transition metal oxide positive electrode active material are used. This allows the advantages of both polyanionic compound positive electrode active materials and layered transition metal oxide positive electrode active materials to be integrated into the battery cell. The polyanionic electrode sheet's low humidity requirement reduces the humidity sensitivity of the positive electrode sheet containing the layered transition metal oxide positive electrode active material, thereby improving the operational stability and safety of the positive electrode sheet containing the layered transition metal oxide positive electrode active material. Furthermore, the use of a positive electrode sheet containing only one type of positive electrode active material facilitates mass production of positive electrode sheets and improves production efficiency.
[0026] In one embodiment, the battery cell assembly includes at least two different first positive electrode sheets. In the composite battery cell, the first positive electrode sheet, the separator, and the negative electrode sheet are arranged in sequence, and the different first positive electrode sheets are connected by tabs and arranged in parallel.
[0027] In one embodiment, the composite battery cell includes a first positive electrode sheet A or a first positive electrode sheet B and a second positive electrode sheet, wherein the second positive electrode sheet is a layered oxide-polyanion composite positive electrode sheet; the positive electrode active material constituting the first positive electrode sheet is only a polyanion compound type positive electrode active material or only a layered transition metal oxide type positive electrode active material; the positive electrode active material contained in the layered oxide-polyanion composite positive electrode sheet includes a layered transition metal oxide type positive electrode active material and a polyanion compound type positive electrode active material.
[0028] In one embodiment, the layered oxide-polyanion composite positive electrode plate includes a positive electrode active coating whose positive electrode active material is only layered metal oxide and a positive electrode active coating whose positive electrode active material is only polyanion compound; on the same side of the current collector of the layered oxide-polyanion composite positive electrode plate, the positive electrode active coating containing layered transition metal oxide positive electrode active material and the positive electrode coating containing polyanion compound positive electrode active material are arranged in sequence along the direction away from the surface of the current collector.
[0029] In one embodiment, the battery cell assembly is composed of at least one electrode assembly unit, each electrode assembly unit includes at least one first positive electrode sheet A or first positive electrode sheet B, a layered oxide-polyanion composite positive electrode sheet and a negative electrode sheet; in the electrode assembly unit, the first positive electrode sheet A or first positive electrode sheet B, the diaphragm, the negative electrode sheet, the diaphragm, and the layered oxide-polyanion composite positive electrode sheet are arranged in sequence; in the battery cell assembly, the first positive electrode sheet A or the first positive electrode sheet B is connected to the layered oxide-polyanion composite positive electrode sheet through electrode ears and arranged in parallel.
[0030] In one embodiment, in the composite battery cell, A1 represents the number of first positive electrode sheets (sheets), A3 represents the number of layered oxide-polyanion composite positive electrode sheets (sheets), and A1 / A3=0.001-2000.
[0031] In one embodiment, A1 / A3=0.005-200.
[0032] In one embodiment, A1 / A3=0.01-100.
[0033] In one embodiment, the positive electrode active material used in the first positive electrode plate is a polyanion compound positive electrode active material. In the above-mentioned composite battery cell, the layered oxide-polyanion composite positive electrode plate and the polyanion compound positive electrode plate are used in combination, thereby expanding the areal density range of the positive electrode plate containing the layered transition metal oxide positive electrode active material. It also enables simultaneous charging and discharging of the two aforementioned positive electrode active materials, fully leveraging the cyclic advantages of the polyanion compound positive electrode plate and efficiently utilizing the advantages of both materials, forming a complementary advantage.
[0034] In one embodiment, the positive electrode active material used in the first positive electrode plate is the layered transition metal oxide positive electrode active material. In the above-mentioned composite battery cell, a layered oxide-polyanion composite positive electrode plate and a layered transition metal oxide positive electrode plate are used together. Based on the high safety performance advantages of the polyanion composite, the composite battery cell using the layered transition metal oxide positive electrode active material can also have the advantages of high energy density and good safety.
[0035] In one embodiment, the current collector of the positive electrode plate includes two side surfaces disposed opposite to each other, each of the side surfaces being provided with the positive electrode active coating, and a ratio K2 of the total capacity per unit area of the positive electrode active coating disposed on any one side surface to the total capacity per unit area of the positive electrode active coating disposed on the other side surface is 0.9 to 1.1. The total capacity per unit area of the positive electrode active coating disposed on the same side surface is determined according to Formula II: Sn, Cm, Wm, and i in Formula II have the same meanings as those in Formula I. h in Formula II represents the number of layers of the positive electrode active coating layer disposed on the same side, and h is an integer greater than or equal to 1. In the above-described positive electrode plate, the positive electrode active coating layers located on different sides of the current collector meet a specific K2 value range. As a result, the capacity of both sides of the current collector of the positive electrode plate is substantially balanced, thereby enabling the positive electrode plate to simultaneously possess good energy density, rate performance, and cycle performance.
[0036] In one embodiment, the mass content of the positive electrode active material in the positive electrode active coating layer is 80-98%.
[0037] In one embodiment, the gram capacity of the layered transition metal oxide positive electrode active material is 80 to 300 mAh / g, the gram capacity of the polyanion compound positive electrode active material is 50 to 200 mAh / g, and the gram capacity of the Prussian blue compound positive electrode active material is 50 to 280 mAh / g.
[0038] In one embodiment, the surface density of each positive active layer is 40 to 500 g / m 2 .
[0039] In one embodiment, the negative electrode plate includes a negative electrode active material, and the negative electrode active material includes at least one of a carbon-based negative electrode active material, a titanium-based negative electrode active material, an alloy-based negative electrode active material, a carbonyl compound-based negative electrode active material, a Schiff base compound-based negative electrode active material, an organic free radical compound-based negative electrode active material, an organic sulfide-based negative electrode active material, and the like.
[0040] In one embodiment, the carbon-based negative electrode active material includes at least one of hard carbon, soft carbon, graphene, and carbon nanotubes.
[0041] In one embodiment, the titanium-based negative electrode active material includes at least one of an oxide titanium-based material and a polyanion titanium-based material. In one embodiment, the oxide titanium-based material includes Na2Ti3O7, Na 0.6 (Cr 0.6 Ti 0.4 )O2、Li4Ti5O 12 At least one of the polyanionic titanium-based materials includes at least one of NaTiOPO4 and NaTi2(PO4)3.
[0042] In one embodiment, the alloy-based negative electrode active material includes at least one of a Sn-based alloy, a Sb-based alloy, an In-based alloy, a Si-based alloy, and a Ge-based alloy.
[0043] Example 1
[0044] This embodiment uses different layered transition metal oxide positive electrode active materials, polyanion compound positive electrode active materials, Prussian blue compound positive electrode active materials, and Prussian white compound positive electrode active materials to construct positive electrode plates with different positive electrode active coating compositions, wherein a positive electrode plate containing only a single positive electrode active material in all the positive electrode active coatings contained therein is used as the first positive electrode plate, and a positive electrode plate containing a positive electrode active coating containing at least two positive electrode active materials is used as the second positive electrode plate.
[0045] 1. The first positive electrode
[0046] The first positive electrode sheet referred to in this embodiment refers to a positive electrode sheet comprising only one positive electrode active material. The schematic structural diagram of the first-phase positive electrode sheet is shown in Figure 1 . Positive electrode active coatings comprising only one positive electrode active material are symmetrically disposed on both sides of the positive electrode current collector, labeled first positive electrode active coating 1-1 and second positive electrode active coating 1-2, respectively.
[0047] (1) Polyanion compound type positive electrode
[0048] 1) Preparation of the olivine-type first positive electrode sheet: A polyanionic compound NaFePO4 with an olivine structure and a gram capacity of 100 mAh / g is used as the positive electrode active material. NaFePO4, a binder PVDF, and a conductive agent acetylene black are uniformly mixed in a mass ratio of 90:5:5 to form a positive electrode coating slurry. The positive electrode coating slurry is then applied to the two opposite sides of the positive electrode current collector and dried, thereby forming a symmetrical first positive electrode active coating 1-1 and a second positive electrode active coating 1-2 on the two sides of the positive electrode current collector. The positive electrode active material contained in the first positive electrode active coating 1-1 and the second positive electrode active coating 1-2 is only NaFePO4. The polyanionic compound-type positive electrode sheet thus prepared is marked as the olivine-type first positive electrode sheet. In the prepared olivine-type first positive electrode sheet, the surface density of the positive electrode active coating included is 300 g / m 2 The positive electrode sheet is marked as the olivine type first positive electrode sheet I, and the surface density of the positive active coating included is 200g / m 2 The positive electrode piece is marked as olivine-type first positive electrode piece II.
[0049] 2) Preparation of NASICON type first positive electrode plate: using NASICON, a polyanionic compound with a gram capacity of 120 mAh / g, as the positive electrode active material, NASICON, a binder PVDF, and a conductive agent acetylene black are mixed uniformly in a mass ratio of 90:5:5 to form a positive electrode coating slurry, and then the above-mentioned positive electrode coating slurry is coated on the two back-to-back sides of the positive electrode current collector respectively, and dried, thereby forming a symmetrically arranged first positive electrode active coating 1-1 and a second positive electrode active coating 1-2 on the two sides of the positive electrode current collector. The positive electrode active material contained in the first positive electrode active coating 1-1 and the second positive electrode active coating 1-2 is only NASICON. The polyanionic compound type positive electrode plate thus prepared is marked as the NASICON type first positive electrode plate. In the prepared NASICON type first positive electrode plate, the surface density of the included positive electrode active coating is 120 g / m 2 The positive electrode sheet is marked as NASICON type first positive electrode sheet I, with the positive electrode active coating surface density of 100g / m 2 The positive electrode sheet is marked as NASICON type first positive electrode sheet II.
[0050] The structural schematic diagram of the olivine-type first positive electrode sheet and the NASICON-type first positive electrode sheet prepared above is shown in FIG1 .
[0051] (2) Layered transition metal oxide type positive electrode
[0052] Preparation of NaMnO2 first positive electrode sheet: Using layered transition metal oxide NaMnO2 with a gram capacity of 180 mAh / g as the positive electrode active material, NaMnO2, binder PVDF, and conductive agent acetylene black are mixed evenly in a mass ratio of 80:10:10 to prepare a positive electrode coating slurry, and then the above-mentioned positive electrode coating slurry is coated on the two back-to-back sides of the positive electrode current collector respectively, and dried, thereby forming a symmetrically arranged first positive electrode active coating 1-1 and a second positive electrode active coating 1-2 on the two sides of the positive electrode current collector. The positive electrode active material contained in the first positive electrode active coating 1-1 and the second positive electrode active coating 1-2 is only NaMnO2. The layered transition metal oxide positive electrode sheet thus prepared is marked as NaMnO2 first positive electrode sheet. In the prepared NaMnO2 first positive electrode sheet, the surface density of the included positive electrode active coating is 200 g / m 2 The positive electrode sheet is marked as NaMnO2 first positive electrode sheet I, with the positive electrode active coating surface density of 300g / m 2 The positive electrode piece is marked as NaMnO2 first positive electrode piece II.
[0053] The structural schematic diagram of the NaMnO2 first positive electrode sheet prepared above is shown in FIG1 .
[0054] (3) Prussian blue compound type positive electrode
[0055] A Prussian blue compound Na2Fe[Fe(CN)6] with a gram capacity of 150 mAh / g is used as the positive electrode active material. Na2Fe[Fe(CN)6], a binder PVDF, and a conductive agent acetylene black are mixed uniformly in a mass ratio of 90:5:5 to prepare a positive electrode coating slurry. The positive electrode coating slurry is then applied to two opposite sides of the positive electrode current collector, respectively, and dried to form a first positive electrode active coating 1-1 and a second positive electrode active coating 1-2 symmetrically arranged on the two sides of the positive electrode current collector. The positive electrode active material contained in the first positive electrode active coating 1-1 and the second positive electrode active coating 1-2 is only Na2Fe[Fe(CN)6]. The Prussian blue compound type positive electrode sheet thus prepared is marked as a Na2Fe[Fe(CN)6] first positive electrode sheet. In the prepared Na2Fe[Fe(CN)6] first positive electrode sheet, the surface density of the positive electrode active coating included is 100 g / m 2 The positive electrode sheet is marked as Na2Fe[Fe(CN)6] first positive electrode sheet I, with the positive electrode active coating surface density of 120g / m 2 The positive electrode plate is marked as Na2Fe[Fe(CN)6] first positive electrode plate II.
[0056] The structural schematic diagram of the Na2Fe[Fe(CN)6] first positive electrode sheet prepared above is shown in FIG1 .
[0057] 2. Second positive electrode
[0058] The second positive electrode sheet referred to in this embodiment refers to a positive electrode sheet comprising at least two positive electrode active materials. A first feasible structural form of the second positive electrode sheet is shown in FIG2 , wherein a first positive electrode active coating 2-1 and a second positive electrode active coating 2-2 are symmetrically disposed on the two sides of the positive electrode current collector. The first positive electrode active coating 2-1 contains only the first positive electrode active material, and the second positive electrode active coating 2-2 contains only the second positive electrode active material. Furthermore, the first and second positive electrode active materials are different. A second possible structural form of the second positive electrode sheet is shown in Figure 3 . A composite first positive electrode active coating 3-1 and second positive electrode active coating 3-2 are disposed on one side of the positive electrode current collector, and a third positive electrode active coating 3-3 is disposed on the other side of the positive electrode current collector. The first positive electrode active coating 3-1 contains only the first positive electrode active material, the second positive electrode active coating 3-2 contains only the second positive electrode active material, and the third positive electrode active coating 3-3 contains only the third positive electrode active material. The third positive electrode active material is different from at least one of the first and second positive electrode active materials. A third possible structural form of the second positive electrode sheet is shown in Figure 4 . A blended positive electrode active coating 4-1 is symmetrically disposed on both sides of the positive electrode current collector. The blended positive electrode active coating 4-1 contains two different types of positive electrode active materials (the first positive electrode active material and the second positive electrode active material). The fourth feasible structural form of the second positive electrode plate is shown in Figure 5. A blended positive electrode active coating 5-1 is provided on one side of the positive electrode current collector, and the blended positive electrode active coating 5-1 contains two different types of positive electrode active materials (a first positive electrode active material and a second positive electrode active material). A single-phase positive electrode active coating 5-2 using only one positive electrode active material is provided on the other side of the positive electrode current collector.
[0059] (1) Symmetrical layered coating of the second positive electrode sheet
[0060] Layered transition metal oxide NaMnO2 with a gram capacity of 180 mAh / g is used as the positive electrode active material, and NaMnO2, binder PVDF, and conductive agent acetylene black are mixed evenly in a mass ratio of 80:10:10 to prepare the first positive electrode coating slurry; polyanionic compound NaFePO4 with an olivine structure and a gram capacity of 100 mAh / g is used as the positive electrode active material, and NaFePO4, binder PVDF, and conductive agent acetylene black are mixed evenly in a mass ratio of 90:5:5 to prepare the second positive electrode coating slurry. The first positive electrode coating slurry is applied on one side of the positive electrode current collector and dried to form a first positive electrode active coating 2-1. Then, the second positive electrode coating slurry is applied on the surface of the first positive electrode active coating 2-1 and dried to form a second positive electrode active coating 2-2. Then, the above operation is repeated on the other side of the positive electrode current collector to symmetrically arrange the first positive electrode active coating 2-1 (using the positive electrode active material as the layered transition metal oxide NaMnO2) and the second positive electrode active coating 2-2 (using the positive electrode active material as the polyanion compound NaFePO4) composited with each other on the two sides of the positive electrode current collector. The surface density of the first positive electrode active coating 2-1 is 80g / m 2 The surface density of the second positive electrode active coating 2-2 is 150 g / m 2 The symmetrical layered coating second positive electrode sheet thus prepared is labeled as a layered oxide-polyanion layered coating positive electrode sheet.
[0061] The structural schematic diagram of the layered oxide-polyanion layered coating positive electrode sheet prepared above is shown in FIG2 .
[0062] (2) Symmetrical co-doped second positive electrode
[0063] The polyanion compound NaFePO4 with an olivine structure and a gram capacity of 100mAh / g and the layered transition metal oxide NaMnO2 with a gram capacity of 180mAh / g are used as positive electrode active materials. The above-mentioned NaFePO4 and NaMnO2 are mixed in a mass ratio of 90:80, and then the resulting blended positive electrode active material, binder PVDF, and conductive agent acetylene black are evenly mixed in a mass ratio of 90:5:5 to prepare a positive electrode coating slurry. The above-mentioned positive electrode coating slurry is then coated on the two back-to-back sides of the positive electrode current collector respectively, and dried, thereby forming two symmetrically arranged blended positive electrode active coating layers 4-1 on the two sides of the positive electrode current collector. The positive electrode active material contained in each layer of the blended positive electrode active coating layer 4-1 is a blend of NaFePO4 and NaMnO2, and the surface density of each layer of the blended positive electrode active coating layer 4-1 is 220g / m 2 The layered transition metal oxide positive electrode sheet thus prepared is marked as a symmetrical co-doped second positive electrode sheet.
[0064] The structural schematic diagram of the symmetrical co-doped second positive electrode sheet prepared above is shown in FIG4 .
[0065] (2) Asymmetric second positive electrode
[0066] The polyanionic compound NaFePO4 with an olivine structure and a gram capacity of 100 mAh / g and the layered transition metal oxide NaMnO2 with a gram capacity of 180 mAh / g are used as positive electrode active materials. The above-mentioned NaFePO4 and NaMnO2 are mixed in a mass ratio of 90:80, and then the resulting blended positive electrode active material, binder PVDF, and conductive agent acetylene black are mixed in a mass ratio of 90:5:5 to form a first positive electrode coating slurry. The above-mentioned polyanionic compound NaFePO4, binder PVDF, and conductive agent acetylene black are mixed in a mass ratio of 90:5:5 to form a second positive electrode coating slurry. The above-mentioned first positive electrode coating slurry is applied to one side of the positive electrode current collector and dried to form a blended positive electrode active coating 5-1. The second positive electrode coating slurry is then applied to the other side of the positive electrode current collector and dried to form a single-phase positive electrode active coating 5-2. The surface density of the blended positive electrode active coating 5-1 is 200 g / m 2 The surface density of the single-phase positive electrode active coating 5-2 is 300g / m 2 The layered transition metal oxide positive electrode sheet thus prepared is marked as an asymmetric second positive electrode sheet.
[0067] The structural schematic diagram of the asymmetric second positive electrode plate prepared above is shown in FIG5 .
[0068] According to formula I Calculate the total capacity per unit area of the positive electrode sheet prepared in this embodiment; in Formula I, Sn represents the surface density of any layer of positive electrode active coating included in the positive electrode sheet, in the layer of positive electrode active coating, Cm represents the gram capacity of any positive electrode active material, Wm represents the mass percentage of the positive electrode active material in the layer of positive electrode active coating, i represents the number of categories of positive electrode active materials included in each layer of positive electrode active coating, i is an integer greater than or equal to 1, k represents the number of layers of positive electrode active coating included in each positive electrode sheet, k is an integer greater than or equal to 1. K1 involved in Table 1 is the ratio of the total capacity per unit area of the positive electrode sheet A to the total capacity per unit area of the positive electrode sheet B. In Formula I, It represents the capacity level per unit area of a certain layer of positive electrode active coating in the positive electrode sheet. After calculating the capacity per unit area of each layer of positive electrode active coating, the calculation results are summed up, that is, according to Calculate and finally get the capacity level per unit area of the entire positive electrode sheet.
[0069] For the first positive electrode plate, the total capacity is calculated as follows: the mass content of the positive electrode active material used in the first positive electrode active coating 1-1 is W1, the gram capacity of the positive electrode active material is C1, and the surface density of the first positive electrode active coating 1-1 is S1. Then, the capacity per unit area of the first positive electrode active coating 1-1 is S1×W1×C1. Correspondingly, the capacity of the second positive electrode active coating 1-2 is also calculated according to the above method. Since the first positive electrode active coating 1-1 and the second positive electrode active coating 1-2 are symmetrically arranged, the total capacity per unit area of the first positive electrode plate is 2×S1×W1×C1.
[0070] For the symmetrical layered coating of the second positive electrode sheet, the total capacity is calculated as follows: on either side of the positive electrode current collector, the mass content of the positive electrode active material in the first positive electrode active coating 2-1 is W1, the gram capacity of the positive electrode active material is C1, and the surface density of the first positive electrode active coating 2-1 is S1. Then, the capacity per unit area of the first positive electrode active coating 2-1 is S1×W1×C1. The mass content of the positive electrode active material in the second positive electrode active coating 2-2 is W2, the gram capacity of the positive electrode active material is C2, and the surface density of the second positive electrode active coating 2-2 is S2. Then the capacity per unit area of the second positive electrode active coating 2-2 is S2×W2×C2, and correspondingly, the capacity per unit area of the positive electrode active coating on this side is (S1×W1×C1+S2×W2×C2). In addition, the capacity of the positive electrode active coating located on the other side of the positive electrode current collector is also calculated according to the above method. Since the positive electrode active coating arranged on the other side of the positive electrode current collector is symmetrical with the first positive electrode active coating 2-1 and the second positive electrode active coating 2-2, the total capacity per unit area of the first positive electrode sheet is 2×(S1×W1×C1+S2×W2×C2).
[0071] For the symmetrical co-doped second positive electrode plate, the calculation method of its total capacity is as follows: in one layer of the blended positive electrode active coating 4-1, the mass content of one positive electrode active material (polyanion compound NaFePO4) is W1, the gram capacity of the positive electrode active material is C1, the mass content of the other positive electrode active material (layered transition metal oxide NaMnO2) is W2, the gram capacity of the positive electrode active material is C2, and the surface density of the blended positive electrode active coating 4-1 is S1. Then the capacity per unit area of the blended positive electrode active coating 4-1 is S1×(W1×C1+W2×C2). Correspondingly, the capacity of the other layer of the blended positive electrode active coating 4-1 is also calculated according to the above method. Since the two layers of the blended positive electrode active coating 4-1 are symmetrically arranged, the total capacity per unit area of the second positive electrode plate is 2×(S1×(W1×C1+W2×C2)).
[0072] For the asymmetric second positive electrode sheet, the total capacity is calculated as follows: in a mixed positive electrode active coating 5-1 containing multiple positive electrode active materials, the mass content of one positive electrode active material (polyanion compound NaFePO4) is W1, the gram capacity of the positive electrode active material is C1, the mass content of another positive electrode active material (layered transition metal oxide NaMnO2) is W2, the gram capacity of the positive electrode active material is C2, and the surface density of the mixed positive electrode active coating 5-1 is S1, then the surface density of the mixed positive electrode active coating 5-1 is The capacity per unit area is S1×(W1×C1+W2×C2). In the single-phase positive electrode active coating 5-2 containing only one positive electrode active material, the mass content of the positive electrode active material (polyanion compound NaFePO4) is W3. The gram capacity of the third positive electrode active material is C3, the surface density of the single-phase positive electrode active coating 5-2 is S2, and the capacity per unit area of the single-phase positive electrode active coating 5-2 is S2×W3×C3; the total capacity per unit area of the second positive electrode sheet is (S1×(W1×C1+W2×C2)+S2×W3×C3).
[0073] Table 1. Calculation of total capacity per unit area of each positive electrode sheet
[0074] Example 2
[0075] In this embodiment, different positive and negative electrode sheets and separators prepared in Example 1 are used to prepare different sodium ion battery cells.
[0076] The negative electrode sheet used in this embodiment is prepared as follows: hard carbon is used as the negative electrode active material, and the hard carbon, conductive agent acetylene black, binder sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) are mixed in a mass ratio of 94:1:2:3 to prepare a negative electrode coating slurry; then the above-mentioned negative electrode coating slurry is applied to the two back-to-back sides of the negative electrode current collector respectively, and dried, thereby forming two symmetrical layers of negative electrode active coating on the two sides of the negative electrode current collector.
[0077] The diaphragm used in this embodiment is a polyethylene film.
[0078] The positive electrode sheets prepared in Example 1 were used in different combinations with the negative electrode sheets prepared in this example to construct sodium ion battery cells, and the cells using different positive electrode sheet combinations were numbered. The specific groupings are shown in Tables 2 and 3. The cells shown in Table 2 are single-combination cells using only one type of positive electrode sheet, and the cells shown in Table 3 are composite cells using two types of positive electrode sheets. Using the data shown in Table 1, the capacity per unit area of the composite cells using a combination of positive electrode sheets is calculated as shown in Table 4. In Table 4, K1 is the ratio of the total capacity per unit area of the positive electrode sheet A to the total capacity per unit area of the positive electrode sheet B in the composite cell.
[0079] A sodium ion battery using a single-combination cell is prepared as follows: 60 positive electrode sheets 6-1 and 61 negative electrode sheets 6-2 are used, with the positive electrode sheets 6-1 and the negative electrode sheets 6-2 being spaced apart in sequence, and each electrode sheet being separated by a diaphragm 6-3. A single-combination cell is prepared by a lamination or winding process, and a structural schematic diagram of the single-combination cell is shown in FIG6 ; the single-combination cell is then placed in a battery casing, and then the battery casing is subjected to treatments such as welding the tabs and baking. After the moisture content is tested to be qualified, an appropriate amount of electrolyte is injected into the battery casing, and the battery casing is encapsulated. The sodium ion battery is prepared by aging, formation, and vacuum packaging.
[0080] A sodium ion battery using a composite cell is prepared as follows: 60 positive electrode sheets (including 30 positive electrode sheets A7-1 and 30 positive electrode sheets B7-2) and 61 negative electrode sheets 7-3 are used, and the positive electrode sheets A7-1, the negative electrode sheets 7-3, the positive electrode sheets B7-2, the negative electrode sheets 7-3, the positive electrode sheets A7-1, ... are arranged in a repeated order, and each adjacent electrode sheet is separated by a diaphragm 7-4. A single composite cell is prepared by a lamination or winding process, and a structural schematic diagram of the composite cell is shown in FIG7 ; then the single composite cell is placed in a battery case, and then the battery case is subjected to treatments such as welding the tabs and baking. After the moisture content test is qualified, an appropriate amount of electrolyte is injected into the battery case, and the battery case is encapsulated. The sodium ion battery is prepared by aging, formation, and vacuum packaging.
[0081] Table 2. Positive electrode sheets used for single combination battery cells
[0082] Table 3. Combination of positive plates included in composite battery cells
[0083] Table 4. Capacity distribution per unit area of the positive electrode assembly in the composite battery cell
[0084] Test Case
[0085] 1. Participants
[0086] In this test example, the sodium ion battery prepared in Example 2 was used as a test object to conduct relevant performance tests.
[0087] 2. Test content
[0088] (1) Energy density
[0089] The sodium-ion battery was charged at a constant current and constant voltage of 0.33C to 4.25V, cut off at 0.02C, and then discharged at 0.33C to 2.8V. The capacity, average voltage and cell mass were recorded. The energy density of the sodium-ion battery was calculated according to the following formula: Energy density = capacity * average voltage / battery mass.
[0090] (2) DC impedance
[0091] The sodium ion battery under test was charged to 4.25V at a constant current and constant voltage of 0.33C, cut off at 0.02C, then discharged at 0.33C for 90min, left for 10min, and the terminal voltage V1 was recorded; then discharged at 2C (current I) for 10s, and the terminal voltage V2 was recorded. The DC impedance of the sodium ion battery was calculated according to the following formula: DC impedance = |V1-V2| / I.
[0092] (3) Cycle performance
[0093] The sodium ion battery under test was placed in a constant temperature box at 45℃, charged at a constant current and constant voltage of 1C, cut off at 0.02C, and then discharged at 1C, cycled to 80% SOH, and the number of cycles was recorded.
[0094] 3. Test results
[0095] The test results of this test example are shown in Table 5. In order to analyze the test results more intuitively, the tested cells will be grouped and discussed below according to the type of positive electrode active material included in the cell.
[0096] Among the composite cells tested, the positive electrode active materials used in composite cells 1, 2, 5, 6, 7, 8, and 9 all included the polyanionic compound NaFePO4 with an olivine structure and a gram capacity of 100 mAh / g, and the layered transition metal oxide NaMnO2 with a gram capacity of 180 mAh / g. Regarding the single-composite cells, the positive electrode active materials used in single-composite cells 1 and 2 were the polyanionic compound NaFePO4 with an olivine structure and a gram capacity of 100 mAh / g, while the positive electrode active materials used in single-composite cells 5 and 6 were the layered transition metal oxide NaMnO2 with a gram capacity of 180 mAh / g. Therefore, the performance of composite cells 1, 2, 5, 6, 7, 8, and 9 was analyzed using single-composite cells 1, 2, 5, and 6 as a reference. Compared to the reference single-combination cells each using only one positive electrode active material, composite cells 1, 2, 5, 6, 7, 8, and 9, by integrating different types of positive electrode active materials into the same cell, exhibit superior cycling characteristics compared to single-combination cells containing only one positive electrode active material. Furthermore, these composite cells maintain energy density and DC impedance at levels suitable for their application, without experiencing a significant drop in energy density or a significant increase in DC impedance compared to single-combination cells. Composite cells 1 and 2 both utilize first-generation positive electrode sheets, each containing only one positive electrode active material. However, as shown in Table 4, composite cell 1 meets the requirement that the ratio of the total capacity per unit area of any two positive electrode sheets falls within the range of 0.9 to 1.1, while composite cell 2 does not meet this requirement. The data in Table 5 demonstrate that the overall performance of composite cell 1 is superior to that of composite cell 2. On the other hand, composite battery cells 5 to 9 all include a second positive electrode plate containing two positive electrode active materials. In these composite battery cells: the second positive electrode plate included in composite battery cells 5, 6, and 7 does not have a positive electrode active coating containing a blend of multiple positive electrode active materials. The second positive electrode plates used in these composite battery cells are constructed by layered coating on the same side or by separating the positive electrode active coatings containing different types of positive electrode active materials on both sides of the current collector to obtain a second positive electrode plate with different types of positive electrode active materials separated in different active coatings. In these positive electrode plates; the second positive electrode plates included in composite battery cells 8 and 9 are both provided with at least one layer of positive electrode active coating prepared by blending more than one positive electrode active material. Different types of positive electrode active materials have certain differences in material properties. For example, the surface stress conditions of the two are inconsistent, which makes the dispersion uniformity of the system containing different types of positive electrode active materials blended together lower than the dispersion uniformity of the system containing only the same type of positive electrode active materials. If the different positive electrode active materials are unevenly distributed, it will easily make the coating of the positive electrode active slurry difficult, and will also have a certain adverse effect on the electrical properties of the positive electrode active coating formed thereby.By comparison, among the composite battery cells 5 to 9, the number of cycles measured for the composite battery cells 5 to 7 is higher than the number of cycles measured for the composite battery cells 8 and 9, which can illustrate the above problem.
[0097] Among the composite cells tested, composite cells 3 and 4 both used the polyanionic compound NASICON with a gram capacity of 120 mAh / g and the Prussian blue-based compound Na2Fe[Fe(CN)6] with a gram capacity of 150 mAh / g for their positive electrode active materials. Regarding the single-composite cells, single-composite cells 3 and 4 used the polyanionic compound NASICON with a gram capacity of 120 mAh / g, while single-composite cells 7 and 8 both used the Prussian blue-based compound Na2Fe[Fe(CN)6] with a gram capacity of 150 mAh / g for their positive electrode active materials. Therefore, the performance of composite cells 3 and 4 was analyzed using single-composite cells 3, 4, 7, and 8 as a reference.
[0098] Compared to the reference single-combination cells, each using only one positive electrode active material, composite cells 3 and 4, by integrating different types of positive electrode active materials into the same cell, achieve better cycling characteristics than single-combination cells containing only one positive electrode active material. Furthermore, these composite cells maintain energy density and DC impedance at levels suitable for their application, without experiencing a significant drop in energy density or a significant increase in DC impedance compared to single-combination cells. Composite cells 3 and 4 both use first-generation positive electrode sheets, each containing only one positive electrode active material. However, according to the data shown in Table 4, composite cell 3 meets the requirement that the ratio of the total capacity per unit area of any two positive electrode sheets falls within the range of 0.9 to 1.1, while composite cell 4 does not meet this requirement. The data shown in Table 5 demonstrate that the overall performance of composite cell 3 is superior to that of composite cell 4.
[0099] Table 5. Sodium ion battery performance test results of this test example
Claims
1. A composite cell suitable for sodium ion batteries, The composite battery cell includes positive electrode sheets, the number of types of the positive electrode sheets is greater than 1, and among the positive electrode sheets, at least two of the positive electrode sheets contain positive electrode active material components with different compositions; The positive electrode sheet includes at least one of a first positive electrode sheet and a second positive electrode sheet; the first positive electrode sheet contains only one positive electrode active material; the second positive electrode sheet includes at least two positive electrode active materials; The composite battery cell further comprises a negative electrode sheet and a separator. In the composite battery cell, the positive electrode sheet and the negative electrode sheet are arranged at intervals, and a separator is further arranged between the positive electrode sheet and the negative electrode sheet.
2. The composite battery cell suitable for sodium ion battery according to claim 1, wherein: The positive electrode active materials contained in the composite battery cell include at least two of layered transition metal oxide positive electrode active materials, polyanion compound positive electrode active materials, Prussian blue compound positive electrode active materials, and Prussian white compound positive electrode active materials. The positive electrode active materials are used to construct the positive electrode active coating of the positive electrode plate.
3. The composite battery cell suitable for sodium ion battery according to claim 1, wherein: In the composite battery cell, the ratio of the total capacity per unit area of any one of the positive electrode sheets to the total capacity per unit area of any other one of the positive electrode sheets is K1=0.9-1.1, and the total capacity per unit area of each positive electrode sheet is expressed by Formula I: In the formula I, Sn represents the surface density of any layer of the positive electrode active coating included in the positive electrode plate, in the layer of the positive electrode active coating, Cm represents the gram capacity of any one of the positive electrode active materials, Wm represents the mass percentage of the positive electrode active material in the layer of the positive electrode active coating, i represents the number of categories of the positive electrode active materials included in each layer of the positive electrode active coating, i is an integer greater than or equal to 1, k represents the number of layers of the positive electrode active coating included in each positive electrode plate, k is an integer greater than or equal to 1.
4. The composite battery cell suitable for sodium ion battery according to claim 1, wherein: In the second positive electrode plate, the positive electrode active coatings constructed using different types of the positive electrode active materials are layered and composited and / or are respectively arranged on both sides of the current collector of the first positive electrode plate.
5. The composite battery cell suitable for sodium ion battery according to claim 2, wherein: The first positive electrode plate includes a polyanion compound type positive electrode plate and a layered transition metal oxide type positive electrode plate. The positive electrode active material contained in the polyanion compound type positive electrode plate is a polyanion compound type positive electrode active material, and the positive electrode active material contained in the layered transition metal oxide type positive electrode plate is a layered transition metal oxide type positive electrode active material.
6. The composite battery cell suitable for sodium ion battery according to claim 5, wherein: In the composite battery cell, A1 represents the number of the polyanion compound type positive electrode sheets, A2 represents the number of the layered transition metal oxide type positive electrode sheets, and A1 / A2=0.005-200.
7. The composite battery cell suitable for sodium ion battery according to claim 1, wherein: The battery cell assembly includes at least two different first positive electrode sheets. In the composite battery cell, the first positive electrode sheet A or the first positive electrode sheet B, the separator, and the negative electrode sheet are arranged in sequence, and different first positive electrode sheets are connected by tabs and arranged in parallel.
8. The composite battery cell suitable for sodium ion battery according to claim 2, wherein: The composite battery cell comprises the first positive electrode sheet and the second positive electrode sheet, wherein the second positive electrode sheet is a layered oxide-polyanion composite positive electrode sheet; The positive electrode active material constituting the first positive electrode plate is only the polyanion compound type positive electrode active material or only the layered transition metal oxide type positive electrode active material; The positive electrode active material contained in the layered oxide-polyanion composite positive electrode plate includes layered transition metal oxide positive electrode active materials and polyanion compound positive electrode active materials.
9. The composite battery cell suitable for sodium ion battery according to claim 8, wherein: The layered oxide-polyanion composite positive electrode plate includes the positive electrode active coating whose positive electrode active material is only layered metal oxide and the positive electrode active coating whose positive electrode active material is only polyanion compound; on the same side of the current collector of the layered oxide-polyanion composite positive electrode plate, along the direction away from the current collector surface, the positive electrode active coating containing the layered transition metal oxide positive electrode active material and the positive electrode coating containing the polyanion compound positive electrode active material are arranged in sequence.
10. The composite battery cell suitable for sodium ion battery according to claim 8, wherein: The battery cell assembly includes at least two different first positive electrode sheets. In the composite battery cell, the first positive electrode sheet A or the first positive electrode sheet B, the separator, the negative electrode sheet, the separator, and the layered oxide-polyanion composite positive electrode sheet are respectively The different positive electrode plates are connected through the tabs and arranged in parallel.
11. The composite battery cell suitable for sodium ion battery according to claim 8, wherein: In the composite battery cell, A1 represents the number of the first positive electrode sheets A or the first positive electrode sheets B, A3 represents the number of the layered oxide-polyanion composite positive electrode sheets, and A1 / A3=0.005-200.
12. The composite battery cell suitable for sodium ion battery according to claim 8, wherein: The positive electrode active material used in the first positive electrode plate is the polyanion compound positive electrode active material.
13. The composite battery cell suitable for sodium ion battery according to claim 8, wherein: The positive electrode active material used in the first positive electrode plate is the layered transition metal oxide positive electrode active material.
14. The composite battery cell suitable for sodium ion battery according to any one of claims 1 to 13, wherein: The current collector of the positive electrode plate includes two side surfaces arranged back to back, each of which is provided with a positive electrode active coating, and the ratio of the total capacity per unit area of the positive electrode active coating arranged on any one of the side surfaces to the total capacity per unit area of the positive electrode active coating arranged on the other side surface is K2=0.9-1.1, and the total capacity per unit area of the positive electrode active coating arranged on the same side surface is determined according to Formula II, Sn, Cm, Wm, and i included in the formula II have the same meanings as their respective meanings in the formula I. The h included in the formula II represents the number of layers of the positive electrode active coating arranged on the same side, and h is an integer greater than or equal to 1.
15. The composite battery cell suitable for sodium ion battery according to any one of claims 1 to 13, wherein: The mass content of the positive electrode active material in the positive electrode active coating layer is 80 to 98%.
16. The composite battery cell suitable for sodium ion battery according to any one of claims 2 to 13, wherein: The gram capacity of the layered transition metal oxide positive electrode active material is 80 to 300 mAh / g, the gram capacity of the polyanion compound positive electrode active material is 50 to 200 mAh / g, and the gram capacity of the Prussian blue compound positive electrode active material is 50 to 280 mAh / g.
17. The composite battery cell suitable for sodium ion battery according to any one of claims 1 to 13, wherein: The surface density of each positive electrode active layer is 40 to 500 g / m 2 .
18. The composite battery cell suitable for sodium ion battery according to any one of claims 1 to 13, wherein: The negative electrode plate includes a negative electrode active material, and the negative electrode active material includes at least one of a carbon-based negative electrode active material, a titanium-based negative electrode active material, an alloy-based negative electrode active material, a carbonyl compound-based negative electrode active material, a Schiff base compound-based negative electrode active material, an organic free radical compound-based negative electrode active material, an organic sulfide-based negative electrode active material, and the like.
19. A sodium ion battery, comprising the composite battery cell according to any one of claims 1 to 19.
Citation Information
Patent Citations
Manufacturing method of high-energy-density quasi-solid-state sodium ion battery
CN112290081A
Positive pole piece with both capacity and cycling stability and sodium ion battery
CN115207279A
Novel combined type layered structure of sodium ion battery pole piece
CN116417571A
Battery cell, battery pack and vehicle
CN217606878U
Electrode assembly, battery monomer, battery and electric equipment
CN219017742U
Cited By
Sodium secondary battery and electric device
CN120767378A
Battery cell
CN122370312A