Mesoporous biochar, and preparation method therefor and use thereof
Through hydrothermal pretreatment and pyrolysis technology, uniform mesoporous biochar was prepared, which solved the problem of uneven pore structure of biochar and improved its performance in screening and manganese ion adsorption.
Patent Information
- Application Number
- PCT/CN2023/135795
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2023-12-01
- Publication Date
- 2024-11-28
AI Technical Summary
The pore structure of existing biochar is uneven and the mesoporous size is difficult to control, which limits its further utilization and application in the field of screening.
Hydrothermal pretreatment is used to regulate the structure and proportion of the three components of biomass, and uniform mesoporous biochar is prepared through pyrolysis, with a pore size distribution of 2.5-3.6nm. It has a simple process, low cost and no pollution, and is suitable for large-scale production.
The uniform mesoporous structure of biochar is realized, and its application performance in the field of screening is improved, especially the adsorption ability of manganese ions in water is improved.
Smart Images

Figure CN2023135795_28112024_PF_FP_ABST
Abstract
Description
Mesoporous biochar and its preparation method and application Technical Field
[0001] The present invention belongs to the technical field of biochar preparation, and in particular relates to a mesoporous biochar and a preparation method and application thereof. Background Art
[0002] Biochar, with its well-developed pores and rich functional groups, has been widely used in soil remediation, carbon sequestration and emission reduction, and wastewater and exhaust gas treatment. Currently, biomass-based carbon materials are favored by scientists due to their wide availability of raw materials and stable physical and chemical properties. Numerous studies have shown that pore structure determines the usefulness of biochar. Most biochars have a multi-level pore structure, where micropores primarily serve as adsorption, mesopores act as sieving, and macropores act as transport and conduction. Therefore, regulating the pore structure of biochar has both practical and theoretical significance for the further utilization of biomass-based porous carbon.
[0003] Biomass is a macromolecular structure composed of cellulose, hemicellulose and lignin interwoven and combined. However, the pyrolysis characteristics of cellulose, hemicellulose and lignin are different, resulting in uncontrollable pyrolysis process and products. Therefore, how to break the intertwined structure of biomass macromolecules is of great significance for analyzing the pyrolysis process and regulating the composition of products. At present, the pretreatment methods for breaking the three-component structure of biomass mainly include physical, chemical, and biological pretreatment methods. However, after treatment by the above methods, the obtained biochar all has a multi-level pore structure with uneven pore structure. The mesopore size of the carbon material is difficult to be effectively controlled, which is not conducive to the further utilization and application of biochar in the field of screening.
[0004] Summary of the Invention
[0005] The purpose of the present invention is to provide a mesoporous biochar and its preparation method and application, in response to the problems in the prior art that the pore structure of biomass is uneven and the mesopore size of carbon materials is difficult to be effectively controlled. Hydrothermal pretreatment is used to regulate the structure and proportion of the three components of biomass, and then uniform mesoporous biochar is prepared by pyrolysis with a pore size distribution of 2.5-3.6nm. The process is simple, low cost, pollution-free, and easy to large-scale production.
[0006] In order to achieve the above objectives, the technical solutions adopted in this application are:
[0007] The first object of the present invention is a method for preparing biomass-based mesoporous biochar, comprising the following steps:
[0008] S1. The biomass straw is crushed and sieved, then added to water, stirred evenly, and placed in a reactor for hydrothermal reaction pretreatment. After the hydrothermal reaction is completed, it is immediately cooled to room temperature, filtered, washed, and dried to obtain a precursor;
[0009] S2. The precursor is placed in a container and carbonized at 400-600° C. under a protective gas atmosphere. After carbonization, the precursor is cooled to room temperature, washed, and dried to obtain biomass-based mesoporous biochar.
[0010] Preferably, in S1, the biomass straw is crop straw, which is crushed and passed through an 18-mesh sieve.
[0011] Preferably, in S1, the mass ratio of the biomass straw to water is 1:9-15.
[0012] Preferably, in S1, the temperature of the hydrothermal reaction is 160-240° C., and the time is 10-60 min.
[0013] Preferably, in S2, the protective gas is nitrogen, the pyrolysis time is 2 to 4 hours, and the heating rate is 10 to 20°C / min.
[0014] Preferably, in S1 and S2, the drying temperature is 45-60° C. and the drying time is 24-48 hours.
[0015] The second object of the present invention is to provide mesoporous biochar prepared by the above method, wherein the pore size of the mesoporous biochar is 2.5 to 3.6 nm.
[0016] The third object of the present invention is to provide the use of the above-mentioned mesoporous biochar in removing manganese ions from water.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention adopts hydrothermal as a pretreatment method to hydrolyze cellulose and hemicellulose to obtain a biomass precursor rich in lignin, and then utilizes a pyrolysis carbonization method to carbonize the precursor into biochar to obtain biochar with a uniform mesoporous structure.
[0019] The present invention utilizes mild and controllable hydrothermal conditions as a pretreatment method to hydrolyze cellulose and hemicellulose without damaging the lignin structure. The uniform mesoporous structure of the obtained biochar originates from the natural structure of lignin. The conditions for preparing the mesoporous biochar are controllable and the process is repeatable, which is an effective method for preparing uniform mesoporous biochar. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] FIG1 shows the pH change of the pretreatment liquid of the hydrothermal reaction according to an embodiment of the present invention;
[0021] FIG2 shows the change in conductivity of the pretreatment liquid of the hydrothermal reaction according to an embodiment of the present invention;
[0022] FIG3 shows the solid yields at the same hydrothermal temperature in the embodiments of the present invention;
[0023] FIG4 is an infrared spectrum of a precursor after pretreatment of a hydrothermal reaction according to an embodiment of the present invention;
[0024] FIG5 is a thermogravimetric analysis of a pretreated precursor of a hydrothermal reaction according to an embodiment of the present invention;
[0025] FIG6 is an infrared spectrum of the mesoporous biochar prepared in an embodiment of the present invention;
[0026] FIG7 is a thermogravimetric analysis of mesoporous biochar according to an embodiment of the present invention;
[0027] FIG8 is an X-ray diffraction pattern of mesoporous biochar according to an embodiment of the present invention;
[0028] FIG9 is a scanning electron microscope image of mesoporous biochar according to an embodiment of the present invention;
[0029] FIG10 is a nitrogen adsorption-desorption curve of the mesoporous biochar according to an embodiment of the present invention;
[0030] FIG11 is the pore size distribution of mesoporous biochar according to an embodiment of the present invention;
[0031] Figure 12 shows the effect of mesoporous biochar on Mn at the same contact time in the embodiment of the present invention. 2+ adsorption capacity;
[0032] Figure 13 shows the effect of mesoporous biochar on Mn at the same contact time in the embodiment of the present invention. 2+ Adsorption isotherm
[0033] FIG14 is a standard curve of manganese ion adsorption by mesoporous biochar according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the data and drawings in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0035] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0036] Example 1
[0037] A method for preparing biomass-based mesoporous biochar comprises the following steps:
[0038] S1. The biomass corn stalks were crushed and passed through an 18-mesh sieve using a screening machine. The sieved material was the obtained biomass powder. 10 g of the biomass powder was added to a hydrothermal reactor, and then 90 mL of deionized water was added and stirred evenly. The reactor was then placed in an oven for hydrothermal reaction pretreatment at 240 ° C for 60 min. After the hydrothermal reaction was completed, the reactor was immersed in room temperature water and quickly cooled to room temperature to terminate the pretreatment. The pretreated solid-liquid mixture was separated by vacuum filtration, and the solid product was washed with deionized water and dried at 55 ° C for 24 h to obtain a precursor;
[0039] S2. Weigh 5 g of the precursor, place it in a quartz boat, compact it and put it into a quartz tube, then put it into a tube furnace, use nitrogen as the insulation gas, and carbonize it at 500 ° C for 2 h with a heating rate of 10 ° C / min. After carbonization, cool it to room temperature, wash it with deionized water, and dry it at 55 ° C for 24 h to obtain mesoporous biochar.
[0040] Example 2
[0041] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the time for the hydrothermal reaction pretreatment in S1 is 50 minutes.
[0042] Example 3
[0043] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the time for the hydrothermal reaction pretreatment in S1 is 40 minutes.
[0044] Example 4
[0045] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the time for the hydrothermal reaction pretreatment in S1 is 30 minutes.
[0046] Example 5
[0047] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the time for the hydrothermal reaction pretreatment in S1 is 20 minutes.
[0048] Example 6
[0049] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the time for the hydrothermal reaction pretreatment in S1 is 10 minutes.
[0050] Example 7
[0051] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 220° C. and the time is 60 minutes.
[0052] Example 8
[0053] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 220° C. and the time is 50 minutes.
[0054] Example 9
[0055] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 220° C. and the time is 40 minutes.
[0056] Example 10
[0057] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 220° C. and the time is 30 minutes.
[0058] Example 11
[0059] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 220° C. and the time is 20 minutes.
[0060] Example 12
[0061] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 220° C. and the time is 10 minutes.
[0062] Example 13
[0063] A method for preparing biomass-based mesoporous biochar is basically the same as Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 200° C. and the time is 60 minutes.
[0064] Example 14
[0065] A method for preparing biomass-based mesoporous biochar is basically the same as Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 200° C. and the time is 50 minutes.
[0066] Example 15
[0067] A method for preparing biomass-based mesoporous biochar is basically the same as Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 200° C. and the time is 40 minutes.
[0068] Example 16
[0069] A method for preparing biomass-based mesoporous biochar is basically the same as Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 200° C. and the time is 30 minutes.
[0070] Example 16
[0071] A method for preparing biomass-based mesoporous biochar is basically the same as Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 200° C. and the time is 20 minutes.
[0072] Example 18
[0073] A method for preparing biomass-based mesoporous biochar is basically the same as Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 200° C. and the time is 10 minutes.
[0074] Example 19
[0075] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 180° C. and the time is 60 minutes.
[0076] Example 20
[0077] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 180° C. and the time is 50 minutes.
[0078] Example 21
[0079] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 180° C. and the time is 40 minutes.
[0080] Example 22
[0081] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 180° C. and the time is 30 minutes.
[0082] Example 23
[0083] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 180° C. and the time is 20 minutes.
[0084] Example 24
[0085] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 180° C. and the time is 10 minutes.
[0086] Example 25
[0087] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 160° C. and the time is 60 minutes.
[0088] Example 26
[0089] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 160° C. and the time is 50 minutes.
[0090] Example 27
[0091] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 160° C. and the time is 40 minutes.
[0092] Example 28
[0093] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 160° C. and the time is 30 minutes.
[0094] Example 29
[0095] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 160° C. and the time is 20 minutes.
[0096] Example 30
[0097] A method for preparing biomass-based mesoporous biochar is basically the same as that in Example 1, except that the temperature of the hydrothermal reaction pretreatment in S1 is 160° C. and the time is 10 minutes.
[0098] The pH of the pretreatment solution of the hydrothermal reaction of Example 1-30 of the present invention was detected. FIG. 1 shows the pH of the pretreatment solution of the hydrothermal reaction of Example 1-30 of the present invention.
[0099] pH changes of the pre-treated liquids of Example 1-30 hydrothermal reaction. As shown in Figure 1, the liquid products after pre-treatment under different hydrothermal conditions are acidic, and their pH values are all below 5. This is because the water with higher power ionizes more H + and OH - , at this time, H + and OH - The concentration of H is not lower than that of weak acid or weak base. The autocatalytic effect of acid and base exists in the hydrothermal pretreatment, which can catalyze the hydrolysis of esters and cellobiose in biomass. + and OH -This facilitates the autohydrolysis of water and the breaking of chemical bonds, the primary chemical reactions during hydrothermal pretreatment. Autocatalytic cleavage of glycosidic bonds in hemicellulose and lignin-hemicellulose bonds can occur during hydrothermal pretreatment, producing organic acids, primarily acetic acid and uronic acid, which contribute to the acidic pH of the post-hydrothermal pretreatment solution (typically between 6.5 and 2.5). The temperature and duration of hydrothermal pretreatment determine the intensity of the pretreatment; higher temperatures and longer reaction times indicate stronger pretreatment intensity. Therefore, as pretreatment intensity increases, the pH of the liquid product decreases, indicating a more acidic pH. The pH in the 180°C temperature group decreased more gradually, from 4.7 to approximately 4.3; the pH in the 240°C temperature group decreased most significantly, from 4.4 to approximately 3.1. This increased acidity indicates a greater concentration of hemicellulose degradation products in the solution, a more advanced level of hemicellulose degradation, and the further degradation of some monosaccharides into acidic products, typical of which include acetic acid, formic acid, and furfural. In addition to degradation products such as weak acids and furan compounds, monosaccharides or oligosaccharides are also important components of liquid products. Glucose or xylose produced by cellulose or hemicellulose hydrolysis is further catalytically degraded into organic acids or furan derivatives under higher temperature conditions.
[0100] Hydrothermal pretreatment mainly involves free and active H + and OH - The degradation of xylan in lignocellulose can effectively dissociate the cellulose, hemicellulose and lignin components in the raw material. + Less, it is a mild weak acid pretreatment method. Under high temperature hydrothermal pretreatment conditions, the active H + It can achieve a large amount of xylan removal and a small amount of lignin dissolution. + The activity of the solvent system is related to the charge strength. When the ionic strength of the solution is high, the hydronium ions (H + ) activity is usually enhanced. Therefore, the ionic strength in the solution can be characterized by conductivity. The changes in the conductivity of the liquid product after pretreatment under different hydrothermal conditions are shown in Figure 2. As shown in Figure 2, as the pretreatment intensity increases, the conductivity of the liquid product increases, that is, the ionic strength in the solution becomes higher, H + The increased activity in the solution system makes hemicellulose more easily degraded and a small amount of lignin is dissolved, making the hydrothermal reaction more intense and complete. The conductivity of the liquid product is positively correlated with the intensity of the hydrothermal pretreatment.
[0101] Figure 3 shows the solid yield of corn straw at different hydrothermal temperatures. As the pretreatment temperature increases, the solid residue content gradually decreases. At the same pretreatment temperature, the solid residue content gradually stabilizes with increasing pretreatment time. For example, for 60 minutes, the solid residue content of corn straw decreases from 78.43% at 160°C to 57.53% at 240°C. This indicates that further increasing the pretreatment time does not further reduce the solid residue content. At the same pretreatment time, increasing the pretreatment temperature leads to deeper biomass degradation. During hydrothermal pretreatment, the water extract from the straw first falls into the aqueous phase. Subsequently, hydrolysis reactions occur, cleaving the ester and ether bonds in the lignocellulose. This converts insoluble long-chain polymers into soluble short-chain molecules that enter the liquid phase, resulting in a continuous loss of solid mass. However, the continuously dissolved substances in the liquid phase also interact with each other, undergoing certain reactions to generate new insoluble substances that redeposit on the solid surface, resulting in a decrease in solid mass loss. In summary, the changes in biomass solid products during hydrothermal pretreatment are the manifestation of the combined effects of hydrolysis reaction and precipitation reaction. The decrease in solid yield is caused by the continuous decomposition of hemicellulose and part of the lignin in the biomass.
[0102] FIG4 is an infrared spectrum of the precursor after pretreatment of the hydrothermal reaction of Example 1-30 of the present invention. In FIG4, a is different hydrothermal time at 240°C, b is different hydrothermal time at 220°C, c is different hydrothermal time at 200°C, d is different hydrothermal time at 180°C, and e is different hydrothermal time at 160°C. As shown in FIG4, the main oxygen-containing functional groups of corn straw are: -OH (stretching vibration 3036cm -1 , bending vibration 717cm -1 ), C=O(1786-1718cm -1 ), COC(1095cm -1 ). Corn straw raw material at 1720cm -1 There is a characteristic absorption peak of hemicellulose, which mainly comes from the C=O conjugated bond in xylan. After hydrothermal pretreatment, the absorption peak weakens due to the removal of hemicellulose during the hydrothermal pretreatment process; 1720cm -1The weakening of the characteristic absorption peak is due to the shedding of the acetyl group in xylan. When the hydrothermal pretreatment temperature is 240℃ and the time is 60min, the absorption peak of hemicellulose is the smallest, indicating that the removal rate of hemicellulose is the highest at this time; with the increase of hydrothermal temperature, from 160℃ to 240℃, the absorption peaks of oxygen-containing functional groups including COC, CO, C=O, and -OH gradually increase. This may be because as the hydrothermal temperature increases, hemicellulose gradually hydrolyzes and the cellulose content in the solid product gradually increases, then the proportion of oxygen-containing functional groups in cellulose increases, and the absorption peaks of these oxygen-containing functional groups gradually increase. In summary, the higher the hydrothermal reaction temperature, the greater the contribution of the oxygen-containing functional groups in the cellulose structure to the enhancement of the infrared absorption peak intensity. The absorption peaks of the benzene ring skeleton vibration and the phenolic hydroxyl group absorption peaks also gradually become stronger, indicating that the content of lignin in the solid product also increases relatively, and pseudo-lignin is generated.
[0103] Figure 5 shows thermogravimetric analysis of the pretreated precursors from the hydrothermal reaction of an example of the present invention. In Figure 5, a and b are the TGA and DTG curves of the precursor at 220°C, respectively, while c and d are the TGA and DTG curves of the precursor at 180°C, respectively. Figures 5a and 5c show the TGA curves of the remaining solid components and the corn stover raw material after hydrothermal pretreatment at 180°C and 220°C, respectively. At the same pretreatment temperature, the TG curves nearly overlap with increasing pretreatment time (10-60 minutes). The initial degradation temperature of the raw material is 165.185°C, while that of the solid product after hydrothermal pretreatment increases to approximately 232.490°C and 245.212°C, respectively. This is primarily due to the extraction of hemicellulose, the most easily degradable component, during the hydrothermal pretreatment. The rapid mass loss rates (RMLs) are approximately 61.79%, 74.45%, and 75.01%, respectively. The total mass loss (TML) was about 75.99%, 84.04% and 84.59%, respectively. This is due to the presence of hemicellulose in corn straw, which can greatly reduce the initial temperature of rapid mass loss of fiber. Hemicellulose in corn straw is removed by hydrothermal pretreatment, which increases the initial temperature of rapid mass loss of woody biomass. Based on the extraction efficiency of hemicellulose, corn straw has a higher initial degradation temperature after hydrothermal pretreatment. During the hydrothermal pretreatment process, in addition to the large-scale extraction of hemicellulose, part of the cellulose is also dissolved and degraded, thereby increasing the rapid mass loss rate of the remaining solid components after hydrothermal pretreatment. The total mass loss depends on the residual lignin content in the remaining solid components. During the hydrothermal pretreatment process, a small amount of lignin is dissolved and degraded due to the breaking of the β-aryl ether bond, resulting in an increase in the total mass loss after hydrothermal pretreatment;
[0104] 5c and d show the DTG curves of the residual solid components and corn straw after hydrothermal pretreatment at 180°C and 220°C, respectively. It can be seen that the extraction of hemicellulose leads to the disappearance of the "shoulder peak" of the DTG curve after hydrothermal pretreatment. The maximum degradation temperatures of corn straw and the residual solid after hydrothermal pretreatment are 339.608°C, 378.986°C, and 381.897°C, respectively, and the maximum mass loss rates are 0.843% min-1. -1 、1.080%·min -1 About 1.259%·min -1 At the same pretreatment temperature, the peak shape and position of the DTG curve are almost the same as the extension of pretreatment time, and the maximum weight loss rate decreases with the extension of time. At the same pretreatment time, the maximum weight loss rate decreases with the increase of temperature. The increase in hydrothermal temperature increases the maximum degradation temperature and maximum weight loss rate of corn straw. This is mainly due to the improvement of hemicellulose extraction efficiency and the inhibition of cellulose and lignin dissolution and degradation. The pyrolysis rate of corn straw is increased and the thermal stability is enhanced, which is conducive to the subsequent high-value utilization of biomass.
[0105] Figure 6 is an infrared spectrum of the mesoporous biochar prepared in accordance with an embodiment of the present invention. In Figure 6, a represents different hydrothermal times at 240°C, b represents different hydrothermal times at 220°C, c represents different hydrothermal times at 200°C, d represents different hydrothermal times at 180°C, and e represents different hydrothermal times at 160°C. After the solid product of the hydrothermal pretreatment undergoes pyrolysis, many functional groups in the biochar are reduced. As shown in Figure 6, the peak of the infrared conversion spectrum of the biochar is concentrated in the characteristic region of 1398 cm -1 、1616cm -1 、3468cm -1 Characteristic area 1398cm -1 It is the -CH / -CH3 bending vibration absorption peak, 1600cm -1 The absorption peaks near 1616cm are mainly caused by the stretching vibration of aromatic C=C skeleton and C=O skeleton. -1 The absorption peak at 1395 cm gradually increases, that is, the aromatic C=C and C=O groups increase. The change shows that the biomass mainly undergoes dehydrogenation and deoxygenation reactions during the hydrothermal pretreatment process, the bound water decreases, the hemicellulose decomposes in large quantities, and the aromatization structure appears. At this time, the biochar surface contains a large amount of ketones, esters, and aromatic carbon; 1395 cm -1 The absorption peak at 3468 cm-1 gradually weakened, and the -CH / -CH3 groups decreased, but phenols still existed in the biochar. -1 There are absorption peaks on both sides, confirming the presence of phenolic hydroxyl or alcoholic hydroxyl (3200cm -1 -3550cm -1) exists, with the increase of hydrothermal pretreatment intensity, the biochar -1 The absorption peak at 2923 cm-1 gradually weakened, indicating that the -OH group decreased with the increase of hydrothermal pretreatment intensity. When the hydrothermal temperature was 160 °C and the hydrothermal time was less than 30 minutes, the absorption peak at 2923 cm-1 -1 and 2855cm -1 There is a small absorption peak at 2840cm, which is the CH stretching vibration absorption peak of alkane (2840cm -1 -3000cm -1 ), when the hydrothermal time is longer than 30 min or the hydrothermal temperature is higher than 160 °C, 2923 cm -1 and 2855cm -1 The absorption peak disappeared, indicating that the number of -CH3 and -CH2- groups in the small molecules of the biochar was reduced. Based on the peak intensity and peak area, it was preliminarily determined that the surface functional groups of the hydrothermal pretreated carbon were mainly aromatic hydrocarbons C=C, C=O, phenolic hydroxyl groups, and alcoholic hydroxyl groups.
[0106] The thermal stability of biochar is an important indicator for directly evaluating its stability. The thermal stability was determined by thermogravimetric analysis, and the thermogravimetric (TG) curves and differential thermogravimetric (DTG) curves of biochar with hydrothermal pretreatment temperatures of 180°C and 220°C under N2 atmosphere were obtained. Figure 7 is the thermogravimetric analysis of the mesoporous biochar of an embodiment of the present invention. In Figure 7, a and b are the TGA curves and DTG curves of biochar at 220°C, respectively, and c and d are the TGA curves and DTG curves of biochar at 180°C, respectively. As shown in Figure 7, it can be seen that the thermal weight loss process of biochar under N2 atmosphere can be divided into three stages: the first stage is the water decomposition stage, the temperature is from room temperature to 250℃, the mass loss in this stage is mainly due to the precipitation of corn straw bound water and a small amount of external water, and the weight loss rate is about 2%; the second stage is the volatile decomposition stage, the temperature is 250-500℃, this stage is mainly due to the pyrolysis of cellulose, hemicellulose and part of the lignin in the corn straw, generating a large amount of volatiles, a small amount of tar and char. The maximum weight loss rate occurs in this stage; the third stage is the char decomposition stage, the temperature is 500-800℃, this stage is due to the pyrolysis of the remaining lignin, the process is very slow and char is mainly generated after pyrolysis. After 500℃, the thermal weight loss curve and the pyrolysis rate curve tend to be flat, and there is almost no obvious change in weight loss, indicating that the biochar has been basically carbonized.
[0107] Figures 7a and 7b show the TG curves of mesoporous biochar and corn straw raw material char after hydrothermal pretreatment at 180°C and 220°C. At the same pretreatment temperature, the TG curves nearly overlap with increasing pretreatment time. However, when the hydrothermal temperature is 220°C and the hydrothermal time is 60 minutes, the thermal weight loss platform of the biochar shifts to the right, indicating that the biochar prepared at 220°C and 60 minutes has higher thermal stability. The weight loss temperature of the corn straw biochar is around 160°C, while the weight loss temperatures of the biochar prepared at 180°C and 220°C are around 450°C and 493°C, respectively. The thermal stability of the hydrothermally pretreated biochar is higher than that of the raw material char. The residual thermogravimetric content of organic components in the corn straw biochar prepared at a hydrothermal temperature of 220°C (83.818%) was higher than that in the corn straw biochar prepared at a hydrothermal temperature of 180°C (82.532%), indicating that the higher the hydrothermal pretreatment temperature, the higher the thermal stability of the biochar after hydrothermal pretreatment. Figures 7b and d show the DTG curves of the mesoporous biochar and corn straw raw material charcoal after hydrothermal pretreatment at hydrothermal temperatures of 180°C and 220°C. The maximum degradation temperatures of corn straw charcoal and biochar after hydrothermal pretreatment at hydrothermal temperatures of 180°C and 220°C were 630.551°C, 625.570°C, and 624.920°C, respectively. The maximum mass loss rates were 0.036% min-1, respectively. -1 、0.065%·min -1 About 0.066%·min -1 . At the same pretreatment temperature, the peak shape and position of the DTG curve are almost the same as the extension of pretreatment time, and the maximum weight loss rate decreases with the extension of time. At the same pretreatment time, the maximum weight loss rate decreases with the increase of temperature. The increase in hydrothermal temperature increases the maximum degradation temperature and maximum weight loss rate of biochar. This shows that with the increase in hydrothermal pretreatment intensity, the unstable components in biochar decrease and the biochar becomes more stable.
[0108] The degree of microcrystalline structure development in biochar can influence its properties. Blunt peaks indicate amorphous structures, while sharp peaks indicate crystals. The broad, diffuse peaks that appear at 2θ values of 8°-16° and 18°-30° are primarily due to the 101 and 002 crystal planes of cellulose. Figure 8 shows the X-ray diffraction (XRD) pattern of a mesoporous biochar from an example of the present invention. As shown in Figure 8, the biochar prepared by the present invention exhibits a strong, broadened diffraction peak at 2θ = 23°. The diffraction peak of the C(002) crystal plane around 23° is associated with the amorphous structure of the biochar. During the hydrothermal pretreatment process, the biomass is rapidly hydrolyzed into organic substances such as acids, aldehydes, and phenols due to the catalytic action of hydronium ions. Various aromatic structures are then further formed through dehydration or aldol condensation. The presence of a large number of porous structures and wrinkles on the surface of the material reduces the graphitization and crystallization of the material. When the hydrothermal temperature is 200°C and the time is 30 minutes, a new, weaker diffraction peak appears at 2θ = 43°. This is the 100-face diffraction peak. This is caused by the high-temperature steam entering the intercrystalline layers and catalyzing the oxidation reaction with the carbon atoms within the graphite crystallites that cause lattice distortion or defects, eliminating such distortion or defects. The appearance of these two diffraction peaks indicates the presence of graphite structure in the hydrothermally pretreated carbon. However, the two peaks are relatively slow, indicating a low degree of graphitization.
[0109] The physical morphology of different biochars can be observed through scanning electron microscopy. Figure 9 is a scanning electron microscopy image of the mesoporous biochar of the embodiment of the present invention. In Figure 9, a and b are respectively the biochar prepared in comparative example 1 at different sizes, c and d are respectively the mesoporous carbon prepared in example 29 at different sizes, e and f are respectively the mesoporous carbon prepared in example 16 at different sizes, and g and h are respectively the mesoporous carbon prepared in example 1 at different sizes. As shown in a and b in Figure 9, the pore shape of the corn straw biochar is parallel-walled, the surface is not rough, and there is a tube bundle structure. This is because the high temperature during pyrolysis destroys the structure of the corn straw, and the rupture of cellulose and hemicellulose produces a large amount of volatile substances, which opens the pore channels blocked inside the corn straw, forming a regular arrangement of the surface morphology. The volatile substances contained in the biochar will be carbonized as the pyrolysis temperature increases, and precipitate from the surface of the biochar, generating a rich pore structure on the surface of the biochar, but the corn straw biochar has fewer pores, and the surface is filled with a large number of impurity agglomerates;
[0110] Mesoporous biochar under different hydrothermal pretreatment conditions, as shown in c, d, e, f, g and h in Figure 9, when the corn straw is hydrothermally pretreated, the tubular structure of the biochar still exists, there is a layer of waxy structure on the surface, the particle outline is not obvious, and it presents a soft, loose, colloid-like surface morphology. As the intensity of hydrothermal pretreatment increases, the pores increase and raised wrinkles appear on the surface of biochar. This is the initial stage of microsphere production. When the hydrothermal temperature is greater than 220°C, holes appear on the edge of the tube bundle structure. As the hydrothermal temperature increases, the arrangement of the holes becomes more regular. This may be because under high temperature conditions, carbohydrates are rapidly precipitated from the fiber skeleton of corn stalks, and structures such as hemicellulose and cellulose are depolymerized, leading to the formation of holes, indicating that the hydrothermal pretreatment process can increase the specific surface area of biochar; in addition, the formation of pseudo-lignin can also be observed on the surface of biochar. This may be because hydrothermal pretreatment causes the cracking and modification of lignin subunits, causing the depolymerization and repolymerization of lignin. When the pretreatment temperature is increased to 200°C (or higher), the dehydration and repolymerization of polysaccharide degradation products such as furfural form pseudo-lignin.
[0111] The elements of the mesoporous biochar according to the embodiment of the present invention were analyzed, and the results are shown in Table 1.
[0112] Table 1 Element content of biochar
[0113] As shown in Table 1, the C content of straw biochar is significantly higher than that of straw raw materials, increasing from 45.02% to more than 74%, the N content is increased to 2 times that of the raw materials, and the O content is greatly reduced. After hydrothermal pretreatment of biochar, such as in Example 1, Example 16 and Example 29, the C, N and H contents in the mesoporous carbon are all increased. Among them, with the increase of hydrothermal temperature and time, the C content in the biochar gradually increases from 74.42% to 82.56%; the O content decreases from 15.089% to 12.068%. Hydrothermal pretreatment will cause the oxygen-containing functional groups with low bond energy on the aromatic ring side chain or aliphatic side chain to break and generate free radicals. A large number of oxygen-containing groups are decomposed and released with volatiles. As the pyrolysis temperature increases, the aromatic ring carbon undergoes a condensation reaction, and a small amount of oxygen-containing groups with stable structure merge with the carbon skeleton. This leads to an increase in the relative content of C atoms and a decrease in the relative content of O atoms.
[0114] The O / C, H / C, and (O+N) / C ratios represent the hydrophilicity, aromaticity, and polarity of biochar, respectively. The O / C and (O+N) / C ratios are directly proportional to the hydrophilicity and polarity of the biochar; that is, larger ratios indicate greater hydrophilicity and polarity. The H / C ratio is inversely proportional to the aromaticity of the biochar; a larger ratio indicates less aromaticity. The cation exchange capacity (CEC) of biochar is related to the O / C ratio; generally, a larger O / C ratio indicates a higher CEC value. As shown in Table 1, compared with the raw carbon, the O / C and (O+N) / C ratios of the biochar after hydrothermal pretreatment become smaller, and the H / C ratio varies. Moreover, the O / C and (O+N) / C ratios of the biochar after hydrothermal pretreatment decrease with the increase of the hydrothermal pretreatment intensity, and the H / C ratio first increases and then decreases with the increase of the hydrothermal pretreatment intensity. This indicates that compared with the raw carbon, the hydrothermal pretreated biochar has lower hydrophilicity and polarity and stronger aromaticity.
[0115] The specific surface area, pore volume, and pore size of the corn straw biochar prepared under different conditions were analyzed using a surface area analyzer (ASAP 2460 3.01). Nitrogen adsorption-desorption was used for measurement. The relevant BET data are shown in Table 2.
[0116] Table 2 BET data of biochar
[0117] The BET results of biochar are shown in Table 2. The specific surface area, total pore volume and average pore diameter of corn straw biochar are 1.4668 m 2 ·g -1 , 0.001569m 3 ·g -1, 0.5804 nm. Compared to corn straw biochar, as shown in Examples 1, 16, and 29, the BET surface area, total pore volume, and average pore diameter of the mesoporous carbons after hydrothermal pretreatment increased, indicating favorable changes in pore structure. The BET surface area of straw char increased with increasing hydrothermal pretreatment intensity. This is because as the hydrothermal temperature increases, the organic components and volatile substances in the biomass are gradually released, resulting in a more porous structure in the biochar, leading to a corresponding increase in the biochar's specific surface area. The pore volume of straw char increased and the pore diameter decreased. This is because higher hydrothermal temperatures alter the microporous structure of the corn straw, creating more mesopores and micropores in the biochar. Analysis suggests that low-temperature hydrothermal pretreatment (≤220°C) has limited destructive effect on the straw skeleton structure, resulting in no significant changes in the pore structure of biochars treated at 160°C for 20 minutes and at 200°C for 30 minutes. As the reaction temperature increases, macromolecular structures such as cellulose and hemicellulose within the straw structure begin to decompose and break down. As the temperature further rises to 240°C, the pressure in the reactor increases sharply, the lignin structure in the straw begins to decompose, and a large number of surface pores are generated, so the specific surface area continues to increase.
[0118] Figure 10 shows the nitrogen adsorption and desorption curves of the mesoporous biochar of the embodiment of the present invention. In Figure 10, a is Example 1, b is Example 16, and c is Example 29. As shown in Figure 10, the maximum nitrogen adsorption capacity of the mesoporous biochar of the embodiment can reach 6.3139 cm 3 ·g -1 The maximum nitrogen adsorption capacity of corn straw biochar is only 5.3152 cm 3 ·g -1 ; In Figure 10, a, b, and c all conform to the type II isothermal adsorption model, which represents a combined structure of micropores and mesopores, and also has a more diverse surface morphology.
[0119] Figure 11 shows the pore size distribution of the mesoporous biochar according to the embodiment of the present invention. In Figure 11, a is Example 1, b is Example 16, and c is Example 29. As shown in Figure 11, hydrothermal pretreatment can cause the pore structure of the biochar to change from macropores to mesopores or micropores, thereby improving the pore structure of the biochar. This change may be due to the destruction of the carbon chain structure of the organic matter in the straw during the hydrothermal pretreatment process, which promotes the release of internal volatile substances during the carbonization process of the biochar, so that the prepared biochar has an excellent pore structure. In summary, the hydrothermally pretreated carbon has a better pore structure and a larger specific surface area, which means that the biochar after hydrothermal pretreatment can provide more active sites for the adsorption of heavy metals, which is beneficial to improve the adsorption of Mn 2+ adsorption performance.
[0120] The mesoporous carbon prepared in Example 1 was used to remove manganese ions in water, as follows.
[0121] 1. Adsorption kinetics test
[0122] Prepare a 50 mg / L manganese ion solution, extract 100 mL of the prepared solution and put it into a 250 mL conical flask, add biochar into the conical flask at a ratio of 2 g / L, put it into a constant temperature oscillating box at 25±1℃ and 150 r / min, take samples at 5, 10, 15, 30, 60, 120, 180, and 240 min, take them out and let them stand for 5 minutes, filter the solution with a 0.45 μm filter membrane, put the filtered solution into a 2 ml sampling tube, measure its absorbance value with an atomic absorption spectrophotometer, and obtain the solution concentration and then bring it into the kinetic model for fitting.
[0123] 2. Adsorption isotherm
[0124] Manganese ion solutions with initial concentrations of 10, 30, 50, 100, 150, 200, 300, and 400 mg / L were prepared. 100 mL of the prepared solution was placed in a 250 mL conical flask, and biochar was added to the conical flask at a ratio of 2 g / L. After sealing, the flask was placed in a constant temperature shaking box and shaken at 25±1°C and 150 r / min for 24 hours. After taking out the solution, it was allowed to stand for 5 minutes. The solution was filtered with a 0.45 μm filter membrane, and the filtered solution was placed in a 2 mL sampling tube. The absorbance value was measured using an atomic absorption spectrophotometer. The solution concentration was obtained and then brought into the isotherm for fitting.
[0125] 3. Standard curve of manganese ion
[0126] From a standard manganese solution (1000 mg / L), 1 ml of the standard solution was extracted and added to a 1000 mL volumetric flask. After the volume was adjusted to the mark, the solution was diluted to 1, 2, 3, 4, and 5 mg / L. After shaking, the atomic absorption spectrometry was performed. A standard curve of manganese ion solution was obtained with absorbance as the ordinate and concentration as the abscissa. Figure 14 shows the standard curve of manganese ion adsorption by mesoporous biochar according to an embodiment of the present invention. As shown in Figure 14, the standard curve equation is Y = 0.1983X + 0.00854, where R 2 is 0.998, X is the concentration of manganese ion solution, the unit is mg / L.
[0127] Table 3 Model parameters of biochar adsorption kinetics
[0128] Figure 12 shows the effect of mesoporous biochar on Mn at the same contact time in the embodiment of the present invention. 2+In Figure 12, a is straw biochar, b is Example 1, c is Example 16, and d is Example 29. As shown in Figure 12, in the first hour, the adsorption capacity of biochars of Example 1, Example 16, and Example 29 can reach 39.52 mg / g, 37.12 mg / g, and 36.41 mg / g, respectively, while that of the raw carbon is 30.38 mg / g. These results show that hydrothermal pretreatment of carbon can accelerate the adsorption of Mn 2+ Adsorption. In the initial stage of adsorption, more than 60% of manganese ions are adsorbed by biochar, and equilibrium is gradually reached after rapid adsorption. This is because manganese ions must first be adsorbed on the surface of the adsorbent to form a single layer of manganese molecules. The adsorption reaction at this time is mainly controlled by the reaction process of the adsorption surface. As the single layer adsorption amount of manganese ions adsorbed on the surface reaches saturation, biochar begins to remove manganese ions by chemical adsorption. The calculated adsorption isotherm model fitting parameters and correlation coefficients are shown in Table 3. The regression results show that R 2 The pseudo-second-order kinetic model with a value of 0.991 to 0.999 is most suitable for describing the adsorption of Mn by biochar. 2+ process, which indicates that the adsorption process of biochar and Mn 2+ The interaction is mainly through chemical bonding between specific functional groups, that is, the adsorption process is mainly chemical adsorption.
[0129] Table 4 Model parameters of biochar adsorption isotherms
[0130] Figure 13 shows the effect of mesoporous biochar on Mn at the same contact time in the embodiment of the present invention. 2+ Adsorption isotherms are shown in Figure 13. (a) shows corn straw biochar, (b) shows Example 1, (c) shows Example 16, and (d) shows Example 29. As shown in Figure 13 and Table 4, the adsorption isotherms for corn straw biochar and hydrothermally pretreated biochar all fit the Langmuir model (R² = 0.975-0.989). The fitting results indicate that Mn²⁺ adsorption by corn straw biochar and hydrothermally pretreated biochar occurs as a surface monolayer homogeneous adsorption process. According to this model, the theoretical maximum adsorption capacities of corn straw biochar and hydrothermally pretreated biochar are 87.5029 mg / g, 152.742 mg / g, 176.826 mg / g, and 191.863 mg / g, respectively. Compared to corn straw biochar, hydrothermally pretreated biochar exhibited a maximum adsorption capacity increase of 1.19 times, indicating that hydrothermally pretreated biochar is beneficial for manganese ion adsorption. The adsorption performance of hydrothermally pretreated biochar was superior to that of corn straw biochar under various conditions, demonstrating superior adsorption efficiency.
[0131] It should be noted that when numerical ranges are mentioned in the present invention, it should be understood that both endpoints of each numerical range and any value between the two endpoints may be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes preferred embodiments. Although preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they understand the basic inventive concepts. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0132] Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if such changes and modifications fall within the scope of the claims and their equivalents, the present invention is intended to include such changes and modifications.
Claims
1. A method for preparing biomass-based mesoporous biochar, characterized in that: The following steps are involved: S1. The biomass straw is crushed and sieved, then added into water, stirred evenly, and placed in a reactor for hydrothermal reaction pretreatment. After the hydrothermal reaction is completed, it is immediately cooled to room temperature, filtered, washed and dried to obtain a precursor; S2. Place the precursor in a container and carbonize it at 400-600° C. in a protective gas atmosphere. After carbonization, cool it to room temperature, wash and dry it to obtain biomass-based mesoporous biochar.
2. The method for preparing biomass-based mesoporous biochar according to claim 1, characterized in that: In S1, the biomass straw is crop straw, which is crushed and passed through an 18-mesh sieve.
3. The method for preparing biomass-based mesoporous biochar according to claim 1, characterized in that: In S1, the mass ratio of the biomass straw to water is 1:9-15.
4. The method for preparing biomass-based mesoporous biochar according to claim 1, characterized in that: In S1, the temperature of the hydrothermal reaction is 160-240° C., and the time is 10-60 min.
5. The method for preparing biomass-based mesoporous biochar according to claim 1, characterized in that: In S2, the protective gas is nitrogen, the pyrolysis time is 2 to 4 hours, and the heating rate is 10 to 20°C / min.
6. The method for preparing biomass-based mesoporous biochar according to claim 1, characterized in that: In S1 and S2, the drying temperature is 45-60°C and the drying time is 24-48 hours.
7. A mesoporous biochar prepared by the method according to any one of claims 1 to 6, characterized in that: The pore size of the mesoporous biochar is 2.5-3.6 nm.
8. Use of the mesoporous biochar according to claim 7 in removing manganese ions from water.
Citation Information
Patent Citations
New method for comprehensive utilization of straw resource
CN101811692A
Method for preparing modified wheat straw hydrothermal charcoal by adopting KOH
CN104069813A
Biomass carbon / molybdenum disulfide nano composite material and preparation method thereof
CN107298442A
Mesopore-enriched biochar and preparation method thereof
CN108455603A
Method for preparing porous carbon material through low-temperature hydrothermal and low-temperature carbonization of biomass